Method for preventing metallic copper from corrosion and metallic copper Anti-corrosion structure
By forming a graphene layer on the surface of the copper matrix, the problem of copper oxidation corrosion is solved, better anti-corrosion performance and service life are achieved, and corrosion losses are reduced.
Patent Information
- Application Number
- PCT/CN2023/101146
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-28
- Filing Date
- 2023-06-19
- Publication Date
- 2024-10-03
AI Technical Summary
When copper is exposed to the air for a long time, it causes oxidative corrosion due to the reaction of oxygen and water vapor. The existing protective layer materials have poor electrical and thermal conductivity, high cost and large thickness, and cannot effectively prevent copper corrosion, resulting in widespread use. Huge losses every year.
A graphene layer of at least 2 atomic layers thick is formed on the surface of the copper matrix, which blocks electrochemical reactions and improves the anti-corrosion properties of copper by weakening the charge transfer between corrosive substances and the copper matrix.
The graphene layer effectively reduces interface diffusion and electrochemical reactions, improves the anti-corrosion performance of copper, can significantly extend the service life of copper under normal and high temperature conditions, and reduces corrosion losses.
Smart Images

Figure CN2023101146_03102024_PF_FP_ABST
Abstract
Description
Method for preventing metal copper corrosion, and metal copper anti-corrosion structure
[0001] CROSS-REFERENCE TO RELATED APPLICATIONS
[0002] This application claims priority to Chinese patent application number 2023103159451 filed with the State Intellectual Property Office of China on March 28, 2023, entitled “A method for preventing metallic copper corrosion, and a metallic copper anti-corrosion structure,” the entire contents of which are incorporated by reference into this application. Technical Field
[0003] The present application relates to the technical field of metal anti-corrosion, and in particular to a method for preventing metal copper corrosion and a metal copper anti-corrosion structure. Background Art
[0004] Copper is a widely used nonferrous metal with excellent electrical and thermal conductivity, ductility, and a low melting point. It is easy to smelt and facilitates large-scale, low-cost industrial production and processing, making it widely used in the electrical, light, machinery, construction, and defense industries. A serious problem in copper applications is oxygen corrosion. When copper is exposed to air for long periods, oxygen and water vapor in the air react with the copper to form copper oxides, which significantly impact the quality and even the function of copper products. Currently, methods to mitigate oxygen corrosion of copper are often used, such as coating with other metals, organic coatings, and oxide coatings. However, these methods often suffer from poor electrical and thermal conductivity, are thick, have poor light transmittance, and provide incomplete protection. Due to the widespread use of copper, billions of dollars are lost annually due to copper oxidation corrosion. Therefore, the search for new, low-cost, high-quality, ultra-thin protective coating materials with improved corrosion resistance is of great practical value, economic significance, and environmental significance.
[0005] Summary of the Invention
[0006] The present application provides a method for preventing metallic copper from being corroded and a metallic copper anti-corrosion structure, which can at least improve the anti-corrosion performance of metallic copper.
[0007] Some embodiments of the present application provide a method for preventing metallic copper corrosion, which may include: forming a graphene layer with a thickness of at least 2 atomic layers on a surface of a copper substrate.
[0008] In the above technical solution, the method for preventing metallic copper corrosion provided by some embodiments of the present application can form a graphene layer with a thickness of at least 2 atomic layers on the surface of the copper substrate, which can weaken the charge transfer between the corrosive substance and the copper substrate, making it difficult for the copper substrate to undergo electrochemical reaction through the graphene layer on the surface, thereby improving the corrosion resistance of the copper substrate.
[0009] In some optional embodiments of the present application, the thickness of the graphene formed on the surface of the copper substrate may be 2 to 10 atomic layers.
[0010] In some optional embodiments of the present application, the copper substrate is single crystal copper.
[0011] In the above optional embodiment of the present application, when the copper substrate is single crystal copper, the anti-corrosion performance of the copper substrate is better.
[0012] In some optional embodiments of the present application, the method for obtaining single crystal copper may include:
[0013] Placing polycrystalline copper on a substrate and placing it in a CVD (Chemical Vapor Deposition) furnace, and heating it to 1000° C. to 1080° C. in an atmosphere including an inert gas and hydrogen to perform a single crystal process on the polycrystalline copper;
[0014] The flow rate of the inert gas is 100 sccm to 1000 sccm, and the flow rate of the hydrogen gas is 1 sccm to 50 sccm.
[0015] In some optional embodiments of the present application, the method of forming at least two layers of graphene on the surface of a copper substrate may include:
[0016] Graphene with a thickness of one atomic layer is formed on the surface of a copper substrate to obtain a first graphene layer, and graphene with a thickness of one atomic layer is formed on the surface of a copper-based carrier to obtain a second graphene layer, and then at least one second graphene layer is transferred to the surface of the first graphene layer, and a graphene coupling treatment is performed at 300° C. to 500° C. in an atmosphere including an inert gas and hydrogen.
[0017] Optionally, in the graphene coupling process, the flow rate of the inert gas is 100 sccm to 1000 sccm, and the flow rate of the hydrogen gas is 5 sccm to 100 sccm.
[0018] Optionally, the temperature for performing the graphene coupling treatment is 300°C, 320°C, 350°C, 380°C, 400°C, 420°C, 450°C, 480°C or 500°C.
[0019] Optionally, the graphene coupling treatment time is at least 6 hours.
[0020] Optionally, the graphene coupling treatment time is 6 hours to 24 hours.
[0021] In the above-mentioned optional embodiment, the method for preventing metallic copper corrosion can be performed by forming a first graphene layer with a thickness of one atomic layer on the surface of a copper substrate, and forming a second graphene layer with a thickness of one atomic layer on the surface of a copper-based support, respectively. The second graphene layer is then transferred to the surface of the first graphene layer on the surface of the copper substrate, and a double-layer graphene layer is obtained after a graphene coupling process. In this way, the first graphene layer can achieve a stronger coupling with the surface of the copper substrate, reducing interfacial diffusion. In addition, the second graphene layer is shielded, has less charge transfer, and is essentially neutral, which inhibits the occurrence of electrochemical reactions, thereby improving the corrosion resistance of the copper substrate.
[0022] In some optional embodiments of the present application, when transferring at least one second graphene layer onto the surface of the first graphene layer, one second graphene layer may be transferred each time, and graphene coupling processing may be performed after each transfer of one second graphene layer.
[0023] In some optional embodiments of the present application, a method for forming a first graphene layer or a second graphene layer with a thickness of 1 atomic layer on the surface of a copper substrate or a copper-based carrier may include:
[0024] A first graphene layer or a second graphene layer with a thickness of one atomic layer is deposited on at least a portion of the surface of a copper substrate or a copper-based carrier by chemical vapor deposition at 1000° C. to 1080° C. in an atmosphere including methane, hydrogen and inert gas.
[0025] Optionally, the flow rate of methane is 0.005 sccm to 0.05 sccm, the flow rate of the inert gas is 100 sccm to 1000 sccm, and the flow rate ratio of methane to hydrogen is 1:200 to 1:1500.
[0026] In some optional embodiments of the present application, the method of transferring at least one second graphene layer onto the surface of the first graphene layer may include:
[0027] Before the transfer, a resin layer is formed on the surface of the second graphene layer, and then the other graphene layers except the second graphene layer are etched. Then, the copper-based carrier located on the back of the second graphene layer is etched to obtain the second graphene layer supported on the surface of the resin layer. Then, the second graphene layer supported on the surface of the resin layer is placed on the surface of the first graphene layer for graphene coupling treatment.
[0028] In the above optional embodiment, the resin layer can serve as a carrier for the second graphene layer after it is separated from the copper-based carrier, so that the second graphene layer can be transferred to the surface of the first graphene layer while maintaining a good morphology.
[0029] In some optional embodiments of the present application, the resin layer may include polymethyl methacrylate or polypropylene carbonate.
[0030] In some optional embodiments of the present application, forming a resin layer on the surface of the second graphene layer may include: spin-coating a resin solution dissolved in a solvent onto the surface of the second graphene layer, and baking at a baking temperature of 40° C. to 160° C. for 1 min to 5 min.
[0031] In some optional embodiments of the present application, the solvent may include anisole.
[0032] In some optional embodiments of the present application, when the main component of the resin layer is polymethyl methacrylate, the mass fraction of polymethyl methacrylate in the resin solution can be 3wt% to 13wt%, and the baking temperature can be 80℃ to 160℃; or, when the main component of the resin layer is polypropylene carbonate, the mass fraction of polypropylene carbonate in the resin solution can be 6wt% to 18wt%, and the baking temperature can be 40℃ to 70℃.
[0033] In some optional embodiments of the present application, O2, O3, argon or hydrogen plasma may be used to etch the graphene layers other than the second graphene layer.
[0034] In some optional embodiments of the present application, the copper-based carrier on the back side of the second graphene layer can be etched using a 0.05 mol / L to 0.5 mol / L (NH4)2S2O8 solution and a FeCl3 solution. In some optional embodiments of the present application, the method of forming at least two layers of graphene on the surface of the copper substrate may include:
[0035] A graphene layer with a thickness of multiple atomic layers is deposited on at least a portion of the surface of a copper substrate by chemical vapor deposition at 1000° C. to 1080° C. in an atmosphere including methane, hydrogen and inert gas.
[0036] Optionally, the flow rate of methane is 0.005 sccm to 0.1 sccm, the flow rate of the inert gas is 100 sccm to 1000 sccm, and the flow rate ratio of methane to hydrogen is 1:10 to 1:150.
[0037] In the above optional embodiment of the present application, the method for preventing metallic copper corrosion is to directly deposit graphene on at least part of the surface of the copper substrate by chemical vapor deposition, and control the thickness of the graphene layer by controlling the flow rate of methane and hydrogen. Since the graphene layer is an overlapping of multiple layers of graphene, the defect density that can directly reach the copper surface is greatly reduced, and the graphene layer can block various oxidation pathways, thereby improving the corrosion resistance of the copper substrate.
[0038] Some other embodiments of the present application provide a metal copper anti-corrosion structure, which can be manufactured according to the above-mentioned method for preventing metal copper corrosion.
[0039] In the above embodiment, the graphene layer with a thickness of at least 2 atomic layers can weaken the charge transfer between the corrosive substance and the copper substrate, making it difficult for the copper substrate to undergo electrochemical reaction through the graphene layer on the surface, thereby improving the corrosion resistance of the copper substrate.
[0040] Still other embodiments of the present application provide a metal copper corrosion protection structure, which may include a copper substrate and a graphene layer disposed on at least a portion of the surface of the copper substrate. The thickness of the graphene layer may be at least 2 atomic layers.
[0041] In the above embodiment, the graphene layer with a thickness of at least 2 atomic layers can weaken the charge transfer between the corrosive substance and the copper substrate, making it difficult for the copper substrate to undergo electrochemical reaction through the graphene layer on the surface, thereby improving the corrosion resistance of the copper substrate. BRIEF DESCRIPTION OF THE DRAWINGS
[0042] In order to more clearly illustrate the technical solutions of the embodiments of the present application, the following is a brief introduction to the drawings required for use in the embodiments. It should be understood that the following drawings only show certain embodiments of the present application and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other relevant drawings can be obtained based on these drawings without creative work.
[0043] FIG1 is a comparison diagram of the relationship between the corrosion area and time of the metal copper anti-corrosion structures of Example 1 and Comparative Example 1 at 200° C.;
[0044] FIG2 is an SEM image of the metal copper anti-corrosion structure of Examples 1 to 3 and Comparative Example 1 after being corroded at 230 Pa oxygen and 600° C. for 1 second;
[0045] FIG3 is an SEM image of the metal copper anti-corrosion structure of Examples 1 to 3 and Comparative Example 1 after being corroded at 230 Pa oxygen and 600° C. for 10 minutes;
[0046] FIG4 is a comparison of the anti-corrosion effects of the metal copper anti-corrosion structures of Example 1 and Comparative Example 1 after baking at 250° C. for 6 hours;
[0047] FIG5 is a comparison diagram of the anti-corrosion effects of the metal copper anti-corrosion structures of Examples 1 to 2 and Comparative Example 1 after baking at 250° C. for 0 h, 0.5 h, 10 h, and 15 h. DETAILED DESCRIPTION
[0048] Copper is a widely used nonferrous metal with excellent electrical and thermal conductivity, ductility, and a low melting point. It is easy to smelt and facilitates large-scale, low-cost industrial production and processing, making it widely used in the electrical industry, light industry, machinery manufacturing, construction, and defense industries. However, a serious problem in copper applications is oxygen corrosion. When copper is exposed to air for long periods of time, oxygen and water vapor in the air react with the copper to form copper oxides, which significantly affects the quality and even the function of copper products. Currently, methods to prevent copper from oxygen corrosion are often used, such as coating with other metals, organic protective layers, and oxide protective layers. However, these methods often suffer from poor electrical and thermal conductivity, are thick, have poor light transmittance, and provide incomplete protection. Due to the widespread use of copper, the annual losses from copper oxidative corrosion amount to billions of dollars.
[0049] However, the inventors discovered that when using graphene to protect copper from corrosion, the corrosion protection capability of graphene decreases dramatically at the exposed graphene-copper interface due to interfacial diffusion caused by the weak coupling between the graphene and copper interfaces and the fact that graphene is more inert than copper, acting as a cathode in the electrochemical reaction. Currently, although various approaches have been proposed to address this issue, they all rely on the graphene and copper forming a co-conformable system or on the flatness of the copper surface, making such approaches too complex to address diverse industrial applications.
[0050] Based on the above considerations, in order to improve the corrosion resistance of metallic copper, the inventors have conducted in-depth research and designed a method for preventing metallic copper corrosion. This method forms a graphene layer at least 2 atomic layers thick on the surface of the copper substrate, which can weaken the charge transfer between the corrosive substance and the copper substrate, making it difficult for the copper substrate to undergo electrochemical reactions through the graphene layer on the surface, thereby blocking the following four corrosion failure paths: (1) defects caused by the graphene growth process; (2) interface diffusion caused by weak coupling between graphene and copper; (3) electrochemical reaction between graphene and copper; (4) penetration of corrosive molecules. In addition, this method can also prevent the further expansion of copper corrosion even when defects exist and defects are generated during operation, thereby maintaining good corrosion resistance.
[0051] The embodiments of the present application will be described in detail below with reference to the examples, but it will be understood by those skilled in the art that the following examples are merely illustrative of the present application and should not be considered as limiting the scope of the present application. In the examples, if specific conditions are not specified, the conditions are carried out according to conventional conditions or manufacturer recommendations. The reagents or instruments used are not specified by the manufacturer and are conventional products that can be purchased commercially.
[0052] The following is a detailed description of a method for preventing metal copper corrosion and a metal copper anti-corrosion structure provided in some embodiments of the present application:
[0053] Some embodiments of the present application provide a method for preventing metallic copper corrosion, comprising: forming a graphene layer with a thickness of at least 2 atomic layers on a surface of a copper substrate.
[0054] Optionally, the graphene layer formed on the surface of the copper substrate has a thickness of 2 to 10 atomic layers.
[0055] As an example, the thickness of the graphene layer formed on the surface of the copper substrate can be 2 atomic layers, 3 atomic layers, 4 atomic layers, 5 atomic layers, 6 atomic layers, 7 atomic layers, 8 atomic layers, 9 atomic layers or 10 atomic layers.
[0056] Optionally, the thickness of the graphene layer formed on the surface of the copper substrate is 2 to 4 atomic layers.
[0057] Optionally, the copper substrate is single crystal copper.
[0058] When the copper substrate is single crystal copper, the anti-corrosion performance of the copper substrate is better.
[0059] The method of converting polycrystalline copper into single crystal may include:
[0060] Polycrystalline copper is placed on a substrate and loaded into a CVD furnace, and heated to 1000° C. to 1080° C. in an atmosphere including an inert gas and hydrogen to perform a copper single crystal process.
[0061] As an example, the temperature of the copper single crystallization process may be 1000°C, 1010°C, 1020°C, 1030°C, 1040°C, 1050°C, 1060°C, 1070°C, or 1080°C.
[0062] Optionally, the flow rate of the inert gas in the copper single crystallization process is 100 sccm to 1000 sccm, and the flow rate of the hydrogen gas is 1 sccm to 50 sccm.
[0063] The inert gas in the copper single crystallization process may include any one or more of helium, argon, xenon and nitrogen.
[0064] As an example, the flow rate of the inert gas in the copper single crystallization process can be 100sccm, 200sccm, 300sccm, 400sccm, 500sccm, 600sccm, 700sccm, 800sccm, 900sccm or 1000sccm; the flow rate of hydrogen in the copper single crystallization process can be 1sccm, 2sccm, 5sccm, 8sccm, 10sccm, 20sccm, 30sccm, 40sccm or 50sccm.
[0065] Optionally, the copper single crystallization treatment time may be 10 min to 300 min.
[0066] As an example, the copper single crystallization treatment time may be 10 min, 20 min, 50 min, 80 min, 100 min, 120 min, 150 min, 180 min, 200 min, 220 min, 250 min, 280 min, or 300 min.
[0067] In some embodiments of the present application, a method for forming at least two layers of graphene on a surface of a copper substrate may include:
[0068] Graphene with a thickness of one atomic layer is formed on the surface of a copper substrate to obtain a first graphene layer, and graphene with a thickness of one atomic layer is formed on the surface of a copper-based carrier to obtain a second graphene layer, and then at least one second graphene layer is transferred to the surface of the first graphene layer, and a graphene coupling treatment is performed at 300° C. to 500° C. in an atmosphere including an inert gas and hydrogen.
[0069] As an example, the temperature of the graphene coupling process may be 300°C, 320°C, 350°C, 380°C, 400°C, 420°C, 450°C, 480°C, or 500°C.
[0070] Optionally, in the graphene coupling process, the flow rate of the inert gas is 100 sccm to 1000 sccm, and the flow rate of the hydrogen gas is 5 sccm to 100 sccm.
[0071] The inert gas in the graphene coupling process includes any one or more of helium, argon, xenon and nitrogen.
[0072] As an example, the flow rate of the inert gas in the graphene coupling process can be 100 sccm, 200 sccm, 300 sccm, 400 sccm, 500 sccm, 600 sccm, 700 sccm, 800 sccm, 900 sccm or 1000 sccm; the flow rate of hydrogen in the graphene coupling process can be 1 sccm, 2 sccm, 5 sccm, 8 sccm, 10 sccm, 20 sccm, 30 sccm, 40 sccm, 50 sccm, 60 sccm, 70 sccm, 80 sccm, 90 sccm or 100 sccm.
[0073] Optionally, the graphene coupling treatment time is at least 6 hours.
[0074] As an example, the time of the graphene coupling treatment may be 6 hours, 7 hours, 8 hours, 9 hours, 10 hours, 11 hours or 12 hours.
[0075] Optionally, the graphene coupling treatment time is 6 hours to 24 hours.
[0076] In an embodiment of the present application, a first graphene layer is obtained by forming a graphene layer one atomic layer thick on the surface of a copper substrate, and a second graphene layer is obtained by forming a graphene layer one atomic layer thick on the surface of a copper-based support. The second graphene layer is then transferred to the surface of the first graphene layer on the surface of the copper substrate, and a double-layer graphene layer is obtained after a graphene coupling process. In this way, the first graphene layer can have a stronger coupling with the surface of the copper substrate, reducing interfacial diffusion. At the same time, the second graphene layer is shielded, has less charge transfer, and is essentially neutral, which inhibits the occurrence of electrochemical reactions, thereby improving the corrosion resistance of the copper substrate.
[0077] Optionally, when transferring at least one second graphene layer onto the surface of the first graphene layer, one second graphene layer is transferred each time, and after each second graphene layer is transferred, a graphene coupling process is performed.
[0078] The method of transferring at least one second graphene layer onto the surface of the first graphene layer may include:
[0079] Before the transfer, a resin layer is formed on the surface of the second graphene layer, and then the other graphenes except the second graphene layer are etched. Then, the copper-based carrier on the back of the second graphene layer is etched to obtain the second graphene layer supported on the surface of the resin layer. Then, the second graphene layer supported on the surface of the resin layer is placed on the surface of the first graphene layer for graphene coupling treatment.
[0080] The resin layer includes polymethyl methacrylate or polypropylene carbonate.
[0081] The method of forming a resin layer on the surface of the second graphene layer may include:
[0082] The resin solution dissolved in the solvent is spin-coated onto the surface of the second graphene layer, and baked at 40° C. to 160° C. for 1 minute to 5 minutes.
[0083] The solvent includes anisole. When the main component of the resin layer is polymethyl methacrylate, the mass fraction of polymethyl methacrylate in the resin solution is 3wt% to 13wt%, and the baking temperature is 80°C to 160°C. When the main component of the resin layer is polypropylene carbonate, the mass fraction of polypropylene carbonate in the resin solution is 6wt% to 18wt%, and the baking temperature is 40°C to 70°C.
[0084] Optionally, O2, O3, argon or hydrogen plasma is used to etch the graphene layers other than the second graphene layer.
[0085] Optionally, a 0.05 mol / L to 0.5 mol / L (NH 4 ) 2 S 2 O 8 solution and a FeCl 3 solution are used to etch the copper-based carrier on the back side of the second graphene layer.
[0086] Optionally, the step of etching the copper-based carrier on the back side of the second graphene layer is performed in a water tank and is dried at 60° C. to 90° C. before the graphene coupling treatment is performed.
[0087] The resin layer can serve as a carrier for the second graphene layer after it is separated from the copper-based carrier, so that the second graphene layer can be transferred to the surface of the first graphene layer while maintaining a good morphology.
[0088] The method of forming a first graphene layer or a second graphene layer with a thickness of one atomic layer on the surface of a copper substrate or a copper-based carrier may include:
[0089] A first graphene layer or a second graphene layer with a thickness of one atomic layer is deposited on at least a portion of the surface of a copper substrate or a copper-based carrier by chemical vapor deposition at 1000°C to 1080°C in an atmosphere including methane, hydrogen and inert gas, and then methane and hydrogen are continuously introduced, and the mixture is naturally cooled under atmospheric pressure.
[0090] Optionally, the flow rate of methane is 0.005 sccm to 0.05 sccm, the flow rate of the inert gas is 100 sccm to 1000 sccm, and the flow rate ratio of methane to hydrogen is 1:200 to 1:1500.
[0091] As an example, the flow rate of methane can be 0.005sccm, 0.008sccm, 0.01sccm, 0.02sccm, 0.03sccm, 0.04sccm or 0.05sccm; the flow rate ratio of methane to hydrogen can be 1:200, 1:300, 1:400, 1:500, 1:600, 1:700, 1:800, 1:900, 1:1000, 1:1100, 1:1200, 1:1300, 1:1400 or 1:1500.
[0092] Optionally, the deposition time is 10 min to 30 min.
[0093] As an example, the deposition time may be 10 min, 12 min, 15 min, 18 min, 20 min, 22 min, 25 min, 28 min, or 30 min.
[0094] In some embodiments of the present application, a method for forming at least two layers of graphene on a surface of a copper substrate may include:
[0095] A graphene layer with a thickness of multiple atomic layers is deposited on at least a portion of the surface of a copper substrate by chemical vapor deposition at 1000°C to 1080°C in an atmosphere including methane, hydrogen and inert gas, and then methane and hydrogen are continuously introduced, followed by natural cooling under atmospheric pressure.
[0096] Optionally, the flow rate of methane is 0.005 sccm to 0.1 sccm, the flow rate of the inert gas is 100 sccm to 1000 sccm, and the flow rate ratio of methane to hydrogen is 1:10 to 1:150.
[0097] As an example, the flow rate of methane can be 0.005sccm, 0.008sccm, 0.01sccm, 0.02sccm, 0.03sccm, 0.04sccm, 0.05sccm, 0.06sccm, 0.07sccm, 0.08sccm, 0.09sccm, 0.1sccm; the flow rate ratio of methane to hydrogen can be 1:10, 1:20, 1:30, 1:40, 1:50, 1:60, 1:70, 1:80, 1:90, 1:100, 1:110, 1:120, 1:130, 1:140 or 1:150.
[0098] Optionally, the deposition time is 10 min to 300 min.
[0099] As an example, the deposition time may be 10 min, 20 min, 50 min, 80 min, 100 min, 120 min, 150 min, 180 min, 200 min, 220 min, 250 min, 280 min, or 300 min.
[0100] The method for preventing metallic copper corrosion provided in the embodiments of the present application forms a graphene layer with a thickness of at least 2 atomic layers on the surface of the copper substrate, which can weaken the charge transfer between the corrosive substance and the copper substrate, making it difficult for the copper substrate to undergo electrochemical reactions through the graphene layer on the surface, thereby improving the corrosion resistance of the copper substrate.
[0101] Other embodiments of the present application further provide a metal copper anti-corrosion structure, which is manufactured according to the above-mentioned method for preventing metal copper corrosion.
[0102] A graphene layer with a thickness of at least 2 atomic layers can weaken the charge transfer between corrosive substances and the copper matrix, making it difficult for the copper matrix to undergo electrochemical reactions through the graphene layer on the surface, thereby improving the corrosion resistance of the copper matrix.
[0103] The metal copper anti-corrosion structure comprises a copper substrate and a graphene layer arranged on at least a portion of the surface of the copper substrate, wherein the thickness of the graphene layer is at least 2 atomic layers.
[0104] The following is a further detailed description of a method for preventing metal copper corrosion and a metal copper anti-corrosion structure of the present application in conjunction with embodiments.
[0105] Example 1
[0106] The present invention provides a method for preventing copper corrosion, which comprises the following steps:
[0107] S1. Copper single crystal treatment
[0108] A 25 μm thick rolled copper foil was placed on a quartz substrate and loaded into a CVD furnace, heated to 1040°C in an atmosphere of 500 sccm Ar and 10 sccm H2, and kept at 1040°C for 120 minutes to transform the polycrystalline copper foil into a single crystal.
[0109] S2, forming a graphene layer with a thickness of one atomic layer on the surface of the copper-based support and the copper substrate
[0110] At least two 25μm thick single-crystallized rolled copper foils were placed on a quartz substrate and loaded into a CVD furnace. Graphene was deposited on at least a portion of the surface of the single-crystallized rolled copper foil at 1040°C for 20 minutes in an atmosphere of 0.01sccm CH4, 10sccm H2 and 500sccm Ar to form a graphene layer with a thickness of one atomic layer. Methane and hydrogen were continued to be introduced, and the mixture was naturally cooled at atmospheric pressure.
[0111] S3, graphene layer coupling
[0112] An 8wt% anisole solution of polymethyl methacrylate is spin-coated onto the surface of the graphene layer on the front of a copper-based carrier and baked at 120°C for 2 min to obtain a polymethyl methacrylate layer. The graphene on the back of the copper-based carrier is completely etched using O2 plasma, and then the copper-based carrier is etched in a water tank with a 0.1mol / L (NH4)2S2O8 solution to obtain a graphene layer supported on the surface of the polymethyl methacrylate layer. The graphene layer supported on the surface of the polymethyl methacrylate layer is then smoothly placed on the surface of the graphene layer on the surface of the copper substrate, with the two graphene layers in direct contact during placement. The graphene layers are then removed from the water tank and dried at 80°C. Finally, the layers are annealed at 400°C for 10 h in an atmosphere of 300sccm Ar and 20sccm H2 to remove the polymethyl methacrylate layer and couple the two graphene layers to obtain a double-layer graphene layer.
[0113] Example 2
[0114] The present embodiment provides a method for preventing metallic copper corrosion. After coupling the two graphene layers in Example 1 to obtain a double-layer graphene layer, the graphene layer supported on the surface of the polymethyl methacrylate layer is smoothly placed on the surface of the double-layer graphene layer on the surface of the copper substrate, so that the two graphene layers are in direct contact during placement. The graphene layers are then removed from the water tank and dried at 80°C. Finally, the layers are annealed at 400°C for 10 hours in an atmosphere of 300 sccm Ar and 20 sccm H2 to remove the polymethyl methacrylate layer and couple the two graphene layers to obtain a triple-layer graphene layer.
[0115] Example 3
[0116] The present embodiment provides a method for preventing metallic copper corrosion. After coupling the two graphene layers in Example 2 to obtain a three-layer graphene layer, the graphene layer supported on the surface of the polymethyl methacrylate layer is smoothly placed on the surface of the three-layer graphene layer on the surface of the copper substrate, so that the two graphene layers are in direct contact during placement. The graphene layers are then removed from the water tank and dried at 80°C. Finally, the layers are annealed at 400°C for 10 hours in an atmosphere of 300 sccm Ar and 20 sccm H2 to remove the polymethyl methacrylate layer and couple the two graphene layers to obtain a four-layer graphene layer.
[0117] Example 4
[0118] The present invention provides a method for preventing copper corrosion, which comprises the following steps:
[0119] S1. Copper single crystal treatment
[0120] A 25 μm thick rolled copper foil was placed on a quartz substrate and loaded into a CVD furnace, heated to 1040°C in an atmosphere of 500 sccm Ar and 10 sccm H2, and kept at 1040°C for 120 minutes to transform the polycrystalline copper foil into a single crystal.
[0121] S2, forming a graphene layer with a thickness of one atomic layer on the surface of the copper-based support and the copper substrate
[0122] A 25 μm thick single-crystallized rolled copper foil was placed on a quartz substrate and loaded into a CVD furnace. First, a graphene layer with a thickness of two atomic layers was deposited on at least a portion of the surface of the single-crystallized rolled copper foil in an atmosphere of 0.01 sccm CH4, 20 sccm H2 and 500 sccm Ar at 1040°C for 10 minutes. Then, a graphene layer with a thickness of two atomic layers was deposited on at least a portion of the surface of the single-crystallized rolled copper foil in an atmosphere of 0.05 sccm CH4, 50 sccm H2 and 500 sccm Ar at 1040°C for 30 minutes. Methane and hydrogen were continued to be introduced, and the mixture was naturally cooled at atmospheric pressure to obtain a double-layer graphene layer.
[0123] Comparative Example 1
[0124] The comparative example of the present application provides a method for preventing metallic copper corrosion, which comprises the following steps:
[0125] S1. Copper single crystal treatment
[0126] A 25 μm thick rolled copper foil was placed on a quartz substrate and loaded into a CVD furnace, heated to 1040°C in an atmosphere of 500 sccm Ar and 10 sccm H2, and kept at 1040°C for 120 minutes to transform the polycrystalline copper foil into a single crystal.
[0127] S2, forming a graphene layer with a thickness of one atomic layer on the surface of the copper-based support and the copper substrate
[0128] A 25 μm thick single-crystallized rolled copper foil was placed on a quartz substrate and loaded into a CVD furnace. Graphene was deposited on at least a portion of the surface of the single-crystallized rolled copper foil at 1040°C for 20 minutes in an atmosphere of 0.01 sccm CH4, 10 sccm H2 and 500 sccm Ar to form a graphene layer with a thickness of one atomic layer. Methane and hydrogen were continued to be introduced, and the mixture was naturally cooled at atmospheric pressure to obtain a single-layer graphene layer.
[0129] Test Example 1
[0130] The surface potential and nano-angle-resolved photoelectron spectrum of the graphene layer of Example 1 and Comparative Example 1 were measured using a Kelvin probe force microscope and a nano-angle-resolved photoelectron spectrometer, respectively. The results are shown in Table 1.
[0131] Table 1 Surface potential and Dirac point downward shift of graphene layer in Example 1 and Comparative Example 1
[0132] As shown in Table 1, Kelvin probe atomic force microscopy measurements show that the surface potential of the double-layer graphene layer of Example 1 is about 135mV higher than the surface potential of the single-layer graphene layer of Comparative Example 1, indicating that the double-layer graphene layer is significantly more doped with electrons. Nano-angle-resolved photoelectron spectroscopy results also show that the single-layer graphene layer on Cu is electron-doped, and the Fermi level shifts up by about 0.15eV. However, for the double-layer graphene layer, the transferred electrons cause the Fermi level to shift up by about 0.2eV, and the electrons are mainly doped in the bottom layer, while the top layer is almost electrically neutral. The differential charge density wave calculated by first principles also proves that the lower layer of the double-layer graphene layer has a greatly enhanced coupling with copper, while the upper graphene is approximately charge neutral. Such a large Fermi level shift and unique electron distribution strengthen the coupling between the bottom graphene and Cu, thereby suppressing interface diffusion. More importantly, the top graphene is almost undoped due to the shielding effect, and the active electron density on the surface of the top graphene is greatly reduced. Therefore, O2 is more difficult to be reduced to O 2-, and O 2- The diffusion of Cu is also restricted to the vertical direction, thereby mitigating the galvanic cell reaction on the exposed Cu surface. In this way, the four failure pathways of the graphene coating are blocked: impermeability to corrosive molecules, suppression of electrochemical reactions, reduction of intrinsic defect density, and blocking of interfacial diffusion. The synergistic effect of all four factors leads to the excellent anti-corrosion performance of the multilayer graphene layer.
[0133] Test Example 2
[0134] The oxidized copper surface was observed using an optical microscope. Brightness was used as a criterion for distinguishing oxidized areas from unoxidized areas. The areas of the two were counted. A comparison of the relationship between the corrosion area and time of the metal copper anti-corrosion structures of Example 1 and Comparative Example 1 at 200°C was obtained, as shown in FIG1 .
[0135] As shown in Figure 1, the epitaxial double-layer graphene layer can ensure that the copper oxidation ratio is below 5% after 1000 hours at 200°C, and the oxidation rate protected by the double-layer graphene layer is 5 orders of magnitude lower than that of the single-layer graphene layer.
[0136] Test Example 3
[0137] The oxidation process was observed in situ using an in-situ environmental scanning microscope, and SEM images of the metal copper anti-corrosion structures of Examples 1 to 3 and Comparative Example 1 after corrosion at 230 Pa oxygen and 600° C. for 1 second and 10 minutes were obtained, as shown in Figures 2 and 3.
[0138] As can be seen from Figures 2 and 3, the double-layer graphene layer, the triple-layer graphene layer, and the quadruple-layer graphene layer can all protect the copper surface well, while the single-layer graphene layer is completely destroyed within 1 second, showing the morphology of copper oxide.
[0139] Test Example 4
[0140] Using the naked eye observation method, the anti-corrosion effect comparison diagram of the metal copper anti-corrosion structure of Example 1 and Comparative Example 1 after baking at 250° C. for 6 hours was measured, as shown in FIG4 .
[0141] As shown in Figure 4, the area covered by the single-layer graphene layer has become darker, proving that the surface has been covered with copper oxide, while the area covered by the double-layer graphene layer still retains the brightness of copper.
[0142] Test Example 5
[0143] The oxidized copper surface was observed using an optical microscope, and the anti-corrosion effects of the metal copper anti-corrosion structures of Examples 1 to 2 and Comparative Example 1 after baking at 250° C. for 0 h, 0.5 h, 10 h, and 15 h were compared, as shown in FIG5 .
[0144] As shown in Figure 5, a single-layer graphene layer is completely covered by copper oxide after 0.5 hours of high-temperature oxidation (Figure 4-a). However, double-layer and triple-layer graphene layers can relatively completely protect the copper surface structure for up to 15 hours (Figures 4-b and 4-c). Furthermore, for a single defect, double-layer and triple-layer graphene layers have almost identical abilities to prevent its lateral expansion (defects indicated by arrows in Figures 4-b and 4-c). The advantage of triple-layer graphene lies solely in its ability to reduce the generation of new defects.
[0145] In summary, the method for preventing metallic copper corrosion and the metallic copper anti-corrosion structure of the embodiments of the present application can protect a copper substrate for more than five years at room temperature and normal humidity, and can protect copper for more than 1000 hours at 200°C or more than 6 hours at 250°C. Furthermore, the method for preventing metallic copper corrosion of the embodiments of the present application has no requirements for the crystal plane index and flatness of the copper, or the interlayer angle of the bilayer graphene, and has excellent anti-corrosion effects.
[0146] The foregoing description is merely a specific embodiment of the present application and is not intended to limit the present application. Persons skilled in the art will readily appreciate that various modifications and variations are possible. Any modifications, equivalent substitutions, or improvements made within the spirit and principles of the present application shall be included within the scope of protection of the present application. Industrial Applicability
[0147] Some embodiments of the present application provide a method for preventing metallic copper corrosion, the method comprising forming a graphene layer with a thickness of at least 2 atomic layers on the surface of a copper substrate. Other embodiments of the present application provide a metallic copper corrosion protection structure, the metallic copper corrosion protection structure comprising a copper substrate and a graphene layer disposed on at least a portion of the surface of the copper substrate, the graphene layer having a thickness of at least 2 atomic layers. The method for preventing metallic copper corrosion and the metallic copper corrosion protection structure provided by the embodiments of the present application can weaken the charge transfer between the corrosive substance and the copper substrate by forming a graphene layer with a thickness of at least 2 atomic layers on the surface of the copper substrate, making it difficult for the copper substrate to undergo electrochemical reactions through the graphene layer on the surface, thereby improving the corrosion resistance of the copper substrate.
[0148] Furthermore, it is understood that the method for preventing copper corrosion and the copper corrosion protection structure of the present application are reproducible and can be used in a variety of industrial applications. For example, the method for preventing copper corrosion and the copper corrosion protection structure of the present application can be used in industries that require copper for production and processing.
Claims
1. A method for preventing metallic copper from corroding, characterized in that: The method for preventing metal copper from corroding comprises: forming a graphene layer with a thickness of at least 2 atomic layers on the surface of a copper substrate.
2. The method for preventing metallic copper from corrosion according to claim 1, characterized in that: The graphene layer formed on the surface of the copper substrate has a thickness of 2 to 10 atomic layers.
3. The method for preventing metallic copper from corrosion according to claim 1 or 2, characterized in that: The copper substrate is single crystal copper.
4. The method for preventing metallic copper from corrosion according to claim 3, characterized in that: The method for obtaining the single crystal copper comprises: Placing polycrystalline copper on a substrate and loading it into a CVD furnace, and heating it to 1000° C. to 1080° C. in an atmosphere including an inert gas and hydrogen to perform a single crystal treatment on the polycrystalline copper; The flow rate of the inert gas is 100 sccm to 1000 sccm, and the flow rate of the hydrogen gas is 1 sccm to 50 sccm.
5. The method for preventing metallic copper from being corroded according to any one of claims 1 to 4, characterized in that: The method for forming at least two graphene layers on the surface of the copper substrate comprises: Forming a graphene layer with a thickness of one atomic layer on the surface of the copper substrate to obtain a first graphene layer, and forming a graphene layer with a thickness of one atomic layer on the surface of a copper-based carrier to obtain a second graphene layer, then transferring at least one of the second graphene layers to the surface of the first graphene layer, and performing a graphene coupling treatment at 300° C. to 500° C. in an atmosphere including an inert gas and hydrogen; Optionally, the flow rate of the inert gas in the graphene coupling process is 100 sccm to 1000 sccm, and the flow rate of the hydrogen gas is 5 sccm to 100 sccm; Optionally, the temperature for performing the graphene coupling treatment is 300° C., 320° C., 350° C., 380° C., 400° C., 420° C., 450° C., 480° C. or 500° C.; Optionally, the graphene coupling treatment time is at least 6 hours; Optionally, the graphene coupling treatment time is 6h to 24h.
6. The method for preventing metallic copper from corrosion according to claim 5, characterized in that: When at least one of the second graphene layers is transferred to the surface of the first graphene layer, one of the second graphene layers is transferred each time, and after each transfer of one of the second graphene layers, the graphene coupling process is performed.
7. The method for preventing metallic copper from corrosion according to claim 5, characterized in that: The method of forming a graphene layer with a thickness of one atomic layer on the surface of the copper substrate to obtain the first graphene layer comprises: depositing the first graphene layer with a thickness of one atomic layer on at least a portion of the surface of the copper substrate by chemical vapor deposition at 1000° C. to 1080° C. in an atmosphere comprising methane, hydrogen and an inert gas; or, the method of forming a graphene layer with a thickness of one atomic layer on the surface of the copper-based carrier to obtain the second graphene layer comprises: depositing the second graphene layer with a thickness of one atomic layer on at least a portion of the surface of the copper-based carrier by chemical vapor deposition at 1000° C. to 1080° C. in an atmosphere comprising methane, hydrogen and an inert gas; The flow rate of methane is 0.005 sccm to 0.05 sccm, the flow rate of the inert gas is 100 sccm to 1000 sccm, and the flow rate ratio of methane to hydrogen is 1:200 to 1:1500.
8. The method for preventing metallic copper from corroding according to any one of claims 5 to 7, characterized in that: The method of transferring at least one of the second graphene layers to the surface of the first graphene layer comprises: Before the transfer, a resin layer is first formed on the surface of the second graphene layer, and then the other graphenes except the second graphene layer are etched, and then the copper-based carrier located on the back side of the second graphene layer is etched to obtain the second graphene layer supported on the surface of the resin layer, and then the second graphene layer supported on the surface of the resin layer is placed on the surface of the first graphene layer to perform the graphene coupling treatment.
9. The method for preventing metallic copper from corrosion according to claim 8, characterized in that: The resin layer includes polymethyl methacrylate or polypropylene carbonate.
10. The method for preventing metallic copper from corrosion according to claim 8 or 9, characterized in that: Forming the resin layer on the surface of the second graphene layer includes: spin coating a resin solution dissolved in a solvent onto the surface of the second graphene layer, and baking at a baking temperature of 40° C. to 160° C. for 1 min to 5 min.
11. The method for preventing metal copper from corrosion according to claim 10, characterized in that: The solvent includes anisole.
12. The method for preventing metal copper from corroding according to any one of claims 10 to 11, characterized in that: When the main component of the resin layer is polymethyl methacrylate, the mass fraction of polymethyl methacrylate in the resin solution is 3wt% to 13wt%, and the baking temperature is 80°C to 160°C; or, when the main component of the resin layer is polypropylene carbonate, the mass fraction of polypropylene carbonate in the resin solution is 6wt% to 18wt%, and the baking temperature is 40°C to 70°C.
13. The method for preventing metal copper from corroding according to any one of claims 8 to 12, characterized in that: The other graphene layers except the second graphene layer are etched using O2, O3, argon or hydrogen plasma.
14. The method for preventing metal copper from corroding according to any one of claims 8 to 13, characterized in that: The copper-based carrier located on the back side of the second graphene layer is etched using a 0.05 mol / L to 0.5 mol / L (NH4)2S2O8 solution and a FeCl3 solution.
15. The method for preventing metal copper from corroding according to any one of claims 1 to 4, characterized in that: The method for forming at least two graphene layers on the surface of the copper substrate comprises: In an atmosphere including methane, hydrogen and inert gas at 1000°C to 1080°C, a chemical vapor deposition method is used to deposit the Depositing a graphene layer having a thickness of multiple atomic layers on at least a portion of the surface of the copper substrate; The flow rate of methane is 0.005 sccm to 0.1 sccm, the flow rate of the inert gas is 100 sccm to 1000 sccm, and the flow rate ratio of methane to hydrogen is 1:10 to 1:
150.
16. A metal copper anti-corrosion structure, characterized in that: The metal copper anti-corrosion structure is made according to the method for preventing metal copper corrosion according to any one of claims 1 to 15.
17. A metal copper anti-corrosion structure, characterized in that: The metal copper anti-corrosion structure comprises a copper substrate and a graphene layer arranged on at least a portion of the surface of the copper substrate, and the thickness of the graphene layer is at least 2 atomic layers.
Citation Information
Patent Citations
Preparation method of large-size Cu(111) monocrystal copper foil and ultra-large-size monocrystal graphene
CN105603514A
Method for fabrication and transfer of graphene
CN106458602A
Preparation method for oversized multilayer single crystal graphene and large-size single crystal copper nickel alloy
CN106835260A
Method for preventing metal corrosion through graphene depending on crystal surface
CN107740118A
Production method of graphene foil with a pre-defined number of graphene layers
EP3098198A1