Gas diffusion composite material for fuel cells, and solid polymer fuel cell

The gas diffusion composite material with a microporous carbon layer on a porous base sheet addresses high electrical resistance issues in fuel cells and polymer electrolyte fuel cells, improving power generation and mechanical strength, allowing for thinner, more efficient fuel cell designs.

WO2024190898A1PCT designated stage expired Publication Date: 2024-09-19KYUSHU UNIV
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/010185
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-16
Filing Date
2024-03-15
Publication Date
2024-09-19

AI Technical Summary

Technical Problem

Conventional gas diffusion layers in fuel cells and polymer electrolyte fuel cells face challenges with high electrical resistance, particularly contact resistance, which affects power generation performance, especially at high current densities, and are limited in thinning due to mechanical strength and cost considerations.

Method used

A gas diffusion composite material comprising a porous base sheet made of conductive or non-conductive materials with a microporous carbon layer, where the microporous carbon layer covers or penetrates the base sheet, reducing overall thickness and contact resistance, and enhancing mechanical strength and conductivity.

Benefits of technology

The composite material significantly reduces electrical resistance and improves power generation characteristics by providing excellent current collection and mechanical strength, enabling thinner fuel cell stacks with enhanced performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024010185_19092024_PF_FP_ABST
    Figure JP2024010185_19092024_PF_FP_ABST
Patent Text Reader

Abstract

Provided are: a gas diffusion composite material for fuel cells which is a thin layer and in which electric resistance such as contact resistance is reduced; and a solid polymer fuel cell comprising the same. This gas diffusion composite material for fuel cells: has a porous base material sheet made of an electrically conductive material, and a fine porous carbon layer that contains a water repellent resin and a particulate and / or fibrous carbon material; and has either one of structures (A) to (E). Structure (A): A structure in which the fine porous carbon layer covers one surface of the porous base material sheet. Structure (B): A structure in which the fine porous carbon layer covers both surfaces of the porous base material sheet. Structure (C): A structure in which the fine porous carbon layer covers one surface of the porous base material sheet, and a portion thereof enters the inside of the porous base material sheet. Structure (D): A structure in which the fine porous carbon layer covers one surface of the porous base material sheet, and a portion of the fine porous carbon layer enters the inside of the porous base material sheet, and in which the fine porous carbon layer reaches the opposite surface of the porous base material sheet from the one surface thereof. Structure (E): A structure in which the entirety of the porous base material sheet is embedded in the fine porous carbon layer.
Need to check novelty before this filing date? Find Prior Art

Description

Gas diffusion composites for fuel cells and polymer electrolyte fuel cells

[0001] (Citation of Related Applications) This application claims the benefit of and priority to Japanese Patent Application No. 2023-42109, filed on March 16, 2023. Priority to the aforementioned patent application is expressly claimed, and the entire disclosure of that application is incorporated herein by reference for all purposes. The entire content of this Japanese Patent Application is incorporated herein by reference.

[0002] The present invention relates to a gas diffusion composite material for a fuel cell and a polymer electrolyte fuel cell.

[0003] A polymer electrolyte fuel cell (PEFC) is constructed with a basic unit in which a PEFC unit cell is sandwiched between two separators with gas flow channels, the PEFC unit cell comprising a membrane electrode assembly (MEA) including an electrolyte membrane and electrodes (anode and cathode) laminated on both sides of the electrolyte membrane, and gas diffusion layers (GDLs) laminated on both sides of the membrane electrode assembly.

[0004] The gas diffusion layer of a PEFC requires high gas diffusivity to diffuse gas supplied from the separator to the electrode catalyst layer, high drainage to discharge water produced during electrochemical reactions back to the separator, and high conductivity to extract the generated current. Therefore, a widely used gas diffusion layer for PEFCs is one in which a microporous layer (MPL) made of carbon powder and fluororesin is formed on the surface of a carbon sheet made of carbon fiber as a substrate layer. The MPL is a layer made of a porous composite material of a conductive carbon material and a water-repellent fluororesin. The carbon material forms a conductive network, and the fluororesin acts as an adhesive and provides water repellency.

[0005] As described above, the GDL is required to have high gas diffusivity to diffuse gas supplied from the separator to the electrode catalyst layer. Insufficient gas diffusivity leads to reduced power generation performance, particularly in the high current density region. Furthermore, while the thinner the unit cell in a PEFC, the more efficient the integration, the thicker the GDL is, typically about 150 μm to 1 mm, accounting for a large proportion of the total thickness of the PEFC unit cell. Therefore, if the gas diffusion layer can be made thinner, the PEFC unit cell can be made thinner, improving integration and increasing output. For example, Patent Document 1 reports a fuel cell with a thinner gas diffusion layer than conventional ones. The technology of Patent Document 1 improves gas diffusivity and power generation performance in the high current density region by reducing the thickness of the gas diffusion layer relative to the separator rib width.

[0006] The present inventors have also reported a porous metal gas diffusion layer made of a porous metal sheet in Patent Document 2. The porous metal sheet used is a metal mesh sheet made of metal Sn, a Sn alloy, or stainless steel, or a metal fiber sheet made of metal Ti or a Ti alloy.

[0007] JP 2022-11735 A JP 2022-145670 A

[0008] The gas diffusion layer of Patent Document 1 is self-supporting due to the use of special carbon fibers as a constituent material, and the gas diffusion layer of this document has a limit of thickness that can be reduced to about 150 μm. Also, the porous metal gas diffusion layer of Patent Document 2 can be made about 30 μm thick, which is useful for reducing the thickness of PEFC single cells, but there is room for improvement in terms of electrical resistance, such as contact resistance, that is derived from the metal gas diffusion layer.

[0009] Under these circumstances, an object of the present invention is to provide a gas diffusion composite material for a fuel cell which is a thin layer and has reduced electrical resistance such as contact resistance, and a polymer electrolyte fuel cell including the same.

[0010] The present inventors have conducted extensive research to solve the above problems, and as a result have found that the following invention meets the above object, thereby completing the present invention.

[0011] That is, the present invention relates to the following inventions: <1> A gas diffusion composite material for a fuel cell, comprising: a porous substrate sheet made of a conductive material; and a microporous carbon layer containing a particulate and / or fibrous carbon material and a water-repellent resin, wherein the thickness of the porous substrate sheet is 3 μm or more and 150 μm or less, and wherein the gas diffusion composite material has any one of the following structures (A) to (E): Structure (A): A structure in which the microporous carbon layer covers one side of the porous substrate sheet. Structure (B): A structure in which the microporous carbon layer covers both sides of the porous substrate sheet. Structure (C): A structure in which the microporous carbon layer covers one side of the porous substrate sheet and a portion of the microporous carbon layer has penetrated into the porous substrate sheet. Structure (D): A structure in which the microporous carbon layer covers one side of the porous substrate sheet and a portion of the microporous carbon layer has penetrated into the porous substrate sheet, reaching from one side of the porous substrate sheet to the other side. Structure (E): A structure in which the entire porous substrate sheet is embedded in the microporous carbon layer. <2> The gas diffusion composite material according to <1>, wherein the thickness of the porous substrate sheet is 5 μm or more and 100 μm or less. <3> The gas diffusion composite material according to <1> or <2>, wherein the total thickness is 3 μm or more and 150 μm or less. <4> The gas diffusion composite material according to any one of <1> to <3>, having an overall thickness of 20 μm or more and 100 μm or less. <5> The gas diffusion composite material according to any one of <1> to <4>, wherein the porous substrate sheet is in the form of a mesh sheet, a punched sheet, or an expanded sheet. <6> The gas diffusion composite material according to any one of <1> to <5>, wherein the porous substrate sheet is made of a carbon material. <7> The gas diffusion composite material according to any one of <1> to <5>, wherein the porous substrate sheet is a carbon mesh. <8> The gas diffusion composite material according to any one of <5> to <7>, having any one of Structures (C) to (E). <9> The gas diffusion composite material according to <7>, having Structure (C). <10> The gas diffusion composite material according to any one of <1> to <5>, wherein the porous substrate sheet is made of a metal material. <11> The gas diffusion composite material according to any one of <1> to <5>, wherein the porous substrate sheet is a stainless steel mesh. <12> The gas diffusion composite material according to <11>, having any one of structures (C) to (E).<13> The gas diffusion composite material according to <11>, having a structure (D). <14> A gas diffusion composite material for a fuel cell, comprising: a porous substrate sheet made of a non-conductive material; and a microporous carbon layer containing a particulate and / or fibrous carbon material and a water-repellent resin, wherein the porous substrate sheet has a thickness of 3 μm or more and 150 μm or less, and has one of the following structures (D) and (E). Structure (D): A structure in which the microporous carbon layer covers one side of the porous substrate sheet made of the non-conductive material, and a part of the microporous carbon layer penetrates into the porous substrate sheet made of the non-conductive material, and the microporous carbon layer reaches from one side to the other side of the porous substrate sheet made of the non-conductive material. Structure (E): A structure in which the entire porous substrate sheet is embedded in the microporous carbon layer. <15> The gas diffusion composite for a fuel cell according to any one of <1> to <14>, wherein the particulate and / or fibrous carbon material constituting the microporous carbon layer is carbon black, carbon nanotubes, or a mixture thereof. <16> A polymer electrolyte fuel cell comprising: a membrane electrode assembly having a solid polymer electrolyte membrane, a cathode catalyst layer bonded to one side of the solid polymer electrolyte membrane, and an anode catalyst layer bonded to the other side of the solid polymer electrolyte membrane; a pair of gas diffusion layers laminated on the cathode catalyst layer and the anode catalyst layer, respectively; and a pair of separators sandwiching the membrane electrode assembly via the gas diffusion layer, wherein at least one of the pair of gas diffusion layers is the gas diffusion composite material for a fuel cell according to any one of <1> to <15>.

[0012] According to the present invention, there are provided a gas diffusion composite material for a fuel cell which is a thin layer and has reduced electrical resistance such as contact resistance, and a polymer electrolyte fuel cell including the same.

[0013] FIG. 1 is a structural schematic diagram of a polymer electrolyte fuel cell. FIG. 2 is a schematic diagram of a membrane electrode assembly equipped with a conventional gas diffusion layer. FIG. 3 is a schematic diagram of a gas diffusion composite material for a fuel cell of the present invention (the porous substrate sheet has (A) MPL laminated on one side, (B) MPL laminated on both sides, (C) partially embedded in the MPL (not reaching the back surface), (D) partially embedded in the MPL (reaches the back surface), and (E) completely embedded in the MPL). FIG. 4 is a photograph of the microstructure of the surface of a gas diffusion member 1 (stainless steel mesh sheet, SUS316 977 mesh). FIG. 5 is a photograph of the microstructure of the surface of a gas diffusion member 2 (MPL-composite stainless steel mesh). FIG. 6 is a photograph of the microstructure of the cross section of a gas diffusion member 2 (MPL-composite stainless steel mesh). FIG. 7 is a result of observation of the microstructure of the surface of a gas diffusion member 3 (gas diffusion layer with MPL (reference example)). FIG. 8 is a photograph of the appearance of a gas diffusion member 5 (MPL-composite carbon mesh). 1 shows IV characteristics of PEFC single cells using gas diffusion members 1 to 3. 1 shows IV characteristics of PEFC single cells using gas diffusion members 4 and 5. 1 shows IV characteristics of PEFC single cells using gas diffusion member 6.

[0014] The present invention will be described in detail below with reference to examples, but the present invention is not limited to the examples below and can be practiced with any modifications within the scope of the gist of the present invention. In this specification, the expression "to" is used to include the numerical values ​​or physical quantities before and after it.

[0015] 1. Gas diffusion composite material for fuel cells The present invention relates to a gas diffusion composite material for fuel cells (hereinafter, sometimes referred to as the "gas diffusion composite material of the present invention") that comprises a porous substrate sheet made of a conductive material and a microporous carbon layer containing a particulate and / or fibrous carbon material and a water-repellent resin, wherein the porous substrate sheet has a thickness of 3 μm or more and 150 μm or less, and has any of the following structures (A) to (E):

[0016] Structure (A): A structure in which the microporous carbon layer covers one side of the porous substrate sheet. Structure (B): A structure in which the microporous carbon layer covers both sides of the porous substrate sheet. Structure (C): A structure in which the microporous carbon layer covers one side of the porous substrate sheet, and a part of the microporous carbon layer penetrates into the porous substrate sheet. Structure (D): A structure in which the microporous carbon layer covers one side of the porous substrate sheet, and a part of the microporous carbon layer penetrates into the porous substrate sheet, and the microporous carbon layer reaches from one side of the porous substrate sheet to the other side. Structure (E): A structure in which the entire porous substrate sheet is embedded in the microporous carbon layer.

[0017] Details of the structures (A) to (E) will be described later in "1-3. Arrangement of porous substrate sheet and microporous carbon layer."

[0018] The gas diffusion composite material of the present invention is suitable as a gas diffusion layer for a polymer electrolyte fuel cell.

[0019] The role of the gas diffusion composite material (gas diffusion layer) in a polymer electrolyte fuel cell will be explained below with reference to Figures 1 and 2. Figure 1 is a conceptual diagram showing a typical configuration of a polymer electrolyte fuel cell. In a polymer electrolyte fuel cell, hydrogen is supplied to the fuel electrode (anode), and (reaction 1) 2H → 4H + +4e - The generated proton (H + ) is supplied to the air electrode (cathode) through a solid polymer electrolyte membrane, and the generated electrons are supplied to the air electrode (cathode) through an external circuit (not shown), resulting in (Reaction 2) O2 + 4H + +4e - →2H2O reacts with oxygen to produce water. This electrochemical reaction between the fuel electrode (anode) and the air electrode (cathode) generates a potential difference between the two electrodes.

[0020] Figure 2 shows a schematic diagram of a membrane electrode assembly equipped with a conventional gas diffusion member. The main functions required of a gas diffusion member in a PEFC are moisture retention of the solid polymer electrolyte membrane (approximately 10 μm thick), drainage from the electrode catalyst layer, electronic conduction between the electrode catalyst layer and the separator, and gas transport. Conventional gas diffusion members are commonly composed of a carbon fiber gas diffusion layer (GDL) and a microporous layer (MPL), which is a finer pore layer formed on the surface of the carbon fiber gas diffusion layer that contacts the electrode catalyst layer to improve current collection and water retention. Furthermore, particularly in PEFCs with a thickness of approximately 1 mm, two carbon fiber gas diffusion layers with a thickness of approximately 200 μm are used adjacent to both electrodes. However, these layers have challenges, such as reduced mechanical strength and high cost due to the thinning.

[0021] On the other hand, the gas diffusion composite material of the present invention has a structure in which a microporous carbon layer containing a particulate and / or fibrous carbon material and a water-repellent resin is supported by a porous substrate sheet (e.g., a conductive porous substrate sheet made of metal or carbon) having excellent mechanical strength and a thickness of 3 μm to 150 μm. Because of this structure, the gas diffusion composite material of the present invention has sufficient mechanical strength and conductivity derived from the porous substrate sheet and conductivity and water repellency derived from the microporous carbon layer, and therefore the overall thickness of the gas diffusion composite material can be reduced to 150 μm or less (preferably 100 μm or less, 60 μm or less).

[0022] The gas diffusion composite material of the present invention has a microporous carbon layer on its surface that has excellent current collection properties and low contact resistance. Therefore, by arranging the gas diffusion composite material of the present invention, overvoltage is reduced and power generation characteristics (IV characteristics) are excellent compared to when only a porous substrate sheet without a microporous layer is used.

[0023] A polymer electrolyte fuel cell is normally used as a fuel cell stack by stacking a number of unit cells, which are its basic component, according to the power generation performance. Therefore, instead of a conventional gas diffusion member (carbon fiber gas diffusion layer with MPL), the gas diffusion composite of the present invention, which is composed of a porous substrate sheet made of a conductive material and a microporous carbon layer containing a particulate and / or fibrous carbon material and a water-repellent resin, can be used as the gas diffusion member for the fuel cell and placed between the electrode catalyst layer and the separator, thereby making it possible to significantly reduce the thickness of the fuel cell stack.

[0024] The gas diffusion composite of the present invention can be located on either the cathode side or the anode side, or both.

[0025] The components of the gas diffusion composite material for a fuel cell of the present invention will be described below. Note that, in the solid polymer fuel cell according to the present invention, the components other than the gas diffusion composite material for a fuel cell of the present invention are the same as those of known solid polymer fuel cells, and therefore description thereof will be omitted.

[0026] (1-1. Porous Substrate Sheet) The porous substrate sheet constituting the gas diffusion composite material of the present invention is a sheet-like member made of a conductive material and having a plurality of through-holes.

[0027] The form of the porous substrate sheet is not limited as long as it can achieve the effects of the present invention, and examples thereof include a mesh sheet, a punched sheet, and an expanded sheet.

[0028] In this specification, a "mesh sheet" refers to a sheet-like member formed by weaving thin wires of a constituent material, and the spaces between the woven thin wires form through-spaces (through-holes) that penetrate the mesh in the thickness direction. The thickness of the mesh sheet and the diameter, density, and size of the through-holes may be appropriately designed within a range that does not impair the object of the present invention and maintains strength.

[0029] In this specification, the term "punched sheet" refers to a sheet-like member having a large number of through-holes, which is produced by punching a sheet (strip) of a constituent material with a punching device. The thickness of the punched sheet and the diameter, density, and size of the through-holes may be appropriately designed within a range that does not impair the object of the present invention and maintains strength.

[0030] In this specification, an "expand sheet" refers to a sheet-like member made by cutting slits in a sheet of a constituent material and expanding the slits to form diamond or tortoise shell shapes, etc., and the diamond or tortoise shell shapes formed by expanding the slits become through spaces (through holes) that penetrate the expand sheet in the thickness direction. The diameter and density of the through holes in the expand sheet may be appropriately designed according to the diameter of the through holes, within a range that does not impair the object of the present invention and maintains strength.

[0031] Among the forms of porous substrate sheets, a mesh sheet is preferred. The mesh sheet has a woven structure. Examples of woven structures include plain weave, twill weave, plain tatami weave, and twill tatami weave. "Plain weave" is a weaving method in which vertical and horizontal lines alternately cross one another. "Twill weave" is a weaving method in which vertical and horizontal lines cross every few lines. "Plain tatami weave" is a method of weaving lines like tatami mats. "Twill tatami weave" is a method in which twill weave is applied to plain tatami weave.

[0032] The number of lines (i.e., linear materials) per unit area of ​​the mesh sheet tends to increase in the following order: plain weave < twill weave < plain tatami weave < twill tatami weave. The greater the number of lines per unit area of ​​the mesh sheet, the more smoothly the mesh sheet's surface is. Improved surface smoothness of the mesh sheet can increase the contact area of ​​the gas diffusion member with other components in the fuel cell (e.g., electrode catalyst layer and separator), and increased contact area between components can contribute to improved electrical connectivity between the components.

[0033] The thickness of the porous substrate sheet is 3 μm to 150 μm, preferably 5 μm to 100 μm, 20 μm to 100 μm, 5 μm to 60 μm, or 20 μm to 60 μm. Such a thickness can impart mechanical strength to the gas diffusion composite material of the present invention and ensure self-supporting properties even when a microporous carbon layer is provided. The thickness of the porous substrate sheet can be measured, for example, with a micrometer.

[0034] In the gas diffusion composite material of the present invention, the constituent material of the porous substrate sheet may be selected from materials that have both sufficient durability and electronic conductivity under the operating conditions of a PEFC, specifically, metal materials and carbon materials.

[0035] In this specification, the operating conditions of a PEFC include both the cathode conditions and anode conditions of the PEFC. The cathode conditions of a PEFC refer to the conditions at the cathode during normal operation of the PEFC, where the temperature is from room temperature to about 150°C and a gas containing oxygen such as air is supplied (oxidizing atmosphere), while the anode conditions refer to the conditions at the anode during normal operation of the PEFC, where the temperature is from room temperature to about 150°C and a fuel gas containing hydrogen is supplied (reducing atmosphere).

[0036] There are no limitations on the metal material as long as it does not impair the object of the present invention, but preferred examples include stainless steel, metallic Ti (titanium), and Ti alloys.

[0037] Among porous substrate sheets using metal materials, stainless steel mesh (e.g., SUS304, SUS316, SUS316L, SUS340) is preferred. The thickness of the stainless steel mesh and the diameter, density, and size of the through holes may be appropriately designed within a range that does not impair the object of the present invention and maintains strength.

[0038] The stainless steel mesh can be homemade or commercially available.

[0039] Furthermore, a carbon mesh is preferred as a porous substrate sheet using a carbon material. The carbon mesh is a mesh sheet made of fibrous carbon and has a mesh structure including voids. The thickness of the carbon mesh and the diameter, density, and size of the through-holes may be appropriately designed within a range that does not impair the object of the present invention and maintains strength.

[0040] The carbon mesh can be homemade or commercially available.

[0041] If necessary, the porous substrate sheet may have a conductive material fixed to the surface thereof.

[0042] The microporous carbon layer is formed by applying a coating liquid containing the constituent components of the microporous carbon layer (MPL components) to a porous substrate sheet, but the manner in which the microporous carbon layer is formed depends not only on the MPL components but also on the structure and material of the porous substrate sheet. Because the surface smoothness and the permeability of the coating liquid into the mesh sheet vary depending on the weave of the mesh sheet, an appropriate mesh sheet can be selected depending on the desired structure (structures (A) to (E)).

[0043] (1-2. Microporous Carbon Layer) In the gas diffusion composite material of the present invention, the microporous carbon layer contains a particulate and / or fibrous carbon material and a water-repellent resin. The microporous carbon layer has a smaller pore size, higher density, and superior surface flatness than the porous substrate sheet described above. Therefore, it has excellent electronic conductivity and can reduce contact resistance with the electrode catalyst layer or separator.

[0044] The carbon material constituting the microporous carbon layer is a particulate and / or fibrous carbon material, and the inclusion of a microporous carbon layer containing such a carbon material can impart excellent electrical conductivity to the gas diffusion composite material of the present invention.

[0045] A wide variety of known or commercially available particulate carbon materials can be used. For example, carbon blacks such as ketjen black and acetylene black, graphite, activated carbon, etc. can be used alone or in combination of two or more. The average particle size of the particulate carbon material is usually about 5 nm to 200 nm, preferably about 20 to 80 nm.

[0046] Furthermore, by substituting a part of the particulate carbon material with fibrous carbon material, the current collecting property and gas diffusing property can be further improved.

[0047] As the fibrous carbon material, a wide variety of known or commercially available materials can be used, for example, carbon nanotubes (CNTs), carbon fibers (CFs), etc. can be used alone or in combination of two or more.

[0048] The particulate and / or fibrous carbon material constituting the microporous carbon layer is preferably carbon black, carbon nanotubes, or a mixture thereof.

[0049] The water-repellent resin constituting the microporous carbon layer can be a fluorine-based resin, such as polytetrafluoroethylene resin (PTFE), a copolymer of tetrafluoroethylene and hexafluoropropylene (FEP), a copolymer of tetrafluoroethylene and perfluoropropyl vinyl ether (PFA), or a copolymer of tetrafluoroethylene and ethylene (ETFE), and these can be used alone or in combination of two or more.

[0050] The proportions of the particulate and / or fibrous carbon material and the water-repellent resin that constitute the microporous carbon layer are determined within a range that does not impair the object of the present invention.

[0051] One of the features of the microporous carbon layer in the gas diffusion composite material of the present invention is that it can be formed using the same material as the MPL in the conventionally known gas diffusion layer with MPL. That is, by using a porous substrate sheet as a base, it is possible to form a gas diffusion member (a so-called self-supporting microporous layer) that has sufficient strength to maintain its self-supporting properties and is thinned to the same thickness as the MPL in the gas diffusion layer with MPL (about 20 μm) without using a special carbon material.

[0052] The gas diffusion composite material for a fuel cell of the present invention has a total thickness of 3 μm to 150 μm, preferably 5 μm to 100 μm, 20 μm to 100 μm, 5 μm to 60 μm, or 20 μm to 60 μm. Here, the "total thickness" refers to the total thickness of the porous substrate sheet and the microporous carbon layer. The total thickness can be measured, for example, with a micrometer.

[0053] (1-3. Arrangement of porous base material sheet and microporous carbon layer) As described above, the gas diffusion composite material of the present invention has any one of the following structures (A) to (E). Structure (A): A structure in which the microporous carbon layer covers one side of the porous base material sheet. Structure (B): A structure in which the microporous carbon layer covers both sides of the porous base material sheet. Structure (C): A structure in which the microporous carbon layer covers one side of the porous base material sheet and a part of it penetrates into the porous base material sheet. Structure (D): A structure in which the microporous carbon layer covers one side of the porous base material sheet and a part of the microporous carbon layer penetrates into the porous base material sheet, and the microporous carbon layer reaches from one side of the porous base material sheet to the opposite side. Structure (E): A structure in which the entire porous base material sheet is embedded in the microporous carbon layer

[0054] Structures (A) to (E) of the gas diffusion composite material of the present invention are shown in FIGS. 3(A) to (E), respectively.

[0055] When the gas diffusion composite material of the present invention has the structure (A) in which the microporous carbon layer shown in FIG. 3(A) covers one side of the porous base material sheet, the microporous carbon layer is usually arranged so as to contact the electrode catalyst layer side, and the contact resistance between the electrode catalyst layer and the gas diffusion composite material is reduced. In the case of structure (A), the microporous carbon layer may also be arranged on the separator side. In this case, the contact resistance between the separator and the gas diffusion composite material is reduced.

[0056] When the gas diffusion composite material of the present invention has the structure (B) in which the microporous carbon layer shown in FIG. 3(B) covers both sides of the porous base material sheet, the microporous carbon layer is arranged so as to contact both the electrode catalyst layer side and the separator side, and the contact resistance between the electrode catalyst layer and the gas diffusion composite material and the contact resistance between the separator and the gas diffusion composite material are reduced.

[0057] When the gas diffusion composite material of the present invention has a structure (C) in which the microporous carbon layer shown in FIG. 3(C) covers one side of the porous base material sheet and a part of it penetrates into the porous base material sheet, similar to the case of structure (A), since the microporous carbon layer is usually arranged to contact the electrode catalyst layer side, the contact resistance between the electrode catalyst layer and the gas diffusion composite material is reduced. In the case of structure (C), the microporous carbon layer may also be arranged on the separator side, and in this case, the contact resistance between the separator and the gas diffusion composite material is reduced.

[0058] Further, as shown in FIG. 3(D), in a structure in which the microporous carbon layer covers one side of the porous base material sheet and a part of it penetrates into the porous base material sheet, and the microporous carbon layer reaches from one side to the opposite side of the porous base material sheet (structure (D)), since the component (MPL component) constituting the microporous carbon layer exhibits excellent conductivity, the electric resistance in the thickness direction of the gas diffusion composite material can be reduced. When the porous base material sheet is a mesh sheet, since the permeability of the coating liquid into the mesh sheet changes by changing the fabric structure or mesh diameter of the mesh sheet, the fabric structure, pore diameter, etc. of the porous base material sheet may be appropriately selected so that the MPL component becomes regular inside the porous base material sheet as in the structure shown in FIG. 3(D).

[0059] Also, when the gas diffusion composite material of the present invention has a structure (E) in which the entire porous base material sheet is embedded in the microporous carbon layer shown in FIG. 3(E), the microporous carbon layer is arranged to contact both the electrode catalyst layer side and the separator side, and the contact resistance between the electrode catalyst layer and the gas diffusion composite material and the contact resistance between the separator and the gas diffusion composite material are reduced. At the same time, since the component (MPL component) constituting the microporous carbon layer exhibits better conductivity than the porous base material sheet, the electric resistance in the thickness direction of the gas diffusion composite material can be reduced.

[0060] In the case where the gas diffusion composite material has structure (D) or structure (E), since the component (MPL component) constituting the microporous carbon layer is continuous from one side to the opposite side of the porous base material sheet and exhibits conductivity due to the microporous carbon layer, instead of the conductive porous base material sheet (metal or carbon), a non-conductive porous base material sheet (for example, fluororesin) can also be used.

[0061] That is, another aspect of the present invention is a gas diffusion composite material for a fuel cell, comprising a porous substrate sheet made of a non-conductive material and a microporous carbon layer containing a particulate and / or fibrous carbon material and a water-repellent resin, wherein the thickness of the porous substrate sheet is 3 μm or more and 150 μm or less, and the gas diffusion composite material has either of the following structures (D) and (E): Structure (D): A structure in which the microporous carbon layer covers one side of the porous substrate sheet made of a non-conductive material, and a portion of the microporous carbon layer penetrates into the porous substrate sheet made of a non-conductive material, and the microporous carbon layer reaches from one side to the other side of the porous substrate sheet made of a non-conductive material; and Structure (E): A structure in which the entire porous substrate sheet is embedded in the microporous carbon layer.

[0062] The thickness of the porous substrate sheet made of a non-conductive material is 3 μm to 150 μm, preferably 5 μm to 100 μm, or 5 μm to 50 μm. The overall thickness is 3 μm to 150 μm, preferably 5 μm to 100 μm, 20 μm to 100 μm, 5 μm to 60 μm, or 20 μm to 60 μm. Such a thickness can impart mechanical strength to the gas diffusion composite material of the present invention, and ensure self-supporting properties even when a microporous carbon layer is provided. The thickness of the porous substrate sheet made of a non-conductive material and the overall thickness can be measured, for example, with a micrometer.

[0063] 2. Components other than polymer electrolyte fuel cell and gas diffusion composite material The polymer electrolyte fuel cell of the present invention uses the above-mentioned gas diffusion composite material for fuel cells (self-supporting microporous layer) of the present invention as at least one of the gas diffusion composite materials arranged on the cathode side and the anode side.

[0064] When the gas diffusion composite material for a fuel cell of the present invention has a microporous carbon layer on one side of the porous substrate sheet (structure (A), structure (C), and structure (D)), the gas diffusion composite material for a fuel cell may be arranged so that the side with the microporous carbon layer is in contact with the cathode catalyst layer and / or the anode catalyst layer and the other side without the microporous carbon layer is in contact with the separator, or so that the side with the microporous carbon layer is in contact with the separator and the other side without the microporous carbon layer is in contact with the cathode catalyst layer and / or the anode catalyst layer.

[0065] Furthermore, when the gas diffusion composite material for a fuel cell of the present invention has microporous carbon layers on both sides of the porous substrate sheet (structures (B) and (E)), the gas diffusion composite material for a fuel cell may be arranged so that one side having the microporous carbon layer is in contact with the cathode catalyst layer and / or the anode catalyst layer, and the other side having the microporous carbon layer is in contact with the separator. In this arrangement, the side having the microporous carbon layer is in contact with both the electrode catalyst layer (cathode catalyst layer, anode catalyst layer) side and the separator side, resulting in a lower contact resistance compared to when a gas diffusion composite for a fuel cell having a microporous carbon layer fixed to one side is used.

[0066] Hereinafter, the components of the polymer electrolyte fuel cell of the present invention other than the gas diffusion composite material of the present invention will be described. However, since the components other than the gas diffusion composite material of the present invention are the same as those of known polymer electrolyte fuel cells, they will only be described briefly.

[0067] The membrane electrode assembly (MEA) constituting the polymer electrolyte fuel cell of the present invention includes a solid polymer electrolyte membrane, a cathode catalyst layer bonded to one side of the solid polymer electrolyte membrane, and an anode catalyst layer bonded to the other side of the solid polymer electrolyte membrane.

[0068] The anode catalyst layer and the cathode catalyst layer can be made of conventionally known electrode catalyst layers (e.g., an electrode catalyst layer made of a carbon-based support carrying precious metal fine particles, an oxide support carrying precious metal fine particles, etc.), and therefore detailed explanations thereof will be omitted.

[0069] As the solid polymer electrolyte membrane, any known electrolyte membrane for PEFCs may be used as long as it has proton conductivity and chemical and thermal stability. Examples of electrolyte materials constituting the solid polymer electrolyte membrane include fluorine-based electrolyte materials and hydrocarbon-based electrolyte materials. An electrolyte membrane formed from a fluorine-based electrolyte material is particularly preferred because of its excellent heat resistance, chemical stability, etc.

[0070] As the separator, a known separator can be used, for example, a metal separator, a carbon separator, or the like.

[0071] The polymer electrolyte fuel cell (single cell) of the present invention is stacked in a number appropriate for the power generation performance to form a fuel cell stack, which is then assembled with other associated devices such as a gas supply device and a cooling device before use.

[0072] Although the embodiments of the present invention have been described above, the disclosed embodiments are illustrative in all respects and are not limiting. In particular, matters not explicitly disclosed in the disclosed embodiments, such as the operating conditions of the fuel cell, various parameters, dimensions, weights, and volumes of components, do not deviate from the scope of ordinary practice by a person skilled in the art, and values ​​that can be easily assumed by a person skilled in the art can be used.

[0073] The present invention will be described in more detail below with reference to examples, but is not limited to these. In the following examples, gas diffusion composite members (MPL-composite porous substrate sheets), porous substrate sheets (not composited with MPL), and conventional gas diffusion layers (carbon fiber-based gas diffusion layers with MPL) are collectively referred to as "gas diffusion members."

[0074] <1. Gas Diffusion Member> The following were used as gas diffusion members 1 to 6. The thickness of the gas diffusion member was measured five times with a micrometer (Mitutoyo Corporation, Coolant-proof Micrometer MDC-25MX) and calculated from the average.

[0075] Gas diffusion member 1: Stainless steel mesh (porous substrate sheet) Stainless steel SUS316 / wire mesh (977 mesh) manufactured by Nilaco Corporation was used. The stainless steel mesh sheet was composed of a single layer of twill mesh with a wire diameter of φ13 μm and a thickness of 28 μm. A surface photograph of gas diffusion member 1 (stainless steel mesh) is shown in FIG. 4 .

[0076] Gas diffusion member 2: MPL composite stainless steel mesh (MPL composite porous substrate sheet) The following procedure was used to obtain an MPL composite stainless steel mesh, which is a gas diffusion member 2. 300 μL (300 mg) of pure water and 1500 μL (1695 mg) of polyethylene glycol (PEG) were mixed in a solvent, and 241 mg of highly graphitized carbon black (GCB, Cabot Corporation, FCX200), 576 μL of carbon nanotube dispersion (Meijo Nano Carbon Co., Ltd., MWNT INK) (CNT weight 30 mg), and 22.5 μL of water-repellent resin (DAIKIN Corporation, Polyflon PTFE D-210C) (PTFE weight 30 mg) were added and mixed until uniform to obtain an MPL-forming dispersion. The obtained MPL-forming dispersion was screen-printed onto a stainless steel mesh (gas diffusion member 1) using a screen (screen thickness: 30 μm). Screen printing was performed using a simple screen printer (Print Gokko PG-11, manufactured by Riso Kagaku Corporation) on a stainless steel mesh (gas diffusion member 1) cut slightly larger than the holes in the screen, to obtain gas diffusion member 2 (MPL composite stainless steel mesh). Gas diffusion member 2 had a thickness of 62 μm.

[0077] Gas diffusion member 3: MPL-attached carbon fiber gas diffusion layer (conventional gas diffusion layer) As the gas diffusion member 3, a commercially available MPL-attached gas diffusion layer 22BB (manufactured by SGL Carbon GmbH, Germany, unit area mass 70 gm) made of carbon paper with MPL formed on the surface was used. -2 The gas diffusion member 3 had a thickness of 206 μm.

[0078] Gas Diffusion Member 4: Carbon Mesh (Porous Substrate Sheet) Carbon mesh (bias woven) manufactured by Cosmotec was used as the gas diffusion member 4. The thickness of the gas diffusion member 4 was 45 μm.

[0079] Gas diffusion member 5: MPL composite carbon mesh (MPL composite porous substrate sheet) An MPL composite carbon mesh, which is a gas diffusion member 5, was obtained by the following procedure. 241 mg of GCB, a carbon nanotube dispersion (CNT weight 30 mg), and 22.5 μL of water-repellent resin (PTFE weight 30 mg) were added to a mixed solvent of 300 μL (300 mg) of pure water and 1500 μL (1695 mg) of PEG, and mixed until uniform to obtain an MPL-forming dispersion. The obtained MPL-forming dispersion was screen-printed onto a carbon mesh (gas diffusion member 4) using a screen (screen thickness: 30 μm). For screen printing, a simple screen printing machine (Riso Kagaku Corporation, Print Gokko PG-11) was used, and the screen was cut slightly larger than the holes in the carbon mesh (gas diffusion member 4) to obtain a gas diffusion member 5 (MPL composite carbon mesh). The thickness of the gas diffusion member 5 was 87 μm.

[0080] Gas diffusion member 6: MPL composite carbon mesh (MPL composite porous substrate sheet) A gas diffusion member 6 (MPL composite carbon mesh) was obtained in the same manner as in the manufacturing method of the gas diffusion member 5, except that 1400 μL (1400 mg) of pure water, 750 μL (847.5 mg) of PEG, 120.4 mg of GCB, 15 mg of CNT, and 7.12 mg of PTFE were used. The thickness of the gas diffusion member 6 was 87 μm.

[0081] <2. Evaluation> 2-1. Microstructure Observation Figure 5 shows a surface SEM image of gas diffusion member 2 (MPL composite stainless steel mesh), and Figure 6 shows a cross-sectional SEM image. For reference, Figure 7 shows a surface SEM image of gas diffusion member 3 (conventional gas diffusion layer with MPL), and Figure 8 shows a cross-sectional SEM image. As shown in Figure 5, MPL was uniformly supported over the entire surface of gas diffusion member 2 (MPL composite stainless steel mesh), similar to gas diffusion member 3 (conventional gas diffusion layer with MPL) shown in Figure 7. The cracks observed on the surface of gas diffusion member 2 were determined to be caused by the drying and hardening of the surface material during heat treatment. Furthermore, as shown in Figure 6, no separation of components occurred in the cross section of gas diffusion member 2, similar to the cross section of gas diffusion member 3 shown in Figure 8. Furthermore, MPL components were observed not only on the surface but also on the back side of gas diffusion member 2. From the above, it was determined that the gas diffusion member 2 has a structure (D) (see FIG. 3) in which the MPL component penetrates into the mesh and is continuously connected from the front surface to the back surface.

[0082] FIG. 9 shows a photograph of the appearance of the gas diffusion member 5 (MPL composite carbon mesh). As shown in FIG. 9, the carbon mesh substrate could not be confirmed from the surface, and it was confirmed that MPL was evenly held on the surface. In addition, some of the MPL components penetrated into the carbon mesh, but did not reach the back surface, so it was determined to be structure (C) (see FIG. 3). Similarly, for the gas diffusion member 6 (MPL composite carbon mesh), it was confirmed that MPL was evenly held on the surface, and some of the MPL components penetrated into the carbon mesh, but did not reach the back surface, so it was determined to be structure (C) (see FIG. 3).

[0083] 2-2. Electrochemical evaluation (single cell, initial performance evaluation) A PEFC (single cell) with the following configuration was fabricated and a power generation experiment (IV measurement) was performed. (Solid electrolyte membrane) Nafion membrane (DuPont, Nafion 212, thickness 51 μm) (Anode) Electrode catalyst layer: Pt / C catalyst (Tanaka Kikinzoku Kogyo Co., Ltd.) Gas diffusion layer: Carbon fiber gas diffusion layer (carbon paper) (Cathode) Electrode catalyst layer: Pt / C catalyst (Tanaka Kikinzoku Kogyo Co., Ltd.) Gas diffusion layer: Gas diffusion members 1 to 5

[0084] The single cell power generation evaluation jig incorporating gas diffusion members 1 to 5 was placed in a thermostatic chamber set at 80°C, and a power generation test was carried out under the following conditions. A fuel cell evaluation device (manufactured by Toyo Corporation, model number: PE-8900K) and a potentio / galvanostat (manufactured by Solatron, model number: SI1287) were used. (Anode conditions) Electrode area: 1 cm 2 Supply gas type: 100% H2 Gas supply rate: 139 mL / min Supply gas humidification temperature: 80°C (relative humidity: 100%) (cathode conditions) Electrode area: 1 cm 2 Supply gas type: Air Gas supply rate: 332 mL / min Supply gas humidification temperature: 80°C (relative humidity: 100%)

[0085] (Stainless steel mesh) Figure 10 shows the evaluation results of the current-voltage (IV) characteristics of PEFC (single cell) using gas diffusion members 1 and 2. For reference, data for a single cell using gas diffusion member 3 (a conventional gas diffusion layer with MPL) is also shown.

[0086] As shown in Figure 10, both PEFCs using gas diffusion members 1 and 2 were able to generate electricity, but the PEFC using gas diffusion member 2 composited with MPL exhibited significantly improved IV characteristics compared to gas diffusion member 1 without MPL. Gas diffusion member 2 exhibited performance comparable to that of commercially available gas diffusion member 3 (a conventional gas diffusion layer with MPL). Gas diffusion member 2 also exhibited performance comparable to that of gas diffusion member 3 in terms of activation overvoltage and resistance overvoltage (not shown). From the above, it was confirmed that the power generation performance (IV characteristics) was improved by combining stainless steel mesh with MPL.

[0087] (Carbon mesh) Fig. 11 shows the evaluation results of the IV characteristics of PEFCs (single cells) using gas diffusion members 4 and 5. As shown in Fig. 11, both PEFCs using gas diffusion members 4 and 5 were able to generate electricity, and the PEFC using gas diffusion member 5 composited with MPL was found to have improved IV characteristics compared to gas diffusion member 4 without MPL.

[0088] Figure 12 shows the evaluation results of the IV characteristics of a PEFC (single cell) using gas diffusion member 6. As shown in Figure 12, the PEFC using gas diffusion member 6 exhibited improved IV characteristics compared to gas diffusion member 4 without an MPL, and exhibited performance comparable to that of commercially available gas diffusion member 3 (a conventional gas diffusion layer with an MPL).

[0089] From the above, it was confirmed that the power generation performance (IV characteristics) was improved by combining the carbon mesh with MPL.

[0090] 2-3. Evaluation of Electrical Resistance and Electrical Resistivity Various gas diffusion members, each 1 cm square, were sandwiched between two sheets of carbon paper (EC-TPI-060T, ElectroChem Inc., Raynhan MA, USA) of the same shape and then clamped in a full-cell evaluation jig to measure and evaluate electrical resistivity. First, the electrical resistance of each gas diffusion member was measured by electrochemical impedance (EIS) measurement using an electrochemical property evaluation device, and the electrical resistivity was calculated based on the thickness of the gas diffusion member. All measurements were performed at room temperature and pressure without humidifying or heating the inside of the device.

[0091] Table 1 shows the dimensions of each gas diffusion member (1 × 1 cm (1 cm 2 The table also shows the measurement results of the electrical resistance of each gas diffusion member, the thickness of each gas diffusion member, and the electrical resistivity calculated from the electrical resistance and thickness. Table 1 also shows, as a reference example, carbon paper (EC-TPI-060T, ElectroChem Inc., Raynhan MA, USA), which is commonly used as a gas diffusion layer.

[0092]

[0093] Comparing gas diffusion members 1 and 2, in which the porous substrate sheet is stainless steel mesh, it can be seen that the electrical resistivity is reduced to about 1 / 10 by combining with MPL. As mentioned above, in gas diffusion member 2, the MPL component had permeated to the back surface, which is thought to have improved the conductivity by the MPL component. It was also confirmed that the electrical resistivity was reduced by combining with MPL in gas diffusion members 4 and 5, in which the porous substrate sheet is carbon mesh.

[0094] The present invention is promising as a component of polymer electrolyte fuel cells used in automobiles such as passenger cars and commercial vehicles, as well as in the electric power, gas, and home appliance industries.

Claims

1. A gas diffusion composite material for a fuel cell, comprising: a porous substrate sheet made of a conductive material; and a microporous carbon layer containing particulate and / or fibrous carbon material and a water-repellent resin, wherein the thickness of the porous substrate sheet is 3 μm or more and 150 μm or less, and wherein the gas diffusion composite material for a fuel cell has any one of the following structures (A) to (E). Structure (A): A structure in which the microporous carbon layer covers one side of the porous substrate sheet. Structure (B): A structure in which the microporous carbon layer covers both sides of the porous substrate sheet. Structure (C): A structure in which the microporous carbon layer covers one side of the porous substrate sheet and a part of the microporous carbon layer penetrates into the porous substrate sheet. Structure (D): A structure in which the microporous carbon layer covers one side of the porous substrate sheet and a part of the microporous carbon layer penetrates into the porous substrate sheet, the microporous carbon layer reaching from one side to the opposite side of the porous substrate sheet. Structure (E): A structure in which the entire porous substrate sheet is embedded in the microporous carbon layer.

2. The gas diffusion composite material according to claim 1, wherein the thickness of the porous substrate sheet is from 5 μm to 100 μm.

3. The gas diffusion composite material according to claim 1 or 2, having an overall thickness of 3 μm or more and 150 μm or less.

4. The gas diffusion composite material according to claim 3, having an overall thickness of 5 μm or more and 100 μm or less.

5. A gas diffusion composite material according to any one of claims 1 to 4, wherein the porous substrate sheet is in the form of a mesh sheet, a punched sheet or an expanded sheet.

6. A gas diffusion composite material according to any one of claims 1 to 5, wherein the porous substrate sheet is made of a carbon material.

7. A gas diffusion composite material according to any one of claims 1 to 5, wherein the porous substrate sheet is a carbon mesh.

8. A gas diffusion composite material according to any one of claims 5 to 7, having any one of structures (C) to (E).

9. The gas diffusion composite material according to claim 7, having the structure (C).

10. A gas diffusion composite material according to any one of claims 1 to 5, wherein the porous substrate sheet is made of a metal material.

11. The gas diffusion composite material according to any one of claims 1 to 5, wherein the porous substrate sheet is a stainless steel mesh.

12. The gas diffusion composite material according to claim 11, having any one of structures (C) to (E).

13. The gas diffusion composite material according to claim 11, having a structure (D).

14. A gas diffusion composite material for a fuel cell, comprising a porous substrate sheet made of a non-conductive material, and a microporous carbon layer containing a particulate and / or fibrous carbon material and a water-repellent resin, the thickness of the porous substrate sheet being 3 μm or more and 150 μm or less, and having either of the following structures (D) and (E): Structure (D): A structure in which the microporous carbon layer covers one side of the porous substrate sheet made of the non-conductive material, and a part of the microporous carbon layer penetrates into the porous substrate sheet made of the non-conductive material, and the microporous carbon layer reaches from one side to the opposite side of the porous substrate sheet made of the non-conductive material; Structure (E): A structure in which the entire porous substrate sheet is embedded in the microporous carbon layer.

15. A gas diffusion composite material for a fuel cell according to any one of claims 1 to 14, wherein the particulate and / or fibrous carbon material constituting the microporous carbon layer is carbon black, carbon nanotubes, or a mixture thereof.

16. A solid polymer electrolyte fuel cell comprising: a membrane electrode assembly having a solid polymer electrolyte membrane, a cathode catalyst layer bonded to one side of the solid polymer electrolyte membrane, and an anode catalyst layer bonded to the other side of the solid polymer electrolyte membrane; a pair of gas diffusion layers laminated on the cathode catalyst layer and the anode catalyst layer, respectively; and a pair of separators sandwiching the membrane electrode assembly via the gas diffusion layers, wherein at least one of the pair of gas diffusion layers is a gas diffusion composite material for a fuel cell according to any one of claims 1 to 15.

Citation Information

Patent Citations

  • Fuel cell diffusion layer, its manufacturing method, and manufacturing device

    JP2002124266A

  • Gas diffusion layer, method for producing the same and membrane electrode assembly for fuel cell using the gas diffusion layer, and fuel cell

    JP2014216232A

  • Method of manufacturing metal porous body for fuel cell, and fuel cell

    JP2015228338A

  • Polymer electrolyte fuel cell and porous metal gas diffusion layer

    JP2024043798A

  • Gas diffusion electrode substrate, and membrane electrode assembly and fuel cell provided therewith

    WO2015125748A1