High strength cold rolled and annealed steel and method of manufacturing thereof
The development of MB steel with a martensite-bainite microstructure and a controlled manufacturing process addresses the balance between strength and ductility in conventional steels, achieving high tensile strength and elongation, suitable for automotive and structural applications.
Patent Information
- Application Number
- PCT/IB2024/052882
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-27
- Filing Date
- 2024-03-26
- Publication Date
- 2024-10-03
AI Technical Summary
Conventional high-strength steels face limitations in achieving a balance between tensile strength and ductility due to the requirement of high silicon content, which complicates casting and surface quality, restricting their application in structural and safety components like automobile battery casings.
A new class of steel, MB steel, with a microstructure comprising a mixture of martensite and bainite phases, is developed using a specific chemical composition and a manufacturing process combining thermomechanical, hot rolling, and continuous annealing under controlled conditions, achieving a tensile strength above 1400 MPa and elongation over 7%.
The MB steel exhibits improved mechanical properties, including ultimate tensile strength in the range of 1400-1800 MPa, yield strength of 1000-1300 MPa, and minimum total elongation of 7%, making it suitable for manufacturing structural and safety components with enhanced formability and reduced energy consumption.
Smart Images

Figure IB2024052882_03102024_PF_FP_ABST
Abstract
Description
HIGH STRENGTH COLD ROLLED AND ANNEALED STEEL AND METHOD OF MANUFACTURING THEREOFFIELD OF INVENTION
[0001] The present invention relates to a high strength cold rolled and annealed steel sheet or strip having excellent combination tensile strength and ductility at room temperature, and more particularly to the method of manufacturing the high strength cold rolled and annealed steel adaptable for manufacturing structural and safety components including, battery casing of automobiles.BACKGROUND
[0002] Conventional Steels, such as, IF (interstitial free), BH (bake hardenable), HSLA (high strength low alloy) etc., are well documented in the literature and have been analyzed from various aspects, such as, processing, mechanical behavior, microstructure, and texture, etc., (shown in image below). Their mechanical properties (e.g., strength and ductility) depend on the conventional strengthening mechanisms, which include grain refinement, solid solution strengthening, etc. Advanced high strength steels (AHSS) are multi-phase steels that utilize advance concept of deformation of the ‘composite’ microstructure along with the conventional strengthening mechanism to offer a better combination of mechanical properties.
[0003] Tensile Strength (MPa)
[0004] The AHSS family mainly includes Dual Phase (DP), Complex Phase(CP), Transformation Induced Plasticity (TRIP), Martensitic (MS or MART), andTwinning Induced Plasticity (TWIP) steels where apart from the conventional strengthening mechanism, composite effect is exploited to achieve improved balance between strength and formability. The microstructure of DP steel consists of a mixture of ferrite and martensite while complex phase steels have a mixture of ferrite, martensite, bainite with retained austenite in some cases. TRIP steels typically have some amount of retained austenite with different matrix phase(s), such as, ferrite, bainite and martensite, which transforms to martensite under the influence of stress (transformation induced plasticity (TRIP) effect) and improves balance between strength and ductility. TWIP steels have a fully austenitic microstructure that generates twins on the application of external stress and thereby gives better combination of strength and ductility.
[0005] Out of the different classes of steels described above, TRIP based steels are perhaps the most sought out and researched class. However, a minimum of amount of Si (> 1 wt %) has to be used in order to retain a viable amount of the retained austenite in the final micro structure and extract the benefit of high strength with better combination of elongation. Si is well known to create issues during casting and deteriorate the surface quality. These two factors have limited the application of such steels. An alternate approach has been proposed in this work which primarily utilizes the composite effect to achieve a better combination of strength and elongation. This had led to the development of a new class of steel, identified as, MB steel. Here, MB signifies that the microstructure is a mixture of martensite and bainite.
[0006] The present disclosure is directed to overcome one or more limitations stated above or any other limitation associated with the prior arts.OBJECTIVE OF INVENTION
[0007] It is an object of the invention to solve the problems of the prior art and to provide a new chemical composition, for cold rolled grade steel, for obtaining a microstructure majorly comprising mixture of martensite (M) and bainite (B) phases in the final micro structure. The developed steel is a new class of steel, identified as, MB steel.
[0008] Another objective of the present invention is to develop a high strength bendable steel grade with moderate amount of forming that can be made into steel strips, sheets, and blanks, having tensile strength above 1400 MPa with tensile elongation value over 7%.
[0009] Another objective of the present invention is to develop the high strength cold rolled and annealed steel adaptable for manufacturing automobile and structural components that require moderate amount of forming.
[0010] Another objective of present invention is to provide a new easier manufacturing method combining thermomechanical, hot rolling, cold rolling, and continuous annealing processes for the proposed chemical composition under controlled conditions.SUMMARY OF INVENTION
[0011] This summary is provided to introduce concepts related to a high strength cold rolled and annealed steel, and a method of manufacturing the high strength cold rolled and annealed steel sheet or strip. The concepts are further described below in the detailed description. This summary is not intended to identify key features or essential features of the claimed subject matter, nor is it intended to be used to limit the scope of the claimed subject matter.
[0012] In an embodiment, a high strength cold rolled and annealed steel is provided. The high strength cold rolled and annealed steel comprises the following composition expressed in weight %: Carbon (C): 0.25 - 0.35%, Manganese (Mn): 1.0% - 2.0%, Silicon (Si): 0.02%-0.5%, Sulphur (S): <0.006%, Phosphorus (P): < 0.02%, Aluminium (Al): 0.02-0.5%, Molybdenum (Mo): <0.3%, Nitrogen (N) < 80 ppm, and the remaining being substantially iron and incidental impurities. The high strength cold rolled and annealed steel comprises a microstructure of 10-30% bainite, and 70-90% martensite.
[0013] In an embodiment, the high strength cold rolled and annealed steel exhibits ultimate tensile strength (UTS) in the range of 1400-1800 MPa, yield strength (YS) - 1000-1300 MPa, minimum uniform elongation - 4 % and minimum total elongation - 7 %.
[0014] In an embodiment, the C content in the high strength cold rolled and annealed steel is kept optimum so as to improve the hardenability and hardness of martensite.
[0015] In an embodiment, the Mn content in the high strength cold rolled and annealed steel improves the hardenability further and delay the ferrite transformation.
[0016] In an embodiment, the Mo content improves hardenability of the steel and also enhances the kinetics of bainite formation during continuous annealing.
[0017] In another aspect of the present invention, a method for manufacturing a high strength cold rolled and annealed steel sheet or strip having thickness in the range of 0.5 mm to 2 mm is provided. The method comprises casting molten steel having a composition expressed in weight %: C - 0.25-0.35, Mn - 1.0-2.5, S < 0.006, P < 0.02, Si - 0.02-0.50, Al - 0.02-0.50, Mo - 0.00-0.30, N (ppm) < 80, and the balance being Iron (Fe) and unavoidable impurities to obtain a steel slab. The method also comprises reheating the steel slab to a temperature in the range of 1200 - 1280°C. The method further comprises roughing the steel slab in roughing mill with exit temperature in the range of 1000-1080°C. The method comprises hot rolling the roughed steel slab to produce a steel sheet such that finish rolling is done at a temperature (TFRT) varying in the range 83O°C to 88O°C. The method also comprises cooling the hot rolled steel to a first intermediate temperature in the range of 640 - 680°C at a first intermediate cooling rate in the range of 0.5°C / s - 50°C / s to obtain first intermediate hot rolled steel. The method further comprises coiling the first intermediate hot rolled steel at a coiling temperature in the range of 640 - 680°C. The method comprises pickling the first intermediate hot rolled steel to remove the scale on the steel strip surface. The method also comprises cold rolling the steel strip for further reduction in thickness to obtain cold rolled steel having predetermined thickness. The method further comprises heating the cold rolled steel from ambient temperature to first holding temperature in the range of 800-900°C at a heating rate <20 °C / s to obtain heated cold rolled steel. The method comprises holding the heated cold rolled steel in a furnace in a temperature range of 800-900°C for a time duration of 30 sec - 300 sec. The method also comprisescooling to a room temperature at a cooling rate in the range of 20°C / s - 60°C / s to obtain high strength cold rolled and annealed steel sheet or strip. The high strength cold rolled and annealed steel sheet comprises a micro structure of 10-30% bainite, and 70-90% martensite, wherein the high strength cold rolled and annealed steel exhibits an ultimate tensile strength in the range of 1400-1800 MPa.
[0018] In an embodiment, the high strength cold rolled and annealed steel comprises the composition expressed in weight %: C : 0.28 - 0.32 , Mn: 1.4 - 1.5, Si: 0.0 - 0.2, Al: 0.3 - 0.5, Mo: 0.25 - 0.27, and the balance being Iron (Fe) and unavoidable impurities, wherein the obtained high strength cold rolled and annealed steel exhibits a yield strength (YS) of 1000 - 1260 MPa, ultimate tensile strength (UTS) of 1630 - 1750 MPa, minimum uniform elongation of 4 - 5.2 %, yield ratio (YS / UTS): 0.72 - 0.75, and minimum total elongation of 7 - 9 %.
[0019] In an embodiment, the high strength cold rolled and annealed steel comprises the composition expressed in weight %: C - 0.28, Mn -1.4, Si -0.2, Al- 0.3, Mo - 0.27, and the balance being Iron (Fe) and unavoidable impurities, wherein the obtained high strength cold rolled and annealed steel exhibits a yield strength (YS) of 1188 MPa, ultimate tensile strength (UTS) of 1640 MPa, minimum uniform elongation - 5.2 % and minimum total elongation - 8.6 %.
[0020] In an embodiment, the high strength cold rolled and annealed steel comprises the composition expressed in weight %: C - 0.32, Mn -1.5, Si -0.2, Al- 0.3, Mo - 0.25, and the balance being Iron (Fe) and unavoidable impurities, wherein the obtained high strength cold rolled and annealed steel exhibits a yield strength (YS) of 1204 MPa, ultimate tensile strength (UTS) of 1660 MPa, minimum uniform elongation - 5.1 % and minimum total elongation - 8.8 %.
[0021] In an embodiment, the high strength cold rolled and annealed steel comprises the composition expressed in weight %: C - 0.28, Mn -1.5, Si -0.0, Al- 0.5, Mo - 0.25, and the balance being Iron (Fe) and unavoidable impurities, wherein the obtained high strength cold rolled and annealed steel exhibits a yield strength (YS) of 1147 MPa, ultimate tensile strength (UTS) of 1600 MPa, minimum uniform elongation - 5.1 % and minimum total elongation - 7.3 %.
[0022] In an embodiment, the high strength cold rolled and annealed steel comprises the composition expressed in weight %: C - 0.32, Mn -1.5, Si -0.0, Al - 0.5, Mo - 0.25, and the balance being Iron (Fe) and unavoidable impurities, wherein the obtained high strength cold rolled and annealed steel exhibits a yield strength (YS) of 1210 MPa, ultimate tensile strength (UTS) of 1660 MPa, minimum uniform elongation - 5.2 % and minimum total elongation - 7.7 %.
[0023] In an embodiment, a component produced from the high strength cold rolled and annealed steel is used in automobile applications.
[0024] Other features and aspects of this disclosure will be apparent from the following description and the accompanying drawings.BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 illustrates a flowchart of a method of manufacturing a high strength cold rolled and annealed steel, according to an embodiment of the present invention;
[0026] Figure 2a illustrates a graphical representation of stress versus elongation, obtained during tensile test of high strength cold rolled and annealed steel having composition of MB-1, according to an embodiment of the present invention;
[0027] Figure 2b illustrates a graphical representation of stress versus elongation, obtained during tensile test of high strength cold rolled and annealed steel having composition of MB -2, according to an embodiment of the present invention;
[0028] Figure 2c illustrates a graphical representation of stress versus elongation, obtained during tensile test of high strength cold rolled and annealed steel having composition of MB -3, according to an embodiment of the present invention;
[0029] Figure 2d illustrates a graphical representation of stress versus elongation, obtained during tensile test of high strength cold rolled and annealed steel having composition of MB -4, according to an embodiment of the present invention;
[0030] Figure 3a illustrates an optical image of the high strength cold rolled and annealed steel having composition of MB - 2, according to an embodiment of the present invention;
[0031] Figure 3b illustrates a SEM image of the high strength cold rolled and annealed steel having composition of MB - 2, according to an embodiment of the present invention; and
[0032] Figure 3c illustrates a SEM image of the high strength cold rolled and annealed steel having composition of MB - 4, according to an embodiment of the present invention.
[0033] The drawings referred to in this description are not to be understood as being drawn to scale except if specifically noted, and such drawings are only exemplary in nature.DETAILED DESCRIPTION
[0034] The detailed description of various exemplary embodiments of the disclosure is described herein with reference to the accompanying drawings. It should be noted that the embodiments are described herein in such details as to clearly communicate the disclosure. However, the amount of details provided herein is not intended to limit the anticipated variations of embodiments; on the contrary, the intention is to cover all modifications, equivalents, and alternatives falling within the spirit and scope of the present disclosure as defined by the appended claims.
[0035] It is also to be understood that various arrangements may be devised that, although not explicitly described or shown herein, embody the principles of the present disclosure. Moreover, all statements herein reciting principles, aspects, and embodiments of the present disclosure, as well as specific examples, are intended to encompass equivalents thereof.
[0036] The terminology used herein is for the purpose of describing particular embodiments only and is not intended to be limiting of example embodiments. As used herein, the singular forms “a”, “an” and “the” are intended to include the plural forms as well, unless the context clearly indicates otherwise. It will be furtherunderstood that the terms “comprises”, “comprising”, “includes” and / or “including,” when used herein, specify the presence of stated features, integers, steps, operations, elements and / or components, but do not preclude the presence or addition of one or more other features, integers, steps, operations, elements, components and / or groups thereof.
[0037] It should also be noted that in some alternative implementations, the functions / acts noted may occur out of the order noted in the figures. For example, two figures shown in succession may, in fact, be executed concurrently or may sometimes be executed in the reverse order, depending upon the functionality / acts involved.
[0038] Unless otherwise defined, all terms (including technical and scientific terms) used herein have the same meaning as commonly understood by one of ordinary skill in the art to which example embodiments belong. It will be further understood that terms, e.g., those defined in commonly used dictionaries, should be interpreted as having a meaning that is consistent with their meaning in the context of the relevant art and will not be interpreted in an idealized or overly formal sense unless expressly so defined herein.
[0039] The present disclosure provides a high strength cold rolled and annealed steel adaptable for manufacturing structural and safety components including, battery casing of automobiles. The high strength cold rolled and annealed steel comprises the following composition expressed in weight %: Carbon (C): 0.25 - 0.35%, Manganese (Mn): 1.0% - 2.0%, Silicon (Si): 0.02%-0.5%, Sulphur (S): <0.006%, Phosphorus (P): < 0.02%, Aluminium (Al): 0.02-0.5%, Molybdenum (Mo): <0.3%, Nitrogen (N) < 80 ppm, and the remaining being substantially iron and incidental impurities.
[0040] The high strength cold rolled and annealed steel comprises a structure including a bainitic phase, and martensite phase. In an embodiment, the high strength cold rolled and annealed steel comprises a micro structure of 10-30% bainite, and 70-90% martensite. The high strength cold rolled and annealed steel exhibits an ultimate tensile strength (UTS) in the range of 1400-1800 MPa, yieldstrength (YS) - 1000-1300 MPa, minimum uniform elongation - 4 % and minimum total elongation - 7 %.
[0041] In one embodiment, the high strength cold rolled and annealed steel comprises C - 0.28-0.32, Mn -1.4- 1.5, Si - 0.0-0.2, Al - 0.3-0.5, Mo - 0.25 - 0.27, and the balance being Iron (Fe) and unavoidable impurities.
[0042] The high strength cold rolled and annealed steel exhibits yield strength (YS) in the range of 1000-1260 MPa, ultimate tensile strength (UTS) in the range of 1430-1750 MPa, %Elongation in the range of 7-9%, uniform elongation in the range of 4-5%, and yield ratio (YS / UTS) in the range of 0.7-0.75.
[0043] Referring to Figure 1, an exemplary thermo-mechanical method (100) of manufacturing the high strength cold rolled and annealed steel strip, sheet or blank is illustrated. Each step shown in figure 1 represents one or more process, method or subroutine steps carried out in the method. Furthermore, the order of blocks is illustrative only and the blocks can change in accordance with the present disclosure. Additional blocks can be added, or fewer blocks can be utilized, without departing from this disclosure. The method (100) for manufacturing the high strength cold rolled and annealed steel strip, sheet or blank begins at step (102). At step (102), molten steel having composition expressed in weight %: C - 0.25-0.35, Mn - 1.0-2.5, S < 0.006, P < 0.02, Si - 0.02-0.50, Al - 0.02-0.50, Mo - 0.00-0.30, N (ppm) < 80, and the balance being Iron (Fe) and unavoidable impurities is cast in a casting apparatus to obtain a steel slab.
[0044] At step (104), the steel slab (cast ingots) is reheated inside a furnace kept at a temperature in the range of 1200 - 1280 °C. More preferably, in the range of 1200-1250°C. In the preferred embodiment, the steel slab is reheated to a temperature of 1200 °C.
[0045] At step (106), the heated steel slab obtained in the step (104) is rolled / deformed in the roughing mill with exit temperature in the range of 1000- 1080°C. In the preferred embodiment, the exit temperature is 1070 °C.
[0046] At step (108), the roughed steel slab obtained in step (106) is subjected to a hot working process such as hot rolling process such that finish rolling is doneat a temperature (TFRT) to obtain a hot rolled steel sheet or strip. TFRT varies in the range 83O°C to 88O°C, above Ara temperature of the steel. The hot rolling process may be carried out by passing the steel through a pair of rolls and rolling may be carried out for at least five passes to reduce the thickness of the steel to required size in the range of 2-6 mm. In an embodiment, the hot rolling process is performed by passing the steel through a pair of rolls and rolling is carried out for at least 5 passes.
[0047] At step (110), the hot rolled steel sheet or strip obtained in step (108) is cooled to a first intermediate temperature in the range of 640 - 680°C at a first intermediate cooling rate in the range of 0.5°C / s - 50°C / s to obtain first intermediate hot rolled steel sheet or strip.
[0048] At step (112), the first intermediate hot rolled steel sheet or strip is coiled thereafter at 640 - 680°C. At step (114), the first intermediate hot rolled steel is pickled to remove the scale on the steel sheet or strip surface.
[0049] At step (116), the pickled steel sheet or strip is cold rolled to further reduce the thickness. The pickled hot rolled strip is fed into an industrial cold rolling mill, which may either be a multi- stand tandem rolling mill, or a singlestand / two-stand reversing rolling mill. A state-of-the-art pickling facility, coupled with a multi-stand tandem cold rolling mill, along with its usual accessories like entry welding section, looper sections at the different positions (entry, after pickling, etc.) would be the most desirable option. In the preferred embodiment, the cold rolling reduction is in the range of 50-60%.
[0050] At step (118), the cold rolled steel sheet or strip is heated from ambient temperature to first holding temperature in the range of 800-900°C at a heating rate < 20°C / s to obtain heated cold rolled steel sheet or strip.
[0051] At step (120), the heated cold rolled steel is held in a furnace at a first holding temperature in the range of 800-900°C for a time duration of 30 sec - 300 sec to obtain a soaked and cold rolled steel.
[0052] At step (122), the soaked cold rolled steel sheet or strip is cooled to at a cooling rate in the range of 20°C / s - 60°C / s to obtain high strength cold rolled andannealed steel sheet or strip having thickness in the range of 0.5 mm to 2 mm. The obtained high strength cold rolled and annealed steel sheet or strip comprises a microstructure of 10-30% bainite, and 70-90% martensite. The high strength cold rolled and annealed steel exhibits an ultimate tensile strength in the range of 1400- 1800 MPa.
[0053] A fine hot band grain size is desirable, which may be achieved by austenite pancaking during hot rolling, by substantial deformation of austenite below Tnr temperature. The hot deformation schedule should ensure a substantial amount of deformation (about 50%) under Tm. Immediately after finish rolling, there should be a rapid drop of temperature, to restrict grain growth. Finally, the hot rolled strip may be coiled at a moderate coiling temperature, without any special treatment.
[0054] The cold rolling deformation should be in the range 50-60%, depending on final thickness requirement. The cold rolled steel is subjected to annealing treatment, preferably with continuous annealing facility, as the formation of transformed phases would require faster cooling rate, which is difficult to achieve with batch annealing type facility using a lean chemical composition.
[0055] The annealing treatment should include mainly the following steps:
[0056] The holding at the intermediate annealing temperature (first holding temperature) should be followed by a rapid cooling, to transform the freshly formed austenite to harder phases, such as bainite or martensite. The steel is first cooled rapidly to a temperature, which is above the martensitic transformation temperature, but below the bainitic transformation temperature. Holding at this temperature for a certain duration of time would facilitate transformation of austenite into bainite phase. This may be a partial transformation, after which, another rapid cooling to room temperature would ensure the transformation of remaining austenite into martensite.
[0057] The method (100) of the present disclosure includes melting, casting, heat treatment, thermomechanical hot-rolled routes, cold rolling and annealing which are simple. Slab drop-out temperature, finish rolling temperature, coilingtemperature, annealing temperatures, holding temperature and time, and all have significant effects on final mechanical properties.
[0058] Following portions of the present disclosure provides details about the proportion of each element in a composition of the high strength cold rolled and annealed steel and their role in enhancing properties.
[0059] Carbon (C) may be used in the range of about 0.25-0.35 wt.%: Carbon is cheapest and most effective element that improves the hardenability and hardness of martensite.
[0060] Manganese (Mn): 1.0 to 2.0 wt .%: Manganese was selected to improve the hardenability further and delay the ferrite transformation. This exposes the bainite and martensite area in the continuous cooling diagram.
[0061] Si + Al: 0 - 1 wt %: Silicon and Aluminum are effective elements that delay the carbide precipitation. It ensures that a higher level of carbon remains in solid solution in martensite giving it higher strength.
[0062] Molybdenum (Mo): 0.1 - 0.30 wt %: Molybdenum was selected so that bainite could be formed over larger processing windows during cooling.
[0063] Sulphur (S) may be used in the range of about < 0.005 wt.%, & Phosphorus (P) may be used in the range of about < 0.03 wt.%: Amounts of Sulphur and phosphorus are kept as low as possible. The Sulphur content has to be limited otherwise it results in a very high inclusion level that deteriorates formability. Phosphorus content should be restricted to 0.03% maximum as higher phosphorus levels can lead to reduction in toughness and weldability due to segregation of P into grain boundaries.
[0064] Nitrogen (N) may be used less than 0.008%. Too high a N content makes the steel brittle.
[0065] Micro structure:
[0066] The phases present and their attributes in the final microstructure are the key factors that decides the final mechanical properties of the steel. The target microstructure after the continuous annealing treatment was a mixture of martensite and bainite. When bainite forms, a part of carbon is released frombainite to the remaining austenite. The carbon enriched remaining austenite then transforms to martensite on further cooling to the room temperature. Martensite being a harder phase imposes stress on bainite which then interacts with the external stresses (for example during the uniaxial tensile test) and effectively gives excellent combination of strength and ductility.
[0067] Examples:
[0068] Further embodiments of the present disclosure will be now described with examples of a particular composition of the steel. Experiments have been carried out on the steel with different composition values from the aforementioned ranges by using method of the present disclosure. Results have been compared on various fronts to show the improvement of strength of the steel.
[0069] The chemical composition of the proposed alloys are shown in Table 1.Table -1: Chemical compositions of Martensite-Bainitic steel
[0070] To investigate the properties of the steel, experiments were carried out for specific composition which is reported in Table 1. Tensile specimens were prepared according to ASTM E8 specification, applicable for specimens with thickness 1 - 1.5 mm, and gauge length 25 mm (Heat 1 and Heat 2) and 50 mm (Heat 3 and Heat 4). SEM samples were prepared by following standard methods.
[0071] Different samples of the high strength cold rolled and annealed steel were prepared by utilizing the compositions as mentioned in table 1 followed during the method (100). Other parameters were kept constant (reheating - 1200 deg C, finishrolling - 850 deg C, first intermediate temperature - 640 deg C, coiling temperature - 640 deg C, and cold rolling reduction - 50 - 60 %).
[0072] Standard techniques were followed to prepare the samples for different mechanical properties measurements. The measured properties for the steel samples are depicted in Table 2.Table 2: Measured mechanical properties of different samples with varying composition.
[0073] Now referring to Figures 2a - 2d, which are exemplary embodiments of the present disclosure illustrating a graph with stress versus elongation plot obtained during tensile test of the steel samples as per Table 1 above. The tensile test may be carried using standard tensile test samples. As an example, the test sample may be with a gauge length of 25mm and E8 / E8M-09 configuration, in accordance with ASTM standards. As evident from the graph illustrated in Figure. 2a, the high strength cold rolled and annealed steel with composition of MB-1 exhibits a yield strength (YS) of 1188 MPa, ultimate tensile strength (UTS) of 1640MPa, minimum uniform elongation - 5.2 % and minimum total elongation - 8.6 %. Now referring to, Figure 2b, the steel with composition of MB-2 exhibits a yield strength (YS) of 1204 MPa, ultimate tensile strength (UTS) of 1660 MPa, minimum uniform elongation - 5.1 % and minimum total elongation - 8.8 %. Nowreferring to, Figure 2c, the steel with composition of MB-3 which does not comprise Si in the composition exhibits a yield strength (YS) of 1147 MPa, ultimate tensile strength (UTS) of 1600 MPa, minimum uniform elongation - 5.1 % and minimum total elongation - 7.3 %. Now referring to, Figure 2d, the steel with composition of MB-4 which does not comprise Si in the composition exhibits a yield strength (YS) of 1210 MPa, ultimate tensile strength (UTS) of 1660 MPa, minimum uniform elongation - 5.2 % and minimum total elongation - 7.7 %.
[0074] From, the table-2 and Figures 2a - 2d, it is significant to note that the strength > 1500 MPa combined with a total elongation > 7 % is achieved. More importantly, there is significant post-uniform elongation which would offer the better safety to the component made from the developed steel.
[0075] Figure 3a illustrates optical image of the high strength cold rolled and annealed steel with composition of MB -2 and Figure 3b illustrates SEM image of the obtained high strength cold rolled and annealed steel with composition of MB- 2 reported in Table 1. Figure 3c illustrates SEM image of the obtained high strength cold rolled and annealed steel with composition of MB-4 reported in Table 1. From the figures 3b and 3c, it can be observed that the developed steels exhibits microstructure having bainite, and martensite. The major strength and ductility of the steels is coming from the phase mixture of bainite, and martensite.
[0076] The present invention provides the high strength cold rolled and annealed steel and the method (100) of manufacturing the high strength cold rolled and annealed steel having higher strength with bare minimum addition of alloying elements. The high strength cold rolled and annealed steel is a martensite and bainite steel which makes an important contribution towards the cost effective, futuristic, and strategic light weight application of steel with greater factor of safety. The high strength cold rolled and annealed steel having high strength and superior tensile ductility at room temperature, is specifically required for the automotive and structural applications. The thermo mechanical / hot-rolling process is quite simple and does not require huge energy consumption. Therefore, the method (100) of the present disclosure aids in reducing energy consumption and thus a cost-effective steel manufacturing process. Further, the method (100)provides a new steel developed with leaner chemistry to achieve the required properties by exploiting the existing hot rolling facilities in the integrated steel plants to get desired micro structure.
[0077] It should be understood that the experiments are carried out for particular compositions of the high strength cold rolled and annealed steel reported in Table 1 and the results brought out are reported in Table 2. However, this composition should not be construed as a limitation to the present disclosure as it could be extended to other compositions of the low carbon cold rolled complex phase steel strip, as well.
[0078] Furthermore, the terminology used herein is for describing embodiments only and is not intended to be limiting of the present disclosure. It will be appreciated that several of the above-disclosed and other features and functions, or alternatives thereof, may be combined into other systems or applications. Various presently unforeseen or unanticipated alternatives, modifications, variations, or improvements therein may subsequently be made by those skilled in the art without departing from the scope of the present disclosure as encompassed by the following claims.
[0079] The claims, as originally presented and as they may be amended, encompass variations, alternatives, modifications, improvements, equivalents, and substantial equivalents of the embodiments and teachings disclosed herein, including those that are presently unforeseen or unappreciated, and that, for example, may arise from applicants / patentees and others.
[0080] While the foregoing describes various embodiments of the invention, other and further embodiments of the invention may be devised without departing from the basic scope thereof. The scope of the invention is determined by the claims that follow. The invention is not limited to the described embodiments, versions, or examples, which are included to enable a person having ordinary skill in the art to make and use the invention when combined with information and knowledge available to the person having ordinary skill in the art.
Claims
CLAIMSWe Claim:
1. A high strength cold rolled and annealed steel comprising the following composition expressed in weight %:Carbon (C): 0.25 - 0.35%,Manganese (Mn): 1.0% - 2.0%,Silicon (Si): 0.02%-0.5%,Sulphur (S): <0.006%Phosphorus (P): < 0.02%Aluminium (Al): 0.02-0.5%,Molybdenum (Mo): <0.3%Nitrogen (N) < 80 ppm, and the remaining being substantially iron and incidental impurities, wherein the high strength cold rolled and annealed steel comprises a microstructure of 10-30% bainite, and 70-90% martensite.
2. The high strength cold rolled and annealed steel as claimed in the claim 1, wherein the high strength cold rolled and annealed steel exhibits ultimate tensile strength (UTS) in the range of 1400-1800 MPa, yield strength (YS) - 1000-1300 MPa, minimum uniform elongation - 4 % and minimum total elongation - 7 %.
3. The high strength cold rolled and annealed steel as claimed in the claim 1, wherein the C content in the high strength cold rolled and annealed steel is kept optimum so as to improve the hardenability and hardness of martensite.
4. The high strength cold rolled and annealed steel as claimed in the claim 1, wherein the Mn content in the high strength cold rolled and annealed steel improves the hardenability further and delay the ferrite transformation.
5. The high strength cold rolled and annealed steel as claimed in the claim 1, wherein the Mo content improves hardenability of the steel and also enhances the kinetics of bainite formation during continuous annealing.A method (100) for manufacturing a high strength cold rolled and annealed steel sheet or strip having thickness in the range of 0.5 mm to 2 mm, the method (100) comprising: casting molten steel having a composition expressed in weight %: C - 0.25-0.35, Mn - 1.0-2.5, S < 0.006, P < 0.02, Si - 0.02-0.50, Al - 0.02- 0.50, Mo - 0.00-0.30, N (ppm) < 80, and the balance being Iron (Fe) and unavoidable impurities to obtain a steel slab; reheating the steel slab to a temperature in the range of 1200 - 1280°C; roughing the steel slab in roughing mill with exit temperature in the range of 1000-1080°C; hot rolling the roughed steel slab to produce a steel sheet such that finish rolling is done at a temperature (TFRT), wherein TFRT varies in the range 83O°C to 88O°C; cooling the hot rolled steel to a first intermediate temperature in the range of 640 - 680°C at a first intermediate cooling rate in the range of 0.5°C / s - 50°C / s to obtain first intermediate hot rolled steel; coiling the first intermediate hot rolled steel at a coiling temperature in the range of 640 - 680°C; pickling the first intermediate hot rolled steel to remove the scale on the steel strip surface; cold rolling the steel strip for further reduction in thickness to obtain cold rolled steel having predetermined thickness; heating the cold rolled steel from ambient temperature to first holding temperature in the range of 800-900°C at a heating rate <20 °C / s to obtain heated cold rolled steel; holding the heated cold rolled steel in a furnace in a temperature range of 800-900°C for a time duration of 30 sec - 300 sec; cooling to a room temperature at a cooling rate in the range of 20°C / s - 60°C / s to obtain high strength cold rolled and annealed steel sheet or strip, wherein the high strength cold rolled and annealed steel sheet comprises a microstructure of 10-30% bainite, and 70-90% martensite,wherein the high strength cold rolled and annealed steel exhibits an ultimate tensile strength in the range of 1400-1800 MPa.
7. The method (100) for manufacturing the high strength cold rolled and annealed steel sheet or strip having thickness in the range of 0.5 mm to 2 mm as claimed in the claim 6, wherein the high strength cold rolled and annealed steel comprises the composition expressed in weight %: C : 0.28 - 0.32 , Mn: 1.4 - 1.5, Si: 0.0 - 0.2, Al: 0.3 - 0.5, Mo: 0.25 - 0.27, and the balance being Iron (Fe) and unavoidable impurities, wherein the obtained high strength cold rolled and annealed steel exhibits a yield strength (YS) of 1000 - 1260 MPa, ultimate tensile strength (UTS) of 1630 - 1750 MPa, minimum uniform elongation of 4 - 5.2 %, yield ratio (YS / UTS): 0.72 - 0.75, and minimum total elongation of 7 - 9 %.
8. The method (100) for manufacturing the high strength cold rolled and annealed steel sheet or strip having thickness in the range of 0.5 mm to 2 mm as claimed in the claim 7, wherein the high strength cold rolled and annealed steel comprises the composition expressed in weight %: C - 0.28, Mn -1.4, Si -0.2, Al - 0.3, Mo - 0.27, and the balance being Iron (Fe) and unavoidable impurities, wherein the obtained high strength cold rolled and annealed steel exhibits a yield strength (YS) of 1188 MPa, ultimate tensile strength (UTS) of 1640 MPa, minimum uniform elongation - 5.2 % and minimum total elongation - 8.6 %.
9. The method (100) for manufacturing the high strength cold rolled and annealed steel sheet or strip having thickness in the range of 0.5 mm to 2 mm as claimed in the claim 7, wherein the high strength cold rolled and annealed steel comprises the composition expressed in weight %: C - 0.32, Mn -1.5, Si -0.2, Al - 0.3, Mo - 0.25, and the balance being Iron (Fe) and unavoidable impurities, wherein the obtained high strength cold rolled and annealed steel exhibits a yield strength (YS) of 1204 MPa, ultimate tensile strength (UTS) of 1660 MPa, minimum uniform elongation - 5.1 % and minimum total elongation - 8.8 %.
10. The method (100) for manufacturing the high strength cold rolled and annealed steel sheet or strip having thickness in the range of 0.5 mm to 2mm as claimed in the claim 7, wherein the high strength cold rolled and annealed steel comprises the composition expressed in weight %: C - 0.28, Mn -1.5, Si -0.0, Al - 0.5, Mo - 0.25, and the balance being Iron (Fe) and unavoidable impurities, wherein the obtained high strength cold rolled and annealed steel exhibits a yield strength (YS) of 1147 MPa, ultimate tensile strength (UTS) of 1600 MPa, minimum uniform elongation - 5.1 % and minimum total elongation - 7.3 %.
11. The method (100) for manufacturing the high strength cold rolled and annealed steel sheet or strip having thickness in the range of 0.5 mm to 2 mm as claimed in the claim 7, wherein the high strength cold rolled and annealed steel comprises the composition expressed in weight %: C - 0.32, Mn -1.5, Si -0.0, Al - 0.5, Mo - 0.25, and the balance being Iron (Fe) and unavoidable impurities, wherein the obtained high strength cold rolled and annealed steel exhibits a yield strength (YS) of 1210 MPa, ultimate tensile strength (UTS) of 1660 MPa, minimum uniform elongation - 5.2 % and minimum total elongation - 7.7 %.
12. A component produced from the high strength cold rolled and annealed steel as claimed in the claims 1 to 11, wherein the component is used in automobile applications.
Citation Information
Patent Citations
A hot-pressed member with excellent ductility, a steel sheet for the hot-pressed member, and a method for manufacturing the hot-pressed member.
JP5369714B2
High-yield-ratio high-strength electrogalvanized steel sheet and method for manufacturing the same
US20210381085A1
High-strength member, method for manufacturing high-strength member, and method for manufacturing steel sheet for high-strength member
US20220010414A1
Steel sheet
US20220275493A1
Ultra-high strength hot-rolled steel sheet having excellent bending processability and method for manufacturing same
WO2018117552A1
Cited By
Battery shell steel, preparation method and battery
CN121514273A