Cold asphalt mixture

A room-temperature asphalt mixture with a balanced performance in flow resistance, scattering resistance, and low-temperature workability is achieved by using a specific ratio of plant-derived agents and fatty acid pitch, addressing the limitations of existing mixtures.

JP7596396B2Active Publication Date: 2024-12-09OBAYASHI ROAD CORPORATION
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
JP2022553388
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-10-02
Publication Date
2024-12-09
Estimated Expiration
2040-10-02

AI Technical Summary

Technical Problem

Existing room-temperature asphalt mixtures lack a good balance of flow resistance, aggregate scattering resistance, deflection followability, and low-temperature workability, and are often expensive due to the use of costly property improving agents.

Method used

A room-temperature asphalt mixture composed of aggregate, asphalt, an oily plant-derived property improving agent, and a lubricating solidifying agent, with a ratio of 40:60 to 5:95, utilizing fatty acid pitch as an industrial by-product, and optionally recycled aggregates.

Benefits of technology

The mixture achieves improved flow resistance, aggregate scattering resistance, and deflection followability with low-temperature workability, while being economical by using inexpensive fatty acid pitch, maintaining a balanced performance and reducing costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007596396000001
    Figure 0007596396000001
  • Figure 0007596396000002
    Figure 0007596396000002
  • Figure 0007596396000003
    Figure 0007596396000003
Patent Text Reader

Abstract

[Problem] To provide an ambient-temperature asphalt mixture that exhibits excellent economics and an excellent balance among the flow resistance, aggregate fretting resistance, deflection followability, and low-temperature workability. [Solution] An ambient-temperature asphalt mixture is provided by mixing at least an aggregate, asphalt, a property improver that is a plant-derived oily component, a lubricating solidifying agent (a fatty acid and / or a dimer of a fatty acid and / or a trimer of a fatty acid), and cement, wherein the property improver: lubricating solidifying agent ratio is set in the range of 40 : 60-5 : 95. In addition, a recycled aggregate is mixed as a portion of the aggregate. Moreover, an inexpensive fatty acid pitch, in the form of an industrial by-product in fatty acid production, is used as the property improver.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a cold asphalt mixture used for road paving and the like. [Background technology]

[0002] Conventionally, cold asphalt mixtures that can be applied at room temperature at the construction site have been used for the temporary restoration of paved roads following the excavation of buried pipes under roads and for repairing locally damaged areas of existing paved roads. This type of cold asphalt mixture has the advantage that it can be packed in bags, spread evenly at room temperature at the construction site, and compacted, but it has the problem that it is less durable than normal heated asphalt mixtures and cannot be used for long periods of time. In particular, this cold asphalt mixture can only be used for a short period of time in construction locations with heavy traffic, pavement surfaces that are subject to repeated vibrations, and pavement surfaces on decks that have a large amount of deflection.

[0003] In order to solve the above problems, in recent years, cold asphalt mixtures that can develop strength in a short time by using reactive substances have been developed. Here, such cold asphalt mixtures are composed of at least aggregates (e.g., crushed stone, crushed sand, fine sand, stone powder, etc.), asphalt, a lubricating solidifier (fatty acid and / or fatty acid dimer and / or fatty acid trimer), and an alkaline additive (cement), and various proposals have been made to date to improve the strength, durability, and deflection compliance of the pavement constructed using these mixtures.

[0004] For example, Patent Document 1 proposes the use of a lubricating solidifying material containing 1 to 15 weight percent palmitic acid, 0.3 to 10 weight percent stearic acid, 39 to 59 weight percent oleic acid, 20 to 48 weight percent linoleic acid, and 1 to 15 weight percent linolenic acid.

[0005] Moreover, Patent Document 2 proposes the use of a lubricant solidifying material containing 50 to 100% by weight of saturated fatty acids having 6 to 30 carbon atoms.

[0006] Furthermore, Patent Document 3 proposes using an organic acid polymer having two or more carboxyl and / or sulfo groups in its side chains, and a reactive resin material containing at least divalent metal ions as an alkaline additive (cement). With this room temperature asphalt mixture, the reactive resin material and the alkaline additive undergo a crosslinking and / or polymerization reaction upon addition of water to form an ionomer, which gives the pavement strength and deflection compliance.

[0007] Furthermore, Patent Document 4 proposes using a fatty acid containing oleic acid and linoleic acid, and setting the linoleic acid content to a value greater than 50% by weight based on the total weight of the oleic acid and linoleic acid. [Prior art documents] [Patent documents]

[0008] [Patent Document 1] Patent No. 5916937 [Patent Document 2] Patent No. 6089139 [Patent Document 3] Patent No. 6344873 [Patent Document 4] Patent No. 6458194 Summary of the Invention [Problem to be solved by the invention]

[0009] However, the cold asphalt mixtures proposed in Patent Documents 1 to 4 do not necessarily have a good balance of flow resistance, aggregate scattering resistance, deflection tracking, and workability at low temperatures, and the property improver is expensive. For example, the property improver proposed in Patent Document 4, which is a petroleum lubricant-based liquid, is more expensive than fatty acid pitch, which is an industrial by-product in fatty acid production. For this reason, cold asphalt mixtures containing such expensive property improvers have problems in terms of economic efficiency.

[0010] The present invention has been made in consideration of the above problems, and an object of the present invention is to provide an ambient temperature asphalt mixture which is excellent in balance of flow resistance, aggregate scattering resistance, deflection tracking ability and low temperature workability, as well as being economical. [Means for solving the problem]

[0011] In order to achieve the above object, the present invention provides an asphalt mixture at room temperature that is composed of at least aggregate, asphalt, a property improver which is an oily component derived from plants, a lubricant solidifier (fatty acid and / or fatty acid dimer and / or fatty acid trimer) and cement, and is characterized in that the ratio of the property improver:lubricant solidifier is set in the range of 40:60 to 5:95.

[0012] Here, recycled aggregate may be further mixed into the above-mentioned cold asphalt mixture.

[0013] The property improving agent is preferably a fatty acid pitch. Effect of the Invention

[0014] According to the present invention, it has been experimentally confirmed that a good balance is achieved between the flow resistance, aggregate scattering resistance, deflection follow-up property, and low-temperature workability of the cold asphalt mixture by setting the ratio of property improver:lubricating solidifier in the range of 40:60 to 5:95. In addition, by using inexpensive fatty acid pitch, an industrial by-product of fatty acid production, as the property improver, the cost of the cold asphalt mixture is kept low, making it economical. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0015] An embodiment of the present invention will be described below.

[0016] The cold asphalt mixture of the present invention is a repair material that hardens when water is poured onto it at room temperature to form an asphalt pavement, and is basically composed of a mixture of aggregate, a property improver that is an oily component derived from plants, a lubricating solidifier, and cement. An example of the mixing ratio of various substances that compose this cold asphalt mixture is shown in Table 1.

[0017] [Table 1] As shown in Table 1, the aggregates contained in the asphalt mixture according to this embodiment are 43.0% No. 7 crushed stone (maximum particle size 5 mm), 24.0% crushed sand, 28.0% fine sand, and 5.0% stone powder. The aggregates can be adjusted in particle size by using No. 6 crushed stone (maximum particle size 13 mm) or No. 5 crushed stone (maximum particle size 20 mm) depending on the type of existing pavement.

[0018] Here, as shown in Table 1, the fatty acid as a lubrication solidifier and the fatty acid pitch as a property improver constitute the plasticizer mixture, and this fatty acid mixture and asphalt constitute the binder. The blending ratio of asphalt in the binder is set to 56.1%, and the blending ratio of the plasticizer mixture is set to 43.90%. the above The plasticizer mixture contains fatty acid and fatty acid pitch as a property improver. Here, the fatty acid does not contain pitch since it is produced as a target product.

[0019] Straight asphalt (St.As.60 / 80) is used as the asphalt, and when selecting asphalt, the appropriate one can be selected taking into consideration the aggregate peelability, etc. In addition, decolorized asphalt can also be used depending on the conditions of the construction site.

[0020] Furthermore, ordinary cement is used as the externally added alkaline additive.

[0021] Table 1 shows the mix ratios of each mixture when the total of the various mixtures excluding the cement as an external additive is taken as 100%, with the mix ratios of No. 7 crushed stone, crushed sand, fine sand, and stone powder in the aggregate being 40.2%, 22.4%, 26.2%, and 4.7%, respectively. The mix ratio of the binder is 6.5%, of which 3.65% is asphalt, 2.14% is lubricating solidifier, and 0.71% is property improver. In this case, 0.8% cement is added externally.

[0022] As mentioned above, the plasticizer mixture contains a lubricant solidifier and a property improver. Table 2 shows the types and blending ratios of the lubricant solidifier and property improver.

[0023] [Table 2] In this embodiment, TFA-145WF (model number) manufactured by Tsuno Food Industry Co., Ltd. was used as the fatty acid. In this embodiment, fatty acid pitch, which is an oily component derived from plants, was used as the property improving agent. This fatty acid pitch is an industrial by-product (residue) in the production of fatty acids. In this embodiment, a specially investigated fatty acid pitch (formally indicated as "TFA-B60" in Table 2) was used.

[0024] In this embodiment, the ratio of fatty acid pitch: fatty acid in the room temperature asphalt mixture is set to 25:75 (shown as "Example 1" in Table 2). In Table 2, "Comparative Example 1" refers to a case where no property improver is used and fatty acid (TFA-145WF) is used at 100%, and "Comparative Example 2" refers to a case where mineral oil (aromatic type) is used as a property improver, specifically, Risei Cool Super (product name), a recycling additive manufactured by Santoku Shoji Co., Ltd., and the ratio of fatty acid: mineral oil is set to 75:25. "Comparative Example 3" refers to a case where vegetable oil (recycled waste edible oil) is used as a property improver and the ratio of fatty acid: vegetable oil is set to 75:25.

[0025] Meanwhile, the fatty acid pitch used as a property improving agent in the cold asphalt mixture according to this embodiment ("Example 1" in Table 2) is an industrial by-product (residue), and therefore is less expensive than the mineral oil that has been used conventionally, making it economical. In addition, it has advantages as a biomass material over petroleum-derived materials (for example, a renewable resource and the saving of petroleum resources). In terms of properties, it has been demonstrated in various tests described below that the cold asphalt mixture can ensure high fluidity resistance, aggregate scattering resistance, and deflection following ability, while also improving low-temperature workability, and that a good balance between these is maintained.

[0026] The evaluation of the cold asphalt mixture according to this embodiment (Example 1 in Table 2) will be explained below in comparison with Comparative Examples 1 to 3 in Table 2.

[0027] The evaluation summary is shown in Table 3.

[0028] [Table 3] As shown in Table 3, evaluations were conducted on the following four items:

[0029] 1) Ease of use: The pour point of the plasticizer components is one of the test items for workability during use. The test was carried out by air-cooling a 50g sample from 12.5 to -17.5°C in 2.5°C increments and checking the presence or absence of fluidity at each temperature. In this case, the pour point was determined to be the temperature just before the temperature at which fluidity was lost. If the temperature was -10°C or lower, the pour point was judged as ○ (good), if it was -10 to 0°C, the pour point was judged as △ (passable), and if it was 0°C or higher, the pour point was judged as × (not good).

[0030] 2) Deflection followability: The test items for the deflection follow-up property include a bending test. In this bending test, a specimen was prepared by spraying water at a temperature of 20°C, and the specimen was cured at a temperature of 20°C for 7 days, and then the test temperature was -10°C. As a result of this bending test, (bending strain x 10 -3 ) was judged as ○ (good) if it was 4 or more, as △ (passable) if it was 3 to 4, and as × (unacceptable) if it was less than 3.

[0031] 3) Aggregate scattering resistance: One test item for aggregate scattering resistance is the 20°C Cantablo test, in which water is sprayed at 20°C, the concrete is pressed 50 times on both sides, and after demolding, the concrete is left to harden and cure for 24 hours at 20°C, and then the test is performed at 20°C. As a result of this 20°C Cantablo test, if the loss rate is less than 10%, it is judged as ○ (good), if it is 10-20%, it is △ (passable), and if it is 20% or more, it is judged as × (unacceptable).

[0032] 4) Flow resistance: One test item for fluidity resistance is a wheel tracking test, in which a specimen is prepared by spraying water at a temperature of 20° C. on the specimen, which is then cured for 7 days at a temperature of 20° C., and then tested at a temperature of 60° C. As a result of this wheel tracking test, if the dynamic stability was 3000 times / mm or more, it was judged as ○ (good), if it was 1000 to 3000 times / mm, it was judged as △ (passable), and if it was less than 1000 times / mm, it was judged as × (unacceptable).

[0033] The 20°C Cantablo loss rate (%) obtained by the 20°C Cantablo test to evaluate the aggregate scattering resistance, the dynamic stability DS (times / mm) obtained by the wheel tracking (WT) test to evaluate the flow resistance, and the -10°C bending strain (×10 -3 ) and the pour point (° C.) of the plasticizer component for evaluating the workability during use are shown in Table 2 for Example 1 and Comparative Examples 1 to 3 in Table 4.

[0034] [Table 4] The results shown in Table 4 for each item obtained for Example 1 and Comparative Examples 1 to 3 are shown in Table 5 as ◯ (good), Δ (passable), or × (unacceptable).

[0035] [Table 5] As is clear from the evaluation results shown in Table 5, in Example 1, in which fatty acid and fatty acid pitch were used in combination as plasticizers, the deflection followability (bending strain) and aggregate scattering resistance (20°C cantabro loss rate) were improved compared to Comparative Example 1, in which only fatty acid was used alone, and the flow point of the plasticizer component of the asphalt (workability at low temperatures), which is an indicator of the workability of the asphalt mixture at room temperature, was also improved. On the other hand, in Example 1, although the flow resistance (dynamic stability) is lower than that of Comparative Example 1, it meets the standard value of the number of wheels for plastic deformation on roads with a planned pavement traffic volume of 3,000 vehicles / day or more.

[0036] Incidentally, when an oil-based property-improving agent is added to a room temperature asphalt mixture that utilizes the saponification reaction (neutralization reaction) of fatty acids to impart flexibility, the flexural compliance, aggregate scattering resistance (cantabro loss rate), and flow point of the plasticizer component (workability at low temperatures) improve, but there is a trade-off in properties where the flow resistance (dynamic stability) decreases.

[0037] However, Example 1 has a better balance of the trade-off than Comparative Example 2 in which mineral oil was used instead of fatty acid pitch, and Comparative Example 3 in which vegetable oil was used.

[0038] As a result of the above, it can be confirmed that the fatty acid pitch used in Example 1 is superior to other oil components in terms of its effect as a property improving agent.

[0039] Therefore, the room temperature asphalt mixture of this embodiment uses inexpensive fatty acid pitch, which is an industrial by-product (residue) of fatty acid production, as a property improvement agent, and by setting the fatty acid:fatty acid pitch ratio to 75:25, it is possible to achieve the effects of improving low-temperature workability and economy while maintaining high fluidity resistance, aggregate scattering resistance, and deflection tracking ability.

[0040] In particular, it was confirmed that low-temperature workability can be improved by using a combination of fatty acid + fatty acid pitch (vegetable oil) as a plasticizer. In other words, it was found that fatty acid alone will crystallize and solidify below a certain temperature, although the temperature varies depending on the composition. Therefore, it was confirmed that mixing with materials that are difficult to crystallize and have a low melting point, such as vegetable oil or mineral oil, inhibits the crystallization of fatty acid and lowers the solidification point.

[0041] By the way, in this embodiment, Fatty acid pitch: fatty acid ratio 25:75 However, it was confirmed that the same effect as above can be obtained by setting this ratio in the range of 40:60 to 5:95.

[0042] In addition, in the present invention, recycled aggregate obtained by crushing, adjusting the particle size, and classifying waste materials from asphalt pavement may be used to partially replace the crushed stone and sand shown in Table 1. By using recycled aggregate in this way, it is possible to further reduce the cost of cold asphalt mixtures.

[0043] In addition, the present invention is not limited to the application of the embodiments described above, and various modifications are possible within the scope of the claims and the technical ideas described in the specification.

Claims

1. A cold asphalt mixture comprising at least aggregate, asphalt, a plant-derived property improver which is fatty acid pitch, an industrial by-product of fatty acid production, a lubricating solidifier (a fatty acid and / or a fatty acid dimer and / or a fatty acid trimer, none of which contains pitch), and cement; A cold asphalt mixture characterized in that the ratio of the property improver to the lubricant solidifying agent is set in the range of 40:60 to 5:

95.

2. 2. The cold asphalt mixture according to claim 1, characterized in that recycled aggregate is mixed as a part of the aggregate.

Citation Information

Patent Citations

  • Removing of slag from interior of suction pipe immersed in molten metal bath

    JP1984016937A

  • Optical receiver

    JP1985089139A

  • Wakame seaweed containing root sea tangle

    JP1988044873A

  • Chrominance signal processing circuit for magnetic recording and reproducing device

    JP1989058194A

  • Recycling of recycled asphalt

    JP2015515536A