Aluminum alloy extruded material and method for manufacturing the same

The aluminum alloy extruded material with controlled composition and manufacturing process addresses high costs and mechanical weaknesses by achieving uniform mechanical properties and reduced extrusion pressure, enhancing productivity and formability.

JP7947956B2Active Publication Date: 2026-11-11RESONAC CORP
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
JP2022197959
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2022-12-12
Publication Date
2026-11-11
Estimated Expiration
2042-12-12

AI Technical Summary

Technical Problem

Existing aluminum alloy extrusion methods face challenges such as high production costs, non-uniform mechanical properties, and insufficient extrusion formability, leading to increased costs and potential mechanical weaknesses in certain directions.

Method used

An aluminum alloy composition with specific ranges of Si, Mg, Cu, Fe, Zr, and Ti, along with controlled Mg2Si particle densities and proof stresses, combined with a manufacturing process involving heating, extrusion, die quenching, and aging, to achieve uniform mechanical properties and reduced extrusion pressure.

Benefits of technology

The solution results in an aluminum alloy extruded material with improved mechanical properties, reduced production costs, and enhanced extrusion formability, ensuring consistent strength in the longitudinal direction and improved productivity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007947956000002
    Figure 0007947956000002
  • Figure 0007947956000003
    Figure 0007947956000003
  • Figure 0007947956000004
    Figure 0007947956000004
Patent Text Reader

Abstract

To provide an aluminum alloy extrusion material that can be produced at low cost and exhibits high tensile strength and proof stress.SOLUTION: An aluminum alloy extrusion material comprises Si: 0.90 mass% or more and 2.00 mass% or less, Mg: 0.65 mass% or more and 0.90 mass% or less, Cu: 0.25 mass% or more and 0.50 mass% or less, Fe: 0.050 mass% or more and 0.49 mass% or less, Zr: 0.10 mass% or more and 0.25 mass% or less, Ti: 0.010 mass% or more and 0.10 mass% or less, and B: at or below 1.0 times the mass of Ti, with the balance being Al and unavoidable impurities. In the lengthwise direction of the aluminum alloy extrusion material, 0.2% proof stress at a location equal to or more than 20% and less than 30% from one end, defined as α, is 300 MPa or more, 0.2% proof stress at a location equal to or more than 20% and less than 30% from the other end, defined as β, is 300 MPa or more, and the ratio of the α to the β is 0.95 or more and 1.05 or less.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical Field]

[0001] The present invention relates to aluminum alloy extruded material and a method for manufacturing the same. [Background technology]

[0002] Aluminum alloys are lightweight and strong, and in recent years their applications have expanded to include transportation equipment such as automobiles and railway vehicles, civil engineering and construction fields, as well as household goods such as furniture and daily necessities, and home appliances. There is a demand for further weight reduction of aluminum alloy materials through methods such as thinning the wall thickness, and for this reason, there is a need for further improvement in the strength of the material.

[0003] Patent Document 1 describes a method for manufacturing an aluminum-magnesium-silicon aluminum alloy extruded material, wherein the aluminum alloy contains 0.5-0.9% magnesium, 0.9-1.3% silicon, 0.3-0.5% iron, and 0.005-0.1% titanium by mass%, and further limits copper to 0.4% or less, manganese to 0.30% or less, chromium to 0.10% or less, and zirconium to 0.10% or less, with the remainder being aluminum and unavoidable impurities, and is extruded, then quenched by air cooling, further processing strain of 2-5% is introduced, and then artificial aging is performed.

[0004] Patent Document 2 describes an aluminum alloy extruded material having a chemical composition consisting of Si: 0.70~1.3% (mass%, the same applies hereinafter), Mg: 0.45~1.2%, Cu: less than 0.15~0.40%, Mn: 0.10~0.40%, Cr: 0.06% or less (excluding 0%), Zr: 0.05~0.20%, Ti: 0.005~0.15%, Fe: 0.30% or less, V: 0.01% or less, with the remainder being Al and unavoidable impurities, a yield strength of 350 MPa or more, a particle size of precipitates restricted to 5 μm or less, and an area ratio of fibrous structure in a cross section parallel to the hot extrusion direction of 95% or more.

[0005] Patent Document 3 describes an aluminum alloy extruded material for cutting work, which has a component composition consisting of Si: 0.8 to 2.0 mass%, Mg: 0.7 to 1.0 mass%, Cu: 0.3 to 1.0 mass%, Fe: ≤0.20 mass%, Mn: 0.2 to 0.8 mass%, Cr: 0.1 to 0.4 mass%, Mn+Cr: 0.3 to 0.9 mass%, with the balance being Al and unavoidable impurities, and in which the amounts of Mg and Si further satisfy the relational expression Mg / 1.73+0.2 ≤ Si ≤ Mg / 1.73+1.6, and the metal structure is a fiber structure.

Prior Art Documents

Patent Documents

[0006]

Patent Document 1

Patent Document 2

Patent Document 3

Summary of Invention

Problems to be Solved by the Invention

[0007] In Patent Document 1, a step of introducing processing strain after quenching is incorporated, and the number of steps is larger than that of ordinary processes, which tends to lead to high costs.

[0008] In Patent Document 2, the material has a fibrous structure in the extrusion direction, and the mechanical properties in the direction perpendicular to the extrusion direction may be inferior to those in the direction parallel to the extrusion direction.

[0009] In Patent Document 3, the extrusion formability is insufficient, it is necessary to increase the extrusion pressure to perform forming at a sufficient extrusion speed, and the strain of the extruded product tends to be large. Therefore, it tends to result in high costs in order to maintain the quality as an extruded material.

[0010] Accordingly, an object of the present invention is to provide an aluminum alloy extruded material with low cost and excellent mechanical properties, and a method for producing the same. MEANS FOR SOLVING THE PROBLEMS

[0011] The configuration of the present invention for solving the above problems is as follows.

[0012] [1] An aluminum alloy extruded material cut to a predetermined length, Si: 0.90 mass% or more and 2.00 mass% or less, Mg: 0.65 mass% or more and 0.90 mass% or less, Cu: 0.25 mass% or more and 0.50 mass% or less, Fe: 0.050 mass% or more and 0.49 mass% or less, Zr: 0.10 mass% or more and 0.25 mass% or less, Ti: 0.010 mass% or more and 0.10 mass% or less, B: 1.0 times or less of Ti on a mass basis, and the balance consisting of Al and unavoidable impurities, where, in the length direction of the aluminum alloy extruded material, the 0.2% proof stress at a position 20% or more and less than 30% from one end is defined as α, and the 0.2% proof stress at a position 20% or more and less than 30% from the other end is defined as β, the α is 300 MPa or more, the β is 300 MPa or more, and the ratio of α to β is 0.95 or more and 1.05 or less.

[0013] [2] An aluminum alloy extruded material cut to a predetermined length, Si: 0.90 mass% or more and 2.00 mass% or less, Mg: 0.65 mass% or more and 0.90 mass% or less, Cu: 0.25 mass% or more and 0.50 mass% or less, Fe: 0.050 mass% or more and 0.49 mass% or less, Zr: 0.10 mass% or more and 0.25 mass% or less, Ti: 0.010 mass% or more and 0.10 mass% or less, B: 1.0 times or less of Ti on a mass basis, and the balance consisting of Al and unavoidable impurities, When, in the longitudinal direction of the aluminum alloy extruded material, the density of Mg2Si particles with a particle size of 0.10 μm to 5.0 μm in a cross-section perpendicular to the extrusion direction at a position 20% to less than 30% from one end is denoted as γ, and the density of Mg2Si particles with a particle size of 0.10 μm to 5.0 μm in a cross-section perpendicular to the extrusion direction at a position 20% to less than 30% from the other end is denoted as δ, The aforementioned γ is 1.5 × 10 3 pieces / mm 2 The above 5.4 × 10 3 pieces / mm 2 The following: The aforementioned δ is 1.5 × 10 3 pieces / mm 2 The above 5.4 × 10 3 pieces / mm 2 The following: An aluminum alloy extruded material in which the ratio of γ to δ is 0.92 or more and 1.08 or less.

[0014] [3] comprising a collision wall panel, a back panel arranged substantially parallel to the collision wall panel, and a plurality of connecting panels connecting the collision wall panel and the back panel at predetermined intervals, An impact absorbing member wherein at least one of the collision wall plate, the back plate, and the connecting plate is made of the aluminum alloy extruded material described in item 1 or 2 above.

[0015] [4] A method for manufacturing an aluminum alloy extruded material as described in paragraph 1 or 2 above, The manufacturing method includes a heating step of a billet made of homogenized aluminum alloy, an extrusion step of extruding the heated billet to obtain an extruded material, a die quenching step of cooling the extruded material obtained by the extrusion process, and an aging step of artificially aging the cooled extruded material. The aforementioned billet has a diameter of 15 cm or more and a length of 30 cm or more. The heating step is performed such that the temperature of the leading end of the billet in the extrusion direction is 400°C or more and 500°C or less, the temperature of the ending end in the extrusion direction is 350°C or more and 450°C or less, and the temperature of the leading end in the extrusion direction is within a range of 60°C or less higher than the temperature of the ending end in the extrusion direction. In a cross section perpendicular to the extrusion direction at the front end in the extrusion direction of the billet heated by the heating step, the number density of Mg₂Si particles having a particle size of 0.10 μm or more and 5.0 μm or less is 1.6×10 3 particles / mm 2 or more and 2.0×10 3 particles / mm 2 or less, the die quenching step cools the billet to 150°C or less at a cooling rate of 7.0°C / sec or more and 80°C / sec or less, and the aging step is performed at 120°C or more and 240°C or less for 2 hours or more and 48 hours or less. A method for producing an aluminum alloy extruded material. [Effects of the Invention]

[0016] Since the aluminum alloy material having the composition described in the preceding paragraphs [1] and [2] is easily deformed by heating, the extrusion pressure can be reduced, the productivity of the aluminum alloy extruded material is improved, and the production cost can be reduced.

[0017] When the aluminum alloy extruded material has the composition, 0.2% proof stress value, and ratio of 0.2% proof stress values described in the preceding paragraph [1], uniform and excellent mechanical properties can be obtained in the longitudinal direction of the extruded material.

[0018] When the aluminum alloy extruded material has the composition, the number density of Mg₂Si particles, and the ratio of the number density of Mg₂Si particles described in the preceding paragraph [2], uniform and excellent mechanical properties can be obtained in the extrusion direction.

[0019] By the production method described in the preceding paragraph [4], an aluminum alloy extruded material having uniform and excellent mechanical properties in the longitudinal direction of the extruded material can be obtained.

[0020] Therefore, according to the present invention, it is possible to provide an aluminum alloy extruded material having uniform and excellent mechanical properties in the longitudinal direction of the extruded material at low cost, and a production method thereof. [Brief Description of the Drawings]

[0021] [Figure 1] Figure 1 shows an example of an aluminum alloy extruded material. [Figure 2] Figure 2 shows an example of a scanning electron microscope (SEM) photograph of a cross-section perpendicular to the extrusion direction of an aluminum alloy extruded material according to one embodiment of the present invention. [Figure 3] Figure 3 shows the image obtained by binarizing the photograph in Figure 2. [Figure 4] Figure 4 is a plan view showing an example of an impact-absorbing member manufactured using an aluminum alloy extruded material according to this embodiment. [Figure 5] Figure 5 is a flow chart showing an example of a method for manufacturing an aluminum alloy extruded material according to one embodiment of the present invention. [Figure 6] Figure 6 shows the extrusion cross-section of the die used in each embodiment and comparative example. [Figure 7] Figure 7 shows the aluminum alloy extruded materials produced in each example and comparative example. [Modes for carrying out the invention]

[0022] Embodiments of the present invention will be described below.

[0023] In the following explanation, unless otherwise specified, the terms "extruded material" and "aluminum alloy extruded material" refer to aluminum alloy extruded material.

[0024] <1. Aluminum alloy extruded material> The chemical composition of the aluminum alloy extruded material according to this embodiment consists of Si, Mg, Cu, Fe, Zr, Ti, B, and the remainder, in the amounts described below, with the remainder being Al and unavoidable impurities. As will be described later, the extruded material according to this embodiment does not need to contain B. That is, the extruded material according to this embodiment may have a chemical composition consisting of Si, Mg, Cu, Fe, Zr, Ti, B, and the remainder (Al and unavoidable impurities), or it may have a chemical composition consisting of Si, Mg, Cu, Fe, Zr, Ti, and the remainder (Al and unavoidable impurities).

[0025] [1-1. Components of aluminum alloy extruded material] [1-1-1.Si] The Si content in the extruded material is 0.90% by mass or more, preferably 1.03% by mass or more, and more preferably 1.05% by mass or more. This is because Si readily forms compounds through interaction with Mg, and the formation of Mg2Si precipitates contributes to improving the strength of the extruded material. Furthermore, by adding Si in excess of the amount of Mg added (described later) to the amount required to produce Mg2Si, the properties such as strength of the extruded material after artificial aging treatment (the aging process described later) can be further enhanced.

[0026] The Si content in the extruded material may be 1.30% by mass or more, or 1.50% by mass or more.

[0027] The Si content in the extruded material is 2.00% by mass or less, and preferably 1.78% by mass or less. This is because it suppresses the precipitation of individual Si particles at grain boundaries and further enhances the toughness of the extruded material. It also reduces the extrusion pressure and improves productivity and yield.

[0028] The Si content in the extruded material may be 1.50% by mass or less, or 1.25% by mass or less.

[0029] [1-1-2.Mg] The Mg content in the extruded material is 0.65% by mass or more, preferably 0.70% by mass or more, more preferably 0.72% by mass or more, and even more preferably 0.74% by mass or more. This is because Mg readily forms compounds through interaction with Si, and the formation of Mg2Si precipitates contributes to improving the strength of the extruded material.

[0030] The Mg content in the extruded material is 0.90% by mass or less, preferably 0.88% by mass or less, and more preferably 0.83% by mass or less. This is because, by keeping the amount of precipitates within an appropriate range, the quenchability is improved and the pressure rise during extrusion is suppressed. Furthermore, the generated Mg2Si precipitates are made easier to solidify at low temperatures, thereby further improving the accuracy of the shape of the product (extruded material).

[0031] [1-1-3.Cu] The Cu content in the extruded material is 0.25% by mass or more, preferably 0.28% by mass or more, more preferably 0.32% by mass or more, and even more preferably 0.36% by mass or more. This is because the inclusion of Cu increases the apparent supersaturation of Mg2Si precipitates and increases the amount of Mg2Si precipitates, thereby improving the age-hardening properties of the extruded material. Furthermore, the fine precipitation of Cu-containing compounds within the crystal grains contributes to improved strength.

[0032] The Cu content in the extruded material is 0.50% by mass or less, preferably 0.45% by mass or less, and more preferably 0.42% by mass or less. This is because it improves extrusion processability and enables extrusion molding at lower extrusion pressures. It also improves the corrosion resistance of the extruded material.

[0033] [1-1-4.Fe] The Fe content in the extruded material is 0.050% by mass or more, preferably 0.080% by mass or more, more preferably 0.10% by mass or more, and even more preferably 0.13% by mass or more. This is because Fe combines with Al and Si to crystallize during casting and also has the effect of suppressing grain coarsening.

[0034] The Fe content in the extruded material is 0.49% by mass or less, preferably 0.45% by mass or less, more preferably 0.35% by mass or less, even more preferably 0.30% by mass or less, even more preferably 0.27% by mass or less, and particularly preferably 0.24% by mass or less. This is to suppress the crystallization of needle-shaped Al-Fe-Si compounds and to further improve extruderability and the toughness of the extruded product.

[0035] [1-1-5.Zr] Zr precipitates as Zr-containing fine particles during homogenization and becomes a nucleus for crystal grains generated during extrusion. The Zr content in the extruded material is 0.10% by mass or more, preferably 0.11% by mass or more, and more preferably 0.13% by mass or more. This is because it increases the number of Zr-containing fine particles, i.e., nuclei for recrystallization, and suppresses the coarsening of crystal grains, which will be discussed later.

[0036] The Zr content in the extruded material is 0.25% by mass or less, preferably 0.20% by mass or less, and more preferably 0.17% by mass or less. This is because it improves the fluidity of the molten alloy during casting, facilitating the formation of the extruded material by casting, and consequently improving the productivity of the extruded material.

[0037] [1-1-6.Ti] Ti has the effect of refining the crystal grains during casting, and in addition, it has the effect of suppressing ingot cracking during casting. The Ti content in the extruded material is 0.010% by mass or more, preferably 0.020% by mass or more, and more preferably 0.025% by mass or more.

[0038] The Ti content in the extruded material is 0.10% by mass or less, preferably 0.085% by mass or less, and more preferably 0.060% by mass or less. This is because it improves the fluidity of the molten alloy during casting, facilitating the formation of the extruded material by casting, and consequently improving the productivity of the extruded material.

[0039] [1-1-7.B] Like Ti, B is also effective in refining crystal grains, and it is thought that adding it generates and disperses TiB2 particles. Furthermore, it is thought that the TiB2 particles act as solidification nuclei for the crystals, leading to the refinement of crystal grains described later. B may or may not be included. Here, "not containing B" means not containing B other than unavoidable impurities, and B as an unavoidable impurity may be included. When B is included, the B content in the extruded material is preferably 0.050 times or more by mass of Ti, more preferably 0.10 times or more, and even more preferably 0.15 times or more. The reason for this is to suppress the coarsening of crystal grains, described later.

[0040] The B content in the extruded material is preferably 1.0 times or less by mass, more preferably 0.50 times or less, and more preferably 0.25 times or less, compared to Ti. This is because excess B suppresses the binding of with Mg, thereby suppressing the consumption of Mg that should be binding with Si.

[0041] [1-1-8. Other Elements] As unavoidable impurities in the extruded material, for example, it is preferable to reduce the content of Mn and Cr as much as possible. This is because it reduces the susceptibility to hardening, minimizes the effect of variations in cooling rate on strength, and makes the quality of the extruded material more stable. Specifically, the content of Mn and Cr is preferably less than 0.05% by mass, more preferably less than 0.01% by mass, and most preferably less than 0.0005% by mass or not present at all.

[0042] [1-2.0.2% proof stress] Figure 1 shows an example of an aluminum alloy extruded material.

[0043] The aluminum alloy extruded material is cut to a predetermined length, for example, about 5 meters, for easier handling.

[0044] In this embodiment, when the aluminum extruded material has a 0.2% yield strength of α at a position 20% or more but less than 30% from one end in the longitudinal direction (extrusion direction), and a 0.2% yield strength of β at a position 20% or more but less than 30% from the other end, it is preferable that α is 300 MPa or more, β is 300 MPa or more, and the ratio of α to β is 0.95 or more but less than 1.05.

[0045] Here, the 0.2% yield strength is the value measured by the method described in the examples below (the value obtained using a No. 5 test specimen (dimensions will be described below) according to JIS Z 2241).

[0046] In this invention, in an aluminum alloy extruded material of a predetermined length that has been cut, the present invention focuses on two positions: one 20% to less than 30% from one end and another 20% to less than 30% from the other end. By ensuring a 0.2% yield strength of 300 MPa or more at both of these positions, high mechanical properties are secured.

[0047] Furthermore, in this invention, the ratio of the 0.2% yield stress at both positions (α / β) is 0.95 or more and 1.05 or less, thereby ensuring uniformity of the mechanical properties in the longitudinal direction of the aluminum alloy extruded material.

[0048] [1-3.Mg2Si particles] Figure 2 shows an example of a scanning electron microscope (SEM) photograph (Example 1) of a cross-section perpendicular to the extrusion direction of an aluminum alloy extruded material according to one embodiment of the present invention. Here, Mg2Si particles are particles identified by quantitative analysis of the amount of each element in EDX mapping in the same field of view. Specifically, Mg2Si particles are defined in this analysis as particles with a Mg content of 30 mass% to 80 mass%, a Si content of 10 mass% to 40 mass%, and the remainder being Al (which may include unavoidable impurities; the total content of Mg and Si may be 100 mass% (no remainder)), and a mass-based ratio of Mg to Si, Mg / Si, of 1.5 to 2.5. The black dots in the photograph in Figure 2 are Mg2Si particles.

[0049] Figure 3 is a binarized version of the photograph in Figure 2. The particle size of the Mg2Si particles is between 0.10 μm and 5.0 μm (particles outside this size range are not Mg2Si particles in this invention). The particle size of the Mg2Si particles is determined based on the binarized image of the SEM. The particle size of the Mg2Si particles is the diameter calculated from the area of ​​the black areas in the binarized image, which are treated as circles.

[0050] In this embodiment, when the aluminum extruded material has a density of Mg2Si particles with a particle size of 0.10 μm to 5.0 μm in a cross-section perpendicular to the extrusion direction at a position 20% to less than 30% from one end in the longitudinal direction (extrusion direction), and the density of Mg2Si particles with a particle size of 0.10 μm to 5.0 μm in a cross-section perpendicular to the extrusion direction at a position 20% to less than 30% from the other end, then γ is 1.5 × 10⁻⁶ 3 pieces / mm 2 The above 5.4 × 10 3 pieces / mm 2 The following applies, where δ is 1.5 × 10 3 pieces / mm 2 The above 5.4 × 10 3 pieces / mm 2 The following conditions apply, and it is preferable that the ratio of γ to δ is 0.92 or more and 1.08 or less.

[0051] The aforementioned γ and δ are 2.0 × 10 3 pieces / mm 2 More preferably, the above is 2.4 × 10 3 pieces / mm 2 It is even more preferable that the above conditions are met, because the solid solution of Mg is suppressed, and the extrudeability is improved.

[0052] The values ​​of γ and δ are 5.2 × 10 3 pieces / mm 2 It is more preferable that the following conditions apply: 4.7 × 10 3 pieces / mm 2 The following is even more preferable, as it improves the yield strength of the extruded material.

[0053] The number of Mg2Si particles was determined using a JEOL JSM-7000F field emission scanning electron microscope at a magnification of 1,000x, with a field of view of 121 μm × 90.9 μm = 10,998.9 μm. 2 These can be counted in four fields of view. The density of Mg2Si particles can be calculated by dividing the total number of Mg2Si particles (NM) in the four fields of view by the area of ​​the four fields of view. That is, the density of Mg2Si particles is NM / (4 × 10⁹⁹⁸) [particles / μm]. 2 ]=10 6 ×NM / (4×10998.9)[pcs / mm 2 ]

[0054] In this invention, in an aluminum alloy extruded material of a predetermined length that has been cut, we focus on a position 20% to less than 30% from one end and a position 20% to less than 30% from the other end, and set the density of Mg2Si particles of a predetermined size at both of these positions to 1.5 × 10⁻⁶. 3 pieces / mm 2 The above 5.4 × 10 3 pieces / mm 2 High mechanical properties are ensured by the following:

[0055] Furthermore, in this invention, the uniformity of mechanical properties in the longitudinal direction of the aluminum alloy extruded material is ensured by having a density of Mg2Si particles (γ / δ) of 0.92 or more and 1.08 or less at both positions.

[0056] [1-4. Impact absorbing material] The aluminum alloy extruded material according to this embodiment is suitable as an impact absorbing member.

[0057] The impact-absorbing members of this embodiment can be applied to, for example, beam materials such as front pillars, center pillars, and rear pillars, frame materials such as side members and bumper stays, bumper reinforcements, crash boxes, battery cases, front underrun protectors, and rear underrun protectors in vehicles such as automobiles, but are not limited to these applications and can also be applied to impact-absorbing structures in railway vehicles and the like.

[0058] Figure 4 is a plan view showing an example of an impact-absorbing member manufactured using an aluminum alloy extruded material according to this embodiment.

[0059] As shown in this figure, the impact absorbing member 2 comprises a collision wall plate 3, a back plate 4 arranged substantially parallel to the collision wall plate 3, and a plurality of connecting plates 5, 5 that connect the collision wall plate 3 and the back plate 4 at predetermined intervals.

[0060] The collision wall panel 3, the back panel 4, and the connecting panels 5, 5 may all be made of the aluminum alloy material according to this embodiment, or only a part of them may be made of the aluminum alloy material according to this embodiment.

[0061] <2. Method for manufacturing aluminum alloy extruded material> Figure 5 is a flow chart showing an example of a method for manufacturing an aluminum alloy extruded material according to one embodiment of the present invention. An example of a method for manufacturing an aluminum alloy extruded material according to one embodiment of the present invention will be described below, but the method for manufacturing the extruded material according to the present invention is not limited to this example.

[0062] As shown in Figure 5, the method for manufacturing an aluminum alloy extruded material according to one example of this embodiment includes a melting step, a casting step, a homogenization step, a heating step, an extrusion step, a die quenching step, and an aging step. However, not all of these steps are necessarily required; for example, if the material after casting is available, the melting step and casting step are unnecessary, and if the material after homogenization is available, each step up to the homogenization step is unnecessary.

[0063] [2-1. Melting Process] In the melting process, molten aluminum alloy is prepared. The chemical composition of the molten metal is preferably the same as the chemical composition of the aluminum alloy extruded material to be obtained, and the elements contained in the aluminum alloy extruded material are as described above.

[0064] [2-2. Casting Process] In the casting process, billets (extrusion material) are obtained by casting the molten metal obtained in the melting process. The casting method is not particularly limited, but examples include vertical float continuous casting, vertical hot-top continuous casting, and horizontal continuous casting.

[0065] The billet size is preferably 15 cm or more in diameter and 30 cm or more in length.

[0066] [2-3. Homogenization process] In the homogenization process, a homogenization treatment is performed to homogenize the metal structure of the billet obtained in the casting process and to sufficiently dissolve the atoms contained in the aluminum alloy. A high-strength extruded material can be obtained through the homogenization process. The chemical composition of the aluminum alloy (billet) used in the homogenization process is preferably the same as the chemical composition of the aluminum alloy extruded material to be obtained, and the elements contained in the aluminum alloy extruded material are as described above.

[0067] The homogenization treatment temperature is preferably 500°C or higher, more preferably 530°C or higher, and even more preferably 550°C or higher. This is to sufficiently homogenize the metal structure of the billet and to sufficiently solid-solve the atoms contained in the aluminum alloy. The homogenization treatment temperature is preferably 600°C or lower, and more preferably 570°C or lower. This is to suppress the melting of intermetallic compounds, thereby suppressing the coarsening of the intermetallic compound particles and improving the mechanical properties of the extruded material.

[0068] The homogenization treatment time is preferably 3 hours or more, more preferably 8 hours or more, and even more preferably 12 hours or more. This is to sufficiently homogenize the metal structure of the billet and to sufficiently solid dissolve the atoms contained in the aluminum alloy. The homogenization treatment time is preferably 24 hours or less, more preferably 20 hours or less, and even more preferably 18 hours or less. This is to suppress the coarsening of intermetallic compound particles and improve the mechanical properties of the extruded material.

[0069] It is preferable to cool the billet after homogenization. The temperature of the billet after cooling is preferably 150°C or lower, and more preferably 100°C or lower. The billet may also be cooled to 50°C or lower for storage. Cooling methods include, but are not limited to, water cooling, mist cooling, air cooling, fan cooling, and air cooling. The cooling rate is preferably 100°C / h or higher, and more preferably 150°C / h or higher.

[0070] [2-4. Heating process] In the heating process, the homogenized billet is heated to reduce its deformation resistance. The heating process also causes the components constituting the billet to solidify. The elements and their content in the aluminum alloy material constituting the billet used in the heating process are as described above in the description of the aluminum alloy extruded material.

[0071] In the aluminum alloy extruded material of this embodiment, as described above, the density of Mg2Si particles with a particle size of 0.10 μm or more and 5.0 μm or less is ultimately 1.5 × 10⁻⁶. 3 pieces / mm 2 The above 5.4 × 10 3 pieces / mm 2 One of our goals is to keep it within the following range.

[0072] It is desirable to precipitate Mg2Si particles in this extruded material during the aging process described later. This is to appropriately control the particle size and density of the precipitated Mg2Si particles.

[0073] Therefore, it is desirable to ensure that Mg2Si particles are not present in the aluminum alloy material before the aging process. If Mg2Si particles are present in the aluminum alloy material before the aging process, the amount of Mg and Si dissolved in the aluminum alloy material will decrease, making it impossible to sufficiently precipitate Mg2Si particles during the aging treatment.

[0074] To prevent the presence of Mg2Si particles in the aluminum alloy material before the aging process, it is desirable to pass the extrusion process through a predetermined temperature range to cause the Mg2Si particles to solid-solve as Mg and Si.

[0075] The heating temperature in the heating process takes into account the heat generated during the extrusion process by the billet itself and the heating of the material due to friction with the die, etc. However, if the heating temperature is too low, the deformation resistance of the billet in the extrusion process will increase.

[0076] On the other hand, if the heating temperature in the heating process is too high, the Mg2Si particles will grow excessively and become coarse during the heating process, making it impossible to sufficiently solid-solve the Mg2Si particles as Mg and Si in the extrusion process.

[0077] Furthermore, in the initial stages of extrusion, the amount of heat generated by the billet itself during processing and by friction with the die is lower compared to the later stages. Therefore, if the heating temperature in the heating process is the same throughout the entire extrusion direction, the leading end of the extrusion direction may not be able to reach the required temperature during the extrusion process, potentially preventing sufficient solid solution of Mg2Si particles as Mg and Si. Alternatively, the end of the extrusion direction may become too hot during the extrusion process.

[0078] Therefore, in this embodiment, the heating temperature in the heating process is set to 400°C to 500°C at the leading end of the billet in the extrusion direction, and to 350°C to 450°C at the ending end in the extrusion direction, with the temperature at the leading end being higher than the temperature at the ending end.

[0079] By making the temperature at the leading end of the extrusion direction higher than the temperature at the ending end of the extrusion direction, the Mg2Si particles can be sufficiently dissolved as Mg and Si even in the initial stages of extrusion, and the temperature at the ending end of the extrusion direction can be prevented from becoming too high.

[0080] Furthermore, the above heating temperature prevents the billet from becoming excessively deformable during the extrusion process, and also prevents the Mg2Si particles from growing excessively and becoming coarse during the heating process.

[0081] It is preferable that the temperature difference between the leading and trailing ends of the billet in the extrusion direction be 60°C or less. This is because if the temperature difference exceeds 60°C, Mg2Si particles tend to grow excessively at the leading end of the billet during the heating process.

[0082] On the other hand, it is preferable that the temperature difference between the leading and trailing ends of the billet in the extrusion direction be 15°C or more. This is because the billet may become too hot near the trailing end during extrusion.

[0083] In the heating process, the billet that has undergone the heating process at the above heating temperature has a density of Mg2Si particles with a particle size of 0.10 μm or more and 5.0 μm or less at the leading edge of the billet in the extrusion direction, in a cross section perpendicular to the extrusion direction, of 1.6 × 10⁻¹⁴ 3 pieces / mm 2 The above 2.0 × 10 3 pieces / mm 2 The following is preferable:

[0084] If the density of Mg2Si particles is as described above during the heating process, then in the extrusion process, the Mg2Si particles can be sufficiently dissolved as Mg and Si, ensuring that Mg and Si are dissolved in the aluminum alloy material before the aging process, and the particle size and density of Mg2Si particles precipitated during the aging process can be appropriately controlled.

[0085] [2-5. Extrusion Process] In the extrusion process, the billet heated in the heating process is extruded to obtain an extruded material. Specifically, for example, the billet heated in the heating process is loaded into a container and pressed against an extrusion mold (hereinafter referred to as a die) having a predetermined opening shape to obtain an extruded material having a desired cross-sectional shape. The extruded material according to this embodiment preferably has a hollow shape. The extrusion speed is preferably 5.0 m / min or more, and more preferably 6.5 m / min or more. This is because it puts strain on the material, making it easier to form a metallic structure with crystal grains of a predetermined shape. It also improves the productivity of the extruded material.

[0086] Furthermore, as described above, during the extrusion process, the billet itself heats up due to processing heat and friction with the die, causing the Mg2Si particles contained in the billet to dissolve as Mg and Si in the aluminum alloy material.

[0087] [2-6. Die Quench Process] In the die quenching process, the extruded material obtained by the extrusion process is cooled. The cooling method is not particularly limited, but examples include water cooling, mist cooling, fan cooling, and air cooling. A supersaturated solid solution is formed in the die quenching process. The cooling rate is 7.0°C / sec or higher, preferably 10°C / sec or higher, and more preferably 12°C / sec or higher. This is because it suppresses the precipitation of the solid-solution components and makes it easier to maintain the supersaturated solid solution. It also improves the productivity of the extruded material.

[0088] The cooling rate should be 80°C / sec or less, preferably 40°C / sec or less, and more preferably 20°C / sec or less. This is to suppress deformation of the extruded material due to thermal shrinkage during cooling.

[0089] The target temperature for the die quenching process is 150°C or lower, preferably 100°C or lower, and more preferably 50°C or lower.

[0090] After the die quenching process, the extruded material may be stored at room temperature, for example, below 30°C, until the aging process described later. The time from the die quenching process to the aging process (natural aging process) is preferably within 72 hours. Although aging progresses even at room temperature, it will not affect the subsequent metal structure or mechanical properties if kept within 72 hours.

[0091] [2-7. Aging Process] In the aging process, the extruded material, which has been cooled in the die quenching process, is subjected to artificial aging treatment. The aging process promotes the growth of Mg2Si-based precipitates in the extruded material, improving its strength.

[0092] The aging treatment temperature is 120°C or higher, preferably 140°C or higher, and more preferably 160°C or higher. This is because it facilitates the precipitation of Mg2Si-based precipitates in the extruded material. The aging treatment temperature is 240°C or lower, preferably 220°C or lower, and more preferably 200°C or lower. This is because it suppresses the excessive growth of Mg2Si-based precipitates in the extruded material and improves the strength of the extruded material.

[0093] The aging treatment time is 2 hours or more, preferably 4 hours or more, and more preferably 5 hours or more. This is to allow sufficient precipitation of Mg2Si-based precipitates. The aging treatment time is 48 hours or less, preferably 16 hours or less, and more preferably 8 hours or less. This is to suppress the excessive growth of Mg2Si-based precipitates in the extruded material and improve the strength of the extruded material. It also improves the productivity of the extruded material. [Examples]

[0094] The aluminum alloy extruded material and its manufacturing method according to the present invention will be described in more detail below with reference to examples and comparative examples, but the present invention is not limited thereto.

[0095] <1. Fabrication of aluminum alloy extruded materials> Using an aluminum alloy consisting of Si:0.94 mass%, Mg:0.73 mass%, Cu:0.38 mass%, Fe:0.26 mass%, Zr:0.14 mass%, Ti:0.042 mass%, B:0.004 mass%, with the remainder being aluminum and unavoidable impurities, a billet with a circular cross-section and a diameter of 156 mm was produced by continuous casting.

[0096] The B content of 0.004 mass% is 0.095 times the Ti content of 0.042 mass% on a mass basis.

[0097] The obtained billets were subjected to a homogenization treatment at 560°C for 14 hours. The billets were then cooled to 30°C at 180°C / h. Next, prior to the extrusion process, the cooled billets were heated (heating process). Table 1 shows the tip temperature, trailing end temperature, and temperature difference between the tip and trailing end of the billets for each example and comparative example during this heating process.

[0098] [Table 1]

[0099] Figure 6 shows the extrusion cross-section (extrusion hole) of the die used in each embodiment and comparative example. In each embodiment and comparative example, the extruded material 1 shown in Figure 7 is formed using this die D1. This extruded material 1 is a hollow extruded material in which a partition wall 12 that divides the interior (hollow part) into two is integrally formed on the outer wall 11 which has a rectangular cross-section.

[0100] The die D1 shown in Figure 6 is equipped with an extrusion hole D10 having an outer wall forming hole D11 for forming the outer wall 11 of the extruded material 1, and an inner partition wall forming hole D12 for forming the inner partition wall 12. The outer wall forming hole D11 of this die D1 has a horizontal dimension L1 of 150 mm and a vertical dimension L2 of 125 mm. Furthermore, the width T1 of the outer wall forming hole D11 and the inner partition wall 12 is 5.5 mm, the inner radius of curvature Ri in the outer wall forming hole D11 is 3 mm, and the outer radius of curvature Ro is 6 mm.

[0101] In each example and comparative example, a billet heated to the billet temperature shown in Table 1 was extruded using die D1 shown in Figure 6 in an 8-inch direct extruder. The extrusion speed in each example and comparative example during this extrusion process was 8.0 m / min. The length of the extruded material was 33.4 m.

[0102] Immediately after the extrusion process, the temperature was cooled to 40°C at a cooling rate of 30°C / sec (die quenching process).

[0103] The extruded material after the die quenching process was cut into 5m lengths.

[0104] The extruded material after the die quenching process was subjected to artificial aging treatment (aging process) at 180°C for 6 hours to obtain an aluminum alloy extruded material of a predetermined length (5 m). In the following description, unless otherwise specified, the extruded material refers to the aluminum alloy extruded material obtained after the aging process. Furthermore, the aluminum alloy extruded material after the aging treatment becomes the aluminum alloy extruded material according to the present invention.

[0105] <2.Various measurements> [2-1. Measurement of the abundance density of Mg2Si particles in billets] In each example and comparative example, the temperature history (heating rate and holding time) of the leading edge in the extrusion direction of the billet during the heating process was measured using a thermocouple. Subsequently, a 1 cm cube-shaped test specimen was cut from another billet (equivalent to the billet used in each example and comparative example) before the heating process, and the temperature history measured for this test specimen was reproduced in a laboratory heat treatment furnace. The test specimen was then rapidly cooled to fix its state at the end of the heating process. This test specimen was cut perpendicular to the extrusion direction, and an observation cross-section was formed using a JEOL cross-section polisher.

[0106] Using a JEOL JSM-7000F field emission scanning electron microscope, at a magnification of 1,000x, the area measured was 121 μm × 90.9 μm = 10998.9 μm. 2 Four images of the field of view were acquired, and EDX mapping analysis was performed.

[0107] Using the obtained mapping analysis results and binarized images (e.g., Figure 3), the number of Mg2Si particles with a particle size between 0.10 μm and 5.0 μm was counted across four fields of view. The density of Mg2Si particles was calculated by dividing the number of counted Mg2Si particles by the area of ​​the four fields of view. The definition of counted Mg2Si particles is as described above.

[0108] Table 1 shows the density of Mg2Si particles measured for the billets used in each example and comparative example.

[0109] [2-2. Measurement of 0.2% yield strength of extruded materials] Test specimens were cut from the aluminum alloy extruded material obtained in each example and comparative example at positions 21% from one end and 20% from the other end in the longitudinal direction (extrusion direction), and measured according to the method specified in JIS Z 2241. The measurement was performed on test specimen No. 5.

[0110] In this invention, a test piece cut from the 21% position from one end means a test piece that includes the 21% position from one end in its middle section.

[0111] The specific test specimens were cut along the extrusion direction with a gauge length of 50 mm, a parallel section length of 60 mm, a width of 25 mm, a thickness of 2 mm, and a shoulder radius of 30 mm. Tensile strength was calculated by performing a tensile test (in accordance with JIS Z 2241) at room temperature (24°C) with a crosshead speed of 2 mm / min, and the 0.2% yield stress was measured using the offset method.

[0112] Table 1 shows the 0.2% yield stresses α and β measured for each example and comparative example, with α being the 0.2% yield stress at a position 21% from one end in the longitudinal direction (extrusion direction), and β being the 0.2% yield stress at a position 20% from the other end.

[0113] Furthermore, Table 1 shows the ratio α / β of the 0.2% yield strength α at a position 21% from one end to the 0.2% yield strength β at a position 20% from the other end.

[0114] [2-3. Measurement of the abundance density of Mg2Si particles in extruded material] From the aluminum alloy extruded material obtained in each example and comparative example, test specimens were cut at 21% from one end and 20% from the other end in the longitudinal direction (extrusion direction). The cut specimens were then cut perpendicular to the extrusion direction, and a cross-section for observation was formed using a JEOL cross-section polisher. Using a JEOL field emission scanning electron microscope JSM-7000F, at a magnification of 1,000x, the cross-section was 121 μm × 90.9 μm = 10998.9 μm. 2 Four images of the field of view were acquired, and EDX mapping analysis was performed.

[0115] Using the obtained mapping analysis results and binarized images (e.g., Figure 3), the number of Mg2Si particles with a particle size between 0.10 μm and 5.0 μm was counted in NM across four fields of view. The density of Mg2Si particles was calculated by dividing the counted number of Mg2Si particles in NM by the area of ​​the four fields of view. The definition of a countable Mg2Si particle is as described above.

[0116] Table 1 shows the Mg2Si particle densities γ and δ measured for each example and comparative example. The density of Mg2Si particles with a particle size of 0.10 μm to 5.0 μm was determined as γ in a cross-section perpendicular to the extrusion direction at a position 21% from one end in the length direction (extrusion direction), and the density of Mg2Si particles with a particle size of 0.10 μm to 5.0 μm was determined as δ in a cross-section perpendicular to the extrusion direction at a position 20% from the other end.

[0117] Furthermore, Table 1 shows the ratio γ / δ of the abundance density γ of Mg2Si particles at a position 21% from one end to the abundance density δ of Mg2Si particles at a position 20% from the other end.

[0118] <3. Evaluation> The aluminum alloys in each embodiment exhibit excellent extrudeability. Therefore, the productivity of the aluminum alloy extruded materials in each embodiment can be improved, and as a result, the manufacturing cost of the extruded materials can be reduced. Furthermore, the aluminum alloy extruded materials in each embodiment all have high 0.2% yield strengths α and β at both ends, and their ratio α / β is close to 1, indicating high uniformity in the extrusion direction. In addition, the aluminum extruded materials in each embodiment all have Mg2Si densities γ and δ at both ends, and their ratio γ / δ is close to 1, indicating high uniformity in the extrusion direction.

[0119] Comparative Examples 1 and 2 have a large temperature difference between the billet tip and end, and a high density of Mg2Si at the billet tip. As a result, the extruded materials of Comparative Examples 1 and 2 have a ratio of 0.2% yield strength α / β between one end and the other end that is considerably less than 1, indicating low uniformity in the extrusion direction, and the ratio of Mg2Si density γ / δ between one end and the other end is considerably greater than 1, indicating low uniformity in the extrusion direction.

[0120] Comparative Example 3 has an extremely high temperature at the billet tip and an extremely high density of Mg2Si at the billet tip. As a result, the extruded material of Comparative Example 3 has a ratio of α / β of 0.2% yield strength between one end and the other end that is considerably less than 1, a high density of Mg2Si at one end, a ratio of γ / δ of Mg2Si density between one end and the other end that is considerably greater than 1, and considerably low uniformity in the extrusion direction.

[0121] Comparative Example 4 has an extremely high billet end temperature, a small temperature difference between the billet tip and end, and a high density of Mg2Si at the billet tip. As a result, the extruded material of Comparative Example 4 has a ratio of α / β of 0.2% yield strength between one end and the other end that is considerably greater than 1, and a ratio of γ / δ of Mg2Si density between one end and the other end that is considerably less than 1, resulting in considerably low uniformity in the extrusion direction.

[0122] From the above, it can be seen that the aluminum alloy extruded material according to the present invention is low-cost, has high yield strength, and exhibits high uniformity of mechanical properties in the extrusion direction. Furthermore, it can be seen that the method for manufacturing the aluminum alloy extruded material according to the present invention yields an aluminum alloy extruded material that is low-cost, has high yield strength, and exhibits high uniformity of mechanical properties in the extrusion direction. [Industrial applicability]

[0123] The aluminum alloy extruded material of this invention can be used as a high-strength structural material. [Explanation of Symbols]

[0124] 1: Aluminum alloy extruded material 2: Impact absorbing material 3: Collision wall plate 4: Back plate 5: Connecting plate

Claims

1. An aluminum alloy extruded material cut to a predetermined length, Si: 0.90% by mass or more and 2.00% by mass or less, Mg: 0.65% by mass or more and 0.90% by mass or less, Cu: 0.25% by mass or more and 0.50% by mass or less, Fe: 0.050% by mass or more and 0.49% by mass or less, Zr: 0.10% by mass or more and 0.25% by mass or less, Ti: 0.010% by mass or more and 0.10% by mass or less, B: Less than 1.0 times Ti by mass basis, The remainder consists of Al and unavoidable impurities. When the 0.2% proof stress of the aluminum alloy extruded material is α at a position 20% or more but less than 30% from one end in the longitudinal direction, and β at a position 20% or more but less than 30% from the other end, The above α is 300 MPa or more, The above β is 300 MPa or more, An aluminum alloy extruded material in which the ratio of α to β is 0.95 or more and 1.05 or less.

2. An aluminum alloy extruded material cut to a predetermined length, Si: 0.90% by mass or more and 2.00% by mass or less, Mg: 0.65% by mass or more and 0.90% by mass or less, Cu: 0.25% by mass or more and 0.50% by mass or less, Fe: 0.050% by mass or more and 0.49% by mass or less, Zr: 0.10% by mass or more and 0.25% by mass or less, Ti: 0.010% by mass or more and 0.10% by mass or less, B: Less than 1.0 times Ti by mass basis, The remainder consists of Al and unavoidable impurities. In the longitudinal direction of the aluminum alloy extruded material, at a position between 20% and less than 30% from one end, the Mg particles with a particle size of 0.10 μm to 5.0 μm are present in a cross section perpendicular to the extrusion direction. 2 Let γ be the density of Si particles. At a position 20% to less than 30% from the other end, in a cross section perpendicular to the extrusion direction, Mg particles with a particle size of 0.10 μm to 5.0 μm are present. 2 When the density of Si particles is denoted as δ, The aforementioned γ is 1.5 × 10 3 pieces / mm 2 The above 5.4 x 10 3 pieces / mm 2 The following: said δ is 1.5×10 3 pieces / mm 2 or more and 5.4×10 3 pieces / mm 2 or less. An aluminum alloy extruded material in which the ratio of γ to δ is 0.92 or more and 1.08 or less.

3. The device comprises a collision wall panel, a back panel arranged substantially parallel to the collision wall panel, and a plurality of connecting panels that connect the collision wall panel and the back panel at predetermined intervals. An impact absorbing member wherein at least one of the collision wall plate, the back plate, and the connecting plate is made of an aluminum alloy extruded material as described in claim 1 or 2.

4. A method for manufacturing an aluminum alloy extruded material according to claim 1 or 2, The manufacturing method includes a heating step of a billet made of homogenized aluminum alloy, an extrusion step of extruding the heated billet to obtain an extruded material, a die quenching step of cooling the extruded material obtained by the extrusion process, and an aging step of artificially aging the cooled extruded material. The aforementioned billet has a diameter of 15 cm or more and a length of 30 cm or more. The heating step is performed such that the temperature of the leading end of the billet in the extrusion direction is 400°C or more and 500°C or less, the temperature of the ending end in the extrusion direction is 350°C or more and 450°C or less, and the temperature of the leading end in the extrusion direction is within a range of 60°C or less higher than the temperature of the ending end in the extrusion direction. In a cross-section perpendicular to the extrusion direction at the leading edge of the billet heated by the aforementioned heating step, Mg particles of 0.10 μm or more and 5.0 μm or less 2 The density of Si particles is 1.6 × 10⁻⁶ 3 pieces / mm 2 The above 2.0 x 10 3 pieces / mm 2 The following: The die quenching process involves cooling the material to 150°C or below, with a cooling rate of 7.0°C / sec to 80°C / sec. The aforementioned aging process is carried out at a temperature of 120°C to 240°C for a period of 2 hours to 48 hours. A method for manufacturing aluminum alloy extruded materials.

Citation Information

Patent Citations

  • High strength aluminum alloy excellent in intergranular corrosion resistance, and its production

    JP1998219381A

  • Aluminum alloy extruded shape material excellent in axial collapse characteristic

    JP2000054048A

  • Al-mg-si type aluminum compound extrusion material

    JP2000128017A

  • Impact absorbing member excellent in crushing crack resistance

    JP2001003128A

  • Al-mg-si aluminum alloy extrusion molded material showing excellent resistance to impact fracture

    JP2003221636A