Oxidation catalyst having entraps

The catalyst's unique zone structure and platinum distribution enhance resistance to phosphorus contamination, maintaining effective diesel exhaust purification by oxidizing carbon monoxide, hydrocarbons, and nitric oxide.

KR103044387B1Active Publication Date: 2026-11-06UMICORE AG & CO KG
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
KR1020227042715
Authority / Receiving Office
KR · KR
Patent Type
Patents
Current Assignee / Owner
Priority Date
2020-05-06
Filing Date
2021-05-06
Publication Date
2026-11-06
Estimated Expiration
2041-05-06

AI Technical Summary

Technical Problem

Existing oxidation catalysts for diesel engines are impaired by phosphorus contamination from oil additives, leading to reduced performance over their service life.

Method used

A catalyst design with distinct material zones, where material region B has a higher platinum group metal load and larger pore ratio than region A, providing enhanced resistance to phosphorus contamination, and is supported on a carrier substrate with specific pore distributions and materials like aluminum oxide.

Benefits of technology

The catalyst maintains effective oxidation of carbon monoxide, hydrocarbons, and nitric oxide in diesel exhaust, with reduced sensitivity to phosphorus compounds, ensuring prolonged catalyst efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 112022130688880-PCT00002_ABST
    Figure 112022130688880-PCT00002_ABST
Patent Text Reader

Abstract

The present invention relates to a catalyst comprising: a carrier substrate having a length L and having a first end a and a second end b; a material zone A containing a platinum group metal on a support material, said material zone A having a load of 40 to 150 g / l based on the volume of said carrier substrate; and a material zone B containing a platinum group metal on a support material, said material zone B having a load of 75 to 200 g / l based on the volume of said carrier substrate, said material zone B having a platinum group metal content greater than that of said material zone A, calculated in g / l based on the volume of said carrier substrate, and said material zone B having a ratio of 20 to 30% of pores having a diameter of 0.5 to 50 μm.
Need to check novelty before this filing date? Find Prior Art

Description

Technology Field

[0001] The present invention relates to an oxidation catalyst for purifying exhaust gas of a diesel engine, comprising a phosphorus trap. Background Technology

[0002] The raw exhaust gas from diesel engines consists of carbon monoxide (CO), hydrocarbons (HC), and nitrogen oxides (NO₂). x In addition, it contains a relatively high oxygen content of up to 15 vol%. It also includes particulate emissions resulting from the partial incomplete combustion of fuel in the cylinder, which are mainly composed of soot residues and, in some cases, organic agglomerates.

[0003] Diesel particulate filters with or without a catalytically active coating are suitable for removing particulate emissions, while nitrogen oxides can be converted to nitrogen by, for example, selective catalytic reduction (SCR) in a so-called SCR catalyst, and carbon monoxide and hydrocarbons are rendered harmless by oxidation in a suitable oxidation catalyst.

[0004] Oxidation catalysts are extensively disclosed in the literature. An oxidation catalyst is a so-called flow-through substrate, made of, for example, ceramic or metal, on which a precious metal, for example, platinum and palladium, is supported as a catalytic active component on a porous, high-melting-point oxide with a large surface area, for example, aluminum oxide.

[0005] A pre-zoned oxidation catalyst is also disclosed, having material zones of different compositions in the direction of exhaust gas flow, to which the exhaust gas comes into continuous contact.

[0006] For example, US2010 / 257843, US2011 / 099975 and WO2012 / 079598 A1 disclose a zoned oxidation catalyst containing platinum and palladium.

[0007] In addition to the components already mentioned, diesel engine exhaust gases frequently contain phosphorus compounds derived from oil additives. These phosphorus compounds are deposited on the diesel oxidation catalyst, impairing its oxidation capacity during its service life.

[0008] These problems and the possibility of solving them have already been disclosed in the literature.

[0009] For example, JP 2015066516A discloses a ternary catalyst containing a complex oxide of magnesium and cerium as an phosphate trap in the top layer.

[0010] JP2013146706A teaches a two-layer catalyst in which the lower layer contains a precious metal, the upper layer does not contain a precious metal or contains less precious metal than the lower layer, and the upper layer has a higher porosity than the lower layer.

[0011] There is still a need for oxidation catalysts that are effectively protected from phosphorus contamination throughout their entire service life.

[0012] Therefore, the present invention, as a catalyst,

[0013] · A carrier substrate having a first end a and a second end b and a length L,

[0014] · A material zone A containing a platinum group metal on a support material, wherein the load is 40 to 150 g / l based on the volume of the carrier substrate, and

[0015] · A material region B containing a platinum group metal on a support material, wherein the material region B is a load of 75 to 200 g / l based on the volume of the carrier substrate, and

[0016] The present invention relates to a catalyst in which material region B has a platinum group metal content greater than material region A, calculated in g / l based on the volume of the carrier substrate, and material region B has a ratio of 20 to 30% of pores with a diameter of 0.5 to 50 μm.

[0017] Material region B contains, for example, only platinum, only palladium, or platinum and palladium as platinum group metals. It is particularly preferable that the weight ratio of platinum and palladium be 20:1 to 1:5, and a weight ratio of 10:1 to 1:3 is preferred.

[0018] In material zone B, the platinum group metal is present in an amount of particularly 0.53 to 2.5 g / l, preferably 0.60 to 1.4 g / l, based on the volume of the carrier substrate.

[0019] Material zone B has a ratio of 20 to 30% of pores with a diameter of 0.5 to 50 μm.

[0020] In the context of this application, the ratio of pores is understood to mean the volume of pores relative to the total volume. Accordingly, in the case of the present invention, for example, a ratio of pores in material zone B of 20% means that 20% of the total volume of material zone B is formed of pores with a diameter of 0.5 to 50 μm.

[0021] The ratio of voids in the material region or catalyst region can be measured by a method comprising the following steps:

[0022] · Step of selecting the catalyst region to be investigated,

[0023] · A step of generating a cross-section of the catalyst region to be investigated, wherein the pores are filled with an organic resin,

[0024] · A step of generating an image of the cross-section using a scanning electron microscope (SEM),

[0025] · Step of selecting the area to be examined within the SEM image,

[0026] · A step of converting a selected partial region of the SEM image into a binary image using an image analysis program,

[0027] · A step of measuring the ratio of the pores after performing a porosity distribution calculation using the binary image using an image analysis program.

[0028] To create a cross-section of a catalyst region in which the pores are filled with an organic resin, a cross-section method known to those skilled in the art may be used.

[0029] The generation of cross-sectional images by scanning electron microscopy (SEM) is also performed according to methods known and comprehensively disclosed. Specific measurement conditions are not critical, that is, they do not affect the final result. In this case, the detection of backscattered primary electrons is used as the imaging method. These backscattered primary electrons provide signal intensity that depends on the average atomic number of the material being irradiated. Thus, heavier atoms scatter more and appear brighter, while lighter atoms appear darker. Consequently, in the obtained SEM image, pores appear dark gray to black, while the material of the washcoat appears brighter. FIG. 1 shows an SEM image of the catalyst of Example 1 below generated in this manner, in which the support and the two material regions A and B can be easily distinguished from each other. In the next step, a partial region or multiple partial regions to be irradiated in the SEM image, for example, a region of the material region, is selected, and a binary image is generated using a threshold method with image analysis software. In the context of the present invention, image analysis software was programmed using Matlab version 2019 and the attached image processing toolbox. FIG. 2 shows a binary image generated from the SEM image of FIG. 1 using image analysis software. In the image, voids appear in black, and the material of the washcoat appears in white. Gray areas are unselected areas of interest. Subsequently, the ratio of voids is calculated through a morphological image processing method using image analysis software. To perform void analysis, in addition to the Matlab programming image analysis software, other programs known to those skilled in the art, such as the ImageJ program which can be adjusted as needed as a programming plugin, may also be used.

[0030] The support material of material zone B may be aluminum oxide, doped aluminum oxide, silicon oxide, magnesium oxide, titanium oxide, or a mixture of two or more of these materials, or a mixed oxide or a complex oxide. However, the support material of material zone B is specifically aluminum oxide.

[0031] Material region A contains, for example, only platinum, only palladium, or platinum and palladium as platinum group metals. A weight ratio of platinum to palladium is particularly preferred to be 20:1 to 1:5, and a weight ratio of 15:1 to 1:1 is preferred.

[0032] In material region A, the platinum group metal is present in an amount of 0.18 to 1.4 g / l, particularly 0.25 to 0.7 g / l, based on the volume of the carrier substrate.

[0033] The platinum group metal of material region A is present on the support material. For this purpose, any material familiar to those skilled in the art is considered as the support material. In particular, it is selected from the group consisting of aluminum oxide, doped aluminum oxide, silicon oxide, magnesium oxide, titanium oxide, and a mixture or mixed oxide or complex oxide of two or more of these materials, having a BET surface area of ​​30 to 250 m² / g, preferably 100 to 200 m² / g (measured according to DIN 66132).

[0034] Aluminum oxide, magnesium / aluminum mixed oxide, and aluminum / silicon mixed oxide are preferred.

[0035] In addition, for example, aluminum oxide doped with 1 to 10 wt%, particularly 3 to 6 wt%, lanthanum oxide can also be used.

[0036] The ratio of pores in material zone A is not important. It is preferable that the ratio of pores with a diameter of 0.5 to 50 μm in material zone A is 10 to 30%.

[0037] In the oxidation catalyst according to the present invention, the loading of material region B is expressed in g / l in each case and is preferably higher than the loading of material region A based on the volume of the carrier substrate.

[0038] The loading of material zone B is preferably 75 to 150 g / l. The loading of material zone A is preferably 50 to 75 g / l.

[0039] Material region A and material region B can be arranged on the carrier substrate in different ways.

[0040] In a preferred embodiment, material region A is coated over the entire length L of the carrier substrate, while material region B extends from the first end a of the carrier substrate over 20 to 80%, preferably 30 to 70% of the length L, and is located on material region A.

[0041] In a further preferred embodiment, material region A extends from a second end of the carrier substrate for 40 to 60% of length L, while material region B extends from a first end of the carrier substrate for 40 to 60% of length L, wherein,

[0042] L = L A + L B or

[0043] L < L A + L B or

[0044] L > L A + L B And,

[0045] L A is the length of material region A, and L B is the length of material region B.

[0046] L > L A + L BIn this case, it means that a portion of the support remains without the coating. In particular, in this case, a gap of at least 0.5 cm in length, i.e., for example, 0.5 to 1 cm, remains between material zone A and material zone B.

[0047] The catalyst according to the present invention comprises a support. The support is particularly a through-flow substrate, but may also be a wall-flow filter.

[0048] A wall-flow filter is a carrier substrate comprising channels of length L extending parallel between a first end and a second end of the wall-flow filter, alternately closed at the first end or the second end, and separated by porous walls. A through-flow substrate differs from a wall-flow filter in that channels of length L are open at both ends.

[0049] Wall-flow filters have a porosity of, for example, 30 to 80%, and particularly 50 to 75% in the uncoated state. In the uncoated state, their average pore diameter is, for example, 5 to 30 μm.

[0050] Generally, the pores of a wall-flow filter are so-called open pores, meaning they are connected to channels. Additionally, the pores are typically interconnected. This enables, on the one hand, easy coating of the internal pore surfaces, and on the other hand, allows for the easy passage of exhaust gases through the porous walls of the wall-flow filter.

[0051] Similar to wall-flow filters, through-flow materials are known to those skilled in the art and are available on the market. Through-flow materials are made of, for example, silicon carbide, aluminum titanate, or cordierite.

[0052] The catalyst according to the present invention may be prepared by a method familiar to those skilled in the art, for example, by a conventional dip-coating method using a washcoat, i.e., an aqueous suspension of components forming individual material zones, or by a pump and suction coating method. A post-heat treatment (calcination) may follow.

[0053] Those skilled in the art know that, in the case of a wall-flow filter, its average pore size and the average particle size of the coating material can be matched so as to be placed on the porous wall forming the channels of the wall-flow filter (wall-coating). The average particle size of the coating material can be selected to be located within the porous wall forming the channels of the wall-flow filter, that is, the internal pore surfaces are coated (wall-coating). In this case, the average particle size of the coating materials must be small enough to penetrate into the pores of the wall-flow filter.

[0054] In another aspect of the present invention, a carrier substrate composed of a corrugated sheet of an inert material is used. Such a carrier substrate is known to those skilled in the art as a "corrugated substrate." Suitable inert materials are, for example, fibrous materials having an average fiber diameter of 50 to 250 μm and an average fiber length of 2 to 30 mm. Preferably, the fibrous material is heat-resistant and consists of silicon dioxide, in particular glass fibers.

[0055] To manufacture such a carrier substrate, the sheets of the fibrous material are, for example, corrugated in a known manner, and the individual corrugated sheets are formed into a cylindrical monolithic structural body having channels penetrating the body. Preferably, the monolithic structural body having a crosswise corrugated structure is formed by stacking a plurality of corrugated sheets into parallel layers with different corrugation directions between the layers. In one embodiment, non-corrugated (i.e., flat) sheets may be arranged between the corrugated sheets.

[0056] A substrate made of a corrugated sheet can be directly coated with material zone A and material zone B, but it is preferable that the substrate be first coated with an inert material, for example, titanium dioxide, and then coated with a catalytic material.

[0057] The catalyst according to the present invention is highly suitable for the oxidation of carbon monoxide, hydrocarbons, and nitric oxide in the exhaust gas of a diesel engine. In this process, the catalyst according to the present invention is much less sensitive to contamination by phosphorus compounds than catalysts known to date.

[0058] In addition, the present invention relates to a method for purifying exhaust gas of a vehicle operated by a lean-burn engine, for example, a diesel engine, characterized by passing the exhaust gas over a catalyst according to the present invention, wherein the exhaust gas enters at a first end a of a carrier substrate and exits again at a second end b. Specific details for implementing the invention

[0059] Example 1

[0060] a) A commercially available circular through-flow cordierite substrate with dimensions of 5.66" x 4.00", a cell density of 400 cpsi, and a wall thickness of 4 mil was coated over its entire length with a washcoat containing 0.353 g / l of platinum and palladium in a 12:1 mass ratio, supported on commercially available aluminum oxide doped with 5% silicon oxide. The washcoat loading was 60 g / l. The void ratio measured by the above method (see FIGS. 1 and 2) was 15%.

[0061] b) In the second step, the catalyst obtained in step a) was coated with a washcoat containing 0.79 g / l of platinum and palladium in a 1:1 mass ratio, supported on highly porous aluminum oxide, starting from one end and extending over 75% of its length. The washcoat loading was 110 g / l. The pore ratio of the layer applied in the second step (pores have a diameter of 0.5 to 50 µm), measured by the above method (see Figures 1 and 2), was 24%.

[0062] The obtained catalyst is hereinafter referred to as K1.

[0063] Example 2

[0064] a) A commercially available circular through-flow cordierite substrate with dimensions of 5.66" x 4.00", a cell density of 400 cpsi, and a wall thickness of 4 mil was coated with a washcoat containing 0.353 g / l of platinum and palladium in a mass ratio of 12:1, supported on commercially available aluminum oxide doped with 5% silicon oxide, over 50% of its length. The washcoat loading was 60 g / l. The void ratio measured by the above method was 15%.

[0065] b) In the second step, the catalyst obtained in step a) was coated with a washcoat containing 1.4 g / l of platinum and palladium in a 1:1 mass ratio, supported on highly porous aluminum oxide, starting from the uncoated end and extending 50% of its length. The washcoat loading was 75 g / l. The pore ratio of the layer applied in the second step (pores have a diameter of 0.5 to 50 µm), as measured by the above method, was 24%.

[0066] The obtained catalyst is hereinafter referred to as K2.

[0067] Comparative Example 1

[0068] Example 1 was repeated except for the difference that the washcoat loading in step b) was only 60 g / l.

[0069] The obtained catalyst is hereinafter referred to as VK1.

[0070] Comparative Example 2

[0071] a) A commercially available circular through-flow cordierite substrate with dimensions of 5.66" x 4.00", a cell density of 400 cpsi, and a wall thickness of 4 mil was coated with a washcoat containing 0.353 g / l of platinum and palladium in a 3:1 mass ratio, supported on commercially available aluminum oxide doped with 5% silicon oxide, over 50% of its length. The washcoat loading was 100 g / l. The pore ratio (pores with a diameter of 0.5 to 50 µm) measured by the above method was 15%.

[0072] b) In the second step, the catalyst obtained in step a) was coated with a washcoat containing 1.4 g / l of platinum and palladium in a mass ratio of 3:1, supported on highly porous aluminum oxide, starting from the uncoated end and extending 50% of its length. The washcoat loading was 100 g / l. The pore ratio of the layer applied in the second step (pores have a diameter of 0.5 to 50 µm), as measured by the above method, was 15%.

[0073] The obtained catalyst is hereinafter referred to as VK2.

[0074] Comparative test

[0075] a) Catalysts K1, K2, VK1 and VK2 were aged at 650°C with 7% humidity for 50 hours.

[0076] b) A phosphorus-containing oil additive was added to the fuel, and the aged catalyst was aged on an engine test bench for 10, 20, 30, and 40 hours. The addition of the oil additive was calculated for an exposure of 0.6 g / l of P per hour.

[0077] c) For the catalyst treated with phosphorus according to step b), the time (THC slip) at which the loaded hydrocarbon breaks through without further oxidation was measured. To this end, the same amount of diesel was added to all catalysts to generate heat, and the HC slip was measured during this process. It was also measured whether the target temperature of 575°C was reached.

[0078] d) Result

[0079]

[0080] K1 is the only catalyst that reaches a target temperature of 575°C for an exposure of 24 g / L. VK1, which has a lower washcoat loading in material zone B, already reached 525°C at 18 g / L in the above test.

[0081] Compared to VK2, K2 is more resistant to phosphorus and is depleted by a breakthrough of 5,000 ppm HC at 540°C at only 12 g / L P, whereas VK2 is depleted by a breakthrough of 8,000 ppm HC at 490°C at the same exposure.

Claims

Claim 1 As a catalyst, the carrier substrate having a first end a and a second end b and a length L; a material zone A containing a platinum group metal on a support material, said material zone A having a load of 40 to 150 g / l based on the volume of said carrier substrate; and a material zone B containing a platinum group metal on a support material, said material zone B having a load of 75 to 200 g / l based on the volume of said carrier substrate, said material zone B having a platinum group metal content greater than that of said material zone A, calculated in g / l based on the volume of said carrier substrate, said material zone B having a ratio of 20 to 30% of pores having a diameter of 0.5 to 50 μm, said carrier substrate is coated with said material zone A and said material zone B, said material zone A is coated over the entire length L of said carrier substrate, while said material zone B is coated from the first end a of said carrier substrate over a length L of 20 Extending over 80%, wherein the material region B is located on the material region A, or wherein the material region A extends over 40 to 60% of the length L from the second end of the carrier substrate, while the material region B extends over 40 to 60% of the length L from the first end of the carrier substrate, where L = L A + L B or L < L A + L B or L > L A + L B and,L A is the length of material region A, and L B is a catalyst, which is the length of material region B. Claim 2 A catalyst according to claim 1, characterized in that material region A contains palladium and platinum as platinum group metals. Claim 3 A catalyst according to paragraph 2, characterized in that the weight ratio of platinum to palladium in material zone A is 20:1 to 1:

5. Claim 4 A catalyst according to any one of claims 1 to 3, characterized in that the platinum group metal of material region A is present in an amount of 0.18 to 0.53 g / l based on the volume of the carrier substrate. Claim 5 A catalyst characterized in that, in any one of claims 1 to 3, material region B contains platinum and palladium as platinum group metals. Claim 6 A catalyst according to claim 5, characterized in that the weight ratio of platinum to palladium in material zone B is 20:1 to 1:

5. Claim 7 A catalyst according to any one of claims 1 to 3, characterized in that the platinum group metal of material region B is present in an amount of 0.53 to 1.06 g / l based on the volume of the carrier substrate. Claim 8 A catalyst according to any one of claims 1 to 3, characterized in that material region A is coated over the entire length L of the carrier substrate, while material region B extends from a first end a of the carrier substrate over 40 to 80% of the entire length L, and material region B is located on material region A. Claim 9 A catalyst characterized in that, in any one of claims 1 to 3, the carrier substrate is a flow-through substrate. Claim 10 A catalyst characterized in that, in any one of claims 1 to 3, the ratio of the pores is measured by a method comprising the following steps: · selecting a catalyst region to be irradiated; · generating a cross-section of the catalyst region to be irradiated, wherein the pores are filled with an organic resin; · generating an image of the cross-section using a scanning electron microscope (SEM); · selecting a partial region to be irradiated from the SEM image; · converting the selected partial region of the SEM image into a binary image using an image analysis program; and · measuring the ratio of the pores after performing a porosity distribution calculation using the binary image using an image analysis program. Claim 11 A method for purifying exhaust gas of a vehicle operated by a lean-burn engine, characterized by passing the exhaust gas over a catalyst described in any one of claims 1 to 3, wherein the exhaust gas enters the catalyst at a first end a of a carrier substrate and exits again at a second end b.

Citation Information

Patent Citations

  • Architectural diesel oxidation catalyst for enhanced no2 generator

    KR1020130129241A

  • Catalyst for the reduction of nitrogen oxides

    KR1020210053342A

  • Zoned Catalysts for Diesel Applications

    US20100257843A1

  • Diesel oxidation catalyst having a capture region for exhaust gas impurities

    WO2017093720A1