Silicone-Based Compositions Containing Carbon Nanostructures for Conductive and EMI Shielding Applications - Patent application

Silicone-based compositions incorporating carbon nanostructures address the challenge of EMI shielding in high-frequency circuits by enhancing conductivity and shielding efficiency through dispersed and cross-linked carbon nanotube fragments, achieving effective performance in reduced-size, lightweight articles.

JP7595678B2Active Publication Date: 2024-12-06CABOT CORP
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
JP2022550763
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2020-04-06
Filing Date
2021-02-24
Publication Date
2024-12-06
Estimated Expiration
2041-02-24

AI Technical Summary

Technical Problem

There is a need to improve conductive and electromagnetic interference (EMI) shielding properties of silicone-based compositions, particularly in smaller circuits operating at higher frequencies, as existing materials face challenges in achieving effective conductivity and EMI shielding efficiency.

Method used

The use of silicone-based compositions containing carbon nanostructures (CNS), such as fractured carbon nanotubes and stretched CNS strands, which are dispersed and cross-linked within a silicone matrix, providing improved connectivity and conductivity through branched fragments, even at low loadings.

Benefits of technology

The compositions exhibit enhanced electrical conductivity and EMI shielding performance, maintaining mechanical properties with reduced weight and size, achieving volume resistivity below 10^4 ohm cm and shielding efficiency of at least 35 dB at 1.5 GHz for a 2 mm thick sample.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007595678000012
    Figure 0007595678000012
  • Figure 0007595678000013
    Figure 0007595678000013
  • Figure 0007595678000014
    Figure 0007595678000014
Patent Text Reader

Abstract

Carbon nanostructures are used to prepare curable silicone-based compositions that can be used to fabricate various molded parts for EMI shielding applications. In one example, the cured material contains carbon nanostructures, carbon nanostructure fragments, broken carbon nanotubes, expanded carbon strands, and / or dispersed carbon nanostructures dispersed in a silicone component.
Need to check novelty before this filing date? Find Prior Art

Description

[Background technology]

[0001] Characterized by many attractive properties, silicones have found applications in various fields such as food and beverage, automotive, aerospace, communications, pharmaceutical, pulp and paper, coatings, paints, textiles, electronics and other industries. Silicones are used to manufacture rigid or flexible articles, as processing aids, in adhesives or sealants, etc. A general overview of the widespread use of silicones is given, for example, by M. Andriot et al. in Silicones in Industrial Applications, Inorganic Polymers, Gleria, RDJM, Ed. Nova Science Publishers: 2007; pp 61-161.

[0002] One emerging application for silicones relates to products, such as mats, sheets, pads, gaskets and other articles, designed to shield against the occurrence of electromagnetic interference (EMI) or electrostatic discharge (ESD). EMI may be generated by communication systems, radios, televisions, electronic devices, or electronic circuits in such devices. Problems associated with EMI are exacerbated by the continuing goal of reducing circuit size and achieving higher operating frequencies. Electromagnetic radiation may interfere with and / or disrupt the operation of circuits or systems in various devices between equipment. In some circumstances, electromagnetic sparks may initiate a combustion process, causing serious hazards.

[0003] Some current EMI applications of silicones include the use of electrically conductive metals, alloys, metal / non-metal composites, and carbon additives such as carbon black, graphite, graphene-based materials, and carbon nanotubes.

[0004] For example, US Patent No. 8,715,533 discloses a dielectric raw material having carbon dispersed in a silicone rubber-based material containing silicone rubber as the main material. The carbon is distributed inhomogeneously in the silicone rubber-based material or distributed such that at least some of the carbons are in contact with each other. According to this reference, the dielectric raw material may contain 150 to 300 parts by weight of carbon per 100 parts by weight of silicone rubber. The dielectric raw material may be formed by crosslinking and molding a mixture of silicone rubber in a non-crosslinked state, non-crosslinked organic polymer, and carbon. At least two types of carbon having different shapes and selected from spherical carbon, tabular carbon, carbon fiber having an aspect ratio of 11 or less, carbon nanotubes, and conductive carbon may be combined and mixed to form the dielectric raw material.

[0005] According to U.S. Pat. No. 7,479,516, nanocomposites containing functionalized and solubilized nanomaterials, such as functionalized and solubilized single-walled carbon nanotubes, multi-walled carbon nanotubes, carbon nanoparticles, carbon nanosheets, carbon nanofibers, carbon nanoropes, carbon nanoribbons, carbon nanofibrils, carbon nanoneedles, carbon nanohorns, carbon nanocones, carbon nanoscrolls, carbon nanodots, or combinations thereof, are used for electrical, thermal, and mechanical applications.

[0006] EP 3546524 A1 discloses carbon nanotubes used as conductive filters to impart conductivity to insulating silicone rubber.

[0007] According to US 2010 / 0308279, conductive silicone elastomers are prepared using carbon nanotubes in the form of individual or aggregates with macromorphologies resembling those of cotton candy, bird nest, combed yarn or open net. Preferred multi-walled carbon nanotubes have a diameter of 1 micron or less, and preferred single-walled carbon nanotubes have a diameter of less than 5 nm.

[0008] Furthermore, Korean Patent Publication No. 1753845 describes a conductive polymer composite containing nanotubes.

[0009] As shown in U.S. Pat. No. 9,181,278, a method for preparing a carbon nanotube composite having metal particles on its surface includes the steps of introducing an acyl halide to the surface, reacting the acyl halide group with an amine group of a polysiloxane to bond the polysiloxane to the surface through an amide group, and introducing metal particles to other functional groups of the polysiloxane to bond the metal particles to the surface of the carbon nanotube composite.

[0010] ANTIS TM - A multi-walled carbon nanotube-silicone masterbatch under the trade name SIL 102 is designed as an additive for silicone-based static dissipative and electrically conductive applications.

[0011] US Patent Application Publication No. 2018 / 0177081 describes an EMI shielding composite prepared using a carbon nanostructure filter in which crosslinked carbon nanotubes (CNTs) are encapsulated in a polymeric encapsulating material. To obtain the EMI shielding composite, the filter is first treated to remove at least a portion of the polymeric encapsulating material and then mixed with a curable matrix material.

[0012] US 2019 / 0352543 describes a composite composition that includes a crosslinked silicone foam having polydimethylsiloxane moieties and electromagnetically responsive particles, such as crosslinked multi-walled carbon nanotube networks, held within the crosslinked silicone foam.

[0013] MF Arif describes a sensor based on carbon nanostructure-polydimethylsiloxane nanocomposites in Strong linear-piezoresistive-response of carbon nanostructures reinforced hyperelastic polymer nanocomposites, Composites Part A 113 (2018), pp. 141-149.

[0014] In the chapter Lightweight Electromagnetic Interference Shielding Materials and Their Mechanisms by Liying Zhang, Shuguang Bi and Ming Liu et al. (submitted on July 23, 2018, reviewed on October 26, 2018, and published on December 2, 2018 in the IntechOpen book (Man-Gui Han, editor) under the title Electromagnetic Materials and Devices), desirable properties and various current materials for EMI shielding applications are described. Summary of the Invention

[0015] With the continuing goal towards smaller circuits and higher operating frequencies, there continues to be a demand for improved conductive or EMI shielding. There is also a demand for improved properties that characterize silicone-based compositions and articles. As used herein, silicone-based polymers include polysiloxanes and siloxane (-Si-O-) nThus, uncured silicone-based polymers (including the polymers in the CNS masterbatches described below) may contain hybrid polymers that do not yet contain siloxane moieties as they cure by the formation of siloxanes.

[0016] In some aspects of the invention, the invention relates to a silicone-based composition comprising a silicone-based polymer and carbon nanostructures (CNTs). In some embodiments, the composition or article comprises carbon nanostructures, fragments of carbon nanostructures, broken carbon nanotubes, extended CNS strands and / or dispersed CNTs distributed in the silicone-based component.

[0017] As used herein, the term "carbon nanostructure" or "CNS" refers to carbon nanotubes (CNTs), often multiple-walled (also known as multi-walled) carbon nanotubes (MWCNTs), which can exist as polymeric structures by interdigitating, branching, crosslinking, and / or sharing a common layer. CNSs are therefore considered to have CNTs, e.g., MWCNTs, as the base monomeric units of their polymeric structures. Typically, CNSs are grown on a substrate (e.g., a fiber material) under CNS growth conditions. In such cases, at least some of the CNTs in the CNS are aligned substantially parallel to one another, similar to the parallel CNT alignment found in conventional carbon nanotube forests.

[0018] Typically, CNSs are grown on a substrate (e.g., a fiber material) under CNS growth conditions. They can be separated from the substrate to form CNS flakes. Some of the embodiments described herein use coated or encapsulated CNSs. Additionally, CNS flakes, powders, dispersions, or other forms in which the CNS can be initially provided can also be used.

[0019] In certain instances, the CNS is provided at 0.01-15 wt% of the formulation, such as 0.1-10 wt%, or at a loading of 3-5 wt%. In many cases, a loading of 5 wt% or less can result in a volume resistivity of the silicone-containing composition of less than 2 Ω·cm. Furthermore, it has been found that a relatively small amount of CNS (e.g., less than 1 wt%, less than 0.5 wt%, less than 0.1 wt%, or less than 0.05 wt%, e.g., loadings of 0.01 wt% to 1 wt%) can be sufficient to reach the electrical percolation threshold for silicone-based polymeric CNS systems. This effect is believed to be at least in part due to the formation of branched fragments, allowing better connectivity between them, making for improved conductive connections.

[0020] In some cases, it can be used with additional additives such as carbon black, fumed silica, nickel-coated graphite, and / or metal flakes. In other implementations, it can be used in combination with silica, nickel-coated graphite, metal flakes, particles, wires, nanowires and fibers, carbon fibers, CNTs, graphene, graphite, and other additives commonly used in silicone-based compositions. Still other additives and mixtures of additives can be used as well.

[0021] The thorough dispersion of CNSs in the uncured precursor intended for the silicone-based polymer and the formation of a well- or fully-dispersed composition may be an important aspect of the present invention, and some implementations described herein relate to the mode in which the CNS is combined with the precursor intended for the silicone-based polymer (alone or in combination with one or more additives). The encapsulated or coated CNS can be used without the need to remove the binder or coating. Some embodiments prepare a masterbatch concentrate in a liquid or solid medium by a masterbatch (MB) process. The masterbatch is then diluted to prepare a system with the desired CNS loading. The concentrate is diluted with the same or different medium used in the preparation of the masterbatch. The medium may be a resin, a resin mixture, a polymer, a solvent, a solvent mixture, a solution, or a combination thereof. The complete dispersion of the CNS can result in the desired electrical properties even at very low loadings. It is believed that this effect is at least in part due to the formation of branched fragments, allowing better connectivity between them, making for improved conductive connections.

[0022] The precursors intended for silicone-based polymers can be cured using peroxide or platinum-catalyzed curing agents in one-component or two-component systems. Concentrate curing by hydroxyl groups of the polymer reacting with siloxane curing agents can also be used, as can moisture-based curing or irradiation. In some cases, silicone-based compounds are cured by amino-containing curing agents. Other curing techniques and curing agents known in the art or developed in the future can also be used. Alternatively or in addition, following curing, silicone-based rubbers or elastomers can be post-cured, for example by heating to a temperature that can form additional siloxane bonds.

[0023] Many of the embodiments described herein relate to silicone-based systems (also referred to herein as "composites") containing CNS that can be molded or extruded to form certain shapes or configurations. Among these, systems characterized by good mechanical properties (tensile strength, hardness), electrical conductivity and / or thermal conductivity are of particular interest.

[0024] CNSs may offer various advantages over conventional CNTs, likely due to their unique structure, and in contrast to CNTs, CNSs may be provided in a form (e.g., powder) that is easy and safe to handle on an industrial scale.

[0025] The compositions described herein can be used to prepare a variety of rigid or flexible articles, molded parts, field gratings, adhesives, sealants, electrodes for ESD and / or EMI shielding applications, such as for wire and cable applications. Materials according to embodiments of the invention can often be easily prepared at attractive cost, molded to produce parts of reduced size and / or weight, and provide good mechanical properties, such as tensile strength, tear strength, etc., and good EMI shielding performance, such as EMI shielding performance in the frequency range of 1 kHz to 300 GHz.

[0026] In one embodiment, the cured polymer composite comprises a cured siloxane polymer or a cured silyl-terminated hybrid polymer, and at least one CNS-derived material dispersed in the cured polymer and selected from the group consisting of carbon nanostructures, carbon nanostructure fragments, broken carbon nanotubes, stretched CNS strands, dispersed CNS, and any combination thereof. The carbon nanostructures or carbon nanostructure fragments comprise a plurality of multi-walled carbon nanotubes that are branched, interdigitated, entangled, and / or cross-linked in the polymeric structure by sharing a common layer. The broken carbon nanotubes are derived from carbon nanostructures and are branched and share a common layer with each other. The stretched CNS strands are derived from carbon nanostructures and comprise CNTs that are linearly arranged relative to each other. The dispersed CNS comprises exfoliated broken CNTs that do not share a common layer with each other.

[0027] The cured polymer composite may contain 0.01-15 wt% of the CNS-derived material, for example 1-10 wt%, 3-5 wt%, less than 10 wt%, less than 5 wt%, less than 1 wt%, less than 0.5 wt%, less than 0.1 wt%, less than 0.05 wt%, or between 0.01 wt% and 1 wt%.

[0028] Siloxane polymer is Me3SiO(SiMe2O) n Me, where n is 2 or more and at least one methyl group is selected from R' and -(O-SiR'R'') n-, where R' and R'' are independently linear or branched alkyl, linear or branched haloalkyl, aryl, haloaryl, alkoxy, aralkyl, silacycloalkyl, alkenyl, acrylate, methacrylate, amino, imino, hydroxy, epoxy, ester, alkoxy, isocyanate, phenol, polyurethane oligomer, polyamide oligomer, polyester oligomer, polyether oligomer, polyol, carboxypropyl, or halo. The silyl terminated hybrid polymer may comprise an alkoxysilane terminated polyacrylate, polyurethane, epoxy, or polyether.

[0029] The uncured polymer composite has a tensile strength of greater than 0.5 MPa or between 0.5 MPa and 10 MPa, an elongation at break of 40% to 300%, and a compressibility of 10 5 The composition may have one or more of a deposition resistivity of less than Ω·cm. The uncured polymer may be crosslinked. The composition may be a cured polymer composition having a shielding efficiency of at least 35 dB at 1.5 GHz for a 2 mm thick sample. The carbon nanostructures may be coated with or in a mixture with a binder.

[0030] The cured polymer composite may further comprise at least one additive selected from the group consisting of fumed silica, precipitated silica, semiconductor oxides, nickel coated graphite, metals, metal alloys, carbon fibers, CNTs, graphene, graphite, carbon black, clays, metal carbides, metal nitrides, metal phosphates, metal sulfates, metal carbonates, metal halides, metal hydroxides, glass, and organic fibers.

[0031] An article for electromagnetic interference shielding may include the cured polymer composite of any of the above embodiments.

[0032] In certain other embodiments, a method for preparing a polymer composite for electromagnetic interference shielding includes combining carbon nanostructures with an uncured polymer comprising a curable and moldable polymer selected from polysiloxanes or silyl-terminated hybrid polymers to form a mixture, dispersing the carbon nanostructures in the uncured polymer to produce a CNS-derived material selected from broken carbon nanotubes, stretched CNS strands, dispersed CNS, and any combination thereof. The carbon nanostructures or carbon nanostructure fragments include a plurality of multi-walled carbon nanotubes that are branched, interdigitated, entangled, and / or cross-linked in the polymeric structure by sharing a common layer. The broken carbon nanotubes are derived from carbon nanostructures and are branched and share a common layer with each other. The stretched CNS strands are derived from carbon nanostructures and include CNTs that are linearly arranged relative to each other. The dispersed CNS includes exfoliated broken CNTs that do not share a common layer with each other.

[0033] The combining step may include dispersing the carbon nanostructures until not more than one fragment of the carbon nanostructure having a bundle width greater than 50 microns is seen upon observation of a microscopic image of the mixture having an area of ​​1000 microns by 1400 microns or equivalent, the mixture being prepared for observation by diluting the mixture with additional uncured polymer to a loading of about 0.1% CNS-derived material and compressing a drop-sized aliquot between two glass microscope slides.

[0034] Polysiloxane is Me3SiO(SiMe2O) n Me, where n is 2 or more and at least one methyl group is selected from R' and -(O-SiR'R'') n-, where R' and R'' are independently linear or branched alkyl, linear or branched haloalkyl, aryl, haloaryl, alkoxy, aralkyl, silacycloalkyl, alkenyl, acrylate, methacrylate, amino, imino, hydroxy, epoxy, ester, alkoxy, isocyanate, phenol, polyurethane oligomer, polyamide oligomer, polyester oligomer, polyether oligomer, polyol, carboxypropyl, or halo. The silyl terminated hybrid polymer may comprise an alkoxysilane terminated polyacrylate, polyurethane, epoxy, or polyether.

[0035] The combining step may include mixing the carbon nanostructures with a medium selected from oil, reactive diluent, non-reactive diluent, aqueous solvent, non-aqueous solvent, or plasticizer to form a masterbatch, and mixing the masterbatch with an uncured polymer to form a mixture. The method may further include combining the mixture with a letdown polymer selected from polysiloxane or silyl-terminated hybrid polymer. The polysiloxane may be a component of a one-component curable silicone-based polymer system or a two-component curable silicone-based polymer system. The carbon nanostructures may be provided in an amount of 0.01-15 wt%, 1-10 wt%, 3-5 wt%, less than 10 wt%, less than 5 wt%, less than 1 wt%, less than 0.5 wt%, less than 0.1 wt%, less than 0.05 wt%, or 0.01%-1 wt%. The carbon nanostructures may be coated with or in a mixture with a binder.

[0036] The weight of the binder relative to the weight of the coated carbon nanostructures may range from about 0.1% to about 10%. The method may further include adding at least one additive to the mixture, the additive being selected from the group consisting of fumed silica, precipitated silica, semiconductor oxides, nickel coated graphite, metals, metal alloys, carbon fibers, CNTs, graphene, graphite, carbon black, clays, metal carbides, metal nitrides, metal phosphates, metal sulfates, metal carbonates, metal halides, metal hydroxides, glass, and organic fibers. The method may further include curing or allowing the mixture to cure. The mixture may be cured in the presence of one or more of a catalyst, heat, a crosslinking agent, moisture, microwave radiation, blue LED, ultraviolet light, electron beam radiation, and a photoinitiator. The polymer composite may be prepared according to any of the methods described above. Observation of optical microscope images of the mixtures having an area of ​​1000 microns by 1400 microns or equivalent reveals no more than one fragment of carbon nanostructures with bundle widths greater than 50 microns; polymer composites are prepared for observation by diluting the polymer composite with additional uncured polymer to a CNS loading of about 0.1% and compressing a drop-sized aliquot between two glass microscope slides.

[0037] In another embodiment, the curable polymer composition may comprise an uncured polymer comprising a curable and moldable polymer selected from polysiloxanes or silyl-terminated hybrid polymers and a CNS-derived material selected from broken carbon nanotubes, stretched CNS strands, dispersed CNS, and any combination thereof. The carbon nanostructures or fragments of carbon nanostructures comprise a plurality of multi-walled carbon nanotubes that are branched, interdigitated, entangled, and / or cross-linked in the polymeric structure by sharing a common layer. The broken carbon nanotubes are derived from carbon nanostructures and are branched and share a common layer with each other. The stretched CNS strands are derived from carbon nanostructures and comprise CNTs that are linearly arranged relative to each other. The dispersed CNS comprises exfoliated broken CNTs that do not share a common layer with each other.

[0038] When the curable polymer composition is prepared for observation in an optical microscope by diluting the composition with additional uncured polymer to a loading of about 0.1% CNS-derived material and compressing a drop-sized aliquot between two glass microscope slides to create a sample, a microscope image showing an area of ​​the sample of 1000 microns by 1400 microns or equivalent in area can contain no more than one fragment of a carbon nanostructure having a bundle width greater than 50 microns.

[0039] Polysiloxane is Me3SiO(SiMe2O) n Me, where n is 2 or more and at least one methyl group is selected from R' and -(O-SiR'R'') n-, where R' and R'' are independently linear or branched alkyl, linear or branched haloalkyl, aryl, haloaryl, alkoxy, aralkyl, silacycloalkyl, alkenyl, acrylate, methacrylate, amino, imino, hydroxy, epoxy, ester, alkoxy, isocyanate, phenol, polyurethane oligomer, polyamide oligomer, polyester oligomer, polyether oligomer, polyol, carboxypropyl, or halo. The silyl-terminated hybrid polymer may comprise an alkoxysilane-terminated polyacrylate, polyurethane, epoxy, or polyether. The curable polymer composition may further comprise an oil, a reactive diluent, a non-reactive diluent, an aqueous solvent, a non-aqueous solvent, or a plasticizer. The polysiloxane may be a component of a one-component curable silicone-based polymer system or a two-component curable silicone-based polymer system. The CNS-derived material may be present in an amount of 0.01-15 wt%, e.g., 1-10 wt%, 3-5 wt%, less than 10 wt%, less than 5 wt%, less than 1 wt%, less than 0.5 wt%, less than 0.1 wt%, less than 0.05 wt%, or 0.01-1 wt%. The CNS-derived material may further comprise a binder. The weight of the binder relative to the weight of the CNS-derived material may range from about 0.1% to about 10%. The curable polymer composition may further comprise at least one additive selected from the group consisting of fumed silica, precipitated silica, semiconductor oxides, nickel-coated graphite, metals, metal alloys, carbon fibers, CNTs, graphene, graphite, carbon black, clays, metal carbides, metal nitrides, metal phosphates, metal sulfates, metal carbonates, metal halides, metal hydroxides, glass, and organic fibers.

[0040] The above and other features and advantages of the present invention, including various details of the assembly and combination of elements, will now be more particularly described with reference to the accompanying drawings and are the subject of the claims. It will be understood that the particular methods and apparatus embodying the invention are shown by way of illustration and not as limitations of the invention. The principles and features of this invention can be employed in various and numerous embodiments without departing from the scope of the invention.

[0041] In the accompanying drawings, where reference characters refer to the same parts throughout the different views, the drawings are not necessarily to scale, emphasis instead being placed upon illustrating the principles of the invention. [Brief description of the drawings]

[0042] [Figure 1A] FIG. 2B is a diagram showing the difference between Y-shaped MWCNTs originating from but not in carbon nanostructures (FIG. 2A) and branched MWCNTs in carbon nanostructures (FIG. 2B). [Figure 1B] FIG. 2B is a diagram showing the difference between Y-shaped MWCNTs originating from but not in carbon nanostructures (FIG. 2A) and branched MWCNTs in carbon nanostructures (FIG. 2B). [Figure 2A] This is a TEM image showing the characteristic features of multi-walled carbon nanotubes found in carbon nanostructures. [Figure 2B] This is a TEM image showing the characteristic features of multi-walled carbon nanotubes found in carbon nanostructures. [Figure 3A] 1 is a SEM image of an exemplary carbon nanostructure obtained as flake material. [Figure 3B] 1 is a SEM image of an exemplary carbon nanostructure obtained as flake material. [Figure 4] 1 is an optical micrograph of an uncured silicone-based resin filled with dispersed CNS. [Diagram 5] 1 is a graph showing percolation curves for CNS in LSR and HTV polysiloxane formulations. [Figure 6A] 1 is a graph showing the EMI shielding capabilities of various filled polysiloxane formulations versus frequency. [Figure 6B] 1 is a graph showing the EMI shielding capabilities of various filled polysiloxane formulations versus frequency. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0043] The present invention will now be described more fully hereinafter with reference to the accompanying drawings showing exemplary embodiments of the invention. However, the present invention may be embodied in many different forms and should not be construed as limited to the embodiments set forth herein. Rather, these embodiments are provided so that this disclosure will be thorough and complete, and will fully convey the scope of the invention to those skilled in the art.

[0044] Generally, the present invention relates to conductive polymer systems in which the polymeric component comprises one or more silicone-based polymers and the conductivity is provided by at least one carbon additive. Many of the embodiments described herein relate to moldable systems. Of these, of particular interest are good mechanical properties (properties often associated with the utilized polymers), such as tensile strength or hardness, and / or electrical conductivity (imparted by the carbon additive). Furthermore, the materials described herein can have characteristics that are desirable in EMI shielding applications, such as light, corrosion resistance, ease of manufacture, flexibility, and attractive shielding efficiency based on reflection and / or absorption mechanisms.

[0045] The compositions are prepared using carbon nanostructures (CNSs, singular CNS), where carbon nanostructures refer to multiple carbon nanotubes (CNTs) that are branched, e.g., dendritic, interdigitated, entangled, and / or share a common layer with each other, and cross-linked in a polymeric structure. The operations performed to prepare the compositions described herein can produce CNT fragments, broken CNTs, and / or drawn CNS strands. CNS fragments are derived from CNS and include multiple CNTs that are branched, interdigitated, entangled, and / or cross-linked in a polymeric structure, as in a larger CNS. Broken CNTs are derived from CNS, branched, and share a common layer with each other. Drawn CNS strands are structures derived from CNS (including from CNS fragments and broken CNTs) where the constituent CNTs are linearly arranged relative to each other. Preferably, the procedures performed to prepare the compositions described herein produce more completely exfoliated, dispersed CNS that are capable of retaining the connections and intersections between the constituent CNTs made during manufacture of the CNS.

[0046] Highly entangled CNSs are macroscopic in size and can be considered to have carbon nanotubes (CNTs) as the basic monomeric units of their polymeric structures. For many CNTs in a CNS structure, at least one of the lateral layers of the CNT is shared with some other CNT. In general, each carbon nanotube in a CNS does not necessarily have to be branched, cross-linked, or share a common layer with other CNTs, but at least some of the CNTs in a carbon nanostructure may be interdigitated with each other and / or with branched, cross-linked, or common layer-sharing carbon nanotubes in the remainder of the carbon nanostructure.

[0047] As is known in the art, carbon nanotubes (CNTs or CNTs in the plural) are made up of interconnected sp 2Carbon nanotubes are carbonaceous materials that contain at least one sheet of hybridized carbon atoms forming a honeycomb lattice that forms a cylindrical or tubular structure. Carbon nanotubes can be single-walled carbon nanotubes (SWCNTs) or multi-walled carbon nanotubes (MWCNTs). SWCNTs are similar to fullerenes in that they are sp 2 They can be considered as a hybridized carbon allotrope. The structure is a cylindrical tube containing six-membered carbon rings. The similar MWCNTs, on the other hand, have multiple concentric cylindrical tubes. The number of these concentric layers is variable, for example, from 2 to 25 or more. Typically, MWNTs may be 10 nm or more, compared to 0.7 to 20 nm for typical SWNTs.

[0048] In many of the CNSs used in the present invention, the CNTs are, for example, MWCNTs having at least two coaxial carbon nanotubes. The number of layers present, as determined, for example, by transmission electron microscopy (TEM) at a magnification sufficient to analyze the number of layers in a particular case, may be in the range of 2 to 30, etc., such as 4 to 30; 6 to 30; 8 to 30; 10 to 30; 12 to 30; 14 to 30; 16 to 30; 18 to 30; 20 to 30; 22 to 30; 24 to 30; 26 to 30; 28 to 30; 2 to 28; 4 to 30; 5 ... 28;6~28;8~28;10~28;12~28;14~28;16~28;18~28;20~28;22~28;24~28;26~28;2~26;4~26;6~26;8~26;10~26;12~26;14~26;16~26;18~26;20~26;22~26;24~26;2~24;4~24;6~24;8~24;10~24;12~2 4;14~24;16~24;18~24;20~24;22~24;2~22;4~22;6~22;8~22;10~22;12~22;14~22;16~22;18~22;20~22;2~20;4~20;6~20;8~20;10~20;12~20;14~20;16~20;18~20;2~18;4~18;6~18;8~18;10~18;1 2-18;14-18;16-18;2-16;4-16;6-16;8-16;10-16;12-16;14-16;2-14;4-14;6-14;8-14;10-14;12-14;2-12;4-12;6-12;8-12;10-12;2-10;4-10;6-10;8-10;2-8;4-8;6-8;2-6;4-6; or 2-4.

[0049] Because CNSs are polymeric, branched and crosslinked networks of the same order as CNTs, at least some of the chemical structure observed in individual CNTs also applies to CNSs. In addition, some of the attractive properties often associated with the use of CNTs also appear in materials incorporating CNSs. These include, for example, attractive physical properties including electrical conductivity, maintaining or enabling good tensile strength when incorporated into silicone-based compositions, thermal stability (sometimes comparable to diamond crystals or in-plane graphite sheets), and / or chemical stability, to name a few.

[0050] However, as used herein, the term "CNS" is not a synonym for individual, unentangled structures, such as "monomeric" fullerenes (the term "fullerene" broadly refers to allotropes of carbon in the form of hollow spheres, ellipsoids, tubes, e.g., carbon nanotubes, and other shapes). Indeed, many embodiments of the present invention highlight the observed or anticipated differences and advantages of using CNSs over their CNT building blocks. Without wishing to be bound by theory, it is believed that the combination of branching, cross-linking, and sharing of layers between carbon nanotubes in CNSs reduces or minimizes van der Waals forces that are often problematic when using individual carbon nanotubes as well, especially when it is desirable to prevent aggregation.

[0051] In addition to or instead of performance characteristics, CNTs that are part of or derived from a CNS can be characterized by a number of properties, at least some of which may be relied upon to distinguish them from other nanomaterials, such as conventional CNTs (i.e., CNTs that are not derived from a CNS and may be provided as individual, pure or intact CNTs).

[0052] In many cases, CNTs present in or derived from a CNS have a typical diameter of 100 nanometers (nm) or less, for example, about 5 to about 100 nm, for example, about 10 to about 75 nm, about 10 to about 50 nm, about 10 to about 30 nm, about 10 to about 20 nm.

[0053] In certain embodiments, at least one of the CNTs has a length of 2 microns or more as determined by SEM. For example, at least one of the CNTs has a length of 2-2.25 microns; 2-2.5 microns; 2-2.75 microns; 2-3.0 microns; 2-3.5 microns; 2-4.0 microns; 2.25-2.5 microns; 2.25-2.75 microns; 2.25-3 microns; 2.25-3.5 microns; 2.25-4 microns; 2.5-2.75 microns; 2.5-3 microns; 2.5-3.5 microns; 2.5-4 microns; 3-3.5 microns; 3-4 microns; or 3.5-4 microns or more. In some embodiments, more than one portion, such as at least about 0.1%, at least about 1%, at least about 10%, at least about 15%, at least about 20%, at least about 25%, at least about 30%, at least about 35%, at least 40%, at least 45%, at least about 50%, or even a fraction of more than half, of the CNTs may have a length greater than 2 microns, e.g., within the ranges specified above, as determined by SEM.

[0054] The morphology of CNTs present in a CNS, in fragments of a CNS, or in disrupted CNTs derived from a CNS is often characterized by a high aspect ratio, typically with lengths greater than 100 times their diameter, and in certain cases even greater. For example, in a CNS (or CNS fragment), the aspect ratio of the length to the diameter of a CNT may range from about 200 to about 1000, e.g., 200-300; 200-400; 200-500; 200-600; 200-700; 200-800; 200-900; 300-400; 300-500; 300-600; 300-700; 300-800; 300-900; 300-1000; 400- It may be 500; 400-600; 400-700; 400-800; 400-900; 400-1000; 500-600; 500-700; 500-800; 500-900; 500-1000; 600-700; 600-800; 600-900; 600-1000; 700-800; 700-900; 700-1000; 800-900; 800-1000; or 900-1000.

[0055] In CNSs, as well as in structures derived from CNSs (e.g., in fragments of CNSs, or in broken CNTs, stretched CNS strands, or dispersed CNSs), at least one of the CNTs is characterized by a certain "branching density." As used herein, the term "branching" refers to the characteristic of single-walled carbon nanotubes branching multiple times (two or more) into connected multi-walled carbon nanotubes. One embodiment has a branching density whereby there are at least two branches along the 2 micrometer length of the carbon nanostructure as determined by SEM. There can also be three or four branches.

[0056] Additional features (e.g., detected using TEM or SEM) can be used to characterize the type of branching found in a CNS versus structures such as Y-shaped CNTs that do not originate from a CNS: For example, Y-shaped CNTs have catalyst particles at or near the regions (points) of branching, whereas such catalyst particles are not at or near the regions of branching that occur in CNSs, CNS fragments, broken CNTs, stretched CNS strands, or dispersed CNSs.

[0057] Additionally or alternatively, the number of layers observed in a region (point) of a branch in a CNS, CNS fragment, broken CNT, or dispersed CNS differs from one side of the branch (e.g., before the branch point) to the other side of this region (e.g., after or past the branch point). Such a change in the number of layers is also referred to herein as an "asymmetry" in the number of layers, and is not observed in regular Y-shaped CNTs (where the same number of layers is observed in both the region before and after the branch point).

[0058] Diagrams illustrating these features are provided in Figures 1A and 1B. An exemplary Y-shaped CNT 11, not derived from CNS, is shown in Figure 1A. The Y-shaped CNT 11 includes a catalyst particle 13 at or near the branch point 15. Regions 17 and 19 are located before and after the branch point 15, respectively. For a Y-shaped CNT, such as Y-shaped CNT 11, regions 17 and 19 are characterized by the same number of layers, i.e., two layers in the diagram.

[0059] In contrast, in a CNS (FIG. 1B), the CNT building block 111 branching at branch point 115 does not contain catalyst particles at or near this point, as seen in catalyst-deficient region 113. Furthermore, the number of layers present in region 117, located in front of (or on a first side of) branch point 115, is different from the number of layers in region 119, located after, behind, or on the other side relative to branch point 115. More specifically, the three-layer feature seen in region 117 is not seen throughout region 119, causing the asymmetry described above.

[0060] These features are highlighted in the TEM images of Figures 2A and 2B.

[0061] More specifically, the CNS branch in TEM region 40 of Figure 2A is devoid of catalyst particles. In the TEM of Figure 2B, first channel 50 and second channel 52 show the asymmetry in the number of layers that the branched CNS features, while arrow 54 indicates the area representing layer sharing.

[0062] One, more than one or all of these features may be found in the silicone-based compositions described herein.

[0063] Suitable techniques for preparing CNS are described, for example, in U.S. Patent Application Publication No. 2014 / 0093728, published April 3, 2014, U.S. Patent Nos. 8,784,937, 9,005,755, 9,107,292, and 9,447,259, the entire contents of which are incorporated herein by reference.

[0064] As described in these documents, CNS can be grown on a suitable substrate, for example on a catalytically treated fiber material. The product can be a fiber-containing CNS material. In some cases, the CNS is separated from the substrate to form flakes.

[0065] As seen in US2014 / 0093728, carbon nanostructures obtained as flake material (i.e., individual particles with finite dimensions) exist as three-dimensional microstructures due to the entanglement and cross-linking of their highly aligned carbon nanotubes. The aligned morphology reflects the formation of carbon nanotubes on a growth substrate under rapid carbon nanotube growth conditions (e.g., several microns per second, e.g., about 2 microns per second to about 10 microns per second), thereby inducing substantially perpendicular carbon nanotube growth from the growth substrate. Without being bound by any theory or mechanism, it is believed that the rapid rate of carbon nanotube growth on the growth substrate may contribute, at least in part, to the complex structural morphology of the carbon nanostructures. In addition, the bulk density of the CNSs can be tuned to some extent by adjusting the carbon nanostructure growth conditions, e.g., by varying the concentration of transition metal nanoparticle catalyst particles that are placed on the growth substrate to initiate carbon nanotube growth.

[0066] The flakes can be further processed, for example, by cutting or fluffing (operations that may include mechanical ball milling, grinding, blending, etc.), chemical treatment, or any combination thereof.

[0067] In some embodiments, the CNS used is "coated", also referred to herein as "sized" or "encapsulated". In a typical sizing process, a coating is applied to the CNTs forming the CNS. The sizing process can form a partial or complete coating non-covalently attached to the CNTs, and in some cases can act as a binder. Additionally or alternatively, a sizing agent may be applied to a preformed CNS in a post-coating (encapsulation) process. Using a sizing agent with binding properties, the CNS can be formed into larger structures, for example, pellets or pellets. In other embodiments, pellets or pellets are formed independently of the function of sizing.

[0068] The amount of coating may vary. For example, based on the total weight of the coated CNS material, the coating may be about 0.1 wt % to about 10 wt % (e.g., by weight, about 0.1% to about 0.5%; about 0.5% to about 1%; about 1% to about 1.5%; about 1.5% to about 2%; about 2% to about 2.5%; about 2.5% to about 3%; about 3% to about 3.5%; about 3.5% to about 4%; about 4% to about 4.5%; about 4.5% to about 5%; about 5% to about 5.5%; about 5.5% to about 6%; about 6% to about 6.5%; about 6.5% to about 7%; about 7% to about 7.5%; about 7.5% to about 8%; about 8% to about 8.5%; about 8.5% to about 9%; about 9% to about 9.5%; or about 9.5% to about 10%).

[0069] Various types of coatings can be selected. In many cases, sizing solutions commonly used to coat carbon or glass fibers could be utilized to coat the CNS. Specific examples of coating materials include, but are not limited to, fluorinated polymers such as poly(vinyldifluoroethylene) (PVDF), poly(vinyldifluoroethylene-co-hexafluoropropylene) (PVDF-HFP), poly(tetrafluoroethylene) (PTFE), polyimides, water-soluble binders such as poly(ethylene) oxide, polyvinyl-alcohol (PVA), cellulose, carboxymethylcellulose (CMC), starch, hydroxypropylcellulose, regenerated cellulose, polyvinylpyrrolidone (PVP), and copolymers and mixtures thereof. In many implementations, the CNS used is treated with polyurethane (PU), thermoplastic polyurethane (TPU), or polyethylene glycol (PEG).

[0070] In some cases, polymers such as epoxies, polyesters, vinyl esters, polyetherimides, polyetherketoneketones, polyphthalamides, polyetherketones, polyetheretherketones, polyimides, phenol-formaldehyde, bismaleimides, acrylonitrile-butadiene styrene (ABS), polycarbonates, polyethyleneimines, polyurethanes, polyvinyl chloride, polystyrenes, polyolefins, polypropylenes, polyethylenes, polytetrafluoroethylenes, elastomers such as polyisoprene, polybutadiene, butyl rubbers, nitrile rubbers, ethylene-vinyl acetate polymers, siloxane-based polymers and fluorosilicone polymers, including those described below, combinations thereof, or other polymers or polymeric blends, can also be used. Conductive polymers such as polyanilines, polypyrroles, and polythiophenes can also be used to improve electrical conductivity.

[0071] The coating material can be selected to contribute particular properties to the silicone-based composition or for its dispersibility, affinity and / or miscibility with the silicone-based composition or the precursor materials used to make it. Some implementations employ coating materials that can help stabilize the CNS dispersion in the matrix for the uncured silicone-based formulations and / or CNS masterbatches described herein.

[0072] In many implementations, the CNS are separated from their growth substrate and can be provided in the form of discrete particulate material (e.g., CNS flakes, pellets, etc.), or in compositions further comprising a coating or encapsulant, and / or in the form of pellets or pellets. Specific embodiments described herein use CNS material having a CNT purity of 97% or greater. Alternatively, the CNS material may include some amount of the growth substrate, in which case it may be desirable to include glass fibers in the composition.

[0073] In some embodiments, the CNS is provided in the form of flake material after it has been removed from the growth substrate on which the carbon nanostructures were initially formed. As used herein, the term "flake material" refers to individual particles having finite dimensions. For example, in FIG. 3, an exemplary depiction of the CNS material after separation of the CNS from the growth substrate is shown. The flake structure 100 may have a first dimension 110 of about 1 nm to about 35 μm thick (including any value therebetween and any portion thereof), particularly 1 nm to about 500 nm thick. The flake structure 100 may have a second dimension 120 of about 1 micron to about 750 microns high (including any value therebetween and any portion thereof). The flake structure 100 may have a third dimension 130 that can be about 1 micron to about 750 microns (including any value therebetween and any portion thereof). Two or all of the dimensions 110, 120, and 130 may be the same or different.

[0074] For example, in some embodiments, second dimension 120 and third dimension 130 can independently be on the order of about 1 micron to about 10 microns, about 10 microns to about 100 microns, about 100 microns to about 250 microns, about 250 microns to about 500 microns, or about 500 microns to about 750 microns.

[0075] The CNTs in a CNS are of variable length, ranging from about 10 nanometers (nm) to about 750 microns (μm) or more. Thus, CNTs may be of any length, ranging from 10 nm to 100 nm, 10 nm to 500 nm, 10 nm to 750 nm, 10 nm to 1 micron, 10 nm to 1.25 microns, 10 nm to 1.5 microns, 10 nm to 1.75 microns, 10 nm to 2 microns, 100 nm to 500 nm, 100 nm to 750 nm, 100 nm to 1 micron, 100 to 1.25 microns, 100 to 1.5 microns, 100 to 1.75 microns, 100 to 2 microns, 500 nm to 750 nm, 500 nm to 1 micron, 500 nm to 1 micron, 500 nm to 1 micron, 500 nm to 1.25 microns, 500 nm to 1 micron. 0.5 microns; 500 nm to 1.75 microns; 500 nm to 2 microns; 750 nm to 1 micron; 750 nm to 1.25 microns; 750 nm to 1.5 microns; 750 nm to 1.75 microns; 750 nm to 2 microns; 1 micron to 1.25 microns; 1.0 micron to 1.5 microns; 1 micron to 1.75 microns; 1 micron to 2 microns; 1.25 microns to 1.5 microns; 1.25 microns to 1.75 microns; 1 micron to 2 microns; 1.5 to 1.75 microns; 1.5 to 2 microns; or 1.75 to 2 microns. In some embodiments, at least one of the CNTs has a length of 2 microns or greater as determined by SEM.

[0076] In FIG. 3B, an SEM image of an exemplary carbon nanostructure obtained as flake material is shown. The carbon nanostructure shown in FIG. 3B exists as a three-dimensional microstructure due to the entanglement and cross-linking of its highly aligned carbon nanotubes. The aligned morphology reflects the formation of carbon nanotubes on the growth substrate under rapid carbon nanotube growth conditions (e.g., several microns per second, e.g., about 2 microns per second to about 10 microns per second), thereby inducing the growth of carbon nanotubes substantially perpendicularly from the growth substrate. Without being bound by any theory or mechanism, it is believed that the rapid rate of carbon nanotube growth on the growth substrate may contribute, at least in part, to the complex structural morphology of the carbon nanostructures. In addition, the bulk density of the carbon nanostructures can be tuned to some extent by adjusting the carbon nanostructure growth conditions, e.g., by varying the concentration of transition metal nanoparticle catalyst particles that are placed on the growth substrate to initiate carbon nanotube growth.

[0077] The flake structure may include a web-like network of carbon nanotubes in the form of carbon nanotube polymers (i.e., "carbon nanopolymers") having a molecular weight of about 15,000 g / mol to about 150,000 g / mol (including all values ​​and any portion therebetween). In some cases, the upper end of the molecular weight range may be about 200,000 g / mol, about 500,000 g / mol, or about 1,000,000 g / mol, or higher. Higher molecular weights are associated with dimensionally longer carbon nanostructures. The molecular weight may also depend on the predominant carbon nanotube diameter and the number of carbon nanotube layers present in the carbon nanostructure. The crosslink density of the carbon nanostructures is about 2 mol / cm. 3 ~about 80mol / cm 3Typically, the crosslink density depends on the growth density of the carbon nanostructures on the surface of the growth substrate, the growth conditions of the carbon nanostructures, etc. It is noted that a typical CNS structure containing many CNTs held in an open web-like arrangement eliminates or negates the effect of van der Waals forces. This structure can be more easily peeled off, which makes them unique and different from regular CNTs, many further steps of peeling or breaking them into branched structures.

[0078] When in web-like form, carbon nanostructures can have a relatively low bulk density. As-produced carbon nanostructures have a bulk density of about 0.003 g / cm 3 ~Approx. 0.015g / cm 3 Further consolidation and / or coating to produce carbon nanostructure flake material or similar morphology may reduce the bulk density to about 0.1 g / cm. 3 ~Approx. 0.15g / cm 3 In some embodiments, optional further modification of the carbon nanostructures can be performed to change the bulk density and / or other properties of the carbon nanostructures. In some embodiments, the bulk density of the carbon nanostructures can be further altered by forming a coating on the carbon nanotubes of the carbon nanostructures and / or by infiltrating the interior of the carbon nanostructures with various materials. Furthermore, coating the carbon nanotubes and / or infiltrating the interior of the carbon nanostructures can tailor the properties of the carbon nanostructures for use in various applications. Additionally, forming a coating on the carbon nanotubes can desirably facilitate manipulation of the carbon nanostructures. Further densification can increase the bulk density to about 1 g / cm. 3 and when combined with chemical modifications to the carbon nanostructures, the bulk density can be increased to about 1.2 g / cm 3 can be raised to an upper limit of

[0079] In addition to the flakes described above, the CNS material can be provided as granules, pellets, or other forms of loose particulate material having a typical particle size of about 1 mm to about 1 cm, e.g., about 0.5 mm to about 1 mm, about 1 mm to about 2 mm, about 2 mm to about 3 mm, about 3 mm to about 4 mm, about 4 mm to about 5 mm, about 5 mm to about 6 mm, about 6 mm to about 7 mm, about 7 mm to about 8 mm, about 8 mm to about 9 mm, or about 9 mm to about 10 mm.

[0080] Commercially, examples of suitable CNS materials are those available from Applied Nanostructured Solutions LLC (ANS), a wholly owned subsidiary of Cabot Corporation (Massachusetts, USA).

[0081] CNS as used herein can be identified and / or characterized by a variety of techniques. Electron microscopy, including techniques such as transmission electron microscopy (TEM) and scanning electron microscopy (SEM), can provide information about characteristics such as frequency of the specific number of layers present, branching, absence of catalyst particles, etc. See Figures 2A-2B.

[0082] Raman spectroscopy can show bands associated with impurities, e.g., the D band (1350 cm -1 The G band (around 1580 cm ) is associated with amorphous carbon; -1 The G' band (around 2700 cm) is associated with crystalline graphite or CNTs. -1 The CNS band is expected to occur at approximately twice the frequency of the D band. In some cases, thermogravimetric analysis (TGA) can distinguish between CNS and CNT structures.

[0083] In some embodiments, CNS is utilized together with one or more additional additives, such as carbon black, CNT, conductive particles, semiconductor particles, fumed silica, nickel-coated graphite, and other additives that are commonly used in silicone-based materials.Such additives can be combined with silicone-based composition before or after CNS is added.When CNS master batch is used, additional additives can be incorporated into master batch or added during let-down process.

[0084] Suitable carbon black particles are 20~1500m 2 / g, e.g. 20~75m 2 / g, 75-150m 2 / g, 100-300m 2 / g, 200-500m 2 / g, 500-1000m 2 / g or 1000~1500m 2 Alternatively, or in addition, suitable carbon blacks may have an oil absorption (OAN) of 30 to 350 mL / 100 g, e.g., 40 to 80 mL / 100 g, 60 to 150 mL / g, 100 to 200 mL / g, 150 to 250 mL / g, 200 to 300 mL / g or 250 to 350 mL / g.

[0085] Suitable commercially available carbon black particles include carbon blacks sold under the Regal®, Black Pearls®, Spheron®, Sterling® and Vulcan® trademarks available from Cabot Corporation, carbon blacks sold under the Raven®, Statex®, Furnex® and Neotex® trademarks and CD and HD series available from Birla Carbon (formerly available from Columbian Chemicals), carbon blacks sold under the Ketjenblack trademark available from Lion Specialty Chemicals Co., Ltd., carbon blacks sold under the Corax®, Durax®, Ecorax® and Purex® trademarks and CK series available from Orion Engineered Carbons (formerly Evonik and Degussa Industries), and carbon blacks available from Denka and Timcal. Alternatively, or in addition, the carbon black may be furnace carbon black, gas black, thermal black, acetylene black or lamp black. The carbon black may be recycled carbon black recovered from plastic or elastomeric materials.

[0086] Carbon black may be present in any concentration typically used in CNS-free silicone-based compositions, typical concentrations may be 0-30 wt%, although higher concentrations are also suitable.

[0087] In further embodiments, CNS can be used with conventional CNTs in their natural or pure form. These CNTs are not derived from CNSs, for example during processing. Suitable CNTs include multi-walled CNTs (MWSNTs), single-walled CNTs (SWCNTs), and modified CNTs. SWCNTs can improve electrical conductivity, and the synergy between CNSs and SWCNTs can improve the electrical conductivity of silicone-based compositions containing both materials beyond the electrical conductivity that either can provide to the silicone-based composition at similar loadings. SWCNTs can also provide thermal conductivity. Suitable modifications to CNTs to add hydroxy, carboxyl, amino, alkyl, halo, metal atoms, and other groups include oxidation, attachment of small molecules via diazonium chemistry, optionally followed by metallization, esterification, amidation, halogenation, addition of groups via cycloaddition, alkylation, metallization, and other modifications known to those skilled in the art. In many cases, CNTs are commercially available from ChengDu Organic Chemicals Co., Ltd., Sigma-Aldrich, Nanocs, Inc., Skyspring Nanomaterials, Inc., OCSiAl, Nanocyl SA, Nano-C, Shenzhen Sanshun Nano New Materials Co., Ltd., etc. Typical loadings of CNTs are 20 wt% or less, although either or both of MWCNTs and SWCNTs can be used in any amount desired by one of skill in the art.

[0088] Silica is another material that can be used with CNS to prepare the materials described herein. Fumed silica is commonly included in silicone-based resins to control rheology in uncured resins and improve mechanical properties in cured silicone-based compositions, such as fracture toughness, ductility, tensile strength, elasticity, and hardness. Surface treatment of fumed silica can prevent crepe hardening of cured silicone-based compositions and improve the compatibility of silica with uncured resins. Suitable surface treatments include those commonly used for fumed silica in silicone-based polymers, including hexamethyldisilazane, dimethyldichlorosilane, and siloxane-based polymers such as PDMS, monohydroxyl-terminated PDMS, and dihydroxyl-terminated PDMS. Fumed silica can be surface treated before being incorporated into uncured silicone-based resins, or a surface treatment can be included in the silicone-based resin formulation. Fumed silica may be incorporated into the silicone-based resin in proportions commonly used by those skilled in the art for silicone-based resins that do not contain CNS, for example, 0-50%, 2-40%, 5-30% or 10-25%. Furthermore, the loading of silica in the silicone-based resin is independent of the presence of CNS. Surprisingly, it has been found that the addition of non-conductive particles, such as fumed silica, to silicone-based compositions containing CNS does not affect their conductivity. The presence of fumed silica does not interfere with the formation of conductive pathways by the CNS and can stabilize their dispersion in various media. Without being bound by a particular theory, it is believed that silica can physically separate dispersed CNS-derived particles and / or hinder re-agglomeration by increasing the viscosity of the uncured silicone-based resin, thereby reducing the mobility of the CNS-derived particles. Alternatively or in addition, silica can act as a dispersion medium to promote de-agglomeration. Silica can be added to any surface area suitable for the silicone-based composition and its desired end use, for example, 50-450 m2. 2Commercially available fumed silicas suitable for use in silicone-based compositions containing CNS include, but are not limited to, CAB-O-SIL TS-530, TS-610, TS-622, M-5, TS-740 and TS-720 silicas available from Cabot Corporation, CLARUS 3160 silica, Ultrabond and Ultrabond 5780 silicas, Aerosil 200, R972, R805 and R208 silicas sold by Evonik Industries, and silicas sold under the name HDK by Wacker Corporation.

[0089] Some compositions may include conductive or semiconductive materials to improve conductivity. Exemplary conductive materials include metal particles, such as silver, gold, palladium, aluminum, copper, or other conductive metals or metal alloys known to those skilled in the art. It is understood by those skilled in the art that such metals do not need to be 100% pure and may have various levels of impurities as long as they retain their conductivity. Alternatively or in addition, the silicone-based composition may include semiconductive metal or metal alloy particles, such as silicon, doped silicon, germanium, doped germanium, gallium arsenide, and other semiconductive metals and alloys known to those skilled in the art. Alternatively or in addition, the silicone-based composition may include semiconductive oxides, such as copper oxide, barium titanate, strontium titanate, zinc oxide, and other semiconductive oxides known to those skilled in the art.

[0090] Any combination of conductive and semiconductive materials may also be used. Alternatively or additionally, composite particles containing two or more materials, with the conductive or semiconductive material disposed on the exterior of the particle, such as nickel-coated graphite, may also be used. The conductive or semiconductive particles may take any shape, such as cubes, flakes, granules, irregular shapes, rods, needles, powders, spheres, or a mixture of any two or more of these. The conductive or semiconductive particles may have a median particle size (by number) of 1 to 200 microns as measured by laser diffraction, SEM, optical microscope, TEM, or any other device that measures particle size on a number basis. The conductive or semiconductive particles may be characterized by a maximum particle size of 500 microns, alternatively 200 microns, alternatively 100 microns, alternatively 50 microns, alternatively 30 microns, and a minimum particle size of 0.0001 microns, alternatively 0.0005 microns, alternatively 0.001 microns. Such materials can be used in sufficient concentrations to form a permeating network of their own, or can be used to enhance conductivity through the network of dispersed CNS. For example, silver-containing particles are often used at loadings from 50 wt% up to 70, 80 or even 80 wt%.

[0091] Alternatively or in addition, it may contain other fillers commonly used with silicone-based materials, including but not limited to hydrophilic and surface-treated precipitated silicas, clays such as montmorillonite, silicon carbide and other metal carbides, metal nitrides such as AlN and BN, phosphates, sulfates and carbonates, halides and other metal salts, metal hydroxides such as calcium hydroxide and sodium hydroxide, glass fibers, glass particles, organic fibers (e.g., polymeric fibers), and carbonized organic fibers. For fumed silica, non-conductive fillers can be used at the same concentration as CNS was included in the composition. Other components that may be present include processing aids, curing agents, photoinitiators, catalysts, additional polymers, and other components commonly used in silicone-based compositions. Components such as those specified here or elsewhere can be added independently, at the appropriate stage of the preparation process, or as part of the silicone-based components used, as is known in the art.

[0092] Silicone-based materials that can benefit from the incorporation of the CNS provided herein include both siloxane polymers and silyl-terminated hybrid polymers that form linear and / or branched polysiloxane segments upon curing, as well as other chemistries, such as, but not limited to, acrylate, polyurethane, epoxy and polyether-based segments. The siloxane segments in the hybrid resins can be part of the polymer backbone, as in the siloxane polymers, or part of a branched or side chain. The hybrid polymers can have at least two end groups that contain silicon atoms, each independently having one, two or three alkoxysilane groups. The alkoxysilane groups can undergo hydrolysis upon curing to form siloxane bonds (e.g., -Si-O-Si-). Crosslinkers and catalysts can also be used to cure the hybrid polymers, similar to the chemistries described below for the siloxane polymers. Exemplary hybrid polymers include those disclosed in U.S. Patent Application Publication No. 2018 / 0298252 and U.S. Pat. No. 9,765,247 and commercially available polymers such as SPUR® polymers available from Momentive, MS Polymers available from Kaneka Corporation, and Geniosil® polymers from Wacker Chemie AG.

[0093] Polysiloxanes, or siloxane polymers, are well-recognized materials found in many applications. The basic polysiloxane structure corresponds to a polydialkylsiloxane, such as linear polydimethylsiloxane (PDMS), which is trimethylsilyloxy terminated: Me3SiO(SiMe2O) n SiMe3 where n=1, 2, 3, 4...etc. All or some of the methyl groups along the chain may be substituted by various organic groups, such as linear or branched alkyl, linear or branched haloalkyl, aryl, haloaryl, alkoxy, aralkyl and silacycloalkyl groups, as well as more reactive groups, such as alkenyl groups, such as vinyl, allyl, propenyl, butenyl, pentenyl, hexenyl, heptenyl, octenyl, octenyl, nonenyl and / or dodenyl groups. The linear and branched groups may have 1-100, such as 1-12, 1-20 or 1-30 carbons. The aromatic groups may have 6-100, such as 6-12, 6-20 or 6-30 carbons. Polar groups such as acrylate, methacrylate, amino, imino, hydroxy, epoxy, ester, alkoxy, isocyanate, phenol, polyurethane oligomer, polyamide oligomer, polyester oligomer, polyether oligomer, polyol, carboxypropyl and / or halo (e.g. fluoro) groups can be bonded to the silicon atom of the siloxane backbone in any combination.Alternatively or in addition, the siloxane polymer can be branched.Alternatively or in addition, the siloxane can have one or more ends terminated with any of these organic groups.

[0094] Silicone-based materials may be uncured or cured. Uncured silicone-based resins may refer to siloxane polymers or oligomers with alternating silicon and oxygen atom structures with various organic radicals bonded to silicon. Alternatively, or in addition, uncured silicone-based resins may be hybrid polymers. Uncured silicone-based resins initially provided in the form of liquid, rubber, or gel can be cured to form solids. Rubbers and other solid resins can increase their molecular weight through curing. Curing may include the formation of crosslinks or other linkages between polymer chains, either at the ends of the polymer chains or along the backbone of the polymer chains. For example, polymer chains or branches are formed or stretched.

[0095] A variety of techniques can be used to cure silicone-containing systems. As known to those skilled in the art, the particular cure package used may depend on the composition of the silicone-containing system. Polymers with siloxane backbones can be cured using peroxides, such as benzoyl peroxide, 2,4-dichlorobenzyl peroxide, t-butyl perbenzoate, dicumyl peroxide, alkyl hydroperoxides, dialkyl peroxides, and other peroxides known to those skilled in the art. Metal-containing catalysts, including, for example, tin, titanium, platinum, or rhodium, can be used. Alternatively, addition-based systems using hydrosilane materials and platinum-containing compounds can be used to cure polysiloxanes, particularly vinyl-containing polysiloxanes. Amine-based cure systems can also be used. Condensation systems can themselves cure at room temperature and ambient humidity. Condensation curable systems can be hydroxy- or alkoxy-functionalized. In one-part RTV systems, for example, the crosslinker exposed to ambient air moisture undergoes a hydrolysis process to form hydroxyl or silanol groups. Further condensation of the silanol with another hydrolyzable group is carried out until a fully cured system is obtained. Typical crosslinkers include alkoxy, acetoxy, ester, enoxy or oxime silanes. Often, methyltrimethoxysilane is used for alkoxy cured systems and methyltriacetoxysilane is used for acetoxy cured systems. Condensation catalysts can be added to fully cure the RTV system to achieve a tack-free surface. Alkoxy or oxime cured systems can use organotitanate catalysts (e.g., tetraalkoxy titanates or chelate titanates), while acetoxy cured systems can use tin catalysts, e.g., dibutyltin dilaurate (DBTDL). Typically, the hybrid polymer is cured in the presence of a catalyst in a hydrolysis and condensation step.

[0096] Free radically curable polymers having a siloxane backbone may be alkenyl-functionalized (e.g., vinyl) and / or alkynyl-functionalized. The cure or cure speed of such polymers can be improved by UV, blue light, peroxide, heat, or a combination thereof.

[0097] Typically, a two-part condensation system contains a crosslinker or hydrosilane material and a condensation or addition (platinum) catalyst in one part, and a polymer in the second part. For addition-based cure systems, an inhibitor can be used to improve shelf life. Cure occurs when the two parts are mixed. In many formulations, the CNS and any other fillers or pigments used are added to the polymer.

[0098] Radiation curing can also be used using electron beam (e-beam), blue LED, microwave or UV light, typically in the presence of a photoinitiator.

[0099] Silicone-based components may include high temperature vulcanizing (HTV) polysiloxanes, room temperature vulcanizing (RTV) polysiloxanes, high viscosity rubbers (HCR) or liquid polysiloxane rubbers (LSR, an abbreviation for liquid silicone rubber). Hybrid polymers or radiation curable polysiloxanes can also be used. Hybrid polymers containing silane functional groups can also be used, such as silyl-modified polyethers, silyl-modified polyurethanes, and other silane-terminated and silane-modified polymers. Curing of such polymers results in the formation of siloxane segments that link the polymer chains together.

[0100] Generally, polysiloxane rubbers are thermosetting elastomers having a backbone of alternating silicon and oxygen atoms and methyl or vinyl side groups. Polysiloxane rubbers are known for their stability and non-reactive properties, and polysiloxane rubbers can withstand extreme conditions, e.g., temperatures from -55 to 300°C (-67 to 572°F). oF), they can maintain their mechanical properties, remain stable and can be used. Many polysiloxane rubbers are relatively easy to manufacture and find use in a wide variety of products. The presence of methyl groups in polysiloxane rubbers can make these materials very hydrophobic.

[0101] The selection of specific silicone components may depend on various factors. For example, one consideration is related to the properties that are targeted in the final product. As is known in the art, silicone-based polymers are often developed to have properties that provide advantages to certain types of applications. For example, improved adhesion may be very important when developing silicone-based adhesives, so silicone-based polymers used to manufacture moldable parts preferably have good mechanical properties (e.g. good tensile strength and / or hardness), while their adhesive properties may be of less interest or irrelevant. Foam relies on increased porosity.

[0102] Many of the embodiments described herein employ silicone-based polymers suitable for preparing silicone-based compositions containing CNS that can be used to manufacture products (e.g., moldable articles or parts) with good mechanical stability (hardness, tensile strength) and good electrical conductivity.

[0103] In some instances, the silicone-based systems containing CNS include a vinyl polysiloxane component that can be prepared from liquid resins that are vinyl-functionalized polydimethylsiloxanes, e.g., vinyl-terminated polydimethylsiloxanes, that are typically used as intermediates in RTV materials.

[0104] The selection of base resin may take into account various factors. For example, in some cases, the base resin may not maintain the incorporation of CNS, which results in an improperly mixed composition. Therefore, one important factor to consider is whether the precursor to the silicone-based polymer forms a dispersion with CNS, especially with the desired concentration of CNS (e.g., 1, 5, 10 wt% or more of CNS based on the total weight of the silicone-based formulation).

[0105] A further factor relates to the viscosity that characterizes the uncured precursor to the silicone-based composition. As known in the art, the viscosity is often a function of shear force and can be characterized by a stress-strain curve. 1 cP to 10,000 cP, 10 cP to 50,000 cP, 100 cP to 100,000 cP, 25,000 cP to 200,000 cP, 100,000 cP to 500,000 cP, 200,000 to 700,000 cP, or 500,000 cP to 1000,000 cP.

[0106] A suitable test for dispersibility involves manually compressing a droplet-sized amount of the material between two microscope slides and observing the material under an optical microscope. A suitable dispersion is achieved when no more than one bundle having a width of more than 50 microns is observed in an image having an area of ​​about 1000 microns by 1400 microns or equivalent (i.e., the actual area of ​​the portion of the specimen analyzed in the image is equal to 1000 microns by 1400 microns). At higher loadings, the CNS loaded material may be opaque. To allow observation under the microscope, it may be necessary to let down the material, for example to a loading of about 0.1 wt%.

[0107] To prepare the systems described herein, the CNS can be combined with the silicone-based uncured precursor prior to curing. The process used to incorporate the CNS into the precursor material can be based on conventional compounding techniques and / or equipment. Dispersion of the CNS into the precursor material can be achieved using equipment such as, for example, a Brabender type mixer, a planetary mixer, a Waring blender, milling (e.g., a two-roll mill), ultrasonics, etc.

[0108] Mixing can be performed under suitable shear force, which may depend on the amount of CNS added and the resin properties.In many cases, a high speed mixer or an internal mixer, such as a Banbury or Brabender mixer, can be used.Any technique used by those skilled in the art to combine particulate fillers with uncured silicone-based resins can be used.

[0109] As one example, the final loading of CNS in the silicone-based resin is about 0.01 to about 15 wt%, for example, 0.01-0.05, 0.05-0.1, 0.1-0.5, 0.5-1, 1-3, 3-5, 5-7, 7-10, 1-10 wt%, 3-5 wt%, less than 10 wt%, less than 5 wt%, less than 1 wt%, less than 0.5 wt%, less than 0.1 wt%, less than 0.05 wt%, 0.01% to 1 wt%, or 10-15 wt%. Ranges within or overlapping these ranges can also be used.

[0110] A preferred implementation relies on masterbatch compounding techniques to prepare a masterbatch or concentrate in which the CNS is first dispersed in a precursor of the silicone-based resin. The use of a masterbatch to predisperse the CNS allows the final composition to be produced at lower shear, especially with liquid or low molecular weight resins. The masterbatch may have a CNS loading of 0.1-15%, for example 5-10%. The matrix of the masterbatch may be a precursor for the silicone-based resin, such as an uncured hybrid polymer or polymer with a siloxane backbone. The precursor may be in the form of a gel, rubber, liquid or solid. For two-component systems, the masterbatch can be formed in either the resin component or the second component, such as a crosslinker or curing agent. Alternatively or in addition, the masterbatch can be prepared in different additives, such as plasticizers, oils, reactive diluents, non-reactive diluents, etc. Suitable reactive diluents include, but are not limited to, lower viscosity (e.g. lower MW) of the silicone precursor in the masterbatch. Alternatively, or in addition, the masterbatch can be prepared in an aqueous or non-aqueous solvent. The masterbatch may include one or more additional components or additives to be incorporated into the final silicone-based composition, such as any of the additives or fillers described above, adsorption promoters such as silanes, and / or other additives known to those skilled in the art.

[0111] The masterbatch can be diluted (let down) into added CNS-free resin or diluted (let down) with a suitable plasticizer in a suitable ratio to form a let down composition. A suitable addition ratio can be from about 0.1 wt% to about 99 wt% (based on the addition ratio of the masterbatch to the CNS-free resin or plasticizer). Exemplary addition ratios are 0.1 to 20 wt% relative to the CNS-free resin, such as 0.5 to 15 wt%, 1 to 5 wt%, 5 to 10 wt%, 10 to 20 wt%, 20 to 30 wt%, 30 to 40 wt%, or 40 to 50 wt%. The CNS-free resin may include one or more additional components or additives that are incorporated into the final silicone-based composition. Alternatively, or in addition, such additional components or additives can be combined with the let down composition in a further processing step.

[0112] As one example, the CNS is premixed with a liquid polysiloxane resin and then processed in an internal mixer without the addition of a peroxide curing agent to prepare a masterbatch in which the CNS is well dispersed. Because the CNS is well dispersed, the masterbatch and the CNS-free resin in appropriate amounts, selected to provide the desired CNS content in the final curable composition, can then be mixed with other ingredients, including curing agents and / or further additives, without drying the silicone-based composition and without compromising the conductive properties of the CNS.

[0113] In another example, the CNS is dispersed in a high viscosity polysiloxane, such as a solid rubber, using an internal mixer without the addition of a peroxide curing agent to prepare a masterbatch in which the CNS is well dispersed. Because the CNS is well dispersed, the masterbatch and neat resin in an appropriate amount selected to result in the desired CNS content in the final curable composition can then be mixed with other ingredients, including curing agents and / or further additives, without drying the silicone-based composition and without compromising the conductive properties of the CNS.

[0114] The same method can be used to prepare two-component silicone-based systems. Typically, such systems include one component in which the resin is combined with a catalyst, and a second component in which the resin is combined with a crosslinker. In these implementations, the CNS masterbatch can be let down into either or both components.

[0115] In some embodiments, the amount of CNS material used to prepare the silicone-based systems described herein is above the percolation threshold, i.e., above the minimum concentration at which the insulating silicone-based material is converted to a conductive material. Without wishing to be held to a particular interpretation, it is believed that at the percolation threshold, there is sufficient CNS (or CNS-derived species, such as CNS fragments, broken CNTs, stretched CNS strands, or dispersed CNS) to form an electrical path through the sample via direct conduction of electricity, via tunneling, or both.

[0116] Experimentally, the percolation threshold can be determined by measuring the volume resistivity of cured samples prepared with various loadings of CNS to find the concentration or concentration range where the volume resistivity changes from a value that characterizes an insulator to a value suitable for EMI or ESD applications. By way of example, adding CNS at a loading of about 0.5 wt% to a silicone-based resin reduces the volume resistivity by 10 15 ohm·cm (for silicone-based resins without CNS additives) to 10 5 to ohm cm, for example about 10 4 Less than ohm cm or 10 3 This can result in a reduction in the volume resistivity to less than ohm·cm, for example 100 ohm·cm to 1000 ohm·cm.

[0117] Further applications employ a combination of CNS with one or more additional additives (eg, carbon black, CNT, silica, silver flakes, nickel coated graphite, etc.) at or just above the percolation threshold for that combination.

[0118] The processing steps carried out in the preparation of silicone-based systems containing CNS as described herein can produce CNS-derived species, such as CNS fragments, broken CNTs, stretched CNS strands and / or dispersed CNS, which are distributed in individual forms (e.g., homogeneously) through the precursors used to transport the CNS or throughout the system. For example, the shear forces associated with the compounding operations used to disperse the CNS in the silicone-based components can result in fragmentation of the initial structure and / or "peeling" of the carbon nanotubes from the original CNS.

[0119] Apart from their reduced size, CNS fragments (a term that also includes partially fragmented CNS) generally have properties of intact CNS and can be identified by electron microscopy and other techniques, as described above. Broken CNTs, elongated CNS strands, and dispersed CNS can be formed, for example, under an appropriate amount of applied shear, when the crosslinks between CNTs in the CNS are broken.

[0120] Exemplary CNS fragment sizes in silicone-based systems containing CNS can be about 0.5 to about 20 μm, such as about 0.5 to about 1 μm; about 1 to about 5 μm; about 5 to about 10 μm; about 10 to about 15 μm; or about 15 to about 20 μm. In some cases, reducing the size of the fragments too much, for example below 0.5 μm, can impair electrical properties associated with utilizing CNS. Carbon black particles and / or CNTs, if used, can range from about 0.1 microns to about 10 microns.

[0121] In many of the cured products, the CNS and / or CNS-derived species are uniformly distributed throughout the silicone-based matrix, as can be seen, for example, in the optical microscope image of FIG.

[0122] The curing process can be carried out according to the procedure typically used by those skilled in the art for the specific silicone-based system used, and the curing agent, catalyst, crosslinker, inhibitor, photoinitiator, etc. In certain embodiments, the cured silicone-based polymer can be subjected to a post-cure, in which the cured silicone is further heated in an oven set at a certain temperature for a certain time. Any combination of time and temperature for post-cure known to those skilled in the art is suitable, such as 177°C for 2 hours, 200°C for 2 hours, or 200°C for 4 hours.

[0123] Many aspects of the present invention relate to moldable compositions that are obtained by a curing step, for example, via an extrusion process or injection molding in a suitable molding process. The curable silicone-based composition can be molded, cured and shaped by any technique suitable for silicone-based polymers, known to those skilled in the art.

[0124] Once cured, the silicone-based systems containing the CNS described herein can have a tensile strength of greater than 0.5 MPa, e.g., from 0.5 MPa to 10 MPa, and / or an elongation at break of from 40% to 300%, e.g., from 45% to 120%, both measured according to ASTM D412.

[0125] Some aspects of the present invention relate to cured compositions that contain silicone-based components and CNS, CNS fragments, broken CNTs, stretched CNS strands and / or dispersed CNS, but are not foams. Indeed, in some instances, measures are taken to minimize the entrapment of air (or other gases) during manufacture. In general, it is desirable for the fractured surface of the sample to be free of air bubbles observable by the naked eye (e.g., about 0.1 mm or larger).

[0126] Lightweight materials are important for some applications, such as EMI or ESD shielding. In this regard, cured silicone-based systems containing CNS, CNS fragments, broken CNTs, stretched CNS strands and / or dispersed CNS have a light weight of less than 2 g / cm. 3 For example, 1.5 g / cm 3 Less than or equal to 1.2g / cm 3 It may have a density below 100 nm and preferably achieves a shielding efficiency of at least 35 dB, such as at least 40 dB, at 1.5 GHz for a 2 mm thick sample.

[0127] In some embodiments, the cured composition containing CNS, CNS fragments, broken CNTs, stretched CNS strands and / or dispersed CNS distributed in a silicone-based polymer can be characterized by its bulk (or bulk) resistivity (i.e., the resistance of a material to leakage current through its body, calculated by the ratio of the potential gradient with respect to the current in a material having the same density). The direct current resistance between the opposing faces of one cubic meter of material is equal to the volume resistivity in SI units (ohm·m or ohm·cm). A protocol for measuring volume resistivity is provided in ASTM-D257-07.

[0128] In some implementations, the volume resistivity (VR) of the cured materials, such as those described herein, characterizes them as electrical conductors, semiconductors, or insulators. In other implementations, cured systems containing silicone-based polymers and CNS, CNS fragments, broken CNTs, stretched CNS strands, and / or dispersed CNS have a volume resistivity of about 10 11 Less than ohm cm, e.g. 10 8 Less than 10 ohm cm 7 Less than 10 ohm cm 6 Less than ohm cm, approximately 10 4The cured silicone-based system may have a bulk resistivity of less than about 50 ohm·cm, less than 35 ohm·cm, less than 10 ohm·cm, less than 5 ohm·cm, less than 4 ohm·cm, less than 3 ohm·cm, less than 2 ohm·cm, or less than 1 ohm·cm. In certain examples, the cured silicone-based system including the CNS, CNS fragments, broken CNTs, stretched CNS strands, and / or dispersed CNS may have a bulk resistivity of less than about 50 ohm·cm, less than 35 ohm·cm, less than 10 ohm·cm, less than 5 ohm·cm, less than 4 ohm·cm, less than 3 ohm·cm, less than 2 ohm·cm, or less than 1 ohm·cm.

[0129] An exemplary plot of the volume resistivity of two vinyl siloxanes containing dispersed CNS and / or CNS-derived species prepared at various CNS loadings is shown in FIG.

[0130] As is known in the art, EMI shielding can occur through one or more of the following mechanisms: reflection, absorption, and multiple reflections. For EMI shielding applications, the cured silicone-based polymer-CNS systems described herein can be characterized by their shielding efficiency (SE), a parameter expressed in decibels (dB), and is given by the following formula: SE=10log(Pi / Po) It can be defined as the ratio of the input power (Pi) to the output power (Po) of the electromagnetic wave according to the above.

[0131] Suitable tests for evaluating the SE of cured silicone-based systems containing CNS, CNS fragments, broken CNTs, extended CNS strands and / or dispersed CNS are those specified in ASTM D4935.

[0132] It has been found that the presence of CNS, CNS fragments, broken nanotubes, extended CNS strands and / or dispersed CNS in a cured siloxane-based composition can exhibit improved EMI shielding compared to a cured silicone-based composition prepared without CNS (and without the addition of other conductive additives such as carbon black, CNT, silica or silver flakes). The improved EMI shielding is maintained even when the CNS is used in combination with fillers that do not contribute to EMI shielding, such as carbon black or fumed silica.

[0133] The compositions described herein can be used to prepare a variety of molded articles, elastomers, coatings, potting or gap-filling formulations, gasketing, films or membranes, aircraft, space or automotive parts, turbine or other engine components, boat or ship parts, turbine blades, medical devices, and the like.

[0134] The present invention is further illustrated by the following non-limiting examples. EXAMPLES

[0135] Conductivity Test Using a voltage / current meter (DC amplification, voltage detector), 6 Volume resistivity Rv or 10 ohms or less 6 Measures volume resistivity up to ohm·cm. The system performs resistance / resistivity testing using a measurement method consistent with ASTM D257-07.

[0136] The samples were cured in a mold having dimensions of 2.5 inches by 0.5 inches by 0.05 inches (63.5 mm by 12.7 mm by 1.18 mm) in a hot press at 20,000 pounds for 10 minutes at 180° C. The mold was then cooled for 5 minutes under a compression of 20 tons. The cooling press was then cooled for 50 minutes. o The temperature was maintained at or below 10° C. After curing, the samples were cooled in a cold press at 20,000 lbs and then the thickness (t) and width (W) of the samples were accurately measured.

[0137] Prior to conductivity testing, a layer of silver paint was applied to both ends of the molded bars and dried for 20 minutes at 23° C. The molded bars (samples) were clamped between two brass electrodes 43 mm apart (L).

[0138] A voltammeter was used to measure the electrical resistance (ohms) between the painted electrodes.

[0139] The following formula: ρ v =(R v xA) / L(ohm cm) (In the formula, A=Wxt(cm 2 ) was used to calculate the volume resistivity.

[0140] A Keithley 6517 Resistance Meter with a Keithley 8009 Resistivity Tester was used to measure the resistance of the 10 6 Volume resistivity Rv exceeding 10 ohms or 6 Volume resistivities in excess of ohm·cm were measured.

[0141] The polymer samples were cured in a circular die with a diameter of 2 mm and a thickness of 2 mm. The curing conditions were 10 6 Volume resistivity of 10 ohms or less 6 The conditions were the same as for samples with volume resistivity less than ohm·cm. Volume resistivity was measured according to the installation manual of the Keithley Model 8009 resistivity tester. The AC voltage was set as 5-10 V. The average results from eight tests per sample were recorded.

[0142] EMI Shielding Test The electromagnetic interference (EMI) shielding efficiency (SE) test standard ASTM D4395-1 was used to evaluate the cured elastomeric compounds over the frequency range of 30 MHz to 1.5 GHz. The construction of the cured elastomeric samples for EMI shielding testing was in accordance with ASTM D4935. EMI test samples were die-cut from 6 in. x 6 in. (15 cm x 15 cm) silicone-based plaques in a hot press at 180°C for 20 minutes and 20,000 pounds. The molds were then cooled under a compression of 20 tons for 5 minutes. The cooling press was then cooled for 50 minutes. o The specimens were maintained at a temperature of 10°C (50°F). Further EMI shielding efficiency tests were performed on the as-molded test plaques in the frequency range of 2.0 GHz to 18 GHz according to IEEE Standard 299. The thickness of the cured samples was 1-2 mm. Precise dimensions were measured as a factor in the efficiency measurements. The test fixture included a signal generator (Marconi, Model 10874-83-1), a spectrum analyzer (Hewlett Packard, Model 8564E), an ASTM shielding efficiency tester (Electro Metrics, EM-2107A), and Quantum Change Tile software (Version 3.4.k.6) installed on a computer. Shielding efficiency (SE) was measured in decibels (dB).

[0143] The measurement and test equipment utilized in performing these tests was calibrated in accordance with ANSI / NCSL Z540-3-2006 by Keystone Compliance, LLC, using reference or interim standards, and the calibration is certified by the National Institute of Standards and Technology (NIST).

[0144] Mechanical Property Testing The samples were cured in a hot press at 20,000 pounds for 10 minutes at 180° C. to form samples of 2 mm thickness. After curing, the samples were cooled in a cold press at 20,000 pounds. A Die-C standard die was used to punch out dumbbell-shaped samples. Tensile properties were measured according to ASTM D412, with a strain rate of 500 mm / min.

[0145] Dispersibility Test A portion of the uncured sample was collected, weighed, and let down with undiluted uncured silicone-based resin having approximately the same viscosity as the resin used to prepare the sample to a total CNS loading of 0.1%. A drop-sized amount of material was collected from the let down and compressed by hand between two microscope slides. Images were taken at 200x and had dimensions of approximately 1000 microns by 1400 microns. When necessary, the width of the carbon nanostructure fragments was measured by hand or using image analysis software. Dispersion was acceptable when no more than one fragment of carbon nanostructures with a bundle width greater than 50 microns was observed.

[0146] Examples 1-9 Curable silicone-based compounds were prepared according to the following mixing procedure: Vinyl-functionalized polydimethylsiloxane (VGM-021 Dimethylmethylvinylsiloxane Gum, 0.2-0.3% Vinylmethylsiloxane, Gelest) was mixed with the fillers listed in Table 1 below in a 680 cc Brabender mixer with roller blades (60° C., 60 rpm, 0.7 fill factor) for 8 minutes to form a dispersion in the first mixing pass and then cooled to room temperature. Carbon black was VULCAN SC72R from Cabot Corporation. CAB-O-SIL TS-530 fumed silica from Cabot Corporation is also available. Nickel-coated graphite (NiGr; E-Fill 2701) was obtained from Oerlikon Metco. FS8 grade silver flake was obtained from Johnson Matthey. PEG-coated CNS was obtained from Cabot Corporation. In the second pass, a corresponding amount of peroxide catalyst (Luperox® 101XL45) was added to the compound from the first pass and mixed for an additional 2 minutes under the same conditions. The resulting material was cooled to room temperature and processed on a two-roll mill for 2 minutes to produce a curable sheet. Table 1: Curable vinyl siloxane compositions of Examples 1-9 [Table 1] Table 2: Properties of the cured vinyl siloxane for Examples 1-9 [Table 2] *VR-deposition resistivity a-ASTM D4935 method b-IEEE 299 method

[0147] Examples 10-15 The curable silicone-based compounds in Examples 10-15 were prepared by combining the masterbatch (MB) with high viscosity vinyl siloxane rubber. A 5% CNS masterbatch (MB) was prepared by dispersing CNS particles directly into VGM-021 polysiloxane vinyl rubber as described in Table 3 using a 680 cc Brabender mixer (60°C, 0.7 loading, 60 rpm, 8 minutes) and cooled to room temperature. The 5% CNS MB mixture was further processed on a two-roll mill for an additional 2 minutes to form a masterbatch sheet. Samples were cut from the masterbatch sheet and weighed to prepare let-down samples with final CNS loadings of 0.05% to 1.0%. For Examples 11-15, the 5% CNS masterbatch sample was mixed with additional vinyl rubber as described in Table 4 in a Brabender mixer (60°C, 0.7 fill rate, 60 rpm, 8 minutes) and then Luperox® 101XL45 peroxide catalyst was added to the mixture. The final composition was mixed in a Brabender mixer (60°C, 0.7 fill rate, 60 rpm) for 2 minutes and transferred to a two-roll mill and processed for 2 minutes to produce a curable silicone-based sheet. Example 11, prepared by the masterbatch route, showed a lower resistivity than Example 2, prepared by directly mixing CNS into the polysiloxane rubber, indicating that the masterbatch route can result in a superior product. The dispersion of the high level of CNS in Example 11 is shown in Figure 4. Table 3: CNS masterbatch in vinyl rubber (5%) [Table 3] Table 4: CNS Letdown Compounds in Vinyl Rubber, Examples 11-15 [Table 4] Table 5: Properties of the cured HTV elastomers of Examples 11-15 [Table 5]

[0148] A curable silicone-based compound was prepared using liquid siloxane resin as follows: Vinyl-functionalized polydimethylsiloxane (DMS-V41 vinylmethylsiloxane, molecular weight 62700 g / mol, Gelest, Inc.) was premixed with CNS pellets in a Flacktek Max 200 Long cup (Part number 501-220LT, Flacktek, Inc.) according to the formula in Table 6 and mixed for 15 seconds at 1500 RPM with a DAC 600 Speedmixer® (Flacktek, Inc.). The CNS-siloxane premix paste was mixed in a Brabender mixer for 8 minutes with a first mixing pass (60° C., 60 rpm, 0.7 fill factor) to disperse the CNS in the resin and then cooled to room temperature. In the second mixing pass, a corresponding amount of Luperox® 101XL45 peroxide catalyst was added to the Brabender mixer and the formulation was mixed for 2 minutes under the same conditions as the first pass, then the material was transferred to a two-roll mill and processed for 2 minutes to make a curable sheet. The final curable polysiloxane composition is listed in Table 6. Table 6: CNS (5%) dispersed in liquid siloxane cured by peroxide [Table 6]

[0149] Examples 17-21 The curable silicone-based compounds of Examples 18-21 were prepared by combining the masterbatch (MB) with a liquid siloxane (DMS-V41 liquid siloxane resin, Gelest, Inc.). A 5% CNS masterbatch (Example 17) was prepared using the formulation in Table 7 and the method of Example 16. Samples were cut from the masterbatch sheet and weighed to prepare letdown samples with final CNS loadings of 0.05% to 1.0%. To prepare the letdowns of Examples 18-21, the cut and weighed 5% CNS masterbatch samples were mixed with additional vinyl rubber in a Flacktek DAC 600 planetary speed mixer (formulation in Table 8; total batch size 165 g). Mixing was done in multiple runs as follows: 2 x 30 sec runs at 1500 rpm, 5 x 60 sec runs at 1500 rpm, 2 x 30 sec runs at 2000 rpm, and 3 x 60 sec runs at 2000 rpm. Between runs, the samples were cooled to prevent heat build-up that could accelerate cure and reduce viscosity. After the masterbatch was well dispersed in the letdown, Luperox® 101XL45 peroxide catalyst was added as described in Table 8, and the final composition was further mixed in a planetary mixer at 1500 rpm for two 1 minute intervals. The temperature was monitored during each mixing run and kept below 80°C. Between the two mixing runs, the samples were cooled to room temperature to avoid overheating. During the second mixing run, the mixing speed was reduced to prevent new air bubbles from being generated, and a vacuum was used to remove remaining air bubbles from the sample. After mixing, the letdown mixture was transferred to a two-roll mill and processed for 2 minutes to produce a curable sheet. The volume resistivity and shielding efficiency for the samples are recorded in Table 9. Table 7: Preparation of CNS masterbatch (5%) in vinyl liquid resin [Table 7] Table 8: CNS Letdown Formulations in Liquid Siloxane Resins, Examples 18-21 [Table 8] Table 9: Properties of the cured polysiloxanes of Examples 16-21 [Table 9]

[0150] Examples 22-23 Examples 22-23 were prepared with platinum-cure (Pt-cure) liquid siloxane rubber (LSR) according to the formulations shown in Table 10. Either neat LSR resin (DMS-V41 siloxane resin, Gelest, Inc.) or the masterbatch prepared according to Example 17 was combined with CAB-O-SIL TS-530 fumed silica (Cabot Corporation).

[0151] For blank (CNS-free) Pt-curable silicone-based compounds, a Flacktek DAC600 planetary speed mixer with a DAC 200 mixer cup was used. TS-539 fumed silica was combined with DMS-V41 resin at 2000 rpm for 5 minutes. The silica-silicone-based dispersion was cooled to room temperature. HMS-301 crosslinker and SIT 7900.2 inhibitor (both from Gelest, Inc.) were added to the mixture and dispersed at 2000 rpm for 1 minute. Finally, platinum catalyst (Platinum (0)-1,3-divinyl-1,1,3,3-tetramethyldisiloxane complex solution, CAS#68478-92-2) was added and the final formulation was mixed at 1000 rpm for 30 seconds. The resulting curable silicone-based samples were cured in the compression mold described above to produce samples for mechanical testing and resistivity measurements. The volume resistivity and shielding efficiency are recorded in Table 11. Table 10: Pt-curable LSR formulations [Table 10] Table 11: Platinum curable LSR formulations [Table 11]

[0152] A platinum curable LSR compound containing CNS was prepared using a masterbatch process. The 5% CNS-polysiloxane masterbatch of Example 17 was cut and weighed to prepare the letdown sample of Example 23. The amounts of masterbatch, additional polysiloxane, and TS-530 silica shown in Table 10 were combined in a 680cc Brabender mixer with roller blades (60°C, 60 rpm, 0.7 fill rate) for 8 minutes to form a dispersion in the first mixing pass, then cooled to room temperature. In the second pass, the corresponding amounts of crosslinker and inhibitor were added to the compound from the first pass and mixed in the Brabender mixer (room temperature, 60 rpm, 0.7 fill rate) for an additional 4 minutes. The material was cooled to room temperature. In the final mixing step in the Brabender, the corresponding amount of catalyst was added into the mixer and mixed for 2 minutes (room temperature, 60 rpm, 0.7 fill rate). The curable siloxane mixture was mixed in a two-roll mill for 2 minutes to produce a curable silicone sheet. The resulting curable polysiloxane sample was cured in the compression mold described above to produce samples for mechanical and resistivity testing. The volume resistivity and shielding efficiency are recorded in Table 11.

[0153] FIG. 5 shows the percolation curves for silicone-based samples containing CNS from Examples 11-16 and 18-21. The data show that electrical conductivity is not dramatically affected by either the choice of catalyst or the addition of silica. The resistivity decreases dramatically even with the addition of small amounts of CNS, and continues to decrease even after percolation is achieved. FIG. 6 shows the change in shielding efficiency versus frequency for various experimental examples (open) and comparative examples (filled). The results show that CNS provides excellent shielding capabilities, and that this shielding is more pronounced at higher frequencies.

[0154] Example 24 Curable hybrid polymer formulations are prepared by combining the masterbatch with additional silyl-terminated prepolymers. As in Example 16, a 5% CNS masterbatch is prepared by premixing CNS particles directly into KANEKA MS POLYMER® S303H silyl-terminated polyether resin, then dispersed under a nitrogen blanket using a 680cc Brabender mixer equipped with roller blades (60°C, 0.7 loading rate, 60 rpm, 8 minutes). The masterbatch is then cooled to room temperature and samples are cut and weighed to prepare letdown samples with final CNS loadings of 0.05% to 5.0%. Samples are weighed and sampled in a humidity-controlled dry box (e.g., less than 3% relative humidity). For a final CNS loading of 1%, the masterbatch sample is combined with additional S303H polymer (57% total polymer), CAB-O-SIL TS-530 hydrophobic silica (10 wt%, Cabot Corporation) and polypropylene glycol plasticizer (PPG3000, 31.4 wt%, Sigma-Aldrich). The fumed silica is first dried at 105°C for 2 hours to remove moisture. The components are blended in a Flacktek DAC 600 planetary speed mixer at 2000 rpm for a total of 10 minutes in 1 minute intervals, during which the sample is cooled to prevent exotherms that may promote curing or lower viscosity. Dibutyltin catalyst (0.6 wt%) is added to the mixture and then the complete mixture (total mass = 165 g) is further mixed at 1500 rpm for an additional 2 minutes. The moisture-curable compound is filled into cartridges or molded at room temperature. The samples can be cured with moisture at room temperature (23° C., 50% relative humidity, 7 days) to provide a material with high conductivity and desirable mechanical properties.

[0155] Example 25 A curable two-part ("A" and "B") silicone formulation is prepared by combining the masterbatch with additional vinyl-functionalized silicone with another part containing a crosslinker silicone. A 5% CNS masterbatch is prepared by premixing the CNS particles directly into the DMS-V41 silicone as described in Example 16, then dispersed under a nitrogen blanket using a 680 cc Brabender mixer equipped with roller blades (60°C, 0.7 charge rate, 60 rpm, 8 minutes). The masterbatch is then cooled to room temperature and samples are cut and weighed to prepare letdown samples with final CNS loadings of 0.05% to 5.0% (based on the total mass of silicone in the final A+B formulation) and 0.19% platinum(0)-1,3-divinyl-1,1,3,3-tetramethyldisiloxane complex solution. The letdown was prepared by blending the components in a Flacktek DAC 600 planetary speed mixer at 2000 rpm for a total of 10 minutes in 1 minute intervals, with the samples cooled between intervals to prevent exotherms that could reduce mixing efficiency or decompose the components.

[0156] When the "A" and "B" components are combined in a 1:1 ratio, the "B" component contains a mixture of 5% CNS masterbatch, polymethylhydrosiloxane (trimethylsilyl terminated, HMS-992 siloxane, Gelest), and enough undiluted DMS-V41 silicone to achieve the desired CNS loading (0.05-5.0%) and a DMS-V41 / HMS-992 ratio of 10:1 (by weight). As with the "A" component, the components are mixed in a Flacktek DAC-600 planetary speed mixer. For the "B" part, care must be taken to ensure that moisture is removed during each mixing step, as moisture may initiate crosslinking reactions with the hydrosilane, reducing its activity. The "A" and "B" components are mixed by hand in a 1:1 ratio and cured at room temperature, typically at indoor conditions (23°C, 10-50% relative humidity), to provide a material with high conductivity and desirable mechanical properties.

[0157] Although the present invention has been particularly shown and described with reference to preferred embodiments thereof, it will be understood by those skilled in the art that various changes in form and details can be made therein without departing from the scope of the invention encompassed by the appended claims. The present invention can be embodied in the following manner. (Appendix 1) a cured polymer comprising a cured siloxane polymer or a cured silyl-terminated hybrid polymer; at least one CNS-derived material dispersed in the cured polymer and selected from the group consisting of carbon nanostructures, fragments of carbon nanostructures, broken carbon nanotubes, elongated CNS strands, dispersed CNS, and any combination thereof; Including, the carbon nanostructures or fragments of carbon nanostructures comprise a plurality of multi-walled carbon nanotubes that are branched, interdigitated, entangled, and / or cross-linked in a polymeric structure by sharing a common layer; the broken carbon nanotubes originate from the carbon nanostructure, are branched, and share a common layer with each other; the elongated CNS strand comprises CNTs derived from the carbon nanostructure and arranged linearly relative to one another; and A cured polymer composite, wherein the dispersed CNTs comprise exfoliated and broken CNTs that do not share a common layer with one another. (Appendix 2) 2. The cured polymer composite of claim 1, wherein the composition comprises 0.01 to 15 wt % of a CNS-derived material. (Appendix 3) The siloxane polymer is Me 3 SiO(SiMe 2 O) n Me, where n is 2 or more and at least one methyl group is selected from R' and -(O-SiR'R'') n -, wherein R' and R'' are independently linear or branched alkyl, linear or branched haloalkyl, aryl, haloaryl, alkoxy, aralkyl, silacycloalkyl, alkenyl, acrylate, methacrylate, amino, imino, hydroxy, epoxy, ester, alkoxy, isocyanate, phenol, polyurethane oligomer, polyamide oligomer, polyester oligomer, polyether oligomer, polyol, carboxypropyl, or halo. (Appendix 4) 4. The cured polymer composite of any one of claims 1 to 3, wherein the silyl-terminated hybrid polymer comprises an alkoxysilane-terminated polyacrylate, polyurethane, epoxy, or polyether. (Appendix 5) Tensile strength of more than 0.5 MPa or 0.5 MPa to 10 MPa, elongation at break of 40% to 300%, and 5 5. The cured polymer composite of any one of claims 1 to 4, having one or more of the following volume resistivities of less than ohm·cm. (Appendix 6) 6. The cured polymer composite of any one of claims 1 to 5, wherein the cured polymer is crosslinked. (Appendix 7) 7. The cured polymer composite of any one of claims 1-6, wherein the cured polymer composition has a shielding efficiency of at least 35 dB at 1.5 GHz for a 2 mm thick sample. (Appendix 8) 8. The cured polymer composite of any one of claims 1 to 7, wherein the carbon nanostructures are coated with or in a mixture with a binder. (Appendix 9) 9. The cured polymer composite of any one of claims 1-8, further comprising at least one additive selected from the group consisting of fumed silica, precipitated silica, semiconductor oxides, nickel coated graphite, metals, metal alloys, carbon fibers, CNTs, graphene, graphite, carbon black, clays, metal carbides, metal nitrides, metal phosphates, metal sulfates, metal carbonates, metal halides, metal hydroxides, glass, and organic fibers. (Appendix 10) 10. An article for electromagnetic interference shielding, comprising the cured polymer composite of any one of claims 1 to 9. (Appendix 11) 1. A method for preparing a polymer composite for electromagnetic interference shielding, comprising: combining the carbon nanostructures with an uncured polymer comprising a curable and formable polymer selected from polysiloxanes or silyl-terminated hybrid polymers to form a mixture and dispersing the carbon nanostructures in the uncured polymer to produce a CNS-derived material selected from broken carbon nanotubes, extended CNS strands, dispersed CNS, and any combination thereof; Including, the carbon nanostructures comprise a plurality of multi-walled carbon nanotubes that are branched, interdigitated, entangled, and / or cross-linked in a polymeric structure by sharing a common wall; the broken carbon nanotubes originate from the carbon nanostructure, are branched, and share a common layer with each other; the elongated CNS strand comprises CNTs derived from the carbon nanostructure and arranged linearly relative to one another; and The method, wherein the dispersed CNS comprises exfoliated and broken CNTs that do not share a common layer with one another. (Appendix 12) 12. The method of claim 11, wherein the combining step comprises dispersing the carbon nanostructures until observation of a microscopic image of the mixture having an area of ​​1000 microns by 1400 microns or equivalent reveals no more than one fragment of carbon nanostructure having a bundle width greater than 50 microns, and the mixture is prepared for observation by diluting the mixture with additional uncured polymer to a loading of about 0.1% CNS-derived material and compressing a drop-sized aliquot between two glass microscope slides. (Appendix 13) The polysiloxane is Me 3 SiO(SiMe 2 O) n Me, where n is 2 or more and at least one methyl group is selected from R' and -(O-SiR'R'') n -, and R' and R'' are independently linear or branched alkyl, linear or branched haloalkyl, aryl, haloaryl, alkoxy, aralkyl, silacycloalkyl, alkenyl, acrylate, methacrylate, amino, imino, hydroxy, epoxy, ester, alkoxy, isocyanate, phenol, polyurethane oligomer, polyamide oligomer, polyester oligomer, polyether oligomer, polyol, carboxypropyl, or halo. (Appendix 14) 14. The method of any one of claims 11 to 13, wherein the silyl-terminated hybrid polymer comprises an alkoxysilane-terminated polyacrylate, polyurethane, epoxy, or polyether. (Appendix 15) 15. The method of any one of claims 11 to 14, wherein the combining step comprises mixing the carbon nanostructures with a medium selected from an oil, a reactive diluent, a non-reactive diluent, an aqueous solvent, a non-aqueous solvent, or a plasticizer to form a masterbatch, and mixing the masterbatch with the uncured polymer to form the mixture. (Appendix 16) 16. The method of any one of claims 11 to 15, further comprising combining the mixture with a let-down polymer selected from a polysiloxane or a silyl-terminated hybrid polymer. (Appendix 17) 17. The method of any one of claims 11 to 16, wherein the polysiloxane is a component of a one-component curable silicone-based polymer system or a two-component curable silicone-based polymer system. (Appendix 18) 18. The method of any one of appendixes 11 to 17, wherein the carbon nanostructures are provided in an amount of 0.01 to 15 wt %. (Appendix 19) 19. The method of any one of claims 11 to 18, wherein the carbon nanostructures are coated with or in a mixture with a binder. (Appendix 20) 20. The method of claim 19, wherein the weight of the binder relative to the weight of the coated carbon nanostructure is about 0.1% to about 10%. (Appendix 21) 21. The method of any one of claims 11 to 20, further comprising adding to the mixture at least one additive selected from the group consisting of fumed silica, precipitated silica, semiconductor oxides, nickel coated graphite, metals, metal alloys, carbon fibers, CNTs, graphene, graphite, carbon black, clays, metal carbides, metal nitrides, metal phosphates, metal sulfates, metal carbonates, metal halides, metal hydroxides, glass, and organic fibers. (Appendix 22) 22. The method of any one of claims 1 to 21, further comprising curing or allowing the mixture to cure. (Appendix 23) 23. The method of any one of claims 11 to 22, wherein the mixture is cured in the presence of one or more of a catalyst, heat, a crosslinking agent, moisture, microwave radiation, blue LED, ultraviolet light, electron beam radiation, and a photoinitiator. (Appendix 24) A polymer conjugate prepared by the method according to any one of claims 11 to 23. (Appendix 25) 25. The polymer composite of claim 24, wherein observation of an optical microscope image of the polymer composite having an area of ​​1000 microns by 1400 microns or equivalent reveals no more than one fragment of carbon nanostructures having a bundle width greater than 50 microns, and the polymer composite is prepared for observation by diluting the polymer composite with additional uncured polymer to a loading of 0.1% CNS and compressing a drop-sized aliquot between two glass microscope slides. (Appendix 26) the uncured polymer comprising a curable, formable polymer selected from a polysiloxane or a silyl-terminated hybrid polymer, and a CNS-derived material selected from disrupted carbon nanotubes, oriented CNS strands, dispersed CNS, and any combination thereof; the carbon nanostructures comprise a plurality of multi-walled carbon nanotubes that are branched, interdigitated, entangled, and / or cross-linked in a polymeric structure by sharing a common wall; the broken carbon nanotubes originate from the carbon nanostructure, are branched, and share a common layer with each other; the elongated CNS strand comprises CNTs derived from the carbon nanostructure and arranged linearly relative to one another; and A curable polymer composition, wherein the dispersed CNS comprises exfoliated and disrupted CNTs that do not share a common layer with one another. (Appendix 27) 27. The curable polymer composition of claim 26, wherein when the curable polymer composition is prepared for observation under an optical microscope by diluting the composition with additional uncured polymer to a loading of about 0.1% CNS-derived material and compressing a drop-sized amount between two glass microscope slides to create a sample, a microscope image showing an area of ​​the sample of 1000 microns by 1400 microns or equivalent in area contains no more than one fragment of carbon nanostructure having a bundle width of more than 50 microns. (Appendix 28) The polysiloxane is Me 3 SiO(SiMe 2 O) n Me, where n is 2 or more and at least one methyl group is selected from R' and -(O-SiR'R'') n -, and R' and R'' are independently linear or branched alkyl, linear or branched haloalkyl, aryl, haloaryl, alkoxy, aralkyl, silacycloalkyl, alkenyl, acrylate, methacrylate, amino, imino, hydroxy, epoxy, ester, alkoxy, isocyanate, phenol, polyurethane oligomer, polyamide oligomer, polyester oligomer, polyether oligomer, polyol, carboxypropyl, or halo. (Appendix 29) 29. The curable polymer composition of any one of claims 26 to 28, wherein the silyl terminated hybrid polymer comprises an alkoxysilane terminated polyacrylate, polyurethane, epoxy, or polyether. (Appendix 30) 30. The curable polymer composition of any one of claims 26 to 29, further comprising an oil, a reactive diluent, a non-reactive diluent, an aqueous solvent, a non-aqueous solvent, or a plasticizer. (Appendix 31) 31. The curable polymer composition of any one of claims 26 to 30, wherein the polysiloxane is a component of a one-component curable silicone-based polymer system or a two-component curable silicone-based polymer system. (Appendix 32) 32. The curable polymer composition of any one of claims 26 to 31, wherein the CNS-derived material is present in an amount of 0.01 to 15 wt %. (Appendix 33) 33. The curable polymer composition of any one of claims 26 to 32, wherein the CNS-derived material further comprises a binder. (Appendix 34) 34. The curable polymer composition of claim 33, wherein the weight of the binder relative to the weight of the CNS-derived material is about 0.1% to about 10%. (Appendix 35) 35. The curable polymer composition of any one of claims 26 to 34, further comprising at least one additive selected from the group consisting of fumed silica, precipitated silica, semiconductor oxides, nickel coated graphite, metals, metal alloys, carbon fibers, CNTs, graphene, graphite, carbon black, clays, metal carbides, metal nitrides, metal phosphates, metal sulfates, metal carbonates, metal halides, metal hydroxides, glass, and organic fibers.

Claims

1. 1. A method for preparing a polymer composite for electromagnetic interference shielding, comprising: combining the carbon nanostructures with an uncured polymer comprising a curable and formable polymer selected from polysiloxanes or silyl-terminated hybrid polymers to form a mixture and dispersing the carbon nanostructures in the uncured polymer to produce a CNS-derived material selected from broken carbon nanotubes, expanded CNS strands, dispersed CNS, and any combination thereof; Including, the carbon nanostructures comprise a plurality of multi-walled carbon nanotubes that are branched, interdigitated, entangled, and / or cross-linked in a polymeric structure by sharing a common wall; the broken carbon nanotubes originate from the carbon nanostructure, are branched, and share a common layer with each other; the drawn CNT strand comprises CNTs derived from the carbon nanostructure and arranged linearly relative to one another; and the dispersed CNTs comprise exfoliated and broken CNTs that do not share a common layer with one another; The method, wherein the combining step includes mixing the carbon nanostructures with a vehicle selected from an oil, a reactive diluent, a non-reactive diluent, or a plasticizer to form a masterbatch, and mixing the masterbatch with the uncured polymer to form the mixture.

2. 2. The method of claim 1, wherein the combining step comprises dispersing the carbon nanostructures until observation of a microscopic image of the mixture having an area of ​​1000 microns by 1400 microns or equivalent reveals no more than one fragment of carbon nanostructure having a bundle width greater than 50 microns, and the mixture is prepared for observation by diluting the mixture with additional uncured polymer to a loading of 0.1% CNS-derived material and compressing a drop-sized amount between two glass microscope slides.

3. 10. The method of claim 1, further comprising combining the mixture with a let-down polymer selected from a polysiloxane or a silyl-terminated hybrid polymer.

4. 10. The method of claim 1, further comprising adding to the mixture at least one additive selected from the group consisting of fumed silica, precipitated silica, semiconductor oxides, nickel coated graphite, metals, metal alloys, carbon fibers, CNTs, graphene, graphite, carbon black, clays, metal carbides, metal nitrides, metal phosphates, metal sulfates, metal carbonates, metal halides, metal hydroxides, glass, and organic fibers.

5. The method of claim 1 further comprising curing or allowing the mixture to cure.

6. 6. The method of claim 5, wherein the mixture is cured in the presence of one or more of a catalyst, heat, a crosslinking agent, moisture, microwave radiation, a blue LED, ultraviolet light, electron beam radiation, and a photoinitiator.

Citation Information

Patent Citations

  • Composite materials formed by shear mixing of carbon nanostructures and related methods

    JP2015533187A

  • Microwave transmission assembly

    JP2015533254A

  • Silicone rubber composition and vulcanized object

    WO2016136275A1