Medium-strength and high-conductivity aluminum alloy monofilament production process and aluminum alloy monofilament produced thereby

Through solution quenching and aging treatment technology, the problem of balancing strength and conductivity of aluminum alloy wires has been solved, and the production of aluminum alloy monofilaments with high conductivity and high strength has been achieved, meeting the needs of improving energy efficiency and reducing carbon emissions. need.

WO2024198562A1PCT designated stage expired Publication Date: 2024-10-03JIANGSU ZHONGTIAN TECH CO LTD

Patent Information

Application Number
PCT/CN2023/141425
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-28
Filing Date
2023-12-25
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

It is difficult to balance the improvement of strength and conductivity of existing aluminum alloy wires, resulting in insufficient breaking force of the wires and unable to meet the needs of carbon emission reduction and energy efficiency improvement.

Method used

The production process of medium-strength and high-conductivity aluminum alloy monofilaments is adopted, and Mg and Si elements are completely redissolved through solid solution quenching treatment. Combined with pre-aging and artificial aging treatment, stress is used to drive the diffusion and precipitation of alloy atoms to promote the formation of strengthening phases. Improve the strength and conductivity of aluminum alloy monofilaments.

Benefits of technology

While maintaining high conductivity, the strength and elongation of aluminum alloy monofilaments are significantly improved, reaching a strength of more than 270MPa, a conductivity of more than 59% IACS, and an elongation of more than 5%, improving the strength of aluminum alloy monofilaments. Overall performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 000001
    Figure 000001
  • Figure 000002
    Figure 000002
  • Figure 000003
    Figure 000003
Patent Text Reader

Abstract

A medium-strength and high-conductivity aluminum alloy monofilament production process. The production process comprises: providing an aluminum alloy rod; carrying out drawing treatment on the aluminum alloy rod to obtain an alloy monofilament, and carrying out pre-aging treatment on the alloy monofilament at 100-150°C during the drawing treatment; and carrying out artificial aging treatment on the alloy monofilament to obtain a medium-strength and high-conductivity aluminum alloy monofilament. Also provided is a medium-strength and high-conductivity aluminum alloy monofilament. The aluminum alloy monofilament has strength greater than or equal to 270 MPa, conductivity greater than or equal to 59% IACS and elongation greater than or equal to 5%. The aluminum alloy monofilament has good tensile strength while having high conductivity.
Need to check novelty before this filing date? Find Prior Art

Description

A medium-strength and high-conductivity aluminum alloy monofilament production process and aluminum alloy monofilament Technical Field

[0001] The present invention relates to the technical field of aluminum alloy materials, and in particular to a production process of medium-strength and high-conductivity aluminum alloy monofilaments and the aluminum alloy monofilaments. Background Art

[0002] Overhead transmission lines are the energy arteries of national economic development. my country's overhead transmission lines are primarily composed of conventional steel-core aluminum stranded wire, resulting in significant energy losses. my country has recently proposed a timetable for achieving carbon peak and carbon neutrality. Using energy-efficient conductors instead of steel-core aluminum stranded wires significantly reduces energy losses in transmission lines, becoming a key development trend in the overhead transmission sector. Currently, domestically produced high-conductivity aluminum alloys with a conductivity of 58.5% IACS have a strength of only 230-250 MPa, resulting in insufficient breaking force. The strength and conductivity of aluminum-magnesium-silicon alloys are known to be mutually exclusive. Increasing strength often results in a significant decrease in conductivity, making it difficult to achieve significant improvements in overall performance using conventional processes. Therefore, there is an urgent need to develop a new aluminum alloy monofilament production process that can improve both strength and elongation while maintaining high conductivity.

[0003] Summary of the Invention

[0004] The purpose of this application is to provide a production process for medium-strength and high-conductivity aluminum alloy monofilaments, which can improve the strength and elongation of the aluminum alloy monofilaments while making the conductivity of the aluminum alloy monofilaments higher.

[0005] Another object of the present application is to provide an aluminum alloy monofilament having a strength of ≥270 MPa, a conductivity of ≥59% IACS, and an elongation of ≥5%.

[0006] In a first aspect, the present application provides a process for producing medium-strength and high-conductivity aluminum alloy monofilaments, comprising:

[0007] Aluminum alloy rods are available;

[0008] Drawing the aluminum alloy rod to obtain alloy monofilaments, and performing a pre-aging treatment at 100-150° C. on the alloy monofilaments during drawing;

[0009] The alloy monofilament is artificially aged to obtain a medium-strength and high-conductivity aluminum alloy monofilament; wherein the temperature of the pre-aging treatment is lower than the temperature of the artificial aging treatment.

[0010] Furthermore, in some embodiments of the present application, the pre-aging treatment includes:

[0011] During the drawing process, the last drawing die and / or the wire storage area are heated to perform a pre-aging treatment of the alloy single wire at 100-150°C.

[0012] Furthermore, in some embodiments of the present application, artificial aging treatment includes:

[0013] The alloy monofilament is aged at 140-160°C for 5-10 hours.

[0014] Further, in some embodiments of the present application, providing the aluminum alloy rod includes: performing a solution treatment on the aluminum alloy rod;

[0015] Solution treatment includes:

[0016] The aluminum alloy rod is cast and rolled to obtain the aluminum alloy rod by heat preservation treatment at 480-530°C for 1-3 hours, quenched and cooled to 50-120°C.

[0017] Furthermore, in some embodiments of the present application, the preparation of the aluminum alloy rod obtained by casting and rolling includes the following steps:

[0018] S11. Alloy smelting: providing raw materials according to the elemental composition of the aluminum alloy rod, melting and obtaining a melt;

[0019] S12, furnace refining: boronizing the melt, refining the melt at 740-750°C, skimming the slag, and allowing it to stand;

[0020] S13, online refining: after the casting starts, the melt is degassed and filtered online to obtain refined aluminum liquid;

[0021] S14, grain refinement: adding 0.05-0.15% by mass of a refiner to the refined aluminum liquid;

[0022] S15. Continuous casting and rolling: The aluminum melt after online refining is cast and rolled using the continuous casting and rolling process to obtain an aluminum alloy rod.

[0023] Furthermore, in some embodiments of the present application, in S12, the refining time is 10 to 15 minutes; and / or

[0024] The standing time is 30 to 40 minutes; and / or

[0025] The standing temperature is 720-730°C.

[0026] Furthermore, in some embodiments of the present application, the continuous casting and rolling includes: continuously casting the online refined melt using a wheel crystallizer at 700-720°C to obtain a cast billet; and rolling the cast billet using a continuous rolling mill at 490-510°C to obtain an aluminum alloy rod.

[0027] Furthermore, in some embodiments of the present application, online refining includes:

[0028] Nitrogen was used for online rotary blowing and degassing at a speed of 400-500 r / min, and online filtration was performed using a filter plate with a porosity of 30 / 50 PPI.

[0029] Furthermore, in some embodiments of the present application, the elemental composition of the aluminum alloy rod includes, by mass fraction, Mg 0.3-0.45%, Si 0.3-0.5%, Fe 0.1-0.15%, Y 0.1-0.3%, La 0.01-0.05%, B 0.001-0.05%, and the rest is Al and other inevitable impurity elements; the total amount of inevitable impurity elements is ≤0.02%.

[0030] In a second aspect, the present application further provides a medium-strength and high-conductivity aluminum alloy monofilament, wherein the element composition of the aluminum alloy monofilament includes, by mass fraction, Mg 0.3-0.45%, Si 0.3-0.5%, Fe 0.1-0.15%, Y 0.1-0.3%, La 0.01-0.05%, B 0.001-0.05%, and the remainder is Al and other inevitable impurity elements; the total amount of inevitable impurity elements is ≤0.02%;

[0031] Furthermore, in some embodiments of the present application, the aluminum alloy monofilament has a strength of ≥270 MPa, a conductivity of ≥59% IACS, and an elongation of ≥5%.

[0032] The existing method for producing medium-strength aluminum alloy wire drawing generally involves smelting aluminum to obtain a molten aluminum, then continuously casting and rolling the aluminum alloy rod, and finally drawing the aluminum alloy rod and then subjecting it to an aging treatment to strengthen the drawn aluminum alloy monofilament and improve its strength. During the continuous casting and rolling process, especially during the process of rolling the aluminum alloy rod from the ingot, the temperature drops significantly, preventing the alloying elements from fully dissolving back. This results in the alloying elements not fully exerting their dispersion precipitation strengthening effect during the subsequent aging treatment, limiting further improvements in alloy properties. Consequently, when the conductivity of the resulting aluminum alloy monofilament reaches 58.5%, its strength and elongation are difficult to further increase, resulting in insufficient breaking force. Furthermore, even if the strength and elongation are slightly increased through high-temperature aging, the conductivity of the aluminum alloy monofilament is difficult to further increase above 58.5%.

[0033] The beneficial effects of this application are:

[0034] The production process of aluminum alloy monofilaments provided in the present application performs a solution quenching treatment on the aluminum alloy rod so that the precipitated Mg and Si elements are completely dissolved back into the aluminum matrix to reach a supersaturated state, thereby providing conditions for maximizing their dispersion strengthening effect during subsequent aging strengthening; a pre-aging treatment is performed during the aluminum alloy monofilament drawing process, and the stress applied to the aluminum alloy rod during drawing provides a driving force for the rapid diffusion and precipitation of alloy atoms, thereby preparing for the precipitation of the second phase in the aluminum alloy monofilament and promoting the rapid and effective precipitation of the strengthening phase in the aluminum alloy monofilament during the artificial aging treatment stage; and the artificial aging treatment is performed after the drawing process, so that the dissolved Mg and Si elements in the aluminum alloy monofilament can be more fully precipitated as a metastable strengthening phase, thereby optimizing the strength and conductivity of the monofilament, thereby improving the strength, conductivity and elongation of the obtained aluminum alloy monofilament, and making the aluminum alloy monofilament have good breaking strength while having high conductivity.

[0035] The present application also provides a medium-strength and high-conductivity aluminum alloy monofilament, wherein the aluminum alloy monofilament has a strength of ≥270 MPa, a conductivity of ≥59% IACS, and an elongation of ≥5%. DETAILED DESCRIPTION

[0036] The following will clearly and completely describe the technical solutions of this application in conjunction with the embodiments. Obviously, the embodiments described are only part of the embodiments of this application, not all of them. Based on the embodiments in this application, all other embodiments obtained by ordinary technicians in this field without making creative efforts are within the scope of protection of this application.

[0037] The technical solutions of the present invention are described clearly and completely below with reference to the embodiments. It is obvious that the embodiments described are only a portion of the embodiments of the present invention, not all of them. All other embodiments derived by persons of ordinary skill in the art based on the embodiments of the present invention without creative effort are also within the scope of protection of the present invention.

[0038] In the description of this application, it should be understood that “multiple” means two or more than two, unless otherwise clearly and specifically defined.

[0039] The disclosure below provides many different embodiments or examples for realizing the different structures of the present application. In order to simplify the disclosure of the present application, the components and settings of specific examples are described below. Of course, they are merely examples, and the purpose is not to limit the present application. In addition, the present application may repeat reference numbers and / or reference letters in different examples, and this repetition is for the purpose of simplicity and clarity, and does not itself indicate the relationship between the various embodiments and / or settings discussed. In addition, the examples of various specific materials provided in the present application, but those of ordinary skill in the art will appreciate the application of other processes and / or the use of other materials.

[0040] The present application provides a process for producing medium-strength and high-conductivity aluminum alloy monofilaments, comprising:

[0041] Aluminum alloy rods are available;

[0042] Drawing the aluminum alloy rod to obtain alloy monofilaments, and performing a pre-aging treatment at 100-150° C. on the alloy monofilaments during the drawing process;

[0043] The alloy monofilament is artificially aged to obtain a medium-strength and high-conductivity aluminum alloy monofilament.

[0044] In some embodiments, the elemental composition of the aluminum alloy rod includes, by mass fraction: Mg (magnesium) 0.3-0.45%, Si (silicon) 0.3-0.5%, Fe (iron) 0.1-0.15%, Y (yttrium) 0.1-0.3%, La (lanthanum) 0.01-0.05%, B (boron) 0.001-0.05%, and the rest is Al (aluminum) and other inevitable impurity elements; the total amount of inevitable impurity elements is ≤0.02%.

[0045] It should be noted that the "pre-aging treatment of the alloy single wire at 100-150°C during drawing" mentioned in the present application should be understood as: during the drawing process, the drawn alloy single wire is subjected to aging treatment at a temperature of 100-150°C.

[0046] In some embodiments, the content of each of the unavoidable impurity elements is ≤0.005%.

[0047] It should be noted that the unavoidable impurity elements are impurity elements that are unavoidably present in the raw materials used in preparing the aluminum alloy rod and / or elements that are unavoidably introduced into the aluminum alloy rod during the preparation process of the aluminum alloy rod, such as hydrogen, oxygen, nitrogen, manganese, and zinc.

[0048] In some embodiments, the pre-aging treatment includes:

[0049] During the drawing process, the alloy single wire is subjected to a pre-aging treatment at 100-150° C. in the last drawing die and / or wire storage area.

[0050] In some embodiments, artificial aging includes:

[0051] The alloy monofilament is aged at 140-160°C for 5-10 hours.

[0052] The present application performs a pre-aging treatment during the drawing process of the aluminum alloy single wire, and uses the stress applied during the drawing of the rod to provide a driving force for the rapid diffusion and precipitation of atoms. The pre-aging treatment prepares for the precipitation of the second phase, promotes the rapid and effective precipitation of the second phase in the artificial aging stage, and achieves the optimization of the single wire strength and conductivity. It should be noted that the temperature of the pre-aging treatment needs to be lower than the temperature of the artificial aging treatment, and the pre-aging temperature is not higher than 150°C. During the alloy preparation process, as the temperature increases, the Mg and Si elements in the alloy will gradually generate GP zones, β'', and β' phases from the dissolved groups. Among them, the GP zone is usually precipitated and formed at low temperature, which can maintain a coherent relationship with Al, and as the temperature gradually increases, its crystal phase gradually transforms into β' phase. Therefore, in the present application, a lower pre-aging temperature is used in the pre-aging stage to allow Mg and Si elements to first precipitate out of the GP zone as crystal nuclei, and then a higher treatment temperature is used in the artificial aging stage to allow Mg and Si elements to grow β'' and β' phase alloys with the GP zone as the core, thereby improving the strength, conductivity and elongation of the aluminum alloy single wire.

[0053] In this application, pre-aging and artificial aging are not two separate aging treatments. Pre-aging serves as a pretreatment for artificial aging, promoting the rapid precipitation of crystalline phases during artificial aging and improving the alloy's electrical conductivity. Furthermore, during the pre-aging process, the pre-aging and drawing processes need to be performed simultaneously. The stress generated during the drawing process provides a driving force for the rapid diffusion and precipitation of alloy atoms, allowing them to uniformly form several GP phases, which serve as crystal nuclei, during the pre-aging process, preparing for the precipitation of crystalline phases during artificial aging.

[0054] In some embodiments, providing the aluminum alloy rod includes: solution treating the aluminum alloy rod;

[0055] Solution treatment includes:

[0056] The aluminum alloy rod is cast and rolled to obtain the aluminum alloy rod by heat preservation treatment at 480-530°C for 1-3 hours, quenched and cooled to 50-120°C.

[0057] Since the temperature of the aluminum alloy drops significantly during the continuous casting and rolling process, a large amount of alloying elements have been precipitated from the matrix, which is not conducive to the subsequent aging strengthening of the aluminum alloy single wire. Therefore, after the aluminum alloy rod is cast and rolled, it is subjected to solid solution quenching treatment to completely dissolve the precipitated Mg and Si elements back into the aluminum matrix to reach a supersaturated state, providing the best conditions for aging strengthening and maximizing the dispersion strengthening effect of the Mg and Si alloying elements.

[0058] In some embodiments, the preparation of the aluminum alloy rod obtained by casting and rolling comprises the following steps:

[0059] S11. Alloy smelting: providing raw materials according to the elemental composition of the aluminum alloy rod, melting and obtaining a melt;

[0060] S12, furnace refining: boronizing the melt, refining the melt at 740-750°C, skimming the slag, and allowing it to stand;

[0061] S13, online refining: after the casting starts, the melt is degassed and filtered online to obtain refined aluminum liquid;

[0062] S14, grain refinement: adding 0.05-0.15% by mass of a refiner to the refined aluminum liquid;

[0063] S15. Continuous casting and rolling: The aluminum melt after online refining is cast and rolled using the continuous casting and rolling process to obtain an aluminum alloy rod.

[0064] In some embodiments, during the alloy smelting process, raw materials providing aluminum, silicon, yttrium, iron, lanthanum, and boron are first put into a smelting furnace to melt, and then raw materials providing magnesium are added to melt and mix.

[0065] In some embodiments, during the alloy smelting process, the melt is sampled and analyzed, and the component ratio of the melt is adjusted according to the analysis results so that the component ratio of the obtained aluminum alloy rod can meet the requirements.

[0066] In some embodiments, one of the raw materials for providing aluminum is an aluminum ingot with a purity of not less than 99.7%.The rare earth elements are provided by a master alloy.

[0067] In some embodiments, in S12, the refining time is 10 to 15 minutes; and / or

[0068] The standing time is 30 to 40 minutes; and / or

[0069] The standing temperature is 720-730°C.

[0070] In some embodiments, step S12 is performed in a tilting holding furnace, which specifically includes:

[0071] The melt is transferred to a tilting holding furnace, and the raw materials providing boron are added for boronization treatment. The melt is stirred and the melt temperature is adjusted to 740-750°C for furnace refining for 10-15 minutes. The surface slag is then completely scraped off, and the temperature is adjusted to 720-730°C for static treatment for 30-40 minutes.

[0072] In some embodiments, the refiner is an aluminum titanium boron rod, which is used to refine the grains in the refined aluminum liquid to refine the grains.

[0073] In some embodiments, the refiner is added online while the refined aluminum liquid flows through the launder.

[0074] In some embodiments, the continuous casting and rolling comprises: continuously casting the online refined melt at 700-720° C. using a wheel crystallizer to obtain a cast billet; and rolling the cast billet at 490-510° C. using a continuous rolling mill to obtain an aluminum alloy rod.

[0075] In some embodiments, online refining includes:

[0076] Nitrogen is used for online rotary blowing and degassing at a speed of 400 to 500 r / min, and online filtration is performed using a filter plate with a porosity of 30 / 50 PPI.

[0077] The present application also provides a medium-strength and high-conductivity aluminum alloy monofilament, wherein the element composition of the aluminum alloy monofilament includes, by mass fraction, Mg 0.3-0.45%, Si 0.3-0.5%, Fe 0.1-0.15%, Y 0.1-0.3%, La 0.01-0.05%, B 0.001-0.05%, and the remainder is Al and other inevitable impurity elements; the total amount of inevitable impurity elements is ≤0.02%;

[0078] The strength of the aluminum alloy monofilament is ≥270MPa, the conductivity is ≥59%IACS, and the elongation is ≥5%.

[0079] In this application, Y is added to the aluminum alloy monofilament. The rare earth Y can form a FeYSiAl phase with the impurity Fe element, reducing the solid solubility of the impurity element in aluminum and improving the electrical conductivity of the alloy. It can also form an Al3Y phase with the matrix Al, improving the mechanical properties of the alloy.

[0080] In order to enable those skilled in the art to clearly understand the above-mentioned implementation details and operations of the present application, and to significantly demonstrate the advanced performance of a medium-strength and high-conductivity aluminum alloy monofilament production process and preparation method provided in the embodiments of the present application, the above-mentioned technical solution is illustrated by multiple embodiments below.

[0081] Example 1

[0082] S11: Add aluminum ingots, aluminum-silicon alloys, and aluminum-rare earth alloys with a purity greater than 99.7% to the melting furnace and heat to melt. Add a certain amount of magnesium ingots to the aluminum melt and stir to melt. Stir the aluminum melt thoroughly and take samples for spectral analysis to ensure that the melt composition is within the required range.

[0083] S12: The aluminum liquid is transferred to a tilting holding furnace, where a trace amount of aluminum-boron alloy is added for boronization. The electromagnetic stirring device at the bottom of the furnace is activated to fully stir the melt. The melt temperature is adjusted to 740°C for refining for 10 minutes. The surface scum is then scraped off, and the temperature is adjusted to 720°C for 40 minutes.

[0084] S13: After casting begins, the melt is degassed and filtered online. A rotary jet degassing box is used for online degassing, using high-purity nitrogen as the degassing medium. Online filtration utilizes a two-stage ceramic foam filter plate with a porosity of 30 / 50 PPI.

[0085] S14: When the aluminum liquid flows through the flow channel, aluminum titanium boron refiner is added online for grain refinement, and the addition amount is 0.1%.

[0086] S15: Continuous casting is carried out using a wheel-type crystallizer. The ingot rolling process is carried out in a 15-stand three-roll rolling mill with a rolling temperature of 500°C. After rolling, an aluminum alloy rod with a diameter of 9.5 mm is obtained, which is then collected after online cooling.

[0087] S16: performing a solution treatment on the alloy rod, with a solution heating temperature of 500°C and a holding time of 2 hours, and then quenching and cooling the rod material to rapidly cool it to below 70°C.

[0088] S17: The rod is drawn on a sliding wire drawing machine. During the drawing, the monofilament is pre-aged at a pre-aging temperature of 130° C., and a monofilament with a diameter of 3.5 mm is obtained after drawing.

[0089] S18: performing aging treatment on the drawn alloy single wire to obtain an aluminum alloy single wire, wherein the aging process is 150° C. / 9 h.

[0090] Analysis and testing revealed the alloy composition of this embodiment to be: Mg 0.38%, Si 0.42%, Fe 0.14%, Y 0.2%, La 0.03%, and B 0.004%. The content of unavoidable impurities was ≤0.005% for each element and ≤0.02% for the total. The resulting single-filament had a strength of 288 MPa and a conductivity of 59.3% IACS.

[0091] Example 2

[0092] S11: Add aluminum ingots, aluminum-silicon alloys, and aluminum-rare earth alloys with a purity greater than 99.7% to the melting furnace and heat to melt. Add a certain amount of magnesium ingots to the aluminum melt and stir to melt. Stir the aluminum melt thoroughly and take samples for spectral analysis to ensure that the melt composition is within the required range.

[0093] S12: The aluminum liquid is transferred to a tilting holding furnace. A trace amount of aluminum-boron alloy is added for boronization. The electromagnetic stirring device at the bottom of the furnace is activated to fully stir the melt. The melt temperature is adjusted to 745°C for refining for 10 minutes. The surface scum is then scraped off and the temperature is adjusted to 720°C for 40 minutes.

[0094] S13: After casting begins, the melt is degassed and filtered online. A rotary jet degassing box is used for online degassing, using high-purity nitrogen as the degassing medium. Online filtration utilizes a two-stage ceramic foam filter plate with a porosity of 30 / 50 PPI.

[0095] S14: When the aluminum liquid flows through the launder, aluminum titanium boron refiner is added online for grain refinement, with the addition amount being 0.08%.

[0096] S15: Continuous casting is carried out using a wheel-type crystallizer. The ingot rolling process is carried out in a 15-stand three-roll rolling mill with a rolling temperature of 505°C. After rolling, an aluminum alloy rod with a diameter of 9.5 mm is obtained, which is then collected after online cooling.

[0097] S16: The alloy rod is subjected to solution treatment, with a solution heating temperature of 490°C and a holding time of 2 hours, and then the rod is quenched and cooled rapidly to below 70°C.

[0098] S17: The rod is drawn on a sliding wire drawing machine. During the drawing, the monofilament is pre-aged at a pre-aging temperature of 120° C., and a monofilament with a diameter of 3.8 mm is obtained after drawing.

[0099] S18: performing aging treatment on the drawn alloy single wire to obtain an aluminum alloy single wire, wherein the aging process is 150° C. / 8 h.

[0100] Analysis and testing revealed the alloy composition of this embodiment to be: Mg 0.33%, Si 0.32%, Fe 0.15%, Y 0.2%, La 0.02%, and B 0.015%. The content of unavoidable impurities was ≤ 0.005% for each element and ≤ 0.02% for the total. The resulting single wire had a strength of 275 MPa and a conductivity of 59.8% IACS.

[0101] Comparative Example 1

[0102] S11: Add aluminum ingots with a purity greater than 99.7%, aluminum-silicon alloy, and aluminum-rare earth alloy to the melting furnace and heat to melt. Add a predetermined amount of magnesium ingots to the molten aluminum and stir to melt. Stir the molten aluminum thoroughly and take samples for spectral analysis to ensure the melt composition is within the required range.

[0103] S12: The aluminum liquid is transferred to a tilting holding furnace, where a trace amount of aluminum-boron alloy is added for boronization. The electromagnetic stirring device at the bottom of the furnace is activated to fully stir the melt. The melt temperature is adjusted to 740°C for refining for 10 minutes. The surface scum is then scraped off, and the temperature is adjusted to 720°C for 40 minutes.

[0104] S13: After casting begins, the melt is degassed and filtered online. A rotary jet degassing box is used for online degassing, using high-purity nitrogen as the degassing medium. Online filtration utilizes a two-stage ceramic foam filter plate with a porosity of 30 / 50 PPI.

[0105] S14: When the aluminum liquid flows through the launder, aluminum titanium boron refiner is added online for grain refinement, with the addition amount being 0.12%.

[0106] S15: Continuous casting is carried out using a wheel-type crystallizer. The billet rolling process is carried out in a 15-stand three-roll rolling mill with a rolling temperature of 500°C. After rolling, an aluminum alloy rod with a diameter of 9.5 mm is obtained, which is then collected after online cooling and quenching.

[0107] S16: The rod material is drawn on a sliding wire drawing machine to obtain a single wire with a diameter of 3.5 mm.

[0108] S17: performing aging treatment on the drawn alloy single wire, and the aging process is 160°C / 8h.

[0109] Analysis and testing revealed that the alloy composition in the comparative example was: Mg 0.47%, Si 0.45%, Fe 0.15%, Y 0.1%, La 0.02%, and B 0.005%. The resulting single fiber had a strength of 276 MPa and a conductivity of 58.2% IACS.

[0110] Comparative Example 2

[0111] S11: Add aluminum ingots with a purity greater than 99.7%, aluminum-silicon alloy, and aluminum-rare earth alloy to the melting furnace and heat to melt. Add a predetermined amount of magnesium ingots to the molten aluminum and stir to melt. Stir the molten aluminum thoroughly and take samples for spectral analysis to ensure the melt composition is within the required range.

[0112] S12: The aluminum liquid is transferred to a tilting holding furnace, where a trace amount of aluminum-boron alloy is added for boronization. The electromagnetic stirring device at the bottom of the furnace is activated to fully stir the melt. The melt temperature is adjusted to 740°C for refining for 10 minutes. The surface scum is then scraped off, and the temperature is adjusted to 730°C for 40 minutes.

[0113] S13: After casting begins, the melt is degassed and filtered online. A rotary jet degassing box is used for online degassing, using high-purity nitrogen as the degassing medium. Online filtration utilizes a two-stage ceramic foam filter plate with a porosity of 30 / 50 PPI.

[0114] S14: When the aluminum liquid flows through the launder, aluminum titanium boron refiner is added online for grain refinement, with the addition amount being 0.08%.

[0115] S15: Continuous casting is carried out using a wheel-type crystallizer. The billet rolling process is carried out in a 15-stand three-roll rolling mill with a rolling temperature of 500°C. After rolling, an aluminum alloy rod with a diameter of 9.5 mm is obtained, which is then collected after online cooling and quenching.

[0116] S16: The rod material is drawn on a sliding wire drawing machine to obtain a single wire with a diameter of 3.7 mm.

[0117] S17: performing aging treatment on the drawn alloy single wire, and the aging process is 155°C / 7h.

[0118] Analysis and testing revealed that the alloy composition in the comparative example was: Mg 0.37%, Si 0.31%, Fe 0.13%, La 0.01%, and B 0.004%. The resulting single wire had a strength of 258 MPa and a conductivity of 58.7% IACS.

[0119] Comparative Example 3

[0120] S11: Add aluminum ingots with a purity greater than 99.7%, aluminum-silicon alloy, and aluminum-rare earth alloy to the melting furnace and heat to melt. Add a predetermined amount of magnesium ingots to the molten aluminum and stir to melt. Stir the molten aluminum thoroughly and take samples for spectral analysis to ensure the melt composition is within the required range.

[0121] S12: The aluminum liquid is transferred to a tilting holding furnace, where a trace amount of aluminum-boron alloy is added for boronization. The electromagnetic stirring device at the bottom of the furnace is activated to fully stir the melt. The melt temperature is adjusted to 740°C for refining for 10 minutes. The surface scum is then scraped off, and the temperature is adjusted to 730°C for 40 minutes.

[0122] S13: After casting begins, the melt is degassed and filtered online. A rotary jet degassing box is used for online degassing, using high-purity nitrogen as the degassing medium. Online filtration utilizes a two-stage ceramic foam filter plate with a porosity of 30 / 50 PPI.

[0123] S14: When the aluminum liquid flows through the launder, aluminum titanium boron refiner is added online for grain refinement, with the addition amount being 0.08%.

[0124] S15: Continuous casting is carried out using a wheel-type crystallizer. The billet rolling process is carried out in a 15-stand three-roll rolling mill with a rolling temperature of 500°C. After rolling, an aluminum alloy rod with a diameter of 9.5 mm is obtained, which is then collected after online cooling and quenching.

[0125] S16: The rod is drawn on a sliding wire drawing machine, and the monofilament is aged at the same time at an aging temperature of 170° C. After drawing, a monofilament with a diameter of 3.7 mm is obtained.

[0126] S17: performing aging treatment on the drawn alloy single wire, and the aging process is 120°C / 7h.

[0127] Analysis and testing revealed that the alloy composition in the comparative example was: Mg 0.4%, Si 0.38%, Fe 0.15%, La 0.015%, and B 0.005%. The resulting single-filament had a strength of 246 MPa and a conductivity of 56.3% IACS.

[0128] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present application, rather than to limit them. Although the present application has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or make equivalent replacements for some or all of the technical features therein. These modifications or replacements do not deviate the essence of the corresponding technical solutions from the scope of the technical solutions of the embodiments of the present application.

Claims

1. A process for producing medium-strength and high-conductivity aluminum alloy monofilament, characterized in that: include: Aluminum alloy rods are available; Drawing the aluminum alloy rod to obtain alloy single wire, and performing a pre-aging treatment at 100-150° C. on the alloy single wire during the drawing process; The alloy single wire is artificially aged to obtain the medium-strength and high-conductivity aluminum alloy single wire; wherein the temperature of the pre-aging treatment is lower than the temperature of the artificial aging treatment.

2. The process for producing medium-strength and high-conductivity aluminum alloy monofilament according to claim 1, characterized in that: The pre-aging treatment includes: In the drawing process, the last drawing die and / or the wire storage area are heated to perform a pre-aging treatment at 100-150° C. on the alloy single wire.

3. The process for producing medium-strength and high-conductivity aluminum alloy monofilament according to claim 1, characterized in that: The artificial aging treatment includes: The alloy single wire is subjected to aging treatment at 140-160° C. for 5-10 hours.

4. The process for producing medium-strength and high-conductivity aluminum alloy monofilament according to claim 1, characterized in that: Providing the aluminum alloy rod comprises: performing a solution treatment on the aluminum alloy rod; The solution treatment comprises: The aluminum alloy rod is cast and rolled at 480-530°C for 1-3 hours, and then quenched and cooled to 50-120°C.

5. The process for producing medium-strength and high-conductivity aluminum alloy monofilament according to claim 4, characterized in that: The preparation of the aluminum alloy rod obtained by casting and rolling comprises the following steps: S11, alloy smelting: providing raw materials according to the elemental composition of the aluminum alloy rod, melting them, and obtaining a melt; S12, furnace refining: boronizing the melt, refining the melt at 740-750° C., deslagging, and standing; S13, online refining: after the casting starts, the melt is degassed and filtered online to obtain refined aluminum liquid; S14, grain refinement: adding 0.05-0.15% by mass of a refiner to the refined aluminum liquid; S15, continuous casting and rolling: the aluminum melt after online refining is cast and rolled by continuous casting and rolling process to obtain the aluminum alloy rod.

6. The process for producing medium-strength and high-conductivity aluminum alloy monofilament according to claim 5, characterized in that: In S12, the refining time is 10 to 15 minutes; and / or The standing time is 30 to 40 minutes; and / or The standing temperature is 720-730°C.

7. The process for producing medium-strength and high-conductivity aluminum alloy monofilament according to claim 5, characterized in that: The continuous casting and rolling comprises: continuously casting the online refined melt at 700-720° C. using a wheel crystallizer to obtain a cast billet; and rolling the cast billet at 490-510° C. using a continuous rolling mill to obtain an aluminum alloy rod.

8. The process for producing medium-strength and high-conductivity aluminum alloy monofilament according to claim 1, characterized in that: The element composition of the aluminum alloy rod includes, by mass fraction, Mg 0.3-0.45%, Si 0.3-0.5%, Fe 0.1-0.15%, Y 0.1-0.3%, La 0.01-0.05%, B 0.001-0.05%, and the rest is Al and other inevitable impurity elements; The total amount of the unavoidable impurity elements is ≤0.02%.

9. A medium-strength and high-conductivity aluminum alloy monofilament, characterized in that: The element composition of the aluminum alloy monofilament includes, by mass fraction, Mg 0.3-0.45%, Si 0.3-0.5%, Fe 0.1-0.15%, Y 0.1-0.3%, La 0.01-0.05%, B 0.001-0.05%, and the rest is Al and other inevitable impurity elements; The total amount of the unavoidable impurity elements is ≤0.02%.

10. The medium-strength and high-conductivity aluminum alloy monofilament according to claim 9, characterized in that: The aluminum alloy monofilament has a strength of ≥270 MPa, a conductivity of ≥59% IACS, and an elongation of ≥5%.

Citation Information

Patent Citations

  • Medium strength aluminium alloy wire with conductivity of 60% IACS, and preparation method thereof

    CN103820685A

  • Medium strength aluminium alloy wire with conductivity of 55% IACS, and preparation method thereof

    CN103820686A

  • Preparation method of intermediate strength aluminum alloy monofilament

    CN103952605A

  • Constant-temperature continuous casting and rolling method of aluminum alloy conductors

    CN108486434A

  • Preparation method of high-strength and high-conductivity aluminum alloy monofilament and aluminum alloy monofilament

    CN115595459A

Cited By

  • High-conductivity high-strength rare earth aluminum alloy conductor material and preparation method thereof

    CN121780956A