Fe-Cr-Ni ALLOY HAVING EXCELLENT WORKABILITY AND HIGH-TEMPERATURE STRENGTH
The optimized Fe—Cr—Ni alloy composition addresses the challenge of balancing high temperature strength and workability in reaction furnaces by controlling alloy components and precipitate distribution, enhancing both room and high temperature performance without expensive additives.
Patent Information
- Application Number
- US19/103013
- Authority / Receiving Office
- US · United States
- Patent Type
- Applications(United States)
- Current Assignee / Owner
- Priority Date
- 2022-08-15
- Filing Date
- 2023-05-01
- Publication Date
- 2026-11-12
AI Technical Summary
Existing Fe—Cr—Ni alloys used in reaction furnaces for polysilicon purification face challenges in achieving both high temperature strength and workability, with conventional alloys either compromising on one or the other, and often requiring expensive elements like Mo and W, or lacking specifications for room temperature and high temperature elongation.
An Fe—Cr—Ni alloy composition optimized with specific ranges of C, Si, Mn, P, S, Ni, Cr, Mo, Cu, Al, Ti, B, Co, Nb, and N, along with controlled precipitate distribution and grain size, ensuring superior workability and high temperature properties.
The alloy achieves balanced 0.2% proof stress and elongation at room and high temperatures, maintaining workability and corrosion resistance, while avoiding expensive elements, thus extending the useful life and productivity of reaction furnaces.
Smart Images

Figure US20260357387A1-D00001
Abstract
Description
TECHNICAL FIELD
[0001] The present invention relates to Fe—Cr—Ni alloys used as construction material for reaction furnaces which require superior strength at high temperatures. Practically, the present invention relates to a technique in which both superior proof stress and superior elongation are realized under room temperature and high temperatures by optimizing compositions during production of alloys.BACKGROUND ART
[0002] In recent years, clean energy by solar power generation has attracted attention. In particular, from the viewpoint of minimizing carbon dioxide generation, it has attracted more attention every year in order to avoid global warming. During the production of solar power installations, as raw material of power generating devices, polysilicon for which crude silicon raw material is purified, is often used. Inside a reaction furnace for purifying polysilicon, a high pressure of not less than 100 MPa of reaction gas and a high temperature of not less than 1100 °F, that is, a very severe environment, is necessary. Material used for the reaction furnace should not only be superior in workability for forming and in corrosion resistance, but also in high temperature strength. Useful service life of the reaction furnace may be shorter and productivity may be deteriorated if high temperature strength is low. In order to satisfy such properties, a desirable Fe—Cr—Ni alloy has been demanded.
[0003] However, if high temperature strength is made high, room temperature strength may also become high, and it may be difficult to process material during the production of the reaction furnace. In addition, since the reaction gas is a corrosive gas including chlorine, superior corrosion resistance is also necessary. A Fe—Cr—Ni alloy, in which workability and high temperature strength are superior, is necessary to solve these problems.
[0004] As a conventional technique focusing on high temperature strength, Patent Document 1 discloses ferritic stainless steel having superior high temperature oxidation resistance, high temperature creep strength, and high temperature tensile strength; however, there is no specified value concerning high temperature elongation in the Claims, and yield strength values of high temperature tensile strength disclosed in the Examples are low.
[0005] In addition, Patent Document 2 discloses a method for producing Ni alloy and Ni alloy material having superior structure stability and high temperature strength; however, the Ni alloy should contain expensive elements such as Mo and W, resulting in increased cost.
[0006] Furthermore, Patent Document 3 proposes an Fe—Cr—Ni alloy in which, during production of an alloy, compositions and precipitate or primary crystalline phase are controlled so as to realize high creep rupture property; however, there is no disclosure concerning room temperature strength, crystal grain size, high temperature 0.2% proof stress and high temperature elongation, that is, it is not an alloy for which workability is considered.
[0007] The Patent Documents are as follows:
[0008] Patent Document 1: Japanese Unexamined Patent Application Publication No. 2016-079437
[0009] Patent Document 2: Japanese Unexamined Patent Application Publication No. 2008-297579
[0010] Patent Document 3: Japanese Patent No. 6675846SUMMARY OF INVENTION
[0011] The present invention has been completed in view of the above problems, and an object of the invention is to provide Fe—Cr—Ni alloys having superior workability and high temperature property.
[0012] The inventors have researched in order to solve the above problems. First, raw materials such as electrolytic iron, Cr, Mo and Ni, were weighed and melted in a high frequency inductive furnace. A crucible was made of magnesia, and the amount of melted raw materials was 20 kg. During this process, concentration of each element such as Ni was changed each time for the purpose of measurement. After melting, the melt alloy was cast in a mold, the casted alloy was forged to have thickness of 20 mm, and the forged alloy was annealed at 1300 °C for 20 to 60 minutes.
[0013] In room temperature tensile test, a round rod test piece according to ASTM E8 was produced from the annealed plate, and the tensile test which was defined in ASTM E8 was performed so as to evaluate 0.2% proof stress and elongation.
[0014] In high temperature tensile test, a round rod test piece according to ASTM E8 was produced from the annealed plate, and the high temperature tensile test which was defined in ASTM E21 was performed at 1100 °F so as to evaluate 0.2% proof stress and elongation.
[0015] In measurement of crystal grain size, test piece of 5 mm×20 mm×15 mm was cut out of the annealed plate, and the microscope test which was defined in ASTM E112 was performed using an optical microscope in a condition in which mirror polishing had been performed on the surface of a cross section perpendicular to the forged and elongated direction, so as to measure average crystal grain diameter.
[0016] In measurement of the number of carbonitrides NbN, NbC, TiN and TiC, and measurement of distribution of precipitates NbN, NbC, TiN, TiC and M23C6, test pieces 5 mm×10 mm×10 mm were cut out of the part of ¼ plate thickness in the annealed plate, and observation and composition analyses were performed using SEM-EDS in a condition in which mirror polishing had been performed on the surface of cross section perpendicular to the forged and elongated direction.
[0017] In hardness test, test pieces 20 mm×50 mm×50 mm were cut out of a surface of the annealed plate, the surface was polished to be roughness No. #320, and a Brinell hardness test using a super hard alloy ball according to ASTM E10 was performed so as to measure hardness.
[0018] By determining an appropriate alloy composition range in this way, the alloy maintaining appropriate workability and high temperature strength could be determined.
[0019] One aspect of the present invention is an Fe—Cr—Ni alloy consisting of, in mass %, C: 0.03 to 0.08%, Si:0.10 to 0.50%, Mn: 0.20 to 1.20%, P:0.001 to 0.040%, S: 0.0001 to 0.0030%, Ni: 35.5 to 45.5%, Cr:23.5 to 26.0%, Mo: 0.30 to 1.50%, Cu: 0.01 to 0.30%, Al:0.010 to 0.150%, Ti: not greater than 0.10%, B: 0.0005 to 0.0050%, Co: 0.02 to 0.30%, Nb: 0.45 to 0.60%, N: 0.15 to 0.30% and Fe and inevitable impurities as the remainder, in which 0.2% proof stress value and elongation in room temperature tensile test which are defined in ASTM E8 satisfy not greater than 400 MPa and not less than 40.0%, respectively, 0.2% proof stress value and elongation in high temperature tensile test at 1100 °F which are defined in ASTM E21 satisfy not less than 140 MPa and not less than 50.0%, respectively, average crystal grain size in microscope test which is defined in ASTM E112 satisfies −3 to 6, in an arbitrarily chosen cross section, total sum of one or more kinds among NbN, NbC, TiN and TiC having longer diameter of 0.5 to 5 μm is reliably contained at 20 to 180 grains / mm2 on average, and in an arbitrarily chosen cross section, total sum of one or more kinds among NbN, NbC, TiN and TiC having a longer diameter of greater than 5 μm is alternatively contained at not greater than 5.0 grains / mm2 on average.
[0020] In the present invention, each component in mass % is controlled to satisfy the following formula.0.120≤Nb×N+Nb×C+Ti×N+Ti×C≤0.150
[0021] In the present invention, each component in mass % is controlled to 0.0020%≤B+P≤0.0400%, and ratio of precipitated material of total sum of one or more kinds among NbN, NbC, TiN, TiC and M23C6 having a longer diameter of 0.5 to 5 μm in an arbitrarily chosen cross section is 10 to 30% in number ratio.
[0022] In the present invention, the value in a hardness test by a super hard alloy ball of the Brinell hardness which is defined in ASTM E10 is 130 to 210.BRIEF DESCRIPTION OF DRAWINGS
[0023] FIG. 1 is an electron micrograph showing typical NbC precipitate observed in the measurement of the number of precipitates in the present invention.
[0024] FIG. 2 is an electron micrograph showing precipitates at grain boundary and precipitates inside a grain in Example 17 in the Examples. Blue spots are precipitates at a grain boundary and red spots are precipitates inside a grain.EMBODIMENTS OF INVENTION
[0025] The present invention is for improving workability and high temperature properties of Fe—Cr—Ni alloy, and is the Fe—Cr—Ni alloy consisting of, in mass %, C: 0.03 to 0.08%, Si:0.10 to 0.50%, Mn: 0.20 to 1.20%, P:0.001 to 0.040%, S: 0.0001 to 0.0030%, Ni: 35.5 to 45.5%, Cr:23.5 to 26.0%, Mo: 0.30 to 1.50%, Cu: 0.01 to 0.30%, Al:0.01 to 0.15%, Ti: not greater than 0.10%, B: 0.0005 to 0.0050%, Co: 0.02 to 0.30%, Nb: 0.45 to 0.60%, N: 0.15 to 0.30% and Fe and inevitable impurities as the remainder. Reasons for definitions within the above ranges are explained.C: 0.03 to 0.08%
[0026] C is an element necessary to maintain 0.2% proof stress of the alloy at room temperature and high temperature. Necessary strength cannot be obtained if the content is less than 0.03%. On the other hand, if the content is greater than 0.08%, the number of NbC and TiC may be increased and room temperature 0.2% proof stress may be too high. Therefore, the C content is set to be 0.03 to 0.08%. It is desirably 0.035 to 0.075% and more desirably 0.04 to 0.07%.Si: 0.10 to 0.50%
[0027] Si is added as a deoxidizing agent, Si is an element necessary to maintain oxidation resistance at high temperature, and sufficient effect cannot be obtained if the content is less than 0.10%. On the other hand, if the content is greater than 0.50%, stability of austenitic phase may be deteriorated and necessary high temperature 0.2% proof stress cannot be obtained, therefore, the content is set to be 0.10 to 0.50%. It is desirably 0.12 to 0.45% and more desirably 0.13 to 0.40%.Mn: 0.20 to 1.20%
[0028] Mn is added as a deoxidizing agent, Mn is an element stabilizing austenitic phase, and sufficient effect cannot be obtained if the content is less than 0.20%. On the other hand, if the content is greater than 1.20%, stability of austenitic phase may be deteriorated and necessary high temperature 0.2% proof stress cannot be obtained, therefore, the content is set to be 0.20 to 1.20%. It is desirably 0.35 to 1.10% and more desirably 0.50 to 1.00%.P: 0.001 to 0.040%
[0029] P is an important element in the present invention, is an element inevitably contained in a steel as an impurity, and is an element segregating at grain boundary and deteriorating high temperature elongation if the content is too high. Therefore, the upper limit should be strictly limited. In the present invention, P is limited to not greater than 0.04%. Desirable upper limit of the content is 0.030%, and a more desirable upper limit is 0.020%. It is more desirable as the lower limit of P content be closer to 0%, in the present invention, based on Example 1, in which 0.01% is mentioned.S: 0.0001 to 0.0030%
[0030] S is an important element in the present invention, forms sulfides, and deteriorates toughness. Therefore, it is more desirable that the S content be as low as possible, and the upper limit is desirably 0.0030%. It is more desirably at not greater than 0.0015% and further more desirably 0.0010%. It should be noted that S is also an element improving welding property since flowability of melt alloy during melting is greatly improved even by addition of a small amount of S. Therefore, S is not limited in particular; however, from the viewpoint of obtaining good welding property, it is desirable to be contained at not less than 0.0001%. It should be noted that S content is controlled within the range of the present invention by desulfurizing by addition of Al and Si.Ni: 35.5 to 45.5%
[0031] Ni is an important element to stabilize austenitic phase and to maintain high temperature 0.2% proof stress. The effect cannot be obtained if the content is less than 35.5%, and raw material cost may increase if the content is greater than 45.5%. Therefore, the content is set to be 35.5 to 45.5%. It is desirably 36.0 to 44.0%, and is more desirably 37.0 to 40.0%.Cr: 23.5 to 26.0%
[0032] Cr is an element improving corrosion resistance and has effects of forming dense oxidation films at high temperature and maintaining high temperature 0.2% proof stress of parent material. The effect cannot be obtained if the content is less than 23.5%. On the other hand, if the content is greater than 26.0%, stability of an austenitic phase may be decreased and necessary high temperature 0.2% proof stress cannot be obtained. Therefore, the content is set to be 23.5 to 26.0%. It is desirably 24.0 to 25.5%, and is more desirably 24.5 to 25.4%.Mo: 0.30 to 1.50%
[0033] Mo is an element improving corrosion resistance, has an effect of strengthening a grain boundary, and is an element necessary to maintain high temperature 0.2% proof stress. The effect cannot be obtained if the content is less than 0.30%. On the other hand, if the content is greater than 1.50%, a phase may be precipitated and high temperature elongation may be deteriorated. Therefore, the content is set to be 0.30 to 1.50%. It is desirably 0.35 to 1.30%, and more desirably 0.40 to 1.00%.Cu: 0.01 to 0.30%
[0034] Cu is an element stabilizing an austenitic phase, improving room temperature elongation, and is necessary for an alloy of the present invention. The content should not be less than 0.01% in order to obtain the effect. On the other hand, if the Cu content is large, high temperature 0.2% proof stress may be decreased. Therefore, the upper limit of Cu content is set to be 0.30%. It is more desirably 0.02 to 0.25%, and is more desirably 0.03 to 0.20%.Al: 0.010 to 0.150%
[0035] Al is a useful element to make oxidation film after rolling denser. From this viewpoint, it is necessary to contain 0.010%. Furthermore, it is also an effective element as a deoxidizing agent. Sufficient effect cannot be obtained, oxides inclusions may be increased, and sufficient high temperature 0.2% proof stress cannot be obtained if the content is less than 0.010%. Furthermore, if the content is greater than 0.150%, Al may bind N to form Al nitride, thereby deteriorating high temperature 0.2% proof stress. Therefore, the content is set to be 0.01 to 0.150%. It is desirably 0.015 to 0.130%, and more desirably 0.020 to 0.100%.Ti: Not greater than 0.10%
[0036] Since Ti is useful forming nitride and carbide and maintaining high temperature 0.2% proof stress, Ti can be added. If the content is greater than 0.10%, the number of nitrides or carbides may be increased and may exceed the range of the present invention. Therefore, the content should be not greater than 0.10%. It is desirably not greater than 0.07%, and more desirably not greater than 0.05%.B: 0.0005 to 0.0050%
[0037] B is an element segregating at a grain boundary, has an effect of improving grain boundary strength at high temperature, and is an important element to maintain high temperature 0.2% proof stress. The effect cannot be obtained if the content is less than 0.0005%, and high temperature elongation may be decreased if the content is greater than 0.0050%. Therefore, the content is set to be 0.0005 to 0.0050%. It is desirably 0.0010 to 0.0045%, and more desirably 0.0015 to 0.0040%.Co: 0.02 to 0.30%
[0038] Co is a useful element and is a necessary element for the alloy of the present invention since only high temperature 0.2% proof stress is improved while not changing strength at room temperature. The effect cannot be obtained if the content is less than 0.02%, and high temperature elongation may be decreased if the content is greater than 0.30%. In addition, raw material cost may be increased. Therefore, the content is set to be 0.02 to 0.30%. It is desirably 0.03 to 0.28%, and more desirably 0.04 to 0.25%.Nb: 0.45 to 0.60%
[0039] Nb is useful since Nb forms nitride and carbide and maintain high temperature 0.2% proof stress. The effect cannot be obtained if the content is less than 0.45%. However, if the content is greater than 0.60%, the number of the nitrides or carbides may be increased, thereby deteriorating high temperature 0.2% proof stress. Therefore, the content is set to be 0.45 to 0.60% It is desirably 0.47 to 0.58%, and more desirably 0.50 to 0.56%.N: 0.15 to 0.30%
[0040] N is an element improving corrosion resistance and is a useful element since N forms nitrides with Nb and Ti. Sufficient effect cannot be obtained if the content is less than 0.15%, and necessary room temperature 0.2% proof stress and high temperature 0.2% proof stress cannot be obtained. On the other hand, if the content is greater than 0.30%, the number of nitrides or carbides may be increased, exceeding the range of the present invention, and therefore room temperature 0.2% proof stress may be too high. Therefore, the content is set to be 0.15 to 0.30%. It is desirably 0.17 to 0.28%, and more desirably 0.20 to 0.25%.
[0041] By satisfying the above mentioned range of the compositions, value of 0.2% proof stress in room temperature tensile test defined in ASTM E8, that is, not greater than 400 MPa can be satisfied. If the value is greater than 400 MPa, workability is inferior, and it is difficult to produce a reaction furnace. It is desirably not greater than 390 MPa, and more desirably not greater than 380 MPa.
[0042] Furthermore, by satisfying the above-mentioned range of the compositions, value of elongation in room temperature tensile test defined in ASTM E8, that is, not less than 40.0% can be satisfied. If the value is less than 40.0%, workability is inferior, and it is not appropriate for producing a reaction furnace. It is desirably not less than 42.0%, and more desirably not less than 43.0%.
[0043] By satisfying the above-mentioned range of the compositions, value of 0.2% proof stress in the high temperature tensile test at 1100 °F defined in ASTM E21, that is, not less than 140 MPa can be satisfied. If the value is less than 140 MPa, it is not appropriate for use in an alloy since cracking may occur under the above-mentioned high temperature environment. It is desirably not less than 150 MPa, and more desirably not less than 160 MPa.
[0044] Furthermore, by satisfying the above-mentioned range of the compositions, value of elongation in the high temperature tensile test defined in ASTM E21, that is, not less than 50.0%, can be satisfied. If the value is less than 50.0%, it is not appropriate for use in alloy since cracking may occur under the above mentioned high temperature environment. It is desirably not less than 55.0%, and more desirably not less than 60.0%.
[0045] Furthermore, by satisfying the above-mentioned range of the compositions, average crystal grain size in the microscope test defined in ASTM E112, −3 to 6, can be satisfied. If the value is less than −3, crystal grain may be coarse and high temperature 0.2% proof stress may be deteriorated. If the value is greater than 6, it is not appropriate for producing a reaction furnace since room temperature 0.2% proof stress is high and workability is inferior. It is desirably −2 to 5, and more desirably −1 to 4.
[0046] Furthermore, by satisfying the above-mentioned range of the compositions, the alloy may exhibit in an arbitrarily chosen cross section, total sum of one or more kinds among NbN, NbC, TiN and TiC having longer diameter of 0.5 to 5 μm is reliably contained at 20 to 180 grains / mm2 on average; and in an arbitrarily chosen cross section, total sum of one or more kinds among NbN, NbC, TiN and TiC having longer diameter of greater than 5 μm is alternatively contained at not greater than 5.0 grains / mm2 on average. If in an arbitrarily chosen cross section, total sum of one or more kinds among NbN, NbC, TiN and TiC having longer diameter of 0.5 to 5 μm is contained at less than 20 grains / mm2 on average, crystal grain may be coarsened in an annealing process and high temperature 0.2% proof stress may not be satisfied. If in an arbitrarily chosen cross section, total sum of one or more kinds among NbN, NbC, TiN and TiC having longer diameter of 0.5 to 5 μm is contained at greater than 180 grains / mm2 on average, or if in an arbitrarily chosen cross section, total sum of one or more kinds among NbN, NbC, TiN and TiC having longer diameter of greater than 5 μm is contained at greater than 5.0 grains / mm2 on average, carbonitride may be an origin point of a void, and high temperature elongation may be low. It is desirable that the total sum of one or more kinds among NbN, NbC, TiN and TiC having longer diameter of 0.5 to 5 μm will be reliably contained at 30 to 170 grains / mm2 on average and a total sum of one or more kinds among NbN, NbC, TiN and TiC having longer diameter of greater than 5 μm is alternatively contained at not greater than 3.0 grains / mm2 on average. It is more desirable that a total sum of one or more kinds among NbN, NbC, TiN and TiC having longer diameter of 0.5 to 5 μm is reliably contained at 40 to 160 grains / mm2 on average and total sum of one or more kinds among NbN, NbC, TiN and TiC having longer diameter of greater than 5 μm is alternatively contained at not greater than 1.0 grains / mm2 on average.0.120≤Nb×N+Nb×C+Ti×N+Ti×C≤0.150 (Formula 1)
[0047] The Formula 1 shows a range of amount of precipitates of carbonitrides. The amount of precipitates of carbonitrides may be small, crystal grain may be coarsened in annealing process, and superior high temperature 0.2% proof stress may not be obtained if the value is less than 0.120. Carbonitrides may be an origin of voids and high temperature elongation may be low if the value is greater than 0.150. It is desirably 0.125 to 0.145, and more desirably 0.130 to 0.140.0.0020%≤B+P≤0.0400% (Formula 2)
[0048] The Formula 2 indicates range of desirable amounts of addition of elements which segregate at grain boundaries. The amount of segregation at a grain boundary may run short, the grain boundary may not be strengthened, and superior high temperature 0.2% proof stress cannot be obtained if the amount is less than 0.0020%. The amount of segregation at a grain boundary may be too large, the grain boundary may be brittle, and high temperature elongation may be low if the amount is greater than 0.0400%. It is desirably 0.0025% to 0.0300%, and more desirably 0.0030% to 0.0200%.
[0049] In addition, the Fe—Cr—Ni alloy is characterized in that ratio of precipitates of a total sum of one or more kinds among NbN, NbC, TiN, TiC and M23C6 having longer diameter of 0.5 to 5 μm in an arbitrarily chosen cross section is 10 to 30%. High temperature 0.2% proof stress cannot be obtained if the ratio is less than 10%, and high temperature elongation is not satisfied if the ratio is greater than 30%. It is desirably 12 to 28%, and more desirably 15 to 25%.
[0050] In addition, the Fe—Cr—Ni alloy is characterized in that value in hardness test of the Brinell hardness by super hard alloy ball which is defined in ASTM E10 is 130 to 210. High temperature 0.2% proof stress cannot be obtained if the value is less than 130, and workability may be inferior and it may be inappropriate for producing a reaction furnace if the value is greater than 210. It is desirably 140 to 200, and more desirably 150 to 190.EXAMPLES
[0051] Raw material in which iron scrap, ferrochromium, ferronickel, stainless steel scrap and the like were controlled in a predetermined ratio was melted in an electric furnace, secondary refining was performed in an AOD (Argon Oxygen Decarburization) furnace or VOD (Vacuum Oxygen Decarburization) furnace so as to control the melt material into kinds of compositions shown in Table 1, and continuous casting was performed so as to obtain a slab. It should be noted that among values shown in Table 1, C and S compositions were analyzed by carbon-sulfur simultaneous analysis apparatus (combustion in oxygen gas flow-infrared absorption method), N composition was analyzed by oxygen-nitrogen simultaneous analysis apparatus (inert gas-impulse heating melting method), and the other compositions were analyzed by fluorescent X-ray analysis. Then, the slab was hot-rolled, and was annealed at 1180 to 1300 °C so as to obtain a hot-rolled annealed steel plate having thickness of 20 mm.TABLE 1CSiMnPSNiCrMoCuExamples10.0310.481.120.0010.000336.424.10.520.1920.0690.20.850.0090.000242.924.91.100.0430.0420.141.020.0110.002044.523.70.890.1140.0320.110.740.0120.000841.525.01.000.1550.0390.280.230.0180.001343.624.40.320.2160.0340.170.600.0060.000739.725.20.920.0870.0570.421.180.0390.000436.225.30.480.0580.0440.330.700.0370.001140.924.60.840.0790.0330.450.650.0220.000540.724.81.460.04100.0350.120.430.0270.001036.625.10.380.27110.0500.350.380.0290.002145.325.51.160.06120.0610.220.910.0010.001037.923.90.620.10130.0740.210.520.0010.001539.424.21.280.02140.0650.310.950.0310.000642.524.50.570.22150.0410.251.080.0090.002337.125.91.320.16160.0320.120.510.0150.000938.925.50.690.09170.0780.390.480.0190.000135.725.60.780.13Comparative180.0330.240.340.009(0.0050)38.723.80.640.13Examples190.0680.380.49(0.044)0.000636.025.30.800.11200.0320.470.990.0170.000837.325.10.890.2521(0.091)0.491.110.0210.000736.525.30.640.04220.0390.341.120.0360.002139.425.30.890.14230.0550.410.840.0290.001339.324.30.990.2124(0.008)0.230.400.0020.000437.524.41.300.5625(0.091)0.30(0.17)0.0270.001536.325.51.46(0) 260.0540.181.130.0010.001140.424.20.500.1827(0.006)0.431.100.0130.001938.525.00.480.08280.0550.270.770.0330.002238.125.20.790.09AlTiBCoNbNEvaluationExamples10.0120.080.00080.130.540.16◯20.0900.040.00180.030.480.19◯30.1240.060.00250.270.470.21◯40.0830.010.00230.170.550.17◯50.1310.050.00380.090.470.21◯60.04000.00140.040.460.29◯70.0860.030.00200.220.580.18◯80.0620.020.00350.080.590.22◯90.0540.010.00430.290.460.27◯100.0500.050.00220.090.530.18◯110.1030.060.00490.110.520.19◯120.03000.00130.050.510.23◯130.1410.010.00060.150.490.21◯140.0700.010.00200.070.460.25◯150.0180.020.00280.020.50.22◯160.0230.060.00090.210.480.24◯170.1110.090.00250.190.480.18◯Comparative180.0140.070.00160.190.570.20XExamples190.0510.03(0.0054)0.210.450.28X200.0400.010.00120.04(0.64)(0.35)X210.112(0.18)0.00400.270.460.21X220.0260.030.0024(0) 0.510.23X230.0300.050.00140.07(0.43)(0.05)X240.0710.020.00380.110.490.17X250.0730.01(0.0000)0.240.470.25X260.0150.05(0.0002)0.140.520.19X270.0920.020.00390.26(0.22)0.21X280.0310.040.0044(0.45)0.470.22X
[0052] Room temperature tensile strength was evaluated by producing a round bar test piece according to ASTM E8 in which longitudinal direction corresponds to direction perpendicular to rolling direction of the hot-rolled annealed steel plate, and by performing tensile test defined in ASTM E8 of this test piece so as to measure 0.2% proof stress and elongation. Samples of which 0.2% proof stress was not greater than 380 MPa and elongation was not less than 43.0% were evaluated as “⊚ (two concentric circles means superior)”, samples of which 0.2% proof stress was not greater than 390 MPa and elongation was not less than 42.0% were evaluated as “o (which means good)”, samples of which 0.2% proof stress was not greater than 400 MPa and elongation was not less than 40.0% were evaluated as “Δ (which means adequate)”, samples not satisfying 0.2% proof stress being not greater than 400 MPa and elongation being not less than 40.0% were evaluated as “x (which means inferior)”, and these are shown in Table 2.
[0053] High temperature tensile strength was evaluated by producing a round bar test piece according to ASTM E8 in which longitudinal direction corresponds to direction perpendicular to rolling direction of the hot-rolled annealed steel plate, and by performing high temperature tensile test at 1100 °F defined in ASTM E21 of this test piece so as to measure 0.2% proof stress and elongation. Samples of which 0.2% proof stress was not less than 160 MPa and elongation was not less than 60.0% were evaluated as “⊚”, samples of which 0.2% proof stress was not less than 150 MPa and elongation was not less than 55.0% were evaluated as “o”, samples of which 0.2% proof stress was not less than 140 MPa and elongation was not less than 50.0% were evaluated as “Δ”, samples not satisfying 0.2% proof stress being not less than 140 MPa and elongation being not less than 50.0% were evaluated as “x”, and they are shown in Table 2.
[0054] Average crystal grain diameter was evaluated as follows. The above hot-rolled annealed steel plate was cut, polished to a mirror surface, and etched electrolytically at 0.16 mA / mm2 using oxalic acid. The microscope test of this test piece was performed as defined in ASTM E112 by a comparison method. Samples satisfying −1 to 4 were evaluated as “⊚”, samples satisfying −2 to −5 were evaluated as “o”, samples satisfying −3 to 6 were evaluated as “Δ”, and samples not satisfying −3 to 6 were evaluated as “x”, and these are shown in Table 2.
[0055] Carbonitrides of NbN, NbC, TiN and TiC were evaluated as follows. The above-mentioned hot-rolled annealed steel plate was cut and mirror polished, and then, observation and composition analysis were performed by SEM-EDS. At 10,000 times of magnification, 100 fields of view were photographed and average of the number of carbonitrides among them was counted. Furthermore, the chemical composition was specified by EDS. Since carbonitrides down to 0.5 μm can be seen at this magnification, 0.5 μm is set to be the lower limit in the present invention. Samples of which the number of carbonitrides having longer diameter of 0.5 to 5 μm was 40 to 160 grains / mm2 on average and the number of carbonitrides having longer diameter of greater than 5 μm was 0 to 1.0 grains / mm2 on average were evaluated as “⊚”, samples of which the number of carbonitrides having longer diameter of 0.5 to 5 μm was 30 to 170 grains / mm2 on average and the number of carbonitrides having longer diameter of greater than 5 μm was greater than 1.0 to 3.0 grains / mm2 on average were evaluated as “o”, samples of which the number of carbonitrides having longer diameter of 0.5 to 5 μm was 20 to 180 grains / mm2 on average and the number of carbonitrides having longer diameter of greater than 5 μm was greater than 3.0 to 5.0 grains / mm2 on average were evaluated as “Δ”, samples of which the number of carbonitrides having longer diameter of 0.5 to 5 μm did not satisfy 20 to 180 grains / mm2 on average or the number of carbonitrides having longer diameter of greater than 5 μm was greater than 5.0 grains / mm2 on average were evaluated as “x”, and these are shown in Table 2.
[0056] As evaluation of the Formula 1, samples satisfying 0.130 to 0.140 were evaluated as “⊚”, samples satisfying 0.125 to 0.145 were evaluated as “o”, samples satisfying 0.120 to 0.150 were evaluated as “Δ”, and samples not satisfying 0.120 to 0.150 were evaluated as “x”, and these are shown in Table 3.
[0057] As evaluation of the Formula 2, samples satisfying 0.0030 to 0.0200% were evaluated as “⊚”, samples satisfying 0.0025 to 0.0300% were evaluated as “o”, samples satisfying 0.0020 to 0.0400% were evaluated as “Δ”, and samples not satisfying 0.0020 to 0.0400% were evaluated as “x” and these are shown in Table 3.
[0058] Distribution of precipitates of NbN, NbC, TiN, TiC and M23C6 was evaluated as follows. The above-mentioned hot-rolled annealed steel plate was cut and mirror polished, and then observation and composition analysis were performed by SEM-EDS. At 1,000 times magnification, 100 fields of view were photographed and distribution of average was measured. Furthermore, the chemical composition was specified by EDS. Samples of which ratio of precipitates precipitating at grain boundary was 15 to 25% were evaluated as “⊚”, samples of which ratio of precipitates precipitating at grain boundary was 12 to 28% were evaluated as “o”, samples of which ratio of precipitates precipitating at grain boundary was 10 to 30% were evaluated as “Δ”, samples of which ratio of precipitates precipitating at grain boundary does not satisfy 10 to 30% were evaluated as “x”, and these are shown in Table 3.
[0059] Hardness was evaluated as follows. The above-mentioned hot-rolled annealed steel plate was cut, and its surface was polished up to roughness No. #320. The Brinell hardness test using a super hard alloy ball defined in ASTM E10 was performed. Samples of which hardness was 150 to 190 were evaluated as “⊚”, samples of which hardness was 140 to 200 were evaluated as “o”, samples of which hardness was 130 to 210 were evaluated as “Δ”, samples of which hardness did not satisfy 130 to 210 were evaluated as “x”, and these are shown in Table 3.
[0060] As total evaluation, samples of which composition, room temperature 0.2% proof stress, room temperature elongation, high temperature 0.2% proof stress, high temperature elongation, average crystal grain size and the number of precipitates were evaluated as “⊚, o, Δ” as disclosed in claim 1 were evaluated as “o”, and samples of which at least one of the above items was evaluated as “x” was evaluated as “x”, and these are shown in Table 3.TABLE 2RoomHightemperatureRoomtemperatureHigh0.2% prooftemperature0.2% prooftemperaturestressElongationstressElongation(MPa)(%)Evaluation(MPa)(%)EvaluationExamples128665.6⊚14373.6Δ235046.5⊚19365.3⊚331556.3⊚18465.9⊚431848.7⊚15861.7◯528168.3⊚15570.1◯633949.5⊚19064.3⊚730759.4⊚17660.1⊚833753.6⊚20155.5◯938542.3◯20653.2Δ1027543.4⊚15088.5◯1132145.8⊚16980.3⊚1232054.3⊚18067.8⊚1339241.9Δ21359.5◯1429541.4Δ16255.5◯1530460.8⊚15173.4◯1633550.9⊚19869.6⊚1729963.9⊚17182.3⊚Comparative1836849.9⊚(121)(41.8)XExamples19346(37.6)X(119)(35.8)X20(421)55.5X167(39.7)X2138140.9Δ158(47.6)X2239757.1Δ(129)(49.1)X2333865.7⊚(113)59.8X2427149.8⊚(109)70.3X25(430)(35.7)X14860.3Δ2638652.8◯(131)71.3X2733442.8◯(134)57.1X2832562.5⊚199(43.5)XAverageAverageASTMnumber ofnumber ofCrystalcarbonitridescarbonitridesgrainof 0.5of moreparticleto 5 μmthan 5 μmsizeEvaluation(grains / mm2)(grains / mm2)EvaluationExamples1−3 Δ 360.3◯22⊚1302.8◯33⊚ 980.9⊚4−1 ⊚ 400.5⊚5−2 ◯ 560.7⊚63⊚1580.8⊚72⊚1232.2◯84⊚1633.9Δ96Δ1673.6Δ100⊚ 450.8⊚11−1 ⊚1112.1◯121⊚1403.3Δ134⊚1724.8Δ143⊚ 380.6◯150⊚ 771.1◯165◯1494.1Δ171⊚1511.7◯Comparative183⊚ 781.3◯Examples195◯ 590.4⊚20(8)X(220)(15.3)X21(7)X(198)2.5X222⊚ 981.6◯23(−5) X (10)0X24−1 ⊚1373.3Δ256Δ 280.2Δ261⊚1122.4◯27(−4) X (15)0.1X284⊚1002.5◯TABLE 3Ratio of precipitatesNb*N + Nb*C +precipitating atHardnessTotalTi*N + Ti*CEvaluationB + PEvaluationgrain boundary (%)EvaluationHBWEvaluationEvaluationExamples10.118X0.0018X33X126X◯20.135⊚0.0108⊚20⊚190⊚◯30.134⊚0.0135⊚22⊚153⊚◯40.113X0.0143⊚19⊚160⊚◯50.129◯0.0218◯20⊚138Δ◯60.149Δ0.0074⊚24⊚172⊚◯70.145◯0.0410X9X148◯◯80.161X0.0405X8X152⊚◯90.142◯0.0263◯26◯203Δ◯100.125◯0.0292◯15⊚128X◯110.139⊚0.0339Δ14◯181⊚◯120.148Δ0.0023Δ23⊚159⊚◯130.142◯0.0016X32X212X◯140.148Δ0.0330Δ10Δ162⊚◯150.136⊚0.0118⊚23⊚145◯◯160.147Δ0.0159⊚21⊚163⊚◯170.147Δ0.0215◯17⊚139Δ◯Comparative180.149Δ0.0106⊚24⊚185⊚XExamples190.167X0.0494X8X179⊚X200.248X0.0182⊚28◯149◯X210.193X0.0250◯29Δ155⊚X220.145◯0.0384Δ25⊚203ΔX230.050X0.0304Δ10Δ119XX240.091X0.0058⊚20⊚125XX250.164X0.0270◯13◯236XX260.139⊚0.0012X32X198◯X270.052X0.0169⊚11Δ160⊚X280.140⊚0.0374Δ20⊚175⊚XSince all of invention samples satisfied the range of the preset invention, they satisfied room temperature strength, high temperature strength, crystal grain size and the number of carbonitrides.
[0062] Since S was greater than the upper limit in Sample No. 18, too much sulfides were formed, and the sample did not satisfy the defined value of high temperature 0.2% proof stress and high temperature elongation.
[0063] Since B and P were greater than the upper limit in Sample No. 19, the grain boundary became brittle, and the sample did not satisfy the defined value of room temperature elongation, high temperature 0.2% proof stress and high temperature elongation. In addition, values of the Formulae 1 and 2 were greater than the upper limit, and the ratio of precipitates precipitating at a grain boundary did not satisfy the lower limit.
[0064] Since N and Nb were greater than the upper limit in Sample No. 20, too much nitrides were precipitated, and the sample did not satisfy the defined value of room temperature 0.2% proof stress, high temperature elongation, the number of precipitates and crystal grain size. In addition, the value of the Formula 1 was greater than the upper limit.
[0065] Since C and Ti were greater than the upper limit in Sample No. 21, too much carbides precipitated, and the sample did not satisfy the defined value of high temperature elongation, the number of precipitates and crystal grain size. In addition, the value of Formula 1 was greater than the upper limit.
[0066] Since Co did not satisfy the lower limit in Sample No. 22, high temperature strength was not increased, and the sample did not satisfy the defined value of high temperature 0.2% proof stress and high temperature elongation.
[0067] Since Nb and N did not satisfy the lower limit in Sample No. 23, nitrides were formed in small amount, and the sample did not satisfy the defined value of high temperature 0.2% proof stress, the number of precipitates, crystal grain size, and lower limit of hardness test. In addition, the value of the Formula 1 did not satisfy the lower limit.
[0068] Since C did not satisfy the lower limit in Sample No. 24, carbides were formed in small amount, and the sample did not satisfy the defined value of high temperature 0.2% proof stress. In addition, the value of the Formula 1 did not satisfy the lower limit. Cu is also greater than the upper limit, and the sample did not satisfy the lower limit of the hardness test.
[0069] Since C was greater than the upper limit and Cu was less than the lower limit in Sample No. 25, room temperature strength was high and the sample did not satisfy the defined value of room temperature 0.2% proof stress and room temperature elongation. Since B also did not satisfy the lower limit, the sample did not satisfy the defined value of high temperature 0.2% proof stress. In addition, the value of the Formula 2 did not satisfy the lower limit and the hardness test value was greater than the upper limit.
[0070] Since B did not satisfy the lower limit in Sample No. 26, the grain boundary was not strengthened, and the sample did not satisfy the defined value of high temperature 0.2% proof stress. In addition, the value of the Formula 2 did not satisfy the upper limit, and ratio of precipitates precipitating at grain boundary was low.
[0071] Since C and Nb did not satisfy the lower limit in Sample No. 27, carbides were formed in small amount, and the sample did not satisfy the defined value of high temperature 0.2% proof stress, the number of precipitates and crystal grain size. In addition, the value of the Formula 1 did not satisfy the lower limit.
[0072] Since Co was greater than the upper limit in Sample No. 28, the sample did not satisfy the defined value of high temperature elongation.
Claims
1. An Fe—Cr—Ni alloy consisting of:in mass %, C: 0.03 to 0.08%, Si:0.10 to 0.50%, Mn: 0.20 to 1.20%, P:0.001 to 0.040%, S: 0.0001 to 0.0030%, Ni: 35.5 to 45.5%, Cr:23.5 to 26.0%, Mo: 0.30 to 1.50%, Cu: 0.01 to 0.30%, Al:0.010 to 0.150%, Ti: not greater than 0.10%, B: 0.0005 to 0.0050%, Co: 0.02 to 0.30%, Nb: 0.45 to 0.60%, N: 0.15 to 0.30%, and Fe and inevitable impurities as the remainder, wherein0.2% proof stress value and elongation in room temperature tensile test which are defined in ASTM E8 satisfy not greater than 400 MPa and not less than 40.0%, respectively;0.2% proof stress value and elongation in high temperature tensile test at 1100 °F which are defined in ASTM E21 satisfy not less than 140 MPa and not less than 50.0%, respectively;average crystal grain size by microscope test as defined in ASTM E112 satisfies −3 to 6;in an arbitrarily chosen cross section, total sum of one or more kinds among NbN, NbC, TiN and TiC having longer diameter of 0.5 to 5 μm is reliably contained at 20 to 180 grains / mm2 on average; andin an arbitrarily chosen cross section, total sum of one or more kinds among NbN, NbC, TiN and TiC having longer diameter greater than 5 μm is alternatively contained at not greater than 5.0 grains / mm2 on average.
2. The Fe—Cr—Ni alloy according to claim 1, wherein each component in mass % is controlled to satisfy the following formula.0.120≤Nb×N+Nb×C+Ti×N+Ti×C≤0.1503. The Fe—Cr—Ni alloy according to claim 1, wherein each component in mass % is controlled to 0.0020%≤B+P≤0.0400%, and ratio of precipitates at grain boundary of total sum of one or more kinds among NbN, NbC, TiN, TiC and M23C6 having longer diameter of 0.5 to 5 μm in an arbitrarily chosen cross section is 10 to 30% in number ratio.
4. The Fe—Cr—Ni alloy according to claim 2, wherein each component in mass % is controlled to 0.0020%≤B+P≤0.0400%, and ratio of precipitates at grain boundary of total sum of one or more kinds among NbN, NbC, TiN, TiC and M23C6 having longer diameter of 0.5 to 5 μm in an arbitrarily chosen cross section is 10 to 30% in number ratio.
5. The Fe—Cr—Ni alloy according to claim 1, wherein the value in hardness test of Brinell hardness by a super hard alloy ball as defined in ASTM E10 is 130 to 210.
6. The Fe—Cr—Ni alloy according to claim 2, wherein the value in hardness test of Brinell hardness by a super hard alloy ball as defined in ASTM E10 is 130 to 210.
7. The Fe—Cr—Ni alloy according to claim 3, wherein the value in hardness test of Brinell hardness by a super hard alloy ball as defined in ASTM E10 is 130 to 210.
8. The Fe—Cr—Ni alloy according to claim 4, wherein the value in hardness test of Brinell hardness by a super hard alloy ball as defined in ASTM E10 is 130 to 210.