Tabernacle Method and Tabernacle Device
The method forms silicon oxide films with reduced leakage current and improved electrical properties by using inhibitory layers and cyclic plasma treatments to address the challenges of selective deposition on insulating films in miniaturized semiconductors.
Patent Information
- Application Number
- KR1020247040050
- Authority / Receiving Office
- KR · KR
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2022-06-14
- Filing Date
- 2023-05-31
- Publication Date
- 2026-11-10
- Estimated Expiration
- 2043-05-31
AI Technical Summary
Existing methods struggle to selectively form silicon oxide films with desired electrical properties on insulating films without affecting conductive films, leading to increased capacitance and RC delay in miniaturized semiconductors.
A method involving the formation of an inhibitory layer on conductive regions, followed by selective deposition and modification of silicon oxide films using metal catalyst gases and silanol-containing gases, combined with cyclic plasma treatments using hydrogen and inert gases to reduce impurities and hydrogen defects.
Achieves the selective formation of silicon oxide films with reduced leakage current and improved electrical properties on insulating films, addressing the challenges of capacitance and RC delay in miniaturized semiconductors.
Smart Images

Figure 112026017592220-PCT00016_ABST
Abstract
Description
Technology Field
[0001] The present disclosure relates to a tabernacle method and a tabernacle apparatus. Background Technology
[0002] A technique is known for selectively depositing a silicon oxide film on the exposed surface of an insulating film for a substrate comprising a surface having an exposed conductive film and an insulating film. (See, for example, Patent Documents 1 to 3.) Prior art literature
[0003] Japanese Patent Publication No. JP 2019-52142, Japanese Patent Publication No. JP 2019-96881, U.S. Patent Publication No. 2021 / 301392 The problem to be solved
[0004] The present disclosure provides a technology that can selectively form a silicon oxide film having desired electrical properties on an insulating film. means of solving the problem
[0005] A film deposition method according to one aspect of the present disclosure is a film deposition method for forming a silicon oxide film on a substrate, comprising: (a) a step of preparing a substrate having a first region on the surface in which an insulating film is exposed and a second region in which a conductive film is exposed; (b) a step of selectively forming an inhibitory layer in the second region that inhibits the formation of the silicon oxide film; (c) a step of forming the silicon oxide film in the first region while the formation of the silicon oxide film in the second region is inhibited by the inhibitory layer; and (d) a step of modifying the silicon oxide film formed in the first region, wherein the step (c) comprises: (c1) a step of supplying a metal catalyst gas to the surface to adsorb the metal catalyst gas to the first region; and (c2) a step of supplying a silanol-containing gas to the surface to react the silanol-containing gas with the metal catalyst gas adsorbed to the first region to form a silicon oxide film, and the step (d) comprises (d1) a process of exposing the surface to a plasma generated from a first gas that does not contain hydrogen gas, and (d2) a process of exposing the surface to a plasma generated from a second gas that contains an inert gas that does not contain hydrogen gas. Effects of the invention
[0006] According to the present disclosure, a silicon oxide film having desired electrical properties can be selectively formed on an insulating film. Brief explanation of the drawing
[0007] Figure 1 is a flowchart illustrating a tabernacle method related to an embodiment. FIG. 2a is a cross-sectional view showing a membrane formation method related to an embodiment. FIG. 2b is a cross-sectional view showing a membrane formation method related to an embodiment. FIG. 2c is a cross-sectional view showing a membrane formation method related to an embodiment. FIG. 2d is a cross-sectional view showing a membrane formation method related to an embodiment. Figure 3 is a flowchart showing an example of step S5. Figure 4 is a flowchart showing an example of a modification process. FIG. 5 is a diagram showing an example of a processing system for carrying out a membrane formation method related to an embodiment. FIG. 6 is a drawing showing an example of a tabernacle apparatus for carrying out a tabernacle method related to an embodiment. Figure 7 is a diagram showing the measurement results of the leakage current (or leak current) of a silicon oxide film. Figure 8 is a diagram showing the measurement results of the infrared absorption spectrum of a silicon oxide film. Figure 9 is a diagram showing the measurement results of the infrared absorption spectrum of a silicon oxide film. Figure 10 is a diagram showing the measurement results of the infrared absorption spectrum of a silicon oxide film. Specific details for implementing the invention
[0008] Hereinafter, non-limiting exemplary embodiments of the present disclosure will be described with reference to the attached drawings. In all the attached drawings, identical or corresponding reference numerals are assigned to identical or corresponding members or parts, and redundant descriptions are omitted.
[0009] [Silicon Oxide Film]
[0010] It is known that for a substrate having a surface in which an insulating film and a conductive film are exposed, an AlO film is formed as the insulating film when the insulating film is selectively formed on the exposed surface of the insulating film. AlO films have a relatively high dielectric constant. For this reason, as semiconductors become miniaturized, if AlO films are used as interlayer insulating films, the capacitance between wirings increases, becoming a factor in RC delay. Furthermore, insulating films used in FSAVs (fully self-aligned vias) are also required to have a dielectric constant lower than that of AlO films. For this reason, silicon oxide films with low dielectric constants are being considered. Below, a method for selectively forming a silicon oxide film on the exposed surface of an insulating film for a substrate having a surface in which an insulating film and a conductive film are exposed is described.
[0011] [The Method of the Tabernacle]
[0012] With reference to FIGS. 1, 2a, 2b, 2c, and 2d, a method for forming a tabernacle related to an embodiment is described. The method for forming a tabernacle related to an embodiment has steps S1 to S7 shown in FIG. 1.
[0013] In step S1, as shown in FIG. 2a, a substrate (100) is prepared having a first region (A1) in which an insulating film (101) is exposed and a second region (A2) in which a conductive film (102) is exposed on its surface (100a).
[0014] The insulating film (101) is, for example, an interlayer insulating film. The interlayer insulating film is preferably a low-dielectric constant (Low-K) film. The insulating film (101) is not particularly limited, but is, for example, a SiO film, a SiN film, a SiOC film, a SiON film, or a SiOCN film. A SiO film means a film containing silicon (or silicon) (Si) and oxygen (O). The atomic ratio of Si to O in a SiO film is not limited to 1:1. The same applies to SiN films, SiOC films, SiON films, and SiOCN films. The insulating film (101) has a concave portion on its surface. The concave portion is, for example, a trench, a contact hole, or a via hole.
[0015] The conductive film (102) is filled into the interior of the concave portion. The conductive film (102) is not particularly limited, but is, for example, a Cu film, a Co film, a Ru film, or a W film.
[0016] The substrate (100) may further have a barrier film. The barrier film is formed along the inner surface of the concave portion. The barrier film is formed between the insulating film (101) and the conductive film (102). The barrier film suppresses metal diffusion from the conductive film (102) to the insulating film (101). The barrier film is not particularly limited, but is, for example, a TaN film or a TiN film. A TaN film refers to a film containing tantalum (Ta) and nitrogen (N). The elemental ratio of Ta to N in a TaN film is not limited to 1:1. The same applies to a TiN film.
[0017] In step S2, the surface (100a) of the substrate (100) is cleaned. For example, in step S2, a reducing gas such as hydrogen (H2) gas is supplied to the surface (100a) of the substrate (100) to remove the natural oxide film formed on the surface (100a) of the substrate (100). The natural oxide film is, for example, formed on the surface of the conductive film (102). In step S2, plasma can be generated from the reducing gas. The reducing gas can be used mixed with a noble gas such as argon (Ar) gas. In step S2, for example, the substrate (100) is heated to a temperature of 120°C or higher and 200°C or lower. Step S2 may be omitted.
[0018] In step S3, the surface (100a) of the substrate (100) is oxidized. For example, in step S3, an oxygen-containing gas, such as oxygen (O2) gas, is supplied to the surface (100a) of the substrate (100) to properly oxidize the surface of the conductive film (102). Since the natural oxide film is removed in advance, the density of oxygen atoms becomes the desired density. As a result, in step S4 described later, a dense inhibition layer (103) (for example, a self-assembled monolayer (SAM)) can be formed on the surface of the conductive film (102). In step S3, for example, the substrate (100) is heated to a temperature of 120°C or higher and 200°C or lower. Step S3 may be omitted.
[0019] In step S4, as shown in FIG. 2b, an inhibitory layer (103) that inhibits the formation of the silicon oxide film (104) described later is selectively formed in the second region (A2). The inhibitory layer (103) is formed, for example, by SAM. For example, in step S4, an organic compound containing fluorine (or fluorine), which is a raw material for SAM, is supplied to the surface (100a) of the substrate (100) to selectively form SAM in the second region (A2) among the first region (A1) and the second region (A2). In step S4, for example, the substrate (100) is heated to a temperature of 120°C or higher and 200°C or lower. The raw material for SAM is not particularly limited, but is, for example, a thiol-based compound.
[0020] Thiol compounds have hydrogenated sulfur as a head group and can be represented by the general formula "R-SH". R is, for example, at least some of the hydrogens in a hydrocarbon group substituted with fluorine. Specific examples of thiol compounds include CF3(CF2)5CH2CH2SH (1H,1H,2H,2H-perfluorooctanediol, PFOT) and CF3(CF2)7CH2CH2SH (1H,1H,2H,2H-perfluorodecanethiol, PFDT).
[0021] Thiol compounds are more easily chemically adsorbed onto the conductive film (102) compared to the insulating film (101). When the insulating film (101) is exposed in the first region (A1) and the conductive film (102) is exposed in the second region (A2), SAM is selectively formed in the second region (A2) among the first region (A1) and the second region (A2).
[0022] The raw materials for SAM are not limited to thiol compounds. For example, the raw materials for SAM may be phosphonic acid compounds. Phosphonic acid compounds can be represented by the general formula "RP(=O)(OH)2". Here, R is, for example, at least some of the hydrogens in a hydrocarbon group are substituted with fluorine.
[0023] In step S5, as shown in FIG. 2c, a silicon oxide film (104) is formed in the first region (A1) while the formation of the silicon oxide film (104) in the second region (A2) is inhibited by the inhibition layer (103). The silicon oxide film (104) is formed, for example, by a chemical vapor deposition (CVD) method. Step S5 includes, for example, steps S51 to S53 shown in FIG. 3.
[0024] In step S51, a metal catalyst gas is supplied to the surface (100a) of the substrate (100) to selectively adsorb the metal catalyst gas to the first region (A1). The metal catalyst gas is, for example, trimethylaluminum (TMA) gas. In step S51, the substrate is heated, for example, to a temperature of 120°C or higher and 300°C or lower.
[0025] In step S52, a silanol-containing gas is supplied to the surface (100a) of the substrate (100), and the silanol-containing gas is reacted with a metal catalyst gas adsorbed in the first region (A1) to form a silicon oxide film (104). Examples of silanol-containing gases include TPSOL (Tris(tert-pentoxy)silanol) and TBSOL (Tris(tert-butoxy)silanol). In step S52, for example, the substrate (100) is heated to a temperature of 120°C or higher and 300°C or lower.
[0026] TMA is adsorbed onto an insulating film (101) having OH groups, but adsorption is inhibited on an inhibitory layer (103). Since the silanol-containing gas reacts with the adsorbed TMA to proceed with film formation, a silicon oxide film is selectively formed on the insulating film (101).
[0027] In step S53, it is determined whether steps S51 to S52 have been performed a set number of times. If the number of times the steps have been performed has not reached the set number (NO in step S53), steps S51 to S52 are performed again. On the other hand, if the number of times the steps have reached the set number (YES in step S53), the process is terminated because the film thickness of the silicon oxide film (104) has reached a predetermined film thickness through plasma treatment. The number of times the steps in step S53 are set according to the film deposition amount so that the silicon oxide film (104) formed in step S5 reaches a predetermined film thickness. The film deposition amount can be adjusted by the supply amount of silanol-containing gas, etc. The predetermined film thickness is, for example, 2 nm or more and 5 nm or less. In this case, in step S6, plasma is likely to act on the entire film thickness direction of the silicon oxide film (104) formed in the preceding step S5. Because of this, the silicon oxide film (104) is modified throughout the entire film thickness direction. Meanwhile, if the film thickness of the silicon oxide film (104) formed in step S5 becomes larger than a predetermined film thickness, it becomes difficult for the modification by plasma to act on a deep position from the surface of the silicon oxide film (104) in step S6. The number of times step S53 is set may be one or multiple times.
[0028] In step S6, as shown in FIG. 2d, the silicon oxide film (104) formed in the first region (A1) is modified by exposing the surface (100a) of the substrate (100) to plasma (P). At this time, the inhibition layer (103) is removed. Step S6 includes, for example, steps S61 to S63 shown in FIG. 4.
[0029] In step S61, the surface (100a) of the substrate (100) is exposed to a plasma generated from a first gas containing hydrogen gas. Accordingly, impurities in the film, including Si-OH bonds, are removed. At this time, the removal of the inhibition layer (103) is also carried out. In step S61, when the silicon oxide film (104) is exposed to the plasma generated from the first gas, hydrogen defects may be generated in the silicon oxide film (104) due to the reaction between the active species contained in the plasma and the silicon oxide film (104). The first gas may be used mixed with an inert gas. The inert gas is, for example, a noble gas such as argon gas.
[0030] An example of the processing conditions for step S61 is as follows.
[0031] Hydrogen gas flow rate: 200~3000 sccm
[0032] Argon gas flow rate: 900~6000 sccm
[0033] Substrate temperature: 120~200℃
[0034] Processing pressure 1~5 Torr (133~667 Pa)
[0035] Processing time: 10~30 seconds
[0036] In step S62, the surface (100a) of the substrate (100) is exposed to a plasma generated from a second gas that contains an inert gas and does not contain hydrogen gas. Accordingly, hydrogen defects generated in the silicon oxide film (104) in step S61 are removed. As a result, both impurities, including Si-OH bonds, and hydrogen defects can be reduced, and the leakage current (or leak current) of the silicon oxide film can be further reduced compared to modification using only one type of plasma from either the first gas or the second gas. The inert gas is a noble gas, such as argon gas, for example.
[0037] An example of the processing conditions for step S62 is as follows.
[0038] Argon gas flow rate: 600~6000 sccm
[0039] Substrate temperature: 120~200℃
[0040] Processing pressure: 1~5 Torr (133~667 Pa)
[0041] Processing time: 10~30 seconds
[0042] In step S63, it is determined whether steps S61 to S62 have been performed a set number of times. If the number of times the steps have been performed has not reached the set number (NO in step S63), steps S61 to S62 are performed again. On the other hand, if the number of times the steps have reached the set number (YES in step S63), the processing is terminated. The number of times the steps in step S63 are set according to the film thickness of the silicon oxide film (104) formed in step S5. The number of times the steps in step S63 may be one or multiple times. The number of times the steps are set is preferably 2 to 6 times.
[0043] When performing steps S61 and S62 multiple times, for example, when switching between steps S61 and S62, the plasma may be maintained or temporarily stopped.
[0044] In step S7, it is determined whether steps S5 and S6 have been performed a set number of times. If the number of times the steps have been performed has not reached the set number (NO in step S7), steps S5 and S6 are performed again. Meanwhile, if the number of times the steps have reached the set number (YES in step S7), the process is terminated because the film thickness of the silicon oxide film (104) has reached the target film thickness. The number of times the steps in step S7 are set according to the target film thickness of the silicon oxide film (104). The target film thickness is, for example, 6 nm. The number of times the steps in step S7 may be one or multiple times. Additionally, if the number of times the steps in step S7 has not reached the set number (NO in step S7), step S4 may be performed again. By performing step S4 again, a dense inhibition layer (103) can be formed, thereby improving inhibition performance. Additionally, if the number of times the steps in step S7 has not reached the set number (NO in step S7), step S3 may be performed again. By repeating step S3, the adsorption capacity of the organic compound forming the inhibition layer (103) can be increased to form a dense inhibition layer (103), thereby improving inhibition performance.
[0045] As described above, according to the film formation method associated with the embodiment, a substrate (100) having a first region (A1) where an insulating film (101) is exposed and a second region (A2) where a conductive film (102) is exposed on the surface is prepared, and a silicon oxide film (104) is selectively formed on the insulating film (101). Next, a cyclic plasma treatment is performed, which includes a process of exposing the silicon oxide film (104) to a plasma generated from a first gas and a process of exposing the silicon oxide film (104) to a plasma generated from a second gas, and a cycle is performed one or more times. By performing cyclic plasma treatment on the silicon oxide film (104), both impurities and hydrogen defects in the film, including Si-OH bonds, can be reduced. As a result, the leakage current of the silicon oxide film (104) can be reduced. In this way, a silicon oxide film (104) having desired electrical characteristics can be selectively formed on the insulating film (101) through the film formation method associated with the embodiment.
[0046] However, as a method for modifying the silicon oxide film, it is also conceivable to perform an oxidation treatment on the silicon oxide film. However, in a substrate (100) having a first region (A1) where the insulating film (101) is exposed and a second region (A2) where the conductive film (102) is exposed on the surface, it is not desirable to perform an oxidation treatment on the silicon oxide film because the conductive film (102) is also oxidized.
[0047] [Processing System]
[0048] Referring to FIG. 5, an example of a processing system for carrying out a membrane formation method related to an embodiment will be described.
[0049] The processing system (PS) is equipped with processing devices (PM1~PM4), a vacuum transfer room (VTM), load lock chambers (LL1~LL3), an air transfer room (LM), load ports (LP1~LP3), and an overall control unit (CU).
[0050] Processing devices (PM1 to PM4) are each connected (or connected) to a vacuum transport chamber (VTM) through gate valves (G11 to G14). The processing devices (PM1 to PM4) are configured to allow the interior to be depressurized to a predetermined vacuum atmosphere (or state). The processing devices (PM1 to PM4) accommodate a substrate (W) inside and perform a desired processing.
[0051] The vacuum transport chamber (VTM) is configured to allow the interior to be depressurized to a predetermined vacuum atmosphere. A first transport device (TR1) capable of transporting a substrate (W) under a depressurized state is installed in the vacuum transport chamber (VTM). The first transport device (TR1) transports the substrate (W) to the processing devices (PM1~PM4) and the load lock chambers (LL1~LL3). The first transport device (TR1) has, for example, two transport arms (FK11, FK12) that can move independently.
[0052] The load lock chambers (LL1–LL3) are each connected to the vacuum return chamber (VTM) via gate valves (G21–G23). The load lock chambers (LL1–LL3) are each connected to the atmospheric return chamber (LM) via gate valves (G31–G33). The load lock chambers (LL1–LL3) are configured to switch their interiors between an atmospheric atmosphere and a vacuum atmosphere.
[0053] The interior of the atmospheric transport chamber (LM) is an atmospheric environment. Inside the atmospheric transport chamber (LM), for example, a down flow of clean air is formed. An aligner (AN) that performs alignment of the substrate (W) is installed inside the atmospheric transport chamber (LM). The aligner (AN) may be installed outside the atmospheric transport chamber (LM). A second transport device (TR2) is installed in the atmospheric transport chamber (LM). The second transport device (TR2) transports the substrate (W) to the load lock chambers (LL1~LL3), load ports (LP1~LP3), and the aligner (AN).
[0054] Load ports (LP1 to LP3) are installed on the long side wall of the waiting transport room (LM). Carriers (C) are installed in the load ports (LP1 to LP3). The carriers (C) include a carrier (C) containing a substrate (W) and an empty carrier (C). The carriers (C) may be, for example, a FOUP (Front Opening Unified Pod).
[0055] The overall control unit (CU) may be, for example, a computer. The overall control unit (CU) is equipped with a CPU (Central Processing Unit), RAM (Random Access Memory), ROM (Read Only Memory), and an auxiliary storage device. The CPU operates according to a program stored in the ROM or the auxiliary storage device and controls each part of the processing system (PS). For example, the overall control unit (CU) controls the operation of the processing unit (PM1~PM4), the first transfer unit (TR1), the second transfer unit (TR2), and the gate valves (G11~G14, G21~G23, G31~G33). For example, the overall control unit (CU) can control the operation of switching the interior of the load lock chambers (LL1~LL3) between an atmospheric atmosphere and a vacuum atmosphere.
[0056] Next, the operation of the processing system (PS) is described. First, the second conveying device (TR2) removes the substrate (W) from the carrier (C), conveys the removed substrate (W) to the aligner (AN), and removes it from the aligner (AN). Next, the aligner (AN) performs alignment of the substrate (W). Next, the second conveying device (TR2) removes the substrate (W) from the aligner (AN), conveys it to the load lock room (LL1), and removes it from the load lock room (LL1). Next, the inside of the load lock room (LL1) is switched from an atmospheric atmosphere to a vacuum atmosphere. After that, the first conveying device (TR1) removes the substrate (W) from the load lock room (LL1) and conveys the removed substrate (W) to the processing device (PM1).
[0057] Next, the processing device (PM1) performs steps S2 to S6 of the film formation method related to the embodiment. Subsequently, the overall control unit (CU) determines whether steps S2 to S6 have been performed a set number of times. If the number of times has not reached the set number, steps S2 to S6 are performed again.
[0058] Meanwhile, when the number of operations reaches the set number, the first transport device (TR1) takes the substrate (W) out of the processing device (PM1), transports the removed substrate (W) to the load lock room (LL3), and removes it from the load lock room (LL3). Subsequently, the interior of the load lock room (LL3) is switched from a vacuum atmosphere to an atmospheric atmosphere. After that, the second transport device (TR2) takes the substrate (W) out of the load lock room (LL3) and places it in the removed carrier (C). In this way, the processing of the substrate (W) is completed.
[0059] In the operation of the processing system (PS) described above, steps S2 to S6 are performed using one processing unit (PM1), but this is not limited thereto. For example, steps S2 to S6 can be performed using at least one of the other processing units (PM2 to PM4). For example, steps S2 to S6 can be performed using two or more of the four processing units (PM1 to PM4). For example, step S51 can be performed using processing unit (PM1), and step S52 can be performed using processing unit (PM2). In this case, the time required for temperature change when performing steps S51 and S52 at different temperatures can be reduced, thereby improving productivity.
[0060] [Tabernacle Equipment]
[0061] Referring to FIG. 6, an example of a film formation device used as a processing device (PM1~PM4) equipped in the processing system (PS) of FIG. 5 will be described.
[0062] The membrane device has a processing container (1), a storage stand (2), a shower head (3), an exhaust unit (4), a gas supply unit (5), an RF power supply unit (8), and a control unit (9).
[0063] The processing vessel (1) is constructed of a metal such as aluminum and has a roughly cylindrical shape. The processing vessel (1) accommodates a substrate (W). The substrate (W) may be, for example, a semiconductor wafer. An inlet / outlet port (11) for bringing in or taking out the substrate (W) is formed on the side wall of the processing vessel (1). The inlet / outlet port (11) is opened and closed by a gate valve (12). An annular exhaust duct (13) with a square cross-section is installed on the main body of the processing vessel (1). A slit (13a) is formed along the inner circumference of the exhaust duct (13). An exhaust port (13b) is formed on the outer wall of the exhaust duct (13). A ceiling wall (14) is installed on the upper surface of the exhaust duct (13) to block the upper opening of the processing vessel (1) through an insulating member (16). The space between the exhaust duct (13) and the insulating member (16) is hermetically sealed by a sealing member (15). The sealing member (15) may be, for example, an O-ring. The partition member (17) divides the interior of the processing container (1) vertically when the mounting base (2) (and cover member (22)) rises to the processing position described later.
[0064] The mounting base (2) supports the substrate (W) horizontally within the processing container (1). The mounting base (2) is formed in the shape of a disc corresponding to the size of the substrate (W) and is supported by a support member (23). The mounting base (2) is formed from a ceramic material such as AlN or a metal material such as aluminum or nickel alloy. A heater (21) for heating the substrate (W) is embedded inside the mounting base (2). The heater (21) is supplied with power from a heater power source (not shown) and generates heat. A thermocouple (not shown) is installed near the upper surface of the mounting base (2). By controlling the output of the heater (21) according to the temperature signal of the thermocouple, the substrate (W) is controlled to a predetermined temperature. A cover member (22) composed of a ceramic material such as alumina (or aluminum oxide) is installed on the mounting base (2) to cover the outer periphery of the upper surface and the side.
[0065] A support member (23) that supports the load-bearing stand (2) is installed on the bottom surface of the load-bearing stand (2). The support member (23) extends downward from the center of the bottom surface of the load-bearing stand (2) through a hole formed in the bottom wall of the processing container (1) and is connected (or connected) to a lifting mechanism (24). By means of the lifting mechanism (24), the load-bearing stand (2) is raised and lowered between the processing position indicated in FIG. 1 and the conveying position below it, indicated by the dashed line, where the substrate (W) can be conveyed, through the support member (23). A flange portion (25) is installed on the bottom of the processing container (1) of the support member (23). A bellows (26) is installed between the bottom surface of the processing container (1) and the flange portion (25). The bellows (26) isolates the condition inside the processing container (1) from the outside air and extends and retracts according to the lifting and lowering movement of the mounting stand (2).
[0066] Three support pins (27) (only two shown) are installed near the bottom surface of the processing container (1) to protrude upward from the lifting plate (27a). The support pins (27) are raised and lowered through the lifting plate (27a) by a lifting mechanism (28) installed below the processing container (1). The support pins (27) are inserted and penetrated through a through hole (2a) installed in the mounting stand (2) at the transfer position, so as to be able to protrude into the upper surface of the mounting stand (2). By raising and lowering the support pins (27), the receiving and delivery of the substrate (W) between the first transfer device (TR1) (Fig. 5) and the mounting stand (2) is achieved.
[0067] The shower head (3) supplies the treatment gas into the treatment vessel (1) in the form of a shower. The shower head (3) is made of metal and is installed facing the mounting base (2). The shower head (3) has a diameter almost identical to that of the mounting base (2). The shower head (3) has a main body (31) and a shower plate (32). The main body (31) is fixed to the ceiling wall (14) of the treatment vessel (1). The shower plate (32) is connected below the main body (31). A gas diffusion space (33) is formed between the main body (31) and the shower plate (32). A gas inlet (36) is provided in the gas diffusion space (33) to penetrate the center of the ceiling wall (14) and the main body (31). An annular projection (34) protruding downward is formed on the edge (or periphery) of the shower plate (32). A gas discharge port (35) is formed on the inner flat portion of the annular protrusion (34). When the mounting base (2) is in the processing position, a processing space (38) is formed between the mounting base (2) and the shower plate (32), and an annular gap (39) is formed by bringing the upper surface of the cover member (22) and the annular protrusion (34) close together.
[0068] The exhaust section (4) exhausts the interior of the processing vessel (1). The exhaust section (4) has an exhaust pipe (41) and an exhaust mechanism (42). The exhaust pipe (41) is connected to the exhaust port (13b). The exhaust mechanism (42) has a vacuum pump and a pressure control valve connected to the exhaust pipe (41). In the process, the gas inside the processing vessel (1) reaches the exhaust duct (13) through the slit (13a), and is exhausted from the exhaust duct (13) through the exhaust pipe (41) to the exhaust mechanism (42).
[0069] The gas supply unit (5) supplies various treatment gases to the shower head (3). The gas supply unit (5) includes a gas source (51) and a gas line (52). The gas source (51) includes a source of various treatment gases, a mass flow controller (or mass flow controller), and a valve. The various treatment gases include at least the gases used in the film formation method associated with the aforementioned embodiment. The various gases are introduced (or introduced) into the gas diffusion space (33) from the gas source (51) through the gas line (52) and the gas inlet (36).
[0070] The film forming device is a capacitively coupled plasma device, wherein the mounting base (2) functions as a lower electrode and the shower head (3) functions as an upper electrode. The mounting base (2) is grounded. The shower head (3) is connected to an RF power supply (8).
[0071] The RF power supply unit (8) supplies high-frequency power (hereinafter referred to as "RF power") to the shower head (3). The RF power supply unit (8) has an RF power source (81), a matching unit (82), and a power supply line (83). The RF power source (81) is a power source that generates RF power. The RF power source has a frequency suitable for generating plasma. The frequency of the RF power is, for example, a frequency within the range of 450 kHz in the low-frequency band to 2.45 GHz in the microwave band. The RF power source (81) is connected to the main body (31) through the matching unit (82) and the power supply line (83). The matching unit (82) has a circuit for matching the load impedance to the internal impedance of the RF power source (81). The RF power supply unit (8) may be configured to supply RF power to the mounting stand (2).
[0072] The control unit (9) is, for example, a computer and is equipped with a CPU (Central Processing Unit), RAM (Random Access Memory), ROM (Read Only Memory), auxiliary storage device, etc. The CPU operates according to a program stored in the ROM or auxiliary storage device and controls the operation of the film-forming device. The control unit (9) may be installed inside the film-forming device or outside the device. When the control unit (9) is installed outside the film-forming device, the control unit (9) can control the film-forming device using communication means such as wired or wireless communication.
[0073] [Example]
[0074] (Example 1)
[0075] In Example 1, to confirm the effect of the film formation method related to the embodiment, leakage current characteristics, which are one of the electrical characteristics of the silicon oxide film, were measured.
[0076] First, a first silicon oxide film was formed on the substrate by supplying TMA gas, an example of a metal catalyst gas, to the substrate, followed by supplying TPSOL gas, an example of a silanol-containing gas. Next, the silicon oxide film was modified by a first cyclic plasma treatment. In the first cyclic plasma treatment, the process of exposing the silicon oxide film to a plasma generated from hydrogen gas and argon gas, and the process of exposing the silicon oxide film to a plasma generated from argon gas, were repeated twice in this order. Next, a second silicon oxide film was formed on the substrate by supplying TMA gas to the substrate, followed by supplying TPSOL gas. Next, the silicon oxide film was modified by a second cyclic plasma treatment. In the second cyclic plasma treatment, the process of exposing the silicon oxide film to a plasma generated from hydrogen gas and argon gas, and the process of exposing the silicon oxide film to a plasma generated from argon gas, were repeated three times in this order. In the first and second cyclic plasma treatments, the time per cycle of the process of exposing the silicon oxide film to plasma generated from hydrogen gas and argon gas was fixed at 15 seconds. In addition, the time per cycle of the process of exposing the silicon oxide film to plasma generated from argon gas was also fixed at 15 seconds.
[0077] For comparison, the first and second cyclic plasma treatments were changed to hydrogen plasma treatments, and a silicon oxide film was formed without changing other conditions. In the hydrogen plasma treatment, a process was performed in which the silicon oxide film was exposed to a plasma generated from hydrogen gas and argon gas. The plasma irradiation time per cycle of this process was fixed at 90 seconds.
[0078] Next, the film thickness and leakage current density of the silicon oxide film formed on the substrate were measured. A spectroscopic ellipsometer was used to measure the film thickness. A mercury probe was used to measure the leakage current density. The results were compared based on the current density flowing through the silicon oxide film when an electric field of 5 MV / cm was applied to the silicon oxide film. The electric field was calculated by dividing the applied voltage by the film thickness. The current density was calculated by dividing the current measured upon voltage application by the electrode area of the mercury probe.
[0079] In Example 1, the film thickness of the silicon oxide film was changed by changing the supply time of the silanol-containing gas, and the leakage current density was measured for silicon oxide films with different film thicknesses.
[0080] Figure 7 is a diagram showing the measurement results of the leakage current of a silicon oxide film. In Figure 7, the horizontal axis represents the film thickness (nm) of the silicon oxide film, and the vertical axis represents the leakage current density (A / cm²) of the silicon oxide film. 2 Figure 7 indicates the leakage current density of the silicon oxide film treated with cyclic plasma, and the triangle indicates the leakage current density of the silicon oxide film treated with hydrogen plasma.
[0081] As shown in Fig. 7, the leakage current density of the silicon oxide film subjected to cyclic plasma treatment is 4.4×10 -8 A / cm 2 ~ 1.5×10 -7 A / cm 2 ...was. In this regard, the leakage current density of the silicon oxide film treated with hydrogen plasma was 2.8×10 -7 A / cm 2 ~ 2.9×10 -7 A / cm 2 ...was. From this result, it was found that the leakage current density was lower when cyclic plasma treatment was performed on the silicon oxide film compared to when hydrogen plasma treatment was performed.
[0082] (Example 2)
[0083] In Example 2, the infrared absorption spectrum of the silicon oxide film was measured to elucidate the mechanism by which the leakage current characteristics of the silicon oxide film change.
[0084] First, a silicon oxide film subjected to cyclic plasma treatment, a silicon oxide film subjected to hydrogen plasma treatment, and a silicon oxide film subjected to neither cyclic plasma treatment nor hydrogen plasma treatment were prepared. Hereinafter, the silicon oxide film subjected to neither cyclic plasma treatment nor hydrogen plasma treatment is referred to as an untreated silicon oxide film.
[0085] Next, the infrared absorption spectra of each prepared silicon oxide film were measured. Fourier Transform Infrared Spectroscopy was used to measure the infrared absorption spectra.
[0086] Figures 8 to 10 show the measurement results of the infrared absorption spectra of each silicon oxide film. In Figures 8 to 10, the horizontal axis represents the wavenumber (cm²). -1 ) is represented, and the vertical axis represents absorbance (au). In Figures 8 to 10, the solid line represents the absorbance of the silicon oxide film treated with cyclic plasma, the dotted line represents the absorbance of the silicon oxide film treated with hydrogen plasma, and the dashed line represents the absorbance of the untreated silicon oxide film.
[0087] In Fig. 8, wavenumber 3500 cm -1 ~ 3700 cm -1 The infrared absorption is due to Si-OH bonds. As shown in Fig. 8, the silicon oxide film treated with cyclic plasma and the silicon oxide film treated with hydrogen plasma have a wavenumber of 3500 cm⁻¹ compared to the untreated silicon oxide film. -1 ~ 3700 cm -1The infrared absorption is small. From this result, it is thought that Si-OH bonds can be removed by performing cyclic plasma treatment or hydrogen plasma treatment on the silicon oxide film.
[0088] In Fig. 9, wavenumber 890 cm -1 The infrared absorption is due to the bending vibrations of the H-Si≡O3 bond. As shown in Fig. 9, the silicon oxide film treated with hydrogen plasma has a wavenumber of 890 cm⁻¹ compared to the untreated silicon oxide film. -1 The infrared absorption is high. From this result, it is believed that hydrogen defects are generated in the silicon oxide film by performing hydrogen plasma treatment on the silicon oxide film. In this regard, the silicon oxide film treated with cyclic plasma has a wavenumber of 890 cm⁻¹ compared to the silicon oxide film treated with hydrogen plasma. -1 The infrared absorption is small. From this result, it is thought that hydrogen defects generated by exposure to a plasma generated from hydrogen gas and argon gas can be removed by exposing the silicon oxide film to a plasma generated from hydrogen gas and argon gas, and then exposing it to a plasma generated from argon gas.
[0089] In Fig. 10, wavenumber 2250 cm -1 The infrared absorption is due to the stretching vibration of H-Si≡O3. As shown in Fig. 10, the silicon oxide film treated with hydrogen plasma has a wavenumber of 2250 cm⁻¹ compared to the untreated silicon oxide film. -1 The infrared absorption is high. From this result, it is believed that hydrogen defects are generated in the silicon oxide film by performing hydrogen plasma treatment on the silicon oxide film. In this regard, the silicon oxide film treated with cyclic plasma has a wavenumber of 2250 cm⁻¹ compared to the silicon oxide film treated with hydrogen plasma. -1The infrared absorption is small. From this result, it is believed that hydrogen defects generated by exposing a silicon oxide film to a plasma generated from hydrogen gas and argon gas can be removed by exposing it to a plasma generated from argon gas after exposing it to a plasma generated from hydrogen gas and argon gas.
[0090] From the results shown in Figures 8 to 10 above, it is believed that by performing cyclic plasma treatment on the silicon oxide film, both Si-OH bonds and hydrogen defects could be reduced, and as a result, the leakage current density of the silicon oxide film was reduced.
[0091] The embodiments disclosed herein are illustrative in all respects and should not be interpreted restrictively. The above embodiments may be omitted, substituted, or modified in various forms without departing from the appended claims and their intent.
[0092] This international application claims priority based on Japanese patent application No. 2022-095858 filed on June 14, 2022, and incorporates the entire contents of said application into this international application.
Claims
Claim 1 A method for forming a silicon oxide film on a substrate comprises: (a) a step of preparing a substrate having a first region on the surface in which an insulating film of low dielectric constant is exposed and a second region in which a conductive film is exposed; (b) a step of selectively forming an inhibitory layer in the second region that inhibits the formation of the silicon oxide film; (c) a step of forming the silicon oxide film in the first region while the formation of the silicon oxide film in the second region is inhibited by the inhibitory layer; and (d) a step of modifying the silicon oxide film formed in the first region to remove impurities in the silicon oxide film, wherein the step (c) comprises: (c1) a step of supplying a metal catalyst gas to the surface to adsorb the metal catalyst gas to the first region; and (c2) a step of supplying a silanol-containing gas to the surface to react the silanol-containing gas with the metal catalyst gas adsorbed to the first region to form a silicon oxide film, and the step (d) comprises: (d1) a step of... to a plasma generated from a first gas including hydrogen gas A film formation method comprising a process of exposing the above surface and (d2) a process of exposing the above surface to a plasma generated from a second gas that does not contain hydrogen gas but contains an inert gas. Claim 2 A film formation method according to claim 1, wherein in the above process (d), a cycle including the above process (d1) and the above process (d2) is performed multiple times. Claim 3 A film formation method according to claim 1, wherein the plasma is maintained when switching between the process (d1) and the process (d2). Claim 4 A film formation method according to claim 1, wherein the plasma is stopped when switching between the process (d1) and the process (d2). Claim 5 In claim 1, the first gas is an inert gas, forming a film method. Claim 6 A method for forming a film that maintains the supply of the inert gas when switching between the above (d1) process and the above (d2) process in claim 5. Claim 7 A film formation method according to claim 1, wherein in the above process (c), a cycle including the above process (c1) and the above process (c2) is performed multiple times. Claim 8 A film formation method according to claim 1, wherein the cycle including the above (c) process and the above (d) process is performed multiple times. Claim 9 A method for forming a film according to claim 8, wherein the above-mentioned (b) process is further included in a cycle performed multiple times. Claim 10 In claim 1, the inhibition layer is formed by a self-assembled monolayer. Claim 11 In claim 1, the metal catalyst gas is a TMA gas in the film formation method. Claim 12 In claim 1, the film formation method wherein the silanol-containing gas is a TPSOL gas. Claim 13 A film deposition apparatus for forming a silicon oxide film on a substrate comprises a processing vessel, a gas supply unit for supplying gas into the processing vessel, and a control unit. The control unit is configured to control the gas supply unit to perform the following steps: (a) a process of preparing a substrate having a surface having a first region in which a low dielectric constant insulating film is exposed and a second region in which a conductive film is exposed; (b) a process of selectively forming an inhibitory layer that inhibits the formation of the silicon oxide film in the second region; (c) a process of forming the silicon oxide film in the first region while inhibiting the formation of the silicon oxide film in the second region by the inhibitory layer; and (d) a process of modifying the silicon oxide film formed in the first region to remove impurities in the silicon oxide film. The process (c) comprises: (c1) a process of supplying a metal catalyst gas to the surface to adsorb the metal catalyst gas to the first region; and (c2) a process of supplying a silanol-containing gas to the surface to react the silanol-containing gas with the metal catalyst gas adsorbed to the first region to form a silicon oxide film. A film forming apparatus comprising a process, wherein the process (d) comprises: (d1) a process of exposing the surface to a plasma generated from a first gas including hydrogen gas; and (d2) a process of exposing the surface to a plasma generated from a second gas including an inert gas and not including hydrogen gas. Claim 14 A film formation method according to claim 1, wherein the low dielectric constant insulating film is a SiO film, SiN film, SiOC film, SiON film, or SiOCN film. Claim 15 A film formation method according to claim 1, wherein the process (d1) exposes the surface to a plasma generated from the first gas to remove impurities including Si-OH bonds, and the process (d2) exposes the surface to a plasma generated from the second gas to remove hydrogen bonds generated while removing the impurities.
Citation Information
Patent Citations
Tabernacle method and tabernacle device
KR1020220059965A
METHOD OF FORMING A SELF-ALIGNED CONTACT USING SELECTIVE SiO2 DEPOSITION
KR1020180093833A
Method of post-deposition treatment for silicon oxide film
KR1020190095142A
Tabernacle Method
KR1020220050198A