Catalyst for water electrolysis and preparing method thereof

A single-step laser-based method forms a carbon-based porous support with heterometallic particles, addressing the inefficiency of existing water electrolysis catalysts by enhancing electron mobility and surface area, leading to improved current density and reaction rates.

US20260357459A1Pending Publication Date: 2026-11-12PUSAN NAT UNIV IND UNIV COOPERATION FOUND
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
US19/669853
Authority / Receiving Office
US · United States
Patent Type
Applications(United States)
Current Assignee / Owner
Priority Date
2025-05-07
Filing Date
2026-05-06
Publication Date
2026-11-12

AI Technical Summary

Technical Problem

Existing water electrolysis technologies suffer from low energy conversion efficiency, and there is a need for more efficient catalysts to enhance this efficiency while reducing the reliance on scarce and costly metals like iridium and platinum.

Method used

A single-step method involving laser irradiation of a polyimide film coated with a solution containing metal precursors forms a carbon-based porous support and heterometallic particles, such as nickel-platinum or iron, to create a water electrolysis catalyst with improved electronic conductivity and specific surface area.

Benefits of technology

The method produces a catalyst with enhanced electron mobility and specific surface area, resulting in superior current density and reaction rates for water electrolysis, outperforming conventional single-metal catalysts.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure US20260357459A1-D00000_ABST
    Figure US20260357459A1-D00000_ABST
Patent Text Reader

Abstract

The present disclosure provides a method for producing a catalyst, and the catalyst thus produced, that can be used in a carbon-neutral oxygen evolution reaction such as water electrolysis. By irradiating the surface of a polyimide film coated with a solution containing nickel and iron precursors with a laser, a carbon-based porous support can be formed through carbonization of the polyimide film, and simultaneously, heterogeneous metal particles can be formed and immobilized on the porous support via photothermal reduction of nickel and iron, enabling the production of a simple catalyst with excellent activity for the oxygen evolution reaction.
Need to check novelty before this filing date? Find Prior Art

Description

CROSS-REFERENCE TO RELATED APPLICATION

[0001] The present application claims priority under 35 U.S.C. § 119 (a) to Korean Patent Application No. 10-2025-0059066 filed in the Korean Intellectual Property Office on May 7, 2025, which is incorporated herein by reference in its entirety.TECHNICAL FIELD

[0002] The present disclosure relates to a catalyst for water electrolysis and a method for producing the same.BACKGROUND OF THE INVENTION

[0003] Water electrolysis can be divided into the oxygen evolution reaction (Oxygen Evolution Reaction; OER) and the hydrogen evolution reaction (Hydrogen Evolution Reaction; HER). The oxygen evolution reaction and the hydrogen evolution reaction each refer to the processes that generate oxygen and hydrogen, respectively, through the electrochemical dissociation of water molecules and can occur at the anode (anode) and cathode (cathode), respectively. The oxygen evolution reaction and the hydrogen evolution reaction can be used in energy storage and conversion systems such as fuel cells, metal-air batteries, and water electrolysis devices, and are attracting attention in the renewable energy field. Water electrolysis uses water as the reactant and applies electricity to split it into hydrogen and oxygen, corresponding to an environmentally friendly oxygen evolution reaction without carbon emissions. However, because water electrolysis does not have high energy conversion efficiency, various attempts are being made to use more catalysts to improve the energy conversion efficiency of water electrolysis while increasing oxygen evolution.

[0004] Various materials that include metals or metal-carbon composites have been studied as catalysts for oxygen evolution reactions and hydrogen evolution reactions. Traditionally, iridium, platinum, iron, nickel, cobalt, and others have been used as metal components of oxygen evolution and hydrogen evolution catalysts. Iridium and platinum are known to exhibit excellent performance in increasing oxygen and hydrogen evolution rates and current densities, but their scarcity and high cost have prompted numerous attempts to replace them. Carbon materials with high electronic conductivity can be used as supports or carriers for metal materials, and efforts are being made to maximize the electronic conductivity and specific surface area of such carbon materials to enhance the overall catalyst performance.SUMMARY OF THE INVENTIONProblem to be Solved

[0005] The purpose of the present disclosure is to provide a single-step method for producing a water electrolysis catalyst that forms a carbon-based porous support while simultaneously forming a heterometallic catalyst particle that can be loaded onto the support, and the catalyst thus produced.Means for Solving the Problem

[0006] One example of the present disclosure relates to a method for producing a water electrolysis catalyst, comprising a step of irradiating a laser onto the surface of a polyimide film coated with a solution containing a first metal precursor and a second metal precursor.

[0007] The coating may comprise applying the solution to the surface of a polyimide film having a thickness of 50 to 150 μm.

[0008] The solution may have the concentration of the first metal precursor and the concentration of the second metal precursor each independently being 1 to 25 mM.

[0009] The first metal is nickel, the second metal is platinum or iron, and the solution may contain the first metal and the second metal in a molar ratio of 3:1 to 1:3.

[0010] The solution may include diethylene glycol as a solvent.

[0011] The laser irradiation may comprise irradiating a CO2 laser at an output of 5 to 15 W.

[0012] The water electrolysis catalyst according to an example of the present disclosure comprises a porous support containing a carbon sheet and heterogeneous metal particles supported on the surface of said porous support, wherein the heterogeneous metal particles include a first metal of nickel and a second metal of platinum or iron.

[0013] The carbon sheet may be a graphene sheet having a thickness of 1 to 10 nm. The heterometallic particles may have an average particle diameter (D50) of 1 to 9 nm. The heterometallic particles may comprise the first metal and the second metal in a molar ratio of 3:1 to 1:3.

[0014] One example of the present disclosure provides a water electrolysis apparatus comprising a water electrolysis catalyst of any example of the present disclosure.Effect of the Invention

[0015] The manufacturing method of the present disclosure, through laser irradiation, simultaneously produces a carbon-based porous support with high electron mobility and large specific surface area, and by reducing metals present in precursor form, can form heterometallic particles, thereby allowing simple fabrication of water electrolysis catalysts.BRIEF DESCRIPTION OF THE DRAWINGS

[0016] FIG. 1 is a schematic diagram showing a method for producing a water electrolysis catalyst according to an example of the present disclosure.

[0017] FIG. 2 is the SEM image of the catalyst prepared in Example 1 at various magnifications (2.00 k×, 25.0 k×, 100.0 k×).

[0018] FIG. 3 is a graph showing the potential required to achieve a current density when a cell is constructed using the catalyst prepared in Example 1 and Comparative Example.

[0019] FIG. 4 is a graph showing the potential required to achieve a current density when a cell is constructed using the catalyst prepared in Example 2 and the comparative example.

[0020] FIG. 5 is a graph showing the hydrogen sensor voltage when a voltage is applied to a two-electrode cell containing the catalyst prepared in the example.DETAILED DESCRIPTION OF THE INVENTION

[0021] Hereinafter, each example of the present disclosure is described in greater detail so that a person of ordinary skill in the art to which the disclosure pertains can readily practice it; however, this is merely an example and the scope of the present disclosure is not limited by the following content.

[0022] The term “including” as used in this specification is employed when listing materials, compositions, devices, and methods useful in the present disclosure and is not limited to the enumerated examples.

[0023] One example of the present disclosure provides a method for preparing a water-electrolysis catalyst comprising a step of irradiating the surface of a polyimide film coated with a solution containing a first metal precursor and a second metal precursor with a laser. The water-electrolysis catalyst includes heterometallic particles comprising the first metal and the second metal, and a carbon-based porous support that carries the heterometallic particles. The water electrolysis catalyst may refer to an oxygen-evolution-reaction catalyst, a hydrogen-evolution-reaction catalyst, or a combination thereof.

[0024] The polyimide film may be used to produce the carbon-based porous support. The porous support may include a carbon sheet. Preferably, the carbon sheet may be a graphene sheet. The porous support formed by irradiating the polyimide film with a laser may include laser-induced graphene (Laser Induced Graphene; LIG).

[0025] The polyimide film may have a thickness of 50 to 150 μm. A commercially available polyimide film may be used. Specifically, the thickness of the polyimide film may be 50 μm or more, 60 μm or more, 70 μm or more, 80 μm or more, 90 μm or more, 100 μm or more, 110 μm or more, 120 μm or more, 130 μm or more, 140 μm or more, or 150 μm or less, 140 μm or less, 130 μm or less, 120 μm or less, 110 μm or less, 100 μm or less, 90 μm or less, 80 μm or less, 70 μm or less, 60 μm or less. Within the above ranges, the formation of laser-induced graphene by laser irradiation and the photothermal reduction of metal precursors can be simultaneously achieved, and heterogeneous metal particles formed by such photothermal reduction can be deposited on the surface of a porous support containing the laser-induced graphene. Moreover, graphene sheets containing laser-induced graphene produced within the above range have high electronic conductivity and specific surface area, thereby contributing to improved energy conversion efficiency of water electrolysis reactions.

[0026] The solution comprising the first metal precursor and the second metal precursor may be coated onto the surface of the polyimide film while maintaining a uniform dispersion of each precursor. The first metal and the second metal derived from the precursors can be reduced by laser irradiation to form alloy particles. Each precursor may include a chloride, nitride, sulfide, or phosphide of the first metal or the second metal, but is not limited to these. The solution may contain diethylene glycol as a solvent. The solvent may evaporate and be removed during the laser irradiation process.

[0027] The solution may contain the concentration of the first metal precursor and the concentration of the second metal precursor each independently in the range of 1 to 25 mM. Specifically, the concentration of the first metal or second metal precursor in the solution may be at least 1 mM, at least 5 mM, at least 10 mM, at least 15 mM, at least 20 mM, or at most 25 mM, at most 20 mM, at most 15 mM, at most 10 mM. By coating the surface of the polyimide film with a solution satisfying the aforementioned concentration ranges and performing laser irradiation, heterogeneous metal particles having particle diameters within the range to be described later can be formed. If the ranges described above are exceeded, control of the heterogeneous metal particle size becomes difficult, or the catalytic activity for water electrolysis may be reduced due to an increase in heterogeneous metal particle size. Preferably, the solution may contain the first metal precursor and the second metal precursor combined in a concentration of 5 to 25 mM.

[0028] The first metal is nickel, and the second metal may be platinum or iron. The solution may contain the first metal and the second metal in a molar ratio of 3:1 to 1:3. Such a molar ratio can be achieved by adjusting the amount of the precursor. A nickel-iron heterometallic particle manufactured using a solution satisfying this molar ratio, and a catalyst comprising it, can exhibit a higher current density than a catalyst containing nickel or iron alone, or a heterometallic particle outside the aforementioned range.

[0029] Coating the polyimide film with the solution may mean applying the solution to at least a portion of the surface of the polyimide film. For example, the coating may involve applying a solution having a concentration of 1 to 25 mM of the first metal precursor or the second metal precursor to the surface of a polyimide film having a thickness of 50 to 150.

[0030] The laser irradiation may be performed with a CO2 laser at an output of 5 to 15 W. Specifically, the output of the CO2 laser may be 5 W or more, 7 W or more, 9 W or more, 11 W or more, 13 W or more, or 14 W or less, 12 W or less, 10 W or less, 8 W or less, 6 W or less. Preferably, the laser output may be from 5 W to 12 W. A laser within the aforementioned output range may be directed directly onto a polyimide film coated with the solution, thereby reducing the metals contained in the solution to form heterogeneous metal particles while simultaneously carbonizing the polyimide film. Through CO2 laser irradiation within the stated output range, the photon energy of the laser is converted to thermal energy in the polyimide film, causing the polyimide to carbonize and forming laser-induced graphene. Specifically, the laser irradiation continuously induces thermal deformation, expansion, volatilization, and rearrangement of the conductive sp2 carbon structure of the polyimide film to form graphene. Compared with conventional carbon-material synthesis methods that use chemical reagents, this laser irradiation is faster and easier, and can form carbon-based porous supports under relatively low-temperature and low-pressure conditions. The laser-induced graphene can exhibit thermal stability even at temperatures above 900 °C and display excellent electrical conductivity of 25 S / cm or greater. Graphene sheets formed by laser irradiation within the described output range may possess nanocrystallinity. Such nanocrystalline graphene sheets and the three-dimensional porous supports comprising them can enhance catalytic performance.

[0031] The laser irradiation can thermally reduce the metals to form alloyed heterometallic particles without further altering the shape and structure of the laser-induced graphene being formed. Simultaneously with the formation of crystalline graphene sheets by the laser irradiation, the metals can form heterometallic particles in a dispersed state on the surface of the crystalline graphene sheets, thereby enhancing the water electrolysis reactivity of the produced catalyst.

[0032] The method for producing the oxygen-evolving catalyst adjusts the concentration of the polyimide film and metal precursor used, as well as the laser power, thereby achieving the fabrication of a carbon-based porous support via carbonization of the polyimide film and the formation of heterogeneous metal particles through metal reduction, all with a single-step laser irradiation. This manufacturing method applies a one-step laser irradiation, and the single step can take less than 30 seconds. Specifically, the single step can take less than 30 seconds, less than 25 seconds, less than 20 seconds, or at least 15 seconds, at least 20 seconds, at least 25 seconds. Compared with multi-step methods involving separate preparation of the catalyst support and catalyst and the loading of the catalyst onto the support, this method is simpler and reduces the required time.

[0033] The present disclosure's example provides a porous support comprising a carbon sheet, and a water electrolysis catalyst comprising heterogeneous metal particles deposited on the surface of the porous support. The catalyst may be manufactured according to the manufacturing method of an example of the present disclosure, and the description identical to that in the manufacturing method is substituted with the description of the preceding example.

[0034] The porous support may include a carbon sheet and have a plurality of pores communicating in three dimensions. The carbon sheet may be a graphene sheet having a thickness of 1 to 10 nm. The graphene sheet may include laser-induced graphene, and, in particular, may be composed of laser-induced graphene. The carbon sheet may have a thickness of at least 1 nm, at least 2 nm, at least 3 nm, at least 4 nm, at least 5 nm, at least 6 nm, at least 7 nm, at least 8 nm, at least 9 nm, or ≤10 nm, ≤9 nm, ≤8 nm, ≤7 nm, ≤6 nm, ≤5 nm, ≤4 nm, ≤3 nm, ≤2 nm. A graphene sheet satisfying the above ranges can provide an electron mobility of approximately 200,000 cm2·V−1·s−1 or greater and a specific surface area of 2,000 m2·g−1 or greater, thereby improving the energy conversion efficiency of water-electrolysis catalysts. The porous support, comprising a carbon sheet satisfying the above thickness range, may have an average pore diameter of 1 to 10 times.

[0035] The heterogeneous metal particles may be alloy nanoparticles having an average particle size (D50) of 1 to 9 nm. The average particle size of the heterogeneous metal particles can be derived by programmatically analyzing the microscopic images of the produced catalyst. A catalyst comprising heterogeneous metal particles that satisfy the aforementioned range can be supported on a porous carrier possessing the previously described electronic mobility and specific surface area characteristics, thereby further enhancing the activity for oxygen evolution reactions.

[0036] The heterogeneous metal particles may comprise a first metal and a second metal in a molar ratio of 3:1 to 1:3. For example, when the heterogeneous metal particles include nickel and iron, nickel and iron may be present in a molar ratio of 1:1 to 1:3. For example, when the heterogeneous metal particles include nickel and platinum, nickel and platinum may be present in a molar ratio of 2:1 to 1:1, or 1.6:1 to 1:1. A catalyst containing heterogeneous metal particles that satisfy the above ranges may exhibit a higher current density compared with a catalyst containing single-metal particles of the first metal or the second metal.

[0037] The water electrolysis catalyst, by including heterometal particles, can achieve economical yet superior current density compared with conventional single-metal catalysts based on precious metals such as platinum, and by forming the heterometal particles on a carbon sheet containing laser-induced graphene, it can enhance the rate of the water electrolysis reaction based on rapid charge transport.

[0038] In the following, the present disclosure will be described in more detail through specific examples and experimental examples. The following examples and experimental examples are provided as illustrations of the present disclosure, and the present disclosure is not limited by these examples and experimental examples.Example 1-1. One-Step Preparation of a Catalyst for Oxygen Evolution Reaction

[0039] At room temperature, nickel chloride hexahydrate (NiCl2·6H2O) as the nickel precursor and iron chloride hexahydrate (FeCl3·6H2O) as the iron precursor were added to diethylene glycol (DEG, 99%) to achieve a concentration of 5 mM, with the molar ratio of nickel to iron set to 1:3, preparing a total of 40 μL of solution.

[0040] The commercially available polyimide film (thickness 10) was cut to a size of 10 mm×10 mm, then after immersing the polyimide film in the solution and removing it, laser irradiation was performed for 30 seconds at atmospheric pressure using a CO2 laser system (BC-GTC 6040B-RD 80W) with a laser output of 7.2 W and a scan speed of 250 mm / s (laser wavelength 10.6, scan mode), thereby producing an oxygen evolution reaction catalyst (hereinafter referred to as “Fe3Ni-LIG”).Example 1-2

[0041] When preparing the precursor solution, except for adjusting the molar ratio of nickel to iron to 1:1, the oxygen evolution reaction catalyst (hereinafter referred to as “FeNi-LIG”) was prepared by the same method as in the above examples.Examples 1-3

[0042] Except for adjusting the molar ratio of nickel to iron to 3:1 when preparing the precursor solution, the oxygen evolution reaction catalyst (hereinafter referred to as “FeNi3-LIG”) was prepared by the same method as described in the above example.Comparative Example 1-1

[0043] When preparing the precursor solution, except when a nickel precursor is not used, the oxygen evolution reaction catalyst (hereinafter referred to as “Fe-LIG”) was prepared by the same method as described in the above example.Comparative Example 1-2

[0044] When preparing the precursor solution, except for cases where an iron precursor is not used, the oxygen evolution reaction catalyst (hereinafter referred to as “Ni-LIG”) was prepared by the same method as described in the above example.Example 2-1. One-Step Preparation of a Catalyst for Hydrogen Evolution Reaction

[0045] At room temperature, add nickel precursor nickel chloride hexahydrate (NiCl2·6H2O) and platinum precursor hexachloroplatinic acid hydrate (H2PtCl6·6H2O) to diethylene glycol (DEG, 99%) to achieve a concentration of 5 mM, with the molar ratio of nickel to platinum set to 1:3, preparing a total of 10 mL of solution.

[0046] The commercially available polyimide film (thickness 10 μm) was cut to a size of 10 mm×10 mm, immersed in the solution, removed, and then, at atmospheric pressure, irradiated with a CO2 laser system (BC-GTC 6040B-RD 80W) at a laser output of 11.2 W and a scan speed of 250 mm / s (laser wavelength 10.6 μm, scan mode) for 30 seconds to produce a hydrogen evolution reaction catalyst (hereinafter referred to as “Pt3Ni-LIG”).Example 2-2

[0047] When preparing the precursor solution, except for adjusting the Ni-to-Pt molar ratio to 1:1, the hydrogen evolution reaction catalyst (hereinafter referred to as “PtNi-LIG”) was prepared by the same method as Example 2-1.Example 2-3

[0048] During the preparation of the precursor solution, except for adjusting the molar ratio of nickel to platinum to 3:1, the hydrogen evolution reaction catalyst (hereinafter referred to as “PtNi3_LIG”) was prepared by the same method as Example 2-1 in the preceding experiment.Comparative Example 2

[0049] Except when a nickel precursor is not used, the hydrogen evolution reaction catalyst (hereinafter referred to as “Pt-LIG”) was prepared by the same method as the above example 2-1 during the preparation of the precursor solution.Experimental Example 1. Verification of Catalyst Physical Properties

[0050] The surface morphology of the catalyst prepared in Example 1 was analyzed by scanning electron microscopy (SEM, Mira 3, Tescan) and shown in FIG. 2.

[0051] Referring to FIG. 2, a porous support composed of laser-induced graphene was synthesized, and it was confirmed that heterogeneous metal particles of nickel and iron were deposited on its surface. Analysis of the SEM images with the ImageJ program showed that the average particle size of the heterogeneous metal particles was 4.5 nm.Experimental Example 2. Evaluation of Catalyst Performance

[0052] The electrochemical performance of a catalyst for the oxygen evolution reaction can be evaluated by comparing the magnitude of overpotential required to achieve a specific current density. Specifically, the catalyst performance was assessed using a potentiostat (VSP, Biologic) configured in a three-electrode system. A Pt wire (CE-100, EC Frontier) and a Hg / HgO (20% KOH) electrode (RE-61AP, ALS) were used as the counter electrode and reference electrode, respectively, and the catalyst from Example 1 or Comparative Example 1 was employed as the working electrode, with 1 M KOH as the electrolyte. Using this three-electrode system, linear sweep voltammetry (LSV) was performed from +1.1 V to +1.9 V at a scan rate of 5 mV / s versus the reversible hydrogen electrode (RHE), and the results for each catalyst are shown in FIG. 3.

[0053] Based on the LSV curves for each catalyst, the overpotential at 10 mA / cm2 or 50 mV cm2 was determined and presented in Table 1 below.TABLE 1Overpotential (mV)Overpotential (mV)catalystbased on 10 mA / cm2based on 50 mA / cm2Comparative Example l-l (Fe-LIG)521—Example l-1 (Fe3Ni-LIG)408560Example l-2 (FeNi-LIG)400612Example l-3 (FeNi3-LIG)439611Comparative example l-2 (Ni-LIG)539—

[0054] At 50 mA / cm2, the comparative catalysts exhibited difficulty in measuring overpotential, whereas the exemplified catalysts required a lower overpotential level to achieve the same current density compared to the comparative catalysts, confirming superior activity relative to single-metal-based catalysts.]

[0055] Using a similar method, the electrochemical performance of the catalysts for the hydrogen evolution reaction was evaluated by overpotential. In Example 2 and Comparative Example, the catalysts were used as the working electrode, and a three-electrode system with 1 M KOH as the electrolyte was employed; linear sweep voltammetry (LSV) was performed from +0.1 V to −0.9 V at a scan rate of 5 mV / s versus the reversible hydrogen electrode (RHE), and the results for each catalyst are shown in FIG. 4.

[0056] Based on the LSV curves for each catalyst, the overpotential at 10 mA / cm2 was determined and presented in Table 2 below.TABLE 2Overpotential (mV)catalystbased on 10 mA / cm2Comparative Example 2 (Pt-LIG)204Example 2-1 (Pt3Ni-LIG)117Example 2-2 (PtNi-LIG)216Example 2-3 (PtNi3-LIG)252Comparative Example l-2 (Ni-LIG)332

[0057] In the examples, the catalysts were found to exhibit superior activity compared to single-metal-based catalysts, as they require a lower overpotential to achieve the same current density relative to comparative catalysts.Experimental Example 3. Confirmation of Hydrogen Generation

[0058] A homemade gas collection device equipped with a digital hydrogen sensor was fabricated, and the collection of generated hydrogen gas was verified by the water displacement method. A rubber tube was connected to the portion of the catalyst-containing electrode where the electrode was immersed in a water-filled cell, which is expected to produce hydrogen. The catalyst fabricated in Example 2-2 was immersed in water on the hydrogen-generating electrode side, and the digital hydrogen sensor was placed on the upper side so as not to come into contact with water. By varying the voltage applied to the two-electrode cell, the gas collected in the mass cylinder through the rubber tube was monitored.

[0059] The hydrogen concentration in the gas was monitored as a digital signal by the hydrogen sensor, and the voltage of the hydrogen sensor (Hydrogen sensing voltage) was measured for each applied external voltage of 1.8 V, 2.0 V, and 2.2 V and shown in FIG. 5. Referring to FIG. 5, when an external voltage of 1.8 V was applied, the hydrogen sensor voltage increased from 0.75 V to 0.97 V; when 2.0 V was applied, it increased from 0.8 V to 1.22 V; and when 2.2 V was applied, it increased from 0.74 V to 1.26 V. These results are consistent with the expectation that a higher applied voltage leads to a greater generation of hydrogen gas and consequently a higher hydrogen-sensor voltage due to hydrogen detection.

Claims

1. A method for manufacturing a water electrolysis catalyst, comprising: coating a surface of a polyimide film and irradiating a laser onto the surface of the polyimide film coated with a solution containing a first metal precursor and a second metal precursor.

2. The method of claim 1, wherein the coating comprises applying the solution to the surface of the polyimide film having a thickness of 50 to 150 μm.

3. The method of claim 1, wherein a concentration of the first metal precursor and a concentration of the second metal precursor in the solution are each independently 1 to 25 mM.

4. The method of claim 1, wherein a first metal is nickel, a second metal is platinum or iron, and the solution comprises the first metal and the second metal in a molar ratio of 3:1 to 1:3.

5. The method of claim 1, wherein the solution comprises diethylene glycol as a solvent.

6. The method of claim 1, wherein the irradiating comprises irradiating a CO2 laser at an output of 5 to 15 W.

7. A water electrolysis catalyst, comprising: a porous support comprising a carbon sheet; andheterometallic particles supported on a surface of the porous support,wherein the heterometallic particles comprise nickel as a first metal and platinum or iron as a second metal.

8. The water electrolysis catalyst of claim 7, wherein the carbon sheet is a graphene sheet having a thickness of 1 to 10 nm.

9. The water electrolysis catalyst of claim 7, wherein the heterometallic particles have an average particle diameter (D50) of 1 to 9 nm.

10. The water electrolysis catalyst of claim 7, wherein the heterometallic particles comprise the first metal and the second metal in a molar ratio of 3:1 to 1:3.