Manufacturing method of positive electrode additives, positive electrode additives and positive electrode comprising the same

By forming a coated divalent metal oxide with an amorphous organic layer, the anode additive achieves enhanced stability and performance in lithium-ion batteries, addressing atmospheric and moisture-induced degradation.

KR103046100B1Active Publication Date: 2026-11-11LG CHEM LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
KR1020210032558
Authority / Receiving Office
KR · KR
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-03-12
Publication Date
2026-11-11
Estimated Expiration
2041-03-12

AI Technical Summary

Technical Problem

Existing anode materials with excess lithium, such as Li6CoO4, suffer from poor atmospheric stability due to phase separation and gelation, leading to degradation of battery characteristics during manufacturing and performance issues.

Method used

A method involving the preparation of a divalent metal oxide represented by Li a MO b, where M is Co, Mn, or Fe, and a coating layer formed through mixing with an organometallic salt and heat-treating to create an amorphous organic layer with transition metal particles, enhancing atmospheric and moisture resistance.

Benefits of technology

The method results in an anode additive with improved stability and minimal lithium byproduct generation, preventing gelation and maintaining electrochemical performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 112021029325154-PAT00001_ABST
    Figure 112021029325154-PAT00001_ABST
Patent Text Reader

Abstract

The present invention relates to a method for manufacturing an anode additive, an anode additive, and an anode containing the same.
Need to check novelty before this filing date? Find Prior Art

Description

Technology Field

[0001] The present invention relates to a method for manufacturing an anode additive, an anode additive, and an anode containing the same. Background Technology

[0003] Recently, the demand for rechargeable batteries as an energy source has been increasing rapidly. Among these rechargeable batteries, lithium-ion batteries, which possess high energy density and voltage, long cycle life, and low self-discharge rate, have been commercialized and are widely used.

[0004] Although graphite is primarily used as a negative electrode material for lithium secondary batteries, it is difficult to increase the capacity of lithium secondary batteries because graphite has a low capacity of 372 mAh / g per unit mass. Accordingly, to increase the capacity of lithium secondary batteries, negative electrode materials that form intermetallic compounds with lithium, such as silicon, tin, and their oxides, are being developed and used as non-carbon negative electrode materials that have a higher energy density than graphite. However, these non-carbon negative electrode materials have a problem in that although they have a large capacity, their initial efficiency is low, resulting in a large amount of lithium consumption during initial charge-discharge and significant irreversible capacity loss.

[0005] In response to this, a method has been studied and proposed to overcome irreversible capacity loss of the anode by using a material that can provide a lithium ion source or storage to the cathode material and exhibits electrochemical activity after the first cycle so as not to degrade the overall performance of the battery. Specifically, as a sacrificial cathode material or an irreversible additive (or over-discharge prevention agent), a method is known to apply an oxide containing an excess amount of lithium, such as Li6CoO4 (hereinafter L6C), to the cathode.

[0006] However, oxides containing an excess amount of lithium, such as L6C, undergo phase separation into LiOH, Li2CO3, etc. due to chemical reactions with CO2 and H2O in the atmosphere during battery manufacturing environments using conventional cathode materials, which can lead to an increase in viscosity or gelation of the composition when preparing a slurry composition for electrode manufacturing. In other words, oxides containing an excess amount of lithium, such as L6C, have a problem of poor stability when exposed to the atmosphere. As a result, it is difficult to apply the composition for forming an active material layer uniformly, and this can cause problems such as degradation of battery characteristics.

[0007] Accordingly, technology is being developed to form a coating layer such as B2O3 or NH4H2PO4 on an oxide containing an excess amount of lithium, and existing coating technologies adopt a method of coating by dry mixing the material to be coated. Although this method is generally widely used because it is convenient and has low process costs, there is a problem that the charge / discharge characteristics of the oxide containing an excess amount of lithium deteriorate, and there are limitations in improving stability when exposed to the atmosphere because the coating is not formed well.

[0008] Therefore, a coating technology is needed that can increase stability upon atmospheric exposure while maintaining the inherent properties of oxides containing an excess amount of lithium. The problem to be solved

[0010] The present invention provides a method for manufacturing an anode additive that can increase stability upon exposure to the atmosphere while maintaining the charging capacity of the lithium metal oxide, which is an anode additive containing an excess amount of lithium. means of solving the problem

[0012] To solve the above problem, the present invention provides a method for manufacturing an anode additive comprising: a step of preparing a divalent metal oxide represented by the following chemical formula 1; and a step of mixing the divalent metal oxide with an organometallic salt and heat-treating to form a coating layer on the surface of the divalent metal oxide; wherein the organometallic salt comprises one or more transition metals capable of coordination bonding and having a metal oxidation number of +3 to +6.

[0013] [Chemical Formula 1]

[0014] Li a MO b

[0015] In the above chemical formula 1,

[0016] M is one or more selected from the group consisting of Co, Mn, and Fe, and

[0017] 3 <a<7, 3<b<5이다.

[0019] In addition, the present invention provides an anode additive comprising: a divalent metal oxide represented by the above chemical formula 1; an amorphous organic coating layer located on the surface of the divalent metal oxide; and transition metal particles contained within the amorphous organic coating layer, capable of coordination bonding, and having a metal oxidation number of +3 to +6.

[0020] In addition, the present invention provides an anode comprising the above-mentioned anode additive. Effects of the invention

[0022] According to the method for manufacturing an anode additive of the present invention, an anode additive with improved stability upon exposure to the atmosphere while maintaining initial charging capacity can be manufactured through a simple and mild process.

[0023] The cathode additive produced according to the manufacturing method of the present invention hardly undergoes phase separation even when exposed to atmospheric and moisture conditions, resulting in minimal generation of lithium byproducts. In other words, it exhibits excellent atmospheric stability, and thus can prevent gelation when preparing a slurry composition for battery manufacturing. Accordingly, degradation of battery performance can also be prevented. Brief explanation of the drawing

[0025] Figure 1 is a diagram showing a TEM image of the anode additive of Example 6. Figure 2 is a diagram showing a TEM image of the anode additive of Comparative Example 1. Figure 3(a) shows XRD data of the anode additive of Example 4 before and after atmospheric exposure, and Figure 3(b) shows XRD data of the anode additive of Example 9 before and after atmospheric exposure. Figure 4 is a diagram showing XRD data before and after atmospheric exposure of the anode additive of Comparative Example 1. Specific details for implementing the invention

[0026] Terms and words used in this specification and claims should not be interpreted as being limited to their ordinary or dictionary meanings, but should be interpreted in a meaning and concept consistent with the technical spirit of the invention, based on the principle that the inventor can appropriately define the concept of the terms to best describe his invention.

[0027] In this specification, terms such as “comprising,” “comprising,” or “having” are intended to specify the existence of the implemented features, numbers, steps, components, or combinations thereof, and should not be understood as precluding the existence or addition of one or more other features, numbers, steps, components, or combinations thereof.

[0029] The present invention will be described in more detail below.

[0031] Method for manufacturing anode additives

[0032] A method for manufacturing an anode additive according to the present invention comprises the step of preparing a divalent metal oxide represented by the following chemical formula 1 (hereinafter, the first step); and the step of mixing the divalent metal oxide with an organometallic salt and heat-treating to form a coating layer on the surface of the divalent metal oxide (hereinafter, the second step); wherein the organometallic salt comprises one or more transition metals capable of coordination bonding and having a metal oxidation number of +3 to +6.

[0033] [Chemical Formula 1]

[0034] Li a MO b

[0035] In the above chemical formula 1,

[0036] M is one or more selected from the group consisting of Co, Mn, and Fe, and

[0037] 3 <a<7, 3<b<5이다.

[0039] According to the method for manufacturing an anode additive of the present invention, there is an advantage in that an anode additive with improved stability upon atmospheric exposure while maintaining initial charging capacity can be manufactured through a simple and mild process.

[0041] The following explains the steps in detail.

[0043] (1) Stage 1

[0044] The method for manufacturing an anode additive according to the present invention includes the step of preparing a lithium metal oxide represented by the following chemical formula 1.

[0045] [Chemical Formula 1]

[0046] Li a MO b

[0047] In the above chemical formula 1,

[0048] M is one or more selected from the group consisting of Co, Mn, and Fe, and

[0049] 3 <a<7, 3<b<5이다.

[0051] In the present invention, the preparation of the above-mentioned lithium metal oxide may be performed by mixing an M-containing raw material and a lithium-containing raw material and then calcining them to produce a lithium metal oxide represented by Chemical Formula 1.

[0052] The above M-containing raw material may be an acetate, carbonate, nitrate, sulfate, halide, sulfide, oxide, or combination thereof of M metal, but is not limited thereto.

[0053] If the above M is cobalt, the cobalt-containing raw material is cobalt It may be an acetate, carbonate, nitrate, sulfate, halide, sulfide, or oxide of the metal, etc. The above cobalt-containing raw material is, for example, CoSO₄ 4, It may be Co(OCOCH3)2ㆍ4H2O, Co(NO3)2ㆍ6H2O, CoSO4ㆍ7H2O, Co(OH)2, Co3O4, CoO, or a combination thereof, but is not limited thereto.

[0054] When the above M is manganese, the manganese-containing raw material may be, but is not limited to, an acetate, carbonate, nitrate, sulfate, halide, sulfide, or oxide of manganese metal.

[0055] When the above M is iron, the iron-containing raw material may be an acetate, carbonate, nitrate, sulfate, halide, sulfide, or oxide of iron metal, but is not limited thereto.

[0056] The above lithium-containing raw materials may include, for example, lithium-containing carbonates (e.g., lithium carbonate, etc.), hydrates (e.g., lithium hydroxide hydrate (LiOH·H2O), etc.), hydroxides (e.g., lithium hydroxide, etc.), nitrates (e.g., lithium nitrate (LiNO3), etc.), chlorides (e.g., lithium chloride (LiCl), etc.), lithium oxides (e.g., Li2O, Li2O2, etc.), and one of these alone or a mixture of two or more may be used, but is not limited thereto.

[0057] The above M-containing raw material and the above lithium-containing raw material may be mixed in a molar ratio of 1:3 to 1:6 in terms of stoichiometry, but are not limited thereto.

[0059] In the present invention, the calcination may be performed in an inert atmosphere to increase reaction efficiency and suppress side reactions. Specifically, the calcination may be performed in a nitrogen atmosphere or an argon atmosphere.

[0060] In the present invention, the firing may be performed at a temperature of 500 to 1000°C. Specifically, the firing temperature may be 600 to 650°C or 750 to 800°C.

[0061] In the present invention, the firing may be performed for 2 to 12 hours. For example, when the firing temperature is 600 to 650°C, the firing time may be 6 to 12 hours, and when the firing temperature is 750 to 800°C, the firing time may be 2 to 6 hours.

[0062] When the calcination temperature and calcination time are within the above ranges, an appropriate reaction rate can be achieved to prevent unreacted raw materials from remaining. In addition, single-phase synthesis is possible, and it has the effect of preventing excessive grain growth that would make crushing difficult.

[0064] In the present invention, the lithium metal oxide may be one or more selected from Li6CoO4, Li6MnO4, and Li5FeO4. Specifically, the lithium metal oxide may be Li6CoO4. When the lithium metal oxide is the above-mentioned material, it is well matched with the operating voltage range of the battery, which is 2.5 to 4.25V, and has an advantageous effect in that there are relatively few side reactions caused by metal leaching.

[0066] When mixing the above-mentioned raw materials, a moisture remover may be optionally added. Examples of the moisture remover include citric acid, tartaric acid, glycolic acid, or maleic acid, and a mixture of one or more of these may be used.

[0068] In the present invention, the lithium metal oxide has an average particle size (D 50 It may be composed of particles having a diameter of 40 μm or less. Specifically, the above-mentioned darium metal oxide is composed of particles with an average particle size (D 50 The particles may be composed of particles with a size of 40 μm or less and 38 μm or less. To achieve this, the particles may be ground using a jet mill or classified using a standard sieve. Although the average particle size of the lithium metal oxide is not necessarily limited to this range, when it falls within the above range, the manufacturing method of the present invention can sufficiently form a coating layer on the surface of the lithium metal oxide to improve atmospheric stability, and a lithium metal oxide of an appropriate size can be obtained by taking into account the thickness of the surface coating layer.

[0070] (2) Stage 2

[0071] A method for manufacturing an anode additive according to the present invention comprises the step of mixing the lithium metal oxide and an organometallic salt and heat-treating to form a coating layer on the surface of the lithium metal oxide.

[0072] According to the second step above, a coating layer can be formed on the surface of the lithium metal oxide through a simple process of mixing an organometallic salt with the lithium metal oxide and heat treating it, thereby improving the atmospheric stability and moisture resistance of the lithium metal oxide.

[0073] Through the above heat treatment, a coating layer can be formed on the surface of part or all of the darium metal oxide after the organometal salt is melted, and the organic functional groups among the organometal salt constitute an amorphous organic coating layer, and the metal atoms among the organometal salt are located inside the amorphous organic coating layer and can be composed of metal particles.

[0074] The above amorphous organic coating layer is located on the surface of the lithium metal oxide and can primarily perform the role of protecting the lithium metal oxide from the atmosphere and moisture, and the metal atoms are located inside the amorphous organic coating layer and act as a channel for lithium ions, thereby preventing the degradation of electrochemical performance when applied to a battery due to the formation of the amorphous organic coating layer.

[0076] In the present invention, the organometallic salt comprises one or more transition metals capable of coordination bonding and having a metal oxidation state of +3 to +6. This is a metal that can increase the conductivity of lithium ions within the organometallic salt-derived coating layer by performing the role of a lithium ion pathway as described above.

[0077] In this regard, the transition metal may include one or more metals selected from the group consisting of Sc, Y, Ti, Zr, V, Nb, Mo, W, Co, Rh, Ni, Pd, and Cu, and specifically may be Zr, Mo, or a combination thereof, most preferably Zr.

[0078] The form of the above organometallic salt is not particularly limited, but specifically, it may be one or more selected from the group consisting of metal acetylacetonate, metal stearate, metal dodecyl sulfate, metal oleate, metal laurate, metal myristate, metal palmitate, metal dodecylbenzenesulfonate, metal alkoxide, and metal hydrogen phosphate, and specifically, it may be metal acetylacetonate.

[0079] More specifically, the organometallic salt used in the present invention may be one or more selected from the group consisting of zirconium acetylacetonate and molybdenyl acetylacetonate, most preferably zirconium acetylacetonate.

[0081] In the present invention, the heat treatment may be performed at 150 to 400°C. More specifically, the heat treatment may be at 150°C or higher, 180°C or higher, 400°C or lower, 300°C or lower, or 250°C or lower. When the heat treatment temperature is within the above range, the organometallic salt can be sufficiently dissolved to uniformly form a coating layer without causing decomposition of the darium metal oxide represented by Chemical Formula 1. In addition, there is an effect of significantly improving atmospheric stability by preventing the crystallization of the amorphous region of the coating layer.

[0083] In the present invention, the heat treatment may be performed for 1 to 5 hours. Specifically, the heat treatment time may be 1 hour or more, 2 hours or more, 3 hours or more, and 5 hours or less. When the heat treatment time is within the above range, the crystalline phase of the lithium metal oxide represented by Chemical Formula 1 increases, thereby reducing side reactions and improving electrochemical capacity.

[0085] In the present invention, the heat treatment may be performed in a vacuum or an inert atmosphere to increase reaction efficiency and suppress side reactions. Specifically, the heat treatment may be performed under a nitrogen atmosphere or an argon atmosphere.

[0087] In the present invention, the content of the organometallic salt may be 0.5 to 20 parts by weight based on 100 parts by weight of the darium metal oxide, and specifically, it may be 1 part by weight or more, 2 parts by weight or more, 10 parts by weight or less, 8 parts by weight or less, 6 parts by weight or less, 5 parts by weight or less, 4 parts by weight or less, for example, 3 parts by weight. When the content of the organometallic salt is within the above range, it is desirable that a coating layer is sufficiently formed on the surface of the darium metal oxide, thereby achieving the effect of significantly improving atmospheric stability while minimizing the degradation of electrochemical performance.

[0089] anode additive

[0090] The anode additive according to the present invention is characterized by comprising: a divalent metal oxide represented by the following chemical formula 1; an amorphous organic coating layer located on the surface of the divalent metal oxide; and transition metal particles included inside the amorphous organic coating layer, capable of coordination bonding, and having a metal oxidation number of +3 to +6.

[0091] [Chemical Formula 1]

[0092] Li a MO b

[0093] In the above chemical formula 1,

[0094] M is one or more selected from the group consisting of Co, Mn, and Fe, and

[0095] 3 <a<7, 3<b<5이다.

[0097] The above-mentioned anode additive can be manufactured according to the manufacturing method of the present invention described above.

[0098] As described above, the amorphous organic coating layer may be derived from an organic functional group among the organometal salts, and the transition metal particles contained within the amorphous organic coating layer, capable of coordination bonding and having a metal oxidation state of +3 to +6, may be derived from a metal atom among the organometal salts.

[0100] The anode additive according to the present invention has the effect of preventing a rapid deterioration in electrochemical performance by maintaining the mobility of lithium ions through metal atoms disposed inside the amorphous organic coating layer, while improving atmospheric and moisture stability by protecting the surface of the lithium metal oxide through the amorphous organic coating layer.

[0102] In the present invention, the thickness of the coating layer may be 10 to 200 nm, specifically, 20 nm or more, 30 nm or more, 40 nm or more, 50 nm or more, 150 nm or less, 100 nm or less, most preferably 50 to 100 nm.

[0103] When the thickness of the above organometallic salt-derived coating layer is within the above range, the atmospheric stability and moisture stability of the anode additive can be effectively improved.

[0105] anode

[0106] The anode according to the present invention is characterized by including the anode additive. Since the anode includes the anode additive of the present invention, when applied to a battery, it may exhibit excellent atmospheric stability and moisture stability, and also excellent electrochemical performance.

[0107] The above-mentioned positive electrode comprises a positive electrode current collector and a positive electrode active material layer formed on the current collector, and the positive electrode active material layer comprises the positive electrode additive and the positive electrode active material.

[0108] The above-mentioned anode additive and the above-mentioned anode active material may be included in the anode active material layer in a weight ratio of 1:97 to 10:90.

[0109] The above-mentioned positive electrode active material is a layered compound such as lithium cobalt oxide (LiCoO2) or lithium nickel oxide (LiNiO2), or a compound substituted with one or more transition metals; lithium iron oxide such as LiFe3O4; and a compound with the chemical formula Li 1+c1 Mn 2-c1 Lithium manganese oxides such as O4 (0≤c1≤0.33), LiMnO3, LiMn2O3, LiMnO2, etc.; lithium copper oxide (Li2CuO2); vanadium oxides such as LiV3O8, V2O5, Cu2V2O7, etc.; chemical formula LiNi 1-c2 M c2 Ni-site type lithium nickel oxide represented by O2 (wherein M is at least one selected from the group consisting of Co, Mn, Al, Cu, Fe, Mg, B, and Ga, satisfying 0.01≤c2≤0.3); chemical formula LiMn 2-c3 M c3 A lithium manganese composite oxide represented by O2 (wherein M is at least one selected from the group consisting of Co, Ni, Fe, Cr, Zn and Ta, satisfying 0.01≤c3≤0.1) or Li2Mn3MO8 (wherein M is at least one selected from the group consisting of Fe, Co, Ni, Cu and Zn); or one or more selected from LiMn2O4 in which a portion of the Li of the chemical formula is substituted with alkaline earth metal ions.

[0110] The above positive current collector is not particularly limited as long as it is conductive without causing chemical changes in the battery, and for example, stainless steel, aluminum, nickel, titanium, calcined carbon, or aluminum or stainless steel surface treated with carbon, nickel, titanium, silver, etc. may be used. In addition, the above positive current collector may typically have a thickness of 3 to 500 μm, and fine irregularities may be formed on the surface of the current collector to increase the adhesion of the positive active material. For example, it may be used in various forms such as a film, sheet, foil, net, porous body, foam, nonwoven fabric, etc.

[0111] The above-described positive active material layer may include a positive conductive material and a positive binder together with the positive additive and positive active material prepared according to the present invention described above.

[0112] At this time, the positive electrode conductive material is used to impart conductivity to the electrode, and in the battery being constructed, any material that has electronic conductivity without causing chemical changes can be used without special limitations. Specific examples include graphite such as natural graphite or artificial graphite; carbon-based materials such as carbon black, acetylene black, Ketjen black, channel black, furnace black, lamp black, thermal black, and carbon fiber; metal powder or metal fiber such as copper, nickel, aluminum, or silver; conductive whiskey such as zinc oxide or potassium titanate; conductive metal oxide such as titanium oxide; or conductive polymers such as polyphenylene derivatives, and one of these alone or a mixture of two or more may be used.

[0113] In addition, the anode binder serves to improve adhesion between anode active material particles and adhesion between the anode active material and the anode current collector. Specific examples include polyvinylidene fluoride (PVDF), vinylidene fluoride-hexafluoropropylene copolymer (PVDF-co-HFP), polyvinyl alcohol, polyacrylonitrile, carboxymethylcellulose (CMC), starch, hydroxypropylcellulose, regenerated cellulose, polyvinylpyrrolidone, tetrafluoroethylene, polyethylene, polypropylene, ethylene-propylene-diene polymer (EPDM), sulfonated-EPDM, styrene butadiene rubber (SBR), fluororubber, or various copolymers thereof, and one of these alone or a mixture of two or more may be used.

[0115] The above secondary battery may include the positive electrode; the negative electrode; a separator interposed between the positive electrode and the negative electrode; and an electrolyte.

[0116] The above-mentioned cathode comprises a cathode current collector and a cathode active material layer formed on the current collector, wherein the cathode active material layer comprises a cathode active material, and as the cathode active material, a compound capable of reversible intercalation and deintercalation of lithium may be used. Specific examples include carbonaceous materials such as artificial graphite, natural graphite, graphitized carbon fiber, and amorphous carbon; metallic compounds capable of alloying with lithium such as Si, Al, Sn, Pb, Zn, Bi, In, Mg, Ga, Cd, Si alloys, Sn alloys, or Al alloys; and SiO₂ β Examples include metal oxides capable of doping and dedoping lithium, such as (0 < β < 2), SnO2, vanadium oxide, and lithium vanadium oxide; or composites comprising the metal compound and carbonaceous material, such as Si-C composites or Sn-C composites, and any one or more of these may be used. Additionally, a metallic lithium thin film may be used as the negative electrode active material. Furthermore, the carbon material may include low-crystallinity carbon and high-crystallinity carbon. Representative examples of low-crystallinity carbon include soft carbon and hard carbon, while representative examples of high-crystallinity carbon include amorphous, plate-like, flake-like, spherical, or fibrous natural or artificial graphite, Kish graphite, pyrolytic carbon, mesophase pitch-based carbon fiber, meso-carbon microbeads, mesophase pitches, and high-temperature calcined carbon such as petroleum or coal tar pitch-derived cokes.

[0118] The above-mentioned negative current collector is not particularly limited as long as it has high conductivity without causing chemical changes in the secondary battery, and for example, copper, stainless steel, aluminum, nickel, titanium, calcined carbon, copper or stainless steel surface-treated with carbon, nickel, titanium, silver, etc., and aluminum-cadmium alloy may be used. In addition, the above-mentioned negative current collector may typically have a thickness of 3 μm to 500 μm, and, similar to the positive current collector, fine irregularities may be formed on the surface of the current collector to strengthen the bonding strength of the negative active material. For example, it may be used in various forms such as a film, sheet, foil, net, porous body, foam, nonwoven fabric, etc.

[0119] The above-described cathode active material layer may include a cathode conductive material and a cathode binder together with the cathode active material described above.

[0120] The above cathode conductive material and cathode binder may be the same as those previously described for the anode.

[0122] The above separator separates the negative electrode and the positive electrode and provides a pathway for the movement of lithium ions. Any separator commonly used in secondary batteries can be used without special restrictions, and it is particularly desirable that it has low resistance to the movement of electrolyte ions and excellent electrolyte wettability. Specifically, a porous polymer film, such as a porous polymer film made of a polyolefin-based polymer like ethylene homopolymer, propylene homopolymer, ethylene / butene copolymer, ethylene / hexene copolymer, and ethylene / methacrylate copolymer, or a laminated structure of two or more layers thereof may be used. In addition, a conventional porous nonwoven fabric, such as a nonwoven fabric made of high-melting-point glass fiber or polyethylene terephthalate fiber, may be used. Furthermore, a coated separator containing ceramic components or polymer materials may be used to ensure heat resistance or mechanical strength, and it may optionally be used in a single-layer or multi-layer structure.

[0124] Examples of the above electrolytes that can be used in the manufacture of lithium secondary batteries include organic liquid electrolytes, inorganic liquid electrolytes, solid polymer electrolytes, gel-type polymer electrolytes, solid inorganic electrolytes, molten inorganic electrolytes, etc., but are not limited to these.

[0125] Specifically, the electrolyte may include a non-aqueous organic solvent and a metal salt.

[0126] As the above-mentioned non-aqueous organic solvent, for example, aprotic organic solvents such as N-methyl-2-pyrrolidinone, propylene carbonate, ethylene carbonate, butylene carbonate, dimethyl carbonate, diethyl carbonate, gamma-butyl lactone, 1,2-dimethoxyethane, tetrahydroxyfranc, 2-methyl tetrahydrofuran, dimethyl sulfoxide, 1,3-dioxolone, formamide, dimethylformamide, dioxolone, acetonitrile, nitromethane, methyl formate, methyl acetate, phosphate triester, trimethoxymethane, dioxolone derivatives, sulfolane, methyl sulfolane, 1,3-dimethyl-2-imidazolidinone, propylene carbonate derivatives, tetrahydrofuran derivatives, ether, methyl propionate, ethyl propionate, etc. may be used.

[0127] In particular, among the above carbonate-based organic solvents, ethylene carbonate and propylene carbonate, which are cyclic carbonates, are high-viscosity organic solvents with high dielectric constants that effectively dissociate lithium salts, so they can be used preferably. Furthermore, if low-viscosity, low-dielectric constant linear carbonates such as dimethyl carbonate and diethyl carbonate are mixed with these cyclic carbonates in appropriate proportions, an electrolyte with high electrical conductivity can be produced, making it even more preferable to use.

[0128] The metal salt mentioned above may be a lithium salt, and the lithium salt is a substance that dissolves well in the non-aqueous electrolyte; for example, as the anion of the lithium salt, F - , Cl - , I- , NO3 - , N(CN)2 - , BF4 - , ClO4 - , PF6 - , (CF3)2PF4 - , (CF3)3PF3 - , (CF3)4PF2 - , (CF3)5PF - , (CF3)6P - , CF3SO3 - , CF3CF2SO3 - , (CF3SO2)2N - , (FSO2)2N - , CF3CF2(CF3)2CO - , (CF3SO2)2CH - , (SF5)3C - , (CF3SO2)3C - , CF3(CF2)7SO3 - , CF3CO2 - , CH3CO2 - , SCN - and (CF3CF2SO2)2N - One or more types selected from the group consisting of can be used.

[0129] In addition to the above electrolyte components, the above electrolyte may further include one or more additives for the purpose of improving the lifespan characteristics of the secondary battery, suppressing the reduction of the secondary battery capacity, and improving the discharge capacity of the secondary battery, such as, for example, a haloalkylene carbonate-based compound such as difluoroethylene carbonate, pyridine, triethylphosphite, triethanolamine, cyclic ether, ethylene diamine, n-glyme, triamide hexaphosphate, nitrobenzene derivative, sulfur, quinone imine dye, N-substituted oxazolidinone, N,N-substituted imidazolidine, ethylene glycol dialkyl ether, ammonium salt, pyrrole, 2-methoxyethanol, or aluminum trichloride.

[0131] As described above, a lithium secondary battery containing a positive electrode additive manufactured according to the present invention is useful in portable devices such as mobile phones, laptop computers, and digital cameras, and in the field of electric vehicles such as hybrid electric vehicles (HEVs), because the degradation of electrochemical performance is suppressed.

[0133] Hereinafter, embodiments of the present invention are described in detail so that those skilled in the art can easily implement the invention. However, the present invention may be embodied in various different forms and is not limited to the embodiments described herein.

[0135] Examples and Comparative Examples: Preparation of Anode Additives

[0136] Example 1

[0137] Li2O and CoO were mixed in a molar ratio of 3:1, and then calcined at a temperature of 600°C for 12 hours under a nitrogen atmosphere to produce Li6CoO4.

[0138] The prepared Li6CoO4 was classified using a standard sieve (interval: 38 μm) to obtain only particles with a size of 38 μm or less.

[0139] To the Li6CoO4 particles obtained above, 1 part by weight of zirconium acetylacetonate was mixed based on 100 parts by weight of Li6CoO4, and heat-treated at a temperature of 220°C for 4 hours under a nitrogen atmosphere to produce Li6CoO4 with an organic-inorganic coating layer containing zirconium elements formed on the surface of the particles.

[0140] The prepared Li6CoO4 with an organic-inorganic coating layer was classified using a standard mesh (interval: 38 μm) to obtain only particles with a size of 38 μm or less, thereby obtaining the final anode additive.

[0142] Example 2

[0143] A cathode additive was obtained using the same method as in Example 1, except that 2 parts by weight of zirconium acetylacetonate were mixed based on 100 parts by weight of Li6CoO4.

[0145] Example 3

[0146] A cathode additive was obtained using the same method as in Example 1, except that 3 parts by weight of zirconium acetylacetonate were mixed based on 100 parts by weight of Li6CoO4.

[0148] Example 4

[0149] A cathode additive was obtained using the same method as in Example 1, except that 4 parts by weight of zirconium acetylacetonate were mixed based on 100 parts by weight of Li6CoO4.

[0151] Example 5

[0152] A cathode additive was obtained using the same method as in Example 1, except that 5 parts by weight of zirconium acetylacetonate were mixed based on 100 parts by weight of Li6CoO4.

[0154] Example 6

[0155] A cathode additive was obtained using the same method as in Example 1, except that 6 parts by weight of zirconium acetylacetonate were mixed based on 100 parts by weight of Li6CoO4.

[0157] Example 7

[0158] A cathode additive was obtained using the same method as in Example 1, except that 10 parts by weight of zirconium acetylacetonate were mixed based on 100 parts by weight of Li6CoO4.

[0160] Example 8

[0161] An anode additive was obtained using the same method as in Example 1, except that molybdenyl acetylacetonate was mixed in 2 parts by weight based on 100 parts by weight of Li6CoO4 instead of zirconium acetylacetonate.

[0163] Example 9

[0164] An anode additive was obtained using the same method as in Example 1, except that molybdenyl acetylacetonate was mixed in 4 parts by weight based on 100 parts by weight of Li6CoO4 instead of zirconium acetylacetonate.

[0166] Example 10

[0167] A cathode additive was obtained using the same method as in Example 1, except that molybdenyl acetylacetonate was mixed in 6 parts by weight based on 100 parts by weight of Li6CoO4 instead of zirconium acetylacetonate.

[0169] Comparative Example 1

[0170] Li2O and CoO were mixed in a molar ratio of 3:1, and then calcined at a temperature of 600°C for 12 hours under a nitrogen atmosphere to produce Li6CoO4.

[0171] The prepared Li6CoO4 was classified using a standard sieve (interval: 38 μm) to obtain only particles with a size of 38 μm or less.

[0172] The Li6CoO4 particles obtained above were heat-treated at a temperature of 220°C for 4 hours under a nitrogen atmosphere, and classified using a standard mesh (interval: 38 μm) to obtain only particles with a size of 38 μm or less, thereby obtaining an anode additive without a surface coating layer.

[0174] Comparative Example 2

[0175] An anode additive was obtained using the same method as in Example 1, except that 4 parts by weight of aluminum acetylacetonate were mixed based on 100 parts by weight of Li6CoO4 instead of zirconium acetylacetonate.

[0177] Comparative Example 3

[0178] An anode additive was obtained using the same method as in Example 1, except that aluminum acetylacetonate was mixed in 6 parts by weight based on 100 parts by weight of Li6CoO4 instead of zirconium acetylacetonate.

[0180] Comparative Example 4

[0181] An anode additive was obtained using the same method as in Example 1, except that aluminum acetylacetonate was mixed in 10 parts by weight based on 100 parts by weight of Li6CoO4 instead of zirconium acetylacetonate.

[0183] Comparative Example 5

[0184] An anode additive was obtained using the same method as in Example 1, except that zinc stearate was mixed in 10 parts by weight based on 100 parts by weight of Li6CoO4 instead of zirconium acetylacetonate.

[0186] Comparative Example 6

[0187] A cathode additive was obtained using the same method as in Example 1, except that 5 parts by weight of sodium dodecyl sulfate was mixed based on 100 parts by weight of Li6CoO4 instead of zirconium acetylacetonate.

[0189] Comparative Example 7

[0190] An anode additive was obtained using the same method as in Example 1, except that 10 parts by weight of sodium dodecyl sulfate was mixed based on 100 parts by weight of Li6CoO4 instead of zirconium acetylacetonate.

[0192] Experimental Example 1: Analysis of Anode Additives

[0193] (1) TEM analysis

[0194] TEM (FEI, Titan TM TEM images of the anode additives of Example 6 and Comparative Example 1 were obtained using a G2 80-200 device, and are shown in Figures 1 and 2, respectively.

[0195] Referring to Fig. 1, the anode additive of Example 1 has a zirconium acetylacetonate-derived coating layer formed on its surface, specifically an amorphous organic coating layer and zirconium particles with a needle-like structure distributed within it.

[0196] On the other hand, referring to Fig. 2, it was observed that the anode additive of Comparative Example 1, which lacks a surface coating layer, exhibited surface degradation during the TEM sample treatment process, resulting in the formation of a surface modified layer containing amorphous Li2CO3, LiOH, and nanocrystalline CaO.

[0198] (2) XRD phase analysis

[0199] When the anode additives of Example 4, Example 9, and Comparative Example 1 were exposed to a relative humidity of 33% and a temperature of 30°C for 18 hours, the changes in the anode additives were analyzed using an X-ray diffractometer (Brucker, D8 Endeavor).

[0200] Figure 3(a) shows XRD data of the anode additive of Example 4 before and after atmospheric exposure, and Figure 3(b) shows XRD data of the anode additive of Example 9 before and after atmospheric exposure.

[0201] Referring to Fig. 3, the anode additives of Examples 4 and 9 showed almost no degradation of the particle surface even upon exposure to the atmosphere due to the surface coating layer, so peaks corresponding to by-products such as Li2CO3 and LiOH were not observed. On the other hand, referring to Fig. 4, which shows the XRD data of the anode additive of Comparative Example 1 before and after exposure to the atmosphere, it was confirmed through the XRD data that by-products such as Li2CO3 and LiOH were formed.

[0203] Experimental Example 2: Evaluation of Atmospheric Stability

[0204] Each of the anode additives, carbon black conductive material, dispersant, and PVDF binder in Examples 1 to 10 and Comparative Examples 1 to 7 A composition for forming an anode was prepared by mixing in an N-methylpyrrolidone solvent (anode additive: 90-95 wt%, carbon black conductive material: 1-4 wt%, dispersant: 1.5-6 wt%, PVDF binder: 1-2 wt%), and after applying this to one side of an aluminum current collector, an anode was manufactured by drying at 130°C and rolling.

[0205] An electrode assembly was manufactured by interposing a porous polyethylene separator (W-scope, WL20C) between each anode and lithium metal cathode manufactured as described above, and after placing the electrode assembly inside a case, an electrolyte containing 1M LiPF6 in a solvent with a mixed volume ratio of EC / DMC / DEC = 1 / 2 / 1 was injected into the case to manufacture a coin half-cell.

[0207] In addition, each of the anode additives prepared above was placed in a constant temperature and humidity chamber and exposed for 18 hours at a relative humidity of 33% and a temperature of 30℃, and then a coin half-cell was prepared in the same way.

[0209] For the coin-type half-cells manufactured as described above, charging in CC mode at 0.1 C to 4.25 V at 25°C, charging in CV mode until reaching 0.05 C, and discharging in CC mode at 0.1 C until reaching 2.5 V was defined as one cycle, and the charge / discharge capacity of the first and second cycles was measured. The arrows indicate a comparison of the capacity before and after exposure of the cathode additive to the atmosphere.

[0211] Anode Additive (Weight%) First cycle Second cycle Total charging capacity (mAh / g) Charging capacity (mAh / g) Discharge capacity (mAh / g) Charging capacity (mAh / g) Discharge capacity (mAh / g) Example 1 92 753 -> 672 47 -> 25 108 -> 73 20 -> 11 861 -> 744 95 732 -> 605 15 -> 6 25 -> 12 12 -> 4 757 -> 617 Example 2 92 738 -> 690 47 -> 32 126 -> 83 21 -> 14 864 -> 773 95 733 -> 673 28 -> 11 41 -> 24 24 -> 9 774 -> 697 Example 3 95 749 -> 668 21 -> 11 32 -> 18 16 -> 7 781 -> 685 Example 4 95 729 -> 690 23 -> 15 35 -> 24 19 -> 12 764 -> 714 Example 5 95 715 -> 664 18 -> 10 28 -> 17 14 -> 8 743 -> 681 Example 6 92 723 -> 688 43 -> 32 141 -> 115 14 -> 9 865 -> 804 95 709 -> 649 16 -> 16 22 -> 11 9 -> 10 731 -> 669 Example 7 90 689 -> 652 23 -> 21 180 -> 245 6 -> 5 869 -> 897 Example 8 90 646 -> 650 35 -> 31 128 -> 79 19 -> 13 774 -> 729 Example 9 90 537 -> 654 24 -> 24 184 -> 81 6 -> 9 721 -> 735 Example 10 90 497 -> 565 23 -> 22 251 -> 113 5 -> 6 748 -> 677 Comparative Example 1 95 853 -> 597 26 -> 22 21 -> 28 13 -> 17 874 -> 625 Comparative Example 2 90 250 -> 384 6 -> 12 421 -> 147 2 -> 2 672 -> 531 Comparative Example 3 90 378 -> 366 18 -> 12 199 -> 129 2 -> 5 577 -> 495 Comparative Example 4 90 452 -> 378 8 -> 7 287 -> 213 1 -> 1 739 -> 591 Comparative Example 5 90 366 -> 217 12 -> 4 158 -> 246 7 -> 4 524 -> 462 Comparative Example 6 90 803 -> 553 33 -> 27 100 -> 383 11 -> 0 903 -> 936 Comparative Example 7 92 747 -> 481 11 -> 19 0 -> 0 0 -> 0 747 -> 481

[0212] Based on the above results, the initial charge capacity retention rate (%), total charge capacity retention rate (%), and irreversible capacity retention rate (%) were calculated by comparing the periods before and after atmospheric exposure.

[0213] Anode Additive (Weight%) Initial charge capacity retention rate (%) Total charge capacity retention rate (%) Irreversible capacity retention rate (%) Example 1 92 89 86 91 95 83 82 84 Example 2 92 93 89 95 95 92 90 94 Example 3 95 89 88 90 Example 4 95 95 93 98 Example 5 95 93 92 94 Example 6 92 95 93 97 95 92 92 91 Example 7 90 95 103 95 Example 8 90 101 94 101 Example 9 90 122 102 123 Example 10 90 114 91 114 Comparative Example 1 95 70 72 70 Comparative Example 2 90 153 79 153 Comparative Example 3 90 97 86 98 Comparative Example 4 90 84 80 84 Comparative Example 5 90 59 88 60 Comparative Example 6 90 69 104 68 Comparative Example 7 92 64 64 63

[0214] As summarized in the table above, it was confirmed that all batteries of the embodiments prepared including the cathode additive according to the present invention exhibited superior initial charge capacity retention rate (%), total charge capacity retention rate (%), and irreversible capacity retention rate (%) compared to the comparative examples. Although there were some cases where the initial charge capacity was too low, resulting in capacity development occurring in the second cycle, or where the capacity before exposure to the atmosphere was too low, resulting in a similar level of capacity after exposure, it was clearly observed that, even taking these factors into account, the tendency for capacity reduction due to exposure to the atmosphere to be significantly prevented in the embodiments compared to the comparative examples was clearly observed.

[0215] In other words, the anode additive of the example exhibits excellent atmospheric stability due to the coating layer on the surface of the lithium metal oxide, so its electrochemical performance is maintained at a high level even when exposed to the atmosphere.

[0216] In particular, in the case of the battery containing the cathode additive of Examples 1 to 7, which used zirconium acetylacetonate as an organometallic salt when forming the coating layer, the battery capacity was maintained at a high level even compared to the battery containing the cathode additive of Comparative Example 1, which did not have a surface coating layer, and it was found that not only was atmospheric stability improved, but a decrease in electrochemical performance was also prevented.

Claims

Claim 1 A method for manufacturing an anode additive comprising: a step of preparing a divalent metal oxide represented by the following chemical formula 1; and a step of mixing the divalent metal oxide with an organometal salt and heat-treating to form a coating layer on the surface of the divalent metal oxide; wherein the organometal salt comprises one or more transition metals capable of coordination bonding and having a metal oxidation state of +3 to +6, and the coating layer comprises an amorphous organic coating layer composed of organic functional groups among the organometal salts; and transition metal particles located inside the amorphous organic coating layer and composed of transition metals contained in the organometal salt: [Chemical Formula 1]Li a MO b In the above chemical formula 1, M is one or more selected from the group consisting of Co, Mn, and Fe, and 3 <a<7, 3<b<5이다. Claim 2 A method for manufacturing an anode additive according to claim 1, wherein the transition metal capable of coordination bonding and having a metal oxidation number of +3 to +6 comprises one or more selected from the group consisting of Sc, Y, Ti, Zr, V, Nb, Mo, W, Co, Rh, Ni, Pd, and Cu. Claim 3 A method for manufacturing an anode additive according to claim 1, wherein the organometallic salt is one or more selected from the group consisting of metal acetylacetonate, metal stearate, metal dodecyl sulfate, metal oleate, metal laurate, metal myristate, metal palmitate, metal dodecylbenzenesulfonate, metal alkoxide and metal hydrogen phosphate. Claim 4 A method for manufacturing an anode additive according to claim 1, wherein the organometallic salt is one or more selected from the group consisting of zirconium acetylacetonate and molybdenyl acetylacetonate. Claim 5 A method for manufacturing an anode additive according to claim 1, wherein the heat treatment is performed at 150 to 400°C. Claim 6 A method for manufacturing an anode additive according to claim 1, wherein the heat treatment is performed for 1 to 5 hours. Claim 7 A method for manufacturing an anode additive according to claim 1, wherein the heat treatment is performed under vacuum or an inert atmosphere. Claim 8 A method for manufacturing an anode additive according to claim 1, wherein the content of the organometallic salt is 0.5 to 20 parts by weight based on 100 parts by weight of darium metal oxide. Claim 9 A method for manufacturing an anode additive according to claim 1, wherein the lithium metal oxide is one or more selected from Li6CoO4, Li6MnO4, and Li5FeO4. Claim 10 Anode additive comprising: a divalent metal oxide represented by the following chemical formula 1; an amorphous organic coating layer located on the surface of the divalent metal oxide; and transition metal particles contained within the amorphous organic coating layer, capable of coordination bonding, and having a metal oxidation state of +3 to +6: [Chemical Formula 1]Li a MO b In the above chemical formula 1, M is one or more selected from the group consisting of Co, Mn, and Fe, and 3 <a<7, 3<b<5이다. Claim 11 An anode additive according to claim 10, wherein the thickness of the amorphous organic coating layer is 10 to 200 nm. Claim 12 An anode comprising the anode additive of claim 10 or 11.

Citation Information

Patent Citations

  • Rapid composite coating modification method of lithium battery positive electrode material

    CN112151781A

  • Pre-doping agent, positive electrode for lithium ion capacitor, and lithium ion capacitor and manufacturing method of the same

    JP2016012620A

  • Positive electrode active material for secondary battery, and positive electrode for secondary battery and secondary battery comprising the same

    KR1020170063146A

  • Irreversible Additive Comprised in Cathode Material for Lithium Secondary Battery, Preparing Method thereof, and Cathode Material Comprising the Same

    KR1020190059115A

  • Method for preparing positive electrode active material for lithium secondary battery and positive electrode active material thereby

    KR1020210009953A