Methods for preparing regenerated cellulose fibers

WO2024169031A9PCT designated stage expired Publication Date: 2024-11-14THE HONG KONG RES INST OF TEXTILES & APPAREL
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
PCT/CN2023/087924
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-02-15
Filing Date
2023-04-12
Publication Date
2024-11-14

Smart Images

  • Figure CN2023087924_14112024_PF_FP_ABST
    Figure CN2023087924_14112024_PF_FP_ABST
Patent Text Reader

Abstract

A method of preparing a regenerated bacterial cellulose fiber, the method including: contacting bacterial cellulose powder with an aqueous solution including a quaternary ammonium hydroxide and optionally urea under conditions that result in the dissolution of at least a portion of the bacterial cellulose powder thereby forming a cellulose dope including bacterial cellulose; or contacting bacterial cellulose powder with an aqueous solution including a metal complex under conditions that result in the dissolution of at least a portion of the bacterial cellulose powder thereby forming a cellulose dope including bacterial cellulose; and extruding the cellulose dope in a coagulation bath thereby forming the regenerated bacterial cellulose fiber.
Need to check novelty before this filing date? Find Prior Art

Description

METHODS FOR PREPARING REGENERATED CELLULOSE FIBERS

[0001] CROSS-REFERENCE TO RELATED APPLICATIONS

[0002] This application claims priority from U.S. Provisional Patent Application Number 63 / 485,028, filed on February 15, 2023, the content of which is hereby incorporated by reference in its entirety.TECHNICAL FIELD

[0003] The present disclosure generally relates to methods for preparing regenerated cellulose fibers from bacterial cellulose powder produced during kombucha fermentation.BACKGROUND

[0004] Cellulose-based materials obtained from wood, cotton, and bamboo have been widely used for thousands of years as materials for paper, construction, energy, textiles, and furniture. Cotton fibers and wood-based regenerated cellulose fibers are the most common type of cellulosic fiber in textile industry. However, cellulosic fiber exhibit certain disadvantages.

[0005] Cotton is a natural plant fiber, which grows around the seeds of the cotton plant. Cotton fiber is obtained from the cotton plant and then spun into yarn. From there, the cotton yarn is woven or knitted into fabric. According to the World Wildlife Fund, cotton’s most prominent environmental impacts result from the use of pesticides, high consumption of water, and high land space requirement.

[0006] Regenerated cellulosic fibers can be made from cellulose that is extracted from wood pulp, which is then chemically dissolved, and extruded as a continuous filament.

[0007] Conventional processes for preparing regenerated cellulose fiber commonly involve toxic chemicals and / or by products.

[0008] [Rectified under Rule 91, 19.07.2024]For example, the Kraft process, which is generally employed to prepare regenerated cellulosic fibers, can be highly polluting as H2S is used to break the bonding between lignin, hemicellulose, and cellulose as illustrated in Figure 1.

[0009] [Rectified under Rule 91, 19.07.2024]In another example, viscose is produced by reacting cellulose with sodium hydroxide to form alkali cellulose, which in turn, is reacted with highly toxic carbon disulfide to form cellulose xanthate, which is then dissolved in dilute sodium hydroxide and extruded as regenerated cellulose fiber as illustrated in Figure 2.

[0010] New methods for preparing regenerated cellulosic fibers are thus needed, which avoid the use of polluting chemicals used in conventional methods.

[0011] Kombucha is a fermented tea, which has increased in popularity in recent years due in part to the belief that its consumption eliminates toxins, boosts energy, strengthens the immune system, and helps with weight loss. In 2021, the global kombucha market size was valued at USD 2.64 billion and is expected to expand at a compound annual growth rate of 15.6%from 2022 to 2030.

[0012] [Rectified under Rule 91, 19.07.2024]Symbiotic colony of bacteria and yeast (SCOBY) pellicle is a gelatinous biofilm formed during the process of making kombucha that comprises bacterial cellulose as shown in Figure 3. Kombucha bacterial cellulose is free from other biopolymers, such as lignin, hemicellulose, and pectin. It has high purity, high degree of polymerization (DP) and high crystallinity making SCOBY pellicle an attractive alternative source for cellulosic fiber production.

[0013] There still exists a need for improved methods for producing and isolating bacterial cellulose fibers from kombucha SCOBY pellicle.

[0014] SUMMARY

[0015] [Rectified under Rule 91, 19.07.2024]In the present disclosure, bacterial cellulose, using the SCOBY pellicle produced as the side stream of Kombucha fermentation, is developed as sustainable source for regenerated cellulose fibers production. The methods described herein address several challenges, such as (1) the development of solvent systems for dissolving bacterial cellulose efficiently; and (2) optimizing conditions for the wet spinning of regenerated bacterial cellulose fiber as illustrated in Figure 5. Bacterial cellulose with high purity, high degree of polymerization and high crystallinity can be utilized as alternative source for cellulosic fiber production. The advantages of the methods described herein include, but are not limited to fast growth rate of the SCOBY pellicle and bacterial cellulose fiber included therein, pesticide and toxic chemical free, and low water requirements.

[0016] In a first aspect, provided herein is a method of preparing a regenerated bacterial cellulose fiber, the method comprising: contacting bacterial cellulose powder with an aqueous solution comprising a quaternary ammonium hydroxide and optionally urea under conditions that result in the dissolution of at least a portion of the bacterial cellulose powder thereby forming a cellulose dope comprising bacterial cellulose; or contacting bacterial cellulose powder with an aqueous solution comprising a metal complex under conditions that result in the dissolution of at least a portion of the bacterial cellulose powder thereby forming a cellulose dope comprising bacterial cellulose; and extruding the cellulose dope in a coagulation bath thereby forming the regenerated bacterial cellulose fiber.

[0017] In certain embodiments, the bacterial cellulose powder is a kombucha bacterial cellulose powder.

[0018] In certain embodiments, the quaternary ammonium hydroxide is NR4OH, wherein R for each instance is independently alkyl, cycloalkyl, or phenyl; and the metal complex comprises a metal selected from the group consisting of aluminum, calcium, copper, iron, nickel, and zinc.

[0019] In certain embodiments, the quaternary ammonium hydroxide is tetramethylammonium hydroxide, tetraethylammonium hydroxide, tetrapropylammonium hydroxide, or tetrabutylammonium hydroxide; and the metal complex is bis(ethylenediamine) copper (II) hydroxide.

[0020] In certain embodiments, the quaternary ammonium hydroxide is present in the aqueous solution at a concentration between 20-60%w / w; and the metal complex is present in the aqueous solution at a concentration between 0.5 to 2M.

[0021] In certain embodiments, the urea is present in the aqueous solution at a concentration of 0.1-0.5%w / w.

[0022] In certain embodiments, the coagulation bath comprises a primary drawing bath and further comprises a secondary drawing bath.

[0023] In certain embodiments, the primary drawing bath and the secondary drawing bath each independently have a pH between 0-1.

[0024] In certain embodiments, the primary drawing bath and the secondary drawing bath each comprises an aqueous solution of H2SO4 and optionally Na2SO4.

[0025] In certain embodiments, the concentration of H2SO4 in each of the primary drawing bath and the secondary drawing bath is independently 0.25 M to 1 M.

[0026] In certain embodiments, the cellulose dope comprises the bacterial cellulose at a concentration between 2-10%w / w.

[0027] In certain embodiments, the method further comprises: providing a symbiotic colony of bacteria and yeast (SCOBY) pellicle; contacting the SCOBY pellicle with an alkaline aqueous solution thereby forming a treated SCOBY pellicle; optionally washing and drying the treated SCOBY pellicle; and powdering the treated SCOBY pellicle thereby forming the bacterial cellulose powder.

[0028] In certain embodiments, the method further comprises: washing the regenerated bacterial cellulose fiber with water and drying the washed regenerated bacterial cellulose fiber.

[0029] In certain embodiments, the conditions that result in the dissolution of at least a portion of the bacterial cellulose powder comprise: maintaining the aqueous solution comprising the quaternary ammonium hydroxide and optionally urea at 25-50℃ for 8 to 24 h; or maintaining the aqueous solution comprising the metal complex at 75-90 ℃ for 1 to 2 h.

[0030] In certain embodiments, the method comprises: contacting bacterial cellulose powder with an aqueous solution comprising between 20-60%w / w N (C1-C5) 4OH and optionally 0.1-0.5%w / w urea at 25-40℃ for 8 to 24 h resulting in the dissolution of at least a portion of the bacterial cellulose powder thereby forming a cellulose dope comprising bacterial cellulose at a concentration of between 4-10%w / w; or contacting bacterial cellulose powder with an aqueous solution comprising 0.5 M to 2 M bis(ethylenediamine) copper (II) hydroxide at 75-90 ℃ for 1 to 2 h resulting in the dissolution of at least a portion of the bacterial cellulose powder thereby forming a cellulose dope comprising the bacterial cellulose at a concentration of between 2-6%w / w; and extruding the cellulose dope in a coagulation bath comprising a primary drawing bath and a secondary drawing bath, wherein the primary drawing bath and the secondary drawing bath independently have a pH between 0-0.5 thereby forming the regenerated bacterial cellulose fiber.

[0031] In certain embodiments, the cellulose dope comprises bacterial cellulose at a concentration of between 3.5-5.5%w / w.

[0032] In certain embodiments, the method further comprises: providing a symbiotic colony of bacteria and yeast (SCOBY) pellicle; contacting the SCOBY pellicle with an alkaline aqueous solution thereby forming a treated SCOBY pellicle; optionally washing and drying the treated SCOBY pellicle; and powdering the treated SCOBY pellicle thereby forming the bacterial cellulose powder.

[0033] In certain embodiments, the alkaline aqueous solution has pH of 13-14.

[0034] In certain embodiments, the alkaline aqueous solution comprises NaOH.

[0035] In certain embodiments, the method comprises: providing a symbiotic colony of bacteria and yeast (SCOBY) pellicle; contacting the SCOBY pellicle with an alkaline aqueous solution having a pH of 13-13.5 thereby forming a treated SCOBY pellicle; optionally washing and drying the treated SCOBY pellicle; powdering the treated SCOBY pellicle thereby forming the bacterial cellulose powder; contacting bacterial cellulose powder with an aqueous solution comprising between 20-60%w / w N (C1-C5) 4OH and optionally 0.1-0.5%w / w urea at 25-40℃ for 8 to 24 h resulting in the dissolution of at least a portion of the bacterial cellulose powder thereby forming a cellulose dope comprising bacterial cellulose at a concentration of between 3.5-5.5%w / w; or contacting bacterial cellulose powder with an aqueous solution comprising 0.5 M to 2 M bis (ethylenediamine) copper (II) hydroxide at 75-90 ℃ for 1 to 2 h resulting in the dissolution of at least a portion of the bacterial cellulose powder thereby forming a cellulose dope comprising the bacterial cellulose at a concentration of between 3.5-5.5%w / w; and extruding the cellulose dope in a coagulation bath comprising a primary drawing bath and a secondary drawing bath, wherein the primary drawing bath and the secondary drawing bath each comprise an aqueous solution of H2SO4 and Na2SO4 at a pH between 0-0.5 thereby forming the regenerated bacterial cellulose fiber.

[0036] The methods disclosed herein can comprise one of three different bacterial cellulose powder dissolution methods:

[0037] 1. Quaternary ammonium hydroxide (QAH) aqueous solvent system QAH solutions including tetramethylammonium hydroxide (TMAH, 25%aqueous solution) , tetraethylammonium hydroxide (TEAH, 30%aqueous solution) , tetrapropylammonium hydroxide (TPAH, 35%aqueous solution) , tetrabutylammonium hydroxide (TBAH, 55%aqueous solution) can be used as solvent systems for dissolving bacterial cellulose powder.

[0038] Without wishing to be bound by theory, it is believed that anions and cations can play an essential role for bacterial cellulose powder dissolution. Anions can participate in interactions with hydroxyl protons on cellulose, whereas the hydrophobic substituents present on the QAH can interact with the hydrophobic portions of the cellulose via Van der Waals force, resulting in a QA+-cellulose intermediate, which can facilitate dissolution of the bacterial cellulose powder. These effects can result in the disruption of inter-and intra-molecular hydrogen bonds and thus effective dissolution of the bacterial cellulose powder.

[0039] 2. QAH / urea aqueous solvent system

[0040] Without wishing to be bound by theory, it is believed that urea can improve the solubility and stability of cellulose in solution by accumulating near the hydrophobic region via van der Waals forces. The addition of urea into QAH aqueous solution may not only reduce the amount of QAH solution required, but also promote the dissolution at ambient temperature.

[0041] 3. Metal complex based solvent system

[0042] The advantage of using metal complex as solvent system is that they can form stronger metal ligand bonds with substituents present on cellulose. De-complexation of the metal complex can release the cellulose. Different from hydrogen bonding solvent, the proposed metal complexes solvent systems can efficiently increase the solubility of the bacterial cellulose powder.

[0043] The optimization of medium concentration, temperature of the cultivation environment and culture medium were determined by applying Box-Behnken design.

[0044] It is an objective of present disclosure to provide methods of preparing regenerated cellulose fiber from bacterial cellulose. The cellulose pellicle formed in fermentation is purified under alkaline treatment, follow by washing and drying process. After grinding the dried bacterial cellulose, the bacterial cellulose powder can be used in the preparation of the spinning dope, which can then be used to spin the fiber.

[0045] In the present disclosure, the dope preparation by direct dissolution of bacterial cellulose powder in three dissolution systems are investigated. In certain embodiments, the bacterial cellulose powder dissolution methods include 1) tetrabutylammonium hydroxide solution (TBAH, 40%-55%aqueous solution) , 2) tetrabutylammonium hydroxide (TBAH)  / urea aqueous solvent system, 3) metal complex based solvent system. Advantageously, the solvent systems can eliminate high spinning temperature and the use of polluting chemicals and synthetic polymers in both solvents and raw material. The cellulose dope properties are analyzed with different dissolution concentrations. Moreover, the wet spinning of different dopes is demonstrated, and characterization of fiber is conducted.BRIEF DESCRIPTION OF THE DRAWINGS

[0046] The above and other objects and features of the present disclosure will become apparent from the following description of the disclosure, when taken in conjunction with the accompanying drawings.

[0047] Figure 1 depicts the Kraft process.

[0048] Figure 2 depicts viscose production.

[0049] Figure 3 depicts a photograph showing an exemplary SCOBY pellicle.

[0050] Figure 4 depicts a graph showing the solubility and time required for total dissolution of bacterial cellulose in common solvents such as N-methylmorpholine N-oxide (NMMO) , ionic liquid zinc chloride trihydrate, 1-ethyl-3-methylimidazolium acetate (EMIMAc) , and N, N-dimethyl acetamide / lithium chloride (LiCl / DMAc) .

[0051] Figure 5 depicts a flow chart showing an exemplary process for preparing regenerated bacterial cellulose fiber in accordance with certain embodiments described herein.

[0052] Figure 6 depicts theoretical reaction sequences showing the complexation driven dissolution of bacterial cellulose using metal complexes and decomplexation of the metal complexes to regenerate the cellulose.

[0053] Figure 7 depicts a picture showing the product of Example 3 after cutting and grinding.DETAILED DESCRIPTION

[0054] Definitions

[0055] Throughout the present disclosure, unless the context requires otherwise, the word "comprise" or variations such as "comprises" or "comprising" , will be understood to imply the inclusion of a stated integer or group of integers but not the exclusion of any other integer or group of integers. It is also noted that in this disclosure and particularly in the claims and / or paragraphs, terms such as “comprises” , “comprised” , “comprising” and the like can have the meaning attributed to it in U. S. Patent law; e.g., they can mean “includes” , “included” , “including” , and the like; and that terms such as “consisting essentially of” and “consists essentially of” have the meaning ascribed to them in U. S. Patent law, e.g., they allow for elements not explicitly recited, but exclude elements that are found in the prior art or that affect a basic or novel characteristic of the present invention.

[0056] Furthermore, throughout the present disclosure and claims, unless the context requires otherwise, the word “include” or variations such as “includes” or “including” , will be understood to imply the inclusion of a stated integer or group of integers, but not the exclusion of any other integer or group of integers.

[0057] The use of the singular herein includes the plural (and vice versa) unless specifically stated otherwise. In addition, where the use of the term "about" is before a quantitative value, the present teachings also include the specific quantitative value itself, unless specifically stated otherwise.

[0058] As used herein, the term "about" refers to a ±10%, ±7%, ±5%, ±3%, ±1%, or ±0% variation from the nominal value unless otherwise indicated or inferred.

[0059] The present disclosure provides methods of preparing a cellulose dope, a method of preparing regenerated cellulose fiber from the cellulose dope, and products thereof. The regenerated cellulose fiber can optionally contain functional materials that impact the physical, chemical, mechanical, and / or optical properties of the regenerated cellulose fiber.

[0060] In a first aspect, provided herein is a method of preparing a regenerated bacterial cellulose fiber, the method comprising: contacting bacterial cellulose powder with an aqueous solution comprising a quaternary ammonium hydroxide and optionally urea under conditions that result in the dissolution of at least a portion of the bacterial cellulose powder thereby forming a cellulose dope comprising bacterial cellulose; or contacting bacterial cellulose powder with an aqueous solution comprising a metal complex under conditions that result in the dissolution of at least a portion of the bacterial cellulose powder thereby forming a cellulose dope comprising bacterial cellulose; and extruding the cellulose dope in a coagulation bath thereby forming the regenerated bacterial cellulose fiber.

[0061] The regenerated bacterial cellulose fiber prepared in accordance with the methods described herein can be used in many potential applications, including but not limited to, paper and packaging, biomedical and pharmaceuticals, food and cosmetics, biosensors and energy storage, and / or textiles and materials.

[0062] In certain embodiments, the bacterial cellulose powder is a kombucha bacterial cellulose powder derived from a SCOBY pellicle produced during fermentation of a kombucha culture.

[0063] The kombucha culture can comprise a carbon source and a nitrogen source.

[0064] The carbon source is not particularly limited in so long as it can support the growth of the SCOBY. In certain embodiments, the carbon source is selected from the group consisting of ethanol, glucose, sucrose, fructose, galactose, inositol, glycerol, xylose, dextrose, lactose, dextrin, ribitol, mannitol, mannose, maltose, raffinose, coconut palm sugar, sugar cane, jaggery, honey, malt extract, molasses, and the like.

[0065] In certain embodiments, the nitrogen source comprises at least one organic nitrogen source selected from the group consisting of yeast extract, peptone, soybean, casamino acid, tryptone and malt extract, NH4Cl, NH4NO3, NaNO3, (NH4) 2SO4, tea (such as green or black tea) , coffee, red wine, white wine, malts, beers, fruit juice, fruit, fruit rind, vegetables, coconut milk, or other nitrogen containing organic matter.

[0066] In certain embodiments, the kombucha culture comprises tea and sucrose.

[0067] The SCOBY can comprise one or more bacterium and one or more yeast. In certain embodiments, the SCOBY comprises acetic bacteria, lactic acid bacteria, and osmophilic yeast.

[0068] The bacterium is not particularly limited provided it is capable of producing bacterial cellulose. In certain embodiments, the one or more bacterium is selected from the group consisting of Gluconobacter, Komagataeibacter, Pseudomonas, Agrobacterium, Rhizobium, Lactobacillus, Acetobacter, Azotobacter, Gluconacetobacter, Aerobacter, Sarcina, Alcaligenes. Specific examples of bacterium useful in the methods described herein include, but are not limited to Komagataeibacter xylinus, Komagataeibacter intermedius, Komagataeibacter rhaeticus, Komagataeibacter saccharivorans, Komagataeibacter kombuchae, Acetobacter pasteurianus, Acetobacter aceti, Acetobacter xylinum, Acetobacter ransens, and Enterobacter sp.

[0069] The one or more yeast can be selected from the group consisting of Zygosaccharomyces, Candida, Torulaspora, Pichia, Koleckera, Brettanomyces, Schizosaccharomyces, Saccharomyces, Saccharomycodes and Cyberlindnera jadini. Specific examples of yeast useful in the methods described herein include, but are not limited to, Candida stellata, Saccharomycodes ludwigii, Saccharomycodes apiculatus, Schizosaccharomyces pombe, Brettanomyces bruxellensis, Zygosaccharomyces bailii, and Saccharomyces cerevisiae.

[0070] The bacterial cellulose powder can be prepared from the SCOBY pellicle, which is typically generated on the surface of the cultivation medium during fermentation. The SCOBY pellicle can optionally be purified prior to dissolution, wherein the purification comprises liquid-solid extraction with an alkaline aqueous solution to remove any unwanted contaminants. In certain exemplary embodiments, the alkaline solution is prepared by dissolving a metal hydroxide, such as LiOH, NaOH, KOH, Ca (OH) 2, or the like in water. In exemplary embodiments, about 6 –12 g of sodium hydroxide is dissolved in 1 L of water. The SCOBY pellicle can be completely submerged in the alkaline aqueous solution followed by heating, e.g., at 70 -90℃ for 0.5 -1 hour, to assist with purification. The contaminants can diffuse out from the SCOBY pellicle to yield a purified SCOBY pellicle. The alkaline aqueous solution is then exchanged with water and heated, e.g., at 60 -80℃ for 0.5 -1 hour, to wash the SCOBY pellicle. The washing process can optionally be repeated 2, 3, 4, or more times until the pH value of the water washes becomes 6 –8.

[0071] The SCOBY pellicle can optionally be dried, e.g., by vacuum oven, by heating at, e.g., 40 –70℃ for 0.5 -1 h or freeze drying, e.g., for 24 –48 h. The SCOBY pellicle can then be shredded or pulverized into smaller particles, e.g., with diameter < 1.0 mm, and finally grinded to fine powder, e.g., with diameter < 0.2 mm. In certain embodiments, the drying process can be skipped, and the bacterial cellulose can be dissolved in wet status.

[0072] The solubility of cellulose powder in common solvents is exceedingly low. However, by appropriate selection of solvent system and dissolution conditions, both the dissolution rate as well as the solubility of the cellulose powder in the solvent system can be enhanced. Figure 4 shows four common solvent systems for dissolving cellulose powder. While some solvent systems can achieve high solubility and good dissolution rates, they call for the use of organic or ionic liquid solvents, which can be cost prohibitive on large scale and may pose potential health and environmental risks. Moreover, some of the solvent systems call for high temperatures and yield exceedingly slow rates of dissolution (up to 70 hours required for dissolution) , which pose obstacles for widespread use.

[0073] The cellulose powder dissolution systems described herein utilize readily available reagents and are capable rapidly dissolving bacterial cellulose powder resulting in cellulose dopes comprising cellulose at concentrations up to 10%w / w.

[0074] The quaternary ammonium hydroxide can have the chemical structure NR4OH, wherein R for each instance is independently alkyl, cycloalkyl, or phenyl; or two instances of R taken together with the nitrogen to which they are attached form a 3-6 membered heterocycloalkyl. In certain embodiments, each R is independently C1-C4 alkyl. Specific examples of quaternary ammonium hydroxides useful in the methods described herein include, but are not limited to, tetramethylammonium hydroxide, tetraethylammonium hydroxide, tetrapropylammonium hydroxide, and tetrabutylammonium hydroxide.

[0075] In certain embodiments, the metal complex comprises a metal selected from the group consisting of aluminum, calcium, copper, iron, nickel, manganese, indium, tungsten, and zinc; at least one anion selected from the group consisting of bromide, chloride, sulfate, bisulfate, carbonate, bicarbonate, nitrate, acetate, valerate, oleate, palmitate, stearate, laurate, benzoate, lactate, phosphate, tosylate, citrate, maleate, fumarate, succinate, tartrate, napthylate, mesylate, glucoheptonate, lactobionate, laurylsulphonate salts, and the like; and optionally a ligand. The metal can exist in the +1, +2, +3, or +4 oxidation state.

[0076] The type of ligand used is not particularly limited so long as it is capable of coordinating at least a portion of the selected metal. In certain embodiments, the ligand is a monodentate, bidentate, tridentate, or tetradentate ligand. Exemplary ligands include, but are not limited to, bipyridine, phenanthroline, 2-phenylpyridine bipyrimidine, bipyrazyl, glycinate, acetylacetonate, 2, 6-bis (1-methylbenzimidazol-2-yl) pyridine, ethylenediamine, diaminocyclohexane, 1, 3-propanediamine, 1, 3-diamino-2-hydroxypropane, 1, 6-hexanediamine, acetylacetonate (acac) , ethylenediaminetetraacetic acid, diethylenetriaminopentaacetic acid, propylenediaminetetraacetic acid, amino acids, and the like.

[0077] The metal complex must be charged balanced. The ratio of the metal and the at least one anion can be represented by the formula (At+) U (Bu-) T, wherein A represents the metal, B represents the at least one anion, t represents the charge of the metal, u represents the charge of the at least one anion, U is equal to the absolute value of the charge of the at least one anion and T is equal to the absolute value of the charge of the. For example, when metal a charge of 1+ and the anion is SO42-, which has a charge of -2, the charged balance formula would be (A1+) 2 (SO42-) .

[0078] In certain embodiments, the metal complex is bis (ethylenediamine) copper (II) hydroxide.

[0079] The cellulose powder and the aqueous solution can be contacted in a mass ratio between 1-10: 90-99; 1-9: 91-99; 1-8: 92-99; 1-7: 93-99; 1-6: 94-99; 2-6: 90-98; 3-6: 90-97; 3-5:95-97; or 3.5-4.5: 95.5-96.5, respectively.

[0080] The cellulose dope can comprise the bacterial cellulose at a concentration between 1-10%w / w, 2-10%w / w, 3-10%w / w, 4-10%w / w, 5-10%w / w, 6-10%w / w, 7-10%w / w, 1-9%w / w, 1-8%w / w, 1-7%w / w, 1-6%w / w, 2-6%w / w, 3-6%w / w, 3-5%w / w, or 3.5-4.5%w / w. In certain embodiments, the cellulose dope comprises the bacterial cellulose at a concentration of about 4%w / w.

[0081] The quaternary ammonium hydroxide can be present in the aqueous solution at a concentration between 1-60%w / w, 5-60%w / w, 10-60%w / w, 15-60%w / w, 20-60%w / w, 25-60%w / w, 30-60%w / w, 30-55%w / w, 30-50%w / w, 30-45%w / w, 30-40%w / w, 35-40%w / w, 35-60%w / w, 40-60%w / w, 45-60%w / w, 50-60%w / w, 55-60%w / w, or 40-55%w / w. In certain embodiments, the quaternary ammonium hydroxide is present in the aqueous solution at a concentration of about 40%w / w or about 55%w / w.

[0082] Urea can optionally be present in the aqueous solution at a concentration between 0.1-1%w / w, 0.1-0.9%w / w, 0.1-0.8%w / w, 0.1-0.7%w / w, 0.1-0.6%w / w, 0.1-0.5%w / w, 0.1-0.4%w / w, 0.1-0.3%w / w, or 0.15-0.25%w / w. In certain embodiments, the urea is present in the aqueous solution at a concentration of about 0.2%w / w.

[0083] The metal complex can be present in the aqueous solution at a concentration between 0.1 to 2 M, 0.5 to 2 M, 0.5 to 1.5 M, 0.6 to 1.4 M, 0.7 to 1.3 M, 0.8 to 1.2 M, or 0.9 to 1.1 M. In certain embodiments, the metal complex is present in the aqueous solution at a concentration of about 1 M.

[0084] The conditions that result in the dissolution of at least a portion of the bacterial cellulose powder can readily be determined by a person of ordinary skill in the art. Methods such as stirring, sonication, and / or the heating can be used to aid in the dissolution of the bacterial cellulose powder.

[0085] In certain embodiments, the conditions that result in the dissolution of at least a portion of the bacterial cellulose powder comprise: maintaining the aqueous solution comprising the quaternary ammonium hydroxide and optionally urea at 25-60℃, 25-55℃, 30-55℃, 30-50℃ or 35-45℃.

[0086] The aqueous solution comprising the quaternary ammonium hydroxide and optionally urea can be maintained at the desired temperature or temperature range for dissolution until substantially all bacterial cellulose powder has dissolved in the aqueous solution or until the aqueous solution is saturated with the bacterial cellulose powder. If the aqueous solution becomes saturated with the bacterial cellulose, additional portions of the quaternary ammonium hydroxide and / or water can be added. In certain embodiments, the aqueous solution comprising the quaternary ammonium hydroxide and optionally urea is maintained at the desired temperature or temperature range for dissolution for 5 minutes to 24 hours, 30 minutes to 24 hours, 1 to 24 hours, 2 to 24 hours, 3 to 24 hours, 4 to 24 hours, 5 to 24 hours, 6 to 24 hours, 7 to 24 hours, 8 to 24 hours, 9 to 24 hours, 10 to 24 hours, 12 to 24 hours, 14 to 24 hours, 16 to 24 hours, 18 to 24 hours, 20 to 24 hours, 22 to 24 hours, 6 to 18 hours, 8 to 16 hours, or 10 to 14 hours. In certain embodiments, the aqueous solution comprising the quaternary ammonium hydroxide and optionally urea is at the desired temperature or temperature range for dissolution for about 12 hours.

[0087] In certain embodiments, the conditions that result in the dissolution of at least a portion of the bacterial cellulose powder comprise: maintaining the aqueous solution comprising the metal complex at 50-100 ℃, 60-100 ℃, 70-100 ℃, 70-90 ℃, 75-90 ℃, or 80-90 ℃.

[0088] The aqueous solution comprising the metal complex can be maintained at the desired temperature or temperature range for dissolution until substantially all bacterial cellulose powder has dissolved in the aqueous solution or until the aqueous solution is saturated with the bacterial cellulose powder. If the aqueous solution becomes saturated with the bacterial cellulose, additional portions of the metal complex and / or water can be added. In certain embodiments, the aqueous solution comprising the metal complex can be maintained at the desired temperature or temperature range for dissolution for 5 minutes to 5 hours, 30 minutes to 5 hours, 1 hour to 5 hours, 1 hour 4 hours, 1 hour to 3 hours, or 1 hour to 2 hours. In certain embodiments, the aqueous solution comprising the metal complex can be maintained at the desired temperature or temperature range for dissolution for about 90 minutes.

[0089] In certain embodiments, dissolution of bacterial cellulose powder can be accomplished using the methods described herein, such as in TBAH, 40%-55%aqueous solution or TBAH / urea aqueous solvent system at room temperature to 40 ℃ with mild stirring for 8 –24 h; or in an aqueous solution comprising a metal complex at 75 –90 ℃after 1 -2 h dissolution time.

[0090] In certain embodiments, substantially all bacterial cellulose powder has dissolved in the aqueous solution when at least 40%by weight, at least 50%by weight, at least 60%by weight, at least 70%by weight, at least 75%by weight, at least 80%by weight, at least 85%by weight, at least 90%by weight, at least 95%by weight, at least 99%by weight, or all of the bacterial cellulose powder brought in contact with the aqueous solution has dissolved. Any undissolved bacterial cellulose powder can optionally be removed from the aqueous solution using any means, such as filtration, centrifugation and decanting, or the like.

[0091] Any undissolved cellulose powder can optionally be removed from the cellulose dope using at least one filter. In certain embodiments, the cellulose dope is filtered using one or more filters having pore size between 5-500 μm. Filtration of the cellulose dope can be improved by sequentially filtering the cellulose dope through progressively finer filters. This reduces the likelihood that the filter becomes blocked by particles and / or agglomerates larger than the pore size of the filter. Thus, in certain embodiments, the cellulose dope is filtered through 1, 2, 3, 4, 5, 6 or more filters having a pore size between 5-500 μm. The cellulose dope is filtered through 1, 2, 3, 4, 5, 6 or more filters having a pore size between 5-20, 50-100, 100-300, and 300-500 μm. In certain embodiments, the cellulose dope is filtered through 6 filters having a pore size of 500, 300, 100, 50 and 20 and 5 μm, which results in a solution comprising particles having at least one dimension less than 5 μm.

[0092] The optionally filtered cellulose dope can then be degassed by centrifuge. In certain embodiments, the optionally filtered cellulose dope is centrifuged at 3,000 rpm to 8,000 rpm for 5 –30 minutes. Degassing is conducted until substantially all gas is removed from the optionally filtered cellulose dope or until no additional gas is removed.

[0093] The prepared cellulose dope is loaded into an extruder with temperature control of the dope throughout the spinning process. Extrusion rate of the dope through a spinneret can be controlled by a gear pump. The spinneret can be configured horizontally and submersed under the coagulation bath. The formation of cellulose fiber was performed at room temperature in the primary drawing bath (coagulation) and the secondary drawing bath (stretching) . 0.25 M -1.0 M sulfuric acid and sodium sulfate with mole ratio 1: 1 or 1: 1.1 was served as coagulant in both primary drawing bath and secondary drawing bath. The regenerated fiber was then washed with water at 60 -80℃ in washing bath. The fibers were collected and dried at 40 -70 ℃ for 4 -8 hours.

[0094] The structure and property of fibers could be adjusted by the resident time of the fiber in the coagulation bath. Therefore, the rotation speed of the gear pump, take-up speed of primary and secondary drawing bath could be calculated as following equation: v1=v0×σ1v2=v1×σ2

[0095] where:

[0096] ω: rotational speed of gear pump

[0097] n: number of pores on spinneret

[0098] r: radius of pore on spinneret

[0099] C: flow per rotation

[0100] v1: take-up speed of primary drawing bath

[0101] v2: take-up speed of secondary drawing bath

[0102] σ1: primary drawing ratio

[0103] σ2: secondary drawing ratio

[0104] The step of extruding the cellulose dope in a coagulation bath can comprise passing the cellulose dope through a spinneret into a coagulation bath. In certain embodiments, the coagulation bath comprises a primary drawing bath (coagulation) and optionally wet-stretched in a secondary drawing bath (stretching) .

[0105] The spinneret can be a monofilament spinneret or a multifilament spinneret.

[0106] The cellulose dope can be passed through the spinneret at a flow rate between 3 -12, 4 -11, 4 -10, 5 -10, 6 -10, or 7 -9 meters / minute. In certain embodiments, the cellulose dope is passed through the spinneret at a rate about 8 meters / minute.

[0107] The primary and secondary drawing baths can each independently comprise any solvent in which the cellulose dope has low solubility. In certain embodiments, the primary and secondary drawing baths each comprise an aqueous solvent comprising an acid, a metal salt, or a combination thereof. In certain embodiments, the metal salt comprises one or more cations selected from the group consisting of is Li+, Na+, Ca2+, and Mg2+ and one or more anions selected from the group consisting of halides, nitrate, phosphate, carbonate, sulfate, acetate, and the like. Exemplary metal salts include, but are not limited to, NaCl, LiCl, CaCl2, NaBr, LiBr, CaBr2, Li2SO4, Na2SO4, CaSO4, Na3PO4, Li3PO4, and NaOAc. Exemplary acids include, but are not limited to, HCl, H2SO4, and HSO4-. In certain embodiments, the primary and secondary drawing baths comprises H2SO4. In certain embodiments, the primary and secondary drawing baths further comprise Na2SO4.

[0108] The concentration of the metal salt or acid in the primary and secondary drawing baths can range between 0.1 to 3 M, 0.1 to 2.5 M, 0.1 to 2 M, 0.1 to 1.5 M, 0.1 to 1 M, 0.1 to 0.5 M, 0.5 to 3 M, 1 to 3 M, 1.5 to 3 M, 2 to 3 M, 0.5 to 2.5 M, 0.5 to 2 M, 0.5 to 1.5 M, 0.5 to 1 M, 0.25 to 0.75 M, 0.375 to 0.75 M, 1 to 2 M, or 1.5 to 2 M. In certain embodiments, the primary drawing bath comprises the acid at a concentration of about 0.75 M and the metal salt at a concentration of about 0.75 M to about 0.825 and the secondary drawing bath comprises the acid a concentration of about 0.375 M and the metal salt at a concentration of about 0.375 M to about 0.412.

[0109] In instances in which the primary and / or secondary drawing baths comprise both an acid and a metal salt, the molar ratio of the acid to the metal salt can range from 0.01: 1 to 1: 0.01, 1: 0.1 to 1: 5, 1: 0.1 to 1: 4, 1: 0.1 to 1: 3, 1: 0.1 to 1: 2, 1: 0.5 to 1: 2, 1: 0.5 to 1: 1.5, 1: 0.75 to 1: 1.5, 1: 0.75 to 1: 1.4, 1: 0.75 to 1: 1.3, 1: 0.9 to 1: 1.3, 1: 0.9 to 1: 1.2, or 1: 1.1 to 1: 1.2 respectively. In certain embodiments, the molar ratio of the acid to the metal salt in the primary and / or secondary drawing baths range from about 1 to about 1.1, respectively.

[0110] In instances in which the primary and secondary drawing baths comprise an acid, the pH of the primary and secondary drawing baths can independently be 7 or less, 6 or less, 5 or less, 4 or less, 3 or less, 2 or less, 1 or less, 0.5 or less, or 0 or less. In certain embodiments, the pH of each of the primary and secondary drawing baths is independently between -1 and 6, -1 and 5, -1 and 4, -1 and 3, -1 and 2, -1 and 1, -1 and 0, 0 and 6, 0 and 5, 0 and 4, 0 and 3, 0 and 2, 0 and 1, 0 and 0.5. In certain embodiments, the pH of the primary drawing bath is about 0.12 and the pH of the secondary drawing bath is about 0.43.

[0111] The regenerated bacterial cellulose fiber can optionally be stretched in the primary and secondary drawing baths by adjusting the drawing ratio. The regenerated bacterial cellulose fiber can be stretched in the coagulation bath at a drawing ratio between 1-2%.

[0112] The step of wet-stretching regenerated bacterial cellulose fiber in the secondary drawing bath can comprise stretching the regenerated bacterial cellulose fiber at a temperature between 40 to 60℃, 40 to 55℃, 40 to 50℃, 40 to 45℃. In certain embodiments, the step of wet-stretching can comprise stretching the filament can be conducted at about 45℃.

[0113] By modifying the conditions used to prepare the regenerated bacterial cellulose fiber according to the methods described herein, the properties of the thus prepared regenerated cellulose fiber can be modified. In certain embodiments, the regenerated cellulose fiber can have a linear density of 2-9, 3-9, 3-8, 3-7, 3-6, 3-5, 3-9, 4-9, 5-9.6-9, or 6-8 dtex. In certain embodiments, the regenerated cellulose fiber can have a tenacity at maximum load of 0.8-2.0, 0.9-2.0, 1.0-2.0, 1.1-2.0, 1.2-2.0, 1.3-2.0, 1.4-2.0, 1.5-2.0, 1.3-1.6, 1.5-1.6, or 1.6-2.0 cN / dtex.

[0114] Examples

[0115] Example 1 –Cultivation of bacterial cellulose by Kombucha fermentation

[0116] 3 L of water was boiled and during boiling 12%w / w of cane sugar was stirred in. 0.6%w / w of black tea leaves in tea bag was added and the solution was boiled for 15 minutes to 1 hour. After cooling to room temperature, tea bag was removed, and the sweet tea was in inoculated with 33%w / w SCOBY culture and poured into a container previously sterilized. The incubation was carried out at 31℃ for 14 days. Newly formed daughter culture would float, and a cellulose pellicle was formed across the available surface.

[0117] Example 2 –Preparation of bacterial cellulose by alkaline treatment

[0118] The floating bacterial cellulose pellicle was removed from the surface of culture medium and put into a container. 12 g of sodium hydroxide dissolved in 1L of water was poured into the container. The cellulose pellicle was completely submerged into the solution followed by heating to 60℃ for 1 h. The BC pellicle was then washed with water at 60℃ for 1 h. The washing process was repeated 2 –3 times until the pH value became 6 –8. White BC pellicle was obtained after alkaline treatment.

[0119] Example 3 –Preparation of bacterial cellulose powder

[0120] The treated BC pellicle was removed from the solution. The surface liquid was absorbed by dried towel before the BC pellicle was put into to the vacuum oven. The BC pellicle was laid flat on the tray and was evenly distributed. The pellicle was dried in vacuum oven at 60℃ for 12 h. The dried cellulose was then cut into small pieces and further shredded into fine particles by two times mechanical grinding. The first grinding produced particles with diameter < 1.0 mm and the second grinding produced powder with diameter < 0.2 mm.

[0121] Example 4 –Preparation of spinning dope by TBAH aqueous solvent system:

[0122] [Rectified under Rule 91, 19.07.2024]4.5 g of BC powder was placed in 95.5 g of 55%TBAH aqueous solution in a reaction vessel, to achieve the cellulose weight content at 4.5 wt%. The mixture was mechanically stirred at 25 ℃ for 12 h to dissolve the BC powder. After complete dissolution, the solution was degassed by centrifugation at 4,000 rpm for 15 min. Rheology viscosity of the cellulose solution was measured to be around 50 -120 Pa·s. The experimental result was shown in Table 1. Result of Example 4. According to the above experiment, all the BC powder was dissolved in the solvent system and a yellow solution was formed.

[0123] [Rectified under Rule 91, 19.07.2024]Table 1. Result of Example 4 Linear Density and Tenacity of different BC wt%

[0124] Example 5 –Preparation of spinning dope by TBAH / urea aqueous solvent system:

[0125] [Rectified under Rule 91, 19.07.2024]0.1 g / g of urea was introduced into 55%TBAH aqueous solution in order to enhance the cellulose dissolution. The mixture was stirred for 30 min at room temperature until urea was dissolved. 4.5 g of BC powder was placed in 95.5 g of TBAH / urea aqueous solution in a reaction vessel, to achieve the cellulose weight content at 4.5 wt%. The mixture was mechanically stirred at 25 ℃ for 12 h to dissolve the BC powder. After complete dissolution, the solution was degassed by centrifugation at 4,000 rpm for 15 min. Rheology viscosity of the cellulose solution was measured to be around 50 -120 Pa·s. The experimental result was shown in Table 2. Result of Example 5. According to the above experiment, all the BC powder was dissolved in the solvent system and a yellow solution was formed.

[0126] [Rectified under Rule 91, 19.07.2024]Table 2. Result of Example 5 Linear Density and Tenacity of different BC wt%

[0127] Example 6 –Preparation of spinning dope by metal complex based solvent system:

[0128] 4 g of BC powder was placed in 96 g of 1 M Cu (en) 2 (OH) 2 solution in a reaction vessel, to achieve the cellulose weight content at 4 wt%. The mixture was mechanically stirred at 80 ℃ for 1 -2 h to dissolve the BC powder. After complete dissolution, the solution was degassed by centrifugation at 4000 rpm for 15 min. Rheology viscosity of the cellulose solution was measured to be around 50 -120 Pa·s.

[0129] According to the example 6, all the BC powder was dissolved in the solvent system and a viscous dark blue solution was formed.

[0130] Example 7 –Fiber regeneration by wet spinning method

[0131] The fiber was regenerated by wet spinning method using a FET-200 LAB wet-spinning machine.

[0132] 1000 mL cellulose solution prepared as Example 4 –6 was extruded by gear pump at room temperature through a multi-hole spinneret (100 holes, capillary diameter 60 μm or 100 μm) . The formation of cellulose fiber was performed at room temperature in the primary drawing bath (coagulation) and the secondary drawing bath (stretching) . 0.75 M sulfuric acid and sodium sulfate (0.75-0.825 M) served as the coagulant drawing bath and 0.375 M sulfuric acid and sodium sulfate (0.375-0.412 M) served as coagulant in the secondary drawing bath. The regenerated bacterial cellulose fiber can optionally be stretched in the primary and secondary drawing baths by adjusting the drawing ratio. The regenerated bacterial cellulose fiber can be stretched in the coagulation bath at a drawing ratio 1.7%. The regenerated fiber was then washed with water at 60℃ in washing bath. The fibers were collected and dried at 40 -70 ℃ for 4 -8 hour.Industrial applicability

[0133] From environmental point of view, bacterial cellulose fiber is in advantage over traditional regenerated cellulose fiber in terms of the cellulose source purity, less land space area required for production, short production cycle, less water and no pesticide used. In our invention, we use food or beverage waste to generate our bacteria cellulose. In this invention, SCOBY waste of producing kombucha is an excellent choice for our demonstration. In 2021, the global kombucha market size was value at USD 2.64 billion and is expected to expand at a compound annual growth rate (CAGR) of 15.6%from 2022 to 2030 as consumers are shifting to a healthy and wellbeing choice.

[0134] In this invention, bacterial cellulose (BC) will be developed as sustainable source for regenerated cellulose fibers production. The key components of this invention are (1) to develop solvent systems for dissolving bacterial cellulose efficiently, and (2) to find out the optimized condition for the wet spinning of regenerated bacterial cellulose fiber.

[0135] Acronyms

[0136] BC: Bacterial cellulose

[0137] Cu (en) 2 (OH) 2: Bis (ethylenediamine) copper (II) hydroxide

[0138] DP: Degree of polymerization

[0139] KBC: Kombucha bacterial cellulose

[0140] QAH: Quaternary ammonium hydroxide

[0141] SCOBY: Symbiotic Colony of Bacteria and Yeast

[0142] TBAH: Tetrabutylammonium hydroxide

Claims

1.A method of preparing a regenerated bacterial cellulose fiber, the method comprising:contacting bacterial cellulose powder with an aqueous solution comprising a quaternary ammonium hydroxide and optionally urea under conditions that result in the dissolution of at least a portion of the bacterial cellulose powder thereby forming a cellulose dope comprising bacterial cellulose; orcontacting bacterial cellulose powder with an aqueous solution comprising a metal complex under conditions that result in the dissolution of at least a portion of the bacterial cellulose powder thereby forming a cellulose dope comprising bacterial cellulose; andextruding the cellulose dope in a coagulation bath thereby forming the regenerated bacterial cellulose fiber.2.The method of claim 1, wherein the bacterial cellulose powder is a kombucha bacterial cellulose powder.3.The method of claim 1, wherein the quaternary ammonium hydroxide is NR4OH, wherein R for each instance is independently alkyl, cycloalkyl, or phenyl; and the metal complex comprises a metal selected from the group consisting of aluminum, calcium, copper, iron, nickel, and zinc.4.The method of claim 1, wherein the quaternary ammonium hydroxide is tetramethylammonium hydroxide, tetraethylammonium hydroxide, tetrapropylammonium hydroxide, or tetrabutylammonium hydroxide; and the metal complex is bis (ethylenediamine) copper (II) hydroxide.5.The method of claim 1, wherein the quaternary ammonium hydroxide is present in the aqueous solution at a concentration between 20-60%w / w; and the metal complex is present in the aqueous solution at a concentration between 0.5 to 2M.6.The method of claim 1, wherein the urea is present in the aqueous solution at a concentration of 0.1-0.5%w / w.7.The method of claim 1, wherein the coagulation bath comprises a primary drawing bath and further comprises a secondary drawing bath.8.The method of claim 7, wherein the primary drawing bath and the secondary drawing bath each independently have a pH between 0-1.9.The method of claim 7, wherein the primary drawing bath and the secondary drawing bath each comprises an aqueous solution of H2SO4 and optionally Na2SO4.10.The method of claim 9, wherein the concentration of H2SO4 in each of the primary drawing bath and the secondary drawing bath is independently 0.25 M to 1 M.11.The method of claim 1, wherein the cellulose dope comprises the bacterial cellulose at a concentration between 2-10%w / w.12.The method of claim 1 further comprising:providing a symbiotic colony of bacteria and yeast (SCOBY) pellicle;contacting the SCOBY pellicle with an alkaline aqueous solution thereby forming a treated SCOBY pellicle;optionally washing and drying the treated SCOBY pellicle; andpowdering the treated SCOBY pellicle thereby forming the bacterial cellulose powder.13.The method of claim 1 further comprising: washing the regenerated bacterial cellulose fiber with water and drying the washed regenerated bacterial cellulose fiber.14.The method of claim 1, wherein the conditions that result in the dissolution of at least a portion of the bacterial cellulose powder comprise: maintaining the aqueous solution comprising the quaternary ammonium hydroxide and optionally urea at 25-50℃ for 8 to 24 h; or maintaining the aqueous solution comprising the metal complex at 75-90 ℃ for 1 to 2 h.15.The method of claim 1, wherein the method comprises: contacting bacterial cellulose powder with an aqueous solution comprising between 20-60%w / w N (C1-C5) 4OH and optionally 0.1-0.5%w / w urea at 25-40℃ for 8 to 24 h resulting in the dissolution of at least a portion of the bacterial cellulose powder thereby forming a cellulose dope comprising bacterial cellulose at a concentration of between 4-10%w / w; or contacting bacterial cellulose powder with an aqueous solution comprising 0.5 M to 2 M bis (ethylenediamine) copper (II) hydroxide at 75-90 ℃ for 1 to 2 h resulting in the dissolution of at least a portion of the bacterial cellulose powder thereby forming a cellulose dope comprising the bacterial cellulose at a concentration of between 2-6%w / w; andextruding the cellulose dope in a coagulation bath comprising a primary drawing bath and a secondary drawing bath, wherein the primary drawing bath and the secondary drawing bath independently have a pH between 0-0.5 thereby forming the regenerated bacterial cellulose fiber.16.The method of claim 15, wherein the cellulose dope comprises bacterial cellulose at a concentration of between 3.5-5.5%w / w.17.The method of claim 15 further comprising:providing a symbiotic colony of bacteria and yeast (SCOBY) pellicle;contacting the SCOBY pellicle with an alkaline aqueous solution thereby forming a treated SCOBY pellicle;optionally washing and drying the treated SCOBY pellicle; andpowdering the treated SCOBY pellicle thereby forming the bacterial cellulose powder.18.The method of claim 17, wherein the alkaline aqueous solution has pH of 13-14.19.The method of claim 17, wherein the alkaline aqueous solution comprises NaOH.20.The method of claim 1, wherein the method comprises:providing a symbiotic colony of bacteria and yeast (SCOBY) pellicle;contacting the SCOBY pellicle with an alkaline aqueous solution having a pH of 13-13.5 thereby forming a treated SCOBY pellicle;optionally washing and drying the treated SCOBY pellicle;powdering the treated SCOBY pellicle thereby forming the bacterial cellulose powder;contacting bacterial cellulose powder with an aqueous solution comprising between 20-60%w / w N (C1-C5) 4OH and optionally 0.1-0.5%w / w urea at 25-40℃ for 8 to 24 h resulting in the dissolution of at least a portion of the bacterial cellulose powder thereby forming a cellulose dope comprising bacterial cellulose at a concentration of between 3.5-5.5%w / w; orcontacting bacterial cellulose powder with an aqueous solution comprising 0.5 M to 2 M bis (ethylenediamine) copper (II) hydroxide at 75-90 ℃ for 1 to 2 h resulting in the dissolution of at least a portion of the bacterial cellulose powder thereby forming a cellulose dope comprising the bacterial cellulose at a concentration of between 3.5-5.5%w / w; andextruding the cellulose dope in a coagulation bath comprising a primary drawing bath and a secondary drawing bath, wherein the primary drawing bath and the secondary drawing bath each comprise an aqueous solution of H2SO4 and Na2SO4 at a pH between 0-0.5 thereby forming the regenerated bacterial cellulose fiber.