Quantum dot film layer patterning method and quantum dot light-emitting device
By using a high transmittance organic material layer to protect the quantum dot material layer in the quantum dot film layer patterning method, the problem of the photoluminescence quantum yield reduction after the quantum dot film is exposed to the atmospheric environment in the photolithography process is solved, and the photoluminescence quantum yield is achieved. High efficiency and high performance QLED device preparation.
Patent Information
- Application Number
- PCT/CN2023/083178
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-22
- Publication Date
- 2024-11-28
AI Technical Summary
In the prior art, after the quantum dot film is exposed to the atmospheric environment in the photolithography process, the photoluminescent quantum yield is significantly reduced, affecting the efficiency and performance of QLED devices.
A quantum dot film layer patterning method is adopted, first forming a quantum dot material layer on the substrate, and then forming an organic material layer on it, an organic material layer with high transmittance is protected by a high-volume layer, so that it can be made when exposed. Crosslinking occurs or a salt insoluble in the developer is generated, thereby slowing down the PLQY.
Effectively protect the quantum dot material layer, slow down the reduction of photoluminescent quantum yield, improve the efficiency and performance of QLED devices, and is suitable for the preparation of high-efficiency and high-performance QLED devices.
Smart Images

Figure CN2023083178_28112024_PF_FP_ABST
Abstract
Description
Quantum dot film patterning method and quantum dot light-emitting device Technical Field
[0001] The present disclosure relates to the field of display technology, and in particular to a quantum dot film patterning method and a quantum dot light-emitting device. Background Art
[0002] Quantum Dot Light Emitting Diodes (QLEDs) are the most promising next-generation self-luminous display technology. Compared to OLED technology, QLEDs offer significant advantages such as lower energy consumption, higher color purity, and a wider color gamut. Precise fabrication of QLED subpixel regions is a prerequisite for achieving high-resolution display devices. Patterning quantum dot films on substrates through photolithography and development processes is an effective way to achieve high pixel density (and high resolution) in self-luminous QLED display products.
[0003] At present, the technology for forming quantum dot film layers needs to be further improved.
[0004] The above information disclosed in this Background section is only for enhancement of understanding of the background of the present disclosure and therefore it may contain information that does not form the prior art that is already known to a person of ordinary skill in the art.
[0005] Summary of the Invention
[0006] The purpose of the present disclosure is to provide a quantum dot film patterning method and a quantum dot light-emitting device, which can help slow down the reduction of the PLQY of the quantum dot material layer during exposure.
[0007] To achieve the above-mentioned purpose, the present invention adopts the following technical solutions:
[0008] According to a first aspect of the present disclosure, a method for patterning a quantum dot film layer is provided, comprising:
[0009] forming a quantum dot material layer on one side of the substrate;
[0010] forming an organic material layer on a side of the quantum dot material layer away from the substrate, wherein the transmittance of the organic material layer in the ultraviolet band and the visible light band is not less than 80%;
[0011] exposing a predetermined area of the substrate so that the material in the quantum dot material layer located in the predetermined area is cross-linked or generates a salt insoluble in a developer, or / and the material in the organic material layer located in the predetermined area is cross-linked;
[0012] The organic material layer and the quantum dot material layer in non-preset areas of the substrate are removed.
[0013] In an exemplary embodiment of the present disclosure, the material in the organic material layer includes a hydrocarbon mixture having 18-30 carbon atoms.
[0014] In an exemplary embodiment of the present disclosure, the material in the organic material layer further includes a first photosensitive cross-linking agent.
[0015] In an exemplary embodiment of the present disclosure, the hydrocarbon mixture includes 80%-100% of straight-chain alkanes and 0%-20% of other hydrocarbons by weight, and the other hydrocarbons include any one of branched alkanes, cycloalkanes, alkenes, alkynes, or a combination thereof.
[0016] In an exemplary embodiment of the present disclosure, the photosensitive crosslinking agent accounts for 1-30% of the hydrocarbon mixture by weight.
[0017] In an exemplary embodiment of the present disclosure, the material in the organic material layer includes paraffin wax.
[0018] In an exemplary embodiment of the present disclosure, the initial melting temperature of the material in the organic material layer is no greater than 60°C.
[0019] In an exemplary embodiment of the present disclosure, the initial thickness of the organic material layer is 20 nm-80 nm.
[0020] In an exemplary embodiment of the present disclosure, the material of the quantum dot material layer includes a first quantum dot body, a second quantum dot body, a quantum dot ligand, and a second photosensitive crosslinker;
[0021] The quantum dot ligand is connected to the first quantum dot body and / or the second quantum dot body through a coordination bond;
[0022] The quantum dot ligand comprises a first photosensitive group, which is located at the end of the quantum dot ligand molecular structure. The second photosensitive crosslinker is used to induce a crosslinking reaction in the first photosensitive group.
[0023] In an exemplary embodiment of the present disclosure, the first photosensitive group contains a carbon-carbon double bond, or a saturated 3-5 membered heterocyclic structure containing O or S.
[0024] In an exemplary embodiment of the present disclosure, the material of the quantum dot material layer includes a first quantum dot body, a second quantum dot body, a quantum dot ligand and a photoinitiator;
[0025] The quantum dot ligand includes a first quantum dot ligand and a second quantum dot ligand, wherein the first quantum dot ligand is connected to the first quantum dot body through a coordination bond, and the second quantum dot ligand is connected to the second quantum dot body through a coordination bond;
[0026] The first quantum dot ligand comprises a crosslinkable group, which is located at the end of the first quantum dot ligand molecular structure; the second quantum dot ligand comprises a second photosensitive group, which has a structure of -AB, where A is an imino group and B is a protecting group;
[0027] Under light conditions, the second photosensitive group can remove the protective group under the action of the photosensitive initiator to form an amino group; the crosslinkable group can produce crosslinks with the amino group formed by the second photosensitive group removing the protective group or form a salt insoluble in the developer; or the crosslinkable group can produce crosslinks with the amino group formed by the second photosensitive group removing the protective group after being activated by an activator or form a salt insoluble in the developer.
[0028] In an exemplary embodiment of the present disclosure, the crosslinkable group is selected from an epoxy group, a carboxylic acid group or a sulfonic acid group.
[0029] In an exemplary embodiment of the present disclosure, the material in the quantum dot material layer includes a quantum dot body and a quantum dot ligand, the quantum dot ligand includes a coordination group, and the quantum dot body is connected to the quantum dot body through the coordination group;
[0030] The quantum dot ligand comprises a structure -YZ, wherein Z is a solubilizing group selected from a polar group; Y comprises a connecting group and a third photosensitive group connected to each other, wherein the connecting group is connected between the coordinating group and the third photosensitive group; and the connecting group is selected from an alkylene group;
[0031] The third photosensitive group can break bonds under light conditions to decompose the interconnected quantum dot body and the quantum dot ligand into a first material comprising the interconnected quantum dot body, the coordination group and the connecting group, and a second material comprising the solubilizing group;
[0032] The second material is soluble in a developer, and the first material is insoluble in a developer.
[0033] In an exemplary embodiment of the present disclosure, the material in the quantum dot material layer includes a first quantum dot body, a second quantum dot body, a quantum dot ligand, and a third photosensitive cross-linking agent;
[0034] The quantum dot ligand is connected to the first quantum dot body and / or the second quantum dot body through a coordination bond, and the quantum dot ligand contains an alkane chain;
[0035] The third photosensitive crosslinker comprises at least two fourth photosensitive groups, and the fourth photosensitive groups are located at the ends of the molecular structure of the third photosensitive crosslinker;
[0036] The fourth photosensitive group can undergo a carbon-hydrogen insertion reaction with the alkane chain in the quantum dot ligand under light conditions.
[0037] In an exemplary embodiment of the present disclosure, the fourth photosensitive group is selected from a structure comprising a benzophenone group, an azide group, a diazo group or a diaziridine group.
[0038] In an exemplary embodiment of the present disclosure, the material of the quantum dot material layer includes a quantum dot body and at least one quantum dot ligand, and the quantum dot ligand is connected to the quantum dot body through a coordination bond;
[0039] Among the quantum dot ligands, at least one of the quantum dot ligands contains an alkane chain in its molecular structure.
[0040] In an exemplary embodiment of the present disclosure, the quantum dot material layer and the organic material layer are formed in an inert gas or vacuum environment;
[0041] The step of exposing the predetermined area of the substrate is performed in an atmospheric environment.
[0042] In an exemplary embodiment of the present disclosure, the step of removing the organic material layer and the quantum dot material layer in non-preset areas of the substrate includes:
[0043] Performing development to remove the organic material layer and the quantum dot material layer in the non-preset area;
[0044] Wherein, the organic material layer located in the preset area is cross-linked during exposure.
[0045] In an exemplary embodiment of the present disclosure, performing development to remove the organic material layer and the quantum dot material layer in non-preset areas of the substrate includes:
[0046] Performing a first development using a first developer to remove the organic material layer in the non-preset area;
[0047] Performing a second development using a second developer to remove the quantum dot material layer in the non-preset area;
[0048] The first developing solution and the second developing solution are different.
[0049] In an exemplary embodiment of the present disclosure, the step of removing the organic material layer and the quantum dot material layer in non-preset areas of the substrate includes:
[0050] heating the non-preset area and rotating the substrate to melt the organic material layer located in the non-preset area and allow the melted organic material layer to spin out under the action of centrifugal force;
[0051] Performing development to remove the quantum dot material layer located in the non-preset area;
[0052] During exposure, the quantum dot material layer located in the predetermined area undergoes cross-linking or generates salt that is insoluble in a developer.
[0053] In an exemplary embodiment of the present disclosure, the step of removing the organic material layer and the quantum dot material layer in non-preset areas of the substrate includes:
[0054] removing at least a portion of the organic material layer located in the preset area and at least a portion of the organic material layer located in the non-preset area using a first solvent, wherein the temperature of the first solvent is 60° C.-90° C.;
[0055] Performing development using a second developer to remove the quantum dot material layer located in the non-preset area;
[0056] During exposure, the quantum dot material layer located in the predetermined area undergoes cross-linking or generates salt that is insoluble in a developer.
[0057] In an exemplary embodiment of the present disclosure, the temperature of the first developer is less than 60° C.;
[0058] The relative dielectric constant of the second developer is greater than the relative dielectric constant of the first developer.
[0059] In an exemplary embodiment of the present disclosure, the temperature for heating the non-preset area is 70°C-110°C.
[0060] In an exemplary embodiment of the present disclosure, after being treated with the first solvent, the thickness of the organic material layer is no more than 3 nm, or partial voids appear in the organic material layer.
[0061] In an exemplary embodiment of the present disclosure, after removing the organic material layer and the quantum dot material layer in non-preset areas of the substrate, the step further includes:
[0062] The substrate is placed horizontally, subjected to thermal annealing treatment at 60° C.-100° C. for 5 min-30 min, and then cooled to below 35° C.
[0063] In an exemplary embodiment of the present disclosure, after removing the organic material layer and the quantum dot material layer in non-preset areas of the substrate, the step further includes:
[0064] removing at least a portion of the organic material layer located in the predetermined area using a second solvent, wherein the temperature of the second solvent is 60° C.-90° C.;
[0065] The substrate is heated and dried.
[0066] In an exemplary embodiment of the present disclosure, after removing the organic material layer and the quantum dot material layer in non-preset areas of the substrate, the step further includes:
[0067] Heating the substrate and rotating it, and washing the rotating substrate with a third solvent to remove at least a portion of the remaining organic material layer, wherein the temperature of the third solvent is 70° C. to 110° C.;
[0068] The substrate is heated and dried.
[0069] In an exemplary embodiment of the present disclosure, the first photosensitive crosslinker molecular structure contains at least two fifth photosensitive groups, and the fifth photosensitive groups are located at the ends of the first photosensitive crosslinker molecular structure;
[0070] The fifth photosensitive group is selected from a structure comprising a benzophenone group, an azide group, a diazo group or a diaziridine group.
[0071] In an exemplary embodiment of the present disclosure, the substrate comprises:
[0072] substrate;
[0073] A pixel definition layer is provided on one side of the base substrate, wherein the pixel definition layer has a plurality of openings, and the quantum dot material layer is at least partially formed in the openings;
[0074] Wherein, in a direction perpendicular to the base substrate, the height of the pixel definition layer does not exceed 1.5 μm.
[0075] According to a second aspect of the present disclosure, a quantum dot light-emitting layer is provided, which is manufactured using the quantum dot film patterning method described in the first aspect.
[0076] According to a third aspect of the present disclosure, a quantum dot light-emitting device is provided, comprising the quantum dot light-emitting layer as described in the second aspect.
[0077] In an exemplary embodiment of the present disclosure, a quantum dot light-emitting device includes:
[0078] substrate;
[0079] A pixel definition layer is provided on one side of the base substrate, and the pixel definition layer has a plurality of openings;
[0080] A quantum dot light-emitting layer is provided on one side of the base substrate and is located in the opening;
[0081] The organic layer is provided on a side of the quantum dot light-emitting layer away from the base substrate. The transmittance of the organic layer in the ultraviolet band and the visible light band is not less than 80%, and the melting temperature of the material in the organic layer does not exceed 110°C.
[0082] In an exemplary embodiment of the present disclosure, the thickness of the organic layer does not exceed 20 nm.
[0083] In an exemplary embodiment of the present disclosure, the thickness of the organic layer does not exceed 3 nm, and the organic material layer within a single opening is a discontinuous film layer having a plurality of cavities.
[0084] In an exemplary embodiment of the present disclosure, the material in the organic layer includes paraffin wax.
[0085] In an exemplary embodiment of the present disclosure, the quantum dot light-emitting layer has a cross-linked network structure, or / and
[0086] The organic layer has a cross-linked network structure or a salt insoluble in a developer.
[0087] In an exemplary embodiment of the present disclosure, the quantum dot light emitting device further comprises a first electrode, a second electrode, a first carrier transport layer, and a second carrier transport layer;
[0088] The first electrode is provided between the base substrate and the quantum dot light-emitting layer, and the first carrier transport layer is provided between the first electrode and the quantum dot light-emitting layer;
[0089] The second carrier transport layer is provided on a side of the organic layer away from the base substrate, and the second electrode is provided on a side of the second carrier transport layer away from the base substrate.
[0090] The quantum dot film patterning method provided by the present disclosure forms an organic material layer on the surface of the quantum dot material layer before exposure. The organic material layer can protect the quantum dot material layer and help slow down the reduction of the PLQY of the quantum dot material layer during exposure, providing a basis for the production of high-efficiency and high-performance QLED devices. BRIEF DESCRIPTION OF THE DRAWINGS
[0091] The above and other features and advantages of the present disclosure will become more apparent by describing in detail example embodiments thereof with reference to the accompanying drawings.
[0092] FIG1 is a schematic diagram of the PLQY change of an existing quantum dot film during exposure;
[0093] FIG2 is a schematic diagram of a substrate structure in an exemplary embodiment of the present disclosure;
[0094] FIG3 is a schematic structural diagram of forming a quantum dot material layer 200 in an exemplary embodiment of the present disclosure;
[0095] FIG4 is a schematic structural diagram of forming an organic material layer 300 in an exemplary embodiment of the present disclosure;
[0096] FIG5 is a schematic diagram of an exposure structure in an exemplary embodiment of the present disclosure;
[0097] FIG6 is a schematic structural diagram of removing the organic material layer 300 and the quantum dot material layer 200 in non-preset areas in an exemplary embodiment of the present disclosure;
[0098] FIG7 is a schematic structural diagram of a quantum dot material layer 201 formed in an exemplary embodiment of the present disclosure;
[0099] FIG8 is a schematic structural diagram of forming an organic material layer 301 in an exemplary embodiment of the present disclosure;
[0100] FIG9 is a schematic diagram of an exposure structure in an exemplary embodiment of the present disclosure;
[0101] FIG10 is a schematic structural diagram of an exemplary embodiment of the present disclosure in which the organic material layer 301 and the quantum dot material layer 201 in non-preset areas are removed;
[0102] FIG11 is a schematic diagram of a structure of forming a quantum dot material layer 202 in an exemplary embodiment of the present disclosure;
[0103] FIG12 is a schematic structural diagram of forming an organic material layer 302 in an exemplary embodiment of the present disclosure;
[0104] FIG13 is a schematic diagram of an exposure structure in an exemplary embodiment of the present disclosure;
[0105] FIG14 is a schematic structural diagram of an exemplary embodiment of the present disclosure in which the organic material layer 302 and the quantum dot material layer 202 in non-preset areas are removed;
[0106] FIG15 is a schematic diagram of the structure after further processing of the organic material layer in an exemplary embodiment of the present disclosure;
[0107] FIG16 is a schematic structural diagram of an organic material layer after further processing in another exemplary embodiment of the present disclosure;
[0108] FIG17 is a schematic structural diagram of another exemplary embodiment of the present disclosure after further processing of the organic material layer;
[0109] FIG18 is a schematic diagram of a structure of a quantum dot light emitting device formed in an exemplary embodiment of the present disclosure;
[0110] FIG19 is a schematic diagram of a structure of a quantum dot light-emitting device formed in another exemplary embodiment of the present disclosure;
[0111] FIG20 is a schematic diagram of a structure of a quantum dot light-emitting device formed in another exemplary embodiment of the present disclosure;
[0112] FIG21 is a schematic diagram of a structure of a quantum dot light-emitting device formed in another exemplary embodiment of the present disclosure;
[0113] FIG22 is a schematic structural diagram of another exemplary embodiment of the present disclosure in which the organic material layer 300 and the quantum dot material layer 200 in non-preset areas are removed;
[0114] FIG23 is a schematic structural diagram of forming a quantum dot material layer 201 in another exemplary embodiment of the present disclosure;
[0115] FIG24 is a schematic structural diagram of forming an organic material layer 301 in another exemplary embodiment of the present disclosure;
[0116] FIG25 is a schematic diagram of an exposure structure in another exemplary embodiment of the present disclosure;
[0117] FIG26 is a schematic structural diagram of another exemplary embodiment of the present disclosure in which the organic material layer 301 and the quantum dot material layer 201 in non-preset areas are removed;
[0118] FIG27 is a schematic structural diagram of forming a quantum dot material layer 202 in another exemplary embodiment of the present disclosure;
[0119] FIG28 is a schematic structural diagram of forming an organic material layer 302 in another exemplary embodiment of the present disclosure;
[0120] FIG29 is a schematic diagram of an exposure structure in another exemplary embodiment of the present disclosure;
[0121] FIG30 is a graph showing changes in exposure PLQY after an organic material layer is formed on a quantum dot material layer in an exemplary embodiment of the present disclosure;
[0122] FIG31 is a spectrum diagram after an organic material layer is formed on a quantum dot material layer in an exemplary embodiment of the present disclosure;
[0123] FIG. 32 is a graph showing changes in light transmittance of an organic material layer in an exemplary embodiment of the present disclosure.
[0124] The main components in the figure are described as follows:
[0125] 100 - base; 101 - substrate; 110 - first electrode; 120 - pixel definition layer; 130 - first carrier transport layer; 200 - quantum dot material layer; 300 - organic material layer; 400 - second carrier transport layer; 500 - second electrode; 600 - encapsulation layer. DETAILED DESCRIPTION
[0126] Example embodiments will now be described more fully with reference to the accompanying drawings. However, the example embodiments can be implemented in many forms and should not be construed as limited to the examples set forth herein; rather, these embodiments are provided so that this disclosure will be more comprehensive and complete and will fully convey the concepts of the example embodiments to those skilled in the art. The described features, structures, or characteristics may be combined in any suitable manner in one or more embodiments. In the following description, numerous specific details are provided to provide a thorough understanding of the embodiments of the present disclosure.
[0127] In the drawings, the thickness of regions and layers may be exaggerated for clarity. The same reference numerals in the drawings denote the same or similar structures, and thus their detailed description will be omitted.
[0128] The described features, structures or characteristics may be combined in any suitable manner in one or more embodiments. In the following description, many specific details are provided to provide a full understanding of the embodiments of the present disclosure. However, those skilled in the art will appreciate that the technical solutions of the present disclosure can be practiced without one or more of the specific details, or other methods, components, materials, etc. can be adopted. In other cases, well-known structures, materials or operations are not shown or described in detail to avoid obscuring the main technical ideas of the present disclosure.
[0129] When a structure is “on” another structure, it may mean that the structure is integrally formed on the other structure, or that the structure is “directly” disposed on the other structure, or that the structure is “indirectly” disposed on the other structure via another structure.
[0130] The terms "a," "an," and "the" are used to indicate the presence of one or more elements / components; the terms "including" and "having" are used to indicate an open-ended inclusiveness and mean that additional elements / components / etc. may be present in addition to the listed elements / components / etc. The terms "first," "second," etc. are used merely as labels and do not limit the quantity of the items to which they refer.
[0131] In the related art, in order to achieve the high performance of QLED devices, many functional layers in QLED devices, including quantum dot layers, are usually coated or / and deposited in an inert atmosphere environment (some processes are in a vacuum environment). For example, common processes such as spin coating or inkjet printing are all carried out in a nitrogen atmosphere environment. In the process of preparing quantum dot films by photolithography patterning, the exposure process (photolithography machine) and development process (development equipment) used are all mature semiconductor process equipment, but the above-mentioned mature related semiconductor equipment are all carried out in an air (or atmospheric) environment. To establish photolithography and / or development equipment in an inert gas atmosphere will be a huge equipment development cost and is not realistic. Therefore, the photolithography method for quantum dot patterning requires exposure to an air atmosphere for related process. The reality is that the photoluminescence quantum yield (PLQY) of the quantum dot material will be significantly reduced within 0-30 minutes after exposure to the atmosphere, and the most serious reduction can be more than 70%. For details, please refer to the experimental data shown in Figure 1.
[0132] In Figure 1, different quantum dot solutions were spin-coated onto glass substrates to form quantum dot films. The PLQY (photoluminescence quantum yield) of the quantum dot films was measured every five minutes using an integrating sphere. In Figure 1, the ordinate represents the ratio of the PLQY of the quantum dot film at time t (denoted as PLQY-t) to the PLQY at time 0 after spin-coating the quantum dot film (denoted as PLQY-t0), while the abscissa represents the values at different times. QD-I to QD-VI represent different quantum dot samples. The experimental results demonstrate a time-dependent decrease in the PLQY of quantum dot films exposed to air. The results show that the PLQY of the QD films decreases significantly (by 10% to 35%) after just 5 minutes of exposure to air. Although the rate of PLQY decreases gradually after 15 to 20 minutes, the PLQY has already decreased by 20% to 60%, reaching a minimum decrease of approximately 70% after 30 minutes. This is highly detrimental to improving QLED device efficiency. Since transferring the photolithography process to an inert gas atmosphere (such as a nitrogen glove box) is extremely costly and impractical, making the preparation of photolithographically patterned quantum dot films resistant to atmospheric conditions is essential for achieving high-efficiency and high-performance QLED devices.
[0133] As shown in FIG2 to FIG6 , a method for patterning a quantum dot film layer is provided in an embodiment of the present disclosure. The method can be used to form a quantum dot light-emitting device. The method for patterning a quantum dot film layer includes:
[0134] As shown in FIG3 , in step S100 , a quantum dot material layer 200 is formed on one side of a substrate 100 ;
[0135] As shown in FIG4 , in step S200 , an organic material layer 300 is formed on a side of the quantum dot material layer 200 away from the substrate 100 , and the transmittance of the organic material layer 300 in the ultraviolet band and the visible light band is not less than 80%;
[0136] As shown in FIG. 5 , in step S300 , a predetermined area of the substrate 100 is exposed, so that the material in the quantum dot material layer 200 in the predetermined area is cross-linked or generates a salt insoluble in a developer, or / and the material in the organic material layer 300 in the predetermined area is cross-linked;
[0137] As shown in FIG. 6 , in step S400 , the organic material layer 300 and the quantum dot material layer 200 in non-preset areas of the substrate 100 are removed.
[0138] The quantum dot film patterning method provided by the present disclosure forms an organic material layer 300 on the surface of the quantum dot material layer 200 before exposure. The organic material layer 300 can protect the quantum dot material layer 200 and help slow down the reduction of the PLQY of the quantum dot material layer 200 during exposure, providing a basis for the production of high-efficiency and high-performance QLED devices.
[0139] The following describes in detail the steps of patterning the quantum dot film layer provided in the embodiment of the present disclosure with reference to the accompanying drawings:
[0140] As shown in FIG. 2 and FIG. 3 , in step S100 , a quantum dot material layer 200 is formed on one side of a substrate 100 .
[0141] In some embodiments of the present disclosure, the base 100 includes a base substrate 101 and a pixel definition layer 120. The pixel definition layer 120 is arranged on one side of the base substrate 101. The pixel definition layer 120 has multiple openings, and the quantum dot material layer 200 is at least partially formed in the openings.
[0142] Furthermore, in a direction perpendicular to the base substrate 101 , the height of the pixel definition layer 120 does not exceed 1.5 μm.
[0143] In the present disclosure, the quantum dot material in the quantum dot material layer 200 can be a material having photosensitive crosslinking properties or a material not having photosensitive crosslinking properties. In different embodiments, the quantum dot material can be different. It should be noted that, herein, a quantum dot material having photosensitive crosslinking properties means that such quantum dot material can crosslink under light conditions (exposure) to form a network structure, or to form a product that is insoluble in a developer.
[0144] In the present disclosure, the quantum dot material in the quantum dot material layer 200 may include a quantum dot body and at least one quantum dot ligand, wherein the quantum dot ligand may be connected to the surface of the quantum dot body via a coordination bond.
[0145] In some embodiments, at least one of the multiple quantum dot ligands comprises an alkane chain in its molecular structure.
[0146] Quantum dots (QDs) are inorganic semiconductor nanoparticles synthesized via a solution method and are sized between 1 and 10 nm, which is approximately or smaller than the particle's exciton Bohr radius. Due to their small size and large specific surface area, quantum dots are prone to agglomeration, and they also have numerous surface defects. Therefore, when used, the surface of quantum dots is often coated with organic surface ligands, which provide both protection and improved solubility in solution. The migration of charge carriers (electrons and holes) within quantum dots is confined to the interior of the quantum dots, giving them unique optical and electrical properties. Due to their unique size-dependent properties, the absorption and luminescence properties of quantum dots can be easily tuned by controlling the particle size, shape, or surface structure.
[0147] In the present disclosure, the quantum dot body refers to the quantum dot mentioned above, which can be a semiconductor nanocrystal and can have a variety of shapes, such as spherical, conical, multi-armed and / or cubic nanoparticles, nanotubes, nanowires, nanofibers, nanoplate particles, quantum rods, or quantum sheets. Here, the quantum rod can be a quantum dot body having an aspect ratio (length to diameter ratio) (length: width ratio) greater than about 1, such as greater than or equal to about 2, greater than or equal to about 3, or greater than or equal to about 5. For example, the quantum rod can have an aspect ratio of less than or equal to about 50, less than or equal to about 30, or less than or equal to about 20.
[0148] The quantum dot bodies can have a particle diameter (average maximum particle length for non-spherical shapes), for example, from about 1 nm to about 100 nm, from about 1 nm to about 80 nm, from about 1 nm to about 50 nm, or from about 1 nm to 20 nm.
[0149] The energy band gap of the quantum dot body can be controlled according to the size and composition of the quantum dot body, and thus the emission wavelength can be controlled. For example, when the size of the quantum dot body increases, the quantum dot body may have a narrow energy band gap and thus be configured to emit light in a relatively long wavelength region, and when the size of the quantum dot body decreases, the quantum dot body may have a wide energy band gap and thus be configured to emit light in a relatively short wavelength region. For example, the quantum dot body may be configured to emit light in a predetermined wavelength region in the visible light region according to its size and / or composition. For example, the quantum dot body may be configured to emit a second color light, a third color light, or a first color light, the second color light may have, for example, a peak emission wavelength (λmax) in the range of about 430 nm to about 480 nm, the third color light may have, for example, a peak emission wavelength (λmax) in the range of about 600 nm to about 650 nm, and the first color light may have, for example, a peak emission wavelength (λmax) in the range of about 520 nm to about 560 nm, but is not limited thereto.
[0150] For example, the average particle size of the quantum dot bodies formulated to emit light of the second color can be, for example, less than or equal to about 4.5 nm, and, for example, less than or equal to about 4.3 nm, less than or equal to about 4.2 nm, less than or equal to about 4.1 nm, or less than or equal to about 4.0 nm. Within a range, for example, the average particle size of the quantum dot bodies can be from about 2.0 nm to about 4.5 nm, such as from about 2.0 nm to about 4.3 nm, from about 2.0 nm to about 4.2 nm, from about 2.0 nm to about 4.1 nm, or from about 2.0 nm to about 4.0 nm.
[0151] The quantum dot body can have a quantum yield of, for example, greater than or equal to about 10%, greater than or equal to about 20%, greater than or equal to about 30%, greater than or equal to about 50%, greater than or equal to about 60%, greater than or equal to about 70%, or greater than or equal to about 90%.
[0152] The quantum dot body can have a relatively narrow full width at half maximum (FWHM). Here, FWHM is the width corresponding to half the wavelength of the peak absorption point. When the FWHM is narrow, it can be configured to emit light in a narrow wavelength region and obtain higher color purity. The quantum dot body may have a FWHM of, for example, less than or equal to about 50 nm, less than or equal to about 49 nm, less than or equal to about 48 nm, less than or equal to about 47 nm, less than or equal to about 46 nm, less than or equal to about 45 nm, less than or equal to about 44 nm, less than or equal to about 43 nm, less than or equal to about 42 nm, less than or equal to about 41 nm, less than or equal to about 40 nm, less than or equal to about 39 nm, less than or equal to about 38 nm, less than or equal to about 37 nm, less than or equal to about 36 nm, less than or equal to about 35 nm, less than or equal to about 34 nm, less than or equal to about 33 nm, less than or equal to about 32 nm, less than or equal to about 31 nm, less than or equal to about 30 nm, less than or equal to about 29 nm, or less than or equal to about 28 nm. Within a range, it can have a FWHM of, for example, about 2 nm to about 49 nm, about 2 nm to about 48 nm, about 2 nm to about 47 nm, about 2 nm to about 46 nm, about 2 nm to about 45 nm, about 2 nm to about 44 nm, about 2 nm to about 43 nm, about 2 nm to about 42 nm, about 2 nm to about 41 nm, about 2 nm to about 40 nm, about 2 nm to about 39 nm, about 2 nm to about 38 nm, about 2 nm to about 37 nm, about 2 nm to about 36 nm, about 2 nm to about 35 nm, about 2 nm to about 34 nm, about 2 nm to about 33 nm, about 2 nm to about 32 nm, about 2 nm to about 31 nm, about 2 nm to about 30 nm, about 2 nm to about 29 nm, or about 2 nm to about 28 nm.
[0153] For example, the quantum dot body may include a II-VI semiconductor compound, a III-V semiconductor compound, a IV-VI semiconductor compound, a IV semiconductor, a I-III-VI semiconductor compound, a I-II-IV-VI semiconductor compound, a II-III-V semiconductor compound, or a combination thereof. The II-VI semiconductor compound may be, for example, selected from: a binary compound such as CdSe, CdTe, ZnS, ZnSe, ZnTe, ZnO, HgS, HgSe, HgTe, MgSe, MgS, or a mixture thereof; a ternary compound such as CdSeS, CdSeTe, CdSTe, ZnSeS, ZnSeTe, ZnSTe, HgSeS, HgSeTe, HgSTe, CdZnS, CdZnSe, CdZnT e, CdHgS, CdHgSe, CdHgTe, HgZnS, HgZnSe, HgZnTe, MgZnSe, MgZnS, or mixtures thereof; and quaternary compounds such as HgZnTeS, CdZnSeS, CdZnSeTe, CdZnSTe, CdHgSeS, CdHgSeTe, CdHgSTe, HgZnSeS, HgZnSeTe, HgZnSTe, or mixtures thereof, but are not limited thereto. The III-V semiconductor compounds may be selected, for example, from binary compounds such as GaN, GaP, GaAs, GaSb, AlN, AlP, AlAs, AlSb, InN, InP, InAs, InSb, or mixtures thereof; ternary compounds such as GaNPs, GaNAs, GaNSb, GaPAs, GaPSb, AlNPs, AlNAs, AlNSb, AlPAs, AlPSb, InNPs, InNAs, InNSb, InPAs, InPSb, or mixtures thereof; and quaternary compounds such as GaAlNPs, GaAlNAs, GaAlNSb, GaAlPAs, GaAlPSb, GaInNPs, GaInNAs, GaInNSb, GaInPAs, GaInPSb, InAlNPs, InAlNAs, InAlNSb, InAlPAs, InAlPSb, or mixtures thereof, but are not limited thereto. The IV-VI semiconductor compounds may be selected, for example, from: binary compounds such as SnS, SnSe, SnTe, PbS, PbSe, PbTe, or mixtures thereof; ternary compounds such as SnSeS, SnSeTe, SnSTe, PbSeS, PbSeTe, PbSTe, SnPbS, SnPbSe, SnPbTe, or mixtures thereof; and quaternary compounds such as SnPbSSe, SnPbSeTe, SnPbSTe, or mixtures thereof, but are not limited thereto.Group IV semiconductors may be selected from, for example, elemental (mono) semiconductors such as Si, Ge, or mixtures thereof; and binary semiconductor compounds such as SiC, SiGe, and mixtures thereof, but are not limited thereto. Group I-III-VI semiconductor compounds may be, for example, CuInSe2, CuInS2, CuInGaSe, CuInGaS, or mixtures thereof, but are not limited thereto. Group I-II-IV-VI semiconductor compounds may be, for example, CuZnSnSe, CuZnSnS, or mixtures thereof, but are not limited thereto. Group II-III-V semiconductor compounds may include, for example, InZnP, but are not limited thereto.
[0154] The quantum dot body may include a single semiconductor, a binary semiconductor compound, a ternary semiconductor compound, or a quaternary semiconductor compound in a substantially uniform concentration or with locally varying concentration distributions.
[0155] For example, the quantum dot body may include a cadmium (Cd)-free quantum dot body. A cadmium-free quantum dot body is a quantum dot body that does not include cadmium (Cd). Cadmium (Cd) can cause serious environmental / health issues and is a restricted element in many countries under the Restriction of Hazardous Substances (RoHS) directive, and therefore a non-cadmium-based quantum dot body can be effectively used.
[0156] As an example, the quantum dot body may be a semiconductor compound including zinc (Zn) and at least one of tellurium (Te) and selenium (Se). For example, the quantum dot body may be a Zn-Te semiconductor compound, a Zn-Se semiconductor compound, and / or a Zn-Te-Se semiconductor compound. For example, the amount of tellurium (Te) in the Zn-Te-Se semiconductor compound may be less than the amount of selenium (Se). The semiconductor compound may have a peak emission wavelength (λ max ) in a wavelength region less than or equal to approximately 480 nm, for example, from approximately 430 nm to approximately 480 nm, and may be configured to emit light of a second color.
[0157] For example, the quantum dot body may be a semiconductor compound including indium (In), and at least one of zinc (Zn) and phosphorus (P). For example, the quantum dot body may be an In-P semiconductor compound and / or an In-Zn-P semiconductor compound. For example, in an In-Zn-P semiconductor.
[0158] In the compound, a molar ratio of zinc (Zn) to indium (In) may be greater than or equal to about 25. The semiconductor compound may have a peak emission wavelength (λ max ) in a wavelength region less than about 700 nm, for example, about 600 nm to about 650 nm, and may be configured to emit light of a third color.
[0159] The quantum dot body may have a core-shell structure, wherein one quantum dot body surrounds another quantum dot body. For example, the core and shell of the quantum dot body may have an interface, and an element of at least one of the core or shell at the interface may have a concentration gradient, wherein the concentration of the shell element decreases toward the core. For example, the material composition of the shell of the quantum dot body has a higher energy band gap than the material composition of the core of the quantum dot body, and thus the quantum dot body may exhibit a quantum confinement effect.
[0160] The quantum dot body may have a quantum dot core and a multilayer quantum dot shell surrounding the core. Here, the multilayer shell has at least two shells, wherein each shell may be a single composition, an alloy, and / or have a concentration gradient.
[0161] For example, a shell of a multi-layer shell farther from the core may have a higher energy band gap than a shell closer to the core, and thus the quantum dot body may exhibit a quantum confinement effect.
[0162] For example, a quantum dot body having a core-shell structure may, for example, include: a core, the core including a first semiconductor compound, the first semiconductor compound including zinc (Zn), and at least one of tellurium (Te) and selenium (Se); and a shell including a second semiconductor compound disposed on at least a portion of the core and having a composition different from the composition of the core.
[0163] For example, the first semiconductor compound may be a Zn-Te-Se based semiconductor compound including zinc (Zn), tellurium (Te) and selenium (Se), for example, a Zn-Se based semiconductor compound including a small amount of tellurium (Te), for example, a semiconductor compound represented by ZnTexSe1-x, where x is greater than approximately 0 and less than or equal to 0.05.
[0164] For example, in a first semiconductor compound based on Zn-Te-Se, the molar amount of zinc (Zn) may be higher than the molar amount of selenium (Se), and the molar amount of selenium (Se) may be higher than the molar amount of tellurium (Te). For example, in the first semiconductor compound, the molar ratio of tellurium (Te) to selenium (Se) may be less than or equal to about 0.05, less than or equal to about 0.049, less than or equal to about 0.048, less than or equal to about 0.047, less than or equal to about 0.045, less than or equal to about 0.044, less than or equal to about 0.043, less than or equal to about 0.042, less than or equal to about 0.041, less than or equal to about 0.04, less than or equal to about 0.039, less than or equal to about 0.035, less than or equal to about 0.03, less than or equal to about 0.02 9. less than or equal to about 0.025, less than or equal to about 0.024, less than or equal to about 0.023, less than or equal to about 0.022, less than or equal to about 0.021, less than or equal to about 0.02, less than or equal to about 0.019, less than or equal to about 0.018, less than or equal to about 0.017, less than or equal to about 0.016, less than or equal to about 0.015, less than or equal to about 0.014, less than or equal to about 0.013, less than or equal to about 0.012, less than or equal to about 0.011, or less than or equal to about 0.01. For example, in the first semiconductor compound, the molar ratio of tellurium (Te) to zinc (Zn) may be less than or equal to about 0.02, less than or equal to about 0.019, less than or equal to about 0.018, less than or equal to about 0.017, less than or equal to about 0.016, less than or equal to about 0.015, less than or equal to about 0.014, less than or equal to about 0.013, less than or equal to about 0.012, less than or equal to about 0.011, or less than or equal to about 0.010.
[0165] The second semiconductor compound may include, for example, a II-VI semiconductor compound, a III-V semiconductor compound, a IV-VI semiconductor compound, a Group IV semiconductor, a I-III-VI semiconductor compound, a I-II-IV-VI semiconductor compound, a II-III-V semiconductor compound, or a combination thereof. Examples of the II-VI semiconductor compound, the III-V semiconductor compound, the IV-VI semiconductor compound, the IV semiconductor, the I-III-VI semiconductor compound, the I-II-IV-VI semiconductor compound, and the II-III-V semiconductor compound are the same as described above.
[0166] For example, the second semiconductor compound may include zinc (Zn), selenium (Se), and / or sulfur (S). For example, the shell may include ZnSeS, ZnSe, ZnS, or a combination thereof. For example, the shell may include at least one inner shell disposed proximate the core and an outermost shell disposed at the outermost side of the quantum dot body. The inner shell may include ZnSeS, ZnSe, or a combination thereof, and the outermost shell may include ZnS. For example, the shell may have a concentration gradient of one component, and, for example, the amount of sulfur (S) may increase as one moves away from the core.
[0167] For example, a quantum dot body having a core-shell structure may include: a core, the core including a third semiconductor compound, the third semiconductor compound including indium (In), and at least one of zinc (Zn) and phosphorus (P); and a shell disposed on at least a portion of the core and including a fourth semiconductor compound having a composition different from that of the core.
[0168] In the third semiconductor compound based on In-Zn-P, a molar ratio of zinc (Zn) to indium (In) may be greater than or equal to about 25. For example, in the third semiconductor compound based on In-Zn-P, the molar ratio of zinc (Zn) to indium (In) may be greater than or equal to about 28, greater than or equal to about 29, or greater than or equal to about 30. For example, in the third semiconductor compound based on In-Zn-P, the molar ratio of zinc (Zn) to indium (In) may be less than or equal to about 55, for example, less than or equal to about 50, less than or equal to about 45, less than or equal to about 40, less than or equal to about 35, less than or equal to about 34, less than or equal to about 33, or less than or equal to about 32.
[0169] The fourth semiconductor compound may include, for example, a II-VI semiconductor compound, a III-V semiconductor compound, a IV-VI semiconductor compound, a Group IV semiconductor, a I-III-VI semiconductor compound, a I-II-IV-VI semiconductor compound, a II-III-V semiconductor compound, or a combination thereof. Examples of the II-VI semiconductor compound, the III-V semiconductor compound, the IV-VI semiconductor compound, the IV semiconductor, the I-III-VI semiconductor compound, the I-II-IV-VI semiconductor compound, and the II-III-V semiconductor compound are the same as described above.
[0170] For example, the fourth semiconductor compound may include zinc (Zn) and sulfur (S), and optionally selenium (Se). For example, the shell may include ZnSeS, ZnSe, ZnS, or a combination thereof. For example, the shell may include at least one inner shell disposed proximate the core and an outermost shell disposed at the outermost side of the quantum dot body. At least one of the inner shell and the outermost shell may include the fourth semiconductor compound ZnS, ZnSe, or ZnSeS.
[0171] In some embodiments, the quantum dot material is a quantum dot material without photosensitive crosslinking properties. The quantum dot ligand can be oleic acid, stearic acid, oleylamine, long-chain alkylamine, long-chain alkylphosphine, long-chain alkylphosphonic acid, etc., but is not limited thereto.
[0172] In other embodiments, the quantum dot material is a quantum dot material having photosensitive cross-linking properties, wherein the quantum dot ligand can be an organic ligand having a photosensitive group.
[0173] For example, in one embodiment, the structure of the quantum dot ligand includes a first photosensitive group, and the first photosensitive group is located at the end of the quantum dot ligand molecular structure.
[0174] In this type of embodiment, the quantum dot material further includes a second photosensitive crosslinker, which can induce a crosslinking reaction in the first photosensitive group. When the first photosensitive group is selected from a structure containing a carbon-carbon double bond, the photosensitive crosslinker is selected from a photosensitive free radical initiator, which is selected from benzoin and its derivatives, acetophenone derivatives or aromatic ketone derivatives. The first photosensitive group can be a saturated 3-5 membered heterocyclic structure containing a carbon-carbon double bond or containing O or S. Under light conditions, the second photosensitive crosslinker generates free radicals, which can promote the crosslinking of the carbon-carbon double bond in the photosensitive group. When the first photosensitive group is selected from a structure containing a saturated 3-5 membered heterocyclic group containing O or S, the second photosensitive crosslinker is selected from a photoacid generator, which is selected from sulfonium salts, triazines, sulfonates or diazonium salts. The photoacid generator generates hydrogen ions to catalyze the ring opening of the saturated 3-5 membered ring containing O or S to cause a crosslinking reaction.
[0175] Furthermore, the quantum dot body includes a first quantum dot body and a second quantum dot body, and the quantum dot ligand can be connected to the first quantum dot body and / or the second quantum dot body via a coordination bond. When the quantum dot ligand includes a first photosensitive group, under light conditions, the first quantum dot body and the second quantum dot body are cross-linked through the first photosensitive group in the quantum dot ligand to form a network structure.
[0176] In other embodiments, the material of the quantum dot material layer includes a first quantum dot body, a second quantum dot body, a quantum dot ligand, and a photosensitive initiator, and the quantum dot ligand can be of multiple types. For example, the quantum dot ligand includes a first quantum dot ligand and a second quantum dot ligand, and the first quantum dot ligand and the second quantum dot ligand have different structures, wherein the first quantum dot ligand includes a crosslinkable group, and the crosslinkable group is located at the end of the first quantum dot ligand molecular structure, and the second quantum dot ligand includes a second photosensitive group, and the second photosensitive group has a structure of -AB, where A is an imino group and B is a protecting group; under light conditions, the second photosensitive group can remove the protecting group under the action of the photosensitive initiator to form an amino group; the crosslinkable group can form a crosslink with the amino group formed by the removal of the protecting group of the second photosensitive group or form a salt insoluble in the developer; or the crosslinkable group can form a crosslink with the amino group formed by the removal of the protecting group of the second photosensitive group after activation by an activator or form a salt insoluble in the developer. The crosslinkable group is selected from an epoxy group, a carboxylic acid group, or a sulfonic acid group.
[0177] The protecting group is selected from the group consisting of:
[0178] Represents a chemical bond.
[0179] In some other embodiments, the materials in the quantum dot material layer include quantum dot bodies and quantum dot ligands, and the quantum dot ligands are connected to the quantum dot bodies through coordination groups; the quantum dot ligands contain the structure -YZ, Z is a solubilizing group, and the solubilizing group is selected from polar groups; Y includes interconnected connecting groups and a third photosensitive group, and the connecting group is connected between the coordination group and the third photosensitive group; the connecting group is selected from alkylene; the third photosensitive group can break bonds under light conditions to decompose the interconnected quantum dot bodies and quantum dot ligands into a first material containing a quantum dot body, a coordination group and a connecting group, and a second material containing a solubilizing group; the second material can be dissolved in a developer, and the first material is insoluble in a developer.
[0180] After the third photosensitive group breaks the bond under light conditions, an amino group, a hydroxyl group or a carboxyl group is formed at its end.
[0181] In this embodiment, the third photosensitive group is selected from the group consisting of structure.
[0182] The solubilizing groups are selected from quaternary ammonium salt groups.
[0183] In some further embodiments of the present disclosure, the materials in the quantum dot material layer include a first quantum dot body, a second quantum dot body, a quantum dot ligand and a third photosensitive crosslinker; the quantum dot ligand is connected to the first quantum dot body and / or the second quantum dot body through a coordination bond, and the quantum dot ligand contains an alkane chain; the third photosensitive crosslinker contains at least two fourth photosensitive groups, and the fourth photosensitive group is located at the end of the molecular structure of the third photosensitive crosslinker; the fourth photosensitive group can undergo a carbon-hydrogen insertion reaction with the alkane chain in the quantum dot ligand under light conditions, so that different quantum dot bodies are interconnected to form a network structure.
[0184] The fourth photosensitive group is selected from a structure comprising a benzophenone group, an azide group, a diazo group or a diazirine group.
[0185] In some embodiments of the present disclosure, step S100 includes:
[0186] Step S110, dissolving the quantum dot body and the quantum dot ligand in a quantum dot solvent, or dissolving the quantum dot body, the quantum dot ligand and the photosensitive cross-linking agent in a quantum dot solvent to form a quantum dot material mixed solution;
[0187] In step S120 , a quantum dot material mixture is deposited on one side of the substrate 100 to form a quantum dot material layer 200 .
[0188] In the present disclosure, the quantum dot solvent can be selected based on the type of quantum dot. For example, hexane / cyclohexane, heptane, octane, toluene, xylene, etc. can be used to dissolve oil-soluble quantum dots; propylene glycol methyl ether acetate, ethanol, isopropanol, etc. can be used to dissolve amphiphilic (both hydrophilic and lipophilic) or alcohol-soluble quantum dots; and deionized water can be used to dissolve water-soluble quantum dots.
[0189] As shown in FIG. 4 , in step S200 , an organic material layer 300 is formed on a side of the quantum dot material layer 200 away from the substrate 100 .
[0190] The organic material layer 300 can be used to block water and oxygen. When the surface of the quantum dot material layer 200 is covered with the organic material layer 300, the quantum dot material can be prevented from being exposed to the atmosphere, thereby slowing down the reduction of its PLQY.
[0191] Furthermore, the organic material layer 300 has the following characteristics:
[0192] (1) It can effectively protect the quantum dot material layer 200 and slow down the decrease of its PLQY;
[0193] (2) The organic material layer 300 can be removed in a very gentle manner in subsequent processes, or a small amount of residue can be left after removal, so as to minimize the impact on the luminescence performance of the quantum dot film layer;
[0194] (3) It has good light transmittance. Its transmittance in the ultraviolet band and visible light band should be greater than or equal to 80%, and it does not emit light in the visible light band. On the one hand, it is convenient for subsequent exposure, and the exposure measurement does not need to be greatly changed; on the other hand, the organic material layer 300 does not affect the subsequent light output and luminescence spectrum of the quantum dot light-emitting device.
[0195] In some embodiments of the present disclosure, the material in the organic material layer 300 includes a hydrocarbon mixture having 18-30 carbon atoms.
[0196] In some embodiments of the present disclosure, the hydrocarbon mixture includes linear alkanes and branched alkanes, and may also include one or more of cycloalkanes, alkenes, and alkynes, wherein the cycloalkanes may be monocyclic cycloalkanes with side chains.
[0197] In some embodiments, the hydrocarbon mixture comprises, by weight, 80%-100% linear alkanes and 0%-20% other hydrocarbons, wherein the other hydrocarbons include any one or a combination of branched alkanes, cycloalkanes, alkenes, and alkynes. Specifically, in the hydrocarbon mixture, the linear alkanes may comprise 80%, 81%, 82%, 83%, 84%, 85%, 86%, 87%, 88%, 89%, 90%, 91%, 92%, 93%, 94%, 95%, 96%, 97%, 98%, 99%, or 100%. The other hydrocarbons may comprise 20%, 19%, 18%, 17%, 16%, 15%, 14%, 13%, 12%, 11%, 10%, 9%, 8%, 7%, 6%, 5%, 4%, 3%, 2%, 1%, or 0%.
[0198] For example, in some embodiments, the hydrocarbon mixture includes 80%-95% linear alkanes and 5%-20% other hydrocarbons by weight.
[0199] Furthermore, in some embodiments, among the multiple quantum dot ligands included in the quantum dot material layer, at least one quantum dot ligand has an alkane chain in its molecular structure. This allows the chemical composition of the surface of the quantum dot body to be similar to the main components of the organic material layer, helping to increase the wettability of the organic material layer and providing a basis for improving the uniformity of the organic material layer on the surface of the quantum dot material layer. The length and number of alkane chains contained in the quantum dot body can be adjusted based on the proportion or content of the hydrocarbon mixture contained in the organic material layer, and this is not specifically limited in this disclosure.
[0200] In some embodiments of the present disclosure, the initial melting temperature of the material in the organic material layer is no more than 60° C. to prevent the luminescence performance of the quantum dot material layer 200 from being affected by an excessively high melting temperature.
[0201] In some embodiments of the present disclosure, the hydrocarbon mixture may be paraffin wax, that is, the material in the organic material layer 300 includes paraffin wax. The melting temperature of paraffin wax itself is lower than 60°C. Specifically, different types of paraffin wax are classified into different grades according to their melting points, generally with an interval of 2°C, such as grades 52, 54, 56, and 58.
[0202] Preferably, the paraffin wax is sliced paraffin wax at 52-54°C. The reason for using paraffin wax in this melting temperature range is that it has a higher solubility in solvents such as toluene at room temperature. At room temperature, the solution will not precipitate at high concentrations of 100-200 g / mL, remaining stable and easy to store. In contrast, paraffin wax at 60-62°C, at a concentration of 100 g / mL, will become turbid when cooled to room temperature, making it difficult to perform experiments and store.
[0203] To further demonstrate the protective effect of the disclosed organic material layer 300 (including paraffin wax) on the quantum dot material layer 200, the present disclosure applied an organic material layer to the surface of the quantum dot film. As shown in Figure 30, after application of the organic material layer, the quantum dot film exhibited a stable PLQY in the atmosphere. Within a 30-minute measurement window, its PLQY remained above 96% of the PLQY at time 0, effectively protecting the quantum dot film from atmospheric stress. In the figure, "W film" represents the organic material layer.
[0204] In addition, the present disclosure also tested the spectral data of the organic material layer 300. As shown in Figure 31, the experimental results show that the organic material layer 300 itself does not emit light, while the peak position and peak shape of the PL spectrum of the quantum dot film coated with the organic material layer 300 and the original quantum dot film do not change. This shows that the organic material layer 300 itself does not affect the central wavelength position of the quantum dot film's luminescence spectrum, nor does it affect the color purity of subsequent devices.
[0205] Furthermore, the present disclosure tested the transmittance of the organic material layer 300. Figure 32 shows the UV-VIS transmittance data of the organic material layer 300 spin-coated at different rotational speeds. The experimental results show the full-spectrum transmittance of the organic material layer films of different thicknesses (2000 rpm, 3000 rpm, 4000 rpm, and 5000 rpm). It can be seen that the transmittance in the visible light region is above 87%, and the transmittance in the ultraviolet region is above 80%.
[0206] In some embodiments of the present disclosure, the material in the organic material layer 300 further includes a first photosensitive cross-linking agent.
[0207] The first photosensitive crosslinker in the organic material layer 300 includes a fifth photosensitive group in its structural formula. The fifth photosensitive group is located at the end of the first photosensitive crosslinker structural formula. The fifth photosensitive group can be selected from groups including benzophenone structure, azide structure or diazo structure.
[0208] The first photosensitive crosslinker may include multiple fifth photosensitive groups, e.g., at least two. Specifically, the number may be two, three, four, or more. For example, in one embodiment, the photosensitive crosslinker has m terminals, n of which are fifth photosensitive groups, where n ≤ m and m ≥ 2. When the first photosensitive crosslinker includes multiple fifth photosensitive groups, each fifth photosensitive group may be the same or different.
[0209] Specifically, the fifth photosensitive group in the first photosensitive crosslinking agent in the organic material layer 300 can be selected from the group consisting of the following structures:
[0210] in, It is a chemical bond that can be used to connect with other remaining structures in the structural formula of the first photosensitive crosslinking agent.
[0211] X1, X2, X3, and X4 are each independently selected from a halogen atom; specifically, the halogen atom includes fluorine, chlorine, bromine, iodine, etc. Preferably, X1, X2, X3, and X4 are each independently selected from fluorine;
[0212] R1 and R2 represent the remaining molecular chains in the photosensitive group, and are not particularly limited.
[0213] It should be noted that the photosensitive crosslinker contained in the organic material layer 300 may be the same as or different from the photosensitive crosslinker contained in the quantum dot material layer 200. Preferably, the photosensitive crosslinker in the organic material layer 300 and the photosensitive crosslinker in the quantum dot material layer 200 are different and can be dissolved in different solvents.
[0214] In some embodiments of the present disclosure, step S200 includes:
[0215] (1) dissolving the hydrocarbon mixture in a protective material solvent, or dissolving the hydrocarbon mixture and a photosensitive crosslinking agent in a protective material solvent to form a protective material mixed solution;
[0216] (2) A protective material mixture is deposited on the side of the quantum dot material layer 200 away from the substrate 100 to form an organic material layer 300 .
[0217] The protective material solvent can be a non-polar solvent or a weak polar solvent, such as hexane, heptane, octane, gasoline, petroleum ether, ether, carbon disulfide, benzene, toluene, xylene, chloroform, carbon tetrachloride and other solvents.
[0218] In some embodiments of the present disclosure, the quantum dot material solvent in step S100 and the protective material solvent in step S200 may be the same or different. Preferably, the quantum dot solvent and the protective material solvent are different. Furthermore, to avoid affecting the already formed quantum dot material layer 200 when forming the organic material layer 300, the quantum dot solvent and the protective material solvent are selected from different types of solvents. The protective material solvent may be an orthogonal solvent, that is, in the protective material solvent system, the previous quantum dot body and the like have a lower solubility in the solvent, thereby protecting the already formed quantum dot material layer 200.
[0219] For example, the hydrocarbon mixture in the organic material layer 300 can be dissolved in solvents such as hexane, heptane, octane, gasoline, petroleum ether, ether, carbon disulfide, benzene, toluene, xylene, chloroform, and carbon tetrachloride. The quantum dot solvent can be selected from solvents such as propylene glycol methyl ether acetate, ethanol, isopropyl alcohol, or deionized water. Accordingly, the quantum dot body can be an amphiphilic or alcohol-soluble quantum dot body or a water-soluble quantum dot body.
[0220] It should be noted that in step S200 , the initial thickness of the organic material layer 300 may be 20 nm-80 nm, specifically 20 nm, 30 nm, 40 nm, 50 nm, 60 nm, 70 nm or 80 nm, but is not limited thereto.
[0221] In the present disclosure, both step S100 and step S200 are performed in an inert gas (such as nitrogen) or vacuum environment.
[0222] In related technologies, some researchers may form a photoresist layer on the surface of the quantum dot material layer 200 away from the base substrate 100, and then perform processes such as exposure and development.
[0223] It should be noted that the organic material layer disclosed in the present invention is different from the photoresist layer. First, the photoresist layer has strong absorption in the ultraviolet band (300nm-400nm), which is a response to ultraviolet light. Its transmittance in this wavelength range is not high, and in the visible light region, the light transmittance of the photoresist layer is also on the low side, because the photoresist layer generally appears brown or yellow, and has more obvious absorption in the visible light region, so its transmittance will be low. Therefore, at approximately the same thickness, the light transmittance of the photoresist layer is lower than the light transmittance of the organic material layer disclosed in the present invention. Secondly, the film thickness of the photoresist layer is usually between 1um-3um, and the film-forming performance of the photoresist with a thickness of the order of 100 nanometers will gradually deteriorate, and the uniformity of the film layer will be reduced. The material used in the organic material layer disclosed in the present invention has a thin film with a thickness of the order of 100 nanometers (such as 50-300nm), which is significantly thinner than the photoresist layer. In addition, the photoresist currently used in commercial and semiconductor process production, after being coated, exposed, and developed to produce a pattern, usually has a small amount of residual photoresist layer on the surface. For these small amounts of residues, different subsequent processes are suitable for different treatment methods, such as stripping or etching / ashing, in order to clean the residual photoresist layer, and the conditions are relatively harsh. These processes have extremely serious effects on the surface of the quantum dot material layer. The stripping solvent used for stripping will cause damage to the quantum dot material layer, and the plasma used in the etching / ashing process will significantly damage the quantum dot material layer itself, and even cause the quantum dots to fail (cannot emit light). Therefore, the photoresist layers commonly used in the relevant technology cannot be used in the organic material layer disclosed in the present invention. The organic material layer disclosed in the present invention can be easily removed by temperature and solvent, etc., without causing damage to the quantum dot material layer.
[0224] As shown in FIG5 , in step S300 , a predetermined area of the substrate 100 is exposed, so that the material in the quantum dot material layer 200 in the predetermined area is cross-linked or generates a salt insoluble in a developer, or / and the material in the organic material layer 300 in the predetermined area is cross-linked.
[0225] In step S300, a predetermined area of the substrate 100 is exposed in an atmospheric atmosphere. Specifically, the substrate prepared in step S200 is removed from the inert gas atmosphere, and then aligned with a photomask. The upper area is exposed to ultraviolet light using a photolithography machine, while other areas (non-predetermined areas) are not exposed to ultraviolet light.
[0226] In this step, when the quantum dot material layer 200 is a material without photosensitive crosslinking properties, the material in the organic material layer 300 should contain a photosensitive crosslinker to cause crosslinking of the organic material layer 300 when the predetermined area is exposed. When the quantum dot material layer 200 is a material with photosensitive crosslinking properties, the material in the organic material layer 300 may or may not contain a first photosensitive crosslinker.
[0227] Specifically, when the quantum dot material layer 200 is a material having photosensitive cross-linking properties, in step S300 , when the predetermined area is exposed, the material in the quantum dot material layer 200 located in the predetermined area is cross-linked or generates a salt insoluble in the developer.
[0228] For example, the first photosensitive group contained in the quantum dot ligand in the quantum dot material layer 200 is a carbon-carbon double bond. When the preset area is exposed, the second photosensitive crosslinker causes the carbon-carbon double bond to be crosslinked to form a network structure; or
[0229] The first photosensitive group contained in the quantum dot ligand in the quantum dot material layer 200 is a saturated 3-5 membered heterocyclic structure containing O or S. When the preset area is exposed, the second photosensitive crosslinker promotes the ring opening of the saturated 3-5 membered heterocyclic structure containing O or S to undergo a crosslinking reaction, thereby forming a network structure; or
[0230] The quantum dot ligands in the quantum dot material layer 200 include a first quantum dot ligand and a second quantum dot ligand, and the first quantum dot ligand and the second quantum dot ligand have different structures, wherein the first quantum dot ligand includes a crosslinkable group, the second quantum dot ligand includes a second photosensitive group, and the structure of the second photosensitive group is -AB, A is an imino group, and B is a protecting group; when exposing a preset area, the second photosensitive group removes the protecting group under the action of a photosensitive initiator to form an amino group; the crosslinkable group and the amino group formed by removing the protecting group of the second photosensitive group are crosslinked or form a salt insoluble in the developer; or the crosslinkable group can be activated by an activator and can be crosslinked with the amino group formed by removing the protecting group of the second photosensitive group or form a salt insoluble in the developer; or
[0231] The quantum dot ligand contains an alkane chain; the third photosensitive crosslinker contains at least two fourth photosensitive groups, and the fourth photosensitive groups are located at the ends of the molecular structure of the third photosensitive crosslinker; the fourth photosensitive groups can undergo a carbon-hydrogen insertion reaction with the alkane chain in the quantum dot ligand under light conditions, so that the quantum dot ligand and the third photosensitive crosslinker react to form a network structure; or
[0232] The quantum dot ligand comprises a structure -YZ, where Z is a solubilizing group, which is selected from a polar group; Y comprises a connecting group and a third photosensitive group connected to each other, and the connecting group is connected between the coordination group and the third photosensitive group; the connecting group is selected from an alkylene group; the third photosensitive group can break a bond under light conditions to decompose the interconnected quantum dot body and the quantum dot ligand into a first material comprising the interconnected quantum dot body, the coordination group and the connecting group, and a second material comprising the solubilizing group; the second material can be dissolved in a developer, and the first material is insoluble in a developer.
[0233] When the material in the organic material layer 300 includes a first photosensitive crosslinker, the hydrocarbon mixture in the organic material layer 300 undergoes crosslinking when the predetermined area is exposed. Taking the first photosensitive crosslinker included in the organic material layer 300 as an example, when the first photosensitive crosslinker includes different fifth photosensitive groups, the hydrocarbon mixture may undergo different crosslinking reactions. Specifically, the crosslinking reaction of the carbon-hydrogen (CH) bonds in the hydrocarbon mixture is as follows:
[0234] In this disclosure, represents a hydrocarbon molecular chain, For chemical bonds.
[0235] The cross-linking reaction of double bonds (olefins) in hydrocarbon mixtures is as follows:
[0236] The cross-linking reaction of triple bonds (alkynes) in hydrocarbon mixtures is as follows:
[0237] In step S300, taking the example of an organic material layer 300 containing paraffin wax, crosslinking of the organic material layer 300 enhances its stability. Specifically, this can manifest as an increase in the melting temperature of the organic material layer 300 and a decrease in its solubility in the solvent. Furthermore, the degree of crosslinking, and thus the melting temperature and solubility, of the organic material layer 300 can be adjusted by controlling the amount of the first photosensitive crosslinker added or the exposure dose during exposure.
[0238] As shown in FIG. 6 or FIG. 22 , in step S400 , the organic material layer 300 and the quantum dot material layer 200 in non-preset areas of the substrate 100 are removed.
[0239] In the present disclosure, the organic material layer 300 and the quantum dot material layer 200 in non-predetermined areas of the substrate 100 may be removed by various methods.
[0240] The following will describe step S400 in detail with reference to different embodiments.
[0241] Example 1
[0242] As shown in FIG6 , in this embodiment, step S400 includes:
[0243] In step S410 , development is performed to remove the organic material layer 300 and the quantum dot material layer 200 in non-preset areas.
[0244] During exposure, the organic material layer 300 located in the predetermined area is cross-linked.
[0245] In this embodiment, the material in the organic material layer 300 includes a photosensitive crosslinker, and the material in the quantum dot material layer 200 can be either photosensitive or non-photosensitive. During exposure, the organic material layer 300 in the predetermined regions undergoes crosslinking, increasing its melting temperature and decreasing its solubility, making it virtually indestructible during development. However, the organic material layer 300 in non-predetermined regions remains uncrosslinked and can be removed during development.
[0246] For the quantum dot material layer 200, when it is a material with photosensitive cross-linking properties, the quantum dot material layer 200 located in the predetermined area undergoes cross-linking and is substantially not removed during development, while the quantum dot material layer 200 located in the non-preset area does not undergo cross-linking and can be removed during development. When the quantum dot material layer 200 is a material without photosensitive cross-linking properties, the quantum dot material layer 200 located in the predetermined area is substantially not removed during development due to the protection of the organic material layer 300 in that area, while the quantum dot material layer 200 located in the non-preset area is removed during development.
[0247] Specifically, step S410 includes:
[0248] Step S410 , performing a first development with a first developer to remove the organic material layer 300 in non-preset areas;
[0249] In step S420 , a second developing solution is used to perform a second development to remove the quantum dot material layer 200 in areas other than the preset areas.
[0250] The first developer and the second developer are different. Specifically, the relative dielectric constant of the second developer is greater than the relative dielectric constant of the first developer.
[0251] In this embodiment, to reduce process complexity, two development steps are used to remove the organic material layer 300 and quantum dot material layer 200 from non-predetermined areas. The organic material layer 300 contains a hydrocarbon mixture, and the first developer can be a non-polar or weakly polar solvent with a relative dielectric constant of no greater than 3.6.
[0252] Relative dielectric constant ε rIt can be measured using an electrostatic field as follows: First, measure the capacitance C0 of the capacitor with a vacuum between the two plates. Then, use the same distance between the plates but insert a dielectric between them to measure the capacitance Cx. The relative dielectric constant can then be calculated using the following formula:
[0253] ε r =Cx / C0.
[0254] The relative permittivity ε of dry air without carbon dioxide at standard atmospheric pressure is r =1.00053. Therefore, the capacitance Cair of this electrode configuration in air is used instead of C0 to measure the relative permittivity ε r When using the standard, it also has sufficient accuracy (refer to GB / T 1409-2006).
[0255] Specifically, a substance with a relative dielectric constant in the range of 2.8 to 3.6 is a weakly polar solvent; a substance with a relative dielectric constant less than 2.8 is a non-polar solvent. The first developer can be selected from solvents such as hexane, heptane, octane, gasoline, petroleum ether, ether, carbon disulfide, benzene, toluene, xylene, chloroform, and carbon tetrachloride.
[0256] Furthermore, in this embodiment, the temperature of the first developer is less than 60°C. For example, if the organic material layer 300 contains paraffin wax, the melting temperature of paraffin wax itself is less than 60°C. Specifically, different types of paraffin wax are classified into different grades, such as 52, 54, 56, and 58, based on their melting points, generally at 2°C increments. After the organic material layer 300 is cross-linked, its melting temperature will increase to varying degrees. To avoid affecting the cross-linked areas of the organic material layer 300 during development, in this embodiment, the temperature of the first developer is preferably less than 60°C.
[0257] The relative dielectric constant of the second developer is greater than that of the first developer. The second developer can be selected from solvents such as propylene glycol methyl ether acetate, ethanol, isopropyl alcohol, and deionized water. It should be noted that the choice of the second developer also depends on the properties of the quantum dot substrate or quantum dot ligand, and those skilled in the art will select the second developer based on their specific circumstances.
[0258] After step S400 , a patterned quantum dot film layer can be obtained.
[0259] Example 2
[0260] As shown in FIG6 , in this embodiment, step S400 includes:
[0261] Step S410 , heating the non-preset area, rotating the substrate 100 , melting the organic material layer 300 located in the non-preset area, and rotating the melted organic material layer 300 out under the action of centrifugal force;
[0262] In step S420 , development is performed to remove the quantum dot material layer 200 located in non-preset areas.
[0263] During exposure, the quantum dot material layer 200 located in the predetermined area is cross-linked or generates salt that is insoluble in the developer.
[0264] In step S410, in this embodiment, no crosslinking reaction occurs in the organic material layer 300 during exposure, meaning that the organic material layer 300 does not contain a photosensitive crosslinker. In this case, conventional development steps cannot be used to remove the organic material layer 300. Therefore, the present disclosure utilizes a method of heating non-predetermined areas to melt the organic material layer 300 in these areas into a low-viscosity liquid. High-speed rotation is then used to remove the liquid organic material layer 300 using centrifugal force.
[0265] Specifically, the temperature of the non-preset heating area is 70°C-110°C, such as 70°C, 75°C, 80°C, 85°C, 90°C, 95°C, 100°C, 105°C, or 110°C. At this temperature, the organic material layer 300 can melt into a low-viscosity liquid. For example, if the organic material layer 300 includes paraffin wax, the paraffin wax melts at this temperature into a low-viscosity liquid, which can be removed under the action of centrifugal force.
[0266] Furthermore, the organic material layer 300 can be liquefied into a low-viscosity liquid by electrically heating the electrodes in the non-preset areas or using a laser to heat the non-preset areas to above 70°C or 80°C (usually not more than 110°C).
[0267] In this embodiment, the quantum dot material layer 200 is a material with photosensitive cross-linking properties. When exposed, the quantum dot material layer 200 located in the preset area undergoes cross-linking or generates salts that are insoluble in the developer and cannot be removed by the development step. The quantum dot material layer 200 located in the non-preset area does not undergo cross-linking and can be removed by the development step.
[0268] In step S420, development is performed to remove the quantum dot material layer 200 located in non-preset areas. In this step, the developer can refer to the second developer in Example 1 and will not be described in detail here.
[0269] Example 3
[0270] As shown in FIG. 22 , in this embodiment, step S400 includes:
[0271] Step S410 , using a first solvent to remove at least a portion of the organic material layer 300 located in a predetermined area and at least a portion of the organic material layer 300 located in a non-preset area, wherein the temperature of the first solvent is 60° C.-90° C.;
[0272] Step S420 , developing with a second developer to remove the quantum dot material layer 200 located in non-preset areas;
[0273] During exposure, the quantum dot material layer 200 located in the predetermined area is cross-linked or generates salt that is insoluble in the developer.
[0274] In this embodiment, the organic material layer 300 does not contain a photosensitive crosslinking agent, and the quantum dot material layer 200 is a material having photosensitive crosslinking properties. That is, when exposed to light, the organic material layer 300 does not undergo crosslinking.
[0275] In step S410 , the organic material layer 300 does not contain a photosensitive crosslinking agent, and therefore cannot be removed using a conventional developing method. Therefore, in this embodiment, a hot solvent method is used to remove the organic material layer 300 .
[0276] The first solvent can be a non-polar or weakly polar solvent at 60-90° C., such as toluene, petroleum ether, or octane at 60-90° C. Specifically, the exposed substrate is sprayed with the first solvent, so that the thickness of the organic material layer 300 in the predetermined area and the non-predetermined area is significantly reduced or partial voids are formed.
[0277] In step S420, a second developer is used to remove the quantum dot material layer 200 from the non-predetermined areas. In this step, since the organic material layer 300 is significantly thinned or partially voided after step S410, with the thickness after thinning not exceeding 3 nm, the second developer can penetrate the quantum dot material layer 200 and remove the quantum dot material layer 200 from the non-predetermined areas. It should be noted that the thickness of the organic material layer 300 may vary from region to region, with the maximum thickness not exceeding 3 nm.
[0278] In this step, the second developer can refer to Example 1 and will not be described in detail here.
[0279] In the present disclosure, steps S200 to S400 may be repeated to form a plurality of quantum dot film layers and organic material layers.
[0280] For Example 1 and Example 2, as shown in Figures 7 to 14, steps S200 to S400 are repeated to form quantum dot film layers 201 and 202, and organic material layers 301 and 302. Quantum dot material layers 200, 201, and 202 can each be composed of quantum dot materials of different colors. Quantum dot material layer 200 can emit light of a first color, quantum dot material layer 201 can emit light of a second color, and quantum dot material layer 202 can emit light of a third color. The first color can be red, the second color can be green, and the third color can be blue, but are not limited thereto.
[0281] Specifically, after the patterning of the quantum dot material layer 200 and the organic material layer 300 is completed, as shown in FIG7 , the quantum dot material layer 201 is formed on the side of the organic material layer 300 away from the base substrate 101, and as shown in FIG8 , the organic material layer 301 is formed on the side of the quantum dot material layer 201 away from the base substrate 101. Subsequently, as shown in FIG9 and FIG11 , the preset area is exposed, and the organic material layer 301 and the quantum dot material layer 201 in the non-preset area are removed. Next, as shown in FIG11 , the quantum dot material layer 202 is formed on the side of the organic material layer 301 away from the base substrate 101. As shown in FIG12 , the organic material layer 302 is formed on the side of the quantum dot material layer 202 away from the base substrate 101. Subsequently, as shown in FIG13 and FIG14 , the preset area is exposed, and the organic material layer 301 and the quantum dot material layer 201 in the non-preset area are removed.
[0282] For Example 3, steps S200 to S400 are repeated, as shown in Figures 23 to 29 and Figure 16. As shown in Figure 23, a quantum dot material layer 201 is formed on the side of the organic material layer 300 away from the base substrate 101. As shown in Figure 24, an organic material layer 301 is formed on the side of the quantum dot material layer 201 away from the base substrate 101. Subsequently, as shown in Figures 25 and 26, a predetermined area is exposed, and the organic material layer 301 and the quantum dot material layer 201 in the non-predetermined area are removed. Next, as shown in Figure 27, a quantum dot material layer 202 is formed on the side of the organic material layer 301 away from the base substrate 101. As shown in Figure 28, an organic material layer 302 is formed on the side of the quantum dot material layer 202 away from the base substrate 101. Subsequently, as shown in Figures 29 and 16, a predetermined area is exposed, and the organic material layer 301 and the quantum dot material layer 201 in the non-predetermined area are removed.
[0283] In the present disclosure, other steps may be included after step S400. The processing process after step S400 will be described in detail below in combination with different embodiments.
[0284] Example 4
[0285] As shown in FIG. 14 to FIG. 17 , in some embodiments of the present disclosure, for Embodiment 1 and Embodiment 2, after step S400, the following steps are further included:
[0286] In step S500 , the substrate 100 is placed horizontally, subjected to thermal annealing treatment at a temperature of 60° C. to 100° C. for 5 min to 30 min, and then cooled to below 35° C.
[0287] In this embodiment, the remaining organic material layer 300 naturally leveled during the thermal annealing process, resulting in a flatter film. Simultaneously, the remaining solvent molecules in the quantum dot film and organic material layer 300 were evaporated, resulting in a device image as shown in Figure 14. In this embodiment, the final thickness of the organic material layer 300 was approximately 8nm-15nm.
[0288] Example 5
[0289] In some embodiments of the present disclosure, for embodiment 1 and embodiment 2, step S400 further includes:
[0290] Step S500 , removing at least a portion of the organic material layer 300 located in a predetermined area using a second solvent, wherein the temperature of the second solvent is 60° C.-90° C.;
[0291] Step S600 , heating and drying the substrate 100 .
[0292] In step S500, a second solvent is used to soak the substrate or spray the substrate surface to rinse the remaining organic material layer 300, thereby removing a portion of the organic material layer 300 with a certain crosslinking ratio in a predetermined area. The second solvent can be a non-polar solvent or a weakly polar solvent with a temperature of 60°C-90°C, such as toluene, petroleum ether, or octane at 60°C-90°C.
[0293] In step S600, the substrate 100 is post-baked on a hot plate at 70°C to 100°C to remove any residual solvent. The resulting organic material layer 300 is thinner (as shown in FIG. 14 ), with a thickness of 3 nm to 8 nm, or a discontinuous organic material layer 300 (as shown in FIG. 15 ), with a thickness of no more than 3 nm. Specifically, the organic material layer 300 is a discontinuous thin film with a thickness of no more than 3 nm.
[0294] In this embodiment, a relatively large amount of the organic material layer 300 is removed by soaking and spraying with a hot solvent, so as to reduce the influence of the organic material layer 300 itself on the electrical performance of the device.
[0295] Example 6
[0296] In some embodiments of the present disclosure, for embodiment 1, embodiment 2, and embodiment 3, step S400 further includes:
[0297] Step S500 , heating the substrate and rotating it, and washing the rotating substrate with a third solvent to remove at least a portion of the remaining organic material layer;
[0298] Step S600: heating and drying the substrate.
[0299] In step S500, the substrate is heated to 70°C-110°C, and then rotated at high speed (such as 1000rpm to 4000rpm) on a spin coater (or called a glue spreader) at the same ambient temperature. At the same time, the surface of the high-speed rotating substrate is rinsed with a third solvent (a non-polar solvent or a weakly polar solvent, such as toluene, petroleum ether, or octane at 70°C-110°C) at the same temperature or a higher temperature to basically remove the organic material layer 300.
[0300] In step S600 , the substrate is dried on a hot plate at 70° C.-100° C. to remove the residual solvent. The result is shown in FIG. 17 . The thickness of the organic material layer 300 is not more than 1 nm.
[0301] The present disclosure also provides a quantum dot light-emitting layer, which is manufactured using the quantum dot film patterning method described in any of the above embodiments. In one embodiment, the quantum dot light-emitting layer may include patterned quantum dot material layer 200, quantum dot material layer 201, and quantum dot material layer 202.
[0302] The present disclosure also provides a quantum dot light-emitting device, comprising the above-mentioned quantum dot light-emitting layer.
[0303] The quantum dot light-emitting device provided by the present disclosure can be a photoluminescent quantum dot device or an electroluminescent quantum dot device.
[0304] As shown in FIG. 18 to FIG. 20 , in some embodiments of the present disclosure, the quantum dot light-emitting device is an electroluminescent quantum dot device, comprising:
[0305] Base substrate 101;
[0306] The pixel definition layer 120 is disposed on one side of the base substrate 101 and has a plurality of openings;
[0307] The quantum dot light-emitting layer 200' is provided on one side of the base substrate 101 and is located in the opening;
[0308] The organic layer 300' is disposed on the side of the quantum dot light-emitting layer 200' away from the base substrate 101. The transmittance of the organic layer 300' in the ultraviolet and visible light bands is not less than 80%, and the melting temperature of the material in the organic layer 300' does not exceed 110°C.
[0309] In this embodiment, the quantum dot light-emitting layer 200' is made of the quantum dot material layer 200 in any of the above embodiments. In the quantum dot light-emitting device, the quantum dot light-emitting layer 200' has a cross-linked network structure, or / and the organic layer 300' has a cross-linked network structure or a salt that is insoluble in the developer. Furthermore, the melting temperature of the material in the organic layer 300' does not exceed 100°C, or does not exceed 90°C, or does not exceed 80°C, etc. The specific material selection and formation method of the quantum dot light-emitting layer 200' and the organic layer 300' can refer to the above embodiments and will not be described in detail here.
[0310] The quantum dot light emitting device further includes a first electrode 110 , a first carrier transport layer 130 , a second carrier transport layer 400 and a second electrode 500 .
[0311] The first electrode 110 can serve as an anode and is disposed between the base substrate 101 and the quantum dot light-emitting layer 200'. The first carrier transport layer 130 is disposed between the first electrode 110 and the quantum dot light-emitting layer 200'. The second carrier transport layer 400 is disposed on the side of the quantum dot light-emitting layer 200' away from the base substrate 101. The second electrode 500 is disposed on the side of the organic layer 300' away from the base substrate 101 and can serve as a cathode.
[0312] The anode may include a conductor having a high work function, such as a metal, a conductive metal oxide, or a combination thereof. The anode may include, for example, a metal such as nickel, platinum, vanadium, chromium, copper, zinc, or gold, or an alloy thereof; a conductive metal oxide such as zinc oxide, indium oxide, tin oxide, indium tin oxide (ITO), indium zinc oxide (IZO), or fluorine-doped tin oxide; or a combination of a metal and a conductive metal oxide such as ZnO and Al, or SnO2 and Sb, but is not limited thereto.
[0313] The cathode may include a conductor having a lower work function than the anode, such as a metal, a conductive metal oxide, and / or a conductive polymer. The cathode may include, for example, a metal such as aluminum, magnesium, calcium, sodium, potassium, titanium, indium, yttrium, lithium, gadolinium, silver, tin, lead, cesium, barium, or an alloy thereof; a multilayer structure such as LiF / Al, Li2O / Al, Liq / Al, LiF / Ca, and BaF2 / Ca, but is not limited thereto.
[0314] The first carrier transport layer 130 may include a hole injection layer and / or a hole transport layer in a direction away from the base substrate 101 .
[0315] The hole transport layer and the hole injection layer may each have a HOMO energy level between the work function of the first electrode 110' and the HOMO energy level of the quantum dot light-emitting layer 200'. For example, the work function of the first electrode 110', the HOMO energy level of the hole injection layer, the HOMO energy level of the hole transport layer, and the HOMO energy level of the quantum dot light-emitting layer 200' may gradually deepen, and may be, for example, stepped.
[0316] The hole transport layer may have a relatively deep HOMO energy level to match the HOMO energy level of the quantum dot light emitting layer 200 ′. Therefore, the mobility of holes transferred from the hole transport layer to the quantum dot layer may be improved.
[0317] The HOMO energy level of the hole transport layer may be equal to the HOMO energy level of the quantum dot light emitting layer 200' or less than the HOMO energy level of the quantum dot light emitting layer 200' in the range of about 1.0 eV or less. For example, the difference between the HOMO energy levels of the hole transport layer and the quantum dot light emitting layer 200' may be about 0 eV to about 1.0 eV, within a range, such as about 0.01 eV to about 0.8 eV, within a range, such as about 0.01 eV to about 0.7 eV, within a range, such as about 0.01 eV to about 0.5 eV, within a range, such as about 0.01 eV to about 0.4 eV, such as about 0.01 eV to about 0.3 eV, such as about 0.01 eV to about 0.2 eV, such as about 0.01 eV to about 0.1 eV.
[0318] The HOMO energy level of the hole transport layer can be, for example, greater than or equal to about 5.0 eV, within a range, for example, greater than or equal to about 5.2 eV, within a range, for example, greater than or equal to about 5.4 eV, within a range, for example, greater than or equal to about 5.6 eV, within a range, for example, greater than or equal to about 5.8 eV.
[0319] For example, the HOMO energy level of the hole transport layer can be from about 5.0 eV to about 7.0 eV, within the above range, for example, from about 5.2 eV to about 6.8 eV, within the above range, for example, from about 5.4 eV to about 6.8 eV, for example, from about 5.4 eV to about 6.7 eV, for example, from about 5.4 eV to about 6.5 eV, for example, from about 5.4 eV to about 6.3 eV, for example, from about 5.4 eV to about 6.2 eV, for example, from about 5.4 eV to about 6.1 eV, for example, from about 5.6 eV to about 7.0 eV, for example, from about 5.6 eV to about 6.8 eV, for example Such as from about 5.6eV to about 6.7eV, for example, from about 5.6eV to about 6.5eV, for example, from about 5.6eV to about 6.3eV, for example, from about 5.6eV to about 6.2eV, for example, from about 5.6eV to about 6.1eV, for example, from about 5.8eV to about 7.0eV, for example, from about 5.8eV to about 6.8eV, for example, from about 5.8eV to about 6.7eV, for example, from about 5.8eV to about 6.5eV, for example, from about 5.8eV to about 6.3eV, for example, from about 5.8eV to about 6.2eV, for example, from about 5.8eV to about 6.1eV.
[0320] The hole transport layer and the hole injection layer may include a material that satisfies the energy level without particular limitation, and may include, for example, at least one selected from the group consisting of poly(9,9-dioctyl-fluorene-co-N-(4-butylphenyl)-diphenylamine) (TFB), poly(N,N'-bis-4-butylphenyl-N,N'-bisphenyl)benzidine (poly TPD), polyarylamine (polyarylamine), poly(N-vinylcarbazole), poly(3,4-ethylenedioxythiophene) (PEDOT), poly(3,4-ethylenedioxythiophene):polystyrene sulfonate (PEDOT:PSS), polyaniline, polypyrrole, N,N,N',N'-tetrakis(4-methoxyphenyl)-benzidine (TPD), 4,4'-bis[N-(1-naphthyl)-N-phenyl-amino]biphenyl (α-NPD), m-MTDATA (4,4',4"-tris[phenyl(m-tolyl)amino]triphenylamine), 4,4',4"-tris(N-carbazolyl)-triphenylamine (TCTA), 1,1-bis[(di-4-tolylamino)phenyl]cyclohexane (TAPC), p-type metal oxides (e.g., NiO, WO3, MoO3, etc.), carbon-based materials such as graphene oxide, phthalocyanine compounds (e.g., copper phthalocyanine);N,N'-diphenyl-N,N'-bis-[4-(phenyl-m-tolyl-amino)-phenyl]-biphenyl-4,4'-diamine (DNTPD), 4,4',4"-tris(3-methylphenylphenylamino)triphenylamine (m-MTDATA), 4,4',4"-tris(N,N-diphenylamino)triphenylamine (TDATA), 4,4',4"-tris{N-(2-naphthyl)-N-phenylamino}-triphenylamine (2-TNATA), Poly(3,4-ethylenedioxythiophene) / poly(4-styrenesulfonate) (PEDOT / PSS), polyaniline / dodecylbenzenesulfonic acid (PANI / DBSA), polyaniline / camphorsulfonic acid (PANI / CSA), polyaniline / poly(4-styrenesulfonate) (PANI / PSS), N,N'-di(naphthalene-1-yl)-N,N'-diphenyl-benzidine (NPB), triphenylamine-containing polyetherketone (TPAPEK), 4-isopropyl -4'-methyldiphenyliodonium tetrakis(pentafluorophenyl)borate and / or dipyrazino[2,3-f:2',3'-h]quinoxaline-2,3,6,7,10,11-hexacarbonitrile (HAT-CN), carbazole derivatives (e.g. N-phenylcarbazole and / or polyvinylcarbazole), fluorine derivatives, N,N'-bis(3-methylphenyl)-N,N'-diphenyl-[1,1-biphenyl]-4,4'-diamine (TPD), triphenylamine derivatives (e.g. 4, 4',4"-tris(N-carbazolyl)triphenylamine (TCTA)), N,N'-di(naphthalene-1-yl)-N,N'-diphenyl-benzidine (NPB), 4,4'-cyclohexylenebis[N,N-bis(4-methylphenyl)aniline] (TAPC), 4,4'-bis[N,N'-(3-methylphenyl)amino]-3,3'-dimethylbiphenyl (HMTPD), 1,3-bis(N-carbazolyl)benzene (mCP), and combinations thereof, but are not limited thereto.
[0321] One or both of the hole transport layer and the hole injection layer may be omitted.
[0322] The second carrier transport layer 400 may include an electron transport layer and an electron injection layer sequentially disposed in a direction away from the base substrate 101 .
[0323] For example, the LUMO energy levels of the second electrode 500, the electron injection layer, the electron transport layer, and the quantum dot light-emitting layer 200' may gradually become shallower. For example, the LUMO energy level of the electron injection layer may be shallower than the work function of the second electrode 500, and the LUMO energy level of the electron transport layer may be shallower than the LUMO energy level of the electron injection layer, and the LUMO energy level of the quantum dot light-emitting layer 200' may be shallower than the LUMO energy level of the electron transport layer. That is, the work function of the second electrode 500, the LUMO energy level of the electron injection layer, the LUMO energy level of the electron transport layer, and the LUMO energy level of the quantum dot light-emitting layer 200' may have a step-wise (cascade) energy level that gradually decreases in one direction.
[0324] The electron transport layer may include first inorganic nanoparticles. The first inorganic nanoparticles may be, for example, oxide nanoparticles, and may be, for example, metal oxide nanoparticles.
[0325] The first inorganic nanoparticles may be two-dimensional or three-dimensional nanoparticles having an average particle diameter of less than or equal to about 10 nm, within a range of less than or equal to about 8 nm, less than or equal to about 7 nm, less than or equal to about 5 nm, less than or equal to about 4 nm, or less than or equal to about 3.5 nm, or within a range of about 1 nm to about 10 nm, about 1 nm to about 9 nm, about 1 nm to about 8 nm, about 1 nm to about 7 nm, about 1 nm to about 5 nm, about 1 nm to about 4 nm, or about 1 nm to about 3.5 nm.
[0326] For example, the first inorganic nanoparticles may be metal oxide nanoparticles, and the metal oxide nanoparticles include at least one of the following: zinc (Zn), magnesium (Mg), cobalt (Co), nickel (Ni), gallium (Ga), aluminum (Al), calcium (Ca), zirconium (Zr), tungsten (W), lithium (Li), titanium (Ti), tantalum (Ta), tin (Sn), hafnium (Hf), and barium (Ba).
[0327] As an example, the first inorganic nanoparticles may include metal oxide nanoparticles including zinc (Zn), and may include nanoparticles composed of Zn. 1-x Q x Metal oxide nanoparticles represented by Q (0≤x<0.5). Here, Q is at least one metal other than Zn, such as magnesium (Mg), cobalt (Co), nickel (Ni), gallium (Ga), aluminum (Al), calcium (Ca), zirconium (Zr), tungsten (W), lithium (Li), titanium (Ti), tantalum (Ta), tin (Sn), hafnium (Hf), silicon (Si), barium (Ba), or a combination thereof.
[0328] For example, Q may include magnesium (Mg).
[0329] For example, x may be in the range of 0.01≤x≤0.3, eg, 0.01≤x≤0.2.
[0330] The LUMO energy level of the quantum dot light-emitting layer 200' may be a value between the LUMO energy level of the quantum dot light-emitting layer 200' and the LUMO energy level of the electron injection layer 17, and may be about 3.2eV to about 4.8eV, about 3.2eV to about 4.6eV, about 3.2eV to about 4.5eV, about 3.2eV to about 4.3eV, about 3.2eV to about 4.1eV, about 3.4eV to 4.1eV, about 3.5eV to about 4.6eV, about 3.6eV to about 4.6eV, about 3.6eV to about 4.3eV, about 3.6eV to about 4.1eV, about 3.6eV to about 3.9eV, about 3.7eV to about 4.6eV, about 3.7eV to about 4.3eV, about 3.7eV to about 4.1eV, or about 3.7eV to about 3.9eV.
[0331] The thickness of the electron transport layer 133c may be greater than about 10 nm and less than or equal to about 80 nm, and within a range of greater than about 10 nm and less than or equal to about 70 nm, greater than about 10 nm and less than or equal to about 60 nm, greater than about 10 nm and less than or equal to about 50 nm, greater than about 10 nm and less than or equal to about 40 nm, or greater than about 10 nm and less than or equal to about 30 nm.
[0332] The LUMO energy level of the electron injection layer may be between the work function of the second electrode 500 and the LUMO energy level of the electron transport layer. For example, the difference between the work function of the second electrode 500 and the LUMO energy level of the electron injection layer may be less than about 0.5 eV, about 0.001 eV to about 0.5 eV, about 0.001 eV to about 0.4 eV, or about 0.001 eV to about 0.3 eV. As an example, the difference between the LUMO energy level of the electron injection layer and the LUMO energy level of the electron transport layer may be less than about 0.5 eV, about 0.001 eV to about 0.5 eV, about 0.001 eV to about 0.4 eV, or about 0.001 eV to about 0.3 eV. Therefore, electrons can be easily injected from the second electrode 500 into the electron injection layer to reduce the driving voltage of the quantum dot device, and electrons can be effectively transferred from the electron injection layer to the electron transport layer to improve efficiency. Within the range satisfying the aforementioned energy levels, the LUMO energy level of the electron injection layer may be about 3.4eV to about 4.8eV, about 3.4eV to about 4.6eV, about 3.4eV to about 4.5eV, about 3.6eV to about 4.8eV, about 3.6eV to about 4.6eV, about 3.6eV to about 4.5eV, about 3.6eV to about 4.3eV, about 3.9eV to about 4.8eV, about 3.9eV to about 4.6eV, about 3.9eV to about 4.5eV, or about 3.9eV to about 4.3eV.
[0333] The electron injection layer may be thinner than the electron transport layer. For example, the thickness of the electron injection layer may be about 0.01 times to about 0.8 times, about 0.01 times to about 0.7 times, about 0.01 times to about 0.5 times, about 0.1 times to about 0.8 times, about 0.1 times to about 0.7 times, or about 0.1 times to about 0.5 times the thickness of the electron transport layer. The thickness of the electron injection layer 17 may be, for example, less than or equal to about 10 nm, less than or equal to about 7 nm, or less than or equal to about 5 nm. Within a range, the thickness of the electron injection layer 17 may be about 1 nm to about 10 nm, about 1 nm to about 8 nm, about 1 nm to about 7 nm, or about 1 nm to about 5 nm.
[0334] In some embodiments of the present disclosure, the thickness of organic layer 300' does not exceed 20 nm. In other embodiments, the thickness of organic layer 300' does not exceed 3 nm, and within a single opening, organic layer 300' is a discontinuous film layer having multiple cavities. Organic layer 300' is made from the organic material layer 300 described in the above-described embodiment. Furthermore, the material of organic layer 300' includes paraffin wax.
[0335] Furthermore, the quantum dot light-emitting device may also include an encapsulation layer 600. Specifically, after the above-mentioned step S600, as shown in Figures 18 to 21, a second carrier transport layer 400 and a second electrode 500 may be further formed, and then the encapsulation is completed to form an encapsulation layer 600. At this point, a quantum dot light-emitting device can be manufactured.
[0336] In other embodiments, the quantum dot light-emitting device is a photoluminescent quantum dot device. The quantum dot device further includes multiple light-emitting units disposed between the base substrate 101 and the quantum dot light-emitting layer 200'. Each light-emitting unit may correspond to an opening in the pixel definition layer 120. Light emitted by the light-emitting unit may cause the quantum dot light-emitting layer 200' to emit light. The light-emitting unit may be an OLED light-emitting device, the specific structure of which is not described in detail here.
[0337] It should be noted that although the steps of the method of the present disclosure are described in a specific order in the accompanying drawings, this does not require or imply that the steps must be performed in this specific order, or that all steps must be performed to achieve the desired results. Additional or alternative steps, such as omitting certain steps, combining multiple steps into one step, and / or decomposing a step into multiple steps, should all be considered part of this disclosure.
[0338] It should be understood that the present disclosure is not limited in its application to the detailed structure and arrangement of the components set forth in this specification. The present disclosure is capable of other embodiments and can be implemented and executed in a variety of ways. The aforementioned variations and modifications fall within the scope of the present disclosure. It should be understood that the present disclosure disclosed and defined in this specification extends to all alternative combinations of two or more individual features mentioned or evident in the text and / or the drawings. All of these different combinations constitute multiple alternative aspects of the present disclosure. The embodiments of this specification illustrate the best mode known for implementing the present disclosure and will enable those skilled in the art to utilize the present disclosure.
Claims
1. A method for patterning a quantum dot film layer, comprising: forming a quantum dot material layer on one side of the substrate; Forming an organic material layer on a side of the quantum dot material layer away from the substrate, wherein the transmittance of the organic material layer in the ultraviolet band and the visible light band is not less than 80%; Exposing a preset area of the substrate so that the material in the quantum dot material layer located in the preset area is cross-linked or generates a salt insoluble in a developer, or / and the material in the organic material layer located in the preset area is cross-linked; The organic material layer and the quantum dot material layer in non-preset areas of the substrate are removed.
2. The method for patterning a quantum dot film layer according to claim 1, wherein: The material in the organic material layer includes a hydrocarbon mixture having 18-30 carbon atoms.
3. The method for patterning a quantum dot film layer according to claim 2, wherein: The material in the organic material layer further includes a first photosensitive crosslinking agent.
4. The method for patterning a quantum dot film layer according to claim 2, wherein: In terms of weight percentage, the hydrocarbon mixture includes 80%-100% of straight-chain alkanes and 0%-20% of other hydrocarbons. The other hydrocarbons include any one of branched alkanes, cycloalkanes, olefins, and alkynes, or a combination thereof.
5. The method for patterning a quantum dot film layer according to claim 3, wherein: In terms of weight percentage, the photosensitive crosslinking agent accounts for 1-30% of the hydrocarbon mixture.
6. The method for patterning a quantum dot film layer according to claim 1, wherein: The material in the organic material layer includes paraffin wax.
7. The method for patterning a quantum dot film layer according to claim 1, wherein: The initial melting temperature of the material in the organic material layer is not greater than 60°C.
8. The method for patterning a quantum dot film layer according to claim 1, wherein: The initial thickness of the organic material layer is 20nm-80nm.
9. The method for patterning a quantum dot film layer according to claim 1, wherein: The material of the quantum dot material layer includes a first quantum dot body, a second quantum dot body, a quantum dot ligand and a second photosensitive cross-linking agent; The quantum dot ligand is connected to the first quantum dot body and / or the second quantum dot body through a coordination bond; The quantum dot ligand comprises a first photosensitive group, the first photosensitive group is located at the end of the quantum dot ligand molecular structure, and the second photosensitive crosslinking agent is used to induce a crosslinking reaction of the first photosensitive group.
10. The method for patterning a quantum dot film layer according to claim 9, wherein: The first photosensitive group contains a carbon-carbon double bond, or a saturated 3-5-membered heterocyclic structure containing O or S.
11. The method for patterning a quantum dot film layer according to claim 1, wherein: The materials of the quantum dot material layer include a first quantum dot body, a second quantum dot body, a quantum dot ligand and a photosensitive initiator; The quantum dot ligand comprises a first quantum dot ligand and a second quantum dot ligand, wherein the first quantum dot ligand is connected to the first quantum dot body via a coordination bond, and the second quantum dot ligand is connected to the second quantum dot body via a coordination bond; The first quantum dot ligand comprises a crosslinkable group, and the crosslinkable group is located at the end of the molecular structure of the first quantum dot ligand; the second quantum dot ligand comprises a second photosensitive group, and the structure of the second photosensitive group is -AB, where A is an imino group and B is a protecting group; Under light conditions, the second photosensitive group can remove the protective group under the action of the photosensitive initiator to form an amino group; the cross-linkable group can produce cross-links with the amino group formed by the second photosensitive group removing the protective group or form a salt insoluble in the developer; or the cross-linkable group can produce cross-links with the amino group formed by the second photosensitive group removing the protective group after being activated by an activator or form a salt insoluble in the developer.
12. The method for patterning a quantum dot film layer according to claim 11, wherein: The crosslinkable group is selected from epoxy groups, carboxylic acid groups or sulfonic acid groups.
13. The method for patterning a quantum dot film layer according to claim 1, wherein: The material in the quantum dot material layer includes a quantum dot body and a quantum dot ligand, the quantum dot ligand includes a coordination group, and the quantum dot body is connected to the quantum dot body through the coordination group; The quantum dot ligand comprises a structure -YZ, wherein Z is a solubilizing group, and the solubilizing group is selected from a polar group; Y comprises a connecting group and a third photosensitive group connected to each other, and the connecting group is connected between the coordination group and the third photosensitive group; and the connecting group is selected from an alkylene group; The third photosensitive group can break bonds under light conditions to decompose the interconnected quantum dot body and the quantum dot ligand into a first material comprising the interconnected quantum dot body, the coordination group and the connecting group, and a second material comprising the solubilizing group; The second material is soluble in a developing solution, and the first material is insoluble in a developing solution.
14. The method for patterning a quantum dot film layer according to claim 1, wherein: The materials in the quantum dot material layer include a first quantum dot body, a second quantum dot body, a quantum dot ligand and a third photosensitive cross-linking agent; The quantum dot ligand is connected to the first quantum dot body or / and the second quantum dot body through a coordination bond, and the quantum dot ligand contains an alkane chain; The third photosensitive crosslinker comprises at least two fourth photosensitive groups, and the fourth photosensitive groups are located at the ends of the molecular structure of the third photosensitive crosslinker; The fourth photosensitive group can undergo a carbon-hydrogen insertion reaction with the alkane chain in the quantum dot ligand under light conditions.
15. The method for patterning a quantum dot film layer according to claim 14, wherein: The fourth photosensitive group is selected from a structure comprising a benzophenone group, an azide group, a diazo group or a diaziridine group.
16. The method for patterning a quantum dot film layer according to claim 1, wherein: The material of the quantum dot material layer includes a quantum dot body and at least one quantum dot ligand, and the quantum dot ligand is connected to the quantum dot body through a coordination bond; Among the multiple quantum dot ligands, at least one of the quantum dot ligands contains an alkane chain in its molecular structure.
17. The method for patterning a quantum dot film layer according to claim 1, wherein: The quantum dot material layer and the organic material layer are formed in an inert gas or vacuum environment; The step of exposing the predetermined area of the substrate is performed in an atmospheric environment.
18. The method for patterning a quantum dot film layer according to claim 1, wherein: The step of removing the organic material layer and the quantum dot material layer in the non-preset area of the substrate comprises: Performing development to remove the organic material layer and the quantum dot material layer in the non-preset area; Wherein, the organic material layer located in the preset area is cross-linked during exposure.
19. The method for patterning a quantum dot film layer according to claim 18, wherein: Performing development to remove the organic material layer and the quantum dot material layer in non-preset areas of the substrate includes: Performing a first development using a first developer to remove the organic material layer in the non-preset area; Performing a second development using a second developer to remove the quantum dot material layer in the non-preset area; The first developing solution and the second developing solution are different.
20. The method for patterning a quantum dot film layer according to claim 1, wherein: The step of removing the organic material layer and the quantum dot material layer in the non-preset area of the substrate comprises: heating the non-preset area, rotating the substrate, melting the organic material layer located in the non-preset area and allowing the melted organic material layer to spin out under the action of centrifugal force; Performing development to remove the quantum dot material layer located in the non-preset area; During exposure, the quantum dot material layer located in the preset area undergoes cross-linking or generates salt that is insoluble in a developer.
21. The method for patterning a quantum dot film layer according to claim 1, wherein: The step of removing the organic material layer and the quantum dot material layer in the non-preset area of the substrate comprises: Using a first solvent to remove at least a portion of the organic material layer located in the preset area and at least a portion of the organic material layer located in the non-preset area, wherein the temperature of the first solvent is 60° C.-90° C.; Using a second developer to perform development to remove the quantum dot material layer located in the non-preset area; During exposure, the quantum dot material layer located in the preset area undergoes cross-linking or generates salt that is insoluble in a developer.
22. The method for patterning a quantum dot film layer according to claim 19, wherein: The temperature of the first developer is less than 60° C. The relative dielectric constant of the second developer is greater than the relative dielectric constant of the first developer.
23. The method for patterning a quantum dot film layer according to claim 20, wherein: The temperature of heating the non-preset area is 70°C-110°C.
24. The method for patterning a quantum dot film layer according to claim 21, wherein: After being treated with the first solvent, the thickness of the organic material layer is no more than 3 nm, or some voids appear in the organic material layer.
25. The method for patterning a quantum dot film layer according to claim 18 or 20, wherein: After removing the organic material layer and the quantum dot material layer in the non-preset area of the substrate, the step further includes: The substrate is placed horizontally, subjected to thermal annealing treatment at 60° C.-100° C. for 5 min-30 min, and then cooled to below 35° C.
26. The method for patterning a quantum dot film layer according to claim 18 or 20, wherein: After removing the organic material layer and the quantum dot material layer in the non-preset area of the substrate, the step further includes: Using a second solvent to remove at least a portion of the organic material layer located in the preset area, wherein the temperature of the second solvent is 60° C.-90° C.; The substrate is heated and dried.
27. The method for patterning a quantum dot film layer according to any one of claims 18, 20 or 21, wherein: After removing the organic material layer and the quantum dot material layer in the non-preset area of the substrate, the step further includes: Heating the substrate and rotating it, washing the rotating substrate with a third solvent to remove at least a portion of the remaining organic material layer, wherein the temperature of the third solvent is 70° C.-110° C.; The substrate is heated and dried.
28. The method for patterning a quantum dot film layer according to claim 5, wherein: The first photosensitive crosslinking agent molecular structure contains at least two fifth photosensitive groups, and the fifth photosensitive groups are located at the ends of the first photosensitive crosslinking agent molecular structure; The fifth photosensitive group is selected from a structure comprising a benzophenone group, an azide group, a diazo group or a diaziridine group.
29. The method for patterning a quantum dot film layer according to claim 1, wherein: The substrate comprises: substrate substrate; A pixel definition layer is disposed on one side of the base substrate, the pixel definition layer has a plurality of openings, and the quantum dot material layer is at least partially formed in the openings; Wherein, in a direction perpendicular to the substrate, the height of the pixel definition layer does not exceed 1.5 μm.
30. A quantum dot light-emitting layer, produced by the quantum dot film patterning method according to any one of claims 1 to 29.
31. A quantum dot light-emitting device, comprising the quantum dot light-emitting layer as claimed in claim 30.
32. A quantum dot light-emitting device, comprising: substrate substrate; A pixel definition layer, disposed on one side of the base substrate, the pixel definition layer having a plurality of openings; A quantum dot light-emitting layer is disposed on one side of the base substrate and is located in the opening; The organic layer is arranged on the side of the quantum dot light-emitting layer away from the base substrate. The transmittance of the organic layer in the ultraviolet band and the visible light band is not less than 80%, and the melting temperature of the material in the organic layer does not exceed 110°C.
33. The quantum dot light emitting device according to claim 32, wherein: The thickness of the organic layer does not exceed 20 nm.
34. The quantum dot light emitting device according to claim 32, wherein: The thickness of the organic layer does not exceed 3 nm, and the organic layer in a single opening is a discontinuous film layer having a plurality of cavities.
35. The quantum dot light emitting device according to claim 32, wherein: The material in the organic layer includes paraffin wax.
36. The quantum dot light emitting device according to claim 32, wherein: The quantum dot light-emitting layer has a cross-linked network structure, or / and The organic layer has a cross-linked network structure or a salt insoluble in a developer.
37. The quantum dot light emitting device according to claim 32, wherein: The quantum dot light emitting device further comprises a first electrode, a second electrode, a first carrier transport layer and a second carrier transport layer; The first electrode is disposed between the base substrate and the quantum dot light-emitting layer, and the first carrier transport layer is disposed between the first electrode and the quantum dot light-emitting layer; The second carrier transport layer is disposed on a side of the organic layer away from the base substrate, and the second electrode is disposed on a side of the second carrier transport layer away from the base substrate.