Graphite ring, preparation method for same, and epitaxial device

By covering the TaC layer in the graphite ring and partially or completely exposing or covering the SiC layer in the necessary areas, the problem of short replacement cycle and short maintenance cycle of the graphite ring is solved, the replacement and maintenance cycle is extended, the consumption cost is reduced, and the consumption cost is improved. Difficulty of doping concentration control and heat dissipation performance.

WO2024199471A1PCT designated stage expired Publication Date: 2024-10-03HUAWEI TECH CO LTD
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
PCT/CN2024/084914
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-31
Filing Date
2024-03-29
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

The replacement and maintenance cycles of existing graphite rings are short, resulting in high consumption costs, affecting the stability of the epitaxial process and the difficulty of controlling doping concentration.

Method used

Design a graphite ring, including a graphite base and a TaC layer. The TaC layer covers the inner wall of the graphite base to inhibit falling objects and SiC deposition, extend the replacement and maintenance cycle, and partially or fully expose or cover the SiC layer in necessary areas to improve heat dissipation. performance.

Benefits of technology

It extends the replacement and maintenance cycle of graphite rings, reduces consumption costs, reduces the problem of sudden changes in doping concentration in the epitaxial process, and improves the difficulty of doping concentration control and heat dissipation performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN2024084914_03102024_PF_FP_ABST
    Figure CN2024084914_03102024_PF_FP_ABST
Patent Text Reader

Abstract

The present application provides a graphite ring, a preparation method for same, and an epitaxial device. The graphite ring may comprise a graphite matrix and a TaC layer. The structure of the graphite matrix is ring-shaped. The graphite matrix comprises an upper surface, a lower surface, a matrix inner wall and a matrix outer wall. The TaC layer covers the matrix inner wall. Some or all of the surfaces of the graphite matrix other than the matrix inner wall are exposed or cover the SiC layer. According to the graphite ring provided by the present application, the TaC layer covers the matrix inner wall, and the TaC layer can protect the matrix inner wall and inhibit the matrix inner wall from generating a falling object, so that the graphite ring has a long replacement cycle. The TaC layer can also hinder the deposition of SiC, such that the graphite ring has a long maintenance cycle. Some or all of the surfaces of the graphite matrix of the graphite ring of the present application other than the matrix inner wall are exposed or cover the SiC layer, such that the heat dissipation performance of the graphite ring is good.
Need to check novelty before this filing date? Find Prior Art

Description

Graphite ring, graphite ring preparation method and epitaxial equipment

[0001] This application claims priority to the Chinese patent application filed with the State Intellectual Property Office on March 31, 2023, with application number 202310379545.7 and application name “Graphite Rings, Methods for Preparing Graphite Rings and Epitaxial Equipment”, the entire contents of which are incorporated by reference into this application. Technical Field

[0002] The present application relates to the technical field of silicon carbide crystal growth, and in particular to a graphite ring, a method for preparing the graphite ring, and an epitaxial device. Background Art

[0003] Power semiconductor devices, also known as power electronic devices, are high-power electronic devices used in power conversion and power control circuits. The design and manufacture of power semiconductor devices requires the use of epitaxial wafers, which include a substrate and an epitaxial layer disposed on the substrate surface.

[0004] Typically, both the substrate and epitaxy are made of semiconductor materials. Silicon carbide (SiC) is a typical semiconductor material. SiC possesses physical properties such as a wide bandgap, high critical electric field strength, high electron saturation mobility, and high thermal conductivity. These properties give SiC broad application prospects in high-voltage, high-power, high-frequency, and high-temperature resistant power semiconductor devices. Power semiconductor devices using SiC substrates / epitaxial growth are widely used in new energy vehicles, photovoltaic power generation, smart grids, and trams.

[0005] Typically, during the epitaxial growth process, a graphite ring can be used to balance and adjust the temperature field to form a uniform epitaxial growth on the substrate surface.

[0006] The currently disclosed graphite rings have short replacement and maintenance cycles, resulting in high consumption costs of the graphite rings.

[0007] Summary of the Invention

[0008] The present application provides a graphite ring, a method for preparing a graphite ring, and an epitaxial device. The graphite ring may include: a graphite substrate and a TaC layer, wherein the TaC layer covers the inner wall of the graphite substrate. The TaC layer can, on the one hand, inhibit the generation of falling objects on the inner wall of the substrate, and on the other hand, inhibit the reduction of the pore size of the graphite ring. The graphite ring has a longer maintenance cycle and replacement cycle, and the consumption cost of the graphite ring is low.

[0009] In a first aspect, the present application provides a graphite ring for use in a SiC epitaxial process, wherein the graphite ring comprises: a graphite substrate and a TaC layer; the graphite substrate is an annular structural component, and the surface of the graphite substrate comprises: an annular upper surface and a lower surface, an inner wall of the substrate enclosed between the inner diameters of the upper and lower surfaces, and an outer wall of the substrate enclosed between the outer diameters of the upper and lower surfaces; the TaC layer covers the inner wall of the substrate; on the graphite substrate, at least part of the surface other than the inner wall of the substrate is exposed or covered with a SiC layer.

[0010] In this embodiment, the TaC layer covers the inner wall of the base, protecting it and preventing debris from falling off. This allows for a longer replacement cycle for the graphite ring. The TaC layer also hinders SiC deposition, extending the maintenance cycle. The graphite ring provided by this embodiment has a longer replacement and maintenance cycle, resulting in lower consumption costs.

[0011] The graphite ring provided by this implementation method has a longer replacement cycle and maintenance cycle. When the graphite ring provided by this implementation method is applied to the epitaxial process, the problem of sudden changes in epitaxial doping concentration caused by replacement / maintenance of the graphite ring can be reduced, and the difficulty of controlling the epitaxial doping concentration in the epitaxial process is relatively low.

[0012] The graphite ring provided by this embodiment has at least a portion of its surface, except for the inner wall of the graphite substrate, exposed or covered with a SiC layer. Compared to graphite rings whose entire graphite substrate is covered with a TaC layer, the graphite ring provided by this embodiment has better heat dissipation performance.

[0013] In combination with the first implementation method of the first aspect, the TaC layer also covers the first area of ​​the upper surface, which is the area bordering the inner wall of the substrate; and / or, the TaC layer also covers the first area of ​​the lower surface, which is the area bordering the inner wall of the substrate.

[0014] In this implementation, the TaC covering the first area (including the first area of ​​the upper surface and / or the first area of ​​the lower surface) is arranged between the inner wall of the substrate and the exposed graphite substrate, which can hinder the SiC crystals deposited on the surface of the exposed graphite substrate from extending toward the inner wall of the substrate, thereby alleviating the reduction in the aperture of the graphite ring and allowing the graphite ring to have a longer maintenance cycle.

[0015] In the graphite ring provided by this embodiment, the outer wall and all / part of the upper / lower surface of the base are exposed. Compared with graphite rings whose entire surface of the graphite base is covered with a TaC layer, the graphite ring provided by this embodiment has better heat dissipation performance.

[0016] In combination with the second implementation manner of the first aspect, the SiC layer covers the outer wall of the substrate.

[0017] In this implementation, the SiC layer covers the outer surface of the base, which prevents debris from falling from the outer surface, allowing the graphite ring to have a longer replacement cycle. Compared with graphite rings whose entire graphite base surface is covered with a TaC layer, the graphite ring provided by this implementation has better heat dissipation performance.

[0018] In combination with the third implementation method of the first aspect, the SiC layer also covers a second area of ​​the upper surface, which is the area bordering the outer wall of the substrate; and / or, the SiC layer also covers a second area of ​​the lower surface, which is the area bordering the outer wall of the substrate.

[0019] In this implementation, the SiC layer covers the second area of ​​the upper surface and / or the second area of ​​the lower surface. The SiC layer can suppress the second area of ​​the upper surface and / or the second area of ​​the lower surface from dropping, so that the graphite ring has a longer replacement cycle.

[0020] Compared with a graphite ring whose surface of the graphite substrate is covered with a TaC layer, the graphite ring provided by this implementation has better heat dissipation performance.

[0021] In combination with the fourth implementation of the first aspect, the thickness of the TaC layer is 0.1 μm-1000 μm.

[0022] In combination with the fifth implementation of the first aspect, the thickness of the SiC layer is 0.1 μm-1000 μm.

[0023] In combination with the sixth implementation manner of the first aspect, the inner wall of the base includes: at least one annular surface connected in sequence between the upper surface and the lower surface.

[0024] In this implementation, the annular surface can be flexibly configured according to needs, thereby achieving the purpose of flexibly configuring the shape of the area defined by the inner wall of the base.

[0025] In combination with the seventh implementation manner of the first aspect, the at least one annular surface includes: a first guide surface, a limiting surface and a second guide surface, wherein the first guide surface is inclined and the second guide surface is inclined.

[0026] In this implementation, both the first and second guide surfaces function as flow guides, enabling the graphite ring to regulate and stabilize the flow field. When the graphite ring provided by this implementation is applied to an epitaxial growth process, this flow field regulation and stabilization function allows the carbon source gas and silicon source gas to flow evenly across the substrate surface, ultimately resulting in relatively uniform epitaxy.

[0027] In combination with the eighth implementation of the first aspect, on the graphite substrate, all surfaces except the inner wall of the substrate are exposed.

[0028] Compared with a graphite ring whose surface of the graphite substrate is covered with a TaC layer, the graphite ring provided by this implementation has better heat dissipation performance.

[0029] In combination with the ninth implementation of the first aspect, on the graphite substrate, all surfaces except the inner wall of the substrate are covered with a SiC layer.

[0030] Compared with a graphite ring whose surface of the graphite substrate is covered with a TaC layer, the graphite ring provided by this implementation has better heat dissipation performance.

[0031] A second aspect of the present application provides a method for preparing a graphite ring, comprising: placing a graphite substrate in a reaction chamber, the graphite substrate comprising: an annular upper surface and a lower surface, an inner wall of the substrate enclosed between the inner diameters of the upper surface and the lower surface, and an outer wall of the substrate enclosed between the outer diameters of the upper surface and the lower surface; forming a film layer, the film layer comprising: a TaC layer, or the film layer comprising: a TaC layer and a SiC layer, the TaC layer covering the inner wall of the substrate; on the graphite substrate, at least a portion of the surface other than the inner wall of the substrate is exposed or covered with a SiC layer.

[0032] The graphite ring prepared by the preparation method provided in this embodiment may include: a graphite substrate and a TaC layer. The TaC layer covers the inner wall of the substrate and protects the inner wall of the substrate to prevent debris from falling from the inner wall of the substrate, thereby extending the replacement cycle of the graphite ring.

[0033] The TaC layer can hinder the deposition of SiC. In the epitaxial process, the thickness increase of the TaC layer per unit time is small. Therefore, the graphite ring has a longer maintenance cycle.

[0034] The graphite rings produced by this method have long replacement and maintenance cycles, resulting in lower consumable costs. Furthermore, the graphite rings produced by this method have long replacement and maintenance cycles. When applied to epitaxial growth processes, these rings can reduce the problem of sudden changes in epitaxial doping concentration caused by graphite ring replacement / maintenance, making epitaxial doping concentration control in epitaxial growth processes much easier.

[0035] Compared to graphite rings whose entire graphite substrate is covered with a TaC layer, the graphite rings produced in this embodiment have at least a portion of the graphite substrate surface, except for the inner wall, exposed or covered with a SiC layer. The graphite rings produced in this embodiment have better heat dissipation performance.

[0036] In combination with the first implementation method of the second aspect, the step of forming a film layer includes: forming a SiC layer on the surface of the graphite substrate, the surface of the graphite substrate includes: the inner wall of the substrate, the outer wall of the substrate, the upper surface and the lower surface; removing the SiC layer on the target area, the target area includes: the inner wall of the substrate, or the target area includes: the inner wall of the substrate and a third area, the third area includes: the first area of ​​the upper surface, and / or, the first area of ​​the lower surface, the first area is the area bordering the inner wall of the substrate; forming a TaC layer on the target area.

[0037] In combination with the second implementation method of the second aspect, the step of forming a film layer includes: forming a TaC layer on the surface of the graphite substrate, the surface of the graphite substrate includes: the inner wall of the substrate, the outer wall of the substrate, the upper surface and the lower surface; removing the TaC layer on the target area, the target area includes: the outer wall of the substrate, or the target area includes: the outer wall of the substrate and the fourth area, the fourth area includes: the second area of ​​the upper surface, and / or, the second area of ​​the lower surface, the second area is the area bordering the outer wall of the substrate.

[0038] In combination with the third implementation manner of the second aspect, after the step of removing the TaC layer on the target area, the preparation method further includes: forming a SiC layer, where the SiC layer covers the target area.

[0039] A third aspect of the present application provides an epitaxial device, comprising: an epitaxial furnace and the graphite ring provided in the first aspect, wherein the graphite ring is arranged in the epitaxial furnace.

[0040] Among them, the effects of the third aspect can refer to the effects that can be achieved by any implementation method of the first aspect. BRIEF DESCRIPTION OF THE DRAWINGS

[0041] FIG1A is a top view of a graphite ring;

[0042] FIG1B is a cross-sectional view of region A in FIG1A on plane AA′;

[0043] FIG1C is a cross-sectional view of region A in FIG1A on plane AA′;

[0044] Figure 2 is an analysis chart of the consumption cost ratio of each graphite component;

[0045] FIG3 is a graph showing the change of epitaxial doping concentration over time;

[0046] FIG4 is a top view of a graphite ring provided in one possible embodiment;

[0047] FIG5 is a cross-sectional view of area A in FIG4 on the AA' plane;

[0048] FIG6A is a top view of a graphite ring provided in one embodiment;

[0049] FIG6B is a cross-sectional view of region A in FIG6A on plane AA′;

[0050] FIG7A is a top view of a graphite ring provided in one embodiment;

[0051] FIG7B is a cross-sectional view of region A in FIG7A on plane AA′;

[0052] FIG8A is a top view of a graphite ring provided in one embodiment;

[0053] FIG8B is a cross-sectional view of region A in FIG8A on plane AA′;

[0054] FIG9A is a top view of a graphite ring provided in one embodiment;

[0055] FIG9B is a cross-sectional view of region A in FIG9A on plane AA′;

[0056] FIG10A is a top view of a graphite substrate provided in a feasible implementation;

[0057] FIG10B is a cross-sectional view of region A of the graphite substrate provided in FIG10A on the AA′ plane;

[0058] FIG10C is a cross-sectional view of region A of the graphite substrate provided in FIG10A on the AA′ plane;

[0059] FIG10D is a cross-sectional view of region A of the graphite substrate provided in FIG10A on the AA′ plane;

[0060] FIG10E is a cross-sectional view of region A of the graphite substrate provided in FIG10A on the AA′ plane;

[0061] FIG10F is a cross-sectional view of region A of the graphite substrate provided in FIG10A on the AA′ plane;

[0062] FIG11 is an assembly diagram of an epitaxial furnace and a graphite ring provided in a feasible implementation manner;

[0063] FIG12A is a top view of a graphite ring provided in one embodiment;

[0064] FIG12B is a cross-sectional view of region A in FIG12A on plane AA′;

[0065] FIG12C is a cross-sectional view of region A in FIG12A on plane AA′;

[0066] FIG13 is a flow chart of a method for preparing a graphite ring provided in a feasible embodiment;

[0067] FIG14A is a flow chart of a method for preparing a graphite ring provided in a feasible embodiment;

[0068] FIG14B is a process flow chart corresponding to the preparation method provided in FIG14A ;

[0069] FIG15A is a flow chart of a method for preparing a graphite ring according to a feasible embodiment;

[0070] FIG15B is a process flow chart corresponding to the preparation method provided in FIG15A . DETAILED DESCRIPTION

[0071] The technical solutions in the embodiments of the present application will be described below in conjunction with the drawings in the embodiments of the present application. Obviously, the described embodiments are only part of the embodiments of the present application, rather than all the embodiments.

[0072] Hereinafter, the terms "first," "second," etc., are used solely for descriptive purposes to distinguish between identical or similar items with substantially the same function and effect, and are not to be construed as indicating or implying relative importance or implicitly specifying the number of the technical features being referred to. Therefore, a feature defined as "first," "second," etc., may explicitly or implicitly include one or more of such features.

[0073] Also, in the description of the present application, unless otherwise specified, “plurality” means two or more than two.

[0074] Furthermore, in this application, directional terms such as "upper," "lower," "left," "right," "horizontal," and "vertical" are defined relative to the schematic placement of components in the accompanying drawings. It should be understood that these directional terms are relative concepts, used for relative description and clarification, and may change accordingly based on changes in the placement of components in the accompanying drawings. Unless otherwise expressly specified or limited, the term "connection" should be understood broadly. For example, "connection" can mean fixed connection, detachable connection, or integration; it can mean direct connection or indirect connection through an intermediate medium.

[0075] At the same time, in the embodiments of this application, words such as "exemplary" or "for example" are used to indicate examples, illustrations, or descriptions. Any embodiment or design described as "exemplary" or "for example" in the embodiments of this application should not be interpreted as being more preferred or more advantageous than other embodiments or designs. Rather, the use of words such as "exemplary" or "for example" is intended to present the relevant concepts in a concrete manner to facilitate understanding.

[0076] A power conversion module converts direct current (DC) to alternating current (AC) and provides AC power. It can be mounted directly on a printed circuit board (PCB) to power application-specific integrated circuits (ASICs), digital signal processors (DSPs), microprocessors, memory, and field-programmable gate arrays (FPGAs). Power conversion modules are widely used in new energy vehicles, photovoltaic power generation, smart grids, and trams.

[0077] Generally, a power conversion module may include a busbar through which current flows and a power semiconductor device.

[0078] Among them, the busbar can also be called a laminated busbar, which is a power module electrical connection component with a multi-layer laminated structure, and can connect the power distribution points of multiple circuits.

[0079] Power semiconductor devices, also known as power electronic devices, are high-power electronic devices used in power conversion and power control circuits. Typically, power semiconductor devices are made of semiconductor materials and have two operating characteristics: conducting and blocking.

[0080] For example, a Schottky barrier diode (SBD) and a metal-oxide-semiconductor field-effect transistor (MOSFET) are two typical power semiconductor devices.

[0081] An SBD comprises a substrate and an anode and cathode disposed on the substrate. The anode is made of a precious metal, and the cathode is made of an N-type semiconductor material. A Schottky barrier layer forms at the interface between the positive and negative electrodes. When a forward bias is applied across the Schottky barrier layer (the anode is connected to the positive power supply, and the cathode is connected to the negative power supply), the Schottky barrier layer narrows, reducing the internal resistance of the SBD. When the internal resistance of the SBD decreases to a certain level, the SBD enters the on state. When a reverse bias is applied across the Schottky barrier layer, the Schottky barrier layer widens, increasing the internal resistance of the SBD. When the internal resistance of the SBD increases to a certain level, the SBD enters the blocking state. N-type semiconductor material is defined as a semiconductor material with a relatively high number of electrons.

[0082] A MOSFET includes: a substrate, a gate, a source, and a drain disposed on the substrate. The substrate is made of a P-type semiconductor material, and two N-type regions are formed on the substrate, with a PN junction formed between the N-type region and the substrate. A source connected to one of the N-type regions and a drain connected to the other N-type region are then formed. A channel exists between the source and the gate, with the gate located between the source and the gate and above the channel. When no voltage is applied to the gate, the source and gate are disconnected, meaning the MOSFET is in the off state. When a voltage greater than the threshold voltage is applied to the gate, the source and gate are connected, meaning the MOSFET is in the on state. P-type semiconductor material is defined as a semiconductor material with a relatively large number of holes.

[0083] Power semiconductor devices include a substrate, which is a crystal sheet with specific crystal planes and appropriate electrical, optical, and mechanical properties.

[0084] During the crystal growth process, defects are inevitable on the substrate surface. If other components (such as electrodes) are directly made on the substrate, the quality of the entire substrate will be affected, thus adversely affecting the performance of power semiconductor devices.

[0085] Forming an epitaxial layer on the surface of the substrate can make the surface of the substrate smoother and compensate for surface defects of the substrate, thereby ensuring that the power semiconductor device has excellent performance.

[0086] For example, a MOSFET consists of a heavily doped substrate. A lightly doped epitaxial layer is formed on top of the heavily doped substrate to increase the breakdown voltage (BV) of the PN junction. The breakdown voltage of the PN junction is defined as the voltage at which critical breakdown occurs. A higher BV value indicates greater MOSFET reliability. Heavily doped semiconductor materials are defined as those containing a high concentration of dopants, while lightly doped semiconductor materials are defined as those containing a high concentration of dopants.

[0087] Typically, both the substrate and epitaxy are made of semiconductor materials. Silicon carbide (SiC) is a typical semiconductor material. SiC possesses physical properties such as a wide bandgap, high critical electric field strength, high electron saturation mobility, and high thermal conductivity. These properties give SiC broad application prospects in high-voltage, high-power, high-frequency, and high-temperature resistant power semiconductor devices. Power semiconductor devices using SiC substrates / epitaxial growth are widely used in new energy vehicles, photovoltaic power generation, smart grids, and trams.

[0088] In the embodiment of the present application, a power semiconductor device using SiC for substrate / epitaxial growth may be referred to as a SiC electronic power device.

[0089] SiC power electronic devices have high manufacturing costs, which have become the main obstacle to further increasing the penetration rate of SiC power electronic devices in various fields.

[0090] Over 60% of the manufacturing cost of SiC power electronic devices comes from SiC substrates and SiC epitaxy. SiC substrates are defined as substrates made from SiC, and SiC epitaxy is defined as epitaxy made from SiC. In the following examples, unless otherwise specified, substrate refers to SiC substrates, and epitaxy refers to SiC epitaxy.

[0091] Therefore, continuously optimizing the production and manufacturing process to reduce the production costs of SiC substrates and SiC epitaxy is a key factor in improving the market competitiveness of SiC power electronic devices.

[0092] Currently, SiC substrate preparation methods include liquid phase epitaxy (LPE), chemical vapor deposition (CVD), physical vapor transport (PVT), high-temperature sintering, plasma spraying, etc.

[0093] SiC epitaxial growth methods include LPE, CVD, PVT, high-temperature sintering, and ion spraying. The epitaxial growth process is called the epitaxial growth process. The mainstream epitaxial growth process in the industry is CVD.

[0094] Typically, epitaxial growth is performed using epitaxial growth equipment. This equipment can include epitaxial furnaces. These furnaces are categorized by their structure into: horizontal hot-wall single-chip, planetary, vertical cavity, and vertical chamber. Horizontal hot-wall single-chip microcontrollers (MCUs) dominate the epitaxial growth industry domestically and internationally due to their stable structure, simple operation, and mature and stable process.

[0095] The core components of the epitaxial furnace reaction chamber are made of graphite. Graphite retains graphite's inherent chemical and acid resistance, corrosion resistance, and physical properties. In addition to providing physical support for the growth of epitaxial materials, graphite also provides the temperature and airflow fields required for epitaxial growth, creating a reaction space for the epitaxial process.

[0096] The epitaxial process needs to be carried out in a high-temperature environment. As a feasible implementation method, a medium-frequency coil can be used to heat the epitaxial furnace so that the epitaxial furnace can provide the temperature required for the epitaxial process.

[0097] Specifically, the heating process can be as follows: an intermediate frequency coil is placed around the periphery of the epitaxial furnace and connected to a power supply. The power supply can provide alternating current to the intermediate frequency coil. The alternating current flowing through the intermediate frequency coil generates an alternating magnetic field, which in turn generates eddy currents, which in turn generate heat energy, which is used to heat the epitaxial furnace. The heating method using the intermediate frequency coil is also called electromagnetic induction heating.

[0098] The skin effect of induction heating: the maximum current density of induction heating appears on the surface of the cross section of the heated body and decays towards the center according to the law of an exponential function. This phenomenon is called the skin effect.

[0099] Specifically, the surface of the epitaxial furnace generates a large amount of heat and has a high temperature, while the center of the epitaxial furnace generates less heat and has a lower temperature, resulting in large temperature differences between different areas. This temperature difference can lead to uneven epitaxial growth on the substrate surface.

[0100] In order to form a uniform epitaxy on the substrate surface, the graphite part may further include: a graphite ring. The structure of the graphite ring can be seen in Figures 1A, 1B, and 1C. Figure 1A is a top view of the graphite ring, Figure 1B is a cross-sectional view of area A in Figure 1A on the AA' plane, and Figure 1C is a cross-sectional view of area A in Figure 1A on the AA' plane. It can be seen that the graphite ring 100 is a component with an annular structure. During the epitaxial process, the graphite ring 100 can be placed in the area B defined by the inner wall 101 of the substrate graphite ring to adjust and stabilize the temperature field, thereby forming a uniform epitaxy on the substrate surface.

[0101] The process of the CVD epitaxial process can be: placing the graphite ring in the epitaxial furnace; placing the substrate in the area defined by the inner wall 101 of the graphite ring. Under the action of the medium frequency coil, the internal temperature of the epitaxial furnace is heated to 1500℃-1700℃, so that the epitaxial furnace can provide the temperature required for epitaxy. At an appropriate temperature, the carbon source gas and the silicon source gas are transported to the surface of the substrate using hydrogen as a carrier gas. The carbon source gas and the silicon source gas are subjected to processes such as decomposition, diffusion, adsorption, migration and combination to achieve epitaxial growth of SiC single crystal thin film materials on the surface of the substrate. Among them, the carbon source gas is defined as a gas that can provide carbon elements, wherein the carbon element can include: carbon atoms (C); the carbon source gas can include: ethylene (C2H4), propane (C3H 8 ) etc. The silicon source gas is defined as a gas that can provide silicon elements, which may include silicon atoms (Si), and the silicon source gas may include silane (SiH4), trichlorosilane (SiHCl3), etc.

[0102] During the epitaxial growth process, the etching effect of hydrogen carrier gas can cause graphite components to drop debris, a common type of debris. Graphite components typically need to be replaced after a specific epitaxial growth cycle to ensure process stability. The replacement cycle for different graphite components varies significantly based on their function.

[0103] Among many graphite parts, graphite rings have the shortest replacement cycle and are the main consumable cost factor in epitaxial production.

[0104] Please refer to Figure 2, which is an analysis chart of the consumption cost ratio of each graphite part. Figure 2 involves several graphite parts with a relatively high consumption cost, and the graphite parts with a relatively high consumption cost ratio may include: graphite rings, lower half-moon parts, upper half-moon parts, left side wall, right side wall, tray base, upper heat insulation cover, lower heat insulation cover, transition parts, and upper left protective parts. Among the several graphite parts provided in Figure 2, the consumption cost ratio of graphite rings is the highest, which can reach about 14%. In the embodiment of the present application, the consumption cost ratio is defined as the ratio of the consumption cost of a certain graphite part to the consumption cost of all graphite parts.

[0105] One of the factors that accounts for a high proportion of the consumption cost of graphite rings is that the replacement cycle of graphite rings is short.

[0106] One factor that causes the graphite parts to have a shorter replacement cycle is that during the epitaxial process, graphite rings may produce dropped objects, which results in a shorter replacement cycle for the graphite rings.

[0107] In order to alleviate the problem of falling objects from the graphite ring, as a feasible implementation method, a graphite ring with a SiC layer on the surface can be designed. The structure of the graphite ring with a SiC layer on the surface can be seen in Figure 1B. It can be seen that the graphite ring 100 may include: a graphite substrate 110 and a SiC layer 120 provided on the surface of the graphite substrate 110. The presence of the SiC layer 120 can inhibit the generation of falling objects from the graphite substrate 110, thereby allowing the graphite ring 100 to have a longer replacement cycle. The materials used for the graphite substrate 110 include: graphite. The materials used for the SiC layer 120 include: SiC.

[0108] During the epitaxial growth process, SiC generated by the decomposition, diffusion, adsorption, migration and combination of the carbon source gas and the silicon source gas can be continuously deposited on the surface of the SiC layer 120, causing the SiC layer 120 on the surface of the graphite substrate 110 to become thicker.

[0109] For details, please refer to Figures 1B and 1C. Figure 1B is a cross-sectional view of the graphite ring before the epitaxial process begins, while Figure 1C is a cross-sectional view of the graphite ring after the epitaxial process has been carried out for a period of time. Comparing Figures 1B and 1C, it can be seen that the SiC layer 120 becomes thicker after the epitaxial process has been carried out for a period of time.

[0110] As the SiC layer 120 becomes thicker, the inner diameter of the graphite ring gradually decreases. Taking the area defined by the graphite ring as a circular area as an example, the inner diameter of the graphite ring is defined as the diameter of the area defined by the inner wall 101 of the graphite ring.

[0111] The reduction in the inner diameter of the graphite ring may cause the risk of the substrate placed in the area defined by the inner wall 101 of the graphite ring to fall off the graphite ring. The substrate falling off the graphite ring will directly lead to the failure of the epitaxial process.

[0112] In order to reduce the risk of the substrate detaching from the graphite ring, in the related art epitaxial production process, the SiC layer 120 of the graphite ring is maintained or the graphite ring is replaced at a specific frequency. Among them, a common maintenance method is to polish the SiC layer 120.

[0113] For example, the SiC layer 120 of the graphite ring can be polished in the middle of each epitaxial cycle, and the graphite ring can be replaced after 1-2 epitaxial cycles.

[0114] For example, the SiC layer 120 can be polished at a node where the cumulative epitaxial thickness is 250 μm, and the graphite ring can be replaced at a node where the cumulative epitaxial thickness is 500 μm.

[0115] Epitaxial growth processes typically utilize a run-to-run control approach. This approach utilizes forward data feed and feedback to effectively monitor process progress and equipment status, adjust process deviations, and eliminate various process disturbances to improve epitaxial growth yield. The data fed can include the thickness of the graphite ring. The process can also include the doping concentration during the epitaxial growth process.

[0116] Polishing or replacing the graphite ring will cause a sudden change in the ring's thickness, which in turn will cause a sudden change in the epitaxial doping concentration, further increasing the difficulty of controlling the doping concentration. A sudden change is defined as a change per unit time greater than a set value. For example, a sudden change in the graphite ring's thickness can be considered to be an increase or decrease in thickness greater than a set value per unit time.

[0117] During the epitaxial growth process, if a graphite ring with a SiC layer is used, SiC will be deposited on the surface of the graphite ring as the epitaxial growth process progresses, causing the thickness of the graphite ring to increase, requiring frequent polishing / replacement of the graphite ring, resulting in a high consumption cost of the graphite ring.

[0118] Furthermore, frequent polishing / replacement of new graphite rings will also cause sudden changes in the temperature field and flow field during the run-to-run control process, resulting in a jump in the regulation rule of the epitaxial doping concentration, thereby increasing the difficulty of doping concentration control.

[0119] The following illustrates the effect of replacing the graphite ring on the epitaxial doping concentration, using specific figures. Please refer to Figure 3, which shows a graph of the epitaxial doping concentration changing over time. Figure 3 includes three curves: Curve 1 shows the doping concentration changing over time for the first cycle of epitaxy; Curve 2 shows the doping concentration changing over time for the second cycle; and Curve 3 shows the doping concentration changing over time for the third cycle. The first, second, and third cycles were performed consecutively, with the graphite ring replaced during the third cycle. It can be seen that the epitaxial doping concentration experienced the greatest sudden change in the third cycle. This sudden change can be determined from the changes in epitaxial doping concentration corresponding to times (3-8) in the figure.

[0120] During the epitaxial growth process, if a graphite ring without a SiC layer is used, the graphite ring will drop graphite particles as the epitaxial growth process progresses, resulting in a short replacement cycle (service life) of the graphite ring and the need for frequent replacement of new graphite rings. The consumption cost of the graphite ring is high.

[0121] The maintenance and replacement cycles of the currently disclosed graphite rings are relatively short, resulting in high consumption costs for the graphite rings, and ultimately high costs for epitaxial production. In order to solve the problems of the currently disclosed graphite rings with short maintenance and replacement cycles and high consumption costs, an embodiment of the present application provides a graphite ring, please refer to Figures 4, 5, 6A, 6B, 7A, 7B, 8A, 8B, 9A, and 9B. It can be seen that the graphite ring 1 may include: a graphite substrate 11 and a TaC layer 12. Among them, the structure of the graphite substrate 11 is annular, and the graphite substrate 11 includes: an upper surface 111, a lower surface 112, a substrate inner wall 113 enclosed between the inner diameters of the upper surface 111 and the lower surface 112, and a substrate outer wall 114 enclosed between the outer diameters of the upper surface 111 and the lower surface 112. The TaC layer 12 covers the substrate inner wall 113; on the graphite substrate, part or all of the other surfaces except the substrate inner wall 113 are exposed or covered with a SiC layer 13.

[0122] In the graphite ring provided in the embodiment of the present application, the TaC layer 12 covers the inner wall 113 of the base. The TaC layer 12 can protect the inner wall 113 of the base, inhibit the generation of falling objects on the inner wall 113 of the base, and enable the graphite ring 1 to have a longer replacement cycle.

[0123] The TaC layer 12 can also hinder the deposition of SiC. During the epitaxial process, the thickness increase of the TaC layer 12 per unit time is small. Therefore, the graphite ring 1 has a long maintenance cycle.

[0124] The graphite ring 1 provided in the embodiment of the present application has a longer replacement cycle and maintenance cycle. Therefore, the graphite ring provided in the embodiment of the present application has a lower consumption cost.

[0125] The graphite ring 1 provided in the embodiment of the present application has a longer replacement cycle and maintenance cycle. When the graphite ring provided in the embodiment of the present application is applied to the epitaxial process, the problem of sudden changes in epitaxial doping concentration caused by replacement / maintenance of the graphite ring can be reduced, and the difficulty of controlling the epitaxial doping concentration in the epitaxial process is relatively low.

[0126] Thermal conductivity is defined as the amount of heat transferred through a 1-square-meter area over a given period of time under stable heat transfer conditions, with a temperature difference of 1 K between the two surfaces of a 1-meter-thick material. A material's heat dissipation performance is related to its thermal conductivity. The greater the material's thermal conductivity, the better the heat dissipation performance of the device made from it. The smaller the material's thermal conductivity, the worse the heat dissipation performance of the device made from it.

[0127] The thermal conductivity of TaC is 22W / (mK), the thermal conductivity of graphite is 129W / (mK), and the thermal conductivity of SiC is 83W / (mK). TaC has a lower thermal conductivity, and the heat dissipation performance of the TaC layer obtained by TaC is correspondingly poor. In the graphite ring, the larger the area of ​​the TaC layer, the worse the heat dissipation performance of the graphite ring. The graphite ring 1 provided in the embodiment of the present application is on the graphite substrate, and part or all of the surfaces other than the inner wall 113 of the substrate are exposed, or, part or all of the surfaces other than the inner wall 113 of the substrate are covered with SiC layers. Compared with the graphite ring whose surface is covered by the TaC layer on the graphite substrate, the graphite ring provided in the embodiment of the present application has better heat dissipation performance.

[0128] The following is a further description of the various components of the graphite ring 1 provided in the embodiment of the present application:

[0129] The graphite ring 1 provided in the embodiment of the present application may include: a graphite matrix 11.

[0130] Please refer to Figure 10A, which shows a top view of a graphite substrate according to a feasible implementation. Graphite substrate 11 is an annular component. The annular structure of graphite substrate 11 generates eddy currents around the graphite ring during heating with a medium-frequency coil. These eddy currents interact with other eddy currents within the epitaxial furnace, stabilizing the temperature field within the furnace. This indicates that graphite substrate 11 can regulate and stabilize the temperature field.

[0131] Referring to Figures 10A, 10B, 10C, 10D, 10E, and 10F, it can be seen that the graphite substrate 11 includes an upper surface 111, a lower surface 112, a substrate inner wall 113 extending between the inner diameters of the upper surface 111 and the lower surface 112, and a substrate outer wall 114 extending between the outer diameters of the upper surface 111 and the lower surface 112. The present embodiment does not specifically limit the structure of the substrate inner wall 113, and the structure of the substrate inner wall 113 can be configured as required.

[0132] In the embodiment of the present application, the base inner wall 113 is at least one annular surface sequentially connected between the upper surface 111 and the lower surface 112 .

[0133] As a feasible implementation, the base inner wall 113 may include: an annular surface.

[0134] For example, please refer to Figures 10A and 10B, wherein Figure 10B is a cross-sectional view of region A of the graphite substrate provided in Figure 10A on plane AA'. It can be seen that the at least one annular surface may include: a vertically arranged limiting surface 1A.

[0135] During the epitaxial growth process, the epitaxial furnace may include a tray for supporting the substrate. A graphite substrate 11 may be positioned around the tray. The height of the graphite substrate 11 is greater than that of the tray. Therefore, the stop surface 1A can serve as a position limiter for the substrate placed on the tray, preventing it from sliding.

[0136] For example, please refer to Figures 10A and 10C. Figure 10C is a cross-sectional view of region A of the graphite substrate shown in Figure 10A, taken along plane AA'. As can be seen, at least one annular surface may include an inclined flow guide surface 1B. The flow guide surface 1B can regulate and stabilize the flow field, thereby enabling the graphite ring to achieve this flow regulation and stabilization function.

[0137] It is worth noting that FIG10C is only an exemplary illustration of an example in which the guide surface is inclined inward from top to bottom. In the actual design process, the guide surface is inclined outward from top to bottom.

[0138] The graphite ring provided by this implementation is applied to the epitaxial process. Since the graphite ring has the function of regulating and stabilizing the flow field, the carbon source gas and the silicon source gas can flow evenly through the surface of the substrate, and finally a relatively uniform epitaxial growth can be formed on the substrate surface.

[0139] As a feasible implementation method, the base inner wall 113 may also include: a plurality of annular surfaces. The specific number of annular surfaces can be set according to needs, and the embodiment of the present application does not make too many restrictions.

[0140] For example, please refer to Figures 10A and 10D, wherein Figure 10D is a cross-sectional view of region A of the graphite substrate provided in Figure 10A on the AA' plane. The multiple annular surfaces may include: a first limiting surface 1C and a second limiting surface 1D, wherein the first limiting surface 1C is disposed on top of the second limiting surface 1D, and the aperture (first aperture) of the region defined by the first limiting surface 1C is larger than the aperture (second aperture) of the region defined by the second limiting surface 1D.

[0141] During the epitaxial growth process, a tray for supporting the substrate can be placed in the area defined by the second limiting surface 1D. The size of the substrate is limited by the second aperture size. Since the first aperture is larger than the second aperture, a larger substrate can be placed on the tray.

[0142] For example, please refer to Figures 10A and 10E, wherein Figure 10E is a cross-sectional view of region A of the graphite substrate provided in Figure 10A on the AA' plane. The multiple annular surfaces may include: a guide surface 1E and a limiting surface 1F. The guide surface 1E is disposed on top of the limiting surface 1F.

[0143] For example, see Figures 10A and 10F, where Figure 10F is a cross-sectional view of region A of the graphite substrate shown in Figure 10A, taken along the AA' plane. The multiple annular surfaces may include a first flow-guiding surface 1G, a limiting surface 1H, and a second flow-guiding surface 1I. The first flow-guiding surface 1G is disposed on top of the limiting surface 1H, and the limiting surface 1H is disposed on top of the second flow-guiding surface 1I.

[0144] Please continue to refer to FIG. 10F . In order to better fix the graphite ring, as a feasible implementation method, the bottom of the graphite base 11 near the periphery can also be raised downward to form a limiting protrusion 115 .

[0145] Please refer to Figure 11, which is an assembly diagram of an epitaxial furnace and a graphite ring provided in a feasible implementation. As can be seen, the epitaxial furnace can include: a tray 200 and a base 300. The tray 200 is placed on the base 300 and includes: a supporting surface 21 for supporting a substrate.

[0146] The limiting protrusion 115 can be sleeved around the outer wall 31 of the base 300 so that the graphite ring 1 can be better fixed.

[0147] The embodiments of the present application are merely exemplary introductions to the structures of several graphite substrates. The structures of the above-mentioned graphite substrates do not constitute specific limitations. In actual application, the structure of the graphite substrate can be adjusted according to needs, and the applicant does not make too many limitations here.

[0148] The embodiment of the present application does not specifically limit the structure of the base outer wall 114 . For example, the base outer wall 114 may be barrel-shaped.

[0149] The embodiment of the present application does not specifically limit the size of the graphite substrate 11. The size of the graphite substrate 11 may include: the size of the outer diameter of the graphite substrate 11, the size of the inner diameter of the graphite substrate 11, the thickness of the graphite substrate 11, etc.

[0150] As a feasible implementation, the inner diameter of the graphite substrate 11 can be designed based on the size of the substrate used in the subsequent epitaxial process. This allows the substrate to be placed within the area defined by the substrate inner wall 113 during the epitaxial process. Exemplary substrate sizes include 2 inches, 4 inches, 6 inches, 8 inches, and 10 inches.

[0151] As a feasible implementation method, the outer diameter of the graphite substrate 11 can be designed according to the size of the epitaxial furnace chamber so that the graphite substrate can be placed in the epitaxial furnace chamber. For example, the size of the epitaxial furnace chamber can include: 2 inches, 4 inches, 6 inches, 8 inches, and 10 inches.

[0152] As a feasible implementation method, the thickness of the graphite ring can be set according to the height of the tray in the epitaxial furnace. For example, the thickness of the graphite ring is preferably greater than the height of the tray.

[0153] The graphite ring 1 provided in the embodiment of the present application further includes a tantalum carbide (TaC) layer 12 .

[0154] The TaC layer 12 covers the inner wall 113 of the substrate. The TaC layer 12 can protect the inner wall 113 of the substrate and inhibit the generation of debris from the inner wall 113 of the substrate. This allows the graphite ring to have a longer replacement cycle. At the same time, the TaC layer 12 can hinder the deposition of SiC. The graphite ring provided in the embodiment of the present application does not need to be polished on the inner wall of the substrate at a specific frequency. Therefore, the graphite ring has a longer maintenance cycle. The graphite ring 1 provided in the embodiment of the present application has a longer replacement cycle and maintenance cycle. Therefore, the graphite ring provided in the embodiment of the present application has a lower consumption cost.

[0155] Please continue to refer to Figures 4 and 5. Figure 5 is a cross-sectional view of area A on plane AA' in Figure 4. As a feasible implementation, the upper surface 111, the lower surface 112, and the base outer wall 114 can be exposed.

[0156] The graphite ring provided by this implementation is applied to the epitaxial process. As the epitaxial process proceeds, part of the SiC will be deposited on the surface of the exposed graphite substrate 11 (upper surface 111, lower surface 112, and substrate outer wall 114) to form SiC crystals. At this time, the structure of the graphite ring can be seen in Figures 12A and 12B. Figure 12A is a top view of the graphite ring after a period of epitaxial process. Figure 12B is a cross-sectional view of area A of the graphite ring 1 provided in Figure 12A on the AA' plane. It can be seen that after a period of epitaxial process, SiC crystals 400 cover the upper surface 111, the lower surface 112 and the substrate outer wall 114. The SiC crystals 400 can play a role in preventing the upper surface 111, the lower surface 112 and the substrate outer wall 114 from producing falling objects. Therefore, the graphite ring provided by this implementation has a longer replacement cycle.

[0157] As the epitaxial growth process progresses, SiC crystals 400 gradually diffuse into the surrounding area. The structure of the graphite ring at this point can be seen in Figure 12C , which is a cross-sectional view of region A of the graphite ring shown in Figure 12A taken along the AA' plane. It can be seen that the laterally growing SiC crystals 401 can grow toward the inner wall of the substrate, resulting in a decrease in the aperture of graphite ring 1. This reduces the need for regular polishing and maintenance of graphite ring 1, shortening its maintenance cycle.

[0158] In order to make the graphite ring have a longer maintenance cycle, as a feasible implementation method, the TaC layer can cover the first area of ​​the upper surface and / or the first area of ​​the lower surface. In the embodiment of the present application, the first area is the area bordering the inner wall of the base.

[0159] Specifically, please refer to Figures 6A and 6B. Figure 6A is a top view of a graphite ring according to a feasible embodiment, and Figure 6B is a cross-sectional view of region A in Figure 6A taken along the AA' plane. It can be seen that the TaC layer 12 includes a TaC layer 121 covering the first region 111 of the upper surface, a TaC layer 122 covering the inner wall 113 of the substrate, and a TaC layer 123 covering the first region 1121 of the lower surface. The remaining surfaces (1112, 1122, and 114) of the graphite substrate are exposed.

[0160] It is worth noting that Figures 6A and 6B are only exemplary introductions of an example in which the TaC layer 12 covers the first area 1111 of the upper surface and the first area 1121 of the lower surface. In actual application, the TaC layer 12 can cover the first area 1111 of the upper surface and the inner wall 113 of the substrate, or the TaC layer 12 can cover the first area 1121 of the lower surface and the inner wall 113 of the substrate.

[0161] The embodiment of the present application does not impose any specific limitation on the size of the first area, and the size of the first area can be set according to needs.

[0162] In this implementation, the TaC (121, 123) covering the first area (the first area 1111 of the upper surface, and / or the first area 1121 of the lower surface) is arranged between the inner wall 113 of the substrate and the exposed graphite substrate, which can hinder the SiC crystals deposited on the surface of the exposed graphite substrate from extending toward the inner wall of the substrate, thereby alleviating the reduction in the aperture of the graphite ring 1, so that the graphite ring 1 has a longer maintenance cycle.

[0163] In the graphite ring provided by this embodiment, the outer wall and all / part of the upper / lower surface of the base are exposed. Compared with graphite rings whose entire surface of the graphite base is covered with a TaC layer, the graphite ring provided by this embodiment has better heat dissipation performance.

[0164] The present embodiment does not impose a specific limitation on the thickness of the TaC layer 12. The thickness of the TaC layer 12 can be set as required. For example, as a feasible implementation, the thickness of the TaC layer 12 can be in the range of 0.1 μm to 1000 μm. Exemplary thicknesses of the TaC layer 12 can be 0.1 μm, 1 μm, 10 μm, 30 μm, etc.

[0165] In some feasible implementations, the graphite ring 1 further includes: a SiC layer 13 .

[0166] Exemplarily, as a feasible implementation method, the SiC layer can cover: the upper surface, the lower surface, and the outer wall of the substrate; for details, please refer to Figures 7A and 7B. Figure 7A is a top view of the graphite ring provided in a feasible embodiment, and Figure 7B is a cross-sectional view of area A in Figure 7A on the AA' plane. It can be seen that the TaC layer 12 covers the inner wall 113 of the substrate, and the TaC layer 12 has the effect of suppressing the generation of debris from the inner wall 113 of the substrate. The SiC layer 13 covers the upper surface 111, the lower surface 112, and the outer wall 114 of the substrate, and the SiC layer 13 has the effect of suppressing the generation of debris from the upper surface 111, the lower surface 112, and the outer wall 114 of the substrate.

[0167] Exemplarily, as a feasible implementation method, the SiC layer can cover the second area of ​​the upper surface, the second area of ​​the lower surface, and the outer wall of the substrate. For details, please refer to Figures 8A and 8B. Figure 8A is a top view of the graphite ring provided in a feasible embodiment; Figure 8B is a cross-sectional view of area A in Figure 8A on the AA' plane. It can be seen that the TaC layer 121 covers the first area 1111 of the upper surface, the TaC layer 122 covers the inner wall 113 of the substrate, and the TaC layer 123 covers the first area 1121 of the lower surface; the SiC layer 131 covers the second area 1112 of the upper surface, the SiC layer 132 covers the outer wall 114 of the substrate, and the TaC layer 123 covers the second area 1122 of the lower surface. The second area is the area bordering the outer wall 114 of the substrate.

[0168] As an example, as a feasible implementation, a SiC layer can cover the outer wall of the substrate. For details, see Figures 9A and 9B. Figure 9A is a top view of a graphite ring provided in a feasible embodiment; Figure 9B is a cross-sectional view of region A in Figure 9A taken along the AA' plane. It can be seen that TaC layer 121 covers upper surface 111, TaC layer 122 covers inner wall 113 of the substrate, and TaC layer 123 covers lower surface 112; SiC layer 13 covers outer wall 114 of the substrate.

[0169] It is worth noting that Figures 7A, 8A, and 9A are merely exemplary examples of the SiC layer 13 and the TaC layer 12 being in contact. In actual applications, the SiC layer 13 and the TaC layer 12 may be arranged in contact or spaced apart. The spaced-apart arrangement of the SiC layer 13 and the TaC layer 12 means that the graphite substrate between the SiC layer 13 and the TaC layer 12 is exposed.

[0170] The embodiment of the present application does not impose any specific limitation on the size of the second area, and the size of the second area can be set according to needs.

[0171] The graphite ring provided by this embodiment may include: a graphite substrate 11, a TaC layer 12, and a SiC layer 13. The TaC layer 12 and the SiC layer 13 can suppress the generation of falling objects from the graphite substrate, so that the graphite ring has a longer service and replacement cycle.

[0172] The TaC layer (122, 123) is disposed between the inner wall of the substrate and the SiC layer 13, thereby preventing SiC crystals deposited on the surface of the SiC layer from extending toward the inner wall of the substrate. This can alleviate the reduction in the aperture of the graphite ring 1, thereby extending the maintenance cycle of the graphite ring 1. Compared with a graphite ring whose entire surface of the graphite substrate is covered with a TaC layer, the graphite ring provided by this implementation has better heat dissipation performance.

[0173] The present embodiment does not impose any specific limitation on the thickness of the SiC layer 13, and the thickness of the SiC layer 13 can be set as required. For example, as a feasible implementation, the thickness of the SiC layer 13 can be 0.1 μm-1000 μm. Exemplary thicknesses of the SiC layer 13 can be 0.1 μm, 1 μm, 10 μm, 100 μm, 1000 μm, etc.

[0174] The present application also provides a method for preparing a graphite ring. Specifically, please refer to FIG13 , which is a flow chart of a method for preparing a graphite ring provided in a feasible embodiment. It can be seen that the preparation method may include: S131-S132.

[0175] S131: placing a graphite substrate in a reaction chamber.

[0176] In the embodiment of the present application, the reaction place where a film layer (the film layer may include: a SiC layer and a TaC layer, or the film layer may include: a SiC layer) is formed on the surface of the graphite substrate is called a reaction chamber.

[0177] The surface of the graphite substrate may include the upper surface, the lower surface, the inner wall of the substrate and the outer wall of the substrate.

[0178] As a feasible implementation method, the graphite substrate can adopt an existing graphite substrate.

[0179] As a feasible implementation, a graphite substrate can be prepared before placing the graphite substrate in the reaction chamber. Conventional methods for preparing graphite substrates in the art can be employed. For example, graphite columns can be fabricated from isostatically pressed graphite material; the graphite columns can then be mechanically cut or polished to form a ring-shaped graphite substrate.

[0180] The embodiment of the present application does not specifically limit the size of the graphite matrix, wherein the size of the graphite matrix may include: the size of the outer diameter of the graphite ring and the size of the inner diameter of the graphite ring.

[0181] As a feasible implementation, the inner diameter of the graphite substrate can be designed based on the size of the substrate used in the subsequent epitaxial growth process. This allows the substrate to be placed within the area defined by the substrate's inner wall during the epitaxial growth process. Exemplary substrate sizes include 2 inches, 4 inches, 6 inches, 8 inches, and 10 inches.

[0182] As a feasible implementation, the outer diameter of the graphite ring can be designed based on the reaction chamber used in the subsequent epitaxial growth process. This allows the graphite substrate to be placed within the reaction chamber during the epitaxial growth process. Possible reaction chamber sizes include 2 inches, 4 inches, 6 inches, 8 inches, and 10 inches.

[0183] S132: forming a film layer, where the film layer includes a TaC layer, or the film layer includes a TaC layer and a SiC layer.

[0184] The TaC layer covers the inner wall of the substrate; on the graphite substrate, part or all of the surfaces except the inner wall of the substrate are exposed, or part or all of the surfaces except the inner wall of the substrate are covered with the SiC layer.

[0185] The TaC layer may be formed by a conventional method in the art. For example, the TaC layer may be formed by CVD, high-temperature sintering, or ion spraying.

[0186] The following takes the formation of a TaC layer by CVD as an example to further explain the implementation method of forming a TaC layer:

[0187] As a feasible implementation method, the TaC layer can be implemented by heating the reaction chamber so that the heated reaction chamber can provide the temperature required to form the TaC layer. The gas environment in the reaction chamber is: carbon source gas and tantalum source gas. The carbon source gas can decompose carbon atoms (C), and the tantalum source gas can decompose tantalum atoms (Ta). C and Ta can diffuse and adsorb to the surface of the graphite substrate. The C and Ta adsorbed on the surface of the graphite substrate migrate in a direction close to each other and combine to form a TaC layer on the surface of the graphite substrate. Among them, the tantalum source gas can be: tantalum pentachloride (TaCl5) and tantalum tetrachloride (TaCl4).

[0188] As a feasible implementation method, the TaC layer can be implemented by heating the reaction chamber so that the heated reaction chamber can provide the temperature required to form the TaC layer. The gas environment in the reaction chamber is: tantalum source gas. The Ta decomposed by the tantalum source gas can reach the surface of the graphite substrate and combine with the C provided by the graphite substrate to form a TaC layer. The TaC layer obtained by this implementation method is equivalent to the TaC layer being tightly nested in the graphite substrate through in situ growth, thereby significantly increasing the bonding strength between the TaC layer and the graphite substrate and effectively preventing the TaC layer from peeling off.

[0189] As a feasible implementation, the TaC layer can be formed by heating the reaction chamber to provide the temperature required for forming the TaC layer. The gas environment in the reaction chamber is tantalum vapor (Ta) and carbon vapor (C). The Ta and C can combine on the surface of the ink substrate to form a TaC layer.

[0190] TaC has a low thermal conductivity, and the resulting TaC layer has poor heat dissipation performance. In a graphite ring, the larger the TaC layer, the worse the heat dissipation performance. To improve the heat dissipation performance of the graphite ring, in the present embodiment, it is necessary to remove all or part of the TaC layer from the outer surface of the base.

[0191] Specifically, the TaC layer can be removed from all or part of the substrate's surfaces (top, bottom, and outer wall) except the substrate's inner wall by machining or polishing. The structure of the graphite ring produced by removing the TaC layer from all surfaces except the substrate's inner wall can be seen in Figure 4. The structure of the graphite ring produced by partially removing the TaC layer from the substrate's outer wall can be seen in Figure 6A.

[0192] The exposed graphite substrate is prone to droplets. In order to reduce the droplets generated by the graphite substrate, as a feasible implementation method, the graphite ring may include: a graphite substrate and a composite film layer covering the graphite substrate, wherein the composite film layer includes: a TaC layer and a SiC layer.

[0193] The following is an explanation of the method for preparing a graphite ring comprising a composite film layer with reference to the accompanying drawings:

[0194] This embodiment of the present application also provides a method for preparing a graphite ring. The graphite ring includes a composite film layer. Please refer to Figures 14A and 14B. Figure 14A is a flow chart of the graphite ring preparation method provided in a feasible embodiment; Figure 14B is a process flow chart corresponding to the preparation method provided in Figure 14A. The preparation method may include: S141-S143.

[0195] S141: forming a TaC layer on the surface of the graphite substrate.

[0196] The implementation method of forming the TaC layer on the surface of the graphite substrate can refer to the above embodiments and will not be described again here.

[0197] (I) in FIG14B provides a schematic diagram of a graphite substrate, and the surface of the graphite substrate may include: an upper surface 111, a lower surface (not marked in the figure), a substrate inner wall 113 and a substrate outer wall (not marked in the figure).

[0198] 14B (2) is a schematic diagram of a graphite substrate covered with a TaC layer. It can be seen that the TaC layer 12 covers the surface of the graphite substrate.

[0199] S142: removing the TaC layer on the target area.

[0200] In this implementation, the target area includes: the outer wall of the substrate, or the target area includes: the outer wall of the substrate and a fourth area, the fourth area includes: the second area of ​​the upper surface, and / or the second area of ​​the lower surface, the second area is the area bordering the outer wall of the substrate.

[0201] The TaC layer on the target area may be removed by a conventional method for removing the TaC layer in the art, for example, by polishing.

[0202] The structure obtained by removing the TaC layer on the outer wall, upper surface and lower surface of the substrate can be seen in (3A) of Figure 14B. It can be seen that the upper surface 111, the lower surface and the outer wall of the substrate are exposed.

[0203] The structure obtained by removing the TaC layer on the second area of ​​the upper surface, the outer wall of the substrate, and the second area of ​​the lower surface can be seen in (B) of Figure 14B. It can be seen that the second area 1112 of the upper surface, the outer wall of the substrate, and the second area of ​​the lower surface are exposed.

[0204] S143: A SiC layer is formed, and the SiC layer covers the target area.

[0205] The SiC layer can be formed using methods commonly used in the art, such as CVD, high-temperature sintering, ion spraying, etc. Since the SiC layer will not form on the surface of the TaC layer, but can form on the surface of the exposed graphite substrate, the solution provided by this implementation method can form a SiC layer in the target area.

[0206] Based on the structure provided in (3A) of Figure 14B , the structure of the resulting graphite ring after forming the SiC layer can be seen in (4A) of Figure 14B . As can be seen, the graphite ring includes: a graphite substrate 11, a SiC layer 13, and a TaC layer 12; the graphite substrate includes: an upper surface 111, a lower surface, an inner substrate wall 113, and an outer substrate wall. The TaC layer 12 covers the inner substrate wall 113; the SiC layer 13 covers the outer substrate wall, the upper surface 111, and the lower surface.

[0207] Based on the structure provided in (3B) of Figure 14B , the structure of the resulting graphite ring after forming the SiC layer can be seen in (4B) of Figure 14B . As can be seen, the graphite ring can include: a graphite substrate 11, a SiC layer 13, and a TaC layer 12. The graphite substrate includes: an upper surface 111, a lower surface, an inner substrate wall 113, and an outer substrate wall. The TaC layer 12 covers the inner substrate wall 113, a first region 1111 of the upper surface, and a first region of the lower surface; the SiC layer 13 covers the outer substrate wall, a second region 1112 of the upper surface, and a second region of the lower surface.

[0208] This embodiment of the present application also provides a method for preparing a graphite ring comprising a composite film layer. Please refer to Figures 15A and 15B. Figure 15A is a flow chart of a graphite ring preparation method according to a feasible embodiment; Figure 15B is a process flow chart corresponding to the preparation method provided in Figure 15A. The preparation method may include the following steps: S151-S153.

[0209] S151: forming a SiC layer on the surface of the graphite substrate.

[0210] The implementation method of forming the SiC layer can refer to the above embodiments and will not be repeated here.

[0211] FIG15B (I) provides a schematic diagram of a graphite substrate. It can be seen that the surface of the graphite substrate may include: an upper surface 111, a lower surface (not marked in the figure), a substrate inner wall 113 and a substrate outer wall (not marked in the figure).

[0212] FIG15B (2) is a schematic diagram of a graphite substrate covered with a SiC layer. As can be seen, the SiC layer 13 covers the surface of the graphite substrate 11.

[0213] S152: removing the SiC layer on the target area.

[0214] In this implementation, the target area includes: the inner wall of the substrate, or the target area includes: the inner wall of the substrate and a third area, and the third area includes: the first area of ​​the upper surface and / or the first area of ​​the lower surface.

[0215] The SiC layer on the target area may be removed by a conventional SiC layer removal method in the art, for example, by grinding.

[0216] The structure obtained by removing the SiC layer covering the inner wall of the substrate can be seen in (3A) of Figure 15B. It can be seen that the inner wall 113 of the substrate is exposed.

[0217] The structure obtained by removing the SiC layer on the inner wall and the third region of the substrate can be seen in (B) of Figure 15B. It can be seen that the inner wall 113 of the substrate, the first region 1111 of the upper surface, and the first region of the lower surface (not shown) are exposed.

[0218] S153: Form a TaC layer on the target area.

[0219] Part of the outer wall of the graphite substrate is covered by the SiC layer. The embodiment of the present application requires that a TaC layer be formed in the exposed area of ​​the graphite substrate. In order to avoid the formation of a TaC layer on the surface of the SiC layer. In this implementation method, a TaC layer can be formed by utilizing the Ta decomposed from the tantalum source gas and the C on the exposed graphite substrate surface (target area) in an environment where the reaction temperature is lower than the decomposition temperature of SiC under the gas atmosphere of tantalum source gas. The TaC layer covers the first area of ​​the inner wall of the substrate and the outer wall of the substrate. Since the reaction temperature is lower than the decomposition temperature of SiC, the SiC layer cannot decompose C. Therefore, under the gas atmosphere of tantalum source gas, a TaC layer cannot be formed on the surface of the SiC layer.

[0220] Based on the structure provided in (3A) of Figure 15B , the structure of the resulting graphite ring after forming the SiC layer can be seen in (4A) of Figure 15B . It can be seen that the graphite ring can include: a graphite substrate 11, a TaC layer 12, and a SiC layer 13. The graphite substrate can include: an upper surface 111, a lower surface, an inner substrate wall 113, and an outer substrate wall. The TaC layer 12 covers the inner substrate wall 113; the SiC layer 13 covers the outer substrate wall, the upper surface 111, and the lower surface.

[0221] Based on the structure provided in (3B) of Figure 15B , the structure of the resulting graphite ring after forming the SiC layer can be seen in (4B) of Figure 15B . It can be seen that the graphite ring includes: a graphite substrate 11, a SiC layer 13, and a TaC layer 12. The graphite substrate includes: an upper surface 111, a lower surface, an inner substrate wall 113, and an outer substrate wall. The TaC layer 12 covers the inner substrate wall 113, a first region 1111 of the upper surface, and a first region of the lower surface; the SiC layer 13 covers the outer substrate wall, a second region 1112 of the upper surface, and a second region of the lower surface.

[0222] The graphite ring prepared by the preparation method provided in the embodiment of the present application may include: a graphite substrate and a TaC layer. The TaC layer covers the inner wall of the substrate and can protect the inner wall of the substrate to prevent the inner wall from falling off, thereby extending the replacement cycle of the graphite ring.

[0223] The TaC layer can hinder the deposition of SiC. In the epitaxial process, the thickness increase of the TaC layer per unit time is small. Therefore, the graphite ring has a longer maintenance cycle.

[0224] The graphite rings produced in the embodiments of the present application have longer replacement and maintenance cycles, and therefore have lower consumption costs. Furthermore, the graphite rings produced in the embodiments of the present application have longer replacement and maintenance cycles. When the graphite rings provided in the embodiments of the present application are applied to an epitaxial process, the problem of sudden changes in epitaxial doping concentration during the epitaxial process due to replacement / maintenance of the graphite rings can be reduced, and the difficulty of controlling the epitaxial doping concentration during the epitaxial process is relatively low.

[0225] Compared with the graphite ring whose surface of the graphite substrate is covered with a TaC layer, the graphite ring prepared in the embodiment of the present application has a partial or complete exposure or coverage of the SiC layer on the graphite substrate except for the inner wall of the substrate, and the graphite ring has better heat dissipation performance.

[0226] An embodiment of the present application provides an epitaxial device, comprising: an epitaxial furnace and a graphite ring provided in an embodiment of the present application, wherein the graphite ring is arranged in the epitaxial furnace.

[0227] These are only specific embodiments of the present application, but the scope of protection of this application is not limited to them. Any changes or substitutions that can be easily conceived by a person skilled in the art within the technical scope disclosed in this application should be included in the scope of protection of this application. Therefore, the scope of protection of this application should be based on the scope of protection of the claims.

Claims

1. A graphite ring, used in SiC epitaxial process, characterized in that: The graphite ring comprises: a graphite matrix and a TaC layer; The graphite substrate is an annular structural component, and the surface of the graphite substrate includes: an annular upper surface and a lower surface, an inner wall of the substrate surrounded between the inner diameters of the upper surface and the lower surface, and an outer wall of the substrate surrounded between the outer diameters of the upper surface and the lower surface; The TaC layer covers the inner wall of the substrate; On the graphite substrate, at least a portion of the surfaces other than the inner wall of the substrate are exposed or covered with a SiC layer.

2. The graphite ring according to claim 1, characterized in that: On the graphite substrate, all surfaces except the inner wall of the substrate are exposed.

3. The graphite ring according to claim 1, characterized in that: On the graphite substrate, all surfaces except the inner wall of the substrate are covered with SiC layers.

4. The graphite ring according to claim 1, characterized in that: The TaC layer also covers a first region of the upper surface, where the first region of the upper surface is a region bordering the inner wall of the substrate; and / or, The TaC layer also covers a first region of the lower surface, where the first region of the lower surface is a region bordering an inner wall of the substrate.

5. The graphite ring according to any one of claims 1 to 4, characterized in that: The SiC layer covers the outer wall of the substrate.

6. The graphite ring according to any one of claims 1 to 5, characterized in that: The SiC layer covers a second region of the upper surface, and the second region of the upper surface is a region bordering the outer wall of the substrate; and / or, The SiC layer also covers a second region of the lower surface, and the second region of the lower surface is a region bordering the outer wall of the substrate.

7. The graphite ring according to any one of claims 1 to 6, characterized in that: The thickness of the TaC layer is between 0.1 μm and 1000 μm.

8. The graphite ring according to any one of claims 1 to 7, characterized in that: The thickness of the SiC layer is 0.1 μm-1000 μm.

9. The graphite ring according to any one of claims 1 to 8, characterized in that: The inner wall of the base includes: at least one annular surface sequentially connected between the upper surface and the lower surface.

10. The graphite ring according to claim 9, characterized in that The at least one annular surface comprises: a first flow guiding surface, a limiting surface and a second flow guiding surface, wherein the first flow guiding surface is inclined and the second flow guiding surface is inclined.

11. A method for preparing a graphite ring, characterized in that: include: Placing a graphite substrate in a reaction chamber, wherein the graphite substrate is an annular structural component, and the surface of the graphite substrate includes: an annular upper surface and a lower surface, an inner wall of the substrate surrounded between the inner diameters of the upper surface and the lower surface, and an outer wall of the substrate surrounded between the outer diameters of the upper surface and the lower surface; A film layer is formed, wherein the film layer includes: a TaC layer, or the film layer includes: a TaC layer and a SiC layer; the TaC layer covers the inner wall of the substrate; on the graphite substrate, other surfaces except the inner wall of the substrate are at least partially exposed or covered with the SiC layer.

12. The preparation method according to claim 11, characterized in that: The step of forming the film layer comprises: forming a SiC layer on the surface of the graphite substrate, wherein the surface of the graphite substrate includes: an inner wall of the substrate, an outer wall of the substrate, the upper surface and the lower surface; Removing the SiC layer on the target area, the target area includes: the inner wall of the substrate, or the target area includes: the inner wall of the substrate and a third area; the third area includes: the first area of ​​the upper surface, and / or the first area of ​​the lower surface, the first area is an area bordering the inner wall of the substrate; A TaC layer is formed on the target area.

13. The preparation method according to claim 11, characterized in that: The step of forming the film layer comprises: forming a TaC layer on the surface of the graphite substrate, wherein the surface of the graphite substrate includes: an inner wall of the substrate, an outer wall of the substrate, the upper surface and the lower surface; The TaC layer on the target area is removed, wherein the target area includes: the outer wall of the substrate, or the target area includes: the outer wall of the substrate and a fourth area, wherein the fourth area includes: the second area of ​​the upper surface, and / or the second area of ​​the lower surface, and the second area is an area bordering the outer wall of the substrate.

14. The preparation method according to claim 13, characterized in that: After the step of removing the TaC layer on the target area, the preparation method further comprises: A SiC layer is formed, the SiC layer covering the target area.

15. An epitaxial device, characterized in that: include: An epitaxial furnace and a graphite ring as claimed in any one of claims 1 to 10, wherein the graphite ring is arranged in the epitaxial furnace.

Citation Information

Patent Citations

  • Susceptor

    CN101001978A

  • Epitaxially coated semiconductor wafer and device and method for producing an epitaxially coated semiconductor wafer

    CN101225544A

  • Tray, chamber device and epitaxy equipment

    CN102677164A

  • Susceptor and method for manufacturing same

    CN106460168A

  • Preparation method of coating for silicon carbide epitaxial growth equipment carrying disc

    CN111118599A