Coatings for improved surface finish
Coatings of aluminum oxide and silicon dioxide on CMC components address production and machining issues in gas turbines, ensuring a stable, leak-proof seal and efficient operation.
Patent Information
- Application Number
- JP2019182740
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2018-12-14
- Filing Date
- 2019-10-03
- Publication Date
- 2024-12-09
- Estimated Expiration
- 2039-10-03
AI Technical Summary
The transition to ceramic matrix composites (CMCs) in gas turbine engines is hindered by higher production costs, longer manufacturing cycles, limited geometries, porosity leading to cooling flow leaks, and inconsistent machining resulting in rough surfaces that cause efficiency losses.
Application of coatings comprising aluminum oxide and/or silicon dioxide on CMC components to enhance sealing surfaces, using methods like grinding and electrical discharge machining, ensuring a smooth and thermally stable interface.
The coatings provide a seamless, thermally stable seal that prevents cooling flow leaks, maintaining engine efficiency by matching the CMC substrate's thermal expansion and maintaining a smooth surface finish.
Smart Images

Figure 0007596067000001 
Figure 0007596067000002 
Figure 0007596067000003
Abstract
Description
[Technical field]
[0001] The present subject matter relates generally to coatings, and more specifically, to coatings for gas turbine engines. [Background technology]
[0002] The demand for more efficient gas turbine engines has driven higher internal operating temperatures, driving a move towards high temperature materials from metallic nickel-based superalloys to ceramic matrix composites (CMCs), which offer both mechanical strength as well as high temperature resistance. However, CMCs may have higher production costs and / or longer manufacturing cycle times compared to metallic nickel-based superalloys. Additionally, the geometries and / or topologies in which CMC components can be formed may be limited compared to metallic nickel-based superalloys.
[0003] The orthotropic nature of CMCs can lead to porosity and inconsistent machined surface finishes. Porosity in the CMC sealing surface (i.e., applications where the CMC is installed in or near the hot gas path (HGP) of a gas turbine) can allow cooling flow to leak past the seal, resulting in efficiency losses. Additionally, inconsistent machining, for example due to different rates of material removal in the ceramic matrix and / or fibers, can result in ripples or rough surfaces in the finished CMC components. Rough surfaces can create waviness and gaps between the CMC seal and the seal surface, allowing cooling flow to leak, again resulting in efficiency losses in the gas turbine engine. Summary of the Invention
[0004] Aspects of the present embodiments are summarized below. These embodiments are not intended to limit the scope of the claimed embodiments, but rather, these embodiments are intended only to provide a brief outline of possible forms for the embodiments. Moreover, the embodiments may encompass a variety of forms that may be similar or different from the embodiments described below, provided they are within the scope of the claims.
[0005] In one aspect, a ceramic matrix composite (CMC) component includes at least one sealing surface disposed adjacent an interfacing surface to provide a seal therebetween, and a coating disposed on the sealing surface, the coating comprising aluminum oxide and / or silicon dioxide.
[0006] In another aspect, a gas turbine includes a compressor section, a combustor section fluidly coupled downstream from the compressor section, a turbine section fluidly coupled downstream from the combustor section, and a ceramic matrix composite (CMC) component. The CMC component includes at least one seal surface disposed adjacent to an interface surface to provide a seal therebetween, and a coating disposed on the seal surface. The coating includes aluminum oxide and / or silicon dioxide.
[0007] In another aspect, a method of forming a coated ceramic matrix composite (CMC) component includes providing a CMC component, performing at least one of grinding the CMC component and electrical discharge machining (EDM) the CMC component, and depositing a coating onto the CMC component, the coating comprising aluminum oxide and / or silicon dioxide.
[0008] These and other features, aspects, and advantages of the present disclosure will become better understood from the following detailed description when taken in conjunction with the accompanying drawings, in which like reference numerals represent like parts throughout. [Brief description of the drawings]
[0009] [Figure 1] 1 is a side schematic view of a gas turbine engine. [Diagram 2] FIG. 2 is a side schematic view of a turbine airfoil. [Diagram 3] 1 is a summary of coating composition test points. [Figure 4] 1 is a summary of coating compositions selected for further study. [Diagram 5] 1 is a method of forming a CMC component having a coating disposed thereon, according to an aspect of the present embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0010] Unless otherwise specified, the drawings provided herein are intended to illustrate features of embodiments of the present disclosure. These features are believed to be applicable in a wide variety of systems that include one or more embodiments of the present disclosure. Thus, the drawings are not intended to include all conventional features known to those skilled in the art that are required for the implementation of the embodiments disclosed herein.
[0011] In the following specification and claims, reference will be made to a number of terms that shall be defined to have the following meanings.
[0012] The singular forms "a," "an," and "the" include plural references unless the context clearly dictates otherwise.
[0013] "Optional" or "optionally" means that the subsequently described event or circumstance may or may not occur, and the description is meant to include instances in which the event occurs and instances in which it does not occur.
[0014] As used herein throughout the specification and claims, approximation language can be applied to modify any quantitative expression that can be reasonably varied without causing a change in the basic function to which it pertains. Thus, values modified with terms such as "about" and "substantially" are not limited to the exact value specified. In at least some instances, approximation language can correspond to the precision of the instrument for measuring the value. Here, and throughout the specification and claims, range limitations can be combined and / or substituted, and such ranges are identified and include all subranges encompassed therein, unless the context and language dictate otherwise.
[0015] As used herein, the term "axial" refers to a direction aligned with the central axis or shaft of the gas turbine.
[0016] As used herein, the term "circumferential" refers to a direction around (and tangential to) the circumference of a gas turbine, or, for example, a circle defined by the swept area of a rotor of a gas turbine. As used herein, the terms "circumferential" and "tangential" may be synonymous.
[0017] As used herein, the term "radial" refers to directions moving outwardly away from the central axis of the gas turbine. The "radially inward" direction is aligned toward the central axis and moving toward a decreasing radius. The "radially outward" direction is aligned away from the central axis and moving toward an increasing radius.
[0018] Referring now to the drawings, where like reference numbers refer to like components, FIG. 1 illustrates an example of a gas turbine 10 that may incorporate various aspects of the embodiments disclosed herein. As shown, the gas turbine 10 generally includes a compressor section 12 having an inlet 14 disposed at an upstream end of the gas turbine 10 and a casing 16 at least partially surrounding the compressor section 12. The gas turbine 10 further includes a combustion section 18 having at least one combustor 20 downstream from the compressor section 12, and a turbine section 22 downstream from the combustion section 18. As shown, the combustion section 18 may include multiple combustors 20. A shaft 24 extends axially through the gas turbine 10. FIG. 1 illustrates a radial direction 94, an axial direction 92, and a circumferential direction 90.
[0019] 1 , the gas turbine 10 may include a transition piece 52 disposed between a downstream end of the combustor 20 and an upstream end of the turbine section 22. The combustor 20 may include a combustor liner 54 defining a boundary of the combustor 20. The combustion section 18 may include a plurality of substantially cylindrical “can-type” combustors 20 spaced circumferentially around the gas turbine 10, in which case the combustor liner 54 may also be substantially cylindrical. In other embodiments, the combustion section 18 may include an annular combustor 20, in which case the combustor liner 54 may include both an inner liner (not shown) defining a radially inner boundary of the annular combustor 20 as well as an outer liner (not shown) defining a radially outer boundary of the annular combustor 20. The gas turbine 10 may also include a stage 1 nozzle 56 located in the turbine section 22 and disposed axially aft of the transition piece 52, as well as a stage 2 nozzle 58 disposed downstream of the first stage turbine rotor 36. The gas turbine 10 may also include one or more flowpath ducts 60 that define a radially outer boundary of the turbine gas path at an axial location between the rotor and stator (i.e., the blades 36 and the nozzles 34). The "hot section" of the gas turbine may include both the combustor section 18 and its components, and the turbine section 22 and its components.
[0020] During operation, air 26 is drawn into the inlet 14 of the compressor section 12 and progressively compressed to provide compressed air 28 to the combustion section 18. The compressed air 28 enters the combustion section 18 and is mixed with fuel in the combustor 20 to form a combustible mixture. The combustible mixture is combusted in the combustor 20, thereby generating hot gases 30 that flow from the combustor 20 across a first stage 32 of a turbine nozzle 34 to the turbine section 22. The turbine section generally includes one or more rows of rotor blades 36 separated axially by adjacent rows of turbine nozzles 34. The rotor blades 36 are coupled to the rotor shaft 24 via a rotor disk. The rotor shaft 24 rotates about the engine centerline CL. A turbine casing 38 at least partially surrounds the rotor blades 36 and the turbine nozzles 34. Each or a portion of the rows of rotor blades 36 may be concentrically surrounded by a shroud block assembly 40 disposed within the turbine casing 38. The hot gases 30 expand rapidly as they flow through the turbine section 22. Thermal and / or kinetic energy is transferred from the hot gases 30 to each stage of rotor blades 36, which rotates the shaft 24 and produces mechanical work. The shaft 24 may be coupled to a load, such as a generator (not shown), to generate electricity. Additionally or alternatively, the shaft 24 may be used to drive the compressor section 12 of the gas turbine.
[0021] FIG. 2 illustrates an enlarged side view of a portion of the turbine section 22 including a portion of an exemplary rotor blade 36 and shroud block assembly 40 according to various embodiments of the present disclosure. The turbine rotor blade or airfoil 36 extends from an axially forward leading edge 44 to an axially aft trailing edge 46 and from a radially inward root 48 to a radially outward tip 42. The airfoil 36 includes a platform 50 that defines a radially inner boundary of a hot gas path. As shown in FIG. 2, the shroud block assembly 40 generally extends radially 94 outward from the airfoil 36 between a turbine casing 38 (not shown) and a tip portion 42 of the rotor blade 36. The shroud block assembly 40 generally includes mounting hardware 62 for securing a plurality of shroud block segments 100 to the shroud block assembly 40. The plurality of shroud block segments 100 may be arranged circumferentially 90 in an annular arrangement around the rotor blade 36 within the turbine casing 38 (not shown).
[0022] 2 , each shroud block segment 100 may include a slash face 64 that forms a circumferential interface with an adjacent shroud block segment 100. Stated another way, a plurality of shroud block segments 100 may be arranged in the circumferential direction 90, with the slash face 64 of each shroud block segment 100 contacting and / or adjacent to the slash face 64 of the adjacent shroud block segment 100. Each shroud block segment 100 may also include a shroud segment forward edge 68, a shroud segment aft edge 66, and a shroud hot gas surface 76. The shroud segment forward edge 68 and the shroud segment aft edge 66 are located at the axially forward and aft ends, respectively, of each shroud block segment 100, while the shroud hot gas surface 76 is disposed on a radially inward facing surface of each shroud block segment 100 and forms a radially outer boundary of the turbine hot gas path. The platforms 50 may also include a platform forward edge 72, a platform aft edge 70, and a platform circumferential edge 74 disposed at the axially forward, axially aft, and circumferential ends, respectively, of each platform 50. The coatings of the embodiments disclosed herein may be disposed on one or more of the transition piece 52, combustor liner 54, first stage nozzle 56, second stage nozzle 58, other turbine nozzles 34, flowpath ducts 60, slashfaces 64, shroud segment forward edges 68, shroud segment aft edges 66, shroud hot gas surfaces 76, platform forward edges 72, platform aft edges 70, platform circumferential edges 74, as well as other sealing surfaces of the CMC components.
[0023] 3 and 4 summarize a series of test points that were performed to quantify various material properties of the coatings of the embodiments disclosed herein. In each case, coatings of thicknesses of about 0.01 inches to about 0.07 inches were applied to the crucibles using various methods. In one or more cases, coatings of thicknesses of about 0.02 inches to about 0.05 inches were used. Any crucible having suitable heat resistance and surface quality can be used. For example, the crucibles may include one or more graphite crucibles, ceramic rods with rounded edges, machined ceramic surfaces, and / or other suitable crucibles. The coatings may be applied to the crucibles via tape, mold, air spray, hand brushed, applied as a powder followed by crystallization, and / or via other suitable techniques. In addition, various modifications can be made to the application process to reach the desired coating thickness, density, etc. For example, the flow rate at which the coating is applied via the air spray application process can be adjusted. Additionally, the speed at which the crucible is transported under the coater (and / or the speed at which the coater moves over the crucible) can be adjusted. Both the height at which the coating is applied as well as the pressure at which the coating is applied may also be adjusted.
[0024] 3 illustrates the processing temperatures 356 of a number of material systems 352 including specific compositions 354 that were tested, as well as the resulting coefficients of thermal expansion (CTE) 358 and softening points 360. Test points 302, 304, 306, and 308 were all performed on a BAS material system including compositions having various weight percents of barium oxide (i.e., BaO and "B" in "BAS"), aluminum oxide (i.e., Al2O3 and "A" in "BAS"), and silicon dioxide (i.e., SiO2 and "S" in "BAS"). For example, as illustrated by the composition percentages listed in the composition column 354 of FIG. 3, test point 302 includes 33 weight percent silicon dioxide, 61.5 weight percent barium oxide, and 5.5 weight percent aluminum oxide, and test point 304 includes 40.3 weight percent silicon dioxide, 51.3 weight percent barium oxide, and 8.4 weight percent aluminum oxide. Test point 302, performed at a processing temperature 356 of 1300°C, resulted in a CTE 358 of 12.4(x10^-6 / (°C)) and a softening point 360 above 1200°C. Test point 302 provided a good softening point 360 above 1200°C, but the CTE 358 was higher than desired. Test point 304, also performed at a processing temperature 356 of 1300°C, but with a different BAS composition than test point 302, resulted in a CTE 358 of 8.9(x10^-6 / (°C)) and a softening point 360 of 815°C. Thus, test point 304 did not provide the desired CTE 358 or the desired softening point 360. Both test points 306 and 308, performed on various BAS compositions at 1400°C and 1300°C, respectively, yielded good CTEs 358 (i.e., about 8.0(x10^-6 / (°C)) or less), but lower than the desired softening point 360. CTE 358 was not quantified for test point 308.
[0025] 3, test points 310, 312, and 314 were performed with a BAS / SiC material system including a composition by weight of BAS and SiC (silicon carbide), as shown in composition column 354. The BAS material system used in each of test points 310, 312, and 314 included 66.7 weight percent silicon dioxide, 20 weight percent barium oxide, and 13.3 weight percent aluminum oxide (i.e., the same BAS material system as test point 306). Test point 310 was performed with a composition of 98% BAS and 2% SiC, and test point 312 was performed with a coating with a composition of 80% BAS and 20% SiC. Each of test points 310, 312, and 314 was performed at a processing temperature 356 of 1400° C. and resulted in a good CTE 358 (i.e., about 8.0(×10^-6 / (° C.)) or less), but a lower than desirable softening point 360. In addition, test points 312 and 314 resulted in a porous coating.
[0026] 3, test points 316, 318, and 320 were each performed on the SAY material system, which included 54 weight percent silicon dioxide (i.e., SiO2 and the "S" in "SAY"), 18.07 weight percent aluminum oxide (i.e., Al2O3 and the "A" in "SAY"), and 27.93 weight percent yttrium oxide (i.e., Y2O3 and the "Y" in "SAY"). Test points 316, 318, and 320 were performed at processing temperatures 356 of 1300°C, 1350°C, and 1400°C, respectively, and each resulted in a good CTE 358 (i.e., about 8.0(x10^-6 / (°C)) or less) and a good softening point 360 (i.e., greater than 1200°C). However, test point 316 resulted in a porous coating.
[0027] 3, each of the test points 322, 324, 326, 328, 330, and 332 was performed with a coating composition including a mixture of SAY and B2O3 materials. The SAY materials system of each of the test points 322, 324, 326, 328, 330, and 332 includes 54 weight percent silicon dioxide (i.e., SiO2 and the "S" in "SAY"), 18.07 weight percent aluminum oxide (i.e., Al2O3 and the "A" in "SAY"), and 27.93 weight percent yttrium oxide (i.e., Y2O3 and the "Y" in "SAY"), similar to the SAY materials system of the test points 316, 318, and 320. Each of the test points 322, 324, 326, 328, 330, and 332 also includes boron oxide (i.e., B2O3). For example, test point 322 included 97 weight percent SAY material and 3 weight percent boron oxide, and test points 324, 326, and 328 each included 95 weight percent SAY material and 5 weight percent boron oxide. Test points 322, 324, 326, 328, 330, and 332 each provided a good CTE 358 (i.e., about 8.0(x10^-6 / (°C)) or less), but only test points 322, 324, 326, and 328 provided a good softening point 360 (i.e., greater than 1200°C). In addition, test points 322, 324, and 326 all provided porous coatings.
[0028] Continuing to refer to FIG. 3, test points 334, 336, 338, 340, 342, 344, 346, 348, and 350 were each performed with a coating composition including a mixture of SAY and BAS material systems in different ratios and at different processing temperatures 356. Each of test points 334, 336, 338, 340, 342, 344, 346, 348, and 350 includes a SAY material system including 54 weight percent silicon dioxide (i.e., SiO2 and the "S" in "SAY"), 18.07 weight percent aluminum oxide (i.e., Al2O3 and the "A" in "SAY"), and 27.93 weight percent yttrium oxide (i.e., Y2O3 and the "Y" in "SAY"), similar to the SAY material system of test points 316-332. Each of test points 334, 336, 338, 340, 342, 344, 346, 348, and 350 includes a BAS material system including 66.7 weight percent silicon dioxide, 20 weight percent barium oxide, and 13.3 weight percent aluminum oxide (i.e., the same BAS material system as test points 306, 310, 312, and 314). Each of test points 334, 336, 338, 340, 342, 344, 346, 348, and 350 resulted in a good CTE 358 (i.e., about 8.0(×10^-6 / (℃)) or less). Test points 334, 336, 338, 340, 342, 346, and 348 (i.e., all except test points 344 and 350) yielded good softening points 360 (i.e., above 1200° C.). In addition, test points 334, 336, and 340 yielded porous coatings.
[0029] FIG. 4 shows a summary of each of the non-porous coatings with good CTE 358 and softening temperature 360 from FIG. 3. As such, the coatings obtained from test points 318, 320, 328, 338, 342, 346, and 348 are included and summarized in FIG. 4. The coatings obtained from these seven test points were further studied to understand the surface roughness. The coatings obtained from test points 318, 320, 328, 338, and 346 were found to have rough surfaces, while the coatings obtained from test points 342 and 348 were found to have smooth surfaces. The surface finish was quantified in terms of average roughness Ra in microinches (inches x 10^-6). The average roughness Ra is calculated as the average of the measured microscopic peaks and valleys of a surface. Rough surfaces may include surfaces with an average roughness greater than about 150 Ra, or between about 150 Ra and about 250 Ra. A smooth surface may include a surface having an average roughness below about 150 Ra, or below about 100 Ra. In other embodiments, a smooth surface may include a surface having an average roughness of about 10 Ra to about 80 Ra. In other embodiments, a smooth surface may include a surface having an average roughness of about 15 Ra to about 60 Ra. In other embodiments, a smooth surface may include a surface having an average roughness of about 20 Ra to about 50 Ra. In other embodiments, a smooth surface may include a surface having an average roughness of about 30 Ra to about 40 Ra. A smooth surface may include a surface having an average roughness of about 10 Ra to about 150 Ra, and all subranges therebetween.
[0030] The compositions of the material systems included in Figures 3 and 4 may vary around the exact components shown. For example, a SAY composition that includes about 54% S, 18% A, and 28% Y (i.e., test points 316, 318, and 320) may include 2%, 3%, or even 5% tolerance bands around each of the components. For example, the SAY composition may include about 49% to about 59% S, about 13% to about 23% A, and about 23% to about 33% Y, assuming a 5% tolerance band. Similarly, the SAY composition may include about 51% to about 57% S, about 15% to about 21% A, and about 25% to about 31% Y, assuming a 3% tolerance band. Similarly, the SAY composition may include about 52% to about 56% S, about 16% to about 20% A, and about 26% to about 30% Y, assuming a 2% tolerance band. Thus, test points containing a mixture of SAY and BAS materials systems (i.e., test points 334-350) may contain only 70% of the SAY materials system in the overall composition, and the overall composition may contain only 70% of the lower end of each of the ranges due to the 5% tolerance band. For example, a 70:30 ratio SAY:BAS materials system may contain only about 34.3 weight percent S (i.e., silicon dioxide), about 9.1 weight percent aluminum oxide, and about 16.1 weight percent yttrium oxide, taking into account the components of the SAY materials system. Taking into account the BAS material system as well, in a 90:10 SAY:BAS ratio, the silicon dioxide may increase from about 34.3 percent to about 40.5 percent (i.e., the silicon dioxide from the BAS material system adds 6.2% of the total composition), while the aluminum oxide may increase from about 9.1 to about 9.9 percent (i.e., the aluminum oxide from the BAS material system adds about 0.8% of the total composition).
[0031] The BAS material composition at test point 306 was repeated again for test points 310-314 and 334-350 due to its low CTE of 358. This material composition contained 66.7% S, 20% B, and 13.3% A. When surrounded by the 5% tolerance band, these percentages range from about 62% to about 72% S, about 15% to about 25% B, and about 8% to about 18% A. When surrounded by the 3% tolerance band, these percentages range from about 64% to about 70% S, about 17% to about 23% B, and about 10% to about 16% A. When surrounded by the 2% tolerance band, these percentages range from about 65% to about 79% S, about 18% to about 22% B, and about 11% to about 15% A.
[0032] FIG. 5 illustrates a method 500 of forming a coated CMC component according to embodiments disclosed herein. In step 502, the method includes providing a CMC component. The CMC component may include a finished CMC component, a CMC component in a green state, and / or a CMC component that has been solidified but may require one or more post-processing steps, such as heat treatment and / or machining. In step 504, the method may include performing an EDM (electrical discharge machining) process on the CMC component. In step 506, the method 500 may include performing a grinding process on the CMC component. Steps 504 and 506 may be performed in any order. In some embodiments, both steps 504 and 506 are performed. In some embodiments, neither step 504 nor step 506 is performed. In some embodiments, only one of steps 504 and 506 is performed. In step 508, the method 500 may include depositing a coating on the CMC component. The coating may be deposited on the CMC component via spray, plasma spray, and / or air spray, tape, manual brushing, and / or via powder, and subsequently crystallized and / or reacted on the CMC component. In step 510, the method 500 may include heat treating the coated CMC component. In step 512, the method 500 may include grinding the coated CMC component. In step 514, the method 500 may include honing the coated CMC component. In step 516, the method 500 may include extrusion honing the coated CMC component. In step 518, the method 500 may include polishing the coated CMC component. In some embodiments, other steps may be performed. In some embodiments, one or more of steps 502-518 may be omitted.In some embodiments, one or more of steps 502-518 may be performed in a different order than shown in FIG.
[0033] The coatings and / or sealants of the embodiments disclosed herein may be disposed at each of the above locations where the CMC surfaces and / or components define a flowpath boundary and / or interface surfaces with adjacent components (i.e., thereby forming a seal). Stated differently, the coatings of the present embodiments may be desirable to be disposed at any CMC boundary and / or interface surface where enhanced seals and / or improved surface finishes are desired. Surfaces on which the coatings may be disposed may include one or more of the transition piece 52, combustor liner 54, first stage nozzle 56, second stage nozzle 58, other turbine nozzles 34, flowpath ducts 60, one or more slash faces 64, one or more shroud segment forward edges 68, one or more shroud segment aft edges 66, one or more shroud hot gas surfaces 76, platform forward edge 72, platform aft edge 70, platform circumferential edge 74, as well as other sealing surfaces of the CMC components.
[0034] Each of the coatings according to the embodiments disclosed herein may include other oxides than those listed above. For example, boron oxide may include boron dioxide, boron trioxide, boron monoxide, and / or boron suboxide. Similarly, aluminum oxide may include aluminum oxide (I), aluminum oxide (II), and / or aluminum oxide (III). Each of the coatings according to the embodiments disclosed herein may include a glass-like surface that remains smooth during operation. In contrast, other conventional EBCs (environmental barrier coatings) and / or TBCs (thermal barrier coatings) may become brittle and spall over time when exposed to the internal operating temperatures of a gas turbine. Each of the coatings according to the embodiments disclosed herein may include a substantially similar CTE (coefficient of thermal expansion) as the CMC substrate on which they are disposed. For example, in some embodiments, the CTE of the coatings disclosed herein is within about 50% of the CTE of the CMC substrate on which they are disposed. In other embodiments, the CTE of the coatings disclosed herein is within about 20% of the CTE of the CMC substrate on which they are disposed. In other embodiments, the CTE of the coatings disclosed herein is within about 10% of the CTE of the CMC substrate on which they are disposed. In other embodiments, both the coatings disclosed herein and the CMC substrate on which they are disposed comprise a CTE of about 8.0 (x10^-6 / (°C)) or less. With conventional coatings, waviness can form on the sealing surface, allowing undesirable leakage to flow through. By including a CTE that closely matches the CMC substrate on which it is disposed, by including a high softening temperature, and by remaining smooth even when exposed to internal gas turbine operating temperatures, the coatings disclosed herein can provide a smooth sealing surface that is substantially waviness-free, thereby resulting in enhanced sealing. In other words, the coatings disclosed herein can prevent waviness and / or gaps from occurring due to mating and / or interfaces of CMC sealing surfaces, which can lead to increased undesirable leakage flow.
[0035] Although specific features of various embodiments of the present disclosure may be shown in some drawings and not in others, this is for convenience only, and in accordance with the principles of the present disclosure, any feature of a drawing may be referenced and / or claimed in combination with any feature of any other drawing.
[0036] This specification uses examples to disclose embodiments of the present disclosure, including the best mode. The examples are also used to enable any person skilled in the art to practice the disclosure, including making and using any device or system, and performing any incorporated methods. The patentable scope of the embodiments described herein is defined by the claims, and may include other examples that occur to those skilled in the art. Such other examples are intended to be within the scope of the claims if they have structural elements that do not differ from the literal language of the claims, or if they include equivalent structural elements that do not differ substantially from the literal language of the claims. [Explanation of symbols]
[0037] 10. Gas Turbine 12 Compressor Section 14 Entrance 16 Casing 18 Combustion section, combustor section 20 Annular Combustor 22 Turbine Section 24 rotor shaft 26 Air 28 Compressed Air 30 Hot Gas 32 Stage 1 34 Turbine Nozzle 36 Turbine rotor blade, airfoil, first stage turbine rotor 38 Turbine casing 40 Shroud Block Assembly 42 Tip, tip part 44 Leading Edge 46 Trailing edge 48 Base 50 Platform 52 Transition Piece 54 Combustor liner 56 1st stage nozzle, stage 1 nozzle 58 Second stage nozzle 60 Flow duct 62 Mounting Hardware 64 Slash Surface 66 Shroud segment aft edge 68 Shroud segment forward edge 70 Platform rear edge 72 Platform front edge 74 Platform Circumferential Edge 76 Shroud Hot Gas Surface 90 Circumferential direction 92 Axial 94 Radial 100 Shroud Block Segment 302 Test points 304 Test Points 306 Test Points 308 Test Points 310 test points 312 test points 314 Test Points 316 Test Points 318 Test Points 320 test points 322 test points 324 test points 326 test points 328 test points 330 test points 332 test points 334 Test Points 336 Test Points 338 test points 340 test points 342 test points 344 test points 346 test points 348 test points 350 test points 352 Materials 354 Composition column, composition 356 Processing Temperature 358 Coefficient of Thermal Expansion (CTE) 360 Softening point, softening temperature 500 ways CL Engine Centerline
Claims
1. a first shroud block segment (100) having at least one slash face (64) that forms a circumferential interface with an adjacent second shroud block segment (100) to provide a seal between the first shroud block segment (100) and the second shroud block segment (100); a coating disposed on said at least one slashface (64); A ceramic matrix composite (CMC) component comprising: The coating comprises at least a first material system comprising 13-23 wt. % aluminum oxide, 49-59 wt. % silicon dioxide, and 23-33 wt. % yttrium oxide.
2. The ceramic matrix composite (CMC) component of claim 1 , wherein the coating comprises a surface finish with an average roughness of between 10 Ra and 150 Ra.
3. The ceramic matrix composite (CMC) component of claim 1 , wherein the coating comprises a softening point (360) greater than 1200° C.
4. The ceramic matrix composite (CMC) component of claim 1 , wherein the coating comprises a coefficient of thermal expansion (358) of 8.0(×10^-6 / (° C.)) or less.
5. 10. The ceramic matrix composite (CMC) component of claim 1, wherein the coating further comprises 10-30% by weight of a second material system comprising 8-18% by weight aluminum oxide, 62-72% by weight silicon dioxide, and 15-25% by weight barium oxide.
6. The ceramic matrix composite (CMC) component of claim 1 , wherein the coating further comprises 3-5 wt. % boron oxide.
7. A compressor section (12); a combustor section (18) fluidly coupled downstream from the compressor section (12); a turbine section (22) fluidly coupled downstream of the combustor section (18); A gas turbine (10) comprising: A gas turbine (10) wherein the turbine section (22) comprises a ceramic matrix composite (CMC) component according to any one of claims 1 to 6.
8. A method (500) of forming a coated ceramic matrix composite (CMC) component according to any one of claims 1 to 6, comprising the steps of: Providing (502) a CMC component, the CMC component being a shroud block segment (100); performing (504, 506) at least one of grinding the CMC component and electrical discharge machining (EDM) the CMC component; Depositing (508) a coating on the CMC component after grinding or EDM; wherein the coating comprises at least a first material system comprising 13-23 wt. % aluminum oxide, 49-59 wt. % silicon dioxide, and 23-33 wt. % yttrium oxide.
9. After depositing (508) the coating on the CMC component, heat treating (510) the CMC component; honing the CMC component (514) after depositing the coating on the CMC component; After depositing the coating on the CMC component (508), extrusion honing the CMC component (516); grinding the CMC component after depositing the coating on the CMC component; and After depositing the coating on the CMC component (508), polishing the CMC component (518). The method of claim 8, further comprising at least one of:
10. The coating further comprises:
9. The method (500) of claim 8, comprising 10-30% by weight of a second material system comprising 3-5% by weight boron oxide, or 8-18% by weight aluminum oxide, 62-72% by weight silicon dioxide, and 15-25% by weight barium oxide.
Citation Information
Patent Citations
Blade tip coating using high purity powder
JP2009538399A
High-purity powder and coatings prepared therefrom
JP2010505717A
A method for smoothing the surface of a part made of CMC material.
JP2012522714A
Chordal mounting arrangement for low-ductility turbine shroud
JP2013015138A
Low-ductility turbine shroud
JP2013170578A