The introduction of a biaxially oriented SiC layer with controlled dislocation distribution in SiC substrates addresses the processing challenges of SiC substrates, reducing cracks and improving yield by ensuring uniform dislocation distribution and reduced high-density dislocation areas, thus enhancing substrate reliability.
Patent Information
- Application Number
- PCT/JP2023/040962
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-28
- Filing Date
- 2023-11-14
- Publication Date
- 2024-10-03
AI Technical Summary
SiC substrates are challenging to process due to their hardness and high dislocation density, leading to cracks during grinding, polishing, and cutting, which reduces yield and affects the reliability of SiC power devices.
A SiC substrate with a biaxially oriented SiC layer, characterized by uniform distribution of basal plane dislocations, screw dislocations, and edge dislocations, reducing the occurrence of cracks and improving processing yield through controlled rare earth element concentration and orientation.
The biaxially oriented SiC layer minimizes strain and crack formation during substrate processing, enhancing the manufacturing yield and reliability of SiC substrates by ensuring uniform dislocation distribution and reduced high-density dislocation areas.
Smart Images

Figure JP2023040962_03102024_PF_FP_ABST
Abstract
Description
SiC substrate and SiC composite substrate
[0001] The present invention relates to a SiC substrate and a SiC composite substrate.
[0002] SiC (silicon carbide) has attracted attention as a wide-bandgap material capable of controlling high voltages and high power with low loss. In particular, in recent years, power semiconductor devices using SiC materials (SiC power devices) are expected to be used in a variety of applications because they are more compact, consume less power, and are more efficient than those using Si semiconductors. For example, the adoption of SiC power devices can reduce the size and improve the efficiency of converters, inverters, on-board chargers, etc. for electric vehicles (EVs) and plug-in hybrid vehicles (PHEVs). Therefore, the development of SiC wafers, which form the backbone of SiC power devices, has attracted considerable attention.
[0003] To fabricate a SiC power device, it is necessary to epitaxially grow a SiC single crystal on a SiC single crystal substrate. The resulting SiC single crystal substrate contains many dislocations, which can be broadly classified into three types: basal plane dislocations (BPDs), threading screw dislocations (TSDs), and edge dislocations (TEDs). Among these dislocations, basal plane dislocations are inherited by the epitaxially grown film. If present in the drive region of the device, they expand into stacking faults upon current application, adversely affecting the reliability of the SiC device. Regarding these dislocations, Patent Document 1 (Japanese Patent No. 6192948) discloses a SiC single crystal having regions where edge dislocations are unevenly distributed and regions where basal plane dislocations are unevenly distributed. It is described that such a SiC single crystal can suppress performance degradation caused by specific dislocation types. Patent Document 2 (Japanese Patent No. 5750363) describes a volume density of dislocations (mainly basal plane dislocations and threading edge dislocations) having a Burgers vector in the {0001} plane direction of 3700 cm / cm 3A SiC single crystal containing the following low dislocation density region is disclosed. It is also known that breakage and cracks occur when processing SiC single crystal substrates. In this regard, Non-Patent Document 1 (Y. Qiusheng, C. Senkai and P. Jisheng, "Surface and subsurface cracks characteristics of single crystal SiC wafer in surface machining," AIP Conference Proceedings 1653, 020091 (2015)) describes an analysis of the characteristics of cracks that occur on the wafer surface after various processing steps are performed on single crystal SiC wafers.
[0004] Patent No. 6192948 Patent No. 5750363
[0005] Y. Qiusheng, C. Senkai and P. Jisheng, “Surface and subsurface cracks characteristics of single crystal SiC wafer in surface machining,” AIP Conference Proceedings 1653, 020091 (2015)
[0006] According to the disclosure of Non-Patent Document 1, SiC is extremely hard and therefore difficult to process, and a reduction in yield due to fractures and cracks that occur during wafer grinding, polishing, cutting, etc., has become an issue. Although the direct cause has not been clarified, strain within the crystal, such as plastic deformation due to dislocations, may be involved. In this regard, the dislocations present in the SiC single crystals disclosed in Patent Documents 1 and 2 are thought to be distributed unevenly, and in this case, fractures and cracks are likely to occur during substrate processing, such as grinding, polishing, and cutting of the SiC substrate.
[0007] The present inventors have now discovered that by providing a SiC substrate with a biaxially oriented SiC layer with few regions where BPDs are extremely abundant (i.e., with a uniform distribution of BPDs), strain within the crystal of the SiC substrate is reduced, thereby reducing breakage and cracks that may occur during substrate processing such as grinding, polishing, and cutting.
[0008] Therefore, an object of the present invention is to provide a SiC substrate that can reduce breakage and cracks during substrate processing.
[0009] The present invention provides the following aspects: [Aspect 1] A SiC substrate having a biaxially textured SiC layer, wherein, in an XRT image obtained by X-ray topography (XRT) measurement of the biaxially textured SiC layer, when the entire area of the XRT image is divided into a grid pattern with a region of 4 mm length × 4 mm width × 28 μm depth per square, the average value of the volume density of basal plane dislocations (BPDs) per square is X (cm / cm 3 ) and 5X (cm / cm) per square 3 ) or more in no region extending in a straight line in the vertical or horizontal direction is 10 or more consecutive squares. [Aspect 2] In the XRT image, 3 ) or more does not extend over five or more consecutive squares in a straight line either vertically or horizontally. [Aspect 3] When the entire area of the XRT image is divided into a lattice pattern with a vertical area of 4 mm x horizontal area per square, the average value of the number density of screw dislocations (TSDs) per square is expressed as Y ( / cm 2 ) and 2Y ( / cm 2 ) or more does not extend over 10 or more consecutive squares in a straight line either vertically or horizontally. [Aspect 4] When the entire area of the XRT image is divided into a grid pattern with a vertical area of 4 mm x horizontal area per square, the average value of the number density of edge dislocations (TEDs) per square is Z ( / cm 2 ) and 2Z ( / cm 2 ) or more, the number of consecutive squares is not 10 or more in a straight line either vertically or horizontally. [Aspect 5] The SiC substrate according to any one of Aspects 1 to 3. 3 The SiC substrate according to any one of Aspects 1 to 4. [Aspect 6] The rare earth element concentration of the biaxially textured SiC layer is 2.0 × 10 14 ~5.0 x 10 15 atoms / cm 3The SiC substrate according to any one of Aspects 1 to 5. [Aspect 7] A SiC composite substrate comprising a SiC single crystal substrate and the SiC substrate according to any one of Aspects 1 to 6 on the SiC single crystal substrate.
[0010] 1 is a longitudinal cross-sectional view of a SiC composite substrate 10; FIG. 2 is a diagram illustrating a manufacturing process for the SiC composite substrate 10; and FIG. 3 is a conceptual diagram illustrating the configuration of an aerosol deposition (AD) apparatus 50. In the sample of Example 1, 5X (cm / cm) per square was measured from the XRT image. 3 ) or more, and the area is displayed as a black square.
[0011] The SiC substrate according to the present invention includes a biaxially textured SiC layer. In an XRT image obtained by measuring the biaxially textured SiC layer by X-ray topography (XRT), when the entire XRT image is divided into a grid pattern with each grid having a size of 4 mm in length, 4 mm in width, and 28 μm in depth, the average value of the volume density of basal plane dislocations (BPDs) per grid is X (cm / cm). 3 At this time, the biaxially oriented SiC layer has a thickness of 5X (cm / cm) per square. 3 ) or more do not extend in a straight line of 10 or more cells in either the vertical or horizontal direction. Note that "does not extend in a straight line of 10 or more cells in either the vertical or horizontal direction" means that only the number of cells that extend in a straight line vertically and the number of cells that extend in a straight line horizontally are counted, and the number of cells that extend in a straight line diagonally is not counted. In this way, by providing a SiC substrate with a biaxially oriented SiC layer that has few regions with extremely high BPDs (i.e., a uniform distribution of BPDs), strain within the crystal of the SiC substrate is reduced, and breakage and cracks during substrate processing such as grinding, polishing, and cutting can be reduced.
[0012] As mentioned above, SiC is extremely hard and therefore difficult to process, and a reduction in yield due to fractures and cracks that occur during wafer grinding, polishing, cutting, etc., is an issue. In this regard, if dislocations present in a SiC substrate are unevenly distributed, fractures and cracks are likely to occur during substrate processing such as grinding, polishing, and cutting of the SiC substrate. In this regard, the present invention advantageously solves such problems, thereby improving the yield during SiC substrate manufacturing.
[0013] In the biaxially oriented SiC layer of the SiC substrate of the present invention, when the entire XRT image is divided into a grid pattern with a length of 4 mm, a width of 4 mm, and a depth of 28 μm per grid, the average value of the volume density of BPD per grid is X (cm / cm 3 ) and 5X (cm / cm) per square 3 ) or more in a row of 10 or more consecutive squares, preferably 5 or more consecutive squares, and more preferably 2 or more consecutive squares. 3 ) or more in a row of not more than five cells in a row, more preferably not more than four cells, and even more preferably not more than three cells. By reducing the number of regions with an extremely high BPD content in this way, it is possible to more effectively reduce breakage and cracks during substrate processing. In addition, the average value X of the volume density of BPD per cell is 200 to 5000 cm / cm. 3 It is preferable that:
[0014] In the XRT image obtained by XRT measurement, when the entire XRT image is divided into a grid pattern with a region of 4 mm length x 4 mm width per square, the average value of the number density of TSDs per square is Y ( / cm 2 ) and 2Y ( / cm 2 ) or more in a row of 10 or less cells in either a vertical or horizontal line, and more preferably, 6 or less cells in a row. By reducing the number of cells with an extremely high number of TSDs in this way, it is possible to more effectively reduce breakage and cracks during substrate processing. In addition, the average value Y of the number density of TSDs per cell is 100 to 800 / cm 2 It is preferable that:
[0015] In the XRT image obtained by XRT measurement, when the entire XRT image is divided into a grid pattern with a region of 4 mm length x 4 mm width per square, the average value of the number density of TEDs per square is Z ( / cm 2 ) and 2Z ( / cm 2) or more in a row of 10 or less squares in either a vertical or horizontal direction, and more preferably, 4 or less squares in a row. By reducing the number of areas with an extremely high number of TEDs in this way, it is possible to more effectively reduce breakage and cracks during substrate processing. In addition, the average value Z of the number density of TEDs per square is 1000 to 8000 / cm 2 It is preferable that:
[0016] The SiC substrate or the biaxially oriented SiC layer may have an off-axis angle, and in that case, the off-axis angle is preferably 0.1 to 12°, more preferably 1 to 5°, from the
[0001] axis of the SiC substrate or the biaxially oriented SiC layer.
[0017] The biaxially oriented SiC layer preferably contains a rare earth element, examples of which include Y, La, Ce, Pr, Nd, Pm, Sm, Eu, Gd, Tb, Dy, Ho, Er, Tm, Yb, Lu, Sc, and combinations thereof. From the viewpoint of reducing breakage and cracks, the rare earth element is preferably Y.
[0018] When the biaxially oriented SiC layer contains a rare earth element, the rare earth element concentration of the biaxially oriented SiC layer is 2.0×10 14 ~5.0 x 10 15 atoms / cm 3 is preferably 5.0 × 10 14 ~2.0 x 10 15 atoms / cm 3 By setting the concentration of the rare earth element within the above range, it is possible to effectively obtain a biaxially oriented SiC layer with few regions where BPDs are extremely abundant.
[0019] The biaxially oriented SiC layer is preferably oriented in the c-axis and a-axis directions. Furthermore, the SiC substrate is preferably composed of a biaxially oriented SiC layer. The biaxially oriented SiC layer may be a SiC single crystal, a SiC polycrystal, or a mosaic crystal, as long as it is oriented in the two axes of the c-axis and the a-axis. A mosaic crystal is a collection of crystals that do not have clear grain boundaries but whose crystal orientations, along either the c-axis or the a-axis, are slightly different. The method for evaluating the orientation is not particularly limited, and known analytical techniques such as EBSD (Electron Backscatter Diffraction Patterns) and X-ray pole figures can be used. For example, when using the EBSD method, inverse pole figure mapping of the surface (plate surface) of the biaxially oriented SiC layer or a cross section perpendicular to the plate surface can be measured. In the obtained inverse pole figure mapping, when the following four conditions are satisfied, the biaxially oriented SiC layer can be defined as being oriented in two directions, namely, the approximately normal direction and the approximately in-plane direction: (A) the first axis, (B) the second axis, (C) the tilt angle from the first axis is distributed within ±10°; and (D) the tilt angle from the second axis is distributed within ±10°. In other words, when the above four conditions are satisfied, the biaxially oriented SiC layer is determined to be oriented in two directions, namely, the c-axis and the a-axis. For example, when the approximately normal direction to the plate surface is oriented to the c-axis, the approximately in-plane direction may be oriented in a specific direction (e.g., the a-axis) perpendicular to the c-axis. The biaxially oriented SiC layer may be oriented in two directions, namely, the approximately normal direction and the approximately in-plane direction, but it is preferable that the approximately normal direction is oriented to the c-axis. The smaller the tilt angle distribution in the approximately normal direction and / or the approximately in-plane direction, the smaller the mosaic property of the biaxially oriented SiC layer, and the closer it is to zero, the closer it is to a single crystal. Therefore, from the viewpoint of the crystallinity of the biaxially oriented SiC layer, it is preferable that the tilt angle distribution be small in both the approximately normal direction and the approximately in-plane direction, for example, ±5° or less is more preferable, and ±3° or less is even more preferable.
[0020] SiC Composite Substrate The SiC substrate of the present invention is preferably in the form of a SiC composite substrate. That is, according to a preferred embodiment of the present invention, there is provided a SiC composite substrate including a SiC single crystal substrate and the above-described SiC substrate on the SiC single crystal substrate. In this way, by providing a SiC composite substrate with a biaxially textured SiC layer with few regions with extremely high BPDs (i.e., a uniform BPD distribution), it is possible to reduce breakage and cracks during substrate processing.
[0021] The SiC single crystal substrate is typically a layer composed of a SiC single crystal and has a crystal growth plane. The SiC single crystal substrate preferably has an off-axis angle. The polytype, off-axis angle, and polarity of the SiC single crystal are not particularly limited, but the polytype is preferably 4H or 6H, the off-axis angle is preferably 0.1 to 12° from the
[0001] axis of the single crystal SiC, and the polarity may be either the Si-face or the C-face. The polytype is more preferably 4H, the off-axis angle is more preferably 1 to 5° from the
[0001] axis of the single crystal SiC, and the polarity may be either the Si-face or the C-face.
[0022] The SiC substrate of the present invention may be in the form of a freestanding substrate of a biaxially oriented SiC layer alone, or in the form of a SiC composite substrate accompanied by a SiC single crystal substrate. Therefore, if necessary, the biaxially oriented SiC layer may finally be separated from the SiC single crystal substrate. Separation of the SiC single crystal substrate may be performed by any known method, without particular limitation. Examples include a method of separating the biaxially oriented SiC layer using a wire saw, a method of separating the biaxially oriented SiC layer by electrical discharge machining, and a method of separating the biaxially oriented SiC layer using a laser. Furthermore, when a biaxially oriented SiC layer is epitaxially grown on a SiC single crystal substrate, the biaxially oriented SiC layer may be placed on a separate support substrate after separation of the SiC single crystal substrate. The material of the separate support substrate is not particularly limited, and a suitable material may be selected from the viewpoint of material properties. For example, from the viewpoint of thermal conductivity, metal substrates such as Cu, and ceramic substrates such as SiC and AlN may be used.
[0023] Manufacturing Method of SiC Composite Substrate The SiC composite substrate including the SiC substrate of the present invention can be preferably manufactured by (a) forming a predetermined textured precursor layer on a SiC single crystal substrate, (b) heat-treating the textured precursor layer on the SiC single crystal substrate to convert at least a portion thereof near the SiC single crystal substrate into a SiC substrate (biaxially textured SiC layer), and, if desired, (c) performing processing such as grinding or polishing to expose the surface of the biaxially textured SiC layer. However, the manufacturing method of the SiC composite substrate is not limited, as long as it is possible to obtain a SiC substrate having a biaxially textured SiC layer with few regions of extremely high BPD, as described above. For example, a gas phase method such as CVD or sublimation or a liquid phase method such as solution processing may be used. In order to obtain a biaxially textured SiC layer with a uniformly controlled dislocation distribution, it is preferable to control the amount of rare earth element added during the formation of the textured precursor layer, the film formation conditions during the formation of the textured precursor layer (carrier gas flow rate and nozzle size), the heat treatment conditions of the textured precursor layer, etc., as described below. According to this manufacturing method, it is possible to preferably produce a SiC substrate having a biaxially oriented SiC layer with few regions with extremely high BPDs, and it is possible to effectively reduce breakage and cracks during processing of the SiC substrate or a SiC composite substrate using the same.
[0024] A preferred method for manufacturing a SiC composite substrate will now be described. Fig. 1 is a longitudinal cross-sectional view of a SiC composite substrate 10 (a cross-sectional view of the SiC composite substrate 10 cut longitudinally along a plane including the central axis of the SiC composite substrate 10), and Fig. 2 is a process diagram for manufacturing the SiC composite substrate 10.
[0025] As shown in FIG. 1, a SiC composite substrate 10 of this embodiment includes a SiC single crystal substrate 20 and a SiC substrate 30 (corresponding to the SiC substrate of the present invention) on the SiC single crystal substrate.
[0026] 2(a) Step of Forming Textured Precursor Layer As shown in Fig. 2(a), the textured precursor layer 40 will become the SiC substrate (biaxially textured SiC layer) 30 by heat treatment, which will be described later. In the step of forming the textured precursor layer 40, the textured precursor layer 40 is formed on the crystal growth surface of the SiC single crystal substrate 20.
[0027] The orientation precursor layer 40 can be formed by any known method. Examples of methods for forming the orientation precursor layer 40 include solid-phase deposition methods such as aerosol deposition (AD) and HPPD (supersonic plasma particle deposition), vapor-phase deposition methods such as sputtering, evaporation, sublimation, and various CVD (chemical vapor deposition) methods, and liquid-phase deposition methods such as solution growth. A method in which the orientation precursor layer 40 is formed directly on the SiC single crystal substrate 20 can be used. Examples of CVD methods that can be used include thermal CVD, plasma CVD, mist CVD, and metal-organic CVD. Alternatively, a polycrystalline body previously prepared by sublimation, various CVD, sintering, or the like can be used as the orientation precursor layer 40, and then placed on the SiC single crystal substrate 20. Alternatively, a molded body for the orientation precursor layer 40 can be prepared in advance and then placed on the SiC single crystal substrate 20. Such an alignment precursor layer 40 may be a tape-molded body produced by tape casting, or may be a green compact produced by pressure molding using a uniaxial press or the like.
[0028] When forming these textured precursor layers 40, it is preferable that the raw materials for the textured precursor layer 40 contain a rare earth compound. By doing so, the concentration of the rare earth compound in the biaxially textured SiC layer can be controlled, and the distribution of dislocations in the biaxially textured SiC layer can be effectively controlled. The rare earth compound is not particularly limited, but examples thereof include oxides, nitrides, carbides, and fluorides of at least one element selected from the 17 rare earth elements mentioned above. As the rare earth compound, oxides of rare earth elements are preferred, and oxides of Y (yttrium oxide) are more preferred. In addition, the carrier gas (e.g., N 2 The flow rate of ) can effectively control the distribution of dislocations in the biaxially textured SiC layer.
[0029] In addition, when various CVD methods, sublimation methods, solution growth methods, etc. are used to form the textured precursor layer 40 directly on the SiC single crystal substrate 20, epitaxial growth may occur on the SiC single crystal substrate 20, resulting in the formation of the SiC substrate 30, without the heat treatment process described below. However, the textured precursor layer 40 is preferably in an unoriented state upon formation, i.e., amorphous or unoriented polycrystalline, and is preferably oriented using the SiC single crystal as a seed in a subsequent heat treatment process. This effectively reduces crystal defects that reach the surface of the SiC substrate 30. Although the reason for this is unclear, it is believed that the reorganization of the crystalline structure of the solid-phase textured precursor layer once formed using the SiC single crystal as a seed may also be effective in eliminating crystal defects. Therefore, when various CVD methods, sublimation methods, solution growth methods, etc. are used, it is preferable to select conditions that do not cause epitaxial growth in the textured precursor layer 40 formation process.
[0030] However, preferred are methods of forming the texture precursor layer 40 directly on the SiC single crystal substrate 20 using the AD method or various CVD methods, or methods of placing a polycrystalline body separately prepared by sublimation, various CVD methods, sintering, or the like on the SiC single crystal substrate 20. These methods enable the texture precursor layer 40 to be formed in a relatively short time. The AD method is particularly preferred because it does not require a high-vacuum process and has a relatively fast film formation rate. When using a pre-prepared polycrystalline body as the texture precursor layer 40, it is necessary to take measures such as sufficiently smoothing the surface of the polycrystalline body to improve adhesion between the polycrystalline body and the SiC single crystal substrate 20. Therefore, from a cost perspective, the method of directly forming the texture precursor layer 40 is preferred. The method of placing a pre-prepared compact on the SiC single crystal substrate 20 is also preferred as a simple method, but because the texture precursor layer 40 is composed of powder, a sintering process is required in the heat treatment step described below. Both methods can use known conditions, but below we will describe a method of forming an orientation precursor layer 40 directly on a SiC single crystal substrate 20 by the AD method or thermal CVD method, and a method of placing a pre-prepared molded body on a SiC single crystal substrate 20.
[0031] The AD method is a technology in which fine particles or fine particle raw material are mixed with a gas to form an aerosol, and this aerosol is then sprayed at high speed from a nozzle to collide with a substrate, forming a coating. The AD method has the advantage of being able to form a coating at room temperature. An example of a film-forming apparatus (AD apparatus) used in this AD method is shown in FIG. 3 . The AD apparatus 50 shown in FIG. 3 is configured as an apparatus used in the AD method, in which raw material powder is sprayed onto a substrate under an atmosphere at a pressure lower than atmospheric pressure. This AD apparatus 50 includes an aerosol generation unit 52 that generates an aerosol of raw material powder containing raw material components, and a film-forming unit 60 that sprays the raw material powder onto a SiC single crystal substrate 20 to form a film containing the raw material components. The aerosol generating section 52 includes an aerosol generating chamber 53 that contains raw material powder and generates aerosol by receiving a carrier gas supplied from a gas cylinder (not shown), a raw material supply pipe 54 that supplies the generated aerosol to the film forming section 60, and a vibrator 55 that applies vibrations at a frequency of 10 to 100 Hz to the aerosol generating chamber 53 and the aerosol therein. 2 and the like. To effectively control the dislocation density distribution in the biaxially oriented SiC layer, it is also preferable to control the flow rate of the carrier gas, with the flow rate preferably being 2.0 to 6.5 L / min, and may be 4.0 to 6.5 L / min. The film-forming unit 60 includes a film-forming chamber 62 that sprays an aerosol onto the SiC single crystal substrate 20, a substrate holder 64 disposed inside the film-forming chamber 62 and fixing the SiC single crystal substrate 20, and an XY stage 63 that moves the substrate holder 64 in the X- and Y-axis directions. The film-forming unit 60 also includes a spray nozzle 66 having a slit 67 formed at its tip that sprays the aerosol onto the SiC single crystal substrate 20, and a vacuum pump 68 that depressurizes the film-forming chamber 62. The spray nozzle 66 is attached to the tip of the raw material supply pipe 54.
[0032] It is known that the AD method can cause pores in the film or result in a compacted film depending on the film formation conditions. For example, the impact speed of the raw material powder on the substrate, the particle size of the raw material powder, the agglomeration state of the raw material powder in the aerosol, and the amount sprayed per unit time are easily affected. The impact speed of the raw material powder on the substrate is affected by the pressure difference between the film formation chamber 62 and the spray nozzle 66, the opening area of the spray nozzle, and other factors. Therefore, to obtain a dense textured precursor layer, it is necessary to appropriately control these factors. In particular, to effectively control the dislocation density distribution in the biaxially textured SiC layer, it is preferable to control, for example, the opening area (nozzle size) of the spray nozzle.
[0033] In the thermal CVD method, a commercially available or other known film forming apparatus can be used. The source gas is not particularly limited, but silicon tetrachloride (SiCl 4 ) gas and silane (SiH 4 ) gas, and methane (CH 4 ) gas and propane (C 3 H 8 The film formation temperature is preferably 1000 to 2200°C, more preferably 1100 to 2000°C, and even more preferably 1200 to 1900°C.
[0034] It is known that when a film is formed on a SiC single crystal substrate 20 using thermal CVD, epitaxial growth may occur on the SiC single crystal substrate 20, forming a SiC substrate 30. However, the orientation precursor layer 40 is not oriented at the time of its formation, i.e., amorphous or non-oriented polycrystalline, and it is preferable to use a SiC single crystal as a seed crystal during the heat treatment process to cause crystalline rearrangement. It is known that the formation of an amorphous or polycrystalline layer on a SiC single crystal using thermal CVD is affected by factors such as the film formation temperature, the gas flow rates of the Si source and the C source and their ratio, and the film formation pressure. The film formation temperature has a significant effect, and from the perspective of forming an amorphous or polycrystalline layer, a lower film formation temperature is preferable, preferably less than 1700°C, more preferably 1500°C or less, and even more preferably 1400°C or less. However, if the film formation temperature is too low, the film formation rate itself also decreases, so from the perspective of the film formation rate, a higher film formation temperature is preferable.
[0035] When a pre-prepared compact is used as the orientation precursor layer 40, it can be produced by molding raw material powder of the orientation precursor. For example, when press molding is used, the orientation precursor layer 40 is a press-molded body. The press-molded body can be produced by press molding raw material powder of the orientation precursor based on a known method, for example, by placing the raw material powder in a mold and pressing it at a pressure of preferably 100 to 400 kgf / cm. 2 , more preferably 150 to 300 kgf / cm 2 The sheet can be fabricated by pressing the SiC single crystal substrate 20 at a pressure of 1000 psi. Furthermore, the molding method is not particularly limited, and in addition to press molding, tape casting, extrusion molding, slip casting, doctor blade molding, and any combination thereof can be used. For example, when using tape casting, additives such as binders, plasticizers, dispersants, and dispersion media are appropriately added to the raw material powder to form a slurry, and this slurry is then discharged and molded into a sheet by passing it through a narrow slit-shaped discharge port. The thickness of the sheet-shaped molded body is not limited, but from the perspective of handling, a thickness of 5 to 500 μm is preferable. Furthermore, if a thick orientation precursor layer is required, multiple sheets of this molded body can be stacked to achieve the desired thickness. These molded bodies are subsequently heat-treated on the SiC single crystal substrate 20, and the portion near the SiC single crystal substrate 20 becomes the SiC substrate 30. In this method, the molded body must be sintered in the heat treatment process described below. The SiC substrate 30 is preferably formed after the molded body is sintered and integrated with the SiC single crystal substrate 20 as a polycrystalline body. If the compact is not sintered, epitaxial growth using the SiC single crystal as a seed may not occur sufficiently. For this reason, the compact may contain additives such as sintering aids in addition to the SiC raw material.
[0036] (b) Heat Treatment Step As shown in FIG. 2(b), in the heat treatment step, a stack in which the orientation precursor layer 40 is stacked or placed on the SiC single crystal substrate 20 is heat-treated to produce the SiC substrate 30. The heat treatment method is not particularly limited as long as epitaxial growth occurs using the SiC single crystal substrate 20 as a seed, and can be performed in a known heat treatment furnace such as a tubular furnace or a hot plate. In addition to these atmospheric (pressless) heat treatments, pressurized heat treatments such as hot pressing and HIP, or a combination of atmospheric and pressurized heat treatments, can also be used. The heat treatment atmosphere can be selected from vacuum, nitrogen, inert gas, and a combination thereof. The heat treatment temperature is preferably 1700 to 2700°C. Increasing the temperature facilitates growth of the orientation precursor layer 40 with the SiC single crystal substrate 20 as a seed crystal, while aligning the c-axis and a-axis. Therefore, the heat treatment temperature is preferably 1700°C or higher, more preferably 1800°C or higher, even more preferably 1900°C or higher, and particularly preferably 2200°C or higher. On the other hand, if the temperature is excessively high, a portion of the SiC may be lost due to sublimation, or the SiC may undergo plastic deformation, resulting in defects such as warping. Therefore, the heat treatment temperature is preferably 2700°C or lower, more preferably 2500°C or lower. However, since the heat treatment conditions affect the concentration of rare earth elements in the biaxially oriented SiC layer and the distribution of dislocation density in the biaxially oriented SiC layer, it is preferable to appropriately control the conditions (e.g., heat treatment temperature). From this perspective, the heat treatment temperature is preferably 2200 to 2600°C, more preferably 2390 to 2500°C, even more preferably 2400 to 2500°C, and particularly preferably 2400 to 2450°C. The holding time is preferably 2 to 30 hours, more preferably 4 to 20 hours. The heat treatment may also be performed in multiple stages. Even in such a case, the heat treatment temperature and the total holding time are preferably within the above ranges. Furthermore, the heat treatment temperature and the holding time are related to the thickness of the SiC substrate 30 produced by epitaxial growth, and can be adjusted appropriately.
[0037] However, when a pre-formed compact is used as the orientation precursor layer 40, it is necessary to sinter it during the heat treatment, and high-temperature atmospheric pressure firing, hot pressing, HIP, or a combination thereof is suitable. For example, when using hot pressing, the surface pressure is 50 kgf / cm. 2 More preferably, 100 kgf / cm 2 More preferably, 200 kgf / cm 2 The firing temperature is not particularly limited, as long as sintering and epitaxial growth occur. However, since firing conditions affect the concentration of rare earth elements in the biaxially oriented SiC layer and the distribution of dislocations in the biaxially oriented SiC layer, it is preferable to appropriately control the firing conditions (e.g., firing temperature and holding time). From this perspective, the firing temperature is preferably 1700 to 2700°C. The holding time is preferably 2 to 18 hours. The firing atmosphere can be selected from vacuum, nitrogen, an inert gas atmosphere, or a mixture of nitrogen and an inert gas. As described above, firing may be performed in multiple stages, with the firing temperature and total holding time preferably within the above ranges. The raw SiC powder may be composed of at least one of α-SiC and β-SiC, but is preferably composed of β-SiC. The SiC powder is preferably composed of SiC particles having a volume-based D50 particle size of 0.01 to 100 μm.
[0038] In the heat treatment step, the crystals in the orientation precursor layer 40 preferably grow from the crystal growth surface of the SiC single crystal substrate 20 while being oriented in the c-axis and a-axis, and therefore the orientation precursor layer 40 gradually changes from the crystal growth surface into the SiC substrate 30. The SiC composite substrate including the resulting SiC substrate 30 has reduced breakage and cracks that occur during substrate processing.
[0039] 2(c) Grinding and / or Polishing Step As shown in Fig. 2(c), in the grinding step, the orientation precursor layer 40 remaining on the SiC substrate 30 after the heat treatment step is ground and removed to expose the surface of the SiC substrate 30, and the exposed surface is then ground and / or polished to obtain the SiC composite substrate 10.
[0040] It should be noted that the present invention is not limited to the above-described embodiment, and may be embodied in various forms as long as it falls within the technical scope of the present invention. For example, in the above-described embodiment, only one SiC substrate 30 is provided on the SiC single crystal substrate 20, but two or more layers may be provided. Specifically, a second SiC substrate 30 can be provided on the SiC substrate 30 by stacking an orientation precursor layer 40 on the SiC substrate 30 of the SiC composite substrate 10, performing heat treatment, and then grinding and / or polishing in this order.
[0041] The present invention will be explained in more detail by the following examples, which should not be construed as limiting the scope of the present invention.
[0042] Example 1 (1) Preparation of Textured Precursor Layer A raw material powder containing 90.8 wt% of commercially available fine β-SiC powder (volume-based D50 particle size: 0.7 μm) and 9.2 wt% of yttrium oxide powder (volume-based D50 particle size: 0.1 μm) was prepared. These raw material powders were mixed in ethanol using SiC balls in a ball mill for 24 hours and then dried to obtain a mixed powder. A commercially available SiC single crystal substrate (n-type 4H-SiC, diameter approximately 150 mm (6 inches), Si-face, (0001) plane, off-angle 4°, thickness 0.35 mm, no orientation flat) was prepared as the SiC single crystal layer. The mixed powder was sprayed onto the SiC single crystal substrate using the AD device 50 shown in FIG. 3 to form an AD film (textured precursor layer).
[0043] The AD film formation conditions were as follows: First, the carrier gas was N 2The flow rate was 4.0 L / min. The film was formed using a ceramic nozzle with a slit of 5 mm long x 0.4 mm short. The nozzle scanning conditions were a scan speed of 0.5 mm / s, moving 155 mm in a direction perpendicular to the long side of the slit and advancing, moving 5 mm in the long side direction of the slit, moving 155 mm in a direction perpendicular to the long side of the slit and returning, and moving 5 mm in the long side direction of the slit and in the opposite direction from the initial position. After moving 155 mm from the initial position in the long side direction of the slit, scanning was performed in the opposite direction from the previous cycle, and the cycle of returning to the initial position was counted as one cycle, and this cycle was repeated 4000 times. The thickness of the AD film formed in this way was approximately 400 μm.
[0044] (2) Heat Treatment of the Textured Precursor Layer The SiC single crystal substrate on which the AD film serving as the textured precursor layer was formed was removed from the AD apparatus and annealed in an argon atmosphere at 2400°C for 10 hours. That is, the textured precursor layer was heat-treated to form a heat-treated layer.
[0045] (3) Grinding (3-1) Surface Grinding The (0001) surface of the SiC single crystal substrate on which the heat treatment layer was formed was surface-ground to a predetermined thickness using a grinder (a diamond wheel with a grit of 1000 to 6000) to achieve the target thickness and surface condition.
[0046] (3-2) Backside Grinding The (000-1) surface of the SiC single crystal substrate on which the heat treatment layer was formed was surface-ground to a predetermined thickness using a grinder (a diamond wheel with a grit of 1000 to 6000) to obtain the target thickness and surface condition. In this way, a SiC substrate was obtained.
[0047] (4) Evaluation of suppression of cracks and fractures after processing Using an industrial microscope (Nikon, ECLIPSE LV150N), the magnification of the eyepiece was 10x and the magnification of the objective lens was 5x. The entire surface of the SiC substrate obtained in (3) above was observed in polarization mode and differential interference mode, and if cracks or fractures were found, the substrate was considered to have cracks or fractures. In this case, only those cracks or fractures with a length of 100 μm or more were counted as cracks or fractures. The crack and fracture occurrence rate P was calculated by counting the number of SiC substrates with cracks or fractures with a length of 100 μm or more out of 100 SiC substrates produced under the same conditions as the SiC substrate produced as described above. C (%) was calculated. C The yield of the substrate was evaluated by calculating the following. The results are shown in Table 1.
[0048] (5) Polishing (5-1) Surface Polishing The (0001) surface of the SiC substrate obtained in (3) above was polished with diamond abrasive grains, and then finished by chemical mechanical polishing (CMP) to achieve the target thickness and surface condition.
[0049] (5-2) Backside Polishing The (000-1) surface of the SiC substrate obtained in (3) above was polished with diamond abrasive grains to achieve the target thickness and surface condition.
[0050] (6) Evaluation of biaxial orientation of heat-treated layer Using EBSD (Electron Backscatter Diffraction Patterns) under the conditions shown below, inverse pole figure mapping of the surface (plate surface) of the heat-treated layer obtained in (3) above and a cross section perpendicular to the plate surface was measured. As a result, the tilt angle distribution was 0.01° or less in both the approximately normal direction and the approximately plate surface direction, and therefore it was determined that the heat-treated layer was a biaxially oriented SiC layer oriented along the c-axis and the a-axis.
[0051] <EBSD measurement conditions> Measurement device: SEM (SU-5000, manufactured by Hitachi High-Technologies Corporation) equipped with an electron backscatter diffraction device (EBSD) (Nordlys Nano, manufactured by Oxford Instruments) Acceleration voltage: 15 kV Spot intensity: 70 Working distance: 22.5 mm Step size: 0.5 μm Specimen tilt angle: 70° Measurement program: Aztec (version 3.3)
[0052] (7) X-ray Topography (XRT) Measurement of Heat-Treated Layer The SiC substrate produced in (5) above was used as an evaluation sample, and an XRT image of the evaluation sample was obtained under the following conditions.
[0053] <XRT measurement conditions> Measuring device: X-ray topographic imaging system (XRTmicron, manufactured by Rigaku Corporation) Observation mode: reflection Diffraction plane: (11-28) plane X-ray source: Cu, Kα Tube voltage / tube current: 40 kV / 30 mA Detector: XTOP CCD camera Photography area: entire surface of sample
[0054] First, an evaluation was performed on basal plane dislocations (BPDs). The entire area of the obtained XRT image of the entire surface of the sample was divided into a grid pattern with each grid having a size of 4 mm length x 4 mm width x 28 μm depth. The "depth" refers to the penetration depth of the X-rays. In each of the divided regions, the total length of the BPDs was measured using image processing software (manufactured by Rigaku Corporation), and the volume density of BPDs per grid (cm / cm) was calculated. 3 Then, the average value of the volume density in the entire region of the XRT image was calculated to obtain the average value X (cm / cm) of the volume density of BPD per square. 3 ) was calculated. The maximum number of cells in which the area of 5X or more per cell is continuous in a straight line both vertically and horizontally is C 5X (cell), and the maximum number of cells C where an area of 3X or more per cell is continuous in a straight line both vertically and horizontally 3X (Square) was also confirmed. At this time, C 5X and C 3XIn the calculation, only the number of squares that are consecutive in a vertical line and the number of squares that are consecutive in a horizontal line are counted, and the number of squares that are consecutive in a diagonal line is not counted. The results are shown in Table 1. In the sample of Example 1, the XRT image was used to measure the square size by 5X (cm / cm) per square. 3 ) or more, and a schematic diagram showing the area with black squares is shown in Figure 4. 5X The corresponding point A is also shown.
[0055] An evaluation of threading screw dislocations (TSDs) was also carried out. The entire area of the obtained XRT image of the entire surface of the sample was divided into a grid pattern with each grid having a size of 4 mm in length and 4 mm in width. In each of the divided regions, the number of TSDs was measured using image processing software (manufactured by Rigaku Corporation), and the number density of TSDs per grid ( / cm 2 ) was obtained. Then, the average value of the number density in the entire region of the XRT image was calculated, and the average value Y ( / cm 2 ) was calculated. The maximum number of cells in which the area of 2Y or more per cell is continuous in a straight line both vertically and horizontally is C 2Y (Square) was also confirmed. At this time, C 2Y In this calculation, only the number of squares that are consecutive vertically and horizontally in a straight line are counted, and the number of squares that are consecutive diagonally in a straight line is not counted. The results are shown in Table 1.
[0056] Evaluation of edge dislocations (TEDs) was also performed. The entire XRT image of the entire surface of the obtained sample was divided into a grid pattern with each grid having a size of 4 mm in length and 4 mm in width. In each of the divided regions, the number of TEDs was measured using image processing software (manufactured by Rigaku Corporation), and the number density of TEDs per grid ( / cm 2 ) was obtained. Then, the average value of the number density in the entire region of the XRT image was calculated, and the average value Z ( / cm 2 ) was calculated. In addition, the maximum number of cells in which the area of 2Z or more per cell is continuous in a straight line both vertically and horizontally is C 2Z (Square) was also confirmed. At this time, C 2ZIn this calculation, only the number of squares that are consecutive vertically and horizontally in a straight line are counted, and the number of squares that are consecutive diagonally in a straight line is not counted. The results are shown in Table 1.
[0057] (8) Rare Earth Element Concentration in the Heat-Treated Layer After the substrate prepared in the same manner as in (1) and (2) above was polished in the same manner as in (3-1) above, it was cut into chips of approximately 5 mm length x 6 mm width, which were used as evaluation samples. Dynamic secondary ion mass spectrometry (D-SIMS) was performed on the polished (0001) surface of this evaluation sample. The rare earth element (Y in this example) was analyzed using an IMS-7f manufactured by CAMECA, with the primary ion species O 2 + The measurement was carried out at an acceleration voltage of 11.0 kV. RE (atoms / cm 3 The results are shown in Table 1.
[0058] Example 2 In the above (1), the carrier gas is N 2 The SiC substrate was fabricated and evaluated in the same manner as in Example 1, except that the flow rate of the gas was set to 5.5 L / min. The obtained heat-treated layer was confirmed to be a biaxially oriented SiC layer. The results are shown in Table 1.
[0059] Example 3 (Comparative) In the above (1), the carrier gas was N 2 The SiC substrate was fabricated and evaluated in the same manner as in Example 1, except that the flow rate of the gas was set to 3.5 L / min. The obtained heat-treated layer was confirmed to be a biaxially oriented SiC layer. The results are shown in Table 1.
[0060] Example 4 In the above (1), the carrier gas is N 2 The SiC substrate was fabricated and evaluated in the same manner as in Example 1, except that the flow rate of the gas was set to 6.5 L / min. The obtained heat-treated layer was confirmed to be a biaxially oriented SiC layer. The results are shown in Table 1.
[0061] Example 5 In the above (1), the carrier gas is N 2The SiC substrate was fabricated and evaluated in the same manner as in Example 1, except that the flow rate of the gas was set to 6.0 L / min. The obtained heat-treated layer was confirmed to be a biaxially oriented SiC layer. The results are shown in Table 1.
[0062] Example 6 (Comparison) In the above (1), raw material powder containing 80.8 wt % of fine β-SiC powder (volume-based D50 particle size: 0.7 μm) and 19.2 wt % of yttrium oxide powder (volume-based D50 particle size: 0.1 μm) was used, and N 2 The SiC substrate was fabricated and evaluated in the same manner as in Example 1, except that the flow rate of the gas was set to 2.0 L / min. The obtained heat-treated layer was confirmed to be a biaxially oriented SiC layer. The results are shown in Table 1.
[0063] Example 7 In the above (1), the carrier gas is N 2 The SiC substrate was fabricated and evaluated in the same manner as in Example 1, except that the flow rate of the gas was set to 4.5 L / min. The obtained heat-treated layer was confirmed to be a biaxially oriented SiC layer. The results are shown in Table 1.
[0064] Example 8 In the above (1), the carrier gas is N 2 The SiC substrate was fabricated and evaluated in the same manner as in Example 1, except that the flow rate of the gas was set to 5.0 L / min. The obtained heat-treated layer was confirmed to be a biaxially oriented SiC layer. The results are shown in Table 1.
[0065] Example 9 (Comparative) In the above (1), the carrier gas was N 2 The SiC substrate was fabricated and evaluated in the same manner as in Example 1, except that the flow rate of the gas was set to 3.0 L / min. The obtained heat-treated layer was confirmed to be a biaxially oriented SiC layer. The results are shown in Table 1.
[0066] Example 10 (Comparative) In the above (1), the carrier gas N 2 The SiC substrate was fabricated and evaluated in the same manner as in Example 1, except that the flow rate of the gas was set to 2.5 L / min. The obtained heat-treated layer was confirmed to be a biaxially oriented SiC layer. The results are shown in Table 1.
[0067] Example 11: A SiC substrate was fabricated and evaluated in the same manner as in Example 1, except that in (1) above, a ceramic nozzle with a slit having a long side of 5 mm and a short side of 0.5 mm was used for deposition. The obtained heat-treated layer was confirmed to be a biaxially oriented SiC layer. The results are shown in Table 1.
[0068] Example 12: A SiC substrate was fabricated and evaluated in the same manner as in Example 1, except that in (1) above, a ceramic nozzle with a slit having a long side of 5 mm and a short side of 0.6 mm was used for deposition. The obtained heat-treated layer was confirmed to be a biaxially oriented SiC layer. The results are shown in Table 1.
[0069] Example 13 (Comparative) A SiC substrate was produced and evaluated in the same manner as in Example 1, except that in (1) above, a ceramic nozzle with a slit having a long side of 5 mm and a short side of 0.9 mm was used for film formation. The obtained heat-treated layer was confirmed to be a biaxially oriented SiC layer. The results are shown in Table 1.
[0070] Example 14: A SiC substrate was fabricated and evaluated in the same manner as in Example 1, except that in (1) above, a ceramic nozzle with a slit having a long side of 5 mm and a short side of 0.2 mm was used for deposition. The obtained heat-treated layer was confirmed to be a biaxially oriented SiC layer. The results are shown in Table 1.
[0071] Example 15: A SiC substrate was fabricated and evaluated in the same manner as in Example 1, except that in (1) above, a ceramic nozzle with a slit having a long side of 5 mm and a short side of 0.3 mm was used for deposition. The obtained heat-treated layer was confirmed to be a biaxially oriented SiC layer. The results are shown in Table 1.
[0072] Example 16 (Comparative) A SiC substrate was produced and evaluated in the same manner as in Example 1, except that in (1) above, a ceramic nozzle with a slit having a long side of 5 mm and a short side of 1.0 mm was used for film formation. The obtained heat-treated layer was confirmed to be a biaxially oriented SiC layer. The results are shown in Table 1.
[0073] Example 17: A SiC substrate was fabricated and evaluated in the same manner as in Example 1, except that in (1) above, a ceramic nozzle with a slit having a long side of 5 mm and a short side of 0.8 mm was used for deposition. The obtained heat-treated layer was confirmed to be a biaxially oriented SiC layer. The results are shown in Table 1.
[0074] Example 18: A SiC substrate was fabricated and evaluated in the same manner as in Example 1, except that in (1) above, a ceramic nozzle with a slit having a long side of 5 mm and a short side of 0.7 mm was used for deposition. The obtained heat-treated layer was confirmed to be a biaxially oriented SiC layer. The results are shown in Table 1.
[0075] Example 19 (Comparative) A SiC substrate was produced and evaluated in the same manner as in Example 1, except that in (1) above, a ceramic nozzle with a slit having a long side of 5 mm and a short side of 1.1 mm was used for film formation. The obtained heat-treated layer was confirmed to be a biaxially oriented SiC layer. The results are shown in Table 1.
[0076] Example 20 (Comparison) In the above (1), a raw material powder containing 80.8 wt% of fine β-SiC powder (volume-based D50 particle size: 0.7 μm) and 19.2 wt% of yttrium oxide powder (volume-based D50 particle size: 0.1 μm) was used, and a ceramic nozzle with a slit having a long side of 5 mm and a short side of 1.2 mm was used for film formation. An SiC substrate was produced and evaluated in the same manner as in Example 1. The obtained heat-treated layer was confirmed to be a biaxially oriented SiC layer. The results are shown in Table 1.
[0077] Example 21: A SiC substrate was fabricated and evaluated in the same manner as in Example 1, except that in (2) above, annealing was performed in an argon atmosphere at 2410°C for 10 hours. The obtained heat-treated layer was confirmed to be a biaxially oriented SiC layer. The results are shown in Table 1.
[0078] Example 22: A SiC substrate was fabricated and evaluated in the same manner as in Example 1, except that in (2) above, annealing was performed in an argon atmosphere at 2420°C for 10 hours. The obtained heat-treated layer was confirmed to be a biaxially oriented SiC layer. The results are shown in Table 1.
[0079] Example 23 (Comparative) A SiC substrate was fabricated and evaluated in the same manner as in Example 1, except that in (2) above, annealing was performed in an argon atmosphere at 2,370°C for 10 hours. The obtained heat-treated layer was confirmed to be a biaxially oriented SiC layer. The results are shown in Table 1.
[0080] Example 24: A SiC substrate was fabricated and evaluated in the same manner as in Example 1, except that in (2) above, annealing was performed in an argon atmosphere at 2430°C for 10 hours. The obtained heat-treated layer was confirmed to be a biaxially oriented SiC layer. The results are shown in Table 1.
[0081] Example 25: A SiC substrate was fabricated and evaluated in the same manner as in Example 1, except that in (2) above, annealing was performed in an argon atmosphere at 2440°C for 10 hours. The obtained heat-treated layer was confirmed to be a biaxially oriented SiC layer. The results are shown in Table 1.
[0082] Example 26 (Comparative) A SiC substrate was produced and evaluated in the same manner as in Example 1, except that in (1) above, a raw material powder containing 94.9 wt% of fine β-SiC powder (volume-based D50 particle size: 0.7 μm) and 5.1 wt% of yttrium oxide powder (volume-based D50 particle size: 0.1 μm) was used, and in (2) above, annealing was performed in an argon atmosphere at 2460°C for 10 hours. The obtained heat-treated layer was confirmed to be a biaxially oriented SiC layer. The results are shown in Table 1.
[0083] Example 27: A SiC substrate was fabricated and evaluated in the same manner as in Example 1, except that in (2) above, annealing was performed in an argon atmosphere at 2450°C for 10 hours. The obtained heat-treated layer was confirmed to be a biaxially oriented SiC layer. The results are shown in Table 1.
[0084] Example 28: A SiC substrate was fabricated and evaluated in the same manner as in Example 1, except that in (2) above, annealing was performed in an argon atmosphere at 2390°C for 10 hours. The obtained heat-treated layer was confirmed to be a biaxially oriented SiC layer. The results are shown in Table 1.
[0085] Example 29 (Comparative) A SiC substrate was produced and evaluated in the same manner as in Example 1, except that in (2) above, annealing was performed in an argon atmosphere at 2470°C for 10 hours. The obtained heat-treated layer was confirmed to be a biaxially oriented SiC layer. The results are shown in Table 1.
[0086] Example 30 (Comparative) A SiC substrate was fabricated and evaluated in the same manner as in Example 1, except that in (2) above, annealing was performed in an argon atmosphere at 2480°C for 10 hours. The obtained heat-treated layer was confirmed to be a biaxially oriented SiC layer. The results are shown in Table 1.
[0087]
[0088] Although the reason is unclear, it was found that the distribution of BPDs and the like can be controlled by the film formation conditions (carrier gas flow rate, etc.) in the AD method, the rare earth element concentration in the SiC substrate, etc. Specifically, when the entire XRT image of the biaxially oriented SiC layer is divided into a grid pattern with a region of 4 mm length × 4 mm width × 28 μm depth per square, the average value of the volume density of BPDs per square is X (cm / cm 3 ) and 5X (cm / cm) per square 3 It was found that in a SiC substrate in which the area where the cracks are larger than 3X (cm / cm) per square is not more than 10 consecutive squares in a straight line in either direction, it is possible to reduce breakage and cracks during processing. 3 It was found that in a substrate in which the areas with a thickness of 1 / 2 mm or more do not extend in a straight line vertically or horizontally for more than five squares, breakage and cracks during processing can be effectively reduced.
Claims
1. A SiC substrate having a biaxially textured SiC layer, wherein, in an XRT image obtained by measuring the biaxially textured SiC layer with an X-ray topograph (XRT), when the entire area of the XRT image is divided into a lattice shape with an area of 4 mm length × 4 mm width × 28 μm depth per mass, the average value of the volume density of basal plane dislocations (BPDs) per mass is X (cm / cm 3 ), then 5X (cm / cm) per square 3 ) in no area extending in a straight line horizontally or vertically for more than 10 consecutive squares.
2. In the XRT image, 3X (cm / cm) per square 3 2. The SiC substrate according to claim 1, wherein no region where the number of adjacent squares is 5 or more is consecutive in a straight line either vertically or horizontally.
3. When the entire area of the XRT image is divided into a lattice shape with each square having an area of 4 mm vertical x 4 mm horizontal, the average value of the number density of threading screw dislocations (TSDs) per square is Y ( / cm 2 ), then 2Y ( / cm 2 3. The SiC substrate according to claim 1, wherein the region in which the number of squares is 1 or more is not consecutive in a straight line vertically or horizontally.
4. When the entire area of the XRT image is divided into a lattice shape with each square having an area of 4 mm vertical x 4 mm horizontal, the average value of the number density of edge dislocations (TEDs) per square is Z ( / cm 2 ), then 2Z ( / cm 2 3. The SiC substrate according to claim 1, wherein the region in which the number of squares is 1 or more is not consecutive in a straight line vertically or horizontally.
5. The X is 200 to 5000 cm / cm 3 The SiC substrate according to claim 1 or 2.
6. The rare earth element concentration of the biaxially oriented SiC layer is 2.0×10 14 ~5.0 x 10 15 atoms / cm 3 The SiC substrate according to claim 1 or 2.
7. A SiC composite substrate comprising a SiC single crystal substrate and the SiC substrate according to claim 1 or 2 on the SiC single crystal substrate.
Citation Information
Patent Citations
SiC single crystals, SiC wafers, and semiconductor devices
JP5750363B2
sic single crystal, sic wafer, sic substrate and sic device
JP6192948B2
SiC COMPOSITE SUBSTRATE
JP2022131919A
Method for producing rare-earth-containing sic substrate and sic epitaxial layer
WO2021149235A1
Biaxially-oriented sic composite substrate and composite substrate for semiconductor device
WO2021149598A1