Phosphorus-doped titanium dioxide, preparation method therefor and use thereof

By depositing titanium dioxide and silicon dioxide on black phosphorus nanosheets and performing protective calcination, phosphorus-doped titanium dioxide nanomaterials were prepared, which solved the problem of low photocatalytic efficiency of titanium dioxide, achieved absorption of visible light and infrared light, and improved photocatalysis Performance and stability.

WO2024198511A1PCT designated stage expired Publication Date: 2024-10-03SHENZHEN INST OF ADVANCED TECH

Patent Information

Application Number
PCT/CN2023/137884
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-30
Filing Date
2023-12-11
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

The application of existing titanium dioxide in the field of photocatalysis is limited by its wide optical band gap and rapid recombination of photoexcited carriers, resulting in low photocatalytic efficiency. Metal doping may lead to thermodynamic instability, and non-metal doping may lead to crystallization instability. Phase transition and particle size increase reduce catalyst activity.

Method used

By depositing titanium dioxide and silica on black phosphorus nanosheets using the sol-gel method, performing protective calcination, doping black phosphorus into the titanium dioxide crystal lattice, controlling the particle size and crystal phase, and preparing a product with a large specific surface area and uniform particle size. Phosphorus-doped titanium dioxide nanomaterials with adjustable crystallinity broaden the light absorption range to visible light and infrared light.

Benefits of technology

It improves the photocatalytic performance of titanium dioxide, realizes full utilization of visible light and near-infrared light, maximizes the use of solar energy, and improves the efficiency and stability of the photocatalyst.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN2023137884_03102024_PF_FP_ABST
    Figure CN2023137884_03102024_PF_FP_ABST
Patent Text Reader

Abstract

A phosphorus-doped titanium dioxide and a preparation method therefor. The preparation method for the phosphorus-doped titanium dioxide comprises the following steps: S1, using the sol-gel method to deposit titanium dioxide on a black phosphorus nanoplate to obtain a black phosphorus / titanium dioxide composite material; S2, depositing silicon dioxide on the black phosphorus / titanium dioxide composite material prepared in step S1 to obtain a black phosphorus / titanium dioxide / silicon dioxide composite material; and S3, calcining and etching the black phosphorus / titanium dioxide / silicon dioxide composite material obtained in step S2. A titanium dioxide nano material having the characteristics of a large specific surface area, high particle size uniformity, adjustable degree of crystallinity, controllable crystalline phase, etc. is prepared by means of the described method, further improving the photocatalysis properties of titanium dioxide.
Need to check novelty before this filing date? Find Prior Art

Description

A kind of phosphorus-doped titanium dioxide and its preparation method and application Technical Field

[0001] The present invention belongs to the field of photocatalysis, and in particular relates to phosphorus-doped titanium dioxide and a preparation method and application thereof. Background Art

[0002] [Corrected 18.02.2024 according to Rule 26] Since the discovery of titanium dioxide photocatalytic water splitting in 1972, photocatalytic technology has attracted widespread attention due to its use of inexhaustible green solar energy to solve the crisis of energy shortage and environmental pollution. 1-3 Titanium dioxide has the advantages of good chemical stability, strong redox ability, low cost and non-toxicity. It has been widely used in the fields of photocatalytic hydrogen and oxygen release, carbon dioxide reduction, decomposition of harmful substances, nitrogen fixation and organic synthesis. 4-9 However, the inherent wide optical band gap and rapid recombination of photoexcited carriers of TiO2 greatly limit its photocatalytic efficiency.

[0003] [Corrected 18.02.2024 according to Rule 26] In order to solve the above two shortcomings, recent research has focused on partially replacing Ti by doping metals (Ce, Ni, Ag, Pt, Fe, etc.) and non-metals (C, N, S, Si). 4+ and O 2- , thereby improving its performance 10-23 The role of metal doping is to promote the charge separation of photogenerated carriers and reduce their recombination rate. The role of non-metal doping is to move the absorption region of titanium dioxide from the ultraviolet region to the visible light region, while narrowing the band gap of titanium dioxide. In 2020, Chiara Alberoni et al. prepared nanotube (CeTNTx) and nanoparticle (CeTNPx) photocatalysts by doping CeO2 to adjust the electronic properties of nano-titanium dioxide. 10 The results show that the addition of Ce leads to a decrease in the energy gap, thereby improving the visible light absorption rate. When the CeO2 doping amount is 0.25wt%, the degradation rate of methylene blue (MB) of nanotubes and nanoparticles is the highest (0.123min -1 and 0.146min -1 ), and complete degradation was achieved in 120 minutes. In 2012, S. Krejcíkováa et al. used non-ionic surfactant Triton X-114, cyclohexane, AgNO3 aqueous solution and metal precursor as raw materials to prepare silver-doped TiO2 photocatalyst by sol-gel method. 16Compared with pure titanium dioxide catalyst, the absorption spectrum of silver-doped titanium dioxide catalyst shifts to the visible light region, and has excellent photocatalytic activity for the photocatalytic reduction of CO2. In 2021, Maria Sadia et al. synthesized nickel-doped and non-doped titanium dioxide photocatalysts using titanium isopropoxide as a precursor. 18 Studies have shown that nickel-doped titanium dioxide catalysts have a higher catalytic degradation efficiency in neutral red and methylene blue due to the reduced recombination rate of photogenerated electrons and holes. In 2018, Wenyi Huang et al. prepared a high-concentration N-doped anatase titanium dioxide photocatalyst using a low-temperature non-aqueous solvent thermal method. 14 Studies have shown that during the synthesis process, nitrogen atoms penetrate into the titanium dioxide lattice, forming impurity energy levels within the band gap of titanium dioxide, enhancing the absorption of visible light and having excellent performance in the photocatalytic degradation of methylene blue. In 2012, Jian-Wen Shi et al. used carbon spheres as templates and adopted a simple method to synthesize C-doped titanium dioxide hollow spheres (THS). 19 Studies have shown that C doping narrows the band gap of titanium dioxide and produces sub-bandgap absorption, which leads to the photoresponse of THS to visible light and shows higher photocatalytic activity for the decomposition of methylene blue than commercial P25. In 2017, Zhenyu Huang et al. synthesized S-TiO using thiourea dioxide as a sulfur source and a reducing agent. 2-x photocatalyst 15 Studies have shown that S doping leads to the 2-x The absorption edge of Ti is red-shifted. 3+ The introduction of S-TiO forms a localized state at the bottom of the conduction band. 2-x Can absorb visible light. In addition, Ti 3+ As an electron capture agent, it improves the conductivity of the photocatalyst and accelerates the transfer of electrons and holes. Compared with pure TiO2 photocatalyst, S-TiO 2-x The photocatalyst showed excellent photocatalytic activity for the degradation of Rhodamine B under visible light irradiation. In 2018, Zhenbiao Dong et al. reduced Ti-Si-O nanotubes on titanium-silicon alloy with zinc under Ar atmosphere to obtain black silicon-doped nanotubes, which were used as photoanodes for photoelectrochemical (PEC) water splitting. 12 The results show that due to the introduction of Si and Ti into the nanotubes 3+ The addition of / O vacancies enhances light absorption and promotes the separation of photogenerated electron-hole pairs. The photoconversion efficiency can reach 1.22%, which is 7.18 times that of undoped TiO2.

[0004] Existing technical solutions reduce the band gap of titanium dioxide through metal / non-metal doping, reduce the recombination rate of photogenerated electrons and holes, enhance titanium dioxide's absorption of visible light, and improve its photocatalytic performance. However, at the same time, metal ion doping can cause thermodynamic instability in titanium dioxide and introduce some photogenerated carrier recombination centers, which can reduce the performance of the catalyst to a certain extent. Doping with non-metallic elements such as carbon and nitrogen can lead to problems such as phase transformation of titanium dioxide, increase in nanoparticle size, and decrease in specific surface area, which will reduce the activity of the catalyst.

[0005] References

[0006] 1. Duan, Y.; Wang, Y.; Gan, L.; Meng, J.; Feng, Y.; Wang, K.; Zhou, K.; Wang, C.; Han, X.; Zhou,

[0007] 2. Fujishima, A.; Honda, K., Electrochemical Photolysis of Water at a Semiconductor Electrode. Nature 1972, 238(5358), 37-38.

[0008] 3. Li, H.; Zhang, X.; MacFarlane, DR, Carbon Quantum Dots / Cu2O Heterostructures for Solar-Light-Driven Conversion of CO2 to Methanol. Advanced Energy Materials 2015, 5(5).

[0009] 4.Bhethanabotla,V.C.;Russell,D.R.;Kuhn,J.N.,Assessment of mechanisms for enhanced performance of Yb / Er / titania photocatalysts for organic degradation:Role of rare earth elements in the titania phase.Applied Catalysis B:Environmental 2017,202,156-164.

[0010] 5.Gao,M.;Connor,P.K.N.;Ho,G.W.,Plasmonic photothermic directed broadband sunlight harnessing for seawater catalysis and desalination.Energy&Environmental Science 2016,9(10),3151-3160.

[0011] 6.Kuo,T.-R.;Liao,H.-J.;Chen,Y.-T.;Wei,C.-Y.;Chang,C.-C.;Chen,Y.-C.;Chang,Y.-H.;Lin,J.-C.;Lee,Y.-C.;Wen,C.-Y.;Li,S.-S.;Lin,K.-H.;Wang,D.-Y.,Extended visible to near-infrared harvesting of earth-abundant FeS2–TiO2 heterostructures for highly active photocatalytic hydrogen evolution.Green Chemistry 2018,20(7),1640-1647.

[0012] 7.Tian,J.;Hao,P.;Wei,N.;Cui,H.;Liu,H.,3D Bi2MoO6 Nanosheet / TiO2 Nanobelt Heterostructure:Enhanced Photocatalytic Activities and Photoelectochemistry Performance.ACS Catalysis 2015,5(8),4530-4536.

[0013] 8.Wang,M.;Han,Q.;Zhou,Y.;Li,P.;Tu,W.;Tang,L.;Zou,Z.,TiO2 nanosheet-anchoring Au nanoplates:high-energy facet and wide spectra surface plasmon-promoting photocatalytic efficiency and selectivity for CO2 reduction.RSC Advances 2016,6(85),81510-81516.

[0014] 9.Yu,J.;Yang,Y.;Fan,R.;Wang,P.;Dong,Y.,Enhanced photovoltaic performance of dye-sensitized solar cells using a new photoelectrode material:upconversion YbF3-Ho / TiO2 nanoheterostructures.Nanoscale 2016,8(7),4173-4180.

[0015] 10.Alberoni,C.; I.;Infantes-Molina,A.; E.;Talon,A.;Zhao,H.;You,S.;Vomiero,A.;Moretti,E.,Ceria doping boosts methylene blue photodegradation in titania nanostructures.Materials Chemistry Frontiers 2021,5(11),4138-4152.

[0016] 11.Belver,C.;Bedia,J.; M.A.;Rodriguez,J.J.,Solar photocatalytic purification of water with Ce-doped TiO2 / clay heterostructures.Catalysis Today 2016,266,36-45.

[0017] 12.Dong,Z.;Ding,D.;Li,T.;Ning,C.,Black Si-doped TiO2 nanotube photoanode for high-efficiency photoelectrochemical water splitting.RSC Adv 2018,8(11),5652-5660.

[0018] 13.Eadi,S.B.;Kim,S.;Jeong,S.W.;Jeon,H.W.,Novel Preparation of Fe Doped TiO2 Nanoparticles and Their Application for Gas Sensor and Photocatalytic Degradation.Advances in Materials Science and Engineering 2017,2017,1-6.

[0019] 14.Huang,W.;Cheng,H.;Feng,J.;Shi,Z.;Bai,D.;Li,L.,Synthesis of highly water-dispersible N-doped anatase titania based on low temperature solvent-thermal method.Arabian Journal of Chemistry 2018,11(6),871-879.

[0020] 15.Huang,Z.;Gao,Z.;Gao,S.;Wang,Q.;Wang,Z.;Huang,B.;Dai,Y.,Facile synthesis of S-doped reduced TiO2-x with enhanced visible-light photocatalytic performance.Chinese Journal of Catalysis 2017,38(5),821-830.

[0021] 16. S.;Matějová,L.; K.;Obalová,L.;Matěj,Z.; L.; O.,Preparation and characterization of Ag-doped crystalline titania for photocatalysis applications.Applied Catalysis B:Environmental 2012,111-112,119-125.

[0022] 17.Ren,R.;Wen,Z.;Cui,S.;Hou,Y.;Guo,X.;Chen,J.,Controllable Synthesis and Tunable Photocatalytic Properties of Ti(3+)-doped TiO2.Sci Rep 2015,5,10714.

[0023] 18.Sadia,M.;Naz,R.;Khan,J.;Zahoor,M.;Ullah,R.;Khan,R.;Naz,S.;Almoallim,H.S.;Alharbi,S.A.,Metal doped titania nanoparticles as efficient photocatalyst for dyes degradation.Journal of King Saud University-Science 2021,33(2).

[0024] 19.Shi,J.-W.;Chen,J.-W.;Cui,H.-J.;Fu,M.-L.;Luo,H.-Y.;Xu,B.;Ye,Z.-L.,One template approach to synthesize C-doped titania hollow spheres with high visible-light photocatalytic activity.Chemical Engineering Journal 2012,195-196,226-232.

[0025] 20.Vijayan,B.K.;Dimitrijevic,N.M.;Wu,J.;Gray,K.A.,The Effects of Pt Doping on the Structure and Visible Light Photoactivity of Titania Nanotubes.The Journal of Physical Chemistry C 2010,114(49),21262-21269.

[0026] 21.Wu,Q.;Huang,F.;Zhao,M.;Xu,J.;Zhou,J.;Wang,Y.,Ultra-small yellow defective TiO2nanoparticles for co-catalyst free photocatalytic hydrogen production.Nano Energy 2016,24,63-71.

[0027] 22.Xiong,Y.;He,D.;Jaber,R.;Cameron,P.J.;Edler,K.J.,Sulfur-Doped Cubic Mesostructured Titania Films for Use as a Solar Photocatalyst.The Journal of Physical Chemistry C 2017,121(18),9929-9937.

[0028] 23. Yao, L.; Wang, H.; Zhang, Y.; Wang, S.; Liu, X., Fabrication of N doped TiO2 / C nanocomposites with hierarchical porous structure and high photocatalytic activity. Microporous and Mesoporous Materials 2019,288.

[0029] Summary of the Invention

[0030] To address the problems in the prior art, the present invention provides a method for preparing phosphorus-doped titanium dioxide. The phosphorus-doped titanium dioxide prepared by the method provides a titanium dioxide nanomaterial with large specific surface area, high particle size uniformity, adjustable crystallinity, and controllable crystal phase, further enhancing the photocatalytic performance of titanium dioxide.

[0031] The method for preparing phosphorus-doped titanium dioxide comprises the following steps:

[0032] S1: Titanium dioxide was deposited on black phosphorus nanosheets using a sol-gel method to obtain a black phosphorus / titanium dioxide composite material.

[0033] S2: Depositing silicon dioxide on the black phosphorus / titanium dioxide composite material prepared in S1 to obtain a black phosphorus / titanium dioxide / silicon dioxide composite material.

[0034] S3: calcining and etching the black phosphorus / titanium dioxide / silicon dioxide composite material obtained in S2.

[0035] Furthermore, step S1 includes:

[0036] S11: Weigh the corresponding amount of black phosphorus nanosheet solution based on the amount of black phosphorus (C mg), wash it three times with anhydrous ethanol, disperse it in D mL of ethanol, add E mL of anhydrous acetonitrile, and add F mL of concentrated ammonia under stirring to obtain solution a;

[0037] S12: G mL of anhydrous ethanol, H mL of anhydrous acetonitrile, and 1 mL of tetrabutyl titanate (TBOT) were mixed to obtain solution b;

[0038] S13: Stir solution a at room temperature for 5-10 minutes, then quickly add solution b into it, stir for more than 4 hours, centrifuge, wash four times with anhydrous ethanol, and disperse in 30 ml of ethanol to obtain a black phosphorus / titanium dioxide composite material (i.e., BP@TiO2 sample).

[0039] Among them, C:D:E:F:G:H:I=(15~30):(20~30):(5~10):(0.1~0.5):(2~5):(0.5~2):(0.05~0.5).

[0040] Furthermore, step S2 includes:

[0041] To the black phosphorus / titania composite material obtained in step S1 (i.e., the BP@TiO2 sample), polyacrylic acid (PAA, 0.01 g / mL) was added, the mixture was stirred for more than 2 hours, centrifuged, washed with anhydrous ethanol, and dispersed in J mL of ethanol. K mL of water, L mL of concentrated aqueous ammonia, and M mL of tetraethyl orthosilicate (TEOS) were added, the mixture was stirred for more than 4 hours, centrifuged, washed with ethanol and water, and dried to obtain a black phosphorus / titania / silica composite material (i.e., the BP@TiO2@SiO2 sample), where J:K:L:M = (20-30):(2-5):(0.5-2):(0.5-2).

[0042] Specifically, the mass fraction of the ammonia solution is 25-28%, and the drying temperature is 60-70°C.

[0043] Furthermore, step S2 includes:

[0044] The black phosphorus / titanium dioxide / silicon dioxide composite material obtained in step S2 was calcined for 2 h under an argon atmosphere and then cooled to room temperature to obtain a calcined BP@TiO2@SiO2 sample;

[0045] Take N mg of calcined BP@TiO2@SiO2 sample and dissolve it in 0 mL P 2.5 mol / L sodium hydroxide solution, stir it at 50℃ for nearly 8 hours, centrifuge it, wash it with water to obtain phosphorus-doped titanium dioxide, dry it and set it aside.

[0046] Among them, N:O:P=(50~500):(20~50):(0.5~3).

[0047] Specifically, the calcination temperature is 600-800°C, and the drying temperature is 60-70°C.

[0048] Furthermore, the method for preparing phosphorus-doped titanium dioxide includes step S0 before step S1:

[0049] Black phosphorus nanosheets were prepared by electrochemical exfoliation: Ag g of tetrabutylammonium bromide (TBAB) was dissolved in B mL of N,N-dimethylformamide (DMF) as the electrolyte, black phosphorus crystals were used as the cathode, a platinum electrode was used as the counter electrode, and tetrabutylammonium bromide was used as the intercalant. After electrolysis for approximately 5 hours, the product was collected by centrifugation, washed four times with DMF, and then dispersed in DMF. The product was stored in a glove box until ready for use. The ratio of A:B was (2-4):(50-100).

[0050] An object of the present invention is to provide phosphorus-doped titanium dioxide, which is prepared according to any of the above methods for preparing doped titanium dioxide.

[0051] One object of the present invention is to provide a use of the phosphorus-doped titanium dioxide as described above in photocatalysis.

[0052] The present invention uses a sol-gel method to coat black phosphorus nanosheets with titanium dioxide layers and silicon dioxide, followed by protected calcination. During the calcination process, the two advantages of black phosphorus being doped into the titanium dioxide lattice and silicon dioxide effectively protecting the titanium dioxide grains from agglomeration and excessive growth are combined. This allows the preparation of phosphorus-doped titanium dioxide nanomaterials with characteristics such as large specific surface area, high particle size uniformity, adjustable crystallinity, and controllable crystal phase. Phosphorus-doped titanium dioxide nanomaterials have the characteristics of a narrow bandgap and a low recombination rate of photogenerated electrons and holes. The light absorption range is broadened to visible light and infrared light, further enhancing the photocatalytic performance of titanium dioxide and achieving the effect of maximizing the use of sunlight. BRIEF DESCRIPTION OF THE DRAWINGS

[0053] FIG1 is a scanning electron microscope (SEM) image of black-scale nanosheets provided in Example 3 of the present invention;

[0054] FIG2 is a scanning electron microscope (SEM) image of the black phosphorus / titanium dioxide composite material provided in Example 3 of the present invention;

[0055] FIG3 is an X-ray diffraction (XRD) pattern of phosphorus-doped titanium dioxide provided in Example 3 of the present invention;

[0056] FIG4 is a STEM-EDS scanning image of phosphorus-doped titanium dioxide provided in Example 3 of the present invention;

[0057] FIG5 is the UV-visible spectroscopic spectrum of rhodamine provided in Examples 2 and 3 of the present invention. DETAILED DESCRIPTION

[0058] In order to make the above-mentioned objects, features and advantages of the present invention more obvious and easy to understand, the specific embodiments of the present invention are described in detail below with reference to the accompanying drawings, but they should not be understood as limiting the scope of implementation of the present invention.

[0059] The present invention adopts a brand-new method to prepare phosphorus-doped titanium dioxide nanomaterials. Based on the characteristics of black phosphorus nanosheets such as large specific surface area, it is proposed to use black phosphorus (BP) nanosheets with a large specific surface area as a growth template for titanium dioxide, and deposit amorphous titanium dioxide and silicon dioxide layers thereon in succession by the sol-gel method. By utilizing the effective protection calcination of silicon dioxide, effective phosphorus doping of titanium dioxide is achieved, and the particle size, crystal phase, crystallinity and other properties of titanium dioxide are controlled to prepare a phosphorus-doped titanium dioxide photocatalyst with excellent performance. Through the combined effect of phosphorus doping and silicon dioxide protection calcination, the titanium dioxide nanomaterial prepared has the characteristics of large specific surface area, uniform particle size, controllable crystal phase, etc., has a smaller band gap width, a lower photogenerated electron-hole recombination rate, and realizes full utilization of visible light and near-infrared light, thereby maximizing the utilization of solar energy.

[0060] The method for preparing phosphorus-doped titanium dioxide comprises the following steps:

[0061] S1: Titanium dioxide was deposited on black phosphorus nanosheets using a sol-gel method to obtain a black phosphorus / titanium dioxide composite material.

[0062] S2: Depositing silicon dioxide on the black phosphorus / titanium dioxide composite material prepared in S1 to obtain a black phosphorus / titanium dioxide / silicon dioxide composite material.

[0063] S3: calcining and etching the black phosphorus / titanium dioxide / silicon dioxide composite material obtained in S2.

[0064] In one embodiment, black phosphorus nanosheets are prepared by the following steps:

[0065] S0: Preparation of black phosphorus nanosheets by electrochemical exfoliation: Ag g of tetrabutylammonium bromide (TBAB) was dissolved in B mL of N,N-dimethylformamide (DMF) as the electrolyte, black phosphorus crystals were used as the cathode, a platinum electrode was used as the counter electrode, and tetrabutylammonium bromide was used as the intercalation agent. After approximately 5 hours of electrolysis, the product was collected by centrifugation, washed four times with DMF, and then dispersed in DMF. The product was stored in a glove box until ready for use. Where A:B = (2-4): (50-100). The black phosphorus concentration was determined by spectrometry.

[0066] In one embodiment, step S1 includes:

[0067] S11: Prepare solution a: Weigh a corresponding amount of black phosphorus nanosheet solution based on the amount of C mg black phosphorus, wash it three times with anhydrous ethanol, disperse it in D mL ethanol, add E mL anhydrous acetonitrile, and add F mL ammonia water under stirring to obtain solution a.

[0068] S12: Prepare solution b: Mix 0 mL of anhydrous ethanol, 1 mL of anhydrous acetonitrile, and 1 mL of tetrabutyl titanate (TBOT) to obtain solution b.

[0069] S13: Stir solution a at room temperature for 5-10 minutes, then quickly add solution b thereto, stir for more than 4 hours, centrifuge, wash four times with anhydrous ethanol, and disperse in 30 ml of ethanol to obtain a black phosphorus / titanium dioxide composite material (i.e., BP@TiO2 sample).

[0070] Among them, C:D:E:F:G:H:I=(15~30):(20~30):(5~10):(0.1~0.5):(2~5):(0.5~2):(0.05~0.5).

[0071] In one embodiment, step S2 includes:

[0072] To the black phosphorus / titanium dioxide composite material obtained in step S1 (i.e., the BP@TiO2 sample), polyacrylic acid (PAA, 0.01 g / mL) was added, stirred for more than 2 hours, centrifuged, washed with anhydrous ethanol, and dispersed in J mL of ethanol. K mL of water, L mL of ammonia, and M mL of tetraethyl orthosilicate (TEOS) were added, stirred for more than 4 hours, centrifuged, washed with ethanol and water, and dried to obtain a black phosphorus / titanium dioxide / silicon dioxide composite material (i.e., the BP@TiO2@SiO2 sample). Wherein, J:K:L:M = (20-30):(2-5):(0.5-2):(0.5-2).

[0073] In one embodiment, step S3 includes:

[0074] The black phosphorus / titania / silicon dioxide composite material obtained in step S2 was heated to the desired temperature under an argon atmosphere and calcined for 2 hours. After cooling to room temperature, the calcined BP@TiO2@SiO2 sample was obtained. N mg of the calcined BP@TiO2@SiO2 sample was dissolved in 0 mL of a 2.5 mol / L sodium hydroxide solution, stirred at 50°C for approximately 8 hours, centrifuged, and washed with water to obtain the etched phosphorus-doped titanium dioxide (i.e., BP@TiO2 sample). The BP@TiO2 sample was dried and set aside, wherein the N:O:P ratio was (50-500):(20-50):(0.5-3).

[0075] In one embodiment, phosphorus-doped titanium dioxide and a preparation method thereof include the following steps:

[0076] S0: Preparation of black phosphorus nanosheets by electrochemical exfoliation: Ag g of tetrabutylammonium bromide (TBAB) was dissolved in B mL of N,N-dimethylformamide (DMF) as the electrolyte, black phosphorus crystals were used as the cathode, a platinum electrode was used as the counter electrode, and tetrabutylammonium bromide was used as the intercalation agent. After approximately 5 hours of electrolysis, the product was collected by centrifugation, washed four times with DMF, and then dispersed in DMF. The product was stored in a glove box until ready for use. Where A:B = (2-4): (50-100). The black phosphorus concentration was determined by spectrometry.

[0077] S1: Depositing titanium dioxide on black phosphorus nanosheets using a sol-gel method to obtain a black phosphorus / titanium dioxide composite material. Specifically, the process comprises the following steps:

[0078] S11: Prepare solution a: Weigh a corresponding amount of black phosphorus nanosheet solution based on the amount of C mg black phosphorus, wash it three times with anhydrous ethanol, disperse it in D mL ethanol, add E mL anhydrous acetonitrile, and add F mL concentrated ammonia under stirring to obtain solution a.

[0079] S12: Prepare solution b: mix G mL of anhydrous ethanol, H mL of anhydrous acetonitrile, and 1 mL of tetrabutyl titanate (TBOT) to obtain solution b.

[0080] S13: Stir solution a at room temperature for 5-10 minutes, then quickly add solution b thereto, stir for more than 4 hours, centrifuge, wash four times with anhydrous ethanol, and disperse in 30 ml of ethanol to obtain a black phosphorus / titanium dioxide composite material (i.e., BP@TiO2 sample).

[0081] Among them, C:D:E:F:G:H:I=(15~30):(20~30):(5~10):(0.1~0.5):(2~5):(0.5~2):(0.05~0.5).

[0082] S2: Depositing silicon dioxide on the black phosphorus / titanium dioxide composite material prepared in S1 to obtain a black phosphorus / titanium dioxide / silicon dioxide composite material. Specifically, the process comprises the following steps:

[0083] To the black phosphorus / titanium dioxide composite material obtained in step S1 (i.e., the BP@TiO2 sample), polyacrylic acid (PAA, 0.01 g / mL) was added, stirred for more than 2 hours, centrifuged, washed with anhydrous ethanol, and dispersed in J mL of ethanol. K mL of water, L mL of concentrated ammonia, and M mL of tetraethyl orthosilicate (TEOS) were added, stirred for more than 4 hours, centrifuged, washed with ethanol and water, and dried to obtain the black phosphorus / titanium dioxide / silicon dioxide composite material (i.e., the BP@TiO2@SiO2 sample). Wherein, J:K:L:M = (20-30):(2-5):(0.5-2):(0.5-2).

[0084] Optionally, the mass fraction of the ammonia solution is 25-28%, and the drying temperature is 60-70°C.

[0085] S3: calcining and etching the black phosphorus / titanium dioxide / silicon dioxide composite material obtained in S2. Specifically, the process comprises the following steps:

[0086] The black phosphorus / titania / silicon dioxide composite material obtained in step S2 was heated to the desired temperature under an argon atmosphere and calcined for 2 hours. After cooling to room temperature, the calcined BP@TiO2@SiO2 sample was obtained. N mg of the calcined BP@TiO2@SiO2 sample was dissolved in 0 mL of a 2.5 mol / L sodium hydroxide solution, stirred at 50°C for approximately 8 hours, centrifuged, and washed with water to obtain etched phosphorus-doped titanium dioxide (i.e., the BP@TiO2 sample). The sample was then dried and set aside, wherein the N:O:P ratio was (50-500):(20-50):(0.5-3).

[0087] Optionally, the calcination temperature is 600-800°C and the drying temperature is 60-70°C.

[0088] The present invention provides Examples 1-3, all of which are prepared according to the above-mentioned phosphorus-doped titanium dioxide preparation method, except that the amounts of the reagents used are different. For details, refer to the following table:

[0089] The black scale nanosheets prepared in Examples 1-3 were subjected to electron microscope scanning tests; the black phosphorus / titanium dioxide composite material prepared in Example 3 was subjected to electron microscope scanning tests; the phosphorus-doped titanium dioxide prepared in Examples 1-3 was subjected to X-ray diffraction tests; and the phosphorus-doped titanium dioxide prepared in Example 3 was subjected to STEM-EDS scanning tests.

[0090] The scanning electron microscope (SEM) image of the black scale nanosheets prepared in Example 3 is shown in Figure 1. The scanning electron microscope (SEM) image of the black scale nanosheets prepared in Example 1-2 is similar to Figure 1. It can be seen from Figure 1 that the black phosphorus nanosheets are successfully peeled off from the bulk black phosphorus crystals, have good dispersibility, and most of them are single-layer nanosheets.

[0091] A scanning electron microscope (SEM) image of the black phosphorus / titanium dioxide composite material prepared in Example 3 is shown in FIG2 . By comparison with FIG1 , it can be seen that titanium dioxide is successfully coated on the surface of the black phosphorus nanosheets to form a black phosphorus / titanium dioxide composite material.

[0092] The X-ray diffraction (XRD) pattern of the phosphorus-doped titanium dioxide prepared in Example 3 is shown in Figure 3. The X-ray diffraction (XRD) pattern of the phosphorus-doped titanium dioxide prepared in Examples 1-2 is similar to Figure 3. It can be seen from Figure 3 that the prepared phosphorus-doped titanium dioxide is anatase phase, and as the amount of precursor TBOT increases, the prepared phosphorus-doped titanium dioxide has a better crystal structure.

[0093] The STEM-EDS scanning image of phosphorus-doped titanium dioxide prepared in Example 3 is shown in FIG4 , in which Ti, O, Na, Si, and P elements are observed, indicating that the P element is successfully doped into titanium dioxide.

[0094] The present invention also provides a use of the phosphorus-doped titanium dioxide in photocatalysis.

[0095] The catalytic performance of the phosphorus-doped titanium dioxide prepared in Examples 1-3 was evaluated by the degradation rate of rhodamine B.

[0096] Evaluation Method: The photocatalytic activity was evaluated by tracking the degradation of rhodamine B (RhB) over time. The phosphorus-doped titanium dioxide catalyst was dispersed in a 20 mL, 1×10-5 M aqueous solution of rhodamine B (RhB) and stirred in the dark for 30 minutes to ensure adsorption of the RhB dye on the phosphorus-doped titanium dioxide catalyst surface. A 300W xenon lamp was used as the excitation source, and the RhB concentration was determined using a UV-visible spectrophotometer. The intensity of the 553 nm absorption peak was used to track the RhB concentration in the reaction medium as a function of time to obtain the catalytic performance data reported in Figure 5. Figure 5 (left) shows the catalytic efficiency of the phosphorus-doped titanium dioxide prepared in Example 2, achieving a 94% degradation efficiency for rhodamine after 90 minutes of illumination. Figure 5 (right) shows the degradation efficiency of the phosphorus-doped titanium dioxide prepared in Example 3, achieving approximately 90% degradation of rhodamine after 30 minutes of illumination. The phosphorus-doped titanium dioxide prepared in Example 1 also exhibited high rhodamine degradation efficiency.

[0097] The present invention uses a sol-gel method to coat black phosphorus nanosheets with titanium dioxide layers and silicon dioxide, followed by protected calcination. During the calcination process, the black phosphorus is doped into the titanium dioxide lattice, while silicon dioxide effectively protects the titanium dioxide grains from agglomeration and excessive growth. Titanium dioxide nanomaterials with large specific surface area, uniform particle size, adjustable crystallinity, and controllable crystal phase can be prepared. Phosphorus-doped titanium dioxide nanomaterials have the characteristics of a narrow band gap and a low recombination rate of photogenerated electrons and holes. The light absorption range is broadened to visible light and infrared light, further enhancing the photocatalytic performance of titanium dioxide and achieving the effect of maximizing the use of sunlight.

Claims

1. A method for preparing phosphorus-doped titanium dioxide, characterized in that: The following steps are involved: S1: Titanium dioxide is deposited on black phosphorus nanosheets by a sol-gel method to obtain a black phosphorus / titanium dioxide composite material; S2: depositing silicon dioxide on the black phosphorus / titanium dioxide composite material prepared in S1 to obtain a black phosphorus / titanium dioxide / silicon dioxide composite material; S3: calcining and etching the black phosphorus / titanium dioxide / silicon dioxide composite material obtained in S2.

2. The method for preparing phosphorus-doped titanium dioxide according to claim 1, characterized in that: The S1 step includes: S11: According to the amount of C mg of black phosphorus, a corresponding amount of black phosphorus nanosheet solution is weighed, washed three times with anhydrous ethanol, dispersed in D mL of ethanol, added with E mL of anhydrous acetonitrile, and under stirring, added with F mL of concentrated ammonia to obtain solution a; S12: G mL of anhydrous ethanol, H mL of anhydrous acetonitrile and 1 mL of tetrabutyl titanate (TBOT) were mixed to obtain solution b; S13: Stir solution a at room temperature for 5-10 minutes, then quickly add solution b thereto, stir for more than 4 hours, centrifuge, wash four times with anhydrous ethanol, and disperse in 30 ml of ethanol to obtain the black phosphorus / titanium dioxide composite material. Among them, C:D:E:F:G:H:I=(15~30):(20~30):(5~10):(0.1~0.5):(2~5):(0.5~2):(0.05~0.5).

3. The method for preparing phosphorus-doped titanium dioxide according to claim 1, characterized in that: The S2 step includes: Add polyacrylic acid to the black phosphorus / titanium dioxide composite material obtained in step S1, stir for more than 2 hours, centrifuge and wash with anhydrous ethanol, disperse in J mL of ethanol, add K mL of water, L mL of ammonia water and M mL of tetraethyl orthosilicate, stir for more than 4 hours, centrifuge, wash with ethanol and water, and dry to obtain the black phosphorus / titanium dioxide / silicon dioxide composite material, wherein J:K:L:M=(20-30):(2-5):(0.5-2):(0.5-2).

4. The method for preparing phosphorus-doped titanium dioxide according to claim 3, characterized in that: The mass fraction of the ammonia solution is 25-28%, and the drying temperature is 60-70°C.

5. The method for preparing phosphorus-doped titanium dioxide according to claim 1, characterized in that: The S2 step includes: The black phosphorus / titanium dioxide / silicon dioxide composite material obtained in step S2 is heated up and calcined for 2 hours in an argon atmosphere, and then cooled to room temperature to obtain a calcined BP@TiO2@SiO2 sample; Take N mg of the calcined BP@TiO2@SiO2 sample and dissolve it in O mL P 2.5 mol / L sodium hydroxide solution, stir it at 50°C for nearly 8 hours, centrifuge it, wash it with water, and obtain the phosphorus-doped titanium dioxide, dry it, and set it aside. Among them, N:O:P=(50~500):(20~50):(0.5~3).

6. The method for preparing phosphorus-doped titanium dioxide according to claim 5, characterized in that: The calcination temperature is 600-800°C, and the drying temperature is 60-70°C.

7. The method for preparing phosphorus-doped titanium dioxide according to claim 1, characterized in that: Including the S0 step before the S1 step: Ag tetrabutylammonium bromide (TBAB) was dissolved in B mL N,N-dimethylformamide (DMF) as an electrolyte, black phosphorus crystal was used as a cathode, a platinum sheet electrode was used as a counter electrode, and tetrabutylammonium bromide was used as an intercalant. After electrolysis for about 5 hours, the product was collected by centrifugation, washed four times with DMF, dispersed in DMF, and stored in a glove box for later use, wherein A:B = (2-4): (50-100).

8. A phosphorus-doped titanium dioxide, characterized in that: The method for preparing doped titanium dioxide is described in any one of claims 1 to 7.

9. Use of the phosphorus-doped titanium dioxide as claimed in claim 8 in photocatalysis.

Citation Information

Patent Citations

  • Phosphor doping type nano titanium dioxide having efficient sunlight catalytic capability and preparation method thereof

    CN101690896A

  • Aqueous acrylic resin which can degrade formaldehyde by using visible light and preparation method of aqueous acrylic resin

    CN109851706A

  • Black phosphorus quantum dots, titanium dioxide / black phosphorus quantum dot composite material, production methods of black phosphorus quantum dots and titanium dioxide / black phosphorus quantum dot composite material and application of titanium dioxide / black phosphorus quantum dot composite material

    CN110229667A

  • Trititanium dicarbide / titanium dioxide / black phosphorus nanosheet composite photocatalyst, and preparation method and application thereof

    CN111185210A

  • BPQDs / TiO2 binary heterostructure composite photocatalytic material as well as preparation method and application thereof

    CN115155626A

Cited By

  • Defect catalyst and preparation method and application thereof

    CN119281322A

  • Preparation of carbon-doped TiO2 / bismuth sulfide composite material and application of carbon-doped TiO2 / bismuth sulfide composite material in electrochemical corrosion prevention

    CN119932569A

  • Preparation method of hollow carbon spheres embedded with titanium dioxide, electrode catalytic material and application of electrode catalytic material

    CN120356957A

  • Preparation method of hollow carbon sphere embedded with titanium dioxide, electrode catalytic material and application thereof

    CN120356957B