How to collect metal parts
The method of heating resin molded products under normal pressure and using external force to remove the resin layer from metal parts addresses the issues of damage and high costs in existing recovery methods, achieving efficient and cost-effective metal part recovery.
Patent Information
- Application Number
- JP2021057154
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2021-03-30
- Publication Date
- 2024-12-09
- Estimated Expiration
- 2041-03-30
AI Technical Summary
Existing methods for recovering metal parts from resin molded products expose the metal parts to high temperatures for extended periods, leading to damage and require costly high-pressure heating equipment.
A method involving heating the resin molded product under normal pressure to soften the resin layer, allowing it to be removed from the metal parts using external force, without the need for high-pressure equipment, by cutting and applying force along the direction of the metal component.
Reduces heating time, prevents metal part damage, and lowers recovery costs by using normal pressure heating and external force removal techniques.
Smart Images

Figure 0007596199000001 
Figure 0007596199000002 
Figure 0007596199000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for recovering metal parts, and more particularly to a method for recovering metal parts that can reduce the cost of recovering metal parts while suppressing damage to the metal parts. [Background technology]
[0002] There is a known technique for recovering metal parts from a resin molded product in which the metal parts are molded with a resin layer of a thermosetting resin. For example, Patent Document 1 describes a technique in which a resin molded product (resin molded coil 2) in which an acid anhydride is added to a resin layer (molded resin layer 5) is heated at 200°C for 50 hours. This technique can reduce the mechanical strength of the resin layer to an extent that the metal parts (windings 3, 4) can be pulled out from the resin layer.
[0003] Patent Document 2 describes a technique in which water and dry ice are placed in an autoclave together with a resin molded product, pressurized, and heated in the pressurized environment at 200° C. In this technique, the resin layer is made to absorb moisture by decompressing, rapidly cooling, or reheating the heated resin molded product to expand the moisture in the resin layer, thereby reducing the mechanical strength of the resin layer to the extent that it can be broken into pieces.
[0004] These techniques can significantly reduce the mechanical strength of the resin layer, so that the metal parts molded in the resin layer can be recovered in a reusable state without any processing. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] JP 2004-119757 A (for example, paragraphs 0034, 0041, FIG. 1) [Patent Document 2] JP 2001-009436 A (for example, paragraphs 0020 to 0024) Summary of the Invention [Problem to be solved by the invention]
[0006] However, when the mechanical strength of the resin layer is reduced to such an extent that the metal parts can be pulled out, as in the technique of Patent Document 1 described above, the resin molded product having the acid anhydride added to the resin layer needs to be heated at a high temperature of 200° C. for 50 hours or more. Therefore, the metal parts are exposed to such high temperatures for a long period of time, which causes a problem that the metal parts are easily damaged.
[0007] Furthermore, when the mechanical strength of the resin layer is reduced to the extent that it can be broken into pieces, as in the technology of Patent Document 2, it is necessary to heat the resin molded product under high pressure to make the resin layer absorb moisture. Therefore, it is necessary to use a heating device that can withstand high pressure, which causes a problem of increased recovery costs for metal parts.
[0008] The present invention has been made to solve the above-mentioned problems, and aims to provide a method for recovering metal parts that can reduce the cost of recovering metal parts while suppressing damage to the metal parts. [Means for solving the problem]
[0009] In order to achieve this object, the method for recovering metal parts of the present invention is a method for recovering the metal parts from a resin molded product including a metal part and a resin layer of a thermosetting resin that molds the metal part, The resin layer is an epoxy resin, a phenol resin, an unsaturated polyester, a melamine resin or a urea resin, and the temperature of the resin layer is kept at 100° C. or higher and lower than 200° C. The method includes a first step of heating the resin-molded product under normal pressure to soften the resin layer, and a second step of recovering the metal component from the resin-molded product by removing the resin layer softened by the first step from the metal component using an external force. The method for recovering metal parts of the present invention recovers metal parts from a resin molded product comprising a metal part and a resin layer of a thermosetting resin that molds the metal part, and comprises a first step of heating the resin molded product under normal pressure to soften the resin layer, and a second step of recovering the metal part from the resin molded product by removing the resin layer softened by the first step from the metal part by an external force, in which the resin molded product is placed on a support member having a hole or depression extending in the extension direction of the metal part, with the cut surface formed by cutting the resin layer facing the support member, and an external force is applied to push the metal part toward the hole or depression, thereby removing the resin layer from the metal part. Effect of the Invention
[0010] Claim 1 Or 2According to the described method for recovering metal parts, the resin molded product is heated under normal pressure to soften the resin layer, and the softened resin layer is removed from the metal part by external force, so that the heating time of the resin molded product can be shortened. That is, the resin layer is softened to the extent that the resin layer can be removed from the metal part by external force, instead of reducing the mechanical strength of the resin layer to the extent that the metal part can be pulled out of the resin layer as in the conventional method, so that the resin molded product does not need to be heated for a long time. Therefore, it is possible to prevent the metal part from being exposed to high temperatures for a long time, and therefore it is possible to prevent damage to the metal part. In addition, since the resin molded product is heated under normal pressure to soften the resin layer, it is not necessary to use a heating device that can withstand high pressure. Therefore, it is possible to reduce the recovery cost of the metal part. According to the method for recovering metal parts described in claim 1, the resin layer is an epoxy resin, a phenol resin, an unsaturated polyester, a melamine resin, or a urea resin, and the resin layer is softened by heating the resin molded product under normal pressure so that the temperature of the resin layer is 100° C. or more and less than 200° C. Therefore, there is an effect that the resin layer made of such a thermosetting resin can be removed from the metal part by an external force. According to the method for recovering metal parts described in claim 2, the resin layer is removed from the metal part by cutting the resin layer, so that the external force applied to the metal part can be reduced, compared to, for example, removing the resin layer from the metal part by applying an external force to the cut in the resin layer. Furthermore, the resin molded product is placed on a support member having a hole or a recess extending in the extension direction of the metal part, with the cut surface formed by cutting the resin layer facing the support member, and the metal part is pushed toward the hole or the recess of the support member, so that the resin layer can be removed from the metal part. This makes it unnecessary to fix the resin molded product or to apply external forces in multiple directions to the resin molded product when applying an external force to remove the resin layer from the metal part, so that the resin layer can be easily removed from the metal part.
[0011] Claim 3 According to the method for recovering metal parts described in claim 1, Or 2 In addition to the effects of the above-mentioned method for recovering metal parts, the present invention has the following effects: The heating temperature of the resin molded product is lower than the melting point of the metal parts. be Therefore, there is an effect that it is possible to remove the resin layer from the metal part while suppressing damage to the metal part.
[0012] Claim 4 According to the method for recovering metal parts described in the present invention, Article 1 In addition to the effects of the above-mentioned metal part recovery method, the method has the following effect. Since the resin layer is removed from the metal part by making a cut in the resin layer and applying an external force to the cut, the resin layer can be easily removed from the metal part even if the resin layer is in a softened state to such an extent that the metal part cannot be pulled out. In other words, compared to removing the resin layer without making a cut, the resin layer can be removed with a relatively weak external force, which has the effect of suppressing damage to the metal part due to the external force.
[0013] Claim 5 According to the method for recovering metal parts described in the present invention, 4In addition to the effects of the above-described method for recovering metal parts, the method has the following effect: A slit is made in the resin layer that extends along the extension direction of the linear metal part and is cut along a plane including the metal part, and the resin layer is removed from the metal part by applying an external force that widens the slit, so that the external force applied in the direction that bends the linear metal part when removing the resin layer can be suppressed. Therefore, there is an effect that damage to the metal part can be suppressed.
[0014]
[0015] [Brief description of the drawings]
[0016] [Figure 1] FIG. 1(a) is a front view of the resin molded product in the first embodiment, and (b) is a cross-sectional view of the resin molded product taken along line Ib-Ib in FIG. 1(a). [Diagram 2] (a) is a cross-sectional view of a resin molded product showing a cut in the resin layer, (b) is a cross-sectional view of a resin molded product showing a first method of removing the resin layer by applying an external force to the cut, (c) is a cross-sectional view of a resin molded product showing a second method of removing the resin layer by applying an external force to the cut, and (d) is a cross-sectional view of a resin molded product showing a third method of removing the resin layer by applying an external force to the cut. [Diagram 3] (a) is a cross-sectional view of a resin molded product showing a state in which a portion of the resin layer has been removed by a first operation, (b) is a cross-sectional view of a resin molded product showing a method of removing the resin layer remaining after the first operation, (c) is a cross-sectional view of a resin molded product showing a state in which a portion of the resin layer has been removed by a second operation, and (d) is a cross-sectional view of a resin molded product showing a method of removing the resin layer remaining after the second operation. [Figure 4]4(a) is a cross-sectional view of a resin molded product showing a state in which a portion of the resin layer has been removed, (b) is a cross-sectional view of a resin molded product showing a state in which the resin layer has been further removed from the state shown in FIG. 4(a), (c) is a cross-sectional view of a resin molded product showing a state in which a portion of the resin layer has been removed, and (d) is a cross-sectional view of the resin molded product and a supporting member showing a method of removing the resin layer by applying an external force to the resin molded product of FIG. 4(c). [Diagram 5] 1A is a cross-sectional view of a resin molded product of the second embodiment, FIG. 1B is a cross-sectional view of the resin molded product showing a cut in the resin layer, and FIG. 1C is a cross-sectional view of the resin molded product showing a method of removing the resin layer by applying an external force to the cut. [Figure 6] (a) is a cross-sectional view of a resin molded product according to a third embodiment, (b) is a cross-sectional view of the resin molded product showing a state in which a slit is made in the resin layer, (c) is a cross-sectional view of the resin molded product showing a method of removing the resin layer by applying an external force to the slit, and (d) is a cross-sectional view of a resin molded product showing another example. [Figure 7] 1A is a cross-sectional view of a resin molded product according to a fourth embodiment, FIG. 1B is a cross-sectional view of the resin molded product showing a state in which a slit is made in the resin layer, FIG. 1C is a cross-sectional view of the resin molded product showing a method of removing the resin layer by applying an external force to the slit, and FIG. 1D is a cross-sectional view of a resin molded product showing another example. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0017] Hereinafter, preferred embodiments of the present invention will be described with reference to the accompanying drawings. First, the configuration of a resin molded product 1 of the first embodiment will be described with reference to FIG. 1. FIG. 1(a) is a front view of the resin molded product 1 of the first embodiment, and FIG. 1(b) is a cross-sectional view of the resin molded product 1 taken along line Ib-Ib in FIG. 1(a). FIG. 1(b) illustrates a state in which the resin layer 3 located on the inner periphery side of the metal component 2 (left side of FIG. 1(b)) has been removed. FIG. 1(b) illustrates only the cross section of the resin molded product 1, and the hatching of the resin layer 3 is omitted, and the same applies to FIG. 2 and subsequent figures.
[0018] As shown in Fig. 1, the resin molded product 1 is a coil in which a metal part 2 is molded (sealed) with a resin layer 3. The metal part 2 is a twisted wire with a circular cross section made by twisting together multiple conductors, and the metal part 2 formed in a ring shape is molded with the resin layer 3.
[0019] The resin layer 3 is made of a thermosetting resin (epoxy resin in this embodiment), and the rectangular parallelepiped resin layer 3 covers the entire metal part 2. A pair of terminals 4 protrude from the outer surface of the resin layer 3, and although not shown, both ends of the metal part 2 made of conductor wires are connected to the pair of terminals 4.
[0020] The resin molded product 1 has the metal part 2 molded therein by heating and curing the resin layer 3 of a thermosetting resin, and as the manufacturing method thereof can be a known method, a detailed description thereof will be omitted.
[0021] Once hardened by heating, the resin layer 3 will not melt even if it is heated again, but it will soften. Depending on the material, when it is heated above its deflection temperature under load (softening point), it will soften to the extent that it can be easily deformed by an external force. Therefore, by applying an external force to the softened resin layer 3 and removing it from the metal part 2 (see Figure 2), the metal part 2 can be recovered from the resin molded product 1 in a reusable state.
[0022] The deflection temperature under load of the resin layer 3 is a temperature determined by the method specified in JIS K7191-1:2015 (the softening point, for example, in the case of an epoxy resin, is a temperature determined by the method specified in JIS K7234:1986).
[0023] The device (means) used in the step of heating the resin molded product 1 (step 1) can be any known device capable of heating the resin layer 3, such as a heating furnace large enough to accommodate the resin molded product 1.
[0024] In particular, in this embodiment, it is only necessary to soften the resin layer 3 to an extent that it can be removed by an external force, and there is no need to heat the resin layer 3 under high pressure as in the past. In other words, since it is sufficient to heat the resin molded product 1 in a heating furnace at normal pressure, there is no need to use a heating furnace that can withstand high pressure. Therefore, the cost of the equipment for recovering the metal parts 2 can be reduced.
[0025] As described above, the temperature inside the heating furnace is set to a temperature at which the resin layer 3 has a deflection temperature under load (softening point) or higher. Therefore, if the resin layer 3 is an epoxy resin as in this embodiment, the temperature inside the heating furnace is set to, for example, 120° C. or higher so that the temperature of the resin layer 3 becomes 100° C. or higher.
[0026] The heating time of the resin molded product 1 in the heating furnace may be a time until the resin layer 3 is softened (for example, 5 hours or more and 10 hours or less). In other words, since it is only necessary to soften the resin layer 3 to an extent that it can be removed from the metal part 2 by an external force, it is not necessary to heat the resin molded product 1 for a long time (for example, 50 hours or more). This prevents the metal part 2 from being exposed to high temperatures for a long time, thereby preventing deterioration of the metal part 2.
[0027] As described above, the cross-sectional view shown in Fig. 1(b) shows a state in which the resin layer 3 on the inner periphery side of the annular metal part 2 has been removed, but such removal can be performed using a tool having a blade such as a cutter or knife. However, it is also possible to omit the removal of a portion of the resin layer 3 as shown in Fig. 1(b) and only remove the resin layer 3, which will be described later with reference to Figs. 2 to 4.
[0028] In this manner, in this embodiment, the resin layer 3 is softened to a degree that allows the metal part 2 to be pulled out, or embrittled to the extent that the resin layer 3 can be broken into pieces by hitting it with a hammer, as in the conventional method, but the resin layer 3 is softened to a degree that allows it to have a predetermined elasticity. Therefore, it is more difficult to remove the resin layer 3 from the metal part 2 than in the conventional method, and a method for removing the resin layer 3 will be described with reference to FIG. 2.
[0029] Figure 2(a) is a cross-sectional view of the resin molded product 1 showing a cut 30 in the resin layer 3, Figure 2(b) is a cross-sectional view of the resin molded product 1 showing a first method of removing the resin layer 3 by applying an external force to the cut 30, Figure 2(c) is a cross-sectional view of the resin molded product 1 showing a second method of removing the resin layer 3 by applying an external force to the cut 30, and Figure 2(d) is a cross-sectional view of the resin molded product 1 showing a third method of removing the resin layer 3 by applying an external force to the cut 30.
[0030] The removal of the resin layer 3 described below may be performed manually using tools T1 to T3, or may be performed by a mechanized device having such tools T1 to T3 (or a similar means). The same applies to the removal operations described in FIG. 3 and subsequent drawings.
[0031] As shown in Fig. 2(a), after the step (first step) of heating the resin molded product 1 to soften the resin layer 3, the step (second step) of removing the resin layer 3 is performed without cooling the resin molded product 1 (while maintaining the softened state caused by heating in the first step). In the step of removing the resin layer 3, a cutter or other tool having a blade is used to make a slit 30 in the resin layer 3. The cut 30 may be made before the resin layer 3 is softened (heated).
[0032] The slits 30 are cut from the outer surface of the resin layer 3 toward the metal component 2. That is, the slits 30 extend along the extension direction (axial direction) of the linear metal component 2 (perpendicular to the paper surface of FIG. 1) and are cut along a plane including the metal component 2, and in this embodiment, the slits 30 are formed up to the surface of the metal component 2 or near the surface. Note that the near the surface of the metal component 2 refers to a region that is 1 mm or less away from the surface of the metal component 2, but the slits 30 may be formed in a region that is more than 1 mm away from the surface of the metal component 2.
[0033] As shown in FIG. 2(b), the first method for removing the resin layer 3 uses a pair of tools T1 (crowbars) having an L-shaped bent portion T1a at their tip. With the bent portion T1a of each of the pair of tools T1 inserted (hooked) into the slit 30, the base end of each of the tools T1 is pulled to widen the slit 30. This allows the resin layer 3 to be peeled off from the metal part 2. Note that another removal method similar to the first method is, for example, a method in which the tip of a tool such as pliers is inserted into the slit 30 to push it apart.
[0034] 2(c), the second method for removing the resin layer 3 uses a tool T2 (crowbar) whose tip is formed into a flat rod or plate shape. The tip of the tool T2 is inserted into the slit 30, and while the resin molded product 1 is fixed by a fixing means (not shown), the tool T2 is rotated (or pulled) in a direction to widen the slit 30. This allows the resin layer 3 to be peeled off from the metal part 2.
[0035] 2(d), the third method for removing the resin layer 3 uses a tool T3 (pliers with jaws) having a pair of arms T3a at their tips. One of the arms T3a is inserted into the slit 30 to grip the resin layer 3, and while the resin molded product 1 is fixed by a fixing means (not shown), the tool T3 is rotated (or pulled) in a direction to widen the slit 30. This allows the resin layer 3 to be peeled off from the metal part 2.
[0036] As in the first to third methods, by peeling the resin layer 3 from the metal part 2 by applying an external force that widens the slit 30, the resin layer 3 can be easily removed from the metal part 2 even if the resin layer 3 is softened to such an extent that the metal part 2 cannot be pulled out. That is, compared to removing the resin layer 3 without making the slit 30, the resin layer 3 can be removed with a relatively weak external force, and damage to the metal part 2 due to the external force can be suppressed.
[0037] Moreover, the slits 30 extend along the extension direction (axial direction) of the linear metal part 2, and are cut along a plane including the metal part 2. Therefore, the force used to widen the slits 30 and peel off the resin layer 3 acts in the circumferential direction of the metal part 2, which prevents the metal part 2 from bending due to an external force used to remove the resin layer 3. Therefore, damage to the metal part 2 can be prevented.
[0038] In this way, when the resin layer 3 is removed by applying an external force, the metal part 2 may be deformed (damaged) by the external force. In this embodiment, since the metal part 2 is an aluminum conductor, the mechanical strength of the metal part 2 is significantly reduced when the temperature of the metal part 2 exceeds 200° C., and the metal part 2 is easily deformed by the external force when the resin layer 3 is removed. Therefore, the metal part 2 may not be recovered in a reusable state.
[0039] Therefore, it is preferable that the temperature when the above-mentioned resin molded product 1 is heated (first step) is a temperature at which the resin layer 3 reaches or exceeds its deflection temperature under load (softening point), and is a sufficiently low temperature below the melting point of the metal part 2, so that the metal part 2 is not damaged (deformed) by the external force applied when removing the resin layer 3 from the metal part 2, and can maintain its mechanical strength.
[0040] Specifically, in this embodiment, since the resin layer 3 is an epoxy resin and the metal part 2 is aluminum, it is preferable to heat the resin layer 3 (set the temperature of the heating furnace) so that the temperature of the resin layer 3 during heating is 100°C or higher and lower than 200°C. This makes it possible to remove the resin layer 3 by external force while preventing the metal part 2 from being deformed (damaged) by that external force. It is more preferable to heat the resin layer 3 so that the temperature of the resin layer 3 during heating is 120°C or higher and lower than 150°C. This makes it possible to easily remove the resin layer 3 by external force while more effectively preventing the metal part 2 from being damaged by that external force.
[0041] Here, when removing the resin layer 3 by the above-mentioned first to third methods, there are cases where it is not possible to remove all of the resin layer 3 by a single removal operation using the tools T1 to T3. A method for removing the resin layer 3 in such cases will be described with reference to FIG.
[0042] Figure 3(a) is a cross-sectional view of a resin molded product 1 showing a state in which a portion of the resin layer 3 has been removed by a first operation, Figure 3(b) is a cross-sectional view of a resin molded product 1 showing a method of removing the resin layer 3 remaining after the first operation, Figure 3(c) is a cross-sectional view of a resin molded product 1 showing a state in which a portion of the resin layer 3 has been removed by a second operation, and Figure 3(d) is a cross-sectional view of a resin molded product 1 showing a method of removing the resin layer 3 remaining after the second operation.
[0043] As shown in Fig. 3(a), when an external force is applied to the cut 30 to peel off the resin layer 3, a fracture surface 31 where part of the resin layer 3 is broken may be formed in the resin molded product 1. In such a case, as shown in Fig. 3(b), the resin layer 3 is removed using a pair of tools T3.
[0044] Specifically, a part of the resin layer 3 including the cut 30 is gripped by the arm portion T3a of one tool T3, and a part of the resin layer 3 including the fracture surface 31 is gripped by the arm portion T3a of the other tool T3. Then, with the resin layer 3 gripped, the pair of tools T3 are rotated in different directions in the circumferential direction of the metal part 2 (so as to push the metal part 2 out of the resin layer 3). This allows the resin layer 3 to be peeled off from the metal part 2.
[0045] As shown in Fig. 3(c), the second operation may result in the formation of a fractured surface 32 in which a part of the resin layer 3 is fractured again in the resin molded product 1. In this case, as shown in Fig. 3(d), a part of the resin layer 3 including the fractured surface 31 is grasped by the arm portion T3a of one tool T3, and a part of the resin layer 3 including the fractured surface 32 is grasped by the arm portion T3a of the other tool T3. Then, similarly to the second operation described above, the pair of tools T3 are rotated in different directions in the circumferential direction of the metal part 2 (so as to push the metal part 2 out of the resin layer 3). This allows the resin layer 3 to be peeled off from the metal part 2.
[0046] In this way, when the resin layer 3 remains after one or more removal operations, a part of the resin layer 3 including the cut 30 and the fracture surfaces 31, 32 is gripped with a pair of tools T3, and the pair of tools T3 is rotated in different directions in the circumferential direction of the metal part 2 to peel off the resin layer 3. In this way, the force when peeling off the resin layer 3 acts in the circumferential direction of the metal part 2, so that bending of the linear metal part 2 due to the force when removing the resin layer 3 can be suppressed. Therefore, damage to the metal part 2 can be suppressed.
[0047] When peeling off the resin layer 3 using the tool T3, the resin layer 3 may be gripped by three or more tools T3 instead of a pair of tools T3. Also, the resin layer 3 may be gripped by a plurality of tools T3 of different types instead of gripping the resin layer 3 by a plurality of tools T3 of the same type.
[0048] Next, referring to Fig. 4, a case where the resin layer 3 is cut at slits 30a-30d to be cut from the metal part 2 will be described. Fig. 4(a) is a cross-sectional view of the resin molded product 1 showing a state where a part of the resin layer 3 has been cut away, Fig. 4(b) is a cross-sectional view of the resin molded product 1 showing a state where the resin layer 3 has been further cut away from the state shown in Fig. 4(a), Fig. 4(c) is a cross-sectional view of the resin molded product 1 showing a state where a part of the resin layer 3 has been cut away, and Fig. 4(d) is a cross-sectional view of the resin molded product 1 and the supporting member 5 showing a method of removing the resin layer 3 by applying an external force to the resin molded product 1 shown in Fig. 4(c). Note that Fig. 4(d) shows only a cross section of the supporting member 5.
[0049] As shown in Fig. 4(a), when a part of the resin layer 3 is to be removed, a pair of parallel slits 30a, 30b are made along the surface (or its vicinity) of the metal part 2. That is, the slits 30a, 30b extend along the extension direction (axial direction) of the linear metal part 2, and are cut along a plane that does not include the metal part 2. This makes it possible to remove a part of the resin layer 3 along the slits 30a, 30b. Therefore, compared to the case where the resin layer 3 is removed by pushing the slit 30 (see Fig. 3) as described above, it is possible to suppress the application of an external force to the metal part 2, and therefore to suppress damage to the metal part 2.
[0050] Next, as shown in FIG. 4(b), a pair of cuts 30c, 30d are further made in the resin layer 3, the part of which has been cut off by the cuts 30a, 30b, to cut it off. The pair of cuts 30c, 30d are parallel to each other and extend in a direction perpendicular to the pair of cuts 30a, 30b. This makes it possible to remove almost all of the resin layer 3 from the metal part 2 by making the cuts 30a to 30d four times. In this way, by repeating the cutting of the resin layer 3 multiple times to remove almost all of the resin layer 3, it is possible to prevent the metal part 2 from being damaged by an external force.
[0051] In addition, if a small amount of the resin layer 3 remains on the surface of the metal part 2 as shown in FIG. 4(b) after the resin layer 3 has been cut off multiple times, it can be removed by brushing or the like.
[0052] As shown in Figures 4(c) and 4(d), it is also possible to make a cut 30a to cut away a part of the resin layer 3, and then remove the resin layer 3 using a support member 5. Specifically, the support member 5 is a member having an elongated hole 50 (or a recess) having a shape corresponding to the shape of the metal part 2 (in this embodiment, annular). If the surface formed by cutting away the resin layer 3 at the cut 30a is taken as a cut surface 33, the resin molded product 1 is placed on the support member 5 in a position where the cut surface 33 faces the elongated hole 50 of the support member 5, that is, in a position where the metal part 2 is placed above the elongated hole 50.
[0053] Then, in this placed state, an external force is applied to press in the outer surface 34 of the resin layer 3 opposite the cut surface 33. As a result, the resin layer 3 is removed when the metal part 2 is pressed into the long hole 50. Therefore, compared to the case where the resin layer 3 is peeled off using the above-mentioned tools T1 to T3 (see FIG. 3), it is not necessary to fix the resin molded product 1 or to apply external forces in multiple directions to the resin molded product 1.
[0054] Next, second to fourth embodiments will be described with reference to Figures 5 to 7, but the same parts as in the first to fourth embodiments will be denoted by the same reference numerals and their description will be omitted. In addition, the process (first process) of heating the resin molded products 201, 301, and 401 in the second to fourth embodiments described later is performed under the same conditions as in the first embodiment, so the description of this process will be omitted.
[0055] First, the second embodiment will be described. Fig. 5(a) is a cross-sectional view of a resin molded product 201 of the second embodiment, Fig. 5(b) is a cross-sectional view of the resin molded product 201 showing a state in which a slit 230 is made in a resin layer 203, and Fig. 5(c) is a cross-sectional view of the resin molded product 201 showing a method of removing the resin layer 203 by applying an external force to the slit 230. In Fig. 5, the fiber reinforced resin 235 is hatched in dots to facilitate understanding, and the same applies to Fig. 6 and subsequent figures.
[0056] As shown in Fig. 5(a), in the resin molded product 201 of the second embodiment, a resin layer 203 is formed by laminating sheet-shaped fiber reinforced resin 235. The fiber reinforced resin 235 is SMC (Sheet Molding Compounds) in which reinforcing fibers such as glass fiber and carbon fiber are impregnated with a thermosetting resin. In this embodiment, the metal component 2 is molded by winding one sheet of fiber reinforced resin 235 around the metal component 2 multiple times. Therefore, the fiber reinforced resin 235 is formed in a spiral shape with the metal component 2 at the center, from the end E1 on the metal component 2 side to the end E2 on the outer periphery side in a cross-sectional view.
[0057] As shown in FIG. 5(b), when removing the resin layer 203 from the metal part 2, a slit 230 is made toward the inside of the end E2 on the outer periphery side of the fiber reinforced resin 235. After the slit 230 is formed, as shown in FIG. 5(c), one of the pair of arms T3a of the tool T3 is inserted into the slit 230 to grip the end E2 on the outer periphery side of the fiber reinforced resin 235. In this state, the tool T3 is rotated in the circumferential direction of the metal part 2, and the fiber reinforced resin 235 wound around the metal part 2 is peeled off so as to spread it. As a result, almost all of the resin layer 203 can be removed by the operation of peeling off one sheet of fiber reinforced resin 235 from the metal part 2. Therefore, the resin layer 203 can be efficiently removed, and the metal part 2 can be easily recovered.
[0058] Next, a third embodiment will be described. Fig. 6(a) is a cross-sectional view of a resin molded product 301 of the third embodiment, Fig. 6(b) is a cross-sectional view of the resin molded product 301 showing a state in which a slit 330 is made in the resin layer 303, Fig. 6(c) is a cross-sectional view of the resin molded product 301 showing a method of removing the resin layer 303 by applying an external force to the slit 330, and Fig. 6(d) is a cross-sectional view of the resin molded product 301 showing another example.
[0059] 6(a), in the resin molded product 301 of the third embodiment, a resin layer 303 is formed by laminating a plurality of (four in this embodiment) sheet-shaped fiber reinforced resins 235. In the following description, the fiber reinforced resins are denoted by reference characters 235a, 235b, 235c, and 235d in order from the layer closest to the metal component 2.
[0060] Each of the multiple fiber reinforced resins 235a to 235d is wrapped around the metal part 2 from a direction perpendicular to the extension direction of the metal part 2 (the lower side in FIG. 6(a)). A gap S1 is formed between both ends E1, E2 of the fiber reinforced resin 235a in the circumferential direction of the metal part 2. Furthermore, both ends of the fiber reinforced resins 235b to 235d in the circumferential direction of the metal part 2 are configured not to overlap with the gap S1 when viewed in a direction perpendicular to the extension direction of the metal part 2 (when viewed in the up-down direction in FIG. 6(a)).
[0061] As a result, as shown in FIG. 6(b), by providing a slit 330 from the outer surface of the resin layer 303 toward the gap S1, a slit 330 toward the inner side of the fiber reinforced resin 235a (between the metal component 2) can be formed.
[0062] 6(c), one of a pair of arms T3a of the tool T3 is inserted into the slit 330, and the end E2 (or E1) of the fiber reinforced resin 235a is gripped by the tool T3. In this state, the tool T3 is rotated in the circumferential direction of the metal part 2, and the fiber reinforced resin 235a-235d wound around the metal part 2 is peeled off so as to spread it. In this way, almost all of the resin layer 303 can be removed by the operation of peeling off the fiber reinforced resin 235a-235d from the metal part 2. Therefore, the resin layer 303 can be efficiently removed, and the metal part 2 can be easily recovered.
[0063] 6(d), in the resin molded product 301, the positions of the ends of the fiber reinforced resins 235a to 235d may differ from one another in the circumferential direction of the metal part 2. That is, the gaps between the ends of the fiber reinforced resins 235a to 235d may be arranged at positions that do not overlap when viewed in a direction perpendicular to the extension direction of the metal part 2. In such a case, the fiber reinforced resins 235a to 235d may be peeled off one or more sheets at a time after making cuts to cut the fiber reinforced resins 235a to 235d, or the fiber reinforced resins 235a to 235d may be peeled off without making cuts.
[0064] Next, a fourth embodiment will be described. Fig. 7(a) is a cross-sectional view of a resin molded product 401 of the fourth embodiment, Fig. 7(b) is a cross-sectional view of the resin molded product 401 showing a state in which a slit 430 is made in a resin layer 403, Fig. 7(c) is a cross-sectional view of the resin molded product 401 showing a method of removing the resin layer 403 by applying an external force to the slit 430, and Fig. 7(d) is a cross-sectional view of the resin molded product 401 showing another example.
[0065] 7(a), in the resin molded product 401 of the fourth embodiment, a resin layer 403 is formed by laminating a plurality of (eight in this embodiment) sheet-shaped fiber reinforced resin 235. In the following description, in the direction (the vertical direction in FIG. 7(a)) perpendicular to the extension direction of the metal component 2, four sheets located on one side (the upper side in FIG. 7(a)) of the metal component 2 are denoted as fiber reinforced resin 235e, and four sheets located on the other side are denoted as fiber reinforced resin 235f.
[0066] Each of the multiple fiber reinforced resins 235e is wrapped in an arc shape so as to cover the metal part 2 from a direction (the upper side in FIG. 7(a)) perpendicular to the extension direction of the metal part 2. That is, the metal part 2 has an area in the circumferential direction where the fiber reinforced resin 235e is not wrapped, and the multiple fiber reinforced resins 235f are layered so as to cover this area. The multiple fiber reinforced resins 235f are parallel to each other.
[0067] A gap S2 is formed between each of the end portions E1 (E2) of the fiber reinforced resins 235e that are stacked at a position closest to the metal part 2 among the multiple fiber reinforced resins 235e and the end portion E1 (E2) of the fiber reinforced resins 235f that are stacked at a position closest to the metal part 2 among the multiple fiber reinforced resins 235f.
[0068] As a result, as shown in Figure 7 (b), by making a slit 430 from the outer surface of the resin layer 403 toward the gap S2, a slit 430 can be formed toward the inner side (between the metal part 2) of the fiber reinforced resin 235f that is laminated at a position closest to the metal part 2.
[0069] Then, as shown in FIG. 7(c), one of a pair of arms T3a of the tool T3 is inserted into the slit 430, and the end E1 of the fiber reinforced resin 235f (or the fiber reinforced resin 235e) is gripped by the arm T3a of the tool T3. In this state, the tool T3 is rotated in the circumferential direction of the metal part 2, and the laminated fiber reinforced resin 235f is peeled off. This makes it possible to remove a large amount of the resin layer 403 from the metal part 2 at once. Therefore, the resin layer 403 can be efficiently removed, and the metal part 2 can be easily recovered.
[0070] After removing the fiber reinforced resin 235f, the resin layer 235e can be removed by pushing out the metal part 2 using a pair of tools T3a, as in the case described with reference to Fig. 3(d). Also, in the second to fourth embodiments described above, if a small amount of the resin layer 203, 303, 403 remains on the surface of the metal part 2 after the fiber reinforced resin 235 is peeled off, it can be removed by brushing or the like.
[0071] 7(d), in the resin molded product 401, the positions of the ends of the fiber reinforced resins 235e, 235f may differ from each other in the circumferential direction of the metal part 2. That is, the gaps between both ends of the fiber reinforced resins 235e, 235f may be arranged at positions that do not overlap each other when viewed in a direction perpendicular to the extension direction of the metal part 2. In such a case, the fiber reinforced resins 235e, 235f may be peeled off one or more sheets at a time after making a cut to cut the fiber reinforced resins 235e, 235f, or the fiber reinforced resins 235e, 235f may be peeled off without making a cut.
[0072] As described above, according to the method for recovering a metal part 2 of the present invention, the resin-molded product 1, 201, 301, 401 is heated to soften the resin layer 3, 203, 303, 403 to an extent that it can be removed from the metal part 2 by external force. This makes it unnecessary to heat for a long time, and makes it easier to recover the metal part 2 from the resin-molded product 1, 201, 301, 401 in an intact state.
[0073] The present invention has been described above based on the above embodiment, but the present invention is not limited to the above form in any way, and it can be easily inferred that various modifications and improvements are possible within the scope that does not deviate from the spirit of the present invention.
[0074] In each of the above embodiments, the metal part 2 is a twisted wire having a circular cross section formed by twisting together a plurality of conducting wires, but this is not necessarily limited to this. For example, the metal part 2 may be a solid wire having a round bar shape (circular cross section) or a flat plate shape, or may be a twisted wire such as a flat twisted wire. Furthermore, the metal part 2 may have a shape other than a ring shape (for example, a linear shape), and the resin layer 3 may have a shape other than a rectangular parallelepiped (for example, a ring shape). Furthermore, the material of the metal part 2 is not limited to aluminum, and may be other metals such as iron or copper.
[0075] In other words, the configurations such as the above-mentioned metal part 2 and the shape of the resin layer 3 (the fact that the resin molded product 1 is a coil) are examples, and the technical ideas of each of the above-mentioned embodiments can be applied as long as a part containing metal is molded with a thermosetting resin.
[0076] In the above-mentioned embodiments, epoxy resin is exemplified as an example of the resin layer 3, 203, 303, 403 made of a thermosetting resin, but the present invention is not necessarily limited thereto. For example, the resin layer 3, 203, 303, 403 may be made of other thermosetting resins, such as phenolic resin, unsaturated polyester, melamine resin, or urea resin (urea resin), as long as the resin layer is made of a material that is softened by heating. That is, the heating temperature and heating time may be adjusted according to the material of the resin layer (thermosetting resin) so that the resin layer is softened to a degree that it can be peeled off from the metal part 2. For example, if the resin layer is made of phenolic resin or urea resin, the resin layer may be heated to 140°C or higher, and if it is made of melamine resin, the resin layer may be heated to 170°C or higher.
[0077] Although not described in each of the above embodiments, the step (second step) of removing the resin layer 3, 203, 303, 403 from the metal part 2 may be performed at room temperature or below, or in a heated environment (at a temperature equal to or below that of the first step). That is, the step of removing the resin layer 3, 203, 303, 403 may be performed in an environment in which the resin can be kept softened by heating (in a state in which it can be removed from the metal part 2).
[0078] In the above-described embodiments, the resin layer 3, 203, 303, 403 is provided with the slits 30, 30a to 30d, 230, 330, 430, but this is not necessarily limited to this. For example, the slits 30, 230, 330, 430 may be omitted.
[0079] In the above-described embodiments, the cuts 30, 30a to 30d, 230, 330, and 430 are formed in a straight line, but this is not necessarily limited to this, and the shape of the cuts can be appropriately set by combining straight lines and curves as long as it is possible to easily remove the resin layer 3, 203, 303, and 403. Therefore, for example, the resin layer 3 may be removed by forming an L-shaped cut connecting the cut 30a (30b) and the cut 30c (30d) illustrated in FIG. 4, or a U-shaped cut connecting the cuts 30a to 30c.
[0080] In the above second to fourth embodiments, the resin layers 3, 203, 303, and 403 are formed by stacking a plurality of fiber reinforced resins 235 (235a to 235f), but this is not necessarily limited to this. For example, a filler such as silica or calcium carbonate may be added to the resin layers 3, 203, 303, and 403 instead of the fiber reinforced resin.
[0081] In the third and fourth embodiments, the four sheets of fiber reinforced resin 235a-235f are simultaneously peeled off from the metal part 2, but this is not necessarily limited to this. For example, the fiber reinforced resin 235a-235f may be peeled off one by one, or two or three sheets at a time. [Explanation of symbols]
[0082] 1,201,301,401 Resin molded products 2 Metal parts 3,203,303,403 Resin layer 30, 30a~30d, 230, 330, 430 break 33 Resection plane 235, 235a~235f Fiber reinforced resin 5 Supporting member 50 Long hole (hole)
Claims
1. A method for recovering a metal part from a resin-molded product comprising a metal part and a resin layer of a thermosetting resin that molds the metal part, comprising: the resin layer is an epoxy resin, a phenolic resin, an unsaturated polyester, a melamine resin or a urea resin; A method for recovering metal parts, comprising: a first step of heating the resin molded product under normal pressure so that the temperature of the resin layer becomes 100°C or higher but lower than 200°C to soften the resin layer; and a second step of recovering the metal parts from the resin molded product by removing the resin layer softened by the first step from the metal parts by an external force.
2. A method for recovering metal parts from a resin molded product comprising a metal part and a resin layer of a thermosetting resin that molds the metal part, comprising: a first step of heating the resin-molded product under normal pressure to soften the resin layer, and a second step of removing the resin layer softened by the first step from the metal component by an external force, thereby recovering the metal component from the resin-molded product, The second step of the method for recovering metal parts is characterized in that the resin molded product is placed on a support member having a hole or depression extending in the extension direction of the metal part, with the cut surface formed by cutting the resin layer facing the support member, and the resin layer is removed from the metal part by applying an external force that pushes the metal part toward the hole or depression.
3. 3. The method for recovering metal parts according to claim 1, wherein the heating temperature of the resin-molded product in the first step is lower than the melting point of the metal parts.
4. 2. The method for recovering metal parts according to claim 1, wherein in the second step, a cut is made in the resin layer, and an external force is applied to the cut to remove the resin layer from the metal part.
5. The cut line extends along an extension direction of the linear metal component and is cut along a plane including the metal component, 5. The method for recovering metal parts according to claim 4, wherein in the second step, the resin layer is removed from the metal part by applying an external force that widens the slit.
Citation Information
Patent Citations
Rubber crawler disposal method and device therefor
JP1995117742A
Method for treating waste motor
JP1999004564A
Separating and recovering method for metal and synthetic resin and device therefor
JP1999019631A
Method of recovering copper resources from mold parts
JP1999128899A
Recyclable power cable