Cr-Ni alloy pipe
Patent Information
- Application Number
- JP2023541837
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-28
- Publication Date
- 2024-10-03
- Estimated Expiration
- 2043-03-28
AI Technical Summary
Cr-Ni alloy pipes used in oil country tubular goods experience a significant difference between compressive and tensile yield stresses due to welding, leading to reduced strength in welded areas, which complicates their use in harsh oil well environments.
A Cr-Ni alloy tube with specific mechanical properties and chemical composition, including formulas to balance compressive and tensile yield stresses, is produced through controlled cold working and high-frequency induction heating followed by rapid cooling, ensuring high strength and minimal stress difference.
The alloy tube maintains high strength and minimizes the difference between compressive and tensile yield stresses, making it suitable for oil country tubular goods that can withstand environmental stress variations and maintain strength even in welded areas.
Abstract
Description
[Technical field]
[0001] The present invention relates to a Cr-Ni alloy tube. [Background technology]
[0002] In recent years, the conditions for extracting oil wells and gas wells (hereinafter, oil wells and gas wells are collectively referred to simply as "oil wells") from crude oil and natural gas have become severe. Therefore, austenitic alloy pipes containing Cr and Ni and having excellent corrosion resistance (hereinafter, also referred to as "Cr-Ni alloy pipes") are sometimes used for oil well tubular goods used in oil wells.
[0003] In addition to excellent corrosion resistance, OCTG also requires high strength. The strength grade of OCTG is generally defined by the tensile yield stress in the axial direction of the tube. OCTG users determine the environment of the well to be drilled (geologic pressure, temperature and pressure of the production fluid) from exploratory drilling and geological surveys, and select OCTG with a strength grade that can withstand the conditions.
[0004] However, it is known that the compressive yield strength in the axial direction of a cold-worked corrosion-resistant alloy pipe is smaller than the tensile yield stress in the axial direction. As described above, the strength grade of oil country tubular goods is generally determined by the tensile yield strength. Therefore, it is preferable that the difference between the compressive yield stress and the tensile yield stress is small.
[0005] Patent Document 1 discloses an austenitic alloy pipe that has small anisotropy in yield strength and can therefore withstand stress distributions that vary depending on the usage environment. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] International Publication No. 2012 / 128258 Summary of the Invention [Problem to be solved by the invention]
[0007] Incidentally, Cr-Ni alloy pipes as oil well tubular goods may be used by welding with other alloy pipes or steel pipes. In this case, the welded part of the Cr-Ni alloy pipe is softened by the welding heat. Therefore, it is necessary to select an oil well tubular goods with a strength grade that can withstand the target oil well environment while taking into consideration the softening at the welded part.
[0008] In order to maintain high strength even when softening occurs in the weld, it is conceivable to increase the degree of cold working; however, this is not preferable since it results in the compressive yield stress being significantly lower than the tensile yield stress.
[0009] The present invention aims to solve the above problems and provide a Cr-Ni alloy tube having high strength while minimizing the difference between compressive yield stress and tensile yield stress. [Means for solving the problem]
[0010] The present invention has been made to solve the above problems, and the gist of the present invention is the following Cr-Ni alloy tube.
[0011] (1) A Cr-Ni alloy tube, The tensile yield stress YS in the axial direction of the Cr-Ni alloy tube LT and compressive yield stress YS LC , and The specimen was taken from the center of the wall thickness of the Cr-Ni alloy tube so that the longitudinal direction was parallel to the tube axis direction, and was heated from room temperature to 1150°C at a heating rate of 100°C / s using a high-frequency induction heating device, then heated to 1200°C at a heating rate of 25°C / s, held at 1200°C for 180 seconds, and then quenched to room temperature by blowing Ar gas under conditions where the cooling rate in the temperature range from 1200°C to 800°C is 50°C / s. The tensile yield stress YS HT but, The following formulas (i) to (iii) are satisfied: Cr-Ni alloy tube. 0.80≦YSLC / YS LT <0.95 (i) Y.S. HT -0.24×YS LT ≧50.0 (ii) Y.S. LT ≧443×YS LT / YS LC +2.28×YS HT -350 (iii) In the above formula, the meanings of each symbol are as follows: Y.S. LC : Compressive yield stress in the axial direction (MPa) Y.S. LT : Tensile yield stress in the axial direction of the tube (MPa) Y.S. HT : Tensile yield stress of test piece after high-frequency induction heating and quenching (MPa)
[0012] (2) Tensile yield stress YS in the axial direction of the Cr-Ni alloy tube LT is 780MPa or more, The Cr-Ni alloy tube according to (1) above.
[0013] (3) Chemical composition, in mass%, C: 0.030% or less, Si: 0.50% or less, Mn: 1.00% or less, P: 0.030% or less, S: 0.0050% or less, Cr: 19.00~32.00%, Ni: 29.50~55.00%, Mo: 2.50-12.00%, Cu:3.00% or less, V: 0.01 to 0.50%, Nb+Ti: 0.002-1.000%, Al: 0.001 to 0.500%, N: 0.005~0.400%, W: 0 to 1.00%, Co: 0-1.00%, Sn: 0~0.010%, As: 0~0.010%, Zn: 0 to 0.010%, Pb: 0~0.010%, Sb: 0 to 0.010%, B: 0~0.0050%, Ca: 0 to 0.0200%, Mg: 0 to 0.0200%, REM: 0~0.100%, The balance is Fe and impurities. The Cr-Ni alloy tube according to (1) or (2) above.
[0014] (4) The chemical composition is, in mass%, W: 0.01 to 1.00%, Co: 0.01 to 1.00%, Sn: 0.001 to 0.010%, As: 0.001 to 0.010%, Zn: 0.001 to 0.010%, Pb: 0.0005~0.010%, Sb: 0.0005 to 0.010%, B: 0.0001~0.0050%, Ca: 0.0005~0.0200%, Mg: 0.0001 to 0.0200%, and REM: 0.001~0.100%, Contains one or more selected from The Cr-Ni alloy tube according to (3) above.
[0015] (5) The chemical composition further satisfies the following formulas (iv) and (v): The Cr-Ni alloy tube according to (3) or (4) above. 9Mo+100N≧45.0 (iv) Ni+1.4Cu+Mo-0.9Cr-2Si-1.2Mn-5.7C+20N+90(0.15Nb+0.27V+0.3Ti)≦42.0 (v) In the above formula, the element symbols indicate the content (mass%) of each element in the alloy tube, and zero is substituted if the element is not contained.
[0016] (6) The chemical composition further satisfies the following formula (vi): A Cr-Ni alloy tube according to any one of (3) to (5) above. 0.001×YS LT -0.820 <N<0.001×YS LT -0.740 (vi) In the above formula, the meanings of each symbol are as follows: YS LC : Compressive yield stress in the axial direction (MPa) N: N content in alloy tube (mass%) Effect of the Invention
[0017] According to the present invention, a Cr-Ni alloy pipe having high strength can be obtained while minimizing the difference between the compressive yield stress and the tensile yield stress. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0018] Each of the features of the present invention will be described in detail below.
[0019] 1. Mechanical properties The mechanical properties of the Cr-Ni alloy tube according to this embodiment will be described. The Cr-Ni alloy tube according to this embodiment has mechanical properties that satisfy the following formulas (i) to (iii). In the present invention, the Cr-Ni alloy tube means an austenitic alloy tube containing 19.00-32.00% Cr and 29.50-55.00% Ni.
[0020] <Strength anisotropy> The Cr-Ni alloy tube according to the present embodiment has improved strength due to work hardening caused by cold working, but if it is subsequently subjected to heat treatment at high temperature, its strength decreases and it is not possible to maintain the strength required in the usage environment. That is, the Cr-Ni alloy tube according to the present embodiment is in a state in which it is cold worked or has been subjected to heat treatment at a low temperature after cold working. Therefore, the tensile yield stress in the tube axis direction of the Cr-Ni alloy tube is necessarily higher than the compressive yield stress in the tube axis direction.
[0021] However, if the difference between the compressive yield stress and the tensile yield stress in the axial direction is excessive, even if the tensile yield stress is sufficient, the compressive yield stress will be insufficient and the pipe will not be usable as an oil country tubular good. Therefore, the compressive yield stress and the tensile yield stress in the axial direction must satisfy the following formula (i): 0.80≦YS LC / YS LT <0.95 (i) In the above formula, the meanings of each symbol are as follows: Y.S. LC : Compressive yield stress in the axial direction (MPa) Y.S. LT : Tensile yield stress in the axial direction of the tube (MPa)
[0022] Y.S. LC / YS LT The value of YS is preferably 0.82 or more, more preferably 0.84 or more, and even more preferably 0.86 or more. LC / YS LT The value of may be less than or equal to 0.94.
[0023] The tensile yield stress YS in the axial direction of the tube is LT There is no particular need to impose a limit on the tensile yield stress YS in the axial direction of the tube, but as described above, the Cr-Ni alloy tube according to this embodiment is in the cold-worked state or in the state where it has been subjected to a low-temperature heat treatment after cold working, so that the tensile yield stress YS is 780 MPa or more. LTis preferably 800 MPa or more, more preferably 820 MPa or more, even more preferably 840 MPa or more, and even more preferably 850 MPa or more.
[0024] Specifically, the compressive yield stress in the tube axial direction is determined by the following method. A compression test is performed using a method in accordance with ASTM E9 (2019). A cylindrical test piece for the compression test is prepared from the center position of the wall thickness of the Cr-Ni alloy tube. The size of the cylindrical test piece is, for example, 4 mm in parallel diameter and 8 mm in length. The longitudinal direction of the cylindrical test piece is parallel to the tube axial direction of the Cr-Ni alloy tube. A compression test is performed using the cylindrical test piece in air at room temperature (25°C), and the obtained 0.2% offset proof stress is defined as the compressive yield stress in the tube axial direction YS LC (MPa).
[0025] Similarly, the tensile yield stress in the tube axial direction is determined by the following method. A tensile test is performed using a method in accordance with ASTM E8 / E8M (2021). A round bar test piece for the tensile test is prepared from the center position of the wall thickness of the Cr-Ni alloy tube. The size of the round bar test piece is, for example, 4 mm in parallel diameter and 20 mm in gauge length. The longitudinal direction of the round bar test piece is parallel to the tube axial direction of the Cr-Ni alloy tube. A tensile test is performed using the round bar test piece at room temperature (25°C) in air, and the obtained 0.2% offset proof stress is defined as the tensile yield stress YS LT (MPa).
[0026] <Base strength> As described above, the strength of the Cr-Ni alloy tube can be improved by cold working, but excessive working leads to an increase in anisotropy. Therefore, in order to avoid excessive working, it is necessary to sufficiently secure the strength before cold working, that is, the strength in a state without the effect of work hardening (hereinafter also referred to as "base strength"). As a result of the study by the present inventors, it was found that an index of the base strength can be obtained from the tensile yield stress of a test piece in which the effect of work hardening was eliminated by high-frequency induction heating and quenching, and the tensile yield stress in the tube axis direction of the Cr-Ni alloy tube.
[0027] Specifically, by satisfying the following formula (ii), the material has a base strength sufficient for use as an oil country tubular good. Y.S. HT -0.24×YS LT ≧50.0 (ii) In the above formula, the meanings of each symbol are as follows: Y.S. LT : Tensile yield stress in the axial direction of the tube (MPa) Y.S. HT : Tensile yield stress of test piece after high-frequency induction heating and quenching (MPa)
[0028] The test piece after high-frequency induction heating and quenching is obtained by the following procedure. First, a test piece is taken from the center position of the wall thickness of the Cr-Ni alloy tube so that the longitudinal direction is parallel to the tube axis direction. The test piece is prepared in accordance with ASTM E8 / E8M(2021). Specifically, if the wall thickness of the alloy tube is 6 mm or more, a cylindrical test piece with a diameter of 6 mm and a gauge length of 30 mm is used. If the wall thickness of the alloy tube is less than 6 mm, a circular arc test piece with the same thickness as the wall thickness of the alloy tube and a gauge length of 50 mm is used.
[0029] Next, the cylindrical test piece is heated from room temperature to 1150°C at a heating rate of 100°C / s using a high-frequency induction heating device, and then heated to 1200°C at a heating rate of 25°C / s. At this time, the heating area by the high-frequency induction heating device is an area of 3.5 mm from the center in the longitudinal direction of the test piece to both ends and 7.0 mm in the longitudinal direction. The temperature of the test piece is measured using a thermocouple installed in the center of the test piece in the longitudinal direction.
[0030] The test piece is then held at 1200°C for 180 seconds. Immediately after holding, Ar gas is sprayed onto the test piece to rapidly cool it to room temperature at a cooling rate of 50°C / s in the temperature range from 1200°C to 800°C. Then, using the test piece after high-frequency induction heating and rapid cooling, a tensile test is carried out in air at room temperature (25°C) in accordance with JIS Z 2241 (2011), and the obtained 0.2% offset proof stress is the tensile yield stress YS of the test piece after high-frequency induction heating and rapid cooling.HT (MPa).
[0031] <Work hardening ability> In order to improve the strength by cold working while suppressing the increase in anisotropy, it is necessary to have an excellent work-hardening ability that can efficiently work-harden even with a small degree of working. As a result of intensive research by the inventors, it was found that the YS LC / YS LT The reciprocal of YS LT / YS LC It was also found that the tensile yield stress in the axial direction of the Cr-Ni alloy tube and the YS LT / YS LC and the tensile yield stress YS of the test piece after removing the effects of work hardening by high-frequency induction heating and rapid cooling. HT It was found that the above equation is an index of work hardening ability.
[0032] Specifically, by satisfying the following formula (iii), the material has sufficient work hardening ability for use as an oil country tubular good. Y.S. LT ≧443×YS LT / YS LC +2.28×YS HT -350 (iii) In the above formula, the meanings of each symbol are as follows: Y.S. LC : Compressive yield stress in the axial direction (MPa) Y.S. LT : Tensile yield stress in the axial direction of the tube (MPa) Y.S. HT : Tensile yield stress of test piece after high-frequency induction heating and quenching (MPa)
[0033] As described above, from the three mechanical property values of the tensile yield stress and compressive yield stress in the axial direction of the Cr-Ni alloy pipe, and the tensile yield stress of the test piece after high-frequency induction heating and quenching, it is possible to select a Cr-Ni alloy pipe that can maintain high strength even if softening occurs in the weld and is a highly reliable material for oil country tubular goods.
[0034] 2.Chemical composition The chemical composition of the Cr-Ni alloy tube according to this embodiment is not particularly limited as long as it contains a predetermined amount of Cr and Ni and has the above-mentioned mechanical properties. For example, the Cr-Ni alloy tube according to this embodiment preferably has the chemical composition shown below. The reasons for limiting each element are as follows. In the following description, "%" for the content means "mass %".
[0035] C: 0.030% or less Carbon (C) is an element that has the effect of increasing the strength of an alloy. However, if C is contained in excess, it forms Cr carbides at the grain boundaries. The Cr carbides increase the stress corrosion cracking (SCC) susceptibility at the grain boundaries. Therefore, the C content is 0.030% or less. The preferred C content is less than 0.030%, more preferably 0.025%, and even more preferably 0.020% or less. The preferred lower limit of the C content is 0.001%, more preferably 0.003%, and even more preferably 0.005%.
[0036] Si:0.50% or less Silicon (Si) is an element that has the effect of deoxidizing the alloy. However, if Si is contained in excess, the hot workability of the alloy decreases. Therefore, the Si content is 0.50% or less. The preferred Si content is less than 0.50%. The preferred upper limit of the Si content is 0.45%, more preferably 0.40%. The preferred lower limit of the Si content is 0.05%, more preferably 0.10%.
[0037] Mn: 1.00% or less Manganese (Mn) is an element that has the effect of deoxidizing the alloy. Mn is also an austenite forming element and stabilizes the austenite phase. However, if Mn is contained in excess, the hot workability of the alloy decreases. Therefore, the Mn content is 1.00% or less. The preferred Mn content is less than 1.00%. The preferred upper limit of the Mn content is 0.90%, more preferably 0.80%. The preferred lower limit of the Mn content is 0.10%, more preferably 0.30%.
[0038] P:0.030% or less Phosphorus (P) is an impurity element. P increases the stress corrosion cracking susceptibility of the alloy in a hydrogen sulfide environment. Therefore, the P content is preferably small, and is 0.030% or less. The P content is preferably 0.025% or less, and more preferably 0.020% or less.
[0039] S: 0.0050% or less Sulfur (S) is an impurity element. S reduces the hot workability of the alloy. Therefore, the S content is preferably small, and is 0.0050% or less. The S content is preferably 0.0030% or less, and more preferably 0.0010% or less.
[0040] Cr: 19.00~32.00% Chromium (Cr) is an element that has the effect of increasing the stress corrosion cracking resistance (SCC resistance) of the alloy in the presence of Ni. Cr also increases the strength of the alloy by solid solution strengthening. On the other hand, if Cr is contained in excess, the effect is saturated and the hot workability of the alloy is further reduced. Therefore, the Cr content is 19.00 to 32.00%. The lower limit of the Cr content is preferably 21.00%, more preferably 23.00%. The upper limit of the Cr content is preferably 30.00%, more preferably 28.00%.
[0041] Ni: 29.50~55.00% Nickel (Ni) is an austenite forming element and has the effect of stabilizing the austenite phase. Ni also enhances SCC resistance. However, if Ni is contained in excess, the effect is saturated. Therefore, the Ni content is 29.50 to 55.00%. The lower limit of the Ni content is preferably 34.00%, and more preferably 40.00%. The upper limit of the Ni content is preferably 53.00%, and more preferably 50.00%.
[0042] Mo: 2.50-12.00% Molybdenum (Mo) is an element that has the effect of increasing the SCC resistance of the alloy in the presence of Cr and Ni. Mo also increases the strength of the alloy by solid solution strengthening. However, if Mo is contained in excess, the effect becomes saturated and the hot workability of the alloy decreases. Therefore, the Mo content is 2.50 to 12.00%. The preferred lower limit of the Mo content is 3.50%, and more preferably 5.00%. The preferred upper limit of the Mo content is 10.00%, and more preferably 8.00%.
[0043] Cu:3.00% or less Copper (Cu) is an element that is effective in stabilizing the passive film and improving pitting corrosion resistance and general corrosion resistance. However, if Cu is contained in excess, the effect is saturated and hot workability is further reduced. Therefore, the Cu content is 3.00% or less. The preferred Cu content is 2.00% or less, and more preferably 1.20% or less. The preferred lower limit of the Cu content is 0.10%, and more preferably 0.50%.
[0044] V: 0.01 to 0.50% Vanadium (V) is an element that has the effect of increasing the strength of an alloy by finely precipitating within grains as carbides, nitrides, or carbonitrides. It also has the effect of refining grains by pinning grain boundaries. V also increases the solubility of N in the alloy, thereby suppressing the occurrence of pinholes near the surface when the N content is increased to increase the strength of the alloy. However, if V is contained in excess, the amount of precipitates becomes excessive, not only reducing toughness but also increasing the risk of weld cracks in the heat-affected zone. Therefore, the V content is 0.01 to 0.50%. The preferred lower limit of the V content is 0.02%, more preferably 0.03%. The preferred upper limit of the V content is 0.35%, more preferably 0.20%.
[0045] Nb+Ti: 0.002~1.000% Niobium (Nb) and titanium (Ti) are elements that have the effect of increasing the strength of the alloy by finely precipitating in the grains as carbides, nitrides, or carbonitrides. They also have the effect of refining the grains by pinning the grain boundaries. Nb and Ti further increase the solubility of N in the alloy, thereby suppressing the occurrence of pinholes near the surface when the N content is increased to increase the strength of the alloy. However, if Nb and / or Ti is contained in excess, the amount of precipitates becomes excessive, not only reducing the toughness but also increasing the risk of weld cracks in the heat-affected zone. Therefore, one or both of Nb and Ti are contained, and the total content thereof is 0.002 to 1.000%. The lower limit of the total content is preferably 0.010%, more preferably 0.030%. The upper limit of the total content is preferably 0.500%, more preferably 0.300%.
[0046] Al: 0.001 to 0.500% Aluminum (Al) is an element that has the effect of deoxidizing the alloy. However, if Al is contained in excess, it impairs the cleanliness and deteriorates the workability and ductility. Therefore, the Al content is 0.001 to 0.500%. The preferred lower limit of the Al content is 0.005%, more preferably 0.010%. The preferred upper limit of the Al content is 0.300%, more preferably 0.100%. In the present invention, the Al content refers to the content of acid-soluble Al (so-called "sol. Al").
[0047] N: 0.005~0.400% Nitrogen (N) increases the strength of the alloy by solid solution strengthening. If solution heat treatment is performed while containing N, an alloy pipe having high strength can be obtained. If an alloy pipe having high strength is used, the desired strength can be obtained after cold working, even if the cold working is performed with a low degree of working. However, if N is contained in an excessive amount, pinholes are likely to occur near the surface when the alloy is solidified. Furthermore, N reduces the hot workability of the alloy. Therefore, the N content is 0.005 to 0.400%. The lower limit of the N content is preferably 0.010%, more preferably 0.030%, and even more preferably 0.060%. The upper limit of the N content is preferably 0.350%, and more preferably 0.300%.
[0048] In addition to the above elements, the Cr-Ni alloy tube according to the present embodiment may further contain one or more elements selected from W, Co, Sn, As, Zn, Pb, Sb, B, Ca, Mg and REM. There is no need to set a lower limit for the content of any of the elements, and the content may be 0%.
[0049] W: 0~1.00% Tungsten (W) is an optional element. Therefore, W may not be contained. W has the effect of increasing SCC resistance, so it may be contained as necessary. However, if W is contained in excess, the effect is saturated and hot workability is further reduced. Therefore, the W content is 1.00% or less. The preferred W content is 0.50% or less, and more preferably 0.30% or less. The preferred lower limit of the W content is 0.01%, and more preferably 0.05%.
[0050] Co: 0 to 1.00% Cobalt (Co) is an optional element. Therefore, Co may not be contained. Like Ni, Co has the effect of increasing the stability of the austenite phase, so it may be contained as necessary. However, since Co is an extremely expensive element, a high content of Co leads to an increase in cost. Therefore, the Co content is 1.00% or less. The preferred Co content is 0.50% or less, and more preferably 0.30% or less. The preferred lower limit of the Co content is 0.01%, and more preferably 0.05%.
[0051] Sn: 0 to 0.010% Tin (Sn) is an optional element. Therefore, Sn does not have to be contained. Sn has the effect of affecting the convection of the molten pool during welding, increasing the penetration depth, and improving weldability, so it may be contained as necessary. However, if Sn is contained in excess, it not only increases the susceptibility to weld cracking, but also leads to a decrease in corrosion resistance. Therefore, the Sn content is 0.010% or less. The preferred Sn content is 0.008% or less, and more preferably 0.006% or less. The preferred lower limit of the Sn content is 0.001%, and more preferably 0.002%.
[0052] As: 0 to 0.010% Arsenic (As) is an optional element. Therefore, As does not have to be contained. As has the effect of affecting the convection of the molten pool during welding, increasing the penetration depth, and improving weldability, so it may be contained as necessary. However, if As is contained in excess, it not only increases the susceptibility to weld cracking, but also leads to a decrease in corrosion resistance. Therefore, the As content is 0.010% or less. The preferred As content is 0.008% or less, and more preferably 0.006% or less. The preferred lower limit of the As content is 0.001%, and more preferably 0.002%.
[0053] Zn: 0 to 0.010% Zinc (Zn) is an optional element. Therefore, Zn does not have to be contained. Zn has the effect of affecting the convection of the molten pool during welding, increasing the penetration depth, and improving weldability, so it may be contained as necessary. However, if Zn is contained in excess, it not only increases the susceptibility to weld cracking, but also leads to a decrease in corrosion resistance. Therefore, the Zn content is 0.010% or less. The preferred Zn content is 0.008% or less, and more preferably 0.006% or less. The preferred lower limit of the Zn content is 0.001%, and more preferably 0.002%.
[0054] Pb: 0~0.010% Lead (Pb) is an optional element. Therefore, Pb does not have to be contained. Pb has the effect of affecting the convection of the molten pool during welding, increasing the penetration depth, and improving weldability, so it may be contained as necessary. However, if Pb is contained in excess, it not only increases the susceptibility to weld cracking, but also leads to a decrease in corrosion resistance. Therefore, the Pb content is 0.010% or less. The preferred Pb content is 0.008% or less, and more preferably 0.006% or less. The preferred lower limit of the Pb content is 0.0005%, and more preferably 0.001%.
[0055] Sb: 0 to 0.010% Antimony (Sb) is an optional element. Therefore, Sb does not have to be contained. Since Sb has an effect of affecting the convection of the molten pool during welding, increasing the penetration depth, and improving weldability, it may be contained as necessary. However, if Sb is contained in excess, it not only increases the susceptibility to weld cracking, but also leads to a decrease in corrosion resistance. Therefore, the Sb content is 0.010% or less. The preferred Sb content is 0.008% or less, and more preferably 0.006% or less. The preferred lower limit of the Sb content is 0.0005%, and more preferably 0.001%.
[0056] B: 0 to 0.0050% Boron (B) is an optional element. Therefore, B may not be contained. B is an element that contributes to grain boundary strengthening and improves hot workability, so it may be contained as necessary. However, if B is contained in excess, the effect is saturated, and further, liquation cracking occurs at the grain boundary of the heat-affected zone during welding. Therefore, the B content is 0.0050% or less. The preferred B content is 0.0030% or less, and more preferably 0.0015% or less. The preferred lower limit of the B content is 0.0001%, and more preferably 0.0003%.
[0057] Ca: 0 to 0.0200% Calcium (Ca) is an optional element. Therefore, Ca may not be contained. Ca has the effect of fixing S as sulfide and improving the hot workability of the alloy, so it may be contained as necessary. However, if Ca is contained in excess, coarse oxides are formed, and the hot workability of the alloy is rather reduced. Therefore, the Ca content is 0.0200% or less. The preferred Ca content is 0.0100% or less, and more preferably 0.0050% or less. The preferred lower limit of the Ca content is 0.0005%, and more preferably 0.0010%.
[0058] Magnesium: 0 to 0.0200% Magnesium (Mg) is an optional element. Therefore, Mg may not be contained. Like Ca, Mg has the effect of fixing S as sulfide and improving the hot workability of the alloy, so it may be contained as necessary. However, if Mg is contained in excess, coarse oxides are formed, and the hot workability of the alloy is rather reduced. Therefore, the Mg content is 0.0200% or less. The preferred Mg content is 0.0100% or less, more preferably 0.0050% or less, and even more preferably 0.0020% or less. The preferred lower limit of the Mg content is 0.0001%, more preferably 0.0005%.
[0059] REM: 0~0.100% Rare earth elements (REM) are optional elements. Therefore, REM may not be contained. Like Ca and Mg, REM has the effect of fixing S as sulfides and improving the hot workability of the alloy, so it may be contained as necessary. However, if REM is contained in excess, coarse oxides are formed, and the hot workability of the alloy is rather reduced. Therefore, the REM content is 0.100% or less. The preferred REM content is 0.050% or less, and more preferably 0.030% or less. The preferred lower limit of the REM content is 0.001%, and more preferably 0.005%.
[0060] In this embodiment, "REM" refers to Sc, Y, and lanthanoids, a total of 17 elements, and "REM content" refers to the content of one type of REM when there is one type, and the total content of two or more types when there are two or more types. REM is also generally supplied as misch metal, which is an alloy of multiple types of REM. For this reason, one or more individual elements may be added and contained, or they may be added in the form of misch metal, for example.
[0061] The Cr-Ni alloy pipe according to the present embodiment contains the above-mentioned elements, with the balance being Fe and impurities. Here, the term "impurities" refers to components that are mixed in due to various factors in raw materials such as ores and scraps and manufacturing processes during industrial production of alloy materials, and are permissible within a range that does not adversely affect the present invention.
[0062] It is preferable that the chemical composition of the Cr-Ni alloy tube according to this embodiment further satisfies the following formulas (iv) and (v). 9Mo+100N≧45.0 (iv) Ni+1.4Cu+Mo-0.9Cr-2Si-1.2Mn-5.7C+20N+90(0.15Nb+0.27V+0.3Ti)≦42.0 (v) In the above formula, the element symbols indicate the content (mass%) of each element, and zero is substituted if the element is not contained.
[0063] The present inventors analyzed the relationship between the mechanical properties and chemical composition of various Cr-Ni alloy pipes, and as a result, it became clear that in the above chemical composition, Mo and N especially contribute to the base strength. It was also found that by satisfying the above formula (iv), a stable high base strength can be obtained.
[0064] It is not necessary to set an upper limit to the value of 9Mo+100N, but from the viewpoint of suppressing deterioration of hot workability, it is preferably 85.0 or less, and more preferably 83.0 or less.
[0065] In addition, by focusing on the elements that affect the stacking fault energy and analyzing the relationship between mechanical properties and chemical composition, it was found that stable and excellent work-hardening ability can be obtained by satisfying the above formula (v).
[0066] There is no need to set a lower limit for the value on the left side of equation (v), and the lower the value, the better. However, the substantial lower limit is 1.2, taking into account the range of the content of each element.
[0067] The chemical composition of the Cr-Ni alloy tube according to the present embodiment preferably further satisfies the following formula (vi). As described above, when the degree of cold working is high, anisotropy tends to increase. However, by adjusting the N content so as to satisfy the following formula (vi) in relation to the tensile yield stress in the tube axis direction of the Cr-Ni alloy tube, it becomes easier to suppress the increase in anisotropy even when the tube has a strength of 900 MPa or more. 0.001×YS LT -0.820 <N<0.001×YS LT -0.740 (vi) YS LC : Compressive yield stress in the axial direction (MPa) N: N content in alloy tube (mass%)
[0068] 3. Manufacturing method An example of a method for producing a Cr-Ni alloy pipe according to this embodiment will be described.
[0069] First, the austenitic alloy is melted to produce molten metal. The alloy can be melted in an electric furnace, an Ar-O2 mixed gas bottom blowing decarburization furnace (AOD furnace), a vacuum decarburization furnace (VOD furnace), etc.
[0070] The molten metal is then used to produce a casting material, which may be, for example, an ingot, a slab, or a bloom. Specifically, an ingot is produced by an ingot casting method, or a slab or a bloom is produced by a continuous casting method.
[0071] Next, the cast material is hot worked to produce a round billet. The hot working is, for example, hot rolling or hot forging. The produced round billet is then hot worked to produce a mother pipe. Specifically, a mother pipe is produced from the round billet by an extrusion pipe-making process, typically the Ugine-Sejournet process. Alternatively, a mother pipe is produced from the round billet by the Mannesmann pipe-making process.
[0072] The produced mother pipe is subjected to cold working. Cold working includes cold drawing and cold rolling, typically Pilger rolling. Either cold drawing or cold rolling may be adopted in the present invention. Cold drawing imparts a large tensile strain to the alloy pipe in the axial direction, compared to cold rolling. Cold rolling imparts a large strain to the mother pipe not only in the axial direction but also in the circumferential direction. Therefore, cold rolling imparts a large compressive strain to the mother pipe in the circumferential direction, compared to cold drawing.
[0073] A preferable area reduction rate during cold working is 15% or more. Here, the area reduction rate is defined by the following formula (I). A preferable lower limit of the area reduction rate is 20%. On the other hand, if the area reduction rate is too high, not only the roundness of the alloy pipe decreases, but also the anisotropy becomes significant. Therefore, a preferable upper limit of the area reduction rate during cold working is 50%. Reduction of area (%) = 100 × (cross-sectional area of blank pipe before cold working – cross-sectional area of blank pipe after cold working) / cross-sectional area of blank pipe before cold working (I)
[0074] Other treatments may be performed between the hot working and the cold working. For example, a solution heat treatment may be performed on the hot-worked mother pipe. In this case, the mother pipe after the solution heat treatment is descaled to remove scale, and then cold working is performed. Furthermore, cold working may be performed multiple times. When cold working is performed multiple times, a solution heat treatment may be performed as a softening heat treatment between one cold working step and the next cold working step.
[0075] After the cold working, straightening processing using an inclined roll straightener and / or low-temperature heat treatment may be performed in order to reduce anisotropy. Either straightening processing or low-temperature heat treatment may be performed first. However, if the heat treatment temperature is too high, the yield stress is excessively reduced, making it impossible to maintain the strength required in the usage environment. Therefore, when low-temperature heat treatment is performed, the heating temperature is set to 300 to 550°C, and preferably 400 to 500°C.
[0076] There are no particular limitations on the dimensions of the alloy pipe obtained by the above processes, but from the viewpoint of maintaining the necessary strength in the usage environment, the wall thickness of the alloy pipe is preferably 4 mm or more, more preferably 6 mm or more, even more preferably 8 mm or more, and even more preferably 10 mm or more.
[0077] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples. EXAMPLES
[0078] An alloy having the chemical composition shown in Table 1 was melted and cast in a vacuum to obtain an ingot with an outer diameter of 120 mm and a weight of 30 kg. This ingot was hot forged to obtain a material with a thickness of 50 mm. The temperature of the ingot before hot forging was 1200 ° C. Furthermore, hot rolling was performed on the material. At this time, in order to change the product strength, the cold working rate shown in Table 2 was given, and then the thickness after cold rolling was calculated backwards to be unified to 11.5 mm, and the plate thickness of the intermediate alloy material (alloy plate) was determined. Then, a softening heat treatment was performed by heat treatment for 10 minutes at the temperature shown in Table 2 and then water cooling. Next, the cold working rate shown in Table 2 was given to unify the thickness to 11.5 mm. For Test Nos. 22 and 23, after cold working, a solution heat treatment was performed by heat treatment for 10 minutes at the temperature shown in Table 2 and then water cooling. In addition, for Test No. 24, cold working was not performed. In this embodiment, an alloy plate was used instead of an alloy tube from the viewpoint of ease of experimentation.
[0079] [Table 1]
[0080] [Table 2]
[0081] Next, the compressive yield stress YS in the tube axial direction was measured using the method described above. LC (MPa) and tensile yield stress YS LT(MPa) was obtained. Specifically, cylindrical test pieces for compression tests and round bar test pieces for tensile tests were taken from the center of the plate thickness of the alloy plate of each test number, with the longitudinal direction parallel to the rolling direction. The cylindrical test pieces had a parallel part diameter of 4 mm and a length of 8 mm. The round bar test pieces had a parallel part diameter of 4 mm and a gauge length of 20 mm. Compression tests were performed on the cylindrical test pieces for compression tests in air at room temperature (25°C) using a method in accordance with ASTM E9 (2019). The 0.2% offset yield strength obtained from the compression test was calculated as the compressive yield stress YS in the axial direction of the tube. LC (MPa). Furthermore, tensile tests were carried out on the round bar test pieces at room temperature (25°C) in air in accordance with ASTM E8 / E8M (2013). The 0.2% offset yield strength obtained from the tensile test was calculated as the tensile yield stress YS LT (MPa).
[0082] Furthermore, the tensile yield stress YS of the test piece after high-frequency induction heating and quenching was measured by the above-mentioned method. HT (MPa) was obtained. Specifically, a cylindrical test piece for high-frequency induction heating and quenching was taken from the center of the plate thickness of the alloy plate of each test number so that the longitudinal direction was parallel to the rolling direction. The cylindrical test piece was prepared in accordance with ASTM E8 / E8M (2021) and had a diameter of 6 mm and a gauge length of 30 mm. The cylindrical test piece for high-frequency induction heating and quenching was heated from room temperature to 1150 ° C at a heating rate of 100 ° C / s using a high-frequency induction heating device, and then heated to 1200 ° C at a heating rate of 25 ° C / s. At this time, the heating area by the high-frequency induction heating device was a region of 3.5 mm from the center in the longitudinal direction of the test piece to both ends and 7.0 mm in the longitudinal direction. The temperature of the test piece was measured using a thermocouple installed in the center of the longitudinal direction of the test piece.
[0083] The test piece was then held at 1200°C for 180 seconds. Immediately after holding, Ar gas was sprayed onto the test piece, and the test piece was rapidly cooled to room temperature at a cooling rate of 50°C / s in the temperature range from 1200°C to 800°C. Then, using the test piece after high-frequency induction heating and rapid cooling, a tensile test was carried out in air at room temperature (25°C) in accordance with JIS Z 2241 (2011), and the obtained 0.2% offset proof stress was calculated as the tensile yield stress YS HT (MPa).
[0084] The results are shown in Table 2. As shown in Table 2, the alloy materials satisfying all the requirements of the present invention have a high tensile yield stress of 780 MPa or more and a YS LC / YS LT It is possible to make it 0.80 or more. [Industrial Applicability]
[0085] According to the present invention, a Cr-Ni alloy pipe having high strength can be obtained while minimizing the difference between the compressive yield stress and the tensile yield stress. Therefore, by selecting the Cr-Ni alloy pipe according to the present invention as a material for oil country tubular goods, it is possible to obtain highly reliable oil country tubular goods that can maintain high strength even when softening occurs in the welded portion.
Claims
1. A Cr-Ni alloy tube, The tensile yield stress YS of the Cr-Ni alloy tube in the tube axis direction LT and compressive yield stress YS LC , and The Cr-Ni alloy tube was taken from the center of the wall thickness so that the longitudinal direction was parallel to the tube axis direction, and the test piece was heated from room temperature to 1150°C at a heating rate of 100°C / s using a high-frequency induction heating device, then heated to 1200°C at a heating rate of 25°C / s, held at 1200°C for 180 seconds, and then quenched to room temperature under conditions where the cooling rate in the temperature range from 1200°C to 800°C was 50°C / s by blowing Ar gas. The tensile yield stress YS of the test piece was obtained. HT but, The following formulas (i) to (iii) are satisfied: The chemical composition, in mass%, is C: 0.030% or less, Si: 0.50% or less, Mn: 1.00% or less, P: 0.030% or less, S: 0.0050% or less, Cr: 19.00-32.00%, Ni: 29.50-55.00%, Mo: 2.50-12.00%, Cu: 3.00% or less, V: 0.01-0.50%, Nb+Ti: 0.002-1.000%, Al: 0.001-0.500%, N: 0.005-0.400%, W: 0-1.00%, Co: 0-1.00%, Sn: 0 to 0.010%, As: 0 to 0.010%, Zn: 0 to 0.010%, Pb: 0 to 0.010%, Sb: 0 to 0.010%, B: 0 to 0.0050%, Ca: 0-0.0200%, Mg: 0 to 0.0200%, REM: 0-0.100%, The balance is Fe and impurities. Cr-Ni alloy tube. 0.80≦YS LC / YS LT <0.95 ・・・(i) ??? HT .....×. LT ≧.(ii) YS LT ≧443×YS LT / YS LC +2.28×YS HT -350 ・・・(iii) In the above formula, the meanings of each symbol are as follows: Y.S. LC : Compressive yield stress in the tube axial direction (MPa) Y.S. LT : Tensile yield stress in the tube axial direction (MPa) Y.S. HT : Tensile yield stress (MPa) of the test piece after high-frequency induction heating and quenching
2. The tensile yield stress YS of the Cr-Ni alloy tube in the tube axis direction LT is 780 MPa or more; The Cr-Ni alloy tube according to claim 1.
3. The chemical composition, in mass%, W: 0.01-1.00%, Co: 0.01 to 1.00%, Sn: 0.001 to 0.010%, As: 0.001 to 0.010%, Zn: 0.001-0.010%, Pb: 0.0005 to 0.010%, Sb: 0.0005 to 0.010%, B: 0.0001 to 0.0050%, Ca: 0.0005-0.0200%, Mg: 0.0001 to 0.0200%, and REM: 0.001-0.100%, Contains one or more selected from The Cr-Ni alloy tube according to claim 1.
4. The chemical composition further satisfies the following formulas (iv) and (v): The Cr-Ni alloy tube according to any one of claims 1 to 3. 9Mo+100N≧45.0...(iv) Ni+1.4Cu+Mo-0.9Cr-2Si-1.2Mn-5.7C+20N+90 (0.15Nb+0.27V+0.3Ti)≦42.0...(v) In the above formula, the element symbols indicate the content (mass%) of each element in the alloy tube, and zero is substituted if the element is not contained.
5. The chemical composition further satisfies the following formula (vi): The Cr-Ni alloy tube according to any one of claims 1 to 3. 0.001×YS LT -0.820<N<0.001×YS LT -0.740 ・・・(we) In the above formula, the meanings of each symbol are as follows: YS LT: Tensile yield stress in the tube axial direction (MPa) N: N content in alloy tube (mass%)
6. The chemical composition further satisfies the following formula (vi): The Cr-Ni alloy tube according to claim 4. 0.001×YS LT -0.820<N<0.001×YS LT -0.740 ・・・(we) In the above formula, the meanings of each symbol are as follows: YS LT: Tensile yield stress in the tube axial direction (MPa) N: N content in alloy tube (mass%)