Bonding wire for semiconductor devices

A Cu-based bonding wire with a Ni-coated Cu core and controlled Au/Ni surface composition addresses galvanic corrosion and FAB shape issues, providing reliable bonding and reduced clogging for high-temperature applications.

KR103044706B1Active Publication Date: 2026-11-06NIPPON STEEL CHEM & MATERIAL CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
KR1020237043684
Authority / Receiving Office
KR · KR
Patent Type
Patents
Current Assignee / Owner
Priority Date
2021-06-25
Filing Date
2022-03-23
Publication Date
2026-11-06
Estimated Expiration
2042-03-23

AI Technical Summary

Technical Problem

Conventional Cu bonding wires face issues with galvanic corrosion, poor FAB shape, and insufficient bonding reliability under high-temperature environments, particularly in vehicle-mounted and power devices, which are inadequate for high-density packaging and continuous bonding.

Method used

A Cu-based bonding wire with a coating layer containing Ni as the main component on the core material side and Au and Ni on the surface side, with specific concentration ratios and thickness, along with optional additives like Pd, B, P, Mg, Se, Te, As, Sb, Ga, Ge, and In, to enhance bonding reliability and FAB shape.

Benefits of technology

The proposed wire achieves good FAB shape, reliable bonding performance at both the first and second joints, even under harsh high-temperature conditions, and reduces capillary clogging, ensuring high productivity in semiconductor device manufacturing.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 112023141731602-PCT00005_ABST
    Figure 112023141731602-PCT00005_ABST
Patent Text Reader

Abstract

A novel Cu bonding wire is provided that, along with a good FAB shape, has good bonding performance in the second junction and further provides good bonding reliability in the first junction under high temperature environments. The bonding wire for a semiconductor device comprises a core material made of Cu or a Cu alloy and a coating layer containing a conductive metal other than Cu formed on the surface of the core material, wherein the coating layer has a region with Ni as the main component on the core material side in the thickness direction of the coating layer and a region containing Au and Ni on the wire surface side, wherein the thickness of the coating layer is 10 nm or more and 130 nm or less, the ratio of the concentration of Au CAu (mass%) and the concentration of Ni CNi (mass%) for the entire wire CAu / CNi is 0.02 or more and 0.7 or less, and the concentration of Au on the surface of the wire is 10 atomic% or more and 90 atomic% or less.
Need to check novelty before this filing date? Find Prior Art

Description

Technology Field

[0001] The present invention relates to a bonding wire for a semiconductor device. Furthermore, the invention relates to a semiconductor device comprising said bonding wire. Background Technology

[0002] In semiconductor devices, electrodes formed on a semiconductor chip are connected to electrodes on a lead frame or substrate using bonding wires. The bonding wire connection method generally involves a thermal compression method combined with ultrasonics, and general-purpose bonding devices and capillary jigs used to pass the bonding wire through for connection are utilized. The connection process is completed by first bonding to an electrode on the semiconductor chip, forming a loop, and then second bonding the wire portion to an external electrode on a lead frame or substrate. For the first bonding, the tip of the wire is heated and melted by arc heat input to form a free air ball (FAB; hereinafter also simply referred to as "ball" or "FAB") due to surface tension, and then the ball portion is compressed and bonded to an electrode on the semiconductor chip (hereinafter referred to as "ball bonding"). Additionally, for the second bonding, the wire portion is compressed and bonded to an external electrode by applying ultrasonics and a load without forming a ball (hereinafter referred to as "wedge bonding").

[0003] Until now, gold (Au) has been the mainstream material for bonding wires, but replacement with copper (Cu) is progressing, mainly for LSI applications (e.g., Patent Documents 1 to 3). Furthermore, against the backdrop of the recent proliferation of electric and hybrid vehicles, replacement with high-efficiency and high-reliability Cu is expected for applications in vehicle-mounted devices, and furthermore, for applications in power devices (power semiconductor devices) in high-power equipment such as air conditioners and solar power generation systems, due to high thermal conductivity and melting current.

[0004] Cu has the drawback of being more prone to oxidation than Au, so as a method to prevent surface oxidation of the Cu bonding wire, a structure in which the surface of the Cu core material is coated with a metal such as Pd or Ni has been proposed (Patent Document 4). In addition, a Pd-coated Cu bonding wire has been proposed in which the surface of the Cu core material is coated with Pd and Pd and Pt are added to the Cu core material to improve the bonding reliability of the first joint (Patent Document 5). Prior art literature

[0005] Japanese Patent Publication No. Sho 61-48543, Japanese Patent Publication No. 2018-503743, International Publication No. 2017 / 221770, Japanese Patent Publication No. 2005-167020, International Publication No. 2017 / 013796 The problem to be solved

[0006] Vehicle-mounted devices and power devices tend to be exposed to higher temperatures during operation compared to general electronic devices, so the bonding wires used are required to exhibit good bonding reliability under harsh high-temperature environments.

[0007] The inventors conducted an evaluation based on characteristics required for vehicle-mounted devices and found that in conventional Cu bonding wires with a Pd coating layer, galvanic corrosion occurs under high-temperature environments, and thus sufficient bonding reliability at the second joint is not obtained. On the other hand, regarding bare Cu bonding wires without a Pd coating layer, galvanic corrosion does not occur, but the FAB shape is poor, and furthermore, the crimping shape of the first joint is inferior, so not only is it insufficient to accommodate the narrow pitch connections required for high-density packaging, but sufficient bonding reliability at the first joint is not obtained under high-temperature environments.

[0008] We investigated Cu-based bonding wires that achieve a good FAB shape and exhibit minimal deterioration in bonding reliability even under harsh high-temperature environments required for vehicle-mounted devices, and confirmed that Ni-coated Cu bonding wires, in which the surface of a Cu core material is coated with Ni, show reasonably good results in terms of FAB shape and bonding reliability under high-temperature environments. However, regarding Ni-coated Cu bonding wires, it was found that in some cases, sufficient bonding performance (bonding performance of the second joint immediately after bonding) is not obtained.

[0009] As described above, there is a desire to develop a Cu-based bonding wire that has a good FAB shape, good bonding performance in the second joint, and furthermore, good bonding reliability in high-temperature environments, particularly improved bonding reliability in the first joint.

[0010] The present invention provides a novel Cu bonding wire that has a good FAB shape, good bonding performance in the second joint, and further provides good bonding reliability in the first joint under high temperature environments. means of solving the problem

[0011] The inventors, after carefully examining the above problem, discovered that the problem could be solved by having the following configuration, and thus completed the present invention.

[0012] That is, the present invention includes the following contents.

[0013] [1] A bonding wire for a semiconductor device comprising a core material made of Cu or a Cu alloy and a coating layer containing a conductive metal other than Cu formed on the surface of the core material, and

[0014] The coating layer has a region with Ni as the main component on the core material side in the thickness direction of the coating layer, and also has a region containing Au and Ni on the wire surface side.

[0015] The thickness of the coating layer is 10 nm or more and 130 nm or less, and

[0016] Concentration of Au C across the entire wire Au (Mass%) and Ni concentration C Ni Ratio C of (mass %) Au / C Ni α is 0.02 or greater and 0.7 or less, and

[0017] A bonding wire for a semiconductor device having an Au concentration of 10 atomic% or more and 90 atomic% or less on the surface of the wire.

[0018] [2] A bonding wire described in [1], in which the concentration of Au on the surface of the wire is measured by Auger electron spectroscopy (AES) under the following <conditions>.

[0019] <Condition> Position the wire so that the center of the wire width becomes the center of the measuring surface width, and additionally, the measuring surface width is between 5% and 15% of the wire diameter, and the length of the measuring surface is five times the measuring surface width.

[0020] [3] A bonding wire described in [1] or [2], wherein the coating layer further contains Pd as a conductive metal other than Cu.

[0021] [4] Total concentration of Ni, Au, and Pd for the entire wire C M (Mass%) and Ni concentration C Ni Ratio C of (mass %) Ni / C M A bonding wire described in any of [1] to [3] that is 0.5 or more.

[0022] [5] A bonding wire described in any one of [1] to [4], in which the maximum concentration of Ni in the depth direction concentration profile of the wire is 80 atomic% or more.

[0023] [6] A bonding wire described in [5], the depth-direction concentration profile of the wire obtained by measuring Auger electron spectroscopy (AES) under the following <conditions> as Ar sputtering is performed from the surface of the wire in the depth direction.

[0024] <Condition> Position the wire so that the center of the wire width becomes the center of the measuring surface width, and additionally, the measuring surface width is between 5% and 15% of the wire diameter, and the length of the measuring surface is five times the measuring surface width.

[0025] [7] When a Free Air Ball (FAB) is formed using a wire, the crystal orientation of the cross-section perpendicular to the compression bonding direction of the FAB is measured, and the angle difference with respect to the compression bonding direction is 15 degrees or less <100> A bonding wire described in any of [1] to [6] having a crystal orientation ratio of 30% or more.

[0026] [8] An angle difference of 15 degrees or less with respect to the direction of compression bonding <100> Bonding wire described in [7], with a crystal orientation ratio of 50% or more.

[0027] [9] A bonding wire described in any of [1] to [8], having a coating layer thickness of 18 nm or more.

[0028]

[10] A bonding wire described in any one of [1] to [9] comprising one or more elements selected from the group consisting of B, P and Mg (hereinafter referred to as “first additive element”), wherein the total concentration of the first additive element over the entire wire is 1 mass ppm or more and 100 mass ppm or less.

[0029]

[11] A bonding wire described in any one of [1] to

[10] , comprising one or more elements selected from the group consisting of Se, Te, As and Sb (hereinafter referred to as “second addition element”), wherein the total concentration of the second addition element over the entire wire is 1 mass ppm or more and 100 mass ppm or less.

[0030]

[12] A bonding wire described in any one of [1] to

[11] , comprising one or more elements selected from the group consisting of Ga, Ge and In (hereinafter referred to as “third additive element”), wherein the total concentration of the third additive element in the entire wire is 0.011 mass% or more and 1.5 mass% or less.

[0031]

[13] A semiconductor device comprising a bonding wire as described in any of [1] to

[12] . Effects of the invention

[0032] According to the present invention, a novel Cu bonding wire can be provided that has a good FAB shape, good bonding performance in the second joint, and furthermore, good bonding reliability of the first joint under high temperature environments. Brief explanation of the drawing

[0033] Figure 1 is a schematic diagram illustrating the position and dimensions of the measurement surface when performing composition analysis by AES. Figure 2 is a schematic diagram illustrating a cross-section perpendicular to the compression bonding direction of the FAB. Specific details for implementing the invention

[0034] The present invention will be described in detail below based on suitable embodiments thereof. Although reference may be made to the drawings during the description, each drawing merely shows the shape, size, and arrangement of components in a schematic manner to the extent that the invention can be understood. The present invention is not limited to the following embodiments and examples, and may be implemented with arbitrary modifications within the scope of the claims of the present invention and their equivalents without departing from the scope of the claims and equivalents thereof.

[0035] [Bonding wire for semiconductor devices]

[0036] The bonding wire for a semiconductor device according to the present invention (hereinafter simply referred to as "the wire of the present invention" or "the wire") is,

[0037] A core material made of Cu or a Cu alloy, and

[0038] It includes a coating layer containing a conductive metal other than Cu formed on the surface of the core material, and

[0039] The coating layer has a region with Ni as the main component on the core material side in the thickness direction of the coating layer, and also has a region containing Au and Ni on the wire surface side.

[0040] The thickness of the coating layer is 10 nm or more and 130 nm or less, and

[0041] Concentration of Au C across the entire wire Au (Mass%) and Ni concentration C Ni Ratio C of (mass %) Au / C Ni α is 0.02 or greater and 0.7 or less, and

[0042] It is characterized by the concentration of Au on the surface of the wire being 10 atomic percent or more and 90 atomic percent or less.

[0043] As described above, bonding wires used in vehicle-mounted devices or power devices are required to exhibit good bonding reliability under harsh high-temperature environments. For example, bonding wires used in vehicle-mounted devices require bonding reliability under high-temperature environments exceeding 150°C. The inventors conducted an evaluation based on the characteristics required for vehicle-mounted devices and found that in conventional Cu bonding wires with a Pd coating layer, galvanic corrosion occurs under high-temperature environments, and in some cases, sufficient bonding reliability is not obtained at the second joint. Furthermore, regarding bare Cu bonding wires without a Pd coating layer, although galvanic corrosion does not occur, the FAB shape is poor, and furthermore, the crimping shape of the first joint is inferior, making it insufficient to support the narrow-pitch connections required for high-density packaging. In addition, there are cases where sufficient bonding reliability is not obtained at the first joint under high-temperature environments.

[0044] We investigated Cu-based bonding wires that achieve a good FAB shape and exhibit minimal deterioration in bonding reliability even under harsh high-temperature environments required for vehicle-mounted devices, and confirmed that Ni-coated Cu bonding wires, in which the surface of a Cu core material is coated with Ni, show reasonably good results in terms of FAB shape and bonding reliability under high-temperature environments. However, regarding Ni-coated Cu bonding wires, it was found that in some cases, sufficient bonding performance (bonding performance of the second joint immediately after bonding) is not obtained. Furthermore, it was found that when bonding is performed using Ni-coated Cu bonding wires, wire cutting chips accumulate inside the capillary jig, causing clogging (hereinafter this phenomenon is also referred to as "capillary clogging"), which may hinder continuous bonding.

[0045] In contrast, the bonding wire for a semiconductor device comprises a core material made of Cu or a Cu alloy and a coating layer containing a conductive metal other than Cu formed on the surface of the core material, wherein the coating layer has a region mainly composed of Ni on the core material side and a region containing Au and Ni on the wire surface side in the thickness direction of the coating layer, the thickness of the coating layer is 10 nm or more and 130 nm or less, and the concentration of Au C over the entire wire Au (Mass%) and Ni concentration C Ni Ratio C of (mass %) Au / C Ni The inventors have discovered that a bonding wire having a value of 0.02 or more and 0.7 or less, and an Au concentration of 10 atomic% or more and 90 atomic% or less on the wire surface, provides a good FAB shape, good bonding performance at the second junction, and good bonding reliability at the first junction under high temperature environments. Furthermore, with such a wire, the occurrence of capillary clogging during continuous bonding can be suppressed, making it possible to maintain good productivity of the semiconductor device. Thus, the present invention significantly contributes to the practical application and promotion of Cu bonding wires for vehicle-mounted devices, etc.

[0046] <Cu 또는 Cu 합금으로 이루어지는 코어재>

[0047] The wire of the present invention comprises a core material made of Cu or a Cu alloy (hereinafter also simply referred to as "Cu core material").

[0048] The Cu core material is not particularly limited as long as it is made of Cu or a Cu alloy, and a known Cu core material constituting a conventional Pd-coated Cu wire known as a bonding wire for semiconductor devices may be used.

[0049] In the present invention, the concentration of Cu in the Cu core material can be, for example, 97 atomic% or more, 97.5 atomic% or more, 98 atomic% or more, 98.5 atomic% or more, 99 atomic% or more, 99.5 atomic% or more, 99.8 atomic% or more, 99.9 atomic% or more, or 99.99 atomic% or more at the center (axial part) of the Cu core material.

[0050] The Cu core material may contain one or more dopants selected from, for example, the first, second, and third additive elements described below. Suitable content of these dopants is as described below.

[0051] In one embodiment, the Cu core material consists of Cu and unavoidable impurities. In another embodiment, the Cu core material consists of Cu, one or more elements selected from the first, second, and third additive elements described below, and unavoidable impurities. Furthermore, the term "unavoidable impurities" used with respect to the Cu core material also includes elements constituting a coating layer containing a conductive metal other than Cu described below.

[0052] <Cu 이외의 도전성 금속을 함유하는 피복층>

[0053] The wire of the present invention comprises a coating layer containing a conductive metal other than Cu formed on the surface of a Cu core material (hereinafter also simply referred to as a “coating layer”). Although a suitable composition of the coating layer will be described later, in the wire of the present invention, it is preferable that the concentration of the conductive metal other than Cu in the coating layer be 50 atomic% or more.

[0054] In order to achieve a good FAB shape, good bonding performance in the 2nd joint, and furthermore, good bonding reliability in the 1st joint under high temperature environments, it is important that the coating layer of the wire of the present invention satisfies all of the following conditions (1) to (4).

[0055] (1) In the thickness direction of the coating layer, the core material side has a region with Ni as the main component, and the wire surface side has a region containing Au and Ni.

[0056] (2) The thickness of the coating layer is 10 nm or more and 130 nm or less.

[0057] (3) Concentration of Au C throughout the wire Au (Mass%) and Ni concentration C Ni Ratio C of (mass %) Au / C Ni It contains Au and Ni such that the value is between 0.02 and 0.7.

[0058] (4) The wire contains Au such that the concentration of Au on the surface is 10 atomic% or more and 90 atomic% or less.

[0059] -Condition (1)-

[0060] Condition (1) relates to a coating layer having a region with Ni as the main component on the core material side and a region containing Au and Ni on the wire surface side in the thickness direction of the coating layer.

[0061] In the combination of conditions (2) to (4), by including a coating layer that satisfies condition (1), the wire of the present invention has good bonding reliability at the 1st junction under good FAB shape or high temperature environment, and also has excellent bonding performance at the 2nd junction. In addition, by including a coating layer that satisfies condition (1), capillary clogging during continuous bonding can be suppressed, making it possible to maintain good productivity of the semiconductor device.

[0062] In condition (1), the coating layer has a region on the core material side in the thickness direction of the coating layer in which Ni is the main component. In the present invention, the "region in which Ni is the main component" referred to with respect to the coating layer means a region in which the concentration of Ni is 50 atomic% or more. As described below, the coating layer may include Au on the wire surface side in addition to Ni as a conductive metal other than Cu, and may also include conductive metals such as Pd; however, from the perspective of providing a good FAB shape and good bonding reliability of the first joint under high temperature environments, the total concentration C of Ni, Au, and Pd over the entire wire M (Mass%) and Ni concentration C Ni Ratio C of (mass %) Ni / C M It is suitable for the coating layer to include Ni so that this is preferably 0.5 or more, more preferably 0.6 or more, and even more preferably 0.7 or more or 0.8 or more. The above non-C Ni / C M The upper limit of is not specifically limited as long as conditions (2) to (4) are satisfied, and can be, for example, 0.995 or less or 0.99 or less. Such non-C Ni / C M Silver, Ni concentration C of the entire wire measured by the method described in [Measurement of Elemental Content] below. Ni (Mass%) is the total concentration C of Ni, Au, and Pd measured in the same way. M It can be calculated by dividing by (mass%).

[0063] Regarding condition (1), whether the coating layer has a region with Ni as the main component on the core material side or a region containing Au and Ni on the wire surface side in the thickness direction of the coating layer can be confirmed by performing compositional analysis by Auger electron spectroscopy (AES) while excavating in the depth direction (direction toward the center of the wire) from the surface of the wire by Ar sputtering. Specifically, 1) after performing compositional analysis of the wire surface, 2) sputtering by Ar and 3) compositional analysis of the surface after sputtering are repeated to obtain the change in concentration of each element in the depth (center) direction from the surface of the wire (so-called depth direction concentration profile), and can be confirmed from the concentration profile. In the present invention, when obtaining the depth direction concentration profile, the unit of depth was converted to SiO2.

[0064] 1) When performing composition analysis of the wire surface or 3) composition analysis of the surface after sputtering, the position and dimensions of the measurement surface are determined as follows. Furthermore, in the following, the width of the measurement surface refers to the dimension of the measurement surface in the direction perpendicular to the wire axis (wire thickness direction), and the length of the measurement surface refers to the dimension of the measurement surface in the direction of the wire axis (wire length direction). Further explanation is provided with reference to FIG. 1. FIG. 1 is a schematic diagram viewed from a plane of the wire (1), and is illustrated such that the direction of the wire axis (wire length direction) corresponds to the vertical direction (up-down direction) of FIG. 1, and the direction perpendicular to the wire axis (wire thickness direction) corresponds to the horizontal direction (left-right direction) of FIG. 1. FIG. 1 shows the measurement surface (2) in relation to the wire (1), but the width of the measurement surface (2) is the dimension w of the measurement surface in the direction perpendicular to the wire axis. a And, the length of the measuring surface (2) is the dimension l of the measuring surface in the direction of the wire axis. a am.

[0065] In the present invention, the center of the wire width in a direction perpendicular to the wire axis is positioned so that it becomes the center of the width of the measuring surface, and the measuring surface is also determined such that the width of the measuring surface is 5% or more and 15% or less of the wire diameter. The length of the measuring surface is set to be five times the width of the measuring surface. In FIG. 1, the wire width is indicated by the symbol W, and the center of the wire width is indicated by the dotted line X. Accordingly, the measuring surface (2) is positioned so that the center of its width coincides with the dotted line X, which is the center of the wire width, and the width w of the measuring surface a It is determined that the value is between 5% and 15% of the wire diameter (equivalent to the wire width W), i.e., between 0.05W and 0.15W. In addition, the length of the measuring surface l a ne, l a =5w a It satisfies the relationship. By determining the position and dimensions of the measurement surface as above, it is possible to confirm with high precision the existence of regions containing Ni as the main component or regions containing Au and Ni in the coating layer, which is suitable for bringing about a good FAB shape and good bonding in the second joint.

[0066] In the present invention, the fact that the coating layer has a region with Ni as the main component on the core material side and a region containing Au and Ni on the wire surface side in the thickness direction of the coating layer is based on the results measured under the conditions described in the [Analysis of coating layer thickness by Auger electron spectroscopy (AES)] section below.

[0067] The trend of the depth-direction concentration profile obtained for the wire of the present invention according to one embodiment is described below. From the surface of the wire to a certain depth position, there exists a region containing Au and Ni. In this region, there is a tendency for the concentration of Ni to increase as the concentration of Au decreases in the depth direction from the surface of the wire. Furthermore, as the depth direction progresses, the concentration of Ni reaches a maximum value, and subsequently, there is a tendency for the concentration of Cu to increase as the concentration of Ni decreases. Ni may exhibit a maximum concentration at a certain depth position (d1) or may exhibit a maximum value over a certain depth range (d1 to d2). In such a concentration profile, by paying attention to the increase or decrease in the concentration of Au or Ni, the existence of a region containing both Au and Ni or a region where Ni is the main component, and the location of these regions can be determined. Additionally, in such a concentration profile, by paying attention to the increase or decrease in the concentration of Au or Ni, the maximum concentrations of Au and Ni can be determined from the location where their concentrations are maximum. In determining the maximum concentration of Au or Ni in the coating layer, it is appropriate to acquire concentration profiles for multiple measurement surfaces (n≥3) spaced apart from each other by at least 1 mm in the wire axis direction and to adopt the arithmetic mean value. The appropriate range for the maximum concentration of Ni will be described later, but when the maximum concentration of Ni is 50 mass% or more, it can be said that the "region with Ni as the main component" exists.

[0068] In a suitable embodiment, the position showing the maximum concentration of Au in the depth direction concentration profile of the wire is on the surface side of the wire rather than the position showing the maximum concentration of Ni.

[0069] In combination with conditions (2) to (4), from the perspective of realizing even better bonding reliability of the first joint under high temperature environments, the maximum concentration of Ni in the wire depth direction concentration profile is preferably 80 atomic% or more, more preferably 85 atomic% or more, even more preferably 90 atomic% or more, greater than 90 atomic%, greater than 92 atomic%, greater than 94 atomic% or more, or greater than 95 atomic%. The upper limit of the maximum concentration of Ni in the coating layer is not particularly limited and may be, for example, 100 mass%.

[0070] -Condition (2)-

[0071] Condition (2) is about the thickness of the coating layer.

[0072] In combination with conditions (1), (3), and (4), by including a coating layer that satisfies condition (2), the wire of the present invention can have a good FAB shape and good bonding reliability of the first joint under high temperature environments.

[0073] Regarding condition (2), the thickness of the coating layer (the method of calculation will be described later) is 10 nm or more, preferably 12 nm or more, more preferably 14 nm or more, even more preferably 15 nm or more, even more preferably 16 nm or more, particularly preferably 18 nm or more or 20 nm or more, from the perspective of realizing a good FAB shape and good bonding reliability of the first bond. In particular, if the thickness of the coating layer is 18 nm or more, it is suitable because, in addition to realizing a good FAB shape, it is possible to realize an even better compression shape of the first bond and also make it easier to further improve the bonding reliability of the first bond. Therefore, in a suitable embodiment, the thickness of the coating layer is 18 nm or more. In addition, if the thickness of the coating layer is less than 10 nm, eccentricity occurs during FAB formation, and the FAB shape deteriorates, and the compression shape of the first bond tends to deteriorate. In addition, the upper limit of the thickness of the coating layer is 130 nm or less from the perspective of realizing a good FAB shape, and preferably 125 nm or less, 120 nm or less, 115 nm or less, 110 nm or less, 105 nm or less, 100 nm or less, 95 nm or less, or 90 nm or less. If the thickness of the coating layer exceeds 130 nm, release or melting defects occur during FAB formation, and the FAB shape deteriorates, and the compression shape of the 1st joint tends to deteriorate.

[0074] The thickness of the coating layer in condition (2) can be determined from the concentration profile in the depth direction. First, the boundary between the Cu core material and the coating layer is determined based on the concentration of Cu. The location where the concentration of Cu is 50 atomic% is determined as the boundary, and the region where the concentration of Cu is 50 atomic% or higher is the Cu core material, and the region where the concentration is less than 50 atomic% is the coating layer. In the present invention, the boundary between the Cu core material and the coating layer does not necessarily have to be a grain boundary. Furthermore, the thickness of the coating layer can be determined by checking the concentration profile from the wire surface toward the center of the wire and as the distance from the wire surface location to the depth location where the concentration of the core material Cu first reaches 50 atomic%. In the present invention, when determining the thickness of the coating layer from the concentration profile in the depth direction, the unit of depth is converted to SiO2. In addition, it is suitable to acquire concentration profiles for multiple measurement surfaces (n≥3) spaced apart from each other by 1 mm or more in the wire axial direction and to adopt the arithmetic mean value.

[0075] -Condition (3)-

[0076] Condition (3) is the concentration of Au C throughout the wire. Au (Mass%) and Ni concentration C Ni Ratio C of (mass %) Au / C Ni It concerns the scope of.

[0077] In combination with conditions (1), (2), and (4), by including a coating layer that satisfies condition (3), the wire of the present invention can achieve good bonding reliability of the first junction under high temperature environments, good FAB shape, and good bonding performance in the second junction. In addition, by including a coating layer that satisfies condition (3), capillary clogging during continuous bonding can be suppressed, making it possible to maintain good productivity of the semiconductor device.

[0078] For condition (3), non-C Au / C Ni From the perspective of realizing good bondability at the second joint and suppressing capillary clogging during continuous bonding, it is 0.02 or higher, preferably 0.04 or higher, more preferably 0.05 or higher, 0.06 or higher, 0.08 or higher, or 0.1 or higher. Non-C Au / C Ni If α is less than 0.02, the bonding performance at the second joint tends to deteriorate, and the frequency of capillary clogging during continuous bonding also tends to increase. In addition, non-C Au / C Ni The upper limit of is 0.7 or less, preferably 0.65 or less, and more preferably 0.6 or less, 0.55 or less, 0.5 or less, 0.48 or less, 0.46 or less, or 0.45 or less, from the perspective of obtaining a good FAB shape and realizing a good compression shape of the first joint. Au / C Ni If α is greater than 0.7, eccentricity occurs during FAB formation, and along with the deterioration of the FAB shape, the compression shape of the 1st joint tends to deteriorate.

[0079] non-C in condition (3) Au / C Ni is the concentration of Au C of the entire wire measured by the method described in [Measurement of Elemental Content] below. Au (mass%), the concentration of Ni C measured in the same way Ni It can be calculated by dividing by (mass%).

[0080] -Condition (4)-

[0081] Condition (4) is about the concentration of Au on the surface of the wire.

[0082] In combination with conditions (1) to (3), by including a coating layer that satisfies condition (4), the wire of the present invention can have a good FAB shape and good bonding performance at the second junction. In addition, by including a coating layer that satisfies condition (4), capillary clogging during continuous bonding can be suppressed, making it possible to maintain good productivity of the semiconductor device.

[0083] Regarding condition (4), from the perspective of realizing good bonding performance in the second joint and suppressing capillary clogging during continuous bonding, the concentration of Au on the surface of the wire of the present invention is 10 atomic percent or more, preferably 15 atomic percent or more, more preferably 20 atomic percent or more, even more preferably 25 atomic percent or more, even more preferably 30 atomic percent or more, 32 atomic percent or more, 34 atomic percent or more, 35 atomic percent or more, 36 atomic percent or more, 38 atomic percent or more, or 40 atomic percent or more. If the concentration of Au on the surface of the wire is less than 10 atomic percent, the bonding performance in the second joint tends to deteriorate, and the frequency of capillary clogging during continuous bonding also tends to increase. The upper limit of the concentration of Au on the surface of the wire is 90 atomic percent or less, preferably 85 atomic percent or less, more preferably 80 atomic percent or less, 78 atomic percent or less, 76 atomic percent or less, 75 atomic percent or less, 74 atomic percent or less, 72 atomic percent or less, or 70 atomic percent or less, from the perspective of realizing a good FAB shape and realizing a good crimpeding shape of the first joint. If the concentration of Au on the surface of the wire exceeds 90 atomic percent, eccentricity occurs during FAB formation, and the FAB shape deteriorates, and the crimpeding shape of the first joint tends to deteriorate.

[0084] The concentration of Au on the wire surface under condition (4) can be determined by analyzing the composition of the wire surface using Auger electron spectroscopy (AES) with the wire surface as the measurement surface. Here, when determining the concentration of Au on the surface, gaseous components such as carbon (C), sulfur (S), oxygen (O), and nitrogen (N), as well as non-metallic elements, are not considered.

[0085] The compositional analysis of the wire surface can be performed under the same conditions as the compositional analysis of the wire surface described in relation to the method for acquiring a concentration profile in the depth direction. That is, when performing compositional analysis on the wire surface by Auger electron spectroscopy (AES), the position and dimensions of the measurement surface are determined as follows.

[0086] The position is determined such that the center of the wire width in the direction perpendicular to the wire axis becomes the center of the width of the measurement surface, and the measurement surface is determined such that the width of the measurement surface is between 5% and 15% of the wire diameter. The length of the measurement surface is set to be five times the width of the measurement surface. By determining the position and dimensions of the measurement surface as above, the concentration of Au on the wire surface can be measured with high precision, which is suitable for improving the bonding properties of the FAB shape and the second joint. In addition, it is suitable to perform the measurement on multiple measurement surfaces (n≥3) spaced apart from each other by at least 1 mm in the wire axis direction and to adopt the arithmetic mean value.

[0087] The concentration of Au on the wire surface in the above condition (4) is based on the results measured under the conditions described in the [Analysis of wire surface composition by Auger electron spectroscopy (AES)] section below.

[0088] The coating layer may contain one or more dopants selected from, for example, the first additive element, the second additive element, and the third additive element described below. Suitable content of these dopants is as described below.

[0089] The coating layer may also contain Pd as a conductive metal other than Cu. For example, the concentration of Pd C over the entire wire Pd (Mass%) and Ni concentration C Ni Ratio C of (mass %) Pd / C Ni The coating layer may contain Pd in ​​an amount such that α is 0.8 or less, 0.6 or less, 0.5 or less, 0.4 or less, 0.3 or less, 0.2 or less, 0.12 or less, 0.11 or less, 0.1 or less, 0.08 or less, 0.06 or less, or 0.05 or less. If the coating layer contains Pd, non-C Pd / C Ni The lower limit of is not specifically limited and can be, for example, 0.0001 or more, 0.0005 or more, or 0.001 or more, etc.

[0090] In one embodiment, the coating layer consists of Ni and Au and unavoidable impurities. In another embodiment, the coating layer consists of Ni and Au, Pd, one or more elements selected from the first additive element, the second additive element, and the third additive element described below, and unavoidable impurities. Furthermore, the term "unavoidable impurities" used to describe the coating layer also includes elements constituting the aforementioned Cu core material.

[0091] The wire of the present invention may further contain one or more elements selected from the group consisting of B, P, and Mg ("first additive element"). When the wire of the present invention contains the first additive element, it is preferable that the total concentration of the first additive element relative to the entire wire be 1 mass ppm or more. By doing so, a bonding wire that produces a better crimp shape of the first joint can be realized. It is more preferable that the total concentration of the first additive element relative to the entire wire be 2 mass ppm or more, and even more preferable that it be 3 mass ppm or more, 5 mass ppm or more, 8 mass ppm or more, 10 mass ppm or more, 15 mass ppm or more, or 20 mass ppm or more. From the perspective of suppressing the hardening of the wire to reduce chip damage during the first bonding, the total concentration of the first additive element is preferably 100 mass ppm or less, and more preferably 90 mass ppm or less, 80 mass ppm or less, 70 mass ppm or less, 60 mass ppm or less, or 50 mass ppm or less. Accordingly, in a suitable embodiment, the wire of the present invention comprises the first additive element, and the total concentration of the first additive element relative to the entire wire is 1 mass ppm or more and 100 mass ppm or less.

[0092] When the wire of the present invention contains a first additive element, the first additive element may be contained in either the Cu core material or the coating layer, or in both. From the perspective of realizing a bonding wire that produces an even better crimped shape of the first joint, it is suitable for the first additive element to be contained in the Cu core material.

[0093] The wire of the present invention may further contain one or more elements selected from the group consisting of Se, Te, As, and Sb ("second addition element"). When the wire of the present invention contains the second addition element, it is preferable that the total concentration of the second addition element relative to the entire wire be 1 mass ppm or more. By doing so, the bonding reliability of the first joint under high-temperature environments can be improved. It is more preferable that the total concentration of the second addition element relative to the entire wire be 2 mass ppm or more, and even more preferable that it be 3 mass ppm or more, 5 mass ppm or more, 8 mass ppm or more, 10 mass ppm or more, 15 mass ppm or more, or 20 mass ppm or more. From the perspective of realizing a good FAB shape and realizing a good compression shape of the first joint, the total concentration of the second additive element is preferably 100 mass ppm or less, and more preferably 90 mass ppm or less, 80 mass ppm or less, 70 mass ppm or less, 60 mass ppm or less, or 50 mass ppm or less. Accordingly, in a suitable embodiment, the wire of the present invention comprises the second additive element, and the total concentration of the second additive element over the entire wire is 1 mass ppm or more and 100 mass ppm or less.

[0094] When the wire of the present invention contains a second additive element, the second additive element may be contained in either the Cu core material or the coating layer, or in both. From the perspective of further improving the bonding reliability of the first joint under high temperature environments, it is suitable for the second additive element to be contained in the coating layer. When the coating layer contains the second additive element, the second additive element may be contained in the region containing Au and Ni on the wire surface side, or in the region mainly composed of Ni on the core material side. In addition, when the coating layer contains Pd, the second additive element may be contained together with said Pd.

[0095] The wire of the present invention may further contain one or more elements selected from the group consisting of Ga, Ge, and In ("third addition element"). When the wire of the present invention contains the third addition element, it is preferable that the total concentration of the third addition element relative to the entire wire be 0.011 mass% or more. By doing so, the bonding reliability of the first joint under high temperature environments can be further improved. It is more preferable that the total concentration of the third additive element for the entire wire be 0.015 mass% or more, and even more preferable that it be 0.02 mass% or more, 0.025 mass% or more, 0.03 mass% or more, 0.031 mass% or more, 0.035 mass% or more, 0.04 mass% or more, 0.05 mass% or more, 0.07 mass% or more, 0.09 mass% or more, 0.1 mass% or more, 0.12 mass% or more, 0.14 mass% or more, 0.15 mass% or more, or 0.2 mass% or more. From the perspective of realizing a good FAB shape, realizing a good compression shape of the first joint, and realizing good second bonding properties, the total concentration of the third additive element is preferably 1.5 mass% or less, and more preferably 1.4 mass% or less, 1.3 mass% or less, or 1.2 mass% or less. Accordingly, in a suitable embodiment, the wire of the present invention comprises a third additive element, and the total concentration of the third additive element relative to the entire wire is 0.011 mass% or more and 1.5 mass% or less.

[0096] When the wire of the present invention contains a third additive element, the third additive element may be contained in either the Cu core material or the coating layer, or may be contained in both.

[0097] The content of the first, second, and third additive elements in the wire can be measured by the method described in [Measurement of Element Content] below.

[0098] In the wire of the present invention, the total concentration of Cu, Ni, Au, and Pd can be, for example, 98.5 mass% or more, 98.6 mass% or more, 98.7 mass% or more, or 98.8 mass% or more.

[0099] -Other conditions of suitability-

[0100] Below, conditions suitable for the wire of the present invention to satisfy are described.

[0101] The wire of the present invention, when a FAB is formed using the wire, has an angle difference of 15 degrees or less with respect to the compression bonding direction when measuring the crystal orientation of a cross-section perpendicular to the compression bonding direction of the FAB. <100> It is desirable that the ratio of the crystal orientation be 30% or more. By doing so, an even better compression shape of the first joint can be realized.

[0102] As described above, the connection process using a bonding wire is completed by first bonding to an electrode on a semiconductor chip, then forming a loop, and then secondarily bonding the wire portion to an external electrode on a lead frame or substrate. For the first bonding, the tip of the wire is heated and melted by arc heat input to form a FAB by surface tension, and then the said FAB is press-bonded (ball-bonded) to an electrode on a semiconductor chip. The inventors have, based on the results of measuring the crystal orientation of a cross-section perpendicular to the press-bonding direction of the FAB, an angle difference with respect to the press-bonding direction of 15 degrees or less <100> The ratio of the crystal orientation (hereinafter simply "in the cross-section of the FAB") <100> It was discovered that a wire having a ratio of 30% or more (also called the ratio of crystal orientation) can achieve an even better crimped shape of the first joint.

[0103] In terms of realizing an even better compression shape of the first joint, in the cross-section of the FAB <100> A wire is suitable in which the ratio of crystal orientation is more preferably 35% or more, even more preferably 40% or more, even more preferably 45% or more, particularly preferably 50% or more, 55% or more, or 60%. In particular, regarding the cross-section of the FAB <100> A wire having a crystal orientation ratio of 50% or more can realize a particularly good crimp shape of the first joint. Therefore, in a suitable embodiment, in the cross-section of the FAB <100> The ratio of crystal orientation is 30% or more, and more suitably 50% or more. In the cross-section of the FAB <100> The upper limit of the ratio of the determination orientation is not specifically limited, and for example, it may be 100%, 99.5% or less, 99% or less, 98% or less, etc.

[0104] Referring to FIG. 2, a cross-section perpendicular to the compression bonding direction of the FAB is described. FIG. 2 shows a schematic diagram of the FAB (10) formed by surface tension by heating and melting the tip of the wire (1) with arc heat input. The formed FAB (10) is compression bonded to an electrode (not shown) on a semiconductor chip. In FIG. 2, the compression bonding direction of the FAB (10) is the direction indicated by arrow Z (the vertical direction (up and down direction) in FIG. 2), and the cross-section perpendicular to the compression bonding direction Z is the cross-section exposed by cutting the FAB along the dotted line AA perpendicular to the direction Z. Here, the dotted line AA, which serves as a reference when cutting the cross-section, is set to the position where the diameter of the exposed cross-section is maximum, that is, the position where the diameter of the exposed cross-section becomes D when the diameter of the FAB is set to D. In the cross-sectioning process, there may be cases where the straight line AA deviates from the target and the diameter of the exposed cross section becomes smaller than D, but if the diameter of the exposed cross section is 0.9D or larger, the effect of such deviation on the ratio of crystal orientations is negligibly small, so it is considered acceptable.

[0105] The crystal orientation of a cross-section perpendicular to the direction of the FAB's compression bonding can be measured using the Electron Backscattered Diffraction (EBSD) method. The device used for the EBSD method consists of a scanning electron microscope and a detector equipped therewith. The EBSD method is a method for determining the crystal orientation of each measurement point by projecting the diffraction pattern of reflected electrons generated when an electron beam is irradiated onto a sample onto a detector and analyzing the diffraction pattern. Dedicated software (such as OIM analysis by TSL Solutions, Inc.) can be used to analyze the data obtained by the EBSD method. By using the analysis software attached to the device and setting the cross-section perpendicular to the direction of the FAB's compression bonding as the inspection plane, the ratio of a specific crystal orientation can be calculated.

[0106] In the present invention, in the cross-section of the FAB <100> The ratio of the determination orientation to the measured area <100> It is defined as the area of ​​the determined orientation expressed as a percentage. In calculating the said ratio, only the determined orientation identified based on a certain reliability standard within the measurement surface is adopted, and areas where the determined orientation cannot be measured, or areas where the reliability of orientation interpretation is low even if measured, etc., are included in the measurement area and <100> It was calculated by excluding from the area of ​​the determination orientation. If the data excluded here exceeds, for example, 20% of the total, it is highly likely that there was slight contamination on the measurement target, so the process must be repeated starting from the cross-section. Furthermore, in the present invention, regarding the cross-section of the FAB <100> The ratio of the determination orientation was the arithmetic mean of each value of the ratio obtained by measuring for three or more FABs.

[0107] in the cross-section of the FAB <100> The inventors have hypothesized the following reasons why a wire with a crystal orientation ratio of 30% or more can realize an even better compression shape of the first joint.

[0108] It is known that metals deform by sliding in a specific crystal plane or crystal direction (that plane or direction is also referred to as the "sliding plane" or "sliding direction"). The FAB formed using the wire of the present invention is mainly composed of a core material, Cu or a Cu alloy, and its crystal structure is a face-centered cubic structure. When such a crystal structure is adopted, the crystal orientation of the cross-section perpendicular to the compression bonding direction is <100> On the other hand, as the metal slides and deforms at a 45-degree angle with respect to the compression surface, the FAB deforms by expanding radially in the 45-degree direction with respect to the compression surface and in the plane parallel to the compression surface. As a result, it is estimated that the compression shape becomes closer to a perfect circle.

[0109] In the present invention, in the cross-section of the FAB <100> The ratio of crystal orientations tends to fall within the desired range by adjusting the thickness of the coating layer, the Ni concentration in the coating layer, and the Cu purity of the core material. For example, the thickness of the coating layer in the cross-section of the FAB <100> Regarding the reason for the influence on the ratio of crystal orientations, the inventors deduce as follows. That is, during the melting stage, the Ni in the coating layer is appropriately diffused and mixed toward the center of the FAB, and the Cu or Cu alloy containing the appropriately diffused and mixed Ni is, with respect to the compression bonding direction <100> It is thought that the crystal orientation is oriented. Furthermore, if the thickness of the coating layer is within a predetermined range, the diffusion mixing of Ni during melting becomes appropriate, and regarding the compression bonding direction <100> It is inferred that if the thickness of the coating layer is too thin, it is easy for the crystal orientation to become oriented, while if the thickness of the coating layer is too thin, it is easy for a random crystal orientation without orientation to become oriented, and if the thickness of the coating layer is too thick, other crystal orientations are likely to become preferential.

[0110] The diameter of the wire of the present invention is not particularly limited and may be appropriately determined according to the specific purpose, but preferably it may be 15 μm or more, 18 μm or more, or 20 μm or more. The upper limit of the diameter is not particularly limited and may be, for example, 80 μm or less, 70 μm or less, or 50 μm or less.

[0111] Method for manufacturing wire

[0112] An example of a method for manufacturing a bonding wire for a semiconductor device according to the present invention will be described.

[0113] First, raw copper of high purity (4N to 6N; 99.99 to 99.9999 mass% or more) is processed into a large diameter (diameter of about 3 to 6 mm) by continuous casting to obtain an ingot.

[0114] When adding dopants such as the first, second, and third additive elements described above, the methods of addition may include, for example, incorporating them into a Cu core material, incorporating them into a coating layer, depositing them on the surface of a Cu core material, and depositing them on the surface of a coating layer, and multiple combinations of these methods may be used. The effects of the present invention can be achieved regardless of which addition method is adopted. In the method of incorporating the dopant into a Cu core material, a copper alloy containing the dopant at a required concentration can be used as a raw material to manufacture the Cu core material. When obtaining such a copper alloy by adding a dopant to the raw material Cu, a high-purity dopant component may be directly added to Cu, or a master alloy containing about 1% of the dopant component may be used. In the method of incorporating the dopant into a coating layer, the dopant may be incorporated into the Ni, Au, or Pd plating bath (in the case of wet plating) or the target material (in the case of dry plating) when forming the coating layer. In the method of depositing on the surface of a Cu core material or on the surface of a coating layer, the surface of the Cu core material or the surface of the coating layer is used as the deposit surface, and one or more deposition treatments selected from (1) application of an aqueous solution ⇒ drying ⇒ heat treatment, (2) plating method (wet method), and (3) deposition method (dry method) are performed.

[0115] A large-diameter ingot is forged, rolled, and drawn to produce a wire made of Cu or a Cu alloy with a diameter of about 0.7 to 2.0 mm (hereinafter also referred to as "intermediate wire").

[0116] As a method for forming a coating layer on the surface of a Cu core material, electroplating, electroless plating, or deposition methods may be used, but it is industrially preferable to use electroplating, which allows for stable control of the film thickness. For example, a coating layer may be formed on the surface of an intermediate wire. The coating layer may also be deposited at the stage of a large-diameter ingot, or the coating layer may be formed on the surface of the Cu core material after the intermediate wire is drawn and further fined (for example, after drawing to the diameter of the final Cu core material). When forming a coating layer containing Pd, the coating layer may be formed by using a Ni plating solution, a Pd plating solution, or a plating solution containing Ni and Pd in ​​a predetermined ratio, depending on the composition of the desired coating layer. For example, a Ni layer may be formed using a Ni plating solution, and then a Pd layer or a PdNi alloy layer may be formed using a Pd plating solution or a plating solution containing Ni and Pd in ​​a predetermined ratio to form the coating layer. In terms of forming a coating layer with excellent adhesion to the Cu core material, a predetermined coating layer may be formed after performing strike plating of a conductive metal on the surface of the Cu core material.

[0117] The region containing Au and Ni on the wire surface side of the coating layer can be formed by providing an Au layer on the surface side of the coating layer by the same method as described above.

[0118] The wire drawing process can be carried out using a continuous wire drawing device capable of setting multiple diamond-coated dies. If necessary, heat treatment may be performed during the intermediate stage of the wire drawing process. Through heat treatment, constituent elements can be diffused between the Au layer on the wire surface and the underlying Ni layer (or, if provided, a Pd layer or a PdNi alloy layer) to form a region containing Au and Ni on the wire surface side of the coating layer. As a method, it is preferable to promote alloying by continuously quenching the wire at a constant speed in an electric furnace at a constant furnace temperature, as this method can reliably control the Au concentration on the wire surface to a desired range. Furthermore, instead of the method of forming a region containing Au and Ni by heat treatment after additionally forming an Au layer on the coating layer, a method of depositing an alloy region containing Au and Ni from the beginning may be adopted.

[0119] The wire of the present invention can achieve a good FAB shape and good bonding performance at the second joint, and furthermore, good bonding reliability at the first joint under high temperature environments. Therefore, the bonding wire of the present invention can be suitably used, particularly as a bonding wire for vehicle-mounted devices or power devices.

[0120] [Method for manufacturing a semiconductor device]

[0121] A semiconductor device can be manufactured by using the bonding wire for a semiconductor device of the present invention to connect an electrode on a semiconductor chip with an electrode on a lead frame or a circuit board.

[0122] In one embodiment, the semiconductor device of the present invention comprises a circuit board, a semiconductor chip, and a bonding wire for conducting the circuit board and the semiconductor chip, wherein the bonding wire is a wire of the present invention.

[0123] In the semiconductor device of the present invention, the circuit board and the semiconductor chip are not particularly limited, and known circuit boards and semiconductor chips that can be used to construct the semiconductor device may be used. Alternatively, a lead frame may be used instead of a circuit board. For example, the semiconductor device may be configured to include a lead frame and a semiconductor chip mounted on the lead frame, as described in Japanese Patent Publication No. 2020-150116.

[0124] Examples of semiconductor devices include various semiconductor devices provided for electrical products (e.g., computers, mobile phones, digital cameras, televisions, air conditioners, solar power generation systems, etc.) and vehicles (e.g., motorcycles, automobiles, trains, ships, and aircraft, etc.).

[0125] Examples

[0126] The present invention will be described in detail below by presenting examples. However, the present invention is not limited to the examples shown below.

[0127] (Sample)

[0128] First, the method for preparing the sample is explained. The Cu used as the raw material for the Cu core material has a purity of 99.99 mass% or higher (4N) and the remainder consists of unavoidable impurities. In addition, when adding the first, second, and third additive elements, the purity of these elements is 99 mass% or higher and the remainder consists of unavoidable impurities, or a master alloy in which these additive elements are mixed in high concentrations with Cu is used.

[0129] For the core material Cu alloy, raw materials were first loaded into a graphite crucible and melted by heating to 1090 to 1500°C in an inert atmosphere such as N2 gas or Ar gas using a high-frequency furnace, and then an ingot with a diameter of about 3 to 6 mm was manufactured by continuous casting. Next, the obtained ingot was subjected to drawing to produce an intermediate wire with a diameter of about 0.7 to 2.0 mm, and the wire was further fined to the diameter of the wire to be coated by continuously performing drawing operations using a die. For the drawing process, a commercially available lubricant was used, and the drawing speed was set to 20 to 150 m / min. To form the coating layer, pickling treatment with hydrochloric acid or sulfuric acid was performed to remove the oxide film on the wire surface, after which a Ni layer was formed to cover the entire surface of the core material Cu alloy, and an Au layer was provided on the surface. In addition, in some embodiments, after forming the Ni layer, a Pd layer was provided, followed by an Au layer. Electroplating was used to form the Ni, Au, and Pd layers. Commercially available plating solutions were prepared and appropriately formulated for use as the Ni, Au, and Pd plating solutions.

[0130] Subsequently, wire drawing and other processes were performed to process the wire to a final wire diameter of φ20㎛. If necessary, intermediate heat treatment was performed 1 to 2 times at 300 to 700°C for 2 to 15 seconds during the wire drawing process. When performing the intermediate heat treatment, the wire was continuously descaled and N2 gas or Ar gas was flowed. After processing to the final wire diameter, the wire was continuously descaled and tempering heat treatment was performed while N2 gas or Ar gas was flowed. The heat treatment temperature for tempering was set to 200 to 600°C, the wire feed speed was set to 20 to 200 m / min, and the heat treatment time was set to 0.2 to 1.0 second. When the coating layer was thin or the Au concentration was low, the heat treatment temperature was lowered and the wire feed speed was set fast, and in the opposite case, the heat treatment temperature was raised and the wire feed speed was set slow.

[0131] (Testing and Evaluation Methods)

[0132] The testing and evaluation methods are described below.

[0133] [Analysis of Wire Surface Composition by Auger Electron Spectroscopy (AES)]

[0134] The concentration of Au on the wire surface was determined by measuring it using Auger electron spectroscopy (AES) as follows, with the wire surface as the measurement surface.

[0135] First, the bonding wire to be used for measurement was fixed in a straight line in the sample holder. Next, the position was determined such that the center of the wire width in the direction perpendicular to the wire axis became the center of the width of the measurement surface, and the measurement surface was determined such that the width of the measurement surface was between 5% and 15% of the wire diameter. The length of the measurement surface was set to five times the width of the measurement surface. Then, using an AES device (Alvac PHI-700), compositional analysis of the wire surface was performed under conditions of an acceleration voltage of 10 kV, and the surface Au concentration (atomic %) was determined.

[0136] In addition, compositional analysis by AES was performed on three measurement surfaces spaced at least 1 mm apart in the wire axis direction, and the arithmetic mean value was adopted. When determining the concentration of Au on the surface, gaseous components such as carbon (C), sulfur (S), oxygen (O), and nitrogen (N), as well as non-metallic elements, were not considered.

[0137] [Analysis of coating thickness by Auger electron spectroscopy (AES)]

[0138] Depth analysis by AES was used to analyze the thickness of the coating layer. Depth analysis by AES involves analyzing changes in composition along the depth direction by alternately performing composition analysis and sputtering, and it is possible to obtain changes in the concentration of each element along the depth (center) direction from the wire surface (so-called depth direction concentration profile).

[0139] Specifically, a depth-direction concentration profile was obtained by repeating 1) compositional analysis of the wire surface by AES, 2) sputtering with Ar, and 3) compositional analysis of the surface after sputtering. The sputtering in 2) was performed using Ar + The procedure was performed at an acceleration voltage of 2 kV. In addition, for the compositional analysis of the surfaces of 1) and 3), the dimensions of the measurement surface and the conditions for compositional analysis by AES were set to be the same as those described in the [Compositional analysis of wire surface by Auger electron spectroscopy (AES)] section above.

[0140] In addition, the acquisition of the depth-direction concentration profile was performed on three measurement surfaces spaced at least 1 mm apart from each other in the wire axis direction.

[0141] -Thickness of the coating layer-

[0142] In the depth-direction concentration profile obtained, the concentration profile was checked from the wire surface toward the center of the wire, and the distance from the wire surface position to the depth position where the concentration of the core material Cu first reached 50 atomic% was determined as the thickness of the measured coating layer. The arithmetic mean of the values ​​obtained for three measurement surfaces was adopted as the thickness of the coating layer.

[0143] Furthermore, the depth measured in AES analysis is calculated as the product of the sputtering rate and time. Since the sputtering rate is generally measured using the standard sample SiO2, the depth analyzed by AES becomes a SiO2 equivalent value. In other words, the SiO2 equivalent value was used for the unit of the coating layer thickness.

[0144] -Maximum concentration of Ni, etc. in the coating layer-

[0145] In the depth-direction concentration profile obtained, attention was paid to the increase or decrease in Ni concentration, and the maximum concentration was determined from the location where Ni concentration was maximum. The arithmetic mean of the values ​​obtained for three measurement surfaces was adopted as the maximum Ni concentration.

[0146] In addition, regarding the wire of the example, it was confirmed that the core material side has a region with Ni as the main component, the wire surface side has a region containing Au and Ni, the maximum concentration of Ni is 80 atomic percent or more, and the position showing the maximum concentration of Au is located on the surface side rather than the position showing the maximum concentration of Ni. Regarding the wire of the example in which the coating layer has a region containing Pd, it was confirmed that the position showing the maximum concentration of Pd is located on the surface side rather than the position showing the maximum concentration of Ni, and the position showing the maximum concentration of Pd is located between the position showing the maximum concentration of Au and the position showing the maximum concentration of Ni.

[0147] [Measurement of elemental content]

[0148] The content of Au, Ni, Pd, first, second, and third additive elements in the wire was determined by analyzing the solution obtained by dissolving the bonding wire in a strong acid using an ICP emission spectrometer and an ICP mass spectrometer, and detecting the elemental concentrations contained in the entire wire. As the analytical instruments, an ICP-OES (Hitachi High-Tech Science Corp. "PS3520UVDDII") or an ICP-MS (Agilent Technologies Corp. "Agilent 7700x ICP-MS") was used. In addition, the total concentration C of Ni, Au, and Pd M (Mass%) was calculated by summing the respective concentrations of Ni, Au, and Pd.

[0149] [FAB Shape]

[0150] For the evaluation of the FAB shape, a FAB was fabricated on a lead frame using a commercially available wire bonder and observed using a scanning electron microscope (SEM) (Number of evaluations N=100). In addition, the FAB was formed by setting the current value to 30 to 75 mA, the EFO gap to 762 μm, and the tail length to 254 μm, while flowing N2+5% H2 gas at a flow rate of 0.4 to 0.6 L / min, and the diameter was set to a range of 1.5 to 1.9 times the wire diameter. For the determination of the FAB shape, a spherical shape was judged as good, and if there was eccentricity, molding defects, or melting defects, it was judged as defective. Then, it was evaluated according to the following criteria.

[0151] metewand:

[0152] ○: 5 or fewer defective locations

[0153] △: 6 to 10 defects (no practical issues)

[0154] ×: 11 or more defective locations

[0155] [Measurement of crystal orientation in the cross-section of the FAB]

[0156] Using a commercially available wire bonder, a FAB was formed under the conditions described in the [FAB Shape] column above, and the crystal orientation was measured using a cross-section perpendicular to the compression bonding direction of the FAB as the measurement plane. In the present invention, a cross-section perpendicular to the compression bonding direction of the FAB refers to the cross-section exposed by cutting the FAB along the dotted line AA shown in FIG. 2, and the reference dotted line AA was set as the position where the diameter of the exposed cross-section is maximum. For the measurement, the EBSD method was used, and by utilizing the analysis software attached to the device, the above-described procedure <100> The ratio of the crystal orientation was calculated. Measurements were taken for three FABs, and the arithmetic mean of each obtained ratio value was calculated for the cross-section of the FAB. <100> It was determined by the ratio of the determination orientation.

[0157] [Joinability of the 2nd joint]

[0158] The bonding performance of the second bond was evaluated by the second bond window test. The second bond window test is a test in which the ultrasonic current for the second bond is set in 6 steps of 10mA every 10mA from 30mA to 80mA on the horizontal axis, and the load for the second bond is set in 6 steps of 10gf every 10gf from 20gf to 70gf on the vertical axis, and the number of bondable conditions for a total of 36 second bond conditions is determined.

[0159]

[0160] In this test, for each wire of the example and comparative example, 200 bonds were performed for each condition on the lead portion of the lead frame using a commercially available wire bonder. An Ag-plated lead frame was used, and bonding was performed at a stage temperature of 200°C under a flow rate of 0.5 L / min of N2 + 5% H2 gas. Then, the number of conditions under which continuous bonding was possible without problems such as failure to bond or stoppage of the bonder was calculated and evaluated according to the following criteria.

[0161] metewand:

[0162] ◎: 33 conditions or higher

[0163] ○: 30 to 32 conditions

[0164] △: Conditions 26 to 29

[0165] ×: 25 conditions or less

[0166] [Joining reliability of the 1st joint]

[0167] The reliability of the first joint was evaluated by the High Temperature Storage Life Test (HTSL).

[0168] A sample for testing the bonding reliability of the first joint was fabricated by ball-bonding an electrode prepared by depositing a 1.5 μm thick Al-1.0 mass% Si-0.5 mass% Cu alloy on a Si substrate on a standard metal frame using a commercially available wire bonder, and then sealing the ball bonded with a commercially available thermosetting epoxy resin. The balls were formed under the conditions described in the [FAB Shape] column above. The fabricated sample for evaluating bonding reliability was exposed to an environment at a temperature of 175°C using a high-temperature incubator. The bonding life of the first joint was determined by performing a shear test on the ball joint every 500 hours, and set to the time when the shear strength value became half of the initial shear strength. The shear strength value was the arithmetic mean of measurements taken at 50 randomly selected locations on the ball joint. The shear test after the high-temperature exposure test was performed after removing the resin by acid treatment to expose the ball joint. It was then evaluated according to the following criteria.

[0169] metewand:

[0170] ◎: Bond life of 2,000 hours or more

[0171] ○: Bond life 1,000 hours or more and less than 2,000 hours

[0172] ×: Bond life less than 1,000 hours

[0173] [Compression shape]

[0174] The evaluation of the compression shape (flattened shape of the ball) of the 1st joint was performed by forming a ball under the conditions described in the [FAB Shape] column above using a commercially available wire bonder, compression bonding it to an electrode prepared by depositing a 1.5 μm thick Al-1.0 mass% Si-0.5 mass% Cu alloy film on a Si substrate, and observing it from directly above with an optical microscope (N=100 evaluations). The flattened shape of the ball was judged as good if it was close to a perfect circle, and as poor if it was elliptical or petal-shaped. Then, it was evaluated according to the following criteria.

[0175] metewand:

[0176] ◎: No defects

[0177] ○: 1 to 3 defective locations

[0178] △: 4 or 5 defective locations

[0179] ×: 6 or more defects

[0180] [Capillary Life]

[0181] Continuous bonding was performed using a commercially available wire bonder, and the number of bonds was counted until bonding became impossible due to capillary clogging. Then, it was evaluated according to the following criteria.

[0182] metewand:

[0183] ○: Over 1 million times

[0184] ×: Less than 1 million times

[0185] [Chip Damage]

[0186] The evaluation of chip damage was performed by using a commercially available wire bonder to form a ball under the conditions described in the [FAB shape] column above, and then press-bonding it to an electrode prepared by depositing a 1.5 μm thick Al-1.0 mass% Si-0.5 mass% Cu alloy film on a Si substrate, dissolving the wire and electrode in a chemical solution to expose the Si substrate, and observing the Si substrate immediately below the bonding area with an optical microscope (N=50 evaluations). Then, the evaluation was performed according to the following criteria.

[0187] metewand:

[0188] ○: No cracks or signs of bonding

[0189] △: No cracks, but traces of bonding are confirmed in some locations (3 or fewer)

[0190] ×: Other than that

[0191] The evaluation results of the examples and comparative examples are shown in Tables 2 to 4.

[0192]

[0193]

[0194]

[0195] It was confirmed that the wires of Examples No. 1 to 54 all have a coating layer that satisfies all of the specific conditions (1) to (4) of the present invention, and thus have a good FAB shape, good bonding performance in the 2nd joint, and furthermore, good bonding reliability in the 1st joint under high temperature environment.

[0196] In addition, it was confirmed that the wires of Examples No. 13 to 18, 27 to 30, 41 to 43, and 47 to 49, containing a total of 1 mass ppm or more of the first additive element, provide an even better crimp shape of the first joint. It was confirmed that the wires of Examples No. 19 to 30 and 44 to 49, containing a total of 1 mass ppm or more of the second additive element, provide even better bonding reliability of the first joint under high temperature conditions. It was confirmed that the wires of Examples No. 33 to 49, containing a total of 0.011 mass% or more of the third additive element, provide even better bonding reliability of the first joint under high temperature conditions.

[0197] Meanwhile, the wires of Comparative Examples No. 1 to 7 have a coating layer that does not satisfy at least one of the specific conditions (1) to (4) of the present case, and it was confirmed that at least one of the FAB shape, bonding performance in the 2nd joint, and bonding reliability in the 1st joint is defective.

[0198] When a FAB is formed using a wire, the crystal orientation of a cross-section perpendicular to the compression bonding direction of the said FAB is measured such that the angle difference with respect to the compression bonding direction is 15 degrees or less <100> It was confirmed that if the ratio of the crystal orientation is 30% or more, a good compression shape of the first joint can be realized (Examples No. 55 to 65). In particular, the corresponding <100> It was confirmed that if the ratio of the crystal orientation is 50% or more, a particularly excellent compression shape of the 1st joint can be realized (Examples No. 56, 57, 63, 64).

Claims

Claim 1 A bonding wire for a semiconductor device comprising a core material made of Cu or a Cu alloy and a coating layer containing a conductive metal other than Cu formed on the surface of the core material, wherein the coating layer has a region having Ni as the main component on the core material side and a region containing Au and Ni on the wire surface side in the thickness direction of the coating layer, wherein the thickness of the coating layer is 10 nm or more and 130 nm or less, and the concentration of Au C over the entire wire Au (Mass%) and Ni concentration C Ni Ratio C of (mass %) Au / C Ni A bonding wire for a semiconductor device having a value of 0.02 or more and 0.7 or less, and an Au concentration of 10 atomic% or more and 90 atomic% or less on the surface of the wire. Claim 2 A bonding wire for a semiconductor device according to claim 1, wherein the concentration of Au on the surface of the wire is measured by Auger electron spectroscopy (AES) under the following <conditions>. <conditions> The wire is positioned so that the center of the wire width becomes the center of the width of the measurement surface, and furthermore, the width of the measurement surface is 5% or more and 15% or less of the wire diameter, and the length of the measurement surface is five times the width of the measurement surface. Claim 3 A bonding wire for a semiconductor device according to claim 1, wherein the coating layer further contains Pd as a conductive metal other than Cu. Claim 4 In claim 1, the total concentration C of Ni, Au, and Pd for the entire wire M (Mass%) and Ni concentration C Ni Ratio C of (mass %) Ni / C M Bonding wire for semiconductor devices, having a value of 0.5 or higher. Claim 5 A bonding wire for a semiconductor device according to claim 1, wherein the maximum concentration of Ni in the depth direction concentration profile of the wire is 80 atomic% or more. Claim 6 A bonding wire for a semiconductor device according to claim 5, wherein the depth-direction concentration profile of the wire is obtained by measuring by Auger electron spectroscopy (AES) under the following <conditions> while excavating in the depth direction from the surface of the wire by Ar sputtering. <conditions> The wire is positioned so that the center of the width of the wire becomes the center of the width of the measurement surface, and furthermore, the width of the measurement surface is 5% or more and 15% or less of the wire diameter, and the length of the measurement surface is five times the width of the measurement surface. Claim 7 In claim 1, when a Free Air Ball (FAB) is formed using a wire, the result of measuring the crystal orientation of a cross-section perpendicular to the compression bonding direction of the said FAB is such that the angle difference with respect to the compression bonding direction is 15 degrees or less. <100> Bonding wire for semiconductor devices having a crystal orientation ratio of 30% or more. Claim 8 In paragraph 7, the angle difference with respect to the compression bonding direction is 15 degrees or less <100> Bonding wire for semiconductor devices having a crystal orientation ratio of 50% or more. Claim 9 A bonding wire for a semiconductor device according to claim 1, wherein the thickness of the coating layer is 18 nm or more. Claim 10 A bonding wire for a semiconductor device according to claim 1, comprising one or more elements selected from the group consisting of B, P, and Mg (hereinafter referred to as "first additive element"), wherein the total concentration of the first additive element relative to the entire wire is 1 mass ppm or more and 100 mass ppm or less. Claim 11 A bonding wire for a semiconductor device according to claim 1, comprising one or more elements selected from the group consisting of Se, Te, As, and Sb (hereinafter referred to as "second addition element"), wherein the total concentration of the second addition element relative to the entire wire is 1 mass ppm or more and 100 mass ppm or less. Claim 12 A bonding wire for a semiconductor device according to claim 1, comprising one or more elements selected from the group consisting of Ga, Ge, and In (hereinafter referred to as "third addition element"), wherein the total concentration of the third addition element relative to the entire wire is 0.011 mass% or more and 1.5 mass% or less. Claim 13 A semiconductor device comprising a bonding wire for a semiconductor device as described in any one of claims 1 to 12.

Citation Information

Patent Citations

  • Bonding wire for semiconductor device

    KR1020100023893A

  • Bonding wire for semiconductor device

    KR1020100032451A

  • Bonding wire for semiconductor device

    KR1020170029013A

  • Noble metal-coated copper wire for ball bonding

    US20170125135A1