Chrome-free surface treatment agent

JPWO2024143084A5Active Publication Date: 2024-11-26NIPPON PAINT SURF CHEM CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
JP2024530511
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2022-12-27
Filing Date
2023-12-20
Publication Date
2024-11-26
Estimated Expiration
2043-12-20

AI Technical Summary

Technical Problem

Existing chromium-based surface treatment agents for metals face limitations due to environmental regulations, and there is a need for improved chromium-free alternatives that enhance corrosion resistance and chemical resistance.

Method used

A chromium-free surface treatment agent comprising an organic phosphonic acid resin, phosphoric acid compound, complex fluoride, and manganese compound, optionally with a vanadium compound, to improve adhesion and corrosion resistance.

Benefits of technology

The agent significantly enhances the corrosion resistance and chemical resistance of metals, with improved adhesion to both the metal substrate and coating films.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

A chrome-free primer that can improve the corrosion resistance and chemical resistance of metals. The chrome-free primer includes an organic phosphonic acid resin, a phosphoric acid compound, a complex fluoride, and a manganese compound, the organic phosphonic acid resin being a copolymer including a segment derived from a carboxyl group-containing acrylic acid monomer and a segment derived from a phosphonic acid group-containing monomer, and the phosphonic acid group-containing monomer is vinyl phosphonic acid or a phosphonic acid group-containing acrylic acid ester.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a chrome-free surface treatment agent. [Background technology]

[0002] 2. Description of the Related Art Conventionally, in order to improve the corrosion resistance of metals, a method of surface treating metals with a surface treatment agent containing a chromium compound such as a hexavalent chromium compound or a trivalent chromium compound has been known.

[0003] However, according to recent trends in environmental regulations, the use of surface treatment agents containing chromium compounds may be restricted. Therefore, various chromium-free surface treatment agents that do not contain chromium compounds have been developed. For example, chromium-free metal surface treatment agents that are used for metal materials such as zinc-plated steel sheet materials and aluminum-based materials contain zirconium compounds, vanadium compounds, metal fluoro complex compounds, organic phosphorus compounds, inorganic phosphorus compounds, and high acid value resins (see Patent Document 1). [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2014-208874 A Summary of the Invention [Problem to be solved by the invention]

[0005] The technology disclosed in Patent Document 1 improves not only adhesion to metal materials but also adhesion to coating films and corrosion resistance, but there is room for further improvement, particularly in terms of corrosion resistance and chemical resistance at the end faces of metal materials.

[0006] The present invention has been made in view of the above, and has an object to provide a chromium-free primer that can improve the corrosion resistance and chemical resistance of metals. [Means for solving the problem]

[0007] (1) A chrome-free primer comprising an organic phosphonic acid resin, a phosphoric acid compound, a complex fluoride, and a manganese compound, the organic phosphonic acid resin being a copolymer containing a segment derived from a carboxyl group-containing acrylic acid monomer and a segment derived from a phosphonic acid group-containing monomer, the phosphonic acid group-containing monomer being vinyl phosphonic acid or a phosphonic acid group-containing acrylic acid ester.

[0008] (2) The chrome-free primer according to (1), further comprising a vanadium compound.

[0009] (3) The chrome-free primer according to (1) or (2), wherein the complex fluoride is hydrosilicofluoric acid.

[0010] (4) The chrome-free primer according to any one of (1) to (3), wherein the manganese content of the manganese compound relative to the organic phosphonic acid resin (manganese / organic phosphonic acid resin) is 0.05 to 2.0.

[0011] (5) A surface preparation film obtained by curing the chromium-free surface preparation agent according to any one of (1) to (4). Effect of the Invention

[0012] According to the present invention, a chromium-free primer capable of improving the corrosion resistance and chemical resistance of metals can be provided. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0013] The surface treatment agent according to the embodiment of the present invention will be described below, but the present invention is not limited to the description of the following embodiment.

[0014] <Chrome-free surface treatment agent> The chrome-free primer according to the present embodiment (hereinafter, may be referred to as the "primer") contains an organic phosphonic acid resin, a phosphoric acid compound, a complex fluoride, and a manganese compound. It is preferable that the primer further contains a vanadium compound.

[0015] The surface treatment agent according to this embodiment preferably does not contain trivalent and hexavalent chromium. The form of trivalent and hexavalent chromium is not particularly limited and may be metallic chromium, chromium ions, chromium compounds, etc.

[0016] (Organic phosphonic acid resin) The organic phosphonic acid resin is a copolymer containing a segment derived from a carboxyl group-containing acrylic acid monomer and a segment derived from a phosphonic acid group-containing monomer. The segment derived from a carboxyl group-containing acrylic acid monomer reacts with a coating film formed on a film formed by a primer, improving adhesion. The segment derived from a phosphonic acid group-containing monomer reacts with a metal substrate surface to which the primer is applied, improving adhesion. In addition, the crosslinking effect of other components improves chemical resistance. The segment derived from a carboxyl group-containing acrylic acid monomer may be a monomer segment in which the functional group of an acrylic monomer having a functional group other than a carboxyl group is modified to a carboxyl group. The segment derived from a phosphonic acid group-containing monomer may be a monomer segment in which the functional group of a monomer having a functional group other than a phosphonic acid group is modified to a phosphonic acid group.

[0017] The carboxyl group-containing acrylic acid monomer is not particularly limited, but for example, it is preferable to use a (meth)acrylic acid monomer.

[0018] The phosphonic acid group-containing monomer is vinylphosphonic acid, vinylidene-1,1-diphosphonic acid, or a phosphonic acid group-containing acrylic ester.

[0019] The content ratio of the segment derived from the phosphonic acid group-containing monomer in the organic phosphonic acid resin is preferably 20 mol% or more and 95 mol% or less with respect to the total of all segments constituting the organic phosphonic acid resin. When the content ratio of the segment derived from the phosphonic acid group-containing monomer is 20 mol% or more, the phosphonic acid group is sufficiently bonded to the metal substrate surface, and the adhesion and corrosion resistance are improved. On the other hand, when it exceeds 95 mol%, the bond with the coating film is insufficient, and the adhesion and corrosion resistance are reduced.

[0020] The content ratio of the segment derived from the carboxyl group-containing acrylic acid monomer in the organic phosphonic acid resin is preferably 5 mol% or more and 80 mol% or less with respect to the total of all segments constituting the organic phosphonic acid resin. When the content ratio of the segment derived from the carboxyl group-containing acrylic acid monomer is 5 mol% or more, the acrylic acid group is sufficiently bonded to the coating film, and the adhesion and corrosion resistance are improved. On the other hand, when it exceeds 80 mol%, the bond with the metal substrate surface is insufficient, and the adhesion and corrosion resistance are reduced.

[0021] The organic phosphonic acid resin may contain other segments derived from monomers other than those mentioned above. The other monomers are not particularly limited, but may be, for example, hydroxyl group-containing acrylic monomers such as 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, 3-hydroxybutyl (meth)acrylate, and 4-hydroxybutyl (meth)acrylate; methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, 1-methylethyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, t-butyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, lauryl (meth)acrylate, and the like. Examples of the monomers include acrylic acid ester monomers such as methacrylate, phenyl (meth)acrylate, isobornyl (meth)acrylate, cyclohexyl (meth)acrylate, t-butylcyclohexyl (meth)acrylate, and dicyclopentadienyl (meth)acrylate; non-acrylic monomers such as styrene, α-methylstyrene, t-butylstyrene, vinylnaphthalene, acrylonitrile, methacrylonitrile, ethylene, propylene, vinyl acetate, vinyl propionate, butadiene, and isoprene; and (meth)acrylamides such as N-hydroxyethyl (meth)acrylamide, N-hydroxypropyl (meth)acrylamide, and N,N'-methylenebisacrylamide. The content ratio of the other segments in the organic phosphonic acid resin is preferably 30 mol% or less, more preferably 10 mol% or less, and most preferably 0 mol%. The organic phosphonic acid resin is a two-component system of a carboxyl group-containing acrylic acid monomer and a phosphonic acid group-containing monomer, and more preferably does not contain a segment derived from another monomer. When the content of the above other segments in the organic phosphonic acid resin is 30 mol % or less, the resin bonds sufficiently with the metal substrate surface and the coating film, improving adhesion and corrosion resistance.

[0022] The organic phosphonic acid resin can be prepared by carrying out solution polymerization of a monomer mixture containing each of the above monomers. The molecular weight of the organic phosphonic acid resin is preferably 10,000 to 100,000 as a weight average molecular weight. When the weight average molecular weight is 10,000 or more, adhesion and corrosion resistance are improved, and when the weight average molecular weight is 100,000 or less, it is possible to blend without crosslinking with other metal components and increasing viscosity. The weight average molecular weight can be measured by gel permeation chromatography. As the organic phosphonic acid resin, a commercially available one may be used. The commercially available one is not particularly limited, and examples thereof include the ADDIBOND (registered trademark) series manufactured by Solvay.

[0023] By making the organic phosphonic acid resin content 2% by mass or more relative to the total solid content of the surface treatment agent, it is possible to improve the adhesion to metal and the corrosion resistance of the edge surface. By making the organic phosphonic acid resin content 30% by mass or less, it is possible to blend it in a well-balanced manner with other components, making it possible to demonstrate high corrosion resistance, adhesion, and chemical resistance.

[0024] (Phosphate Compounds) The phosphoric acid compound includes compounds having a phosphoric acid group, such as orthophosphoric acid (phosphoric acid) and condensed phosphoric acid, and salts thereof. The inclusion of a phosphoric acid compound in the primer can improve the corrosion resistance of metals. The condensed phosphoric acid is a general term for linear polymeric phosphoric acid produced by dehydration condensation of orthophosphoric acid, and examples of such phosphoric acid include pyrophosphoric acid, tripolyphosphoric acid, polyphosphoric acid, trimetaphosphoric acid, tetrametaphosphoric acid, and ultraphosphoric acid. The salts of the phosphoric acid compounds are not particularly limited, and examples thereof include sodium salts, potassium salts, and ammonium salts.

[0025] The content of the phosphate compound is preferably 30 to 70% by mass relative to the total solid content of the primer. When the content of the phosphate compound is 30% by mass or more, it is possible to improve the corrosion resistance of metal. When the content of the phosphate compound is 70% by mass or less, it is possible to blend it in a well-balanced manner with other components, and it is possible to exhibit high corrosion resistance, adhesion, and chemical resistance.

[0026] (complex fluoride) The complex fluoride is contained in the surface treatment agent to improve the adhesion between the film formed by the surface treatment agent and the metal. Examples of the complex fluoride include hydrosilicic acid such as hydrosilicic acid, zinc hydrosilicic acid, magnesium hydrosilicic acid, nickel hydrosilicic acid, iron hydrosilicic acid, and calcium hydrosilicic acid; zirconium fluorides such as zircon hydrofluoric acid (H2ZrF6) and ammonium hexafluorozirconate ((NH4)2ZrF6); and titanium fluorides such as hydrotitanic acid (H2TiF6) and ammonium hexafluorotitanate ((NH4)2TiF6). The complex fluoride is preferably hydrosilicic acid, since it further improves the adhesion.

[0027] The content of the complex fluoride is preferably 5.0 to 20% by mass relative to the total solid content of the surface treatment agent. When the content of the complex fluoride is 5.0% by mass or more, the adhesion between the coating and the metal becomes good. When the content of the complex fluoride is 20% by mass or less, it can be blended in a well-balanced manner with other components, and it becomes possible to exhibit high corrosion resistance, adhesion, and chemical resistance.

[0028] (Manganese compounds) The manganese compound, when contained in the primer, improves the chemical resistance (acid resistance and alkali resistance) of the metal. Examples of the manganese compound include organic acid salts such as manganese acetate, manganese benzoate, manganese lactate, manganese formate, and manganese tartrate; halides such as manganese chloride and manganese bromide; inorganic acid salts such as manganese nitrate, manganese carbonate, and manganese sulfate; alkoxides such as manganese methoxide; manganese acetylacetonate (II), manganese acetylacetonate (III), manganese dioxide, and manganese oxide.

[0029] By making the content of elemental manganese derived from the manganese compound 1% by mass or more relative to the total solid content of the surface treatment agent, it is possible to improve the chemical resistance of the metal. By making the content of elemental manganese derived from the manganese compound 15% by mass or less, it is possible to blend it in a well-balanced manner with other components, making it possible to exhibit high corrosion resistance, adhesion, and chemical resistance.

[0030] The manganese element content mass ratio of the manganese compound to the organic phosphonic acid resin (manganese / organic phosphonic acid resin) is preferably 0.05 to 2.0. When the manganese / organic phosphonic acid resin is 0.05 or more, a sufficient amount of manganese is secured to exhibit chemical resistance, and therefore the chemical resistance of the metal can be preferably improved. When the manganese / organic phosphonic acid resin is 2.0 or less, the functional group of the organic phosphonic acid resin is not consumed by bonding with manganese, and a sufficient amount of the organic phosphonic acid resin is secured, and therefore the adhesion and corrosion resistance can be preferably improved. From the above viewpoint, the manganese / organic phosphonic acid resin is more preferably 0.1 to 1.0.

[0031] (Vanadium compounds) The vanadium compound, when contained in the undercoat treatment agent, acts as a rust inhibitor and improves the corrosion resistance of metals. The vanadium compound is not particularly limited, but examples thereof include vanadium pentoxide, metavanadic acid, ammonium metavanadate, sodium metavanadate, vanadium oxytrichloride, vanadyl sulfate, vanadyl oxalate, magnesium vanadate, vanadium trioxide, vanadium trichloride, vanadium dioxide, vanadyl acetylacetonate, and vanadium acetylacetonate.

[0032] The vanadium compound content is preferably 5.0 to 20 mass% relative to the total solid content of the primer. When the vanadium compound content is 5.0 mass% or more, the corrosion resistance of metal is improved. When the vanadium compound content is 20 mass% or less, it can be blended in a well-balanced manner with other components, and it is possible to exhibit high corrosion resistance, adhesion, and chemical resistance.

[0033] (Other Ingredients) The surface treatment agent of this embodiment may contain a chelating agent from the viewpoint of improving the stability of the treatment liquid. Examples of the chelating agent that can be used in the surface treatment agent of this embodiment include at least one selected from the group consisting of phosphonic acid chelating agents, aminocarboxylic acid chelating agents, and carboxyethyl group chelating agents.

[0034] Here, examples of phosphonic acid chelating agents include HEDP, NTMP, PBTC, EDTMP, etc. Examples of aminocarboxylic acid chelating agents include EDTA, NTA, DTPA, HEDTA, TTHA, PDTA, DPTA-OH, HIDA, DHEG, GEDTA, CMGA, EDDS, etc. Examples of carboxyethyl group chelating agents include citric acid, structural isomers of citric acid, adipic acid, aminohexanoic acid, etc.

[0035] The total content of the chelating agent contained in the surface treatment agent of this embodiment is preferably 1000 to 15000 mass ppm, more preferably 1500 to 12000 mass ppm. If the total content of the chelating agent is less than 1000 mass ppm, the chelating stabilization effect of the metal component in the aqueous solution becomes insufficient. On the other hand, if the total content of the chelating agent exceeds 15000 mass ppm, the chelating stabilization effect becomes saturated, making it uneconomical.

[0036] The surface treatment agent of the present embodiment may further contain other components to the extent that the above-mentioned functions are not impaired. Examples of other components include known components contained in surface treatment agents, such as crosslinking agents, rust inhibitors, leveling agents, defoamers, and pH adjusters.

[0037] <Metal base material> The metal substrate to be subjected to the surface treatment by the surface treatment agent of the present embodiment is not particularly limited, but examples thereof include metal steel materials such as cold-rolled steel, hot-rolled steel, stainless steel, electrogalvanized steel, hot-dip galvanized steel, zinc-aluminum alloy-based plated steel, zinc-iron alloy-based plated steel, zinc-magnesium alloy-based plated steel, zinc-aluminum-magnesium alloy-based plated steel, aluminum-based plated steel, aluminum-silicon alloy-based plated steel, tin-based plated steel, lead-tin-based plated steel, chromium-based plated steel, and Ni-based plated steel. Examples of aluminum-based materials include metal materials such as pure aluminum and various aluminum alloys. The shape of the metal substrate is not particularly limited, but examples thereof include a plate shape.

[0038] <Surface preparation method> A base treatment method using the base treatment agent of this embodiment includes, for example, a coating process in which the base treatment agent is applied to the surface of a metal substrate, and a baking process in which the base treatment agent applied to the metal substrate is baked and hardened.

[0039] In the coating step, the method for coating the surface of the metal substrate with the primer is not particularly limited, and examples thereof include roll coating, bar coating, spraying, immersion, etc. Prior to the coating step, the surface of the metal substrate may be subjected to a degreasing treatment, pickling, or etching treatment, if necessary.

[0040] In the baking step, after the coating step, the primer coating agent applied to the metal substrate is baked. The baking method is not particularly limited. For example, after the primer coating agent is applied to the surface of the metal substrate, the upper layer may be painted while the primer coating agent is in an uncured state, and then baking may be performed.

[0041] <Surface treatment film> The coating formed by the above-mentioned surface treatment agent (hereinafter, sometimes referred to as "coating") is formed on the surface of the above-mentioned metal substrate. The thickness of the coating is not particularly limited, but is preferably 0.01 to 1.0 μm. The weight of the coating is not particularly limited, but is preferably 0.01 to 1.0 g / m 2 It is preferable that a coating film is formed on the upper layer of the coating. This is because the primer of the present embodiment can obtain a preferable adhesion to the coating film. The paint for forming the coating film is not particularly limited, and a one-coat paint or a primer and a top coat may be used. EXAMPLES

[0042] The present invention will be described in more detail below based on examples, but the present invention is not limited to these examples. However, Examples 1 to 31 are reference examples.

[0043] <Preparation of surface treatment agent> [Examples 1 to 41, Comparative Examples 1 to 6] A primer was obtained by mixing and stirring an organic phosphonic acid resin, a resin (comparative example), a phosphoric acid compound, a complex fluoride, a manganese compound, a vanadium compound, a chelate compound, and ion-exchanged water so that the solid content in the primer was 2 mass% according to the contents shown in the following Tables 1 to 4. The blending amount of each component shown in Tables 1 to 4 indicates the solid content (parts by mass).

[0044] Details of the types of raw materials listed in Tables 1 to 4 are shown below.

[0045] (A1~A3: Organic phosphonic acid resin, A4~A5: Resin (comparative example)) A1: ADDIBOND (registered trademark) 021 (organic phosphonic acid resin (non-volatile content (NV): 20%), copolymer of vinylphosphonic acid and acrylic acid, molar ratio of vinylphosphonic acid: 30%, weight average molecular weight: 30,000 to 90,000, manufactured by Solvay) A2: ADDIBOND® 829 (organic phosphonic acid resin (non-volatile content (NV): 40%), manufactured by Solvay) A3: Julimer AC-10L (polyacrylic acid (non-volatile content (NV): 40%), manufactured by Toagosei Co., Ltd.) A4: Polyvinylphosphonic acid (non-volatile content (NV): 100%, Sigma-Aldrich)

[0046] (B1 to B3: Phosphate compounds) B1: Phosphate B2: Pyrophosphate B3: Polyphosphate

[0047] (C1~C4: complex fluoride) C1: Hydrofluoric acid C2: Titanium hydrofluoric acid (Morita Chemical Industry Co., Ltd.) C3: Fluorozirconate (Morita Chemical Industry Co., Ltd.) C4: Aluminum fluoride

[0048] (D1-D2: Manganese compounds) D1: Manganese nitrate D2: Manganese carbonate

[0049] (E1-E6: Vanadium compounds) E1: Vanadyl sulfate E2: Ammonium metavanadate E3: Sodium metavanadate E4: Vanadyl oxalate E5: Vanadium pentoxide E6: Vanadyl acetylacetonate (VO(C5H7O2)2) (Nasem Vanadyl, manufactured by Nippon Chemical Industry Co., Ltd.)

[0050] (F1~F2: Chelating agents) F1: 1-hydroxyethane-1,1-diphosphonic acid (HEDP) F2: 2-phosphonobutane-1,2,4-tricarboxylic acid (PBTC)

[0051] [Table 1]

[0052] [Table 2]

[0053] [Table 3]

[0054] [Table 4]

[0055] <Preparation of test plate> A hot-dip 55% aluminum-zinc alloy plated steel sheet (substrate shown in Tables 1 to 4: GL) or a hot-dip galvanized steel sheet (substrate shown in Table 2: GI) was subjected to surface treatment using the surface treatment agents shown in Tables 1 to 4. The surface treatment was performed as follows.

[0056] (Degreasing and surface treatment) The steel plate was degreased by spraying an alkaline degreaser (Nippon Paint Surf Chemicals, Surf Cleaner 155) at 60° C. for 10 seconds, rinsed with water, and then dried at 80° C. Next, the surface treatment agents prepared in the Examples and Comparative Examples were applied to the degreased steel plate with a bar coater (number: #3) after adjusting the solid content concentration, and dried in a hot air circulating oven so that the metal substrate reached a temperature of 80° C. to produce a test plate on which a chemical conversion film was formed.

[0057] (Resin layer formation) A commercially available PCM primer paint (Flexicoat 600, manufactured by Nippon Paint Industrial Coatings) was applied (dry film thickness 5.0 μm) and then baked at 200°C. Next, a PCM topcoat paint (polyester paint, Flexicoat 5030, manufactured by Nippon Paint Industrial Coatings) was applied to the baked surface (dry film thickness 15 μm) and then baked at 225°C to prepare a coated steel plate. Appropriate test pieces were cut out from each of the coated steel plates thus prepared to prepare test plates. The test plates obtained as described above were used to carry out the following evaluations.

[0058] <Evaluation> [Combined cycle test (corrosion resistance)] A scratch was made in the coating of each of the test plates prepared above with a cutter knife, reaching the metal substrate, and 150 cycles of the combined cycle test (CCT) specified in JIS H 8502 (JASO M609-91) were performed. After that, the maximum value of the coating blister width from the scratch and the average value of the coating blister width from the end face of the test piece were measured and evaluated according to the following criteria, with a rating of 3.5 or more being considered as passing. The results are shown in Tables 1 to 4. Note that the measurement of the average value means that a location with an average blister width was visually selected from the entire coating blister from the end face of the test piece, and the coating blister width at that location was measured.

[0059] (Evaluation criteria: maximum width of coating blister from scratch) 5: Less than 1mm 4.5: 1mm or more, less than 2mm 4: 2mm or more and less than 3mm 3.5: 3mm or more but less than 4mm 3: 4mm or more but less than 5mm 2.5: 5mm or more and less than 6mm 2: 6mm or more but less than 7mm 1.5:7 or more, less than 8mm 1:8mm or more

[0060] (Evaluation criteria: average value of the blister width of the coating film from the end of the test piece) 5: Less than 4mm 4.5: 4mm to less than 6mm 4: 6mm or more but less than 8mm 3.5: 8mm or more and less than 10mm 3: 10mm or more and less than 12mm 2.5: 12mm or more and less than 14mm 2: 14mm or more and less than 16mm 1.5: 16mm or more and less than 18mm 1:18mm or more

[0061] [First adhesion after bending] Each test plate prepared above was bent 2T (180 degree bending) at 20°C with a spacer in between, in accordance with the test method specified in JIS G3312, and a tape peeling test was carried out on the bent portion. After that, the coating peeling state after the test was visually evaluated according to the following criteria, and a rating of 3.5 or more was considered to be a pass. The results are shown in Tables 1 to 4. 5: No peeling 4.5: 1-10% peeling 4:11-20% peeling 3.5: 21-30% peeling 3:31-40% peeling 2.5:41-50% peeling 2:51-60% peeling 1.5: 61-70% peeling 1:71-80% peeling 0.5: 81-90% peeling 0:91~100% peeling

[0062] [Secondary adhesion after bending] The test plate was immersed in boiling water for 2 hours, and then left indoors for 24 hours. The test plate was evaluated under the same conditions as the primary bending adhesion, under the 2TT condition, and using the same criteria. A score of 3.5 or more was considered to be acceptable, and the results are shown in Tables 1 to 4.

[0063] [Alkaline resistance (chemical resistance)] The alkali resistance of each of the test panels prepared above was evaluated by the following method in accordance with the test method specified in ASTM D714-56. Each of the test panels prepared above was immersed in a 5% by mass aqueous solution of sodium hydroxide at room temperature for 24 hours, and the size and density of blisters generated on the evaluation surface were visually evaluated according to the following criteria, with a rating of 3.5 or more being considered as passing. The results are shown in Tables 1 to 4.

[0064] (Evaluation criteria: Alkali resistance (chemical resistance)) 5: No blister 4.5: The size of a single blister is less than 0.3 mm and the density of occurrence is VF or F. 4: The size of one blister is 0.3 mm or more but less than 0.6 mm and the density of occurrence is VF or F. 3.5: The size of one blister is less than 0.6 mm and the occurrence density is FM. 3: The size of each blister is less than 0.6 mm and the density of occurrence is M. Alternatively, the size of each blister is 0.6 mm or more and less than 1.2 mm and the density of occurrence is F or FM. 2.5: The size of each blister is less than 0.6 mm and the density of occurrence is MD, or the size of each blister is 0.6 mm or more and less than 1.2 mm and the density of occurrence is FM or M, or the size of each blister is 1.2 mm or more and less than 1.8 mm and the density of occurrence is VF or F. 2: The size of each blister is 0.6 mm or more and less than 1.2 mm and the density of occurrence is M or MD, or the size of each blister is 1.2 mm or more and less than 1.8 mm and the density of occurrence is F or FM. 1.5: The size of one blister is 1.2 mm or more and less than 1.8 mm and the density of occurrence is M or MD. 1: The size of a single blister is 1.8 mm or more, or the density of occurrence is D regardless of the size of the blister. The symbols used for occurrence density have the following meanings: VF: The number of blisters is extremely small. F: The number of blisters is small. FM: The number of blisters is intermediate between F and M. M: A large number of blisters occurred. MD: The number of blisters is intermediate between M and D. D: The number of blisters is extremely large.

[0065] [Acid resistance (chemical resistance)] Each test plate prepared above was immersed in a 5% by mass aqueous solution of hydrochloric acid at room temperature for 24 hours, and then the size and density of blisters generated on the evaluation surface were visually evaluated according to the same criteria as in the alkali resistance test, with a rating of 3.5 or higher being considered a pass. The results are shown in Tables 1 to 4.

[0066] From the results in Tables 1 to 4, it is clear that the surface preparation agents of the Examples have higher metal corrosion resistance, adhesion, and chemical resistance than the surface preparation agents of the Comparative Examples. For example, the surface preparation agents of the Examples have higher metal corrosion resistance, adhesion, and chemical resistance (alkali resistance) than the surface preparation agents of Comparative Examples 1, 5, and 6, which do not contain an organic phosphonic acid resin. Also, the surface preparation agents of the Examples have higher metal chemical resistance than the surface preparation agent of Comparative Example 4, which does not contain a manganese compound.

Claims

1. A chrome-free surface treatment agent, comprising: The composition includes an organic phosphonic acid resin, a phosphoric acid compound, a complex fluoride, and a manganese compound, The organic phosphonic acid resin is a copolymer including a segment derived from a carboxyl group-containing acrylic acid monomer and a segment derived from a phosphonic acid group-containing monomer, the phosphonic acid group-containing monomer is vinylphosphonic acid or a phosphonic acid group-containing acrylic acid ester; A chrome-free primer, wherein the manganese element content ratio of the manganese compound to the organic phosphonic acid resin (manganese / organic phosphonic acid resin) is 0.05 to 2.

0.

2. The chrome-free primer according to claim 1 , further comprising a vanadium compound.

3. 3. The chrome-free primer according to claim 1, wherein the complex fluoride is hydrosilicofluoric acid.

4. A primer coating formed by curing the chromium-free primer according to claim 1 or 2.