Photomask blank, method for processing photomask blank, and method for manufacturing photomask blank
Patent Information
- Application Number
- TW114131507
- Authority / Receiving Office
- TW · TW
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2024-08-21
- Filing Date
- 2025-08-19
- Publication Date
- 2026-11-11
- Estimated Expiration
- 2045-08-18
AI Technical Summary
Existing photomask technologies face challenges in transferring resist patterns with high precision onto absorber layers in EUV lithography due to the increase in aspect ratio and interlayer mixing issues when using SOG films as hard masks, which disrupt the periodic structure of multilayer reflective films.
A silicon-containing hard mask film is used, cured at temperatures between 50°C and 180°C, to form a blank photomask that prevents interlayer mixing and maintains EUV light reflectivity, allowing for high-precision pattern transfer.
The silicon-containing hard mask film enables precise transfer of fine resist patterns onto the absorber layer without degrading EUV light reflectivity, improving pattern resolution and accuracy in photomask manufacturing.
Smart Images

Figure TWG2TB001920765_001 
Figure TWG2TB001920765_002
Abstract
Description
[Technical Field]
[0001] The present invention relates to a material for making a photomask, a blank photomask having a hard mask film when etching a thin film formed on a substrate, a processing method for using the blank photomask, and a manufacturing method thereof. [Previous Technology]
[0002] With the miniaturization of semiconductor devices, there are currently exposure methods that use optical projection exposure devices with ArF excimer lasers to transfer patterns onto wafers using light masks. However, exposure methods using such optical projection exposure devices will eventually reach the resolution limit, so there are proposals for new pattern formation methods using direct drawing or imprinting photolithography or EUV photolithography with electron beam lithography devices.
[0003] Among these new lithography technologies, EUV exposure, considered the limit of short-wavelength ultraviolet exposure, uses EUV light with a wavelength of approximately 13.5 nm, which is shorter than that of excimer laser, and is reduced to about 1 / 4 of the usual wavelength for exposure. It has attracted attention as a next-generation lithography technology for semiconductor devices. In EUV exposure, because of the short wavelength, refractive optical systems cannot be used, and there are proposals to use reflective optical systems such as reflective masks (Patent Document 1). As a multilayer film structure used in the above-mentioned reflective mask, the reflective film (multilayer reflective film layer) is usually a multilayer film formed by alternating layers of a material with a relatively high refractive index and a material with a relatively low refractive index at the nanometer level. For example, it is known that a multilayer film formed by alternating layers of Si thin films and Mo thin films is used as a material with a high reflectivity for EUV light of 13~14 nm.
[0004] In the formation of a photomask pattern, for example, a composite substrate has a substrate, on which there are multiple reflective film layers, on which there is a cover layer that serves as a protective layer for the multiple reflective film layers during oxidation or mask cleaning, on which there is a buffer layer to prevent etching damage during the formation of the photomask pattern, on which there is an absorber layer that absorbs EUV light, and on which there is a hard mask layer that is resistant to etching of the absorber layer. A photoresist film is formed on the composite substrate to make a blank photomask. The photoresist film of the blank photomask is patterned by an electron beam, and then a resist pattern is obtained by development. The obtained resist pattern is used as a mask, the absorber layer is etched, and the absorber layer pattern is processed. However, if the photoresist film thickness is maintained in the same manner as before miniaturization when the absorber layer pattern is miniaturized, the ratio of film thickness to pattern, i.e., the aspect ratio, increases. This deteriorates the shape of the photoresist pattern, making it difficult to transfer the pattern smoothly, or, depending on the situation, causing the resist pattern to collapse or peel off. Therefore, the resist film thickness needs to be reduced along with miniaturization.
[0005] On the other hand, regarding the absorber layer etched using resist patterns as a mask, materials such as Ta, TaB, TaBN, TaO, and TaN, with Ta as the main component, or materials with Cr, Cr as the main component and having at least one component selected from N, O, and C, are used. Etching of materials with Ta as the main component can be patterned using chlorine-based dry etching, and etching of materials with Cr as the main component can be patterned using fluorine-based dry etching. However, for the reasons described above, the method of etching the absorber layer using a thin-film resist becomes increasingly difficult to ensure sufficient processing accuracy in the formation of mask patterns for EUV exposure. Therefore, a hard mask layer needs to be formed under the photoresist film.
[0006] Although not a method for processing reflective blank photomasks, for example, in order to dry etch a silicon-based light-shielding film using a thin film resist, a thin chromium-based material film of sufficient thickness as a hard mask is used as the hard mask film, thereby achieving high precision in the mask pattern, is disclosed in Patent Document 2. Similarly, Patent Document 3 discloses that a silicon-based material film can be used as a hard mask for a chromium light-shielding film.
[0007] Furthermore, as mentioned above, regarding the method of forming a hard mask by forming a film between a chromium-based material processed under chlorine-based dry etching conditions and a material containing transition metals and silicon processed under fluorine-based dry etching conditions, it is further proposed to use an SOG film as the hard mask film when processing the chromium-based material film (Patent Document 4).
[0008] When using SOG film as a hard mask film, the SOG film is baked at high temperature after coating to harden it, and it is necessary to prevent it from mixing with the photoresist film. For example, the embodiment in Patent Document 4 uses a baking process at 190°C. On the other hand, the processing method of a reflective blank mask having multiple reflective film layers does not mention whether SOG film can be used as a hard mask, and its practicality as an EUV blank mask is unclear. One reason for this is that when the SOG film is hardened in a reflective blank mask, the multiple reflective film layers stacked under the SOG film are also subjected to high temperature, which disrupts the periodic structure of the multiple reflective film layers, thus causing a decrease in the reflectivity of EUV light or the generation of phase defects.
[0009] An embodiment of Patent Document 5 involves forming a phase transfer film on a quartz substrate, creating a light-shielding layer thereon to prepare a photomask substrate, spin-coating a silicon-containing composition, and baking at 250°C to form a silicon-containing film. [Prior Art Documents] [Patent Documents]
[0010] [Patent Document 1] Japanese Patent Application Publication No. Sho 63-201656 [Patent Document 2] Japanese Patent Application Publication No. 2007-241060 [Patent Document 3] Japanese Patent Application Publication No. 2006-146152 [Patent Document 4] Japanese Patent Application Publication No. 2008-26500 [Patent Document 5] Japanese Patent Application Publication No. 2010-230986 [Summary of the Invention]
[0011] [Problems to be Solved by the Invention] As mentioned above, in the further improvement of the precision of reflective photomask technology, it is required to transfer the resist pattern to the absorber layer with higher precision. The use of SOG film as a hard mask film is useful from the point of view to make up for the insufficient dry etching resistance of thin film photoresist or to improve the pattern resolution of photoresist, but the problems of suppressing the intermixing with photoresist and suppressing the interlayer intermixing of multilayer reflective film layers still remain.
[0012] This invention was made in view of the above-mentioned matters, and its purpose is to provide a blank photomask containing a silicon-containing hard mask film that functions as a hard mask when the absorber layer is processed by dry etching, and also contributes to the improvement of resist pattern resolution; a method for processing the blank photomask using the same; and a method for manufacturing the blank photomask. [Means for Solving the Problem]
[0013] In order to solve the above-mentioned problems, the present invention provides a blank photomask, characterized in that it comprises: a substrate, a multilayer reflective film layer formed on the substrate for reflecting EUV light, an absorber layer formed on the multilayer reflective film layer for absorbing EUV light, a silicon-containing hard mask film formed directly or indirectly on the absorber layer, and a photoresist film formed on the silicon-containing hard mask film; the silicon-containing hard mask film is a cured form of a silicon-containing hard mask film forming composition cured at a temperature of 50°C to 180°C.
[0014] As long as the blank photomask is of this type, because it contains a silicon-containing hard mask film which is useful as a hard mask film, it can transfer fine resist patterns to the absorber layer with high precision. In addition, because the silicon-containing hard mask film can be formed within the above-mentioned temperature range, it will not cause interlayer mixing of the multilayer reflective film, thus improving the transfer accuracy of the resist pattern. That is, by using the blank photomask of the present invention, a photomask containing an absorber layer with fine patterns formed with high precision can be provided without degrading the reflectivity of EUV light. In other words, the blank photomask of the present invention contains a silicon-containing hard mask film that can function as a hard mask when the absorber layer is processed by dry etching, and can also contribute to the improvement of the resolution of the resist pattern.
[0015] Furthermore, the composition for forming the silicon-containing hard masking film is preferably a silicon-containing compound having any one or more of the following general formula (Sx-1), general formula (Sx-2), and substructure (Sx-3). [Chemical 1] (wherein, Ra, Rb, and Rc are each a monovalent organic group with 1 to 30 carbon atoms, which may be the same or different.)
[0016] As long as the composition for forming a silicon-containing hard mask film is as described, it exhibits excellent thermosetting properties, and thus a hardened film can be formed by baking at a temperature of 50°C to 180°C. Furthermore, a silicon-containing hard mask film with excellent resistance to dry etching can be formed. Therefore, as long as a blank photomask containing such a hardened composition for forming a silicon-containing hard mask film is provided, a photomask containing an absorber layer with finely patterned microstructures can be provided.
[0017] In this case, in the above formulas (Sx-1)~(Sx-3), at least one of Ra~Rc should be an organic group having one or more carbon-oxygen single bonds or carbon-oxygen double bonds.
[0018] As long as it is a composition for forming a silicon-containing hard mask film containing a silicon-containing compound having such an organic group, it has excellent thermosetting properties, and thus can be formed by baking at a temperature of 50°C to 180°C.
[0019] The above-mentioned composition for forming silicon-containing hard masking films shall preferably contain a crosslinking catalyst.
[0020] As long as it is a silicon-containing hard mask film forming composition, the thermosetting properties are even better, so that a hardened film can be reliably formed by baking at a temperature of 50°C to 180°C.
[0021] The above-mentioned crosslinking catalyst is preferably a strontium salt, ferrophosphate salt, phosphonium salt, ammonium salt, alkali metal salt, or a polysiloxane having any one of strontium salt, ferrophosphate salt, phosphonium salt, and ammonium salt as part of its structure.
[0022] As long as it is a silicon-containing hard masking film forming composition, the thermosetting properties are particularly excellent, so that a hardened film can be formed more reliably by baking at a temperature of 50°C to 180°C.
[0023] Furthermore, the present invention provides a method for processing a blank photomask, comprising the following steps: (i-1) irradiating the blank photomask of the present invention with an electron beam, and then developing it with a developer to form a photoresist pattern on the photoresist film; (i-2) forming the silicon-containing film pattern on the silicon-containing hard mask film by etching the photoresist pattern as a mask; and (i-3) processing the absorber layer directly or indirectly by etching the silicon-containing film pattern as a mask.
[0024] Because the blank photomask processing method of this invention uses a silicon-containing hard mask film, which has better dry etching resistance to chlorine gases than a photoresist film, as the hard mask, the resist pattern can be transferred to the absorber layer of the blank photomask with high precision. Furthermore, the silicon-containing hard mask film can be formed in a temperature range of 50°C to 180°C, thus preventing interlayer mixing of multiple reflective film layers and improving the transfer accuracy of the resist pattern. In other words, by using the blank photomask processing method of this invention, a photomask containing an absorber layer with finely patterned absorbers that does not degrade the reflectivity of EUV light can be provided.
[0025] Furthermore, the present invention provides a method for manufacturing a blank photomask, comprising the following steps: preparing a substrate; forming a multilayer reflective film layer that reflects EUV light on the substrate; forming an absorber layer that absorbs EUV light on the multilayer reflective film layer; directly or indirectly coating the absorber layer with a silicon-containing hard mask film forming composition that is cured at a temperature of 50°C to 180°C to obtain a coating film; curing the coating film at a temperature of 50°C to 180°C to form a silicon-containing hard mask film; and forming a photoresist film on the silicon-containing hard mask film.
[0026] As long as the method for manufacturing such a blank photomask can form a silicon-containing hard mask film that is useful as a hard mask film, a blank photomask capable of transferring fine resist patterns onto the absorber layer with high precision can be manufactured. Furthermore, by forming the silicon-containing hard mask film within the aforementioned temperature range, interlayer mixing of multiple reflective film layers is not triggered, thus improving the transfer accuracy of the resist pattern. In other words, the method for manufacturing the blank photomask of the present invention can provide a blank photomask that does not degrade the reflectivity of EUV light and can form fine patterns onto the absorber layer with high precision. [Effects of the Invention]
[0027] As described above, by using the blank photomask of the present invention, a photomask with an absorber layer having finely patterned microstructures formed with high precision can be provided without degrading the reflectivity of EUV light. That is, the blank photomask of the present invention is a blank photomask containing a silicon-containing hard mask film that can function as a hard mask when the absorber layer is processed by dry etching, and can also contribute to the improvement of the resolution of the resist pattern.
[0028] Furthermore, according to the blank photomask processing method of the present invention, a photomask with an absorber layer having finely patterned microstructures formed with high precision can be provided without degrading the reflectivity of EUV light.
[0029] Furthermore, according to the blank photomask manufacturing method of the present invention, a blank photomask can be manufactured that does not degrade the reflectivity of EUV light and can form fine patterns on the absorber layer with high precision.
Implementation Method
[0031] As mentioned above, further improvements in the precision of reflective photomask technology require the ability to transfer resist patterns onto the absorber layer with higher accuracy. Using SOG films as hard masking films is useful in compensating for the insufficient dry etching resistance of thin-film photoresists (Patent Document 4), and can also be expected to improve the pattern resolution of the photoresist. However, it is unclear whether SOG films can be used as hard masks in the processing method of reflective photomasks with multiple reflective film layers. Furthermore, it is believed that the following issues exist: in reflective photomask systems, when the SOG film is hardened, high temperatures are also applied to the multiple reflective films stacked beneath the SOG film, disrupting the periodic structure of the multiple reflective films, which could lead to a decrease in EUV light reflectivity or the generation of phase defects.
[0032] The inventors of this invention explored blank photomasks, blank photomask processing methods, and blank photomask manufacturing methods for transferring resist patterns to absorber layers with high precision. Through repeated and in-depth research, they discovered that by using a hardened material formed from a silicon-containing hard mask film forming composition that is cured at a temperature of 50°C to 180°C as a hard mask, it is possible to avoid interlayer mixing of multiple reflective film layers, thereby improving the transfer precision of the resist pattern on the absorber layer. This invention was thus completed.
[0033] That is, the present invention is a blank photomask, characterized in that it comprises: a substrate, a multilayer reflective film layer formed on the substrate for reflecting EUV light, an absorber layer formed on the multilayer reflective film layer for absorbing EUV light, a silicon-containing hard mask film formed directly or indirectly on the absorber layer, and a photoresist film formed on the silicon-containing hard mask film; the silicon-containing hard mask film is a cured form of a silicon-containing hard mask film forming composition cured at a temperature of 50°C to 180°C.
[0034] The blank photomask, the method for processing the blank photomask, and the method for manufacturing the blank photomask of the present invention use a hardened material formed by a silicon-containing hard mask film forming composition that can be cured at a temperature of 50°C to 180°C for use as a hard mask. Therefore, it can prevent interlayer mixing of multiple reflective film layers and improve the transfer accuracy of the resist pattern of the absorber layer. That is, the present invention can provide a blank photomask that can achieve a photomask containing an absorber layer with a finely patterned absorber layer that does not degrade the reflectivity of EUV light, and is therefore extremely useful in the fine patterning of semiconductor device manufacturing.
[0035] Hereinafter, the present invention will be described in detail, but the present invention is not limited thereto.
[0036] <Blank Photomask> First, the structure of the reflective blank photomask and reflective light shield of the present invention will be described below with reference to the drawings. In the description of the drawings, the same reference numerals are added for the same constituent elements, and sometimes the description is omitted. In addition, for convenience, the drawings are sometimes enlarged, and the size ratio of each constituent element is not necessarily the same as the actual size.
[0037] The curing of the composition for forming the silicon-containing hard mask film in this specification is such that when the photoresist material is coated on the silicon-containing hard mask film, the reduction in film thickness of the silicon-containing hard mask film is slight and does not result in intermingling with the photoresist film. At this time, the reduction in film thickness of the silicon-containing hard mask film relative to the film thickness before the photoresist material coating is preferably less than 5%, more preferably less than 3%, further preferably less than 1%, and especially preferably less than 0.5%.
[0038] [Overall Structure of Blank Photomask] The blank photomask (reflective photomask substrate) of the present invention generally comprises a substrate, a multilayer reflective film layer formed on the substrate (e.g., on one of the main surfaces of the substrate) to reflect EUV light (exposure light), an absorber layer (light absorption film) formed on the multilayer reflective film layer, a silicon-containing hard mask film formed directly or indirectly on the absorber layer, and a photoresist film formed on the silicon-containing hard mask film. The blank photomask may also have an etching mask film that functions as an etching mask during the processing of the absorber film. In addition, a back conductive film may also be provided on another main surface (back side) of the substrate. Furthermore, the blank photomask may also include a protective film.
[0039] FIG1 is a schematic cross-sectional view showing an example of the blank photomask (reflective blank photomask) of the present invention. The reflective blank photomask 101 comprises: a substrate 1; a multilayer reflective film layer 2 formed on the substrate 1 that reflects EUV light exposure light; a protective film 3 (any configuration in the present invention) formed on the multilayer reflective film layer 2 to protect the multilayer reflective film layer 2; an absorber layer (light absorption film) 4 formed on the protective film 3 to absorb exposure light; a first layer 5 (any configuration in the present invention) formed on the absorber layer 4 that functions as a hard mask when the absorber layer 4 is patterned by dry etching; a silicon-containing hard mask film 6 that functions as a second layer of hard mask film when the first layer 5 of the hard mask film is patterned by dry etching; and a photoresist film 7 formed on the silicon-containing hard mask film 6.
[0040] Hereinafter, each of the constituent components (necessary components and optional components) of the blank photomask of the present invention will be described in detail.
[0041] [Substrate] The substrate should preferably have low thermal expansion characteristics, for example, it should preferably be formed of a material with a coefficient of thermal expansion within ±2×10-8 / ℃. Examples of such materials include titanium dioxide-doped quartz glass (SiO2-TiO2 type glass). In addition, the surface roughness of the main surface of the substrate should preferably be 0.5 nm or less in terms of RMS value.
[0042] [Back conductive film] A conductive film (back conductive film) for electrostatically holding a reflective light shield to an exposure device (e.g., an EUV scanner) may also be provided on one main surface of the substrate and the other main surface (back side), which is the opposite side.
[0043] The back conductive film should preferably have a thin-film resistance of 100Ω / □ or less, and there are no particular restrictions on the material. Materials containing tantalum (Ta) or chromium (Cr) can be used as examples of back conductive film materials. Furthermore, materials containing oxygen (O) or nitrogen (N) can also be used. The thickness of the back conductive film is sufficient to perform its function for electrostatic clamping and is not particularly limited; it is typically about 20~300nm.
[0044] [Multilayer Reflective Film] The multilayer reflective film is a film that reflects EUV light, the exposure light, in a reflective mask. The multilayer reflective film system is, for example, a periodic stacked structure having a high refractive index layer with a relatively high refractive index for exposure light and a low refractive index layer with a relatively low refractive index for exposure light alternately stacked.
[0045] The high refractive index layer is preferably formed by a material containing silicon (Si), and the low refractive index layer is preferably formed by a material containing molybdenum (Mo). The thickness of the multilayer reflective film is preferably above 270 nm, and more preferably below 400 nm.
[0046] [Protective Film] Any protective film is also called a cover film. The protective film is used to protect multiple reflective layers. The protective film is preferably formed from materials containing ruthenium (Ru), and may also contain titanium (Ti), zirconium (Zr), niobium (Nb), etc. In addition, it may also contain oxygen (O), nitrogen (N), carbon (C), etc. The thickness of the protective film is not particularly limited, but it is preferably above 2 nm and below 5 nm.
[0047] [Absorber Layer] The absorber layer (light-absorbing film) can be any material that absorbs EUV light and can be patterned. There are no particular limitations on the material used as the absorber layer; for example, it is preferable to use a film containing tantalum (Ta), and it may also contain oxygen (O), nitrogen (N), boron (B), etc. There are no particular limitations on the thickness of the absorber layer, but it is preferable to be between 50 nm and 80 nm.
[0048] [First layer of hard mask film] The first layer of the hard mask film of any configuration in this invention is a layer that can function as an etching mask (hard mask) in etching as an absorber layer.
[0049] The first layer of the hard masking film is preferably a material that is resistant to fluorine-based dry etching of the absorber layer and can be removed by chlorine-based dry etching. The first layer of the hard masking film is preferably formed of a material containing chromium (Cr). In addition to chromium, it may contain one or more elements selected from oxygen (O), nitrogen (N), and carbon (C), and is more preferably a material composed of chromium and one or more elements selected from oxygen, nitrogen, and carbon. It is preferably containing nitrogen, and is particularly suitable for chromium nitride (CrN) composed of chromium and nitrogen. In addition, it is preferably containing nitrogen and oxygen, and is particularly suitable for chromium oxide nitride (CrNO) composed of chromium, nitrogen, and oxygen.
[0050] Furthermore, it may also contain nitrogen, oxygen, and carbon. In the case of carbon, it is suitable to be chromium nitride oxide carbide (CrNOC) composed of chromium, nitrogen, oxygen, and carbon. There is no particular limitation on the thickness of the etching mask film, but it is preferably above 5 nm and below 20 nm.
[0051] [Silicon-containing hard mask film (second layer of hard mask film)] The silicon-containing hard mask film (second layer of hard mask film) in this invention is, for example, a layer that can function as an etching mask (hard mask) in the etching of the first layer of hard mask film. In the case of using it as an etching mask in the etching of the first layer of hard mask film, the silicon-containing hard mask film (second layer of hard mask film) is preferably a material that has resistance to chlorine-based dry etching of the first layer of hard mask film and can be removed by fluorine-based dry etching. The silicon-containing hard mask film (second layer of hard mask film) is a hardened material containing silicon (Si), in other words, it is formed by a material containing silicon (Si). Materials containing silicon (Si) may contain one or more elements selected from oxygen (O), nitrogen (N) and carbon (C) in addition to silicon, and are preferably composed of silicon and one or more elements selected from oxygen, nitrogen and carbon.
[0052] In this invention, the silicon-containing hard masking film (the second layer of the hard masking film) is a cured product of a silicon-containing hard masking film forming composition cured at a temperature of 50°C to 180°C. In particular, it is preferable to coat a silicon-containing compound containing (A) a silicon-containing hard masking film forming composition having any one or more of the repeating units represented by the following general formula (Sx-1), repeating units represented by the following general formula (Sx-2), and substructures represented by the following general formula (Sx-3), and to bake the cured product (silicon oxide material film) at a temperature of 50°C to 150°C.
[0053] [Chemical 2] (In the formula, Ra, Rb and Rc are monovalent organic groups with 1 to 30 carbon atoms, which may be the same or different.)
[0054] In the case of a hardened product containing a silicon hard masking film that is cured at a temperature higher than 180°C, the reflectivity of the multilayer reflective film layer will decrease. On the other hand, in the case of a hardened product containing a silicon hard masking film that is cured at a temperature lower than 50°C, even if the product is stored in the environment in which it is used (e.g., a clean room: 23°C), some of it will harden and become a cause of defects.
[0055] The composition for forming a silicon-containing hard masking film (A) above should preferably contain polysiloxane (Sx) and solvent, and may further contain additives such as crosslinking catalysts and crosslinking agents.
[0056] The following describes in more detail the components that (A) may contain in the composition for forming a silicon-containing hard masking film.
[0057] (Polysiloxane (Sx)) Polysiloxane (Sx) is preferably one or more of the repeating unit represented by the following general formula (Sx-1), the repeating unit represented by the following general formula (Sx-2), and the substructure represented by the following general formula (Sx-3).
[0058] [Chemical 3] (In the formula, Ra, Rb, and Rc are monovalent organic groups with 1 to 30 carbon atoms, which may be the same or different.)
[0059] The above-mentioned polysiloxane (Sx) may be a thermally crosslinked polysiloxane (Sx).
[0060] The above-mentioned thermally crosslinked polysiloxane (Sx) can be manufactured by hydrolyzing and condensing the following hydrolyzable monomer (Sm).
[0061] As a hydrolyzable monomer (Sm), examples specifically include tetramethoxysilane, tetraethoxysilane, tetrapropoxysilane, tetraisopropoxysilane, trimethoxysilane, triethoxysilane, tripropoxysilane, triisopropoxysilane, methyltrimethoxysilane, methyltriethoxysilane, methyltripropoxysilane, methyltriisopropoxysilane, ethyl ...methoxysilane, methyltriethoxysilane, methyltripropoxysilane, methyltrimethoxysilane, methyltriethoxysilane, methyltripropoxysilane, methyltriethoxysilane, methyltripropoxysilane, methyltriethoxysilane, methyltripropoxysilane, ethyltriethoxysilane, methyltriethoxysilane, methyltripropoxysilane, methyltriethoxysilane, methyltriethoxysilane, methyltripropoxysilane, methyltriethoxysilane, methyltriethoxysilane, methyltriethoxysilane, methyltriethoxysilane, methyltriethoxysilane, methyltriethoxysilane, methyltriethoxysilane, methyltriethoxysilane, methyltriethoxysilane, methyltriethoxysilane, methyltriethoxysilane, methyltri Methoxysilane, ethyltriethoxysilane, ethyltripropoxysilane, ethyltriisopropoxysilane, vinyltrimethoxysilane, vinyltriethoxysilane, vinyltripropoxysilane, vinyltriisopropoxysilane, propyltrimethoxysilane, propyltriethoxysilane, propyltripropoxysilane, propyltriisopropoxysilane, isopropyltrimethoxysilane, isopropyl Triethoxysilane, isopropyltripropoxysilane, isopropyltriisopropoxysilane, butyltrimethoxysilane, butyltriethoxysilane, butyltripropoxysilane, butyltriisopropoxysilane, dibutyltrimethoxysilane, dibutyltriethoxysilane, dibutyltripropoxysilane, dibutyltriisopropoxysilane, dibutyltriisopropoxysilane, tert-butyltrimethoxysilane, dibutyl Triethoxysilane, tributyltripropoxysilane, tributyltriisopropoxysilane, cyclopropyltrimethoxysilane, cyclopropyltriethoxysilane, cyclopropyltripropoxysilane, cyclopropyltriisopropoxysilane, cyclobutyltrimethoxysilane, cyclobutyltriethoxysilane, cyclobutyltripropoxysilane, cyclobutyltriisopropoxysilane, cyclopentyltrimethoxysilane, cyclopentyl Triethoxysilane, cyclopentyltripropoxysilane, cyclopentyltriisopropoxysilane, cyclohexyltrimethoxysilane, cyclohexyltriethoxysilane, cyclohexyltripropoxysilane, cyclohexyltriisopropoxysilane, cyclohexenyltrimethoxysilane, cyclohexenyltriethoxysilane, cyclohexenyltripropoxysilane, cyclohexenyltriisopropoxysilane, cyclohexenylethyltrimethoxysilane Alkane, cyclohexenylethyltriethoxysilane, cyclohexenylethyltripropoxysilane, cyclohexenylethyltriisopropoxysilane, cyclooctyltrimethoxysilane, cyclooctyltriethoxysilane, cyclooctyltripropoxysilane, cyclooctyltriisopropoxysilane, cyclopentadienylpropyltrimethoxysilane, cyclopentadienylpropyltriethoxysilane, cyclopentadienylpropyltripropoxysilane, Cyclopentadienylpropyltriisopropoxysilane, dicycloheptenyltrimethoxysilane, dicycloheptenyltriethoxysilane, dicycloheptenyltripropoxysilane, dicycloheptenyltriisopropoxysilane, dicycloheptenyltrimethoxysilane, dicycloheptenyltriethoxysilane, dicycloheptenyltripropoxysilane, dicycloheptenyltriisopropoxysilane, adamantyltrimethoxysilane, adamantyltri Ethoxysilane, adamantyltripropoxysilane, adamantyltriisopropoxysilane, phenyltrimethoxysilane, phenyltriethoxysilane, phenyltripropoxysilane, phenyltriisopropoxysilane, benzyltrimethoxysilane, benzyltriethoxysilane, benzyltripropoxysilane, benzyltriisopropoxysilane, methoxyphenyltrimethoxysilane, methoxyphenyltriethoxysilane,Methoxyphenyl tripropoxysilane, methoxyphenyl triisopropoxysilane, tolyl trimethoxysilane, tolyl triethoxysilane, tolyl tripropoxysilane, tolyl triisopropoxysilane, phenylethyl trimethoxysilane, phenylethyl triethoxysilane, phenylethyl tripropoxysilane, phenylethyl triisopropoxysilane, naphthyl trimethoxysilane, naphthyl triethoxysilane, naphthalene Naphthyltriisopropoxysilane, dimethyldimethoxysilane, dimethyldiethoxysilane, methylethyldimethoxysilane, methylethyldiethoxysilane, dimethyldipropoxysilane, dimethyldiisopropoxysilane, diethyldimethoxysilane, diethyldiethoxysilane, diethyldipropoxysilane, diethyldiisopropoxysilane, diethyldimethoxysilane, diethyldiethoxysilane, diethyldipropoxysilane, diethyldiisopropoxysilane, dipropoxysilane Dipropyldimethoxysilane, dipropyldiethoxysilane, dipropyldipropoxysilane, dipropyldiisopropoxysilane, diisopropyldimethoxysilane, diisopropyldiethoxysilane, diisopropyldipropoxysilane, diisopropyldiisopropoxysilane, diisopropyldiisopropoxysilane, dibutyldimethoxysilane, dibutyldiethoxysilane, dibutyldipropoxysilane, dibutyldiisopropoxysilane Dibutyldimethoxysilane, Dibutyldiethoxysilane, Dibutyldipropoxysilane, Dibutyldiisopropoxysilane, Dibutyldimethoxysilane, Dibutyldiethoxysilane, Dibutyldipropoxysilane, Dibutyldiisopropoxysilane, Dicyclopropyldimethoxysilane, Dicyclopropyldiethoxysilane, Dicyclopropyldipropoxysilane Dicyclopropyl diisopropoxysilane, dicyclobutyl dimethoxysilane, dicyclobutyl diethoxysilane, dicyclobutyl dipropoxysilane, dicyclobutyl diisopropoxysilane, dicyclopentyl dimethoxysilane, dicyclopentyl diethoxysilane, dicyclopentyl dipropoxysilane, dicyclopentyl diisopropoxysilane, dicyclohexyl dimethoxysilane, dicyclohexyl Dicyclohexyldiethoxysilane, dicyclohexyldipropoxysilane, dicyclohexyldiisopropoxysilane, dicyclohexenyldimethoxysilane, dicyclohexenyldiethoxysilane, dicyclohexenyldipropoxysilane, dicyclohexenyldiisopropoxysilane, dicyclohexenylethyldimethoxysilane, dicyclohexenylethyldiethoxysilane, dicyclohexenylethyldipropoxysilane, dicyclohexenyldiethyldipropoxysilane, dicyclohexenyldiethoxysilane Hexenylethyl diisopropoxysilane, dicyclooctyl dimethoxysilane, dicyclooctyl diethoxysilane, dicyclooctyl dipropoxysilane, dicyclooctyl diisopropoxysilane, dicyclopentadienylpropyl dimethoxysilane, dicyclopentadienylpropyl diethoxysilane, dicyclopentadienylpropyl dipropoxysilane, dicyclopentadienylpropyl diisopropoxysilane, bis(dicycloheptyl) (Alkenyl)dimethoxysilane, bis(bicycloheptenyl)diethoxysilane, bis(bicycloheptenyl)dipropoxysilane, bis(bicycloheptenyl)diisopropoxysilane, bis(bicycloheptenyl)dimethoxysilane, bis(bicycloheptenyl)diethoxysilane, bis(bicycloheptenyl)dipropoxysilane, bis(bicycloheptenyl)diisopropoxysilane, diadamantyldimethoxysilane,Diadamyl diethoxysilane, diadamyl diethoxysilane, diadamyl dieisopropoxysilane, diphenyl dimethoxysilane, diphenyl diethoxysilane, methylphenyl dimethoxysilane, methylphenyl diethoxysilane, diphenyl dipropoxysilane, diphenyl diisopropoxysilane, trimethylmethoxysilane, trimethylethoxysilane, dimethyl ethyl methoxysilane, dimethyl ethyl ethoxysilane, dimethyl phenyl methoxysilane, dimethyl phenyl ethoxysilane, dimethyl benzyl methoxysilane, dimethyl benzyl ethoxysilane, dimethyl phenethyl methoxysilane, dimethyl phenethyl ethoxysilane, etc.
[0062] Preferably, the above-mentioned hydrolyzable monomer (Sm) includes tetramethoxysilane, tetraethoxysilane, methyltrimethoxysilane, methyltriethoxysilane, ethyltrimethoxysilane, ethyltriethoxysilane, vinyltrimethoxysilane, vinyltriethoxysilane, propyltrimethoxysilane, propyltriethoxysilane, isopropyltrimethoxysilane, isopropyltriethoxysilane, butyltrimethoxysilane, butyltriethoxysilane, isobutyltrimethoxysilane, isobutyltrimethoxysilane, allyltrimethoxysilane, allyltriethoxysilane, cyclopentyltrimethoxysilane, cyclopentyltriethoxysilane, cyclohexyltrimethoxysilane, cyclohexyltriethoxysilane, and cyclohexene. Trimethoxysilane, cyclohexenyltriethoxysilane, phenyltrimethoxysilane, phenyltriethoxysilane, benzyltrimethoxysilane, benzyltriethoxysilane, phenylethyltrimethoxysilane, phenylethyltriethoxysilane, dimethyldimethoxysilane, dimethyldiethoxysilane, diethyldimethoxysilane, diethyldiethoxysilane, diethyldimethoxysilane, diethyldiethoxysilane, methylethyldimethoxysilane, dimethylethyldiethoxysilane, dipropyldimethoxysilane, dibutyldimethoxysilane, methylphenyldimethoxysilane, methylphenyldiethoxysilane, trimethylmethoxysilane, dimethylethylmethoxysilane, dimethylphenylmethoxysilane, dimethylbenzylmethoxysilane, dimethylphenylethylmethoxysilane, etc.
[0063] Regarding other examples of the organic groups represented by Ra, Rb, and Rc in the compounds exemplified above, corresponding to hydrolyzable monomers (Sm), examples can be given of organic groups having one or more carbon-oxygen single bonds or carbon-oxygen double bonds. Specifically, these are organic groups having one or more groups selected from the group consisting of ether bonds, ester bonds, alkoxy groups, hydroxyl groups, etc. Examples can be given by the following general formula (Sm-R). By containing such organic groups, thermosetting properties can be improved, making it suitable for the blank photomask of the present invention. Furthermore, the adhesion to the upper photoresist film becomes good, and a highly rectangular photoresist pattern can be obtained after development.
[0064] [Chemical 4] (In the general formula (Sm-R), P represents hydrogen atoms, cyclic ether groups, hydroxyl groups, alkoxy groups with 1 to 4 carbon atoms, alkyl carbonyloxy groups with 1 to 6 carbon atoms, or alkyl carbonyl groups with 1 to 6 carbon atoms; Q1, Q2, Q3, and Q4 are each independently -CqH(2q-p)Pp- (where P is the same as above, p is an integer from 0 to 3, and q is an integer from 0 to 10 (however, q=0 indicates a single bond.)); u is an integer from 0 to 3; S1 and S2 are each independently represented by -O-, - CO-, -OCO-, -COO-, or -OCOO-. v1, v2, and v3 each independently represent 0 or 1. T is selected from the group consisting of divalent atoms other than carbon, alicyclic, aromatic, or heterocyclic groups. Examples of alicyclic, aromatic, or heterocyclic groups that may also contain heteroatoms such as oxygen atoms as T are shown below. The positions of T with Q2 and Q3 are not particularly limited and can be appropriately selected considering factors such as reactivity due to steric factors or the availability of commercially available reagents for the reaction.
[0065] [Chemical 5]
[0066] As a preferred example of an organic group having one or more carbon-oxygen single bonds or carbon-oxygen double bonds in the general formula (Sm-R), the following can be listed. In addition, in the following formula, (Si) is recorded to indicate the bonding site with Si.
[0067] [Chemical 6]
[0068] [Chemical 7]
[0069] Furthermore, as examples of organic groups for Ra, Rb, and Rc, organic groups containing silicon-silicon bonds may also be used. Specifically, the following can be listed.
[0070] [Chemical 8]
[0071] Furthermore, as examples of organogroups of Ra, Rb, and Rc, organogroups having a protecting group that decomposes by acid may also be used. Specifically, organogroups listed in paragraphs
[0043] to
[0048] of Japanese Patent Application Publication No. 2013-167669 and organogroups obtained from silicon compounds shown in paragraph
[0056] of Japanese Patent Application Publication No. 2013-224279 can be cited.
[0072] In addition, as examples of organic groups of Ra, Rb, and Rc, organic groups having fluorine atoms may also be used. Specifically, organic groups obtained from silicon compounds shown in paragraphs
[0059] to
[0065] of Japanese Patent Application Publication No. 2012-53253 can be cited.
[0073] The above-mentioned hydrolyzable monomer (Sm) system has one, two or three chlorine, bromine, iodine, acetoxy, methoxy, ethoxy, propoxy or butoxy groups bonded as hydrolyzable groups on silicon represented by (Si) in the above substructure.
[0074] [Synthesis method of thermocrosslinkable polysiloxane (Sx)] (Synthesis method 1: Method using acid catalyst) The thermocrosslinkable polysiloxane (Sx) used in this invention can be manufactured, for example, by hydrolyzing and condensing one hydrolyzable monomer (Sm) or a mixture of two or more hydrolyzable monomers (Sm) in the presence of an acid catalyst.
[0075] The acid catalysts used at this time can include organic acids such as formic acid, acetic acid, oxalic acid, maleic acid, methanesulfonic acid, benzenesulfonic acid, and toluenesulfonic acid, as well as inorganic acids such as hydrofluoric acid, hydrochloric acid, hydrobromic acid, sulfuric acid, nitric acid, perchloric acid, and phosphoric acid. The amount of catalyst used is 1×10⁻⁶ to 10 mol relative to 1 mol of monomer, preferably 1×10⁻⁵ to 5 mol, and more preferably 1×10⁻⁴ to 1 mol.
[0076] The amount of water used to obtain thermally crosslinked polysiloxanes (Sx) from these monomers via hydrolysis-condensation is preferably 0.01 to 100 mol, more preferably 0.05 to 50 mol, and even more preferably 0.1 to 30 mol, relative to 1 mol of the hydrolytic substituents bonded to the monomers. As long as it is below 100 mol, the equipment used in the reaction becomes smaller and more economical.
[0077] As one example of the operating method, the hydrolysis-condensation reaction can be initiated by adding a monomer to an aqueous catalyst solution. At this time, an organic solvent can be added to the aqueous catalyst solution, the monomer can be diluted with an organic solvent, or both can be performed. The reaction temperature is 0~100℃, preferably 5~50℃. It is preferable to maintain the temperature at 5~50℃ during the dropwise addition of the monomer, and then allow it to mature at 20~50℃.
[0078] The organic solvent that can be added to the catalyst aqueous solution or that can dilute the monomer is preferably methanol, ethanol, 1-propanol, 2-propanol, 1-butanol, 2-butanol, 2-methyl-1-propanol, acetone, acetonitrile, tetrahydrofuran, toluene, hexane, ethyl acetate, methyl ethyl ketone, methyl isobutyl ketone, cyclohexanone, methyl pentyl ketone, butanediol monomethyl ether, propylene glycol monomethyl ether, ethylene glycol monomethyl ether, butanediol monoethyl ether, propylene glycol monoethyl ether, ethylene glycol monoethyl ether, propylene glycol dimethyl ether, diethylene glycol dimethyl ether, propylene glycol monomethyl ether acetate, propylene glycol monoethyl ether acetate, ethyl pyruvate, butyl acetate, methyl 3-methoxypropionate, ethyl 3-ethoxypropionate, tributyl acetate, tributyl propionate, propylene glycol monobutyl ether acetate, γ-butyrolactone, and mixtures thereof.
[0079] Among these solvents, water-soluble solvents are preferred. Examples include alcohols such as methanol, ethanol, 1-propanol, and 2-propanol; polyols such as ethylene glycol and propylene glycol; polyol condensate derivatives such as butanediol monomethyl ether, propylene glycol monomethyl ether, ethylene glycol monomethyl ether, butanediol monoethyl ether, propylene glycol monoethyl ether, ethylene glycol monoethyl ether, butanediol monopropyl ether, propylene glycol monopropyl ether, and ethylene glycol monopropyl ether; acetone, acetonitrile, and tetrahydrofuran. Among these, solvents with a boiling point below 100°C are particularly preferred.
[0080] Furthermore, the amount of organic solvent used is 0 to 1,000 ml relative to 1 mole of monomer, and preferably 0 to 500 ml. If less organic solvent is used, the reaction vessel becomes smaller and more economical.
[0081] Subsequently, a catalytic neutralization reaction is carried out as needed to obtain an aqueous solution of the reaction mixture. At this time, the amount of alkaline substance that can be used for neutralization is preferably 0.1 to 2 equivalents relative to the acid used in the catalyst. The alkaline substance can be any substance that exhibits alkalinity in water.
[0082] Then, byproducts such as alcohols produced in the hydrolysis-condensation reaction should be removed from the reaction mixture by means of depressurization. The temperature at which the reaction mixture is heated depends on the type of organic solvent added and the type of alcohols produced in the reaction, and is preferably 0-100°C, more preferably 10-90°C, and even more preferably 15-50°C. Furthermore, the depressurization should vary depending on the type of organic solvent and alcohols to be removed, the venting device, the condensation device, and the heating temperature, and should preferably be below atmospheric pressure, more preferably below 80 kPa absolute pressure, and even more preferably below 50 kPa absolute pressure. Although it is difficult to know the exact amount of alcohol removed at this time, it is desirable to remove approximately 80% by mass or more of the alcohols produced.
[0083] Then, the acid catalyst used in the hydrolysis and condensation can also be removed from the reaction mixture. As a method for removing the acid catalyst, water is mixed with a solution of thermally crosslinked polysiloxane, and the thermally crosslinked polysiloxane is extracted with an organic solvent. The organic solvent used at this time should preferably be one that can dissolve the thermally crosslinked polysiloxane and separate into two layers when mixed with water. Examples include methanol, ethanol, 1-propanol, 2-propanol, 1-butanol, 2-butanol, 2-methyl-1-propanol, acetone, tetrahydrofuran, toluene, hexane, ethyl acetate, cyclohexanone, methylpentyl ketone, butanediol monomethyl ether, propylene glycol monomethyl ether, ethylene glycol monomethyl ether, butanediol monoethyl ether, propylene glycol monoethyl ether, ethylene glycol monoethyl ether, butanediol monopropyl ether, propylene glycol monopropyl ether, ethylene glycol monopropyl ether, propylene glycol dimethyl ether, diethylene glycol dimethyl ether, propylene glycol monomethyl ether acetate, propylene glycol monoethyl ether acetate, ethyl pyruvate, butyl acetate, methyl 3-methoxypropionate, ethyl 3-ethoxypropionate, tributyl acetate, tributyl propionate, propylene glycol tributyl ether acetate, γ-butyrolactone, methyl isobutyl ketone, cyclopentyl methyl ether, and mixtures thereof.
[0084] Further, a mixture of a water-soluble organic solvent and a water-poorly soluble organic solvent may also be used. For example, a mixture of methanol and ethyl acetate, ethanol and ethyl acetate, 1-propanol and ethyl acetate, 2-propanol and ethyl acetate, butanediol monomethyl ether and ethyl acetate, propylene glycol monomethyl ether and ethyl acetate, ethylene glycol monomethyl ether and ethyl acetate, butanediol monoethyl ether and ethyl acetate, propylene glycol monoethyl ether and ethyl acetate, ethylene glycol monoethyl ether and ethyl acetate, butanediol monopropyl ether and ethyl acetate, propylene glycol monopropyl ether and ethyl acetate, etc., are also suitable. Mixtures of ethylene glycol monopropyl ether and ethyl acetate, methanol and methyl isobutyl ketone, ethanol and methyl isobutyl ketone, 1-propanol and methyl isobutyl ketone, 2-propanol and methyl isobutyl ketone, propylene glycol monomethyl ether and methyl isobutyl ketone, ethylene glycol monomethyl ether and methyl isobutyl ketone, propylene glycol monoethyl ether and methyl isobutyl ketone, ethylene glycol monoethyl ether and methyl isobutyl ketone, propylene glycol monopropyl ether and methyl isobutyl ketone, methanol and ethyl acetate. Mixtures of cyclopentyl methyl ethers, ethanol-cyclopentyl methyl ethers, 1-propanol-cyclopentyl methyl ethers, 2-propanol-cyclopentyl methyl ethers, propylene glycol monomethyl ether-cyclopentyl methyl ethers, ethylene glycol monomethyl ether-cyclopentyl methyl ethers, propylene glycol monoethyl ether-cyclopentyl methyl ethers, ethylene glycol monoethyl ether-cyclopentyl methyl ethers, propylene glycol monopropyl ether-cyclopentyl methyl ethers, ethylene glycol monopropyl ether-cyclopentyl methyl ethers, methanol-propylene glycol methyl ether acetate mixtures, ethanol-propylene glycol Mixtures of methyl ether acetates, mixtures of 1-propanol-propylene glycol methyl ether acetates, mixtures of 2-propanol-propylene glycol methyl ether acetates, mixtures of propylene glycol monomethyl ether-propylene glycol methyl ether acetates, mixtures of ethylene glycol monomethyl ether-propylene glycol methyl ether acetates, mixtures of propylene glycol monoethyl ether-propylene glycol methyl ether acetates, mixtures of ethylene glycol monoethyl ether-propylene glycol methyl ether acetates, mixtures of propylene glycol monopropyl ether-propylene glycol methyl ether acetates, mixtures of ethylene glycol monopropyl ether-propylene glycol methyl ether acetates, etc., are not limited to these combinations.
[0085] Furthermore, the mixing ratio of the water-soluble organic solvent and the water-poorly soluble organic solvent is appropriately selected, with the water-soluble organic solvent being 0.1 to 1,000 parts by mass relative to 100 parts by mass of the water-poorly soluble organic solvent, preferably 1 to 500 parts by mass, and more preferably 2 to 100 parts by mass.
[0086] Then, cleaning can also be performed using neutral water. Deionized water or ultrapure water is generally acceptable. The amount of water, relative to 1L of the thermally crosslinked polysiloxane solution, is preferably 0.01~100L, more preferably 0.05~50L, and even more preferably 0.1~5L. The cleaning method involves adding both solutions to the same container, stirring and mixing, allowing it to stand, and then separating the water layers. Cleaning once or more is sufficient; however, cleaning more than 10 times may not necessarily achieve the desired cleaning effect, so approximately 1~5 times is preferable.
[0087] Other methods for removing acid catalysts include methods using ion exchange resins or methods that involve immediate removal after neutralization with epoxy compounds such as ethylene oxide and propylene oxide. These methods can be appropriately selected in conjunction with the acid catalyst used in the reaction.
[0088] Sometimes, due to the water washing operation at this time, a portion of the thermally crosslinked polysiloxane escapes into the water layer, achieving an effect substantially equivalent to the separation operation. Therefore, the number of water washes or the amount of washing water should be appropriately selected based on the catalyst removal effect and the separation effect.
[0089] Either a thermally crosslinked polysiloxane solution containing residual acid catalyst or a thermally crosslinked polysiloxane solution after the acid catalyst has been removed, a final solvent is added, and solvent exchange is performed under reduced pressure to obtain the desired thermally crosslinked polysiloxane solution. The solvent exchange temperature at this time depends on the type of reaction solvent and extraction solvent to be removed, and is preferably 0~100°C, more preferably 10~90°C, and even more preferably 15~50°C. In addition, the reduced pressure at this time varies depending on the type of extraction solvent to be removed, the exhaust device, the condenser, and the heating temperature, and is preferably below atmospheric pressure, more preferably below 80 kPa absolute pressure, and even more preferably below 50 kPa absolute pressure.
[0090] At this time, sometimes the thermally crosslinked polysiloxane becomes unstable due to a change in solvent. This can occur due to the compatibility between the final solvent and the thermally crosslinked polysiloxane. To prevent this, a mono- or di-ortho-ol having a cyclic ether as a substituent, as described in Japanese Patent Application Publication No. 2009-126940
[0181] to
[0182] , can be added as a stabilizer. The amount added is 0 to 25 parts by mass relative to 100 parts by mass of the thermally crosslinked polysiloxane in the solution before solvent exchange, preferably 0 to 15 parts by mass, more preferably 0 to 5 parts by mass, and preferably 0.5 parts by mass or more in the case of addition. If necessary, a mono- or di-ortho-ol having a cyclic ether as a substituent can be added to the solution before solvent exchange and a solvent exchange operation can be performed.
[0091] If thermally crosslinked polysiloxanes are concentrated to a certain concentration or higher, they may undergo further condensation reactions, potentially changing into a state where they are no longer soluble in organic solvents. Therefore, it is advisable to obtain a solution of appropriate concentration. Furthermore, if the solution is too dilute, the amount of solvent becomes excessive, so obtaining a solution of appropriate concentration is more economical. The appropriate concentration at this point is preferably 0.1 to 20% by mass.
[0092] Preferably, the final solvent added to the thermally crosslinked polysiloxane solution is an alcohol-based solvent, particularly ideally a monoalkyl ether derivative of ethylene glycol, diethylene glycol, triethylene glycol, propylene glycol, dipropylene glycol, butanediol, etc. Specifically, butanediol monomethyl ether, propylene glycol monomethyl ether, ethylene glycol monomethyl ether, butanediol monoethyl ether, propylene glycol monoethyl ether, ethylene glycol monoethyl ether, butanediol monopropyl ether, propylene glycol monopropyl ether, ethylene glycol monopropyl ether, diacetone alcohol, etc., are preferred.
[0093] As long as these solvents are the main components, non-alcoholic solvents may also be added as auxiliary solvents. Examples of such auxiliary solvents include acetone, tetrahydrofuran, toluene, hexane, ethyl acetate, cyclohexanone, methylpentyl ketone, propylene glycol dimethyl ether, diethylene glycol dimethyl ether, propylene glycol monomethyl ether acetate, propylene glycol monoethyl ether acetate, ethyl pyruvate, butyl acetate, methyl 3-methoxypropionate, ethyl 3-ethoxypropionate, tert-butyl acetate, tert-butyl propionate, propylene glycol monobutyl ether acetate, γ-butyrolactone, methyl isobutyl ketone, cyclopentyl methyl ether, etc.
[0094] In addition, as another reaction operation using an acid catalyst, water or an aqueous organic solvent can be added to the monomer or the monomer's organic solvent to initiate the hydrolysis reaction. In this case, the catalyst can be added to the monomer or the monomer's organic solvent, or to water or an aqueous organic solvent. The reaction temperature is 0~100°C, preferably 10~50°C. It is preferable to heat to 10~50°C during the dropwise addition of water, and then raise the temperature to 20~50°C to allow it to mature.
[0095] When using organic solvents, water-soluble solvents are preferred, such as methanol, ethanol, 1-propanol, 2-propanol, 1-butanol, 2-butanol, 2-methyl-1-propanol, acetone, tetrahydrofuran, acetonitrile, butanediol monomethyl ether, propylene glycol monomethyl ether, ethylene glycol monomethyl ether, butanediol monoethyl ether, propylene glycol monoethyl ether, ethylene glycol monoethyl ether, butanediol monopropyl ether, propylene glycol monopropyl ether, ethylene glycol monopropyl ether, propylene glycol dimethyl ether, diethylene glycol dimethyl ether, propylene glycol monomethyl ether acetate, propylene glycol monoethyl ether acetate, propylene glycol monopropyl ether, etc., as well as mixtures thereof.
[0096] The amount of organic solvent used is 0 to 1,000 ml relative to 1 mole of monomer, and preferably 0 to 500 ml. Using less organic solvent results in a smaller reaction vessel, which is more economical. The obtained reaction mixture can be post-processed in the same manner as described above to obtain a thermally crosslinked polysiloxane.
[0097] (Synthesis Method 2: Method using an alkaline catalyst) In addition, thermally crosslinked polysiloxane (Sx) systems can also be manufactured by hydrolyzing and condensing one or more hydrolyzable monomers (Sm) in the presence of an alkaline catalyst.
[0098] The alkaline catalyst system used at this time includes, for example, methylamine, ethylamine, propylamine, butylamine, ethylenediamine, hexamethylenediamine, dimethylamine, diethylamine, ethylmethylamine, trimethylamine, triethylamine, tripropylamine, tributylamine, cyclohexylamine, dicyclohexylamine, monoethanolamine, diethanolamine, dimethylmonoethanolamine, monomethyldiethanolamine, triethanolamine, diazabicyclooctane, diazabicyclononene, diazabicycloundecene, hexamethylenetetramine, aniline, N,N-dimethylaniline, pyridine, N,N-dimethylaminopyridine, pyrrole, piperidine, pyrrolidine, piperidine, methylpyridine, tetramethylammonium hydroxide, choline hydroxide, tetrapropylammonium hydroxide, tetrabutylammonium hydroxide, ammonia, lithium hydroxide, sodium hydroxide, potassium hydroxide, barium hydroxide, calcium hydroxide, etc. The amount of catalyst used is 1×10⁻⁶ mol to 10 mol relative to 1 mol of silicon monomer, preferably 1×10⁻⁵ mol to 5 mol, and even more preferably 1×10⁻⁴ mol to 1 mol.
[0099] When obtaining thermally crosslinked polysiloxanes from the above monomers via hydrolysis-condensation, the amount of water should preferably be 0.1 to 50 mol per mol of hydrolyzable substituents bonded to the monomers. As long as it is 50 mol or less, the equipment used in the reaction becomes smaller and more economical.
[0100] As one example of the operating method, the addition of a monomer to an aqueous catalyst solution can be used to initiate the hydrolysis-condensation reaction. At this time, an organic solvent can be added to the aqueous catalyst solution, or the monomer can be diluted with an organic solvent, or both can be performed. The reaction temperature is 0~100℃, preferably 5~50℃. It is preferable to maintain the temperature at 5~50℃ during the dropwise addition of the monomer, and then allow it to mature at 20~50℃.
[0101] As an organic solvent that can be added to an aqueous solution of an alkaline catalyst or that can dilute the monomer, it is suitable to use the same organic solvent as that exemplified as that that can be added to an aqueous solution of an acidic catalyst. Furthermore, the amount of organic solvent used is preferably 0 to 1,000 ml relative to 1 mol of monomer for the purpose of carrying out the reaction more economically.
[0102] Subsequently, if necessary, a catalytic neutralization reaction is carried out to obtain an aqueous solution of the reaction mixture. At this time, the amount of acidic substance that can be used in the neutralization is preferably 0.1 to 2 equivalents relative to the alkaline substance used in the catalyst. The acidic substance can be any substance that exhibits acidity in water.
[0103] Then, byproducts such as alcohols generated in the hydrolysis-condensation reaction should be removed from the reaction mixture by means of depressurization. The temperature at which the reaction mixture is heated depends on the type of organic solvent added and the type of alcohol produced in the reaction, and is preferably 0 to 100°C, more preferably 10 to 90°C, and even more preferably 15 to 50°C. Furthermore, the depressurization at this time will vary depending on the type of organic solvent and alcohol to be removed, the exhaust device, the condensation device, and the heating temperature, and is preferably below atmospheric pressure, more preferably below 80 kPa absolute pressure, and even more preferably below 50 kPa absolute pressure. The amount of alcohol removed at this time is difficult to know accurately, but it is desirable to remove about 80% by mass or more of the alcohol produced.
[0104] Then, in order to remove the alkaline catalyst used in the hydrolysis condensation, the thermally crosslinked polysiloxane is extracted with an organic solvent. The organic solvent used at this time should preferably be able to dissolve the thermally crosslinked polysiloxane and separate into two layers if mixed with water. Examples include methanol, ethanol, 1-propanol, 2-propanol, 1-butanol, 2-butanol, 2-methyl-1-propanol, acetone, tetrahydrofuran, toluene, hexane, ethyl acetate, cyclohexanone, methylpentyl ketone, propylene glycol monomethyl ether, ethylene glycol monomethyl ether, propylene glycol monoethyl ether, ethylene glycol monoethyl ether, propylene glycol monopropyl ether, ethylene glycol monopropyl ether, propylene glycol dimethyl ether, diethylene glycol dimethyl ether, propylene glycol monomethyl ether acetate, propylene glycol monoethyl ether acetate, ethyl pyruvate, butyl acetate, methyl 3-methoxypropionate, ethyl 3-ethoxypropionate, tert-butyl acetate, tert-butyl propionate, propylene glycol monobutyl ether acetate, γ-butyrolactone, methyl isobutyl ketone, cyclopentyl methyl ether, and mixtures thereof.
[0105] Furthermore, a mixture of water-soluble organic solvent and water-insoluble organic solvent may also be used.
[0106] Specific examples of the organic solvent used when removing alkaline catalysts may be the same as the organic solvent specifically exemplified by the user when removing acid catalysts, or a mixture of water-soluble organic solvent and water-difficult organic solvent.
[0107] In addition, the mixing ratio of water-soluble organic solvent and water-insoluble organic solvent is appropriately selected. The ratio of water-soluble organic solvent to 100 parts by mass of water-soluble organic solvent is 0.1 to 1,000 parts by mass, preferably 1 to 500 parts by mass, and more preferably 2 to 100 parts by mass.
[0108] Then, rinse with neutral water. Deionized water or ultrapure water is generally acceptable. The amount of water is 0.01 to 100 L relative to 1 L of the thermally crosslinked polysiloxane solution, preferably 0.05 to 50 L, and more preferably 0.1 to 5 L. The rinsing method involves adding both solutions to the same container, stirring to mix, and then allowing the mixture to stand to separate the water layers. One or more rinses are sufficient; even if rinsed more than 10 times, the cleaning effect may not be achieved, so approximately 1 to 5 rinses are preferable.
[0109] A final solvent is added to the cleaned thermally crosslinked polysiloxane solution, and the desired thermally crosslinked polysiloxane solution is obtained by solvent exchange under reduced pressure. The solvent exchange temperature depends on the type of extraction solvent to be removed, and is preferably 0~100°C, more preferably 10~90°C, and even more preferably 15~50°C. Furthermore, the reduced pressure varies depending on the type of extraction solvent to be removed, the exhaust device, the condenser, and the heating temperature, and is preferably below atmospheric pressure, more preferably below 80 kPa absolute pressure, and even more preferably below 50 kPa absolute pressure.
[0110] Preferably, the final solvent added to the thermally crosslinked polysiloxane solution is an alcohol-based solvent, and particularly preferably an alkyl ether of ethylene glycol, diethylene glycol, triethylene glycol, propylene glycol, dipropylene glycol, etc. Specifically, preferably propylene glycol monomethyl ether, ethylene glycol monomethyl ether, propylene glycol monoethyl ether, ethylene glycol monoethyl ether, propylene glycol monopropyl ether, ethylene glycol monopropyl ether, diacetone alcohol, etc.
[0111] In addition, as another reaction operation using an alkaline catalyst, water or an aqueous organic solvent can be added to the monomer or an organic solution of the monomer to initiate the hydrolysis reaction. At this time, the catalyst can be added to the monomer or the organic solution of the monomer, or to water or an aqueous organic solvent. The reaction temperature is 0~100°C, preferably 10~50°C. It is preferable to heat to 10~50°C during the dropwise addition of water, and then raise the temperature to 20~50°C to allow it to mature.
[0112] As for organic solvents that can be used as monomeric organic solutions or aqueous organic solvents, those that are preferably water-soluble include methanol, ethanol, 1-propanol, 2-propanol, 1-butanol, 2-butanol, 2-methyl-1-propanol, acetone, tetrahydrofuran, acetonitrile, propylene glycol monomethyl ether, ethylene glycol monomethyl ether, propylene glycol monoethyl ether, ethylene glycol monoethyl ether, propylene glycol monopropyl ether, ethylene glycol monopropyl ether, propylene glycol dimethyl ether, diethylene glycol dimethyl ether, propylene glycol monomethyl ether acetate, propylene glycol monoethyl ether acetate, propylene glycol monopropyl ether, and polyol condensate derivatives thereof, as well as mixtures thereof.
[0113] The molecular weight of the thermally crosslinked polysiloxane obtained by the above synthesis method 1 or 2 can be adjusted not only by the selection of monomers but also by controlling the reaction conditions during polymerization. It is preferable to use monomers with a weight average molecular weight of 100,000 or less, more preferably 200 to 50,000, and even more preferably 300 to 30,000. As long as the weight average molecular weight is 100,000 or less, there will be no foreign matter or coating spots. Furthermore, the above-mentioned weight average molecular weight data is expressed by gel permeation chromatography (GPC) using RI as a detector, tetrahydrofuran as a dissolution solvent, and polystyrene as a standard, and by converting the molecular weight to polystyrene.
[0114] (Crosslinking catalyst) In the composition for forming a silicon-containing hard masking film, one or more crosslinking catalysts may be further incorporated. Examples of crosslinking catalysts that can be incorporated include compounds represented by the following general formula (Xc0). By containing such a crosslinking catalyst, thermosetting properties can be further improved. LaHbA (Xc0) (where L is lithium, sodium, potassium, rubidium, cesium, strontium, zinc, phosphorus, or ammonium. A is a non-nucleophilic relative ion. a is an integer of 1 or more, b is an integer of 0 or more, and a+b is the valence of the non-nucleophilic relative ion.)
[0115] As for specific compounds represented by general formula (Xc0) used as crosslinking catalysts in the present invention, examples include strontium salts of general formula (Xc-1), ferrous salts of general formula (Xc-2), phosphonium salts of general formula (Xc-3), ammonium salts of general formula (Xc-4), alkali metal salts, etc., or polysiloxanes (Xc-10) having ammonium salts, strontium salts, phosphonium salts, or ferrous salts as part of their structure. Specifically, materials described in paragraphs
[0124] to
[0163] of Japanese Patent Application Publication No. 2020-118960 may be added.
[0116] [Chemical 9]
[0117] [Chemical 10](In the formula, R204, R205, R206, and R207 each independently represent a straight-chain, branched, or cyclic alkyl, alkenyl, alkyl oxyalkyl or alkyl oxyalkenyl group having 1 to 12 carbon atoms, a substituted or unsubstituted aryl group having 6 to 20 carbon atoms, or an aralkyl or aryl oxyalkyl group having 7 to 12 carbon atoms. Some or all of the hydrogen atoms of these groups may also be substituted by alkoxy groups, etc. In addition, R205 and R206 may also form a ring. In the case of ring formation...) R205 and R206 represent alkyl groups having 1 to 6 carbon atoms, respectively. A- indicates a non-nucleophilic relative ion. R208, R209, R210, and R211 are the same as R204, R205, R206, and R207, and can also be hydrogen atoms. R208 and R209, or R208, R209, and R210 can also form rings. In the case of ring formation, R208 and R209, or R208, R209, and R210, represent alkyl groups having 3 to 10 carbon atoms.
[0118] The above-mentioned crosslinking catalysts (Xc-1), (Xc-2), (Xc-3), (Xc-4), and / or (Xc-10) can be used alone or in combination of two or more. The amount of crosslinking catalyst added is preferably 0.01 to 50 parts by weight, more preferably 0.1 to 40 parts by weight, relative to 100 parts by weight of the base polymer (e.g., the thermally crosslinked polysiloxane (Sx) obtained by the above method).
[0119] [Other raw materials] The following raw materials may also be incorporated into the silicon-containing hard mask film forming composition used in this invention.
[0120] (Acid Generator) The composition for forming a silicon hard masking film may also be further incorporated with one or more acid generators. As an acid generator, any substance that functions as an acid precursor, such as a thermal acid generator, a photoacid generator, or an acid propagator, may be used. In this invention, it is more preferable that the incorporated acid generator be a strontium salt, or a photoacid generator that generates acid through the action of high-energy rays. Specifically, the materials described in paragraphs
[0061] to
[0085] of Japanese Patent Application Publication No. 2007-199653 may be added, but are not limited to these.
[0121] The above-mentioned acid generating agent can be used alone or in combination of two or more. When an acid generating agent is added, the amount added is preferably 0.05 to 50 parts, more preferably 0.1 to 10 parts, relative to 100 parts of thermally crosslinked polysiloxane.
[0122] (Crosslinking agent) For compositions containing silicon hard masking films, a crosslinking agent may be added to further improve thermosetting properties. There are no particular limitations on the crosslinking agent; various known crosslinking agents of different systems can be widely used. Examples include melamine-based crosslinking agents, acetylenide-based crosslinking agents, benzoguanamine-based crosslinking agents, urea-based crosslinking agents, β-hydroxyalkylamide-based crosslinking agents, isocyanurate-based crosslinking agents, aziridine-based crosslinking agents, acezoline-based crosslinking agents, epoxy-based crosslinking agents, and phenol-based crosslinking agents. One or more of the above crosslinking agents may be used alone or in combination. The amount of crosslinking agent added is preferably 5 to 50 parts, more preferably 10 to 40 parts, and even more preferably 10 to 30 parts, relative to 100 parts of the above-mentioned composition containing silicon hard masking films.
[0123] (Organic Acid) To improve the stability of the composition used in forming silicon-containing hard masking films, it is advisable to add an organic acid with 1 to 30 carbon atoms, either monovalent or divalent or higher. Examples of acids added at this time include formic acid, acetic acid, propionic acid, butyric acid, valeric acid, hexanoic acid, heptanoic acid, octanoic acid, nonanoic acid, decanoic acid, oleic acid, stearic acid, linoleic acid, perilla oleic acid, benzoic acid, phthalic acid, isophthalic acid, terephthalic acid, salicylic acid, trifluoroacetic acid, monochloroacetic acid, dichloroacetic acid, trichloroacetic acid, oxalic acid, malonic acid, methylmalonic acid, ethylmalonic acid, propylmalonic acid, butylmalonic acid, dimethylmalonic acid, diethylmalonic acid, succinic acid, methylsuccinic acid, glutaric acid, adipic acid, iconic acid, maleic acid, fumaric acid, citrate, citric acid, etc. Oxalic acid, maleic acid, formic acid, acetic acid, propionic acid, citric acid, etc. are particularly suitable. In addition, to maintain stability, two or more acids can be mixed for use.
[0124] The amount of organic acid added is 0.001 to 25 parts by weight relative to 100 parts by weight of thermally crosslinked polysiloxane contained in the composition for forming silicon hard mask film, preferably 0.01 to 15 parts by weight, and more preferably 0.1 to 5 parts by weight.
[0125] Alternatively, the above organic acid can be converted into the pH of the component for forming a silicon hard masking film, and can be mixed in such a way that it is preferably 0≦pH≦7, more preferably 0.3≦pH≦6.5, and even more preferably 0.5≦pH≦6.
[0126] (Solvent) The composition for forming a silicon hard mask film may contain a coating solvent to improve coatability.
[0127] The solvent used as a coating solvent for the composition used in forming the silicon-containing hard mask film should preferably be an organic solvent used directly in the manufacture of the aforementioned silicon-containing compound, and in particular, an alkyl ether of ethylene glycol, diethylene glycol, triethylene glycol, propylene glycol, dipropylene glycol, etc. Specifically, it should preferably be an organic solvent selected from propylene glycol monomethyl ether, ethylene glycol monomethyl ether, propylene glycol monoethyl ether, ethylene glycol monoethyl ether, propylene glycol monopropyl ether, and ethylene glycol monopropyl ether, and may be further diluted as needed.
[0128] Furthermore, in addition to the above-mentioned solvent, a known stabilizing solvent such as water may also be added. In a blank photomask of 152 mm (6 inches) square, in order to form a silicon oxide material layer with a film thickness of 1 to 10 nm, the total amount of solvent including water used is preferably 1,000 to 250,000 parts by weight relative to 100 parts by weight of thermally crosslinked polysiloxane, and is particularly suitable to be 10,000 to 200,000 parts by weight.
[0129] (Stabilizer) In addition, a stabilizer can be added to the composition for forming a silicon-containing hard masking film. An alcohol of one or more nucleotides having a cyclic ether as a substituent can be added as a stabilizer. In particular, if the stabilizer described in paragraphs
[0181] to
[0182] of Japanese Patent Application Publication No. 2009-126940 is added, the stability of the composition for forming a silicon-containing hard masking film can be improved.
[0130] The amount of stabilizer used is preferably 0 to 25 parts by weight relative to 100 parts by weight of the thermally crosslinked polysiloxane (Sx) of the base polymer, especially preferably 0 to 5 parts by weight, and preferably more than 0.5 parts by weight when added.
[0131] (Surfactant) In addition, surfactants may be incorporated into the composition as needed. Specifically, the material described in paragraph
[0185] of Japanese Patent Application Publication No. 2009-126940 may be added.
[0132] The amount of surfactant used is preferably 0 to 10 parts by weight relative to 100 parts by weight of the thermally crosslinked polysiloxane (Sx) of the base polymer, and more preferably 0 to 5 parts by weight.
[0133] [Photoresist Film] The photoresist film is formed on a silicon-containing hard mask film. The type of resist used depends on the pattern exposure method. To form fine patterns as with the blank photomask of this invention, a conventional electron beam exposure method is used; therefore, a chemically amplified electron beam resist using an aromatic resin is generally used. This resist is used in positive and negative forms depending on the type of pattern. The resist film is patterned by an electron beam, and the resist undergoes a predetermined post-irradiation heating and development step to obtain the resist pattern.
[0134] As long as the blank photomask of the present invention described above contains a silicon-containing hard mask film which is useful as a hard mask film, it can transfer fine resist patterns to the absorber layer with high precision. Furthermore, the silicon-containing hard mask film can be formed in a temperature range of 50°C to 180°C, thus preventing interlayer mixing of multiple reflective film layers and improving the transfer accuracy of the resist pattern. In other words, by using the blank photomask of the present invention, a photomask containing an absorber layer with fine patterns formed with high precision can be provided without degrading the reflectivity of EUV light. That is, the blank photomask of the present invention is a blank photomask containing a silicon-containing hard mask film that functions as a hard mask when the absorber layer is processed by dry etching, and also contributes to improving the resolution of the resist pattern.
[0135] <Method for Manufacturing Blank Photomask> The method for manufacturing blank photomask of the present invention includes the following steps: preparing a substrate; forming a multilayer reflective film layer that reflects EUV light on the substrate; forming an absorber layer that absorbs EUV light on the multilayer reflective film layer; directly or indirectly coating the absorber layer with a silicon-containing hard mask film forming composition that is cured at a temperature of 50°C to 180°C to obtain a coating film; curing the coating film at a temperature of 50°C to 180°C to form a silicon-containing hard mask film; and forming a photoresist film on the silicon-containing hard mask film.
[0136] The multilayer reflective film, any protective film, absorber layer, first layer of any hard mask (etched mask film), and any conductive film described above can be formed, for example, by ion beam sputtering or magnetron sputtering.
[0137] The silicon-containing hard masking film described above is formed by coating a silicon-containing hard masking film forming composition (e.g., the silicon-containing hard masking film forming composition) that is cured at a temperature of 50°C to 180°C directly or indirectly onto the absorber layer by means of a method such as spin coating, and then curing the coating film at a temperature of 50°C to 180°C.
[0138] After a coating film is formed by spin coating or the like, it is baked to allow the organic solvent to evaporate and harden. The baking temperature is set to 50~180°C, more preferably 80°C~170°C, and even more preferably 100°C~150°C. The baking time is preferably 10~3,600 seconds, more preferably 300 seconds to 2,400 seconds, and even more preferably 600 seconds to 1,200 seconds.
[0139] As long as the baking conditions are such, the periodic structure of the multilayer reflective film formed under the silicon hard mask film will not be disturbed. The hardened film containing silicon hard mask film with sufficient density of Si-O-Si crosslinking can be formed directly or indirectly on the absorber layer, so high etching resistance to chlorine dry etching conditions can be obtained.
[0140] The thickness of the silicon-containing hard mask film also depends on the thickness of the resist film formed on the upper layer or the thickness of the first layer of the hard mask film on the lower layer. It is preferably 1~50nm, more preferably 5~30nm, and especially preferably 10~25nm. As long as the film thickness is within such a range, because it has sufficient etching resistance, the resist pattern can be transferred to the absorber layer or the first layer of the hard mask film with high precision.
[0141] The lower limit of the silicon content in the aforementioned silicon-containing hard masking film is preferably 5% or more, more preferably 10% or more, and even more preferably 30% or more. As long as the film contains silicon in such a proportion, its curing properties are excellent, thus enabling the reliable provision of silicon-containing hard masking films that can be cured at temperatures between 50°C and 180°C. Furthermore, high etching resistance to chlorine-based dry etching conditions can be obtained.
[0142] The upper limit of the silicon content in the silicon-containing hard mask film is preferably 50% or less, and more preferably 45% or less. As long as the film contains silicon in such a proportion, for example, after dry etching of the Cr-containing hard mask, the silicon-containing hard mask film remaining on the Cr-containing hard mask film pattern can be easily removed.
[0143] The photoresist film can be formed by coating methods such as spin coating.
[0144] The blank photomask of the present invention described above can be manufactured using the blank photomask manufacturing method of the present invention. However, the blank photomask of the present invention can also be manufactured using methods other than those described above.
[0145] <Processing Method of Blank Photomask> The processing method of the blank photomask of the present invention is characterized by comprising the following steps: (i-1) irradiating the blank photomask of the present invention with an electron beam, and then developing it with a developing solution to form a photoresist pattern on the photoresist film; (i-2) forming the silicon-containing film pattern on the silicon-containing hard mask film by etching the photoresist pattern as a mask; (i-3) processing the absorber layer directly or indirectly by etching the silicon-containing film pattern as a mask.
[0146] As long as the blank photomask processing method is used, because a silicon-containing hard mask film, which has better dry etching resistance to chlorine gases than a photoresist film, is used as the hard mask, the resist pattern can be transferred to the absorber layer of the blank photomask with high precision. Furthermore, the silicon-containing hard mask film can be formed in a temperature range of 50°C to 180°C, thus preventing interlayer mixing of multiple reflective film layers and improving the transfer accuracy of the resist pattern. In other words, as long as the blank photomask processing method of the present invention is used, the reflectivity of EUV light will not deteriorate, and a photomask containing an absorber layer with finely patterned absorbers formed with high precision can be provided.
[0147] If a specific example of the processing method of the blank photomask of the present invention is described, it will be as follows.
[0148] First, a substrate is formed, a multilayer reflective film layer on the substrate that reflects EUV light, a protective film on the multilayer reflective film layer for protecting the multilayer reflective film layer, an absorber layer on the protective film layer for absorbing the exposure light, and a Cr-containing hard mask film on the absorber layer that functions as a first layer of hard mask when the absorber layer is patterned by dry etching.
[0149] Then, the previously described composition for forming a silicon-containing hard mask film is coated onto the Cr-containing hard mask film, and a hardened film of the silicon-containing hard mask film is formed by baking at a temperature of 50°C to 180°C. That is, a silicon-containing hard mask film is formed directly or indirectly on the absorber layer. Then, a photoresist film is formed on the silicon-containing hard mask film. A blank photomask is thus obtained.
[0150] The resist film of the blank photomask is patterned by an electron beam, and then formed by heating and developing steps.
[0151] The obtained resist pattern is first transferred to a silicon-containing hard mask film by dry etching. The dry etching conditions can be fluorine-based dry etching performed under commonly used fluorine-containing gas conditions. Examples of fluorine-containing gases include fluorine gas, carbon and fluorine-containing gases such as CF4, CHF3, and C2F6, sulfur and fluorine-containing gases such as SF6, and even mixtures of fluorine-free gases such as helium and nitrogen with fluorine-containing gases. Furthermore, gases such as oxygen can be added as needed.
[0152] Then, the photoresist is stripped off, or left behind, and the obtained silicon-containing hard mask film pattern is used as a hard mask to transfer the pattern to a Cr-containing hard mask film. The hard etching used here can be a chlorine-based dry etching. For example, commonly used oxygen-containing chlorine-based dry etching can be used as the dry etching condition. For example, the mixing ratio of chlorine and oxygen (Cl2 gas: O2 gas) can be set to 1:2 to 20:1 by volume flow rate. Depending on the requirements, a gas mixed with a passive gas such as helium can be used for dry etching. The silicon-containing hard mask film has higher resistance to chlorine-based dry etching than the photoresist film. Therefore, by using the silicon-containing hard mask film as a hard mask, the photoresist pattern can be transferred to the Cr hard mask with high precision.
[0153] The Cr hard mask film pattern is used as a hard mask and transferred to the absorber layer. The dry etching used here is a fluorine-based dry etching performed under common fluorine-containing gas conditions. Examples of fluorine-containing gases include fluorine gas, carbon and fluorine-containing gases such as CF4, CHF3, and C2F6, sulfur and fluorine-containing gases such as SF6, and mixtures of fluorine-free gases such as helium and nitrogen with fluorine-containing gases. In addition, gases such as oxygen can be added as needed. The silicon-containing hard mask film remaining on the Cr hard mask film can be removed by the above-described fluorine-based dry etching. Furthermore, before the above-described fluorine-based dry etching, wet etching can also be performed, similar to that used for general SOG films.
[0154] The Cr hard masking film remaining on the absorber layer can be removed by chlorine-based dry etching. The protective film formed on the multilayer reflective film is resistant to chlorine-based dry etching, so the Cr hard masking film can be removed without damaging the multilayer reflective film.
[0155] The above describes an example of indirectly forming a silicon-containing hard masking film by interposing a Cr hard masking film on the absorber layer. However, the present invention can also directly form a silicon-containing hard masking film on the absorber layer. In this case, the silicon-containing hard masking film pattern can be used as a mask for etching the absorber layer. [Example]
[0156] Hereinafter, synthetic examples, embodiments, and comparative examples are shown to specifically illustrate the present invention, but the present invention is not limited thereto by such description. Furthermore, in the following examples, % represents mass%, and molecular weight Mw is the weight-average molecular weight of polystyrene as determined by GPC.
[0157] [Synthesis Example 1] A mixture of 120g methanol, 0.1g 10% nitric acid, and 60g deionized water was mixed with 30.6g of compound (101), 38.1g of compound (102), and 5.9g of compound (110). The mixture was kept at 40°C for 12 hours to allow for hydrolysis and condensation. After the reaction was complete, 600g propylene glycol ethyl ether (PGEE) was added. The water supplied for hydrolysis and condensation and the byproduct alcohol were distilled off under reduced pressure to obtain 440g of a PGEE solution of polysiloxane compound 1 (compound concentration 10%). The polystyrene-converted molecular weight of polysiloxane compound 1 was determined to be Mw = 2,900.
[0158] [Synthesis Examples 2-8] Using the monomers shown in Table 1 under the same conditions as in Synthesis Example 1, [Synthesis Examples 2] to [Synthesis Examples 8] were carried out to obtain the respective target products (polysiloxane compounds 2-8).
[0159] [Table 1]
[0160] The following denote compounds used in the synthesis examples. PhSi(OCH3)3・・・Compound (100) CH3Si(OCH3)3・・・Compound (101) Si(OCH3)4・・・Compound (102)
[0161] [Chemical 11]
[0162] [Synthesis Example 9] 1400g of ethanol, 700g of ultrapure water, and 50g of 25% tetramethylammonium hydroxide were added to prepare a homogeneous solution at 40°C under nitrogen atmosphere. A mixture of 138.6g of 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane and 37.2g of phenyltrimethoxysilane was slowly added dropwise to this homogeneous solution, and the reaction was carried out at 40°C for 2 hours. After the reaction was completed, 35g of acetic acid was added to the solution to stop the reaction, and the ethanol was removed by vacuum distillation. 2000ml of ethyl acetate was added to the distilled solution, and the aqueous layer was separated. The organic layer was washed twice with 400ml of ultrapure water, and 1000g of PGMEA (propylene glycol monomethyl ether acetate) was added. Water and low-boiling solvents were then distilled off, thereby recovering 600g of a PGMEA solution (compound concentration 20%) of polysiloxane compound 9. The converted molecular weight of polystyrene of polysiloxane compound 9 was determined to be Mw=2800.
[0163] [Preparation of compositions for forming silicon-containing hard masking films] The polysiloxane compounds 1 to 9 obtained in the above synthesis example, crosslinking catalysts (XLC-1 to 3), acid generating agents (AG1 to 4), crosslinking agents (XL1), organic solvents, and water were mixed in the proportions shown in Table 2. Each mixture was filtered through a 0.1 μm fluororesin filter to prepare a silicon-containing underlayer film forming composition solution, which was designated as UDL-1 to 18.
[0164] [Table 2] Composition for forming silicon-containing hard masking films Silicon-containing polymers Crosslinking catalyst additive organic solvents water (parts by weight) (parts by weight) (parts by weight) (parts by weight) (parts by weight) UDL-1 Compound 1 (1) none PGEE (100) water (10) UDL-2 Compound 2 (1) none PGEE (100) water (10) UDL-3 Compound 3 (1) none PGEE (100) water (10) UDL-4 Compound 4 (1) none PGEE (100) water (10) UDL-5 Compound 5 (1) none PGEE (100) water (10) UDL-6 Compound 6 (1) none PGEE (100) water (10) UDL-7 Compound 7 (1) none PGEE (100) water (10) UDL-8 Compound 8 (1) none PGEE (100) water (10) UDL-9 Compound 9 (1) none PGMEA (100) - UDL-10 Compound 1 (1) XLC-1 (0.03) PGEE (100) water (10) UDL-11 Compound 2 (1) XLC-2 (0.03) PGEE (100) water (10) UDL-12 Compound 3 (1) XLC-3 (0.03) PGEE (100) water (10) UDL-13 Compound 4 (1) XLC-1 (0.03) AG1 (0.01) PGEE (100) water (10) UDL-14 Compound 5 (1) XLC-2 (0.03) AG2 (0.01) PGEE (100) water (10) UDL-15 Compound 6 (1) XLC-3 (0.03) AG3 (0.01) PGEE (100) water (10) UDL-16 Compound 7 (1) XLC-1 (0.03) AG4 (0.01) PGEE (100) water (10) UDL-17 Compound 8 (1) XLC-2 (0.03) AG1 (0.01) PGEE (100) water (10) UDL-18 Compound 9 (1) - XL1 (0.3) PGMEA (100) -
[0165] The crosslinking catalyst used is as described below. XLC-1··· Triphenylsilane nitrate XLC-2··· Mono-(triphenylsilane) maleic acid XLC-3··· Triethylphenylammonium iodide
[0166] The organic solvents used are as described below. PGEE···Propylene Glycol Ethyl Ether PGMEA···Propylene Glycol Methyl Ether Acetate
[0167] The acid generating agent used is as described in Table 3 below. [Table 3]
[0168] The crosslinking agent (XL1) used is as follows. [Chemical 12]
[0169] [Solvent Resistance Evaluation] On a substrate, a 4nm Si film and a 3nm Mo film were formed as 1 pair to form 40 pairs, and then a 3nm Si film was formed on the surface to form a multilayer reflective film. A 2.5nm Ru protective layer and a 70nm TaN absorber layer were formed sequentially on the multilayer reflective film. Any of the silicon-containing hard mask film forming compositions (UDL-1 to 18) prepared above were coated on the absorber layer, and the obtained coating was calcined under the baking conditions described in Table 4 to obtain a silicon-containing hard mask film. Thus, the composites of Examples 1-1 to 1-20 were obtained.
[0170] The film thickness from the center to the outer edge of the substrate of the composites obtained in Examples 1-1 to 1-20 was measured, and the average film thickness (a [nm]) was calculated. Then, PGMEA solvent was dispensed onto it, left for 30 seconds and rotated to dry, and baked at 110°C for 600 seconds to evaporate the PGMEA. Then the film thickness (b [nm]) was measured.
[0171] Table 4 below shows the film thicknesses a and b, and the value of (b / a)×100 as an indicator of solvent resistance.
[0172] [Table 4] Example 1 Silicon-containing rigid masking film Forming components Baking conditions Film thickness a (nm) Film thickness b (nm) Solvent resistance temperature time (b / ax 100) (%) Example 1-1 UDL-1 150℃ 600s 200.8 197.6 98.4% Examples 1-2 UDL-2 150℃ 600s 202.1 198.4 98.2% Examples 1-3 UDL-3 150℃ 600s 199.8 196.9 98.5% Examples 1-4 UDL-4 150℃ 600s 201.3 198.4 98.6% Examples 1-5 UDL-5 150℃ 600s 200.4 196.9 98.3% Examples 1-6 UDL-6 150℃ 600s 202.1 199.3 98.6% Examples 1-7 UDL-7 150℃ 600s 200.9 198.1 98.6% Examples 1-8 UDL-8 150℃ 600s 201.1 197.6 98.3% Examples 1-9 UDL-9 150℃ 600s 198.8 195.6 98.4% Examples 1-10 UDL-10 120℃ 600s 201.7 201 99.7% Examples 1-11 UDL-11 120℃ 600s 203.4 202.7 99.7% Examples 1-12 UDL-12 120℃ 600s 200.8 200.1 99.7% Examples 1-13 UDL-13 120℃ 600s 203.7 203 99.7% Examples 1-14 UDL-14 120℃ 600s 202.2 201.6 99.7% Examples 1-15 UDL-15 120℃ 600s 203.5 202.8 99.7% Examples 1-16 UDL-16 120℃ 600s 202.5 201.7 99.6% Examples 1-17 UDL-17 120℃ 600s 202.3 201.5 99.6% Examples 1-18 UDL-18 120℃ 600s 199.5 196.1 98.3% Examples 1-19 UDL-18 140℃ 600s 199.8 198.1 99.1% Examples 1-20 UDL-18 140℃ 1200s 199.7 199.4 99.8%
[0173] As shown in Table 4, the residual film rate ((b / a)×100) after PGMEA washing treatment in Examples 1-1 to 1-20 is over 98%, indicating that crosslinking reaction still occurs on the photomask substrate, demonstrating sufficient solvent resistance. In particular, Examples UDL-10 to 17, which contain crosslinking catalysts, exhibit excellent curing properties and can be processed at lower calcination temperatures. Furthermore, it was confirmed that higher baking temperatures or longer baking times in Examples 1-18 to 1-20 further improve solvent resistance.
[0174] Furthermore, it was confirmed that Examples 1-1 to 1-20 were prepared at temperatures between 50°C and 180°C, and more specifically at temperatures between 120°C and 150°C. All of the silicon-containing hard mask film forming compositions (UDL-1 to 18) prepared above were hardened.
[0175] [Reflectivity] (Reference substrate with attached multilayer reflective film) On the substrate, Si 4nm and Mo 3nm are formed as 1 pair to form 40 pairs, and then Si 3nm is formed on the surface to form a multilayer reflective film. Ru 2.5n is formed as a protective film on the multilayer reflective film. Thus, a reference substrate with attached multilayer reflective film is obtained.
[0176] When measuring the peak reflectance of EUV light (wavelength 13.5 nm, hereinafter the same) on the main surface of the substrate with the attached multilayer reflective film layer of the reference at an incident angle of 6°, it is 65%.
[0177] (Example 2-1) Then, on the main surface of the above-mentioned photomask substrate, a multilayer reflective film and a protective film were formed under the same conditions as those used in the fabrication of the reference substrate with a multilayer reflective film, thus fabricating the substrate with the multilayer reflective film of Example 2-1. This substrate with the multilayer reflective film was baked at 120°C for 600 seconds under the conditions described in the above-mentioned example, where the solvent resistance of the silicon-containing hard masking film was 98% or higher. Thus, the evaluation substrate of Example 2-1 was obtained. The peak reflectance of EUV light (wavelength 13.5 nm, hereinafter the same) on the main surface of this evaluation substrate at an incident angle of 6° was measured and found to be 65%.
[0178] (Example 2-2) The baking conditions on the substrate with the attached multilayer reflective film layer in Example 2-1 were changed to 150°C for 600 seconds. Otherwise, the evaluation substrate of Example 2-2 was fabricated under the same conditions as in Example 2-1. The peak reflectance of EUV light (wavelength 13.5 nm, hereinafter the same) on the main surface of the evaluation substrate at an incident angle of 6° was measured and found to be 65%.
[0179] (Examples 2-3) The baking conditions on the substrate with the attached multilayer reflective film layer in Example 2-1 were changed to 180°C for 600 seconds. Otherwise, the evaluation substrate of Example 2-3 was fabricated under the same conditions as in Example 2-1. The peak reflectance of EUV light (wavelength 13.5 nm, hereinafter the same) on the main surface of the evaluation substrate at an incident angle of 6° was measured and found to be 64%.
[0180] (Comparative Example 2-1) The baking conditions on the substrate with the multilayer reflective film were changed to 200°C for 600 seconds. Otherwise, a substrate for a photomask substrate was fabricated under the same conditions as in Example 2-1. The peak reflectance of EUV light (wavelength 13.5 nm, hereinafter the same) on the main surface of the substrate with the multilayer reflective film at an incident angle of 6° was measured and found to be 62%. Furthermore, when the cross-section of the multilayer reflective film was observed by transmission electron microscopy (TEM), an interdiffusion layer of Si and Mo was observed.
[0181] Based on the above results, it can be seen that as long as the blank photomask of the present invention contains a silicon-containing hard mask film containing a hardened composition for forming a silicon-containing hard mask that is cured at a temperature of 50°C to 180°C, and the silicon-containing hard mask film does not need to be baked at a temperature exceeding 180°C during its formation, the temperature of 50°C to 180°C, as demonstrated in Examples 2-1 to 2-3, will not degrade the EUV light reflectivity of the multilayer reflective film layers, and the film can be formed as a useful silicon-containing hard mask film as a hard mask. On the other hand, it can be seen that in cases where the silicon-containing hard mask film is used, which differs from the present invention, and the baking temperature of the silicon-containing hard mask film needs to exceed 180°C, interlayer mixing of the multilayer reflective film layers occurs, and the EUV light reflectivity degrades.
[0182] [Exposure Evaluation] (Examples 3-1~3-24) On a substrate, a 4nm Si film and a 3nm Mo film were formed as 1 pair to form 40 pairs. Then, a 3nm Si film was formed on the surface to form a multilayer reflective film. On this multilayer reflective film, a 2.5nm Ru film as a protective film and a 70nm TaN absorber layer were formed sequentially. A 6nm thick CrN film was formed on the absorber layer as the first layer of the hard mask film.
[0183] Any of the silicon-containing hard mask film forming components (UDL-1 to 18) prepared above are coated on the CrN film by spin coating, and calcined under the baking conditions described in Table 5 to form a silicon-containing hard mask layer (silicon oxide material film) with a film thickness of 20 nm as the second layer of the hard mask.
[0184] Then, a spin coater was used on the substrate on which the silicon hard mask layer was formed to form a 90 nm or 60 nm thick electron beam chemical amplification resist liquid SEBP-504G manufactured by Shin-Etsu Chemical Industry Co., Ltd. Thus, blank photomasks for each embodiment were produced.
[0185] Then, the photoresist film of each blank photomask was exposed using an electron beam exposure apparatus (EBM5000 manufactured by NuFLARE, accelerating voltage 50keV), and baked at 110°C for 10 minutes (PEB: post-exposure bake). Development was then performed using a 2.38% by mass aqueous solution of tetramethylammonium hydroxide, thereby obtaining a positive photoresist pattern containing a 100nm line pattern. Furthermore, the above exposure was obtained by resolving the top and bottom of the obtained 100nm line and spacing at a 1:1 ratio as the optimal exposure (sensitivity: Eop).
[0186] The line edge roughness of the above resist pattern was measured. The line edge roughness was determined by using a SEM (ADVANTEST CORPORATION E3640) to detect the edges of 32 lines of each 100nm LS pattern at 80 points, and the deviation (standard deviation, σ) was calculated as 3 times the value (3σ), which was taken as LER (nm).
[0187] Then, the photoresist pattern described above is used as an etching mask, and the photomask substrate is processed in the following order.
[0188] First, using the above photoresist pattern as a mask, the silicon-containing hard mask film exposed from the photoresist pattern is patterned by dry etching using a dry etching apparatus under the following fluorine-based dry etching conditions. [Etching conditions for silicon-containing film] RF1 (RIE): CW 54V RF2 (ICP): CW 325W Pressure: 5mTorr SF6: 18sccm O2: 45sccm Etching time: 1min
[0189] Then, after the above photoresist pattern is stripped by oxygen plasma, the exposed Cr hard mask film is patterned by using the patterned silicon hard mask film (silicon film pattern) as a mask and dry etching under the following oxygen-containing chlorine dry etching conditions.
[0190] [Etching Conditions for Cr Hard Mask Film] RF1 (RIE): CW 10W RF2 (ICP): CW 300W Pressure: 5mTorr Cl2: 150sccm O2: 50sccm He: 10sccm Etching Time: 1min
[0191] Then, the exposed absorber layer TaN film is patterned by dry etching under etching condition-1 and continuous etching condition-2, using the patterned Cr hard mask film as a mask.
[0192] [Etching Conditions for TaN Film - 1] RF1 (RIE): CW 54W RF2 (ICP): CW 325W Pressure: 5mTorr SF6: 18sccm He: 130sccm Etching Time: 10sec
[0193] [Etching Conditions for TaN Film - 2] RF1 (RIE): CW 7.6W RF2 (ICP): CW 300W Pressure: 5mTorr Cl2: 150sccm He: 10sccm Etching Time: 5min
[0194] (Comparative Examples 3-1 and 3-2) No silicon-containing hard mask layer was formed on the above-mentioned CrN film. The photoresist film was directly formed with the film thickness shown in Table 5. Otherwise, blank photomasks were made in the same manner as in Examples 3-1 or 3-14. The blank photomasks were processed in the same manner as in Examples 3-1 or 3-14.
[0195] The edge roughness of the patterned lines etched as described above in Examples 3-1 to 3-24 and Comparative Examples 3-1 and 3-2 was measured. The edge roughness was determined using a SEM (ADVANTEST CORPORATION E3640) to inspect 80 edges of 32 lines in each 100nm LS pattern. The deviation (standard deviation, σ) was calculated as three times the value (3σ), which was taken as the LER (nm). A smaller value indicates better performance. Furthermore, the cross-sectional shape (pattern shape) was observed using an electron microscope (S-4800) manufactured by Hitachi High-Tech Corporation. No tailing or undercut shape was observed, which was considered good; obvious tailing or undercut shape was observed, which was considered poor. The results are shown in Table 5.
[0196] [Table 5] Example 3 and Comparative Example 3 Composition for forming silicon-containing hard masking films Baking conditions Resistor film thickness Inhibitor Pattern Etched pattern temperature time (nm) LER(nm) cross-sectional shape LER(nm) Example 3-1 UDL-1 150℃ 600s 90 2.1 rectangle 1.9 Example 3-2 UDL-1 180℃ 600s 90 2.2 rectangle 1.9 Example 3-3 UDL-2 150℃ 600s 90 2.2 rectangle 1.9 Examples 3-4 UDL-3 150℃ 600s 90 2.2 rectangle 1.9 Examples 3-5 UDL-4 150℃ 600s 90 2.2 rectangle 1.9 Examples 3-6 UDL-5 150℃ 600s 90 2.2 rectangle 1.9 Examples 3-7 UDL-6 150℃ 600s 90 2.2 rectangle 1.9 Examples 3-8 UDL-7 150℃ 600s 90 2.3 rectangle 1.9 Examples 3-9 UDL-8 150℃ 600s 90 2.5 rectangle 2.2 Examples 3-10 UDL-9 150℃ 600s 90 2.4 rectangle 2.0 Example 3-11 UDL-10 120℃ 600s 90 2.0 rectangle 1.7 Example 3-12 UDL-10 150℃ 600s 90 2.0 rectangle 1.7 Example 3-13 UDL-10 180℃ 600s 90 2.1 rectangle 1.7 Example 3-14 UDL-10 120℃ 600s 60 2.1 rectangle 1.8 Example 3-15 UDL-11 120℃ 600s 90 2.1 rectangle 1.8 Example 3-16 UDL-12 120℃ 600s 90 1.9 rectangle 1.7 Example 3-17 UDL-13 120℃ 600s 90 2.1 rectangle 1.8 Example 3-18 UDL-13 180℃ 600s 90 2.1 rectangle 1.8 Example 3-19 UDL-13 120℃ 600s 60 2.2 rectangle 1.8 Example 3-20 UDL-14 120℃ 600s 90 2.1 rectangle 1.8 Example 3-21 UDL-15 120℃ 600s 90 2.1 rectangle 1.8 Example 3-22 UDL-16 120℃ 600s 90 2.2 rectangle 1.8 Example 3-23 UDL-17 120℃ 600s 90 2.4 rectangle 2.1 Example 3-24 UDL-18 140℃ 1200s 90 2.3 rectangle 2.1 Comparative Example 3-1 none - - 90 2.7 Push-out shape 2.8 Comparative Example 3-2 none - - 60 3.5 Push-out shape 3.9
[0197] As shown in Table 5, the blank photomask systems of Examples 3-1 to 3-24 containing the silicon-containing hard mask film of the present invention showed good edge roughness of the resist pattern compared to Comparative Examples 3-1 and 3-2 which did not contain the silicon-containing hard mask film, and the pattern shape after etching was also excellent. Examples 3-1 to 3-8, which used polysiloxanes (compounds 1 to 7) containing organic groups having one or more carbon-oxygen single bonds or carbon-oxygen double bonds, showed good edge roughness of the resist pattern. This is presumably due to good adhesion to the resist pattern. Furthermore, Examples 3-11 to 3-23, which used compositions for forming silicon-containing hard mask films containing crosslinking catalysts (UDL-10 to 17), showed even better edge roughness of the resist pattern compared to compositions without crosslinking catalysts, and the edge roughness after etching was also good. It is speculated that this is because the addition of a cross-linking catalyst improves the density of the silicon-containing hard mask film.
[0198] As shown in Comparative Example 3-2, when the resist film thickness was 60 nm, LER degradation was confirmed due to the deterioration of the cross-sectional shape. In Examples 3-14 and 3-19, which contained a silicon-containing hard masking film, no deterioration of the cross-sectional shape was observed, and good LER was obtained. It is presumed that this is because of the good adhesion between the silicon-containing hard masking film and the resist film.
[0199] Based on the above, the blank photomask of the present invention contains a silicon-containing hard mask film that is useful as a hard mask film, thus enabling the transfer of fine resist patterns to the absorber layer with high precision. Furthermore, the silicon-containing hard mask film forming composition used in the present invention can be cured in a temperature range of 50°C to 180°C, thus preventing interlayer mixing of the multilayer reflective films and improving the transfer accuracy of the resist pattern. In other words, the present invention provides a blank photomask that does not degrade the reflectivity of EUV light and provides a photomask with finely patterned patterns formed with high precision.
[0200] This specification includes the following features. [1] A blank photomask, characterized in that it comprises: a substrate, a multilayer reflective film layer formed on the substrate for reflecting EUV light, an absorber layer formed on the multilayer reflective film layer for absorbing EUV light, a silicon-containing hard mask film formed directly or indirectly on the absorber layer, and a photoresist film formed on the silicon-containing hard mask film; the silicon-containing hard mask film is a cured form of a silicon-containing hard mask film forming composition cured at a temperature of 50°C to 180°C. [2] The blank photomask of [1], wherein the composition for forming the silicon-containing hard mask film contains: a silicon-containing compound having any one or more of the repeating unit represented by the following general formula (Sx-1), the repeating unit represented by the following general formula (Sx-2), and the substructure represented by the following general formula (Sx-3); [Chemical 13] (wherein Ra, Rb, and Rc are each a monovalent organic group with 1 to 30 carbon atoms, which may be the same or different.) [3] The blank photomask of [2], wherein at least one of Ra to Rc in the above formula (Sx-1) to (Sx-3) is an organic group having one or more carbon-oxygen single bonds or carbon-oxygen double bonds. [4] The blank photomask of any one of [1] to [3], wherein the composition for forming the silicon-containing hard mask film further contains a crosslinking catalyst. [5] The blank photomask as in [4], wherein the crosslinking catalyst is a strontium salt, ferrophosphate salt, phosphonium salt, ammonium salt, alkali metal salt, or a polysiloxane having any one of strontium salt, ferrophosphate salt, phosphonium salt, and ammonium salt as part of its structure. [6] A method for processing a blank photomask includes the following steps: (i-1) irradiating the blank photomask as in any one of [1] to [5] with an electron beam, and then developing it with a developer to form a photoresist pattern on the photoresist film; (i-2) forming the silicon-containing film pattern on the silicon-containing hard mask film by etching the photoresist pattern as a mask; and (i-3) processing the absorber layer directly or indirectly by etching the silicon-containing film pattern as a mask. [7] A method for manufacturing a blank photomask includes the following steps: preparing a substrate; forming a multilayer reflective film layer that reflects EUV light on the substrate; forming an absorber layer that absorbs EUV light on the multilayer reflective film layer; directly or indirectly coating the absorber layer with a silicon-containing hard mask film forming composition that is cured at a temperature of 50°C to 180°C to obtain a coating film; curing the coating film at a temperature of 50°C to 180°C to form a silicon-containing hard mask film; and forming a photoresist film on the silicon-containing hard mask film.
[0201] Furthermore, the present invention is not limited to the embodiments described above. The embodiments described above are examples; any embodiment having a substantially identical structure to the technical concept described in the claims of the present invention and performing the same effect is included within the technical scope of the present invention. [Simplified Explanation of the Diagram]
[0030] [Fig. 1] A schematic cross-sectional view of an example of a blank photomask of the present invention.
Claims
1. A blank photomask, characterized in that it comprises: a substrate, a multilayer reflective film layer formed on the substrate for reflecting EUV light, an absorber layer formed on the multilayer reflective film layer for absorbing EUV light, a Cr-containing hard mask film formed on the absorber layer, a silicon-containing hard mask film formed on the Cr-containing hard mask film, and a photoresist film formed on the silicon-containing hard mask film; wherein the silicon-containing hard mask film is a cured form of a silicon-containing hard mask film forming composition cured at a temperature of 50°C to 180°C.
2. As in request item 1, the blank photomask, wherein, The composition system for forming a silicon-containing hard mask film contains: a silicon-containing compound having any one or more of the following general formula (Sx-1), the following general formula (Sx-2), and the following general formula (Sx-3); wherein Ra, Rb, and Rc are each a monovalent organic group with 1 to 30 carbon atoms, which may be the same or different.
3. As in request item 2, the blank photomask, wherein, In the above formulas (Sx-1) to (Sx-3), at least one of Ra to Rc is an organic group having one or more carbon-oxygen single bonds or carbon-oxygen double bonds.
4. As in request item 1, the blank photomask, wherein, The composition for forming silicon-containing hard masking films also contains a crosslinking catalyst.
5. As in request item 4, the blank photomask, wherein, The crosslinking catalyst is a strontium salt, ferrophosphate salt, phosphonium salt, ammonium salt, alkali metal salt, or a polysiloxane having any one of strontium salt, ferrophosphate salt, phosphonium salt, and ammonium salt as part of its structure.
6. A method for processing a blank photomask, characterized in that it comprises the following steps: irradiating a blank photomask as claimed in any one of claims 1 to 5 with an electron beam, and then developing it with a developer to form a photoresist pattern on the photoresist film; forming a silicon-containing film pattern on the silicon-containing hard mask film by etching the photoresist pattern as a mask; forming a Cr-containing film pattern on the Cr-containing hard mask film by dry etching the silicon-containing film pattern as a mask; and processing the absorber layer by etching the Cr-containing film pattern as a mask.
7. A method for manufacturing a blank photomask, characterized in that it comprises the following steps: preparing a substrate; forming a multilayer reflective film layer that reflects EUV light on the substrate; forming an absorber layer that absorbs EUV light on the multilayer reflective film layer; forming a Cr-containing hard mask film on the absorber layer; coating a silicon-containing hard mask film forming composition that is cured at a temperature of 50°C to 180°C on the Cr-containing hard mask film to obtain a coating film; curing the coating film at a temperature of 50°C to 180°C to form a silicon-containing hard mask film; and forming a photoresist film on the silicon-containing hard mask film.
Citation Information
Patent Citations
Reflective photomask blank and method for manufacturing reflective photomask
CN117055284A
Reflective mask blank, method for manufacturing same, reflective mask, method for manufacturing same, and method for manufacturing semiconductor device
KR1020170051419A
Coating composition for pattern reversal on soc pattern
KR102426414B1
Reflection type photomask blank, production method of reflection type photomask, and reflection type photomask
TW202407458A
Reflection-type mask blank and method for manufacturing reflection-type mask