Thermally conductive particle and method for producing same, mixture, article, resin composition and thermally conductive thin film

Low-hardness thermally conductive particles formed from aluminum, zinc, and other compounds address the abrasion and viscosity issues of conventional materials, offering improved thermal conductivity and processability in resin compositions.

WO2024202248A1PCT designated stage expired Publication Date: 2024-10-03DAINICHISEIKA COLOR & CHEMICALS MFG CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2023/042935
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-27
Filing Date
2023-11-30
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Conventional thermally conductive materials, such as alumina, exhibit high mechanical abrasion and viscosity issues when used in resin compositions, leading to equipment wear and poor processability, while alternative materials like spherical zinc oxide have low thermal conductivity.

Method used

Development of low-hardness thermally conductive particles composed of aluminum, zinc, and other raw materials like boron, titanium, tungsten, and fluorine compounds, which are fired and pulverized to achieve high thermal conductivity and reduced mechanical wear, along with controlled particle shape and surface properties for improved resin kneading and moldability.

Benefits of technology

The resulting thermally conductive particles provide excellent chemical resistance, water resistance, electrical insulation, and high thermal conductivity, while minimizing equipment wear and enhancing resin composition moldability and processability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JPOXMLDOC01-APPB-T000001
    Figure JPOXMLDOC01-APPB-T000001
  • Figure JPOXMLDOC01-APPB-T000002
    Figure JPOXMLDOC01-APPB-T000002
  • Figure JPOXMLDOC01-APPB-T000003
    Figure JPOXMLDOC01-APPB-T000003
Patent Text Reader

Abstract

This thermally conductive particle contains at least a fired product obtained by firing an aluminum raw material, a zinc raw material and an additional raw material other than the aluminum raw material and the zinc raw material. The content of the zinc raw material relative to 100 parts by mass of the aluminum raw material is 25-70 parts by mass inclusive, the additional raw material contains at least one compound selected from the group consisting of a boron compound, a tungsten compound, a titanium compound, a bismuth compound and a fluorine compound and the content of the additional raw material is 0.05-20 parts by mass inclusive relative to 100 parts by mass of the aluminum raw material, and the thermally conductive particle satisfies predetermined conditions.
Need to check novelty before this filing date? Find Prior Art

Description

Thermally conductive particles, their manufacturing method, mixture, article, resin composition, and thermally conductive thin film

[0001] The present invention relates to thermally conductive particles that are excellent in reducing mechanical wear, and a method for producing the same.

[0002] Currently, many materials are being investigated as thermally conductive materials. As the integration density of semiconductor devices increases, the demand for heat dissipation is becoming stronger, making it essential to develop materials with much higher thermal conductivity and insulating properties than before. Composite materials (resin compositions) obtained by kneading thermally conductive fillers into resins are known to meet these demands.

[0003] Alumina is widely used as a filler in composite materials because it has excellent water resistance, acid resistance, and insulating properties, as well as good thermal conductivity and low cost. However, the alumina powder contained in thermally conductive compositions is a very hard material, which contributes to the accelerated wear of equipment, such as devices that process thermally conductive composite materials into pellets or sheets. When applying thermally conductive fillers to processed products, there is a strong demand for thermally conductive fillers that have both high thermal conductivity and low wear.

[0004] JP 2009-249226 A International Publication No. 2015 / 137468

[0005] Alumina has a high Mohs hardness, which places a load on the blade or extruder shaft, making it difficult to incorporate into resin compositions, etc., and furthermore, worn parts may be mixed in, causing contamination. Furthermore, when applied to resins, the viscosity increases, which can lead to poor moldability and processability. To solve this problem, thermally conductive materials that are less mechanically abrasive than alumina and have a lower viscosity when incorporated into resins have been investigated. However, although the spherical zinc oxide particle powder disclosed in Patent Document 1 has a coated surface, the zinc oxide itself has low thermal conductivity, and therefore requires improvement. Patent Document 2 describes a sintered product of an alumina-based compound and a compound of a metal other than aluminum, but the description is about a sintered product that combines only an aluminum raw material and a zinc raw material.

[0006] The present invention was conceived in consideration of the problems inherent in the prior art. Its objective is to provide low-hardness alumina-based thermally conductive particles (hereinafter sometimes referred to as "thermally conductive particles") that have excellent thermal conductivity, chemical resistance, water resistance, and electrical insulation, as well as low mechanical wear, and can be used to produce materials and articles such as resin compositions that have excellent fillability and moldability, and a method for producing the same. In order to solve the above problem, the inventors conducted extensive research and found that thermally conductive particles produced by firing a mixture of an aluminum raw material, a zinc raw material, and other raw materials selected from the group consisting of at least boron compounds, titanium compounds, tungsten compounds, bismuth compounds, and fluorine compounds at a predetermined temperature to react the raw materials and generate a compound, and then pulverizing the mixture, can achieve both low mechanical wear and high thermal conductivity. Furthermore, they found that controlling the particle shape or surface properties is effective in improving thermal conductivity, resin kneadability, and paint suitability. It has been discovered that the use of these thermally conductive particles can impart high thermal conductivity to the matrix while simultaneously suppressing wear on equipment such as devices used to process and mold thermally conductive composite materials.

[0007] That is, according to the present invention, the following thermally conductive particles and a method for producing the same are provided. [1] Thermally conductive particles containing at least an aluminum raw material, a zinc raw material, and a calcined product obtained by calcining other raw materials other than the aluminum raw material and the zinc raw material, wherein the content of the zinc raw material relative to 100 parts by mass of the aluminum raw material is 25 parts by mass or more and 70 parts by mass or less, and the other raw materials contain at least one selected from the group consisting of boron compounds, tungsten compounds, titanium compounds, bismuth compounds, and fluorine compounds, and the content of the other raw materials relative to 100 parts by mass of the aluminum raw material is 0.05 parts by mass or more and 20 parts by mass or less, and the thermally conductive particles satisfy the following conditions: (1) 50 g of the thermally conductive particles and an epoxy equivalent of 200 g / eq or more and 1000 g / eq or less are viscous liquids obtained by calcining an E-type viscometer at a measurement temperature of 25°C, a cone rotor (3° x R9.7), and a rotation speed of 100 s -1The resin composition for viscosity measurement obtained by the above method was mixed with 50 g of an epoxy resin having a viscosity of 400 mPa·s or more and 900 mPa·s or less when measured under the conditions of (1) and (2). The mixture was then kneaded using a planetary centrifugal mixer at 1,000 rpm for 1 minute and then at 2,000 rpm for 1 minute. The viscosity of the resin composition for viscosity measurement obtained by the above method was measured using an E-type viscometer at a measurement temperature of 25°C, a cone rotor (3°×R9.7), and a rotation speed of 100 s -1(2) 500 parts by mass of SUS304 steel balls with a diameter of 5 mm and 100 parts by mass of the thermally conductive particles are placed in a 250 mL wide-mouth cylindrical container, and the container is rotated at 80 rpm for 3 hours around the central axis of the cylinder of the cylindrical container as the axis of rotation, and the steel balls and the thermally conductive particles are separated using a sieve with 1 mm mesh to obtain thermally conductive particles after an abrasion test. 4 parts by mass of the thermally conductive particles before and after the abrasion test and 8 parts by mass of lithium borate are mixed and ground in a mortar for 5 minutes, and the strength of the iron element is measured using a fluorescent X-ray analyzer. The fluorescent X-ray strength (kcps) of the iron element before and after the abrasion test is calculated using the following formula, and the abrasion degree is 4 kcps or less. Abrasion rate = (fluorescent X-ray intensity of iron element after abrasion test) - (fluorescent X-ray intensity of iron element before abrasion test) (3) A resin composition obtained by kneading 30 parts of a mixed solution obtained by mixing an epoxy resin having an epoxy equivalent of 200 g / eq or more and 1000 g / eq or less and an amine-based curing agent having an amine value of 100 mgKOH / g or more and 500 mgKOH / g or less in a ratio of 3:1 to 4:1 with 70 parts of thermally conductive particles is mold-pressed into a circular sheet molded product having a diameter of 100 mm or more and a thickness of 4 mm or more, heat-cured at a set temperature of 120°C for 1 hour, and after cooling, cut into four equal parts so as to form a fan-shaped test piece with a central angle of 90°. When the thermal conductivity is measured by hot disc thermophysical property measurement, the thermal conductivity is 0.80 W / m·K or more. [2] The thermally conductive particles according to [1], wherein the other raw materials (excluding fluorine compounds) are at least one selected from the group consisting of oxides, oxoacid salts, hydroxides, carbonates, and basic carbonates. [3] The thermally conductive particles according to [1] or [2], which contain at least one element selected from the group consisting of iron, cobalt, copper, manganese, nickel, and chromium and are colored. [4] A mixture obtained by mixing a thermally conductive filler with the thermally conductive particles according to any one of [1] to [3]. [5] The mixture according to [4], wherein the thermally conductive filler is at least one selected from the group consisting of barium sulfate, talc, boron nitride, and magnesium oxide.[6] The method for producing thermally conductive particles according to any one of [1] to [3], comprising firing a raw material mixture containing an aluminum raw material, a zinc raw material, and raw materials other than the aluminum raw material and the zinc raw material, wherein the aluminum raw material is at least one selected from the group consisting of boehmite, aluminum hydroxide, and alumina, and the zinc raw material is at least one selected from the group consisting of zinc oxide and basic carbonate. [7] A method for producing thermally conductive particles, comprising firing the raw material mixture according to [6] at a temperature of 1,000°C or higher and 1,600°C or lower. [8] An article containing the thermally conductive particles according to any one of [1] to [3]. [9] The article according to [8], which is any one of gravure ink, coating liquid, resin composition, and adhesive composition.

[10] A resin composition used to form a thermally conductive resin composition, comprising the mixture according to [4] or [5] and a forming resin.

[11] The resin composition according to

[10] , wherein the content of the mixture relative to the total amount of the molding resin is 5% by mass or more and 95% by mass or less.

[12] A thermally conductive thin film formed by coating the article according to [9].

[13] The article according to [8], which is used as a heat dissipation member for any of electronic device parts, electronic device housings, EV motors, and lithium batteries.

[0008] According to the present invention, it is possible to provide thermally conductive particles that have excellent not only thermal conductivity but also chemical resistance, water resistance, and electrical insulation, and that cause little wear on processing equipment, have good kneadability (filling ability) into resins, and, by adding a colorant, can be used to produce materials and articles such as colored resin compositions that have excellent moldability, and a method for producing the same. Furthermore, according to the present invention, it is possible to provide thermally conductive resin compositions and articles using the thermally conductive particles.

[0009] <Thermal Conductive Particles> Hereinafter, embodiments of the present invention will be described, but the present invention is not limited to the following embodiments. The thermally conductive particles according to this embodiment are obtained by firing a raw material mixture containing an aluminum raw material, a zinc raw material, and other raw materials other than the aluminum raw material and the zinc raw material. The aluminum raw material is at least one selected from the group consisting of alumina, boehmite, and aluminum hydroxide. The zinc raw material is at least one selected from the group consisting of zinc oxides and basic carbonates. The raw material mixture further contains the zinc raw material and other raw materials selected from the group consisting of at least boron compounds, titanium compounds, tungsten compounds, bismuth compounds, and fluorine compounds. The content of the zinc raw material is more than 20 parts by mass and not more than 70 parts by mass per 100 parts by mass of the aluminum raw material. The content of the other raw materials is 0.05 parts by mass or more and 20 parts by mass or less per 100 parts by mass of the aluminum raw material. Details of the thermally conductive particles according to this embodiment will be described below.

[0010] The thermally conductive particles according to this embodiment are primarily composed of α-alumina and zinc aluminate with a spinel crystal structure. The volume-average particle size of these thermally conductive particles is preferably 0.1 μm or more and 50 μm or less. By using a composition containing such thermally conductive particles as a filler, it is possible to impart high thermal conductivity to the composition, and at the same time, the composition has lower hardness compared to a composition containing α-alumina alone, thereby suppressing wear on equipment such as devices used to mold or process the composition. The average particle size can be measured using a laser diffraction particle size distribution analyzer or transmission electron microscope photographs.

[0011] The content of the zinc raw material in the raw material mixture must be more than 20 parts by mass and not more than 70 parts by mass, more preferably 25 parts by mass or more and not more than 65 parts by mass, relative to 100 parts by mass of the aluminum raw material. If the content of the zinc raw material is 20 parts by mass or less, the effect of improving hardness and thermal conductivity cannot be obtained. On the other hand, if the content of the zinc raw material is more than 70 parts by mass, the thermal conductivity decreases. By setting the aluminum raw material and the zinc raw material within the above ranges, it is possible to obtain thermally conductive particles that have excellent thermal conductivity, chemical resistance, water resistance, and low abrasion while maintaining various resistances, and that have good kneadability (miscibility) into resins and can be used to produce materials and articles such as resin compositions with excellent moldability.

[0012] In addition to the zinc raw material, other raw materials other than the aluminum raw material and the zinc raw material are further mixed. These components are used to supplement the zinc component. The oxide raw material is added to solve problems such as when it is difficult to gelatinize the sintered product or when it is desired to adjust the particle size distribution.

[0013] The content of the other raw materials in the raw material mixture is 0.05 parts by mass or more and 20 parts by mass or less, more preferably 0.1 parts by mass or more and 10 parts by mass or less, even more preferably 0.1 parts by mass or more and 8 parts by mass or less, and particularly preferably 0.5 parts by mass or more and 5 parts by mass or less, relative to 100 parts by mass of the aluminum raw material used as the raw material. If the amount of the other raw materials relative to 100 parts by mass of the aluminum raw material used as the raw material is less than 0.05 parts by mass, the particle size distribution will be broad and the filling ability will be reduced. On the other hand, if the amount of the other raw materials relative to 100 parts by mass of the aluminum raw material used as the raw material exceeds 20 parts by mass, the thermal conductivity will actually be reduced. By setting the amount of the other raw materials relative to 100 parts by mass of the aluminum raw material used as the raw material within the above range, the thermally conductive particles will have excellent thermal conductivity, chemical resistance, water resistance, and electrical insulation, and will be able to produce materials or articles such as resin compositions that are low in wear and have excellent moldability.

[0014] The viscosity of the thermally conductive particles according to this embodiment when added to a resin was measured using the value obtained when 50 parts by mass of the particles were added to 50 parts by mass of epoxy resin. The sample used for viscosity measurement was prepared by kneading for 1 minute at 1,000 rpm and degassing for 1 minute at 2,000 rpm using a planetary centrifugal mixer. The resin composition for viscosity measurement obtained by the above method was measured using an E-type viscometer at a measurement temperature of 25°C, with a cone rotor (3° x R9.7), and a rotation speed of 100 s -1 The viscosity was measured under the following conditions. The viscosity of the epoxy resin composition at this time must be 3,000 mPa·s or less, and preferably 2,500 mPa·s or less. If the viscosity exceeds 3,000 mPa·s, the processability will be poor. There is no particular restriction on the lower limit, but if the viscosity is less than 10 mPa·s, it may be difficult to form a coating film. This makes it possible to produce a thermally conductive resin composition with excellent resin moldability or processability.

[0015] Regarding the abrasion resistance of the thermally conductive particles according to this embodiment, 500 parts by mass of 5 mm diameter SUS304 steel balls and 100 parts by mass of the thermally conductive particles were placed in a 250 mL wide-mouth cylindrical bottle and rotated at 80 rpm for 3 hours around the central axis of the cylinder of the cylindrical bottle. The steel balls and the thermally conductive particles were then separated using a 1 mm mesh sieve to obtain thermally conductive particles after the abrasion test. Four parts by mass of the thermally conductive particles before and after the abrasion test were mixed with 8 parts by mass of lithium borate and ground in a mortar for 5 minutes to prepare samples, and the intensity of the iron element was measured using an X-ray fluorescence analyzer. The intensity (kcps) of the fluorescent X-rays of the iron element before and after the abrasion test was calculated using the following formula, and the abrasion resistance was evaluated based on the degree of abrasion of the steel balls. Abrasion resistance = (fluorescent X-ray intensity of the iron element after the abrasion test) - (fluorescent X-ray intensity of the iron element before the abrasion test). The abrasion resistance must be 4 kcps or less. If the abrasion rate exceeds 4 kcps, the thermally conductive particles are too hard and will wear out the devices when they are molded and processed into a resin composition, which is undesirable.

[0016] The thermal conductivity of the thermally conductive particles according to this embodiment was measured using the value obtained when 70 parts by weight of the particles were added to 30 parts by weight of a mixture of epoxy resin and amine-based curing agent. The sample used for thermal conductivity measurement was mold-pressed into a circular sheet with a diameter of 100 mm or more and a thickness of 4 mm or more, heated and cured at a set temperature of 120°C for 1 hour, and then cut into quarters with a 90° central angle. Thermal conductivity was measured using a hot-disk thermophysical property measurement method. The thermal conductivity of the epoxy resin composition must be 0.80 W / m·K or higher, and 0.90 W / m·K or higher is even more preferable. A thermal conductivity of less than 0.80 W / m·K is insufficient in terms of thermal conductivity. This results in high thermal conductivity when used in electronic components, achieving the desired heat dissipation performance.

[0017] The epoxy resin used to measure thermal conductivity and viscosity must have an epoxy equivalent of 200 g / eq or more and 1000 g / eq or less, more preferably 300 g / eq or more and 800 g / eq or less, and even more preferably 350 g / eq or more and 700 g / eq or less. If the epoxy equivalent is less than 200 g / eq, the flexibility when cured is poor, and air bubbles cannot be removed or molding becomes difficult, making various measurements difficult. On the other hand, if it exceeds 1000 g / eq, the viscosity decreases and the flexibility becomes too high, causing particles to settle, making it difficult to prepare a uniform sample and making various measurements difficult. In addition, using an E-type viscometer, the measurement temperature was 25°C, the cone rotor (3° x R9.7), and the rotation speed was 100 s -1 The viscosity of the epoxy resin measured under these conditions must be 400 mPa·s or more and 900 mPa·s or less. When 50 g of thermally conductive particles and 50 g of epoxy resin are mixed, the viscosity becomes 3,000 mPa·s or less, which is more preferable as a viscosity with good moldability. If the viscosity of this epoxy is less than 400 mPa·s, sedimentation occurs, making measurement difficult. If the viscosity of this epoxy is more than 900 mPa·s, workability decreases, such as moldability deteriorates, and measurement becomes difficult, which is undesirable.

[0018] The amine-based curing agent used for thermal conductivity measurement must have an amine value of 100 mgKOH / g to 500 mgKOH / g, preferably 150 mgKOH / g to 450 mgKOH / g. An amine value of less than 100 mgKOH / g is undesirable because the high viscosity makes it difficult to mix uniformly and difficult to handle. An amine value of more than 500 mgKOH / g is undesirable because the cured resin becomes too hard, making various measurements difficult. The ratio of epoxy resin to amine-based curing agent in the mixed solution was set to a range of 3:1 to 4:1 (epoxy resin:amine-based curing agent). Deviations from this blending ratio are undesirable because the resin will not cure sufficiently. Any conventional amine-based curing agent can be used as long as it cures the epoxy resin. Examples of amine-based curing agents include amines, aliphatic amines, aromatic amines, and modified amines.

[0019] The thermally conductive particles according to the present embodiment have excellent thermal conductivity, low wear on processing equipment, and excellent chemical resistance, water resistance, and electrical insulation. Furthermore, they have high wettability with resins and good kneadability (fillability) into resins, making them suitable for use in the production of materials such as resin compositions with excellent moldability, as well as articles such as paints and adhesive compositions.

[0020] The thermally conductive particles according to this embodiment are obtained by firing a raw material mixture containing an aluminum raw material, a zinc raw material, and other raw materials, and are preferably composed mainly of α-alumina and zinc aluminate with a spinel crystal structure.

[0021] (Aluminum raw material) Alumina, boehmite, aluminum hydroxide, etc. can be used as the aluminum raw material. The shape and particle size of the aluminum raw material are not particularly limited, but considering the dispersibility of the thermally conductive particles, particles with an average particle size of 0.1 μm or more and 50 μm or less are preferred. More specific examples of the shape of the aluminum raw material include spherical and amorphous shapes.

[0022] (Raw Material Mixture) The raw material mixture used together with the aluminum raw material contains, in addition to the zinc raw material, other raw materials. The other raw materials are at least one selected from the group consisting of boron compounds, titanium compounds, tungsten compounds, bismuth compounds, and fluorine compounds. These compounds improve the dispersibility of the thermally conductive particles, promote the gelatinization of alumina, or adjust the particle size distribution.

[0023] (Zinc raw material) As the zinc raw material, basic zinc carbonate, zinc hydroxide, zinc oxide, etc. can be used. The shape and particle size of the raw material are not particularly limited, but in consideration of the dispersibility of the thermally conductive particles, it is preferable that the raw material be particles having an average particle size of 0.1 μm or more and 50 μm or less.

[0024] (Other Raw Materials) Examples of other raw materials include boron compounds such as boric acid, sodium borate, ammonium borate, magnesium borate, and lithium borate. Titanium compounds such as rutile or anatase titanium oxide can be used. Tungsten compounds such as tungsten oxide, ammonium tungstate, and sodium tungstate can be used. Bismuth compounds such as bismuth oxide, basic bismuth carbonate, and sodium bismuthate can be used. Fluorine compounds such as lithium fluoride, sodium fluoride, potassium fluoride, and aluminum fluoride can be used. Among these, boric acid, sodium tungstate, titanium oxide, basic bismuth carbonate, sodium fluoride, or aluminum fluoride is preferred because it allows the formation of thermally conductive particles with a high filling rate. Furthermore, the other raw materials (excluding fluorine compounds) are preferably at least one selected from the group consisting of oxides, oxoacid salts, hydroxides, carbonates, and basic carbonates.

[0025] (Coloring agent) Furthermore, the thermally conductive particles according to this embodiment can be colored by adding at least one element selected from the group consisting of iron, cobalt, copper, manganese, and nickel, without adding a pigment or dye.

[0026] (Surface Treatment) The thermally conductive particles according to this embodiment may be surface-treated. Surface-treated thermally conductive particles have improved affinity and dispersibility in resins, allowing for the production of articles such as resin compositions with excellent thermal conductivity. Examples of compounds (treatment agents) used for the surface treatment include fatty acids, fatty acid esters, fatty acid metal salts, phosphate esters, phosphate ester metal salts, silane coupling agents, surfactants, polymer flocculants, titanates, and silicones. These treatment agents can be used alone or in combination. The amount of the compound used for the surface treatment is preferably 0.01 to 5 parts by mass per 100 parts by mass of the thermally conductive particles. Examples of treatment methods include adding a treatment agent to a powder of thermally conductive particles and mixing them together, or adding a treatment agent to a powder of thermally conductive particles in water to disperse the powder, followed by filtering and drying.

[0027] (Use of Thermally Conductive Particles) Among the preferred uses of the thermally conductive particles according to this embodiment, it is effective to add them to various plastics such as thermoplastic resins or thermosetting resins for the purpose of imparting thermal conductivity. Examples of thermoplastic resins include polyethylene resins, polypropylene resins, ethylene-propylene copolymers, ethylene-vinyl acetate copolymers, acrylonitrile-ethylene-styrene copolymers, acrylonitrile-butadiene-styrene copolymers, acrylonitrile-styrene copolymers, polyvinyl chloride resins, polystyrene resins, polyacrylonitrile resins, polyamide resins, thermoplastic polyimide resins, thermoplastic urethane resins, polyaminobismaleimide resins, polyamideimide resins, polyetherimide resins, polymethyl methacrylate resins, polyvinyl acetate resins, polycarbonate resins, polyacetal resins, polyethylene terephthalate resins, polybutylene terephthalate resins, polyphenylene oxide resins, polyphenylene sulfide resins, polysulfone resins, polyethersulfone resins, polyetheretherketone resins, polyallylsulfone resins, bismaleimide triazine resins, polymethylpentene resins, fluorinated resins, liquid crystal polymers, olefin-vinyl alcohol copolymers, ionomer resins, and polyarylate resins. These thermoplastic resins can be used alone or in combination of two or more. Examples of thermosetting resins that can be used include phenolic resins, urea resins, epoxy resins, melamine resins, silicone resins, polyurethane resins, unsaturated polyester resins, alkyd resins, polyimide resins, acrylic resins, and (modified) polyphenylene ethers. These thermosetting resins can be used alone or in combination of two or more.

[0028] <Method for Producing Thermally Conductive Particles> Next, a method for producing thermally conductive particles according to this embodiment will be described. The method for producing thermally conductive particles according to this embodiment includes a step (step (1)) of mixing an aluminum raw material, a zinc raw material, and raw materials other than the aluminum raw material and the zinc raw material to obtain a raw material mixture, and a step (step (2)) of firing the obtained raw material mixture. This production method makes it possible to easily obtain particles that have lower hardness, less mechanical wear, and higher thermal conductivity than conventional alumina. The reason for this is not entirely clear, but the inventors speculate that it is as follows. That is, the thermally conductive particles contain at least α-alumina and spinel crystal structure zinc aluminate. Furthermore, the mixed crystals constituting the filler composition made from this particulate material have a large number of α-alumina fine particles present between spinel crystal structure zinc aluminate particles, which increases the contact area between the particles and reduces the interparticle thermal resistance (interfacial thermal resistance). As a result, the thermal conductivity is higher than that of pure spinel crystal structure zinc aluminate. On the other hand, spinel crystal structure zinc aluminate particles have inferior thermal conductivity to α-alumina, but have excellent mechanical wear resistance, so the produced thermally conductive particles have lower mechanical wear resistance than alumina. The ratio of α-alumina to spinel crystal structure zinc aluminate in the thermally conductive particles (α-alumina:spinel crystal structure zinc aluminate) is preferably in the range of 8:2 to 1:9, more preferably in the range of 6:4 to 4:6. A ratio of 5:5 provides a particularly good balance between thermal conductivity and hardness.

[0029] In step (1), the aluminum raw material, zinc raw material, and other raw materials are mixed. The aluminum raw material, zinc raw material, and other raw materials are mixed using equipment such as a pot mill, Henschel mixer, air mixer, conical blender, planetary ball mill, vibration mill, ribbon mixer, and vertical blender, and then the components are mixed and fired. The components are mixed so that they are uniform. The amount of each component in the raw material mixture is as described above.

[0030] In step (2), the raw material mixture obtained in step (1) is fired at 1,000°C or higher and 1,600°C or lower. Preferably, the firing is performed at 1,200°C or higher and 1,500°C or lower. By firing, the aluminum raw material and the zinc raw material are crystallized to form α-alumina and spinel crystal structure zinc aluminate. If the firing temperature is lower than 1,000°C, the crystalline structures of α-alumina and spinel crystal structure zinc aluminate are difficult to form. In this case, the unreacted zinc raw material remains, resulting in reduced durability. Furthermore, because the thermal conductivity of transition alumina formed at low temperatures is lower than that of α-alumina, firing is preferred to form α-alumina and spinel crystal structure zinc aluminate. On the other hand, firing at temperatures higher than 1,600°C does not significantly change the properties of the resulting thermally conductive particles, resulting in wasted energy consumption. One method for confirming the presence of α-alumina and spinel crystal structure zinc aluminate in the thermally conductive particles is to compare the peaks obtained by powder X-ray diffraction measurement of standard materials of α-alumina and spinel crystal structure zinc aluminate with the peaks obtained by powder X-ray diffraction measurement of the prepared thermally conductive particles. When α-alumina and spinel crystal structure zinc aluminate are present, the peaks are summed, and quantification can be performed by comparing the intensities of each peak. After firing, the fired product can be crushed as needed to obtain the thermally conductive particles according to this embodiment. For crushing, known methods may be used, and various conventionally used devices such as a hammer mill, roll mill, ball mill, jet mill, bead mill, or vibration mill can be used.

[0031] <Thermal Conductive Composition (Mixture)> In the thermal conductive composition (mixture), in addition to the thermally conductive particles according to this embodiment, it is also a preferred embodiment to use them in combination with other thermally conductive fillers such as alumina, boron nitride, graphite, zinc oxide, barium sulfate, talc, and magnesium oxide. Details thereof will be described below.

[0032] Typical fillers are added to materials such as resins, rubbers, and paints to improve strength or functionality. Increasing the amount of thermally conductive filler typically reduces the melt flow and mechanical strength of materials such as resins. Furthermore, because carbon-based fillers are electrically conductive, their intrinsic insulating properties are easily impaired when incorporated into resins. Furthermore, ceramic-based fillers have insulating properties but suffer from low thermal conductivity. Thermally conductive fillers include, for example, metal-based fillers such as silver, copper, aluminum, and iron; inorganic fillers such as alumina, magnesia, silica, boron nitride, aluminum nitride, silicon carbide, boron carbide, and titanium carbide; and carbon-based fillers such as diamond, graphite, and graphite. For electronic devices requiring high electrical insulation, fillers such as alumina, magnesium oxide, zinc oxide, silica, boron nitride, aluminum nitride, and diamond are considered preferable. However, these fillers have many issues in terms of water resistance, chemical resistance, hardness, and electrical insulation.

[0033] In contrast, the thermally conductive particles according to this embodiment overcome the weaknesses of the various fillers described above and have excellent properties, making them suitable for use as improved fillers. Furthermore, it is also preferable to use them together with the various thermally conductive fillers described above to compensate for the weaknesses of existing thermally conductive fillers. That is, in thermally conductive compositions containing the various thermally conductive fillers described above, the use of the thermally conductive particles according to this embodiment is a preferred embodiment, adjusted according to the desired properties. The amount of thermally conductive filler added is preferably 10 parts by mass or more and 150 parts by mass or less per 100 parts by mass of the thermally conductive particles. If the amount of thermally conductive filler added is less than 10 parts by mass, the effect of the thermally conductive filler may be difficult to obtain. Conversely, if the amount of thermally conductive filler added is more than 150 parts by mass, the effect of the thermally conductive particles may be difficult to obtain.

[0034] <Article> The article according to this embodiment is an article (thermally conductive article, thermally conductive material) containing the thermally conductive particles, such as a gravure ink, a coating liquid, a resin composition, an adhesive composition, etc. Note that the article according to this embodiment preferably further contains the various thermally conductive fillers described above, as necessary.

[0035] (Gravure Ink) The thermally conductive particles according to this embodiment can be added to gravure ink used as a top coating agent for battery packaging materials. The content of the thermally conductive particles in the gravure ink is preferably 5% by mass or more and 80% by mass or less, and more preferably 10% by mass or more and 50% by mass or less, based on the total mass of the gravure ink. By using such gravure ink (top coating agent for battery packaging materials), it is possible to produce battery packaging materials that have excellent chemical resistance such as acid resistance, high thermal conductivity, and high thermal emissivity.

[0036] (Coating Liquid) The thermally conductive particles according to this embodiment can be added to a coating liquid such as a paint. The coating liquid can also be a coloring preparation obtained by mixing and dispersing the thermally conductive particles, for example, a colorant, a resin for forming a coating or molded product, and an organic solvent in a vehicle. The content of the thermally conductive particles in the coating liquid is preferably 5% by mass or more and 80% by mass or less, and more preferably 10% by mass or more and 70% by mass or less, based on the total amount of the coating liquid. The coating film or coated molded product formed using the coating liquid prepared in this manner has excellent water resistance, chemical resistance, and insulation properties, retains strength, and also has excellent thermal conductivity.

[0037] Specific examples of resins that can be contained in the coating liquid include thermoplastic resins such as polyolefins, polyesters, polystyrenes, acrylics, fluorine-containing resins, polyamides, celluloses, polycarbonates, and polylactic acid resins; and thermosetting resins such as urethanes, phenols, and silicones. These resins may be in the form of emulsions.

[0038] Specific examples of the liquid medium that can be contained in the coating liquid include water, methanol, ethanol, butanol, acetone, methyl ethyl ketone, methyl isobutyl ketone, toluene, xylene, butyl acetate, cyclohexane, etc. These liquid media may be used in combination of two or more.

[0039] The coating liquid may contain "other components" selected appropriately depending on the application, as long as the object of the present invention is not impaired. Specific examples of "other components" include antioxidants, ultraviolet absorbers, light stabilizers, dispersants, antistatic agents, lubricants, and bactericides.

[0040] A conventionally known method can be used to apply the coating liquid. Specific examples include spray coating, brush coating, electrostatic coating, curtain coating, or a method using a roll coater, and a dipping method. Furthermore, a conventionally known method can also be used to dry the applied coating liquid to form a coating. Specific examples include air drying, baking, and other methods that can be appropriately selected depending on the properties of the coating liquid.

[0041] The coating liquid can be used to produce coated films and coated molded articles by applying the coating to a substrate. The substrate can be selected from metal, glass, natural resin, synthetic resin, ceramics, wood, paper, fiber, nonwoven fabric, woven fabric, leather, and the like, depending on the application. The coating film thus provided with functionality can be used in various industries, such as manufacturing, agriculture, mining, and fishing, in addition to household use. There are also no limitations on the shape of the coating, and it can be in the form of a sheet, film, or the like, depending on the application.

[0042] (Resin Composition) A resin composition can be prepared by blending the thermally conductive particles according to this embodiment with a resin such as a polyamide resin or a polyolefin resin. More specifically, a resin composition can be obtained by blending and mixing the thermally conductive particles with the resin, along with other additives as needed, according to a known method. Furthermore, a predetermined resin molded product can be produced by molding the resulting resin composition in an extrusion molding machine. The content of the thermally conductive particles in the resin composition is preferably 5% by mass or more and 95% by mass or less, based on the total resin composition. By setting the content of the thermally conductive particles within the above range, a resin composition can be obtained that is superior in water resistance, chemical resistance, and insulation, further retains strength, and has better moldability. If the content of the thermally conductive particles exceeds 95% by mass, strength and moldability may decrease. On the other hand, if the content of the thermally conductive particles is less than 5% by mass, thermal conductivity may be insufficient.

[0043] The method for adding thermally conductive particles to a resin is not particularly limited, and conventional methods can be used. For example, the thermally conductive particles can be directly incorporated into the resin, followed by kneading and molding. Other methods include using a composition (masterbatch) in which the thermally conductive particles are pre-dispersed at a high concentration in a resin or lubricant. Other additives include antioxidants, UV absorbers, antistatic agents, antibacterial agents, stabilizers, crosslinking agents, plasticizers, lubricants, mold release agents, flame retardants, and inorganic fillers such as talc, alumina, clay, and silica. Metal soaps and polyethylene waxes can also be used as dispersion aids for the thermally conductive particles. Examples of metal soaps include lithium stearate, magnesium stearate, zinc stearate, calcium stearate, magnesium palmitate, calcium oleate, and cobalt oleate. Examples of polyethylene waxes that can be used include general polymerized, decomposed, and modified polyethylene waxes.

[0044] Various organic and inorganic pigments can also be blended as colorants into the coating liquid and resin composition. Examples of colorants include organic pigments such as phthalocyanine pigments, azo pigments, azomethine pigments, isoindolinone pigments, quinacridone pigments, anthraquinone pigments, dioxazine pigments, and perinone-perylene pigments; composite oxide pigments other than black; titanium oxide pigments such as titanium oxide white pigments, titanium oxide yellow pigments, and titanium oxide black pigments; and inorganic pigments such as carbon black, ultramarine, and red iron oxide. Examples of phthalocyanine pigments include brominated phthalocyanine blue pigments and phthalocyanine green pigments. Examples of azo pigments include polycondensed azo pigments and azomethine azo pigments.

[0045] Furthermore, a resin composition can also be obtained by melt-kneading a masterbatch compound prepared by blending thermally conductive particles, various pigments, and additives with a resin for compounding using an extruder or the like. More specifically, the resin composition can be obtained by (i) blending thermally conductive particles and a dispersing aid with a resin for compounding, adding other additives as needed, and mixing using a mixer such as a Henschel mixer; (ii) kneading the masterbatch compound using a kneader or a heated two-roll mill, cooling it, and then pulverizing it into a coarse powder using a pulverizer; or (iii) feeding the masterbatch compound into an extruder and extruding it into shapes such as beads or columns. The molding method is not particularly limited, and for example, injection molding, extrusion molding, heated compression molding, blow molding, inflation molding, vacuum molding, or the like may be used.

[0046] (Adhesive Composition) The thermally conductive particles according to this embodiment can be added to an adhesive to form an adhesive composition. The type of resin contained in the adhesive is not limited, and any adhesive resin, such as a urethane-based, epoxy-based, vinyl acetate-based, or acrylic-based resin, may be used. The adhesive mechanism is also not limited, and any of a chemical reaction type, solvent volatilization type, hot melt type, and hot pressure type may be used. The content of the thermally conductive particles in the adhesive composition is preferably 5% by mass or more and 80% by mass or less, and more preferably 10% by mass or more and 50% by mass or less, based on the total adhesive composition. By setting the content of the thermally conductive particles within the above range, an adhesive composition with superior thermal conductivity, adhesiveness, water resistance, chemical resistance, and insulating properties can be obtained. If the content of the thermally conductive particles exceeds 80% by mass, the adhesive strength may be insufficient. On the other hand, if the content of the thermally conductive particles is less than 5% by mass, the thermal conductivity may be insufficient.

[0047] The thermally conductive particles according to this embodiment can be used as thermally conductive articles or materials, such as the gravure inks, coating liquids, resin compositions, and adhesive compositions described above, and can be used to produce electronic devices that not only have heat dissipation (thermal conductivity) but also excellent chemical resistance, water resistance, and insulation. More specifically, they can be used in metal circuit boards, circuit boards, metal laminates, metal-clad laminates with inner layer circuits, battery packaging materials, sealants, protective sheets, etc. Furthermore, they can be used as adhesive sheets, heat-dissipating sheets, heat-dissipating coating agents, semiconductor sealants, adhesives, heat-dissipating spacers, greases, etc.

[0048] Liquid Composition (Resin Composition) The liquid composition (resin composition) according to this embodiment is a liquid composition used to form a thermally conductive thin film. The liquid composition contains a thermally conductive component (mixture) containing the aforementioned thermally conductive particles, a forming resin, and, optionally, a liquid medium. The thermally conductive component preferably further contains at least one selected from the group consisting of barium sulfate, talc, boron nitride, and magnesium oxide. The content of the thermally conductive particles in the liquid composition is preferably 5% by mass to 80% by mass, and more preferably 10% by mass to 70% by mass, based on the total weight of the liquid composition. Furthermore, the content of the thermally conductive component (mixture) per 100 parts by mass of the forming resin is preferably 20 parts by mass to 600 parts by mass, and more preferably 20 parts by mass to 200 parts by mass. A thermally conductive thin film formed using the liquid composition prepared in this manner exhibits excellent water resistance, chemical resistance, and insulating properties, retains strength, and exhibits excellent thermal conductivity.

[0049] The forming resin is at least one solvent-soluble resin selected from the group consisting of acrylic resins, urethane resins, urea resins, epoxy resins, rubber resins, fluorine-containing resins, polyamide resins, polyimide resins, silicone resins, cellulose resins, and thermoplastic elastomers. The liquid medium is the same as the liquid medium used in the coating liquid described above.

[0050] <Thermal Conductive Thin Film and Electronic Device Member> The thermally conductive thin film according to this embodiment is a thin film formed by applying the above-described article or the above-described liquid composition (resin composition). The thickness of the thermally conductive thin film is preferably 20 μm or more and 1000 μm or less, and more preferably 50 μm or more and 200 μm or less. The thermally conductive thin film according to this embodiment can also be used as an electronic device member. This electronic device member is a member comprising a metal member and the above-described thermally conductive thin film disposed on the surface of the metal member. Examples of metal members include metal circuit boards, circuit boards, metal laminates, and metal-clad laminates with inner layer circuits.

[0051] The resin composition according to this embodiment can be used in housings for electronic devices, motors (e.g., EV motors), lithium batteries, etc., to efficiently release internal heat to the outside and to reduce the weight compared to conventional metal housings. In addition, the article according to this embodiment can also be used in electronic device components as a heat dissipation member.

[0052] The present invention will be specifically described below based on examples, but the present invention is not limited to these examples. In the examples and comparative examples, "parts" and "%" are by mass unless otherwise specified.

[0053] <Aluminum raw materials> The following aluminum raw materials were used: A-1: ​​aluminum hydroxide (spherical, average particle size 6 μm) A-2: aluminum hydroxide (spherical, average particle size 1 μm) A-3: boehmite (spherical, average particle size 1 μm) A-4: spherical alumina (spherical, average particle size 3 μm) A-5: gamma alumina (irregular shape, average particle size 0.1 μm)

[0054] <Zinc Raw Materials> The following zinc raw materials were used: B-1: basic zinc carbonate (average particle size 10 μm) B-2: zinc oxide (average particle size 1 μm) B-3: zinc aluminate (average particle size 10 μm)

[0055] <Other raw materials> The following raw materials were used: C-1: Boric acid C-2: Sodium tungstate dihydrate C-3: Titanium oxide C-4: Basic bismuth carbonate C-5: Sodium fluoride C-6: Aluminum fluoride

[0056] <Thermal conductive filler> The following fillers were used: D-1: barium sulfate (average particle size 0.9 μm) D-2: talc (average particle size 4.3 μm) D-3: boron nitride (average particle size 20 μm) D-4: magnesium oxide (average particle size 20 μm)

[0057] <Production of Thermally Conductive Particles> (Example 1) 100 parts of aluminum hydroxide (A-1), 27.3 parts of basic zinc carbonate (B-1), 0.5 parts of boric acid (C-1), and 0.5 parts of sodium tungstate dihydrate (C-2) were charged into a small mixer and stirred to obtain a raw material mixture. The obtained raw material mixture was fired in air at 1,250°C for 3 hours and then crushed to obtain powdered thermally conductive particles. Powder X-ray diffraction measurement confirmed the presence of α-alumina and zinc aluminate with a spinel crystal structure.

[0058] (Examples 2 to 22) Powdered thermally conductive particles were obtained in the same manner as in Example 1, except that the types and amounts of raw materials shown in Table 1 were used. For Examples 18 to 22, the thermally conductive filler was added in the amount shown in the table per 100 parts by mass of the fired thermally conductive particles, followed by stirring and mixing in a small mixer. Powder X-ray diffraction measurements confirmed the presence of α-alumina and zinc aluminate with a spinel crystal structure.

[0059] (Comparative Examples 1 to 11, and 14) Powdered thermally conductive particles were obtained in the same manner as in Example 1, except that the types and amounts of raw materials shown in Table 1 were used. For Comparative Example 11, the amount of thermally conductive filler shown in the table was added to 100 parts by mass of the fired thermally conductive particles, followed by stirring and mixing in a small mixer. Powder X-ray diffraction measurement confirmed the presence of α-alumina and zinc aluminate with a spinel crystal structure.

[0060] Comparative Examples 12, 13, and 15 to 17 The raw materials shown in Table 1 were used as the samples of Comparative Examples 12, 13, and 15 to 17, respectively.

[0061] (Comparative Example 18) Powdered thermally conductive particles were obtained in the same manner as in Example 1, except that the types and amounts of raw materials shown in Table 1 were used and the firing temperature was set to 900° C. Powder X-ray diffraction measurement was performed, but the presence of α-alumina could not be confirmed.

[0062]

[0063] (Measurement of Thermal Conductivity) 30 parts of a mixture of epoxy resin (manufactured by Mitsubishi Chemical Corporation, Grade 871, epoxy equivalent weight 390-470 g / eq, viscosity 400-900 mPa·s) and amine-based curing agent (manufactured by ADEKA Corporation, EH-6024, amine value 370 mgKOH / g) in a ratio of 3.5:1 was mixed with 70 parts of the resulting thermally conductive particles to obtain a resin composition, which was then mold-pressed into a circular sheet molded product with a diameter of 100 mm or more and a thickness of 4 mm. The resulting product was then heat-cured at a set temperature of 120°C for 1 hour, allowed to cool, and then cut into four equal sections with a 90° central angle to prepare test specimens. The thermal conductivity of the prepared test specimens was measured using a hot disc thermal property measurement device (trade name "TPS-2500S", manufactured by Kyoto Electronics Manufacturing Co., Ltd.). The results are shown in Table 2.

[0064] (Viscosity Measurement) 50 g of the obtained thermally conductive particles were added to 50 g of epoxy resin (manufactured by Mitsubishi Chemical Corporation, Grade 871, epoxy equivalent weight 390 to 470 g / eq, viscosity 400 to 900 mPa·s) and mixed by hand. The mixed resin composition was kneaded using a planetary centrifugal mixer (kneading: 1000 rpm, 1 minute; degassing: 2000 rpm, 1 minute). The resin composition for viscosity measurement obtained by the above method was measured using an E-type viscometer (trade name "TV-100EH / 200", manufactured by Toki Sangyo Co., Ltd.) at a measurement temperature of 25°C, a cone rotor (3°×R9.7), and a rotation speed of 100 s -1 The viscosity was measured at 1000 mPa·s and evaluated according to the following criteria. The results are shown in Table 2. A: 3000 mPa·s or less C: More than 3000 mPa·s

[0065] (Abrasion Test) Approximately 500 g of 5 mm diameter SUS304 steel balls (trade name "1-9762-02", manufactured by Misumi Corporation) and approximately 100 g of the obtained thermally conductive particles were placed in a cylindrical container, a 250 mL wide-mouth Eyeboy bottle (diameter 62 mm, length 132 mm, manufactured by AS ONE Corporation), and rotated at 80 rpm for 3 hours around the central axis of the cylinder of the cylindrical container as the rotation axis. After that, the steel balls and the thermally conductive particles were separated using a sieve with 1 mm mesh to obtain thermally conductive particles after the abrasion test. To measure the degree of abrasion, 4 g of the thermally conductive particles after the abrasion test were mixed with 8 g of lithium borate and pulverized in a mortar for 5 minutes. Similarly, the thermally conductive particles before the abrasion test were mixed and pulverized in a mortar, and the strength of the iron element was measured using an X-ray fluorescence analyzer (trade name "ZSX Primus II", manufactured by Rigaku Corporation). The difference in the intensity (kcps) of fluorescent X-rays of iron element before and after the abrasion test was calculated using the following formula. The results are shown in Table 2. Abrasion degree = (fluorescent X-ray intensity of iron element after abrasion test) - (fluorescent X-ray intensity of iron element before abrasion test) A: Abrasion degree is 4 kcps or less B: Abrasion degree is more than 4 kcps and 8 kcps or less C: Abrasion degree is more than 8 kcps

[0066] (Acid Resistance) A resin molded article for evaluation made from the resin composition containing 70 parts by mass of the thermally conductive particles prepared above was cut into a size of 20 mm x 20 mm x 60 mm, and the obtained molded article was immersed in a hydrochloric acid solution of pH 2.0 heated to 50°C for 3 hours. The withstand voltage was measured before and after immersion, and the acid resistance was evaluated using the obtained measured values ​​according to the following criteria. The results are shown in Table 2. <Criteria for evaluating acid resistance> A: The withstand voltage after immersion decreased by less than 10% from the initial value before immersion. B: The withstand voltage after immersion decreased by 10% or more but less than 50% from the initial value before immersion. C: The withstand voltage after immersion decreased by 50% or more from the initial value before immersion.

[0067] (Water Resistance) Five parts of thermally conductive particles were immersed in 100 parts of pure water, placed in a container and boiled at 100°C for 5 minutes, then filtered, and the filtrate was used as a measurement sample. The measurement sample prepared as described above was used to measure the electrical conductivity with an electrical conductivity meter, and was judged and evaluated according to the following criteria. The results are shown in Table 2. <Water Resistance Judgment Criteria> A: The increase in electrical conductivity after immersion from the initial value before immersion is less than 300 μS / cm. B: The increase in electrical conductivity after immersion from the initial value before immersion is 300 μS / cm or more but less than 1000 μS / cm. C: The increase in electrical conductivity after immersion from the initial value before immersion is 1000 μS / cm or more.

[0068]

[0069] (Reference Example 1) When measuring thermal conductivity, a test piece was prepared using 70 parts of the thermally conductive particles obtained in Example 1 for 70 parts of the thermally conductive particles. As a thermal conductivity test method, 30 parts of polypropylene (manufactured by Prime Polymer Co., Ltd., MFR: 20 g / 10 min) and 70 parts of the thermally conductive particles were mixed to obtain a resin composition, which was then placed in a plastomill and melt-kneaded at a set temperature of 200 ° C. Next, a test piece was prepared by mold press molding at 175 ° C. using a mold measuring 20 mm in length, 20 mm in width, and 6 mm in height. The thermal conductivity of the prepared test piece was measured using a thermal property measuring device (product name "TPS-2500S", manufactured by Kyoto Electronics Manufacturing Co., Ltd.). The thermal conductivity at this time was 1.18 W / m K.

[0070] (Reference Example 2) A test piece was prepared in the same manner as in Reference Example 1, except that 60 parts of the thermally conductive particles obtained in Example 1 and 10 parts of the thermally conductive rounded discoid particles described in Example 3 of Japanese Patent No. 7185798 were used to prepare the test piece. The thermal conductivity in this case was 1.19 W / m K, and even when particles of different shapes were mixed, the result was within the range of the example, almost the same as when only thermally conductive particles were used.

[0071] (Reference Comparative Example 1) A test piece was prepared in the same manner as in Reference Example 1, except that 70 parts of the thermally conductive particles obtained in Comparative Example 7 were used to prepare the test piece. The thermal conductivity at this time was 0.92 W / m·K.

[0072] (Reference Comparative Example 2) A test piece was prepared in the same manner as in Reference Example 1, except that 70 parts of the thermally conductive particles obtained in Comparative Example 14 were used to prepare the test piece. The thermal conductivity at this time was 1.07 W / m·K.

[0073] <Preparation and Evaluation of Adhesives> (Application Example 1 and Comparative Application Example 1) 35 parts of the thermally conductive particles obtained in Example 1 and Comparative Example 13 were mixed with 65 parts of a polyester polyol having a viscosity of 300 mPa·s, and dispersed using a disperser to prepare a dispersion. 98 parts of the prepared dispersion was mixed with 2 parts of a polyisocyanate having a viscosity of 2,600 mPa·s and stirred using a dissolver to obtain a urethane resin-based chemical reaction adhesive. Each adhesive obtained was uniformly applied to release paper using a glass rod and then placed in a 100°C oven for 2 minutes to volatilize the solvent. This was then placed in a 40°C oven for 96 hours to form a cured coating of the adhesive (Application Example 1 and Comparative Application Example 1). The thermal conductivity of this cured coating was measured, and the thermal conductivity of the cured coating of Comparative Application Example 1, formed using the α-alumina of Comparative Example 13, was 0.49 W / m·K. In contrast, the thermal conductivity of the cured coating of Application Example 1, which was formed using the thermally conductive particles of Example 1, was found to be high at 0.56 W / m·K.

[0074] <Evaluation of Thermally Conductive Particles> (Measurement of Thermal Conductivity (Block)) 50 parts of polypropylene (manufactured by Prime Polymer Co., Ltd., MFR: 20 g / 10 min) and 50 parts of each thermally conductive component were mixed to obtain a resin composition, which was placed in a Plastomill and melt-kneaded at a set temperature of 200°C. Next, using a mold measuring 20 mm in length, 20 mm in width, and 6 mm in height, test pieces were obtained by mold press molding at 175°C. The thermal conductivity of the obtained test pieces was measured using the "Standard Isotropic Measurement Module" of a thermal property measuring device (product name "TPS-2500S", manufactured by Kyoto Electronics Manufacturing Co., Ltd.). The thermal conductivity of the test piece formed using α-alumina of Comparative Example 13 was 0.43 W / m·K. In contrast, the thermal conductivity of the test piece formed using the thermally conductive particles of Example 4 was found to be high at 0.59 W / m·K.

[0075] (Dielectric Breakdown Strength) A resin composition obtained by mixing 30 parts of polypropylene (manufactured by Prime Polymer Co., Ltd., MFR 20 g / 10 min) and 70 parts of thermally conductive particles was placed in a plastomill and melt-kneaded at a set temperature of 200 ° C. Next, a molded body for evaluation was produced by die press molding at 175 ° C. The obtained molded body for evaluation was cut into a size of 100 mm x 100 mm x 1 mm thick to obtain a test piece. The obtained test piece was immersed in oil, and the dielectric breakdown voltage was measured in accordance with JIS K6911 and C2110-1 under conditions of an AC of 10 mA and a voltage rise rate of 2 kV / sec. The dielectric breakdown strength (kV / mm) obtained by dividing the measured dielectric breakdown voltage value by the thickness (mm) of the test piece is shown in Table 3.

[0076]

Claims

1. Thermally conductive particles containing at least an aluminum raw material, a zinc raw material, and a calcined product obtained by calcining other raw materials other than the aluminum raw material and the zinc raw material, wherein the content of the zinc raw material relative to 100 parts by mass of the aluminum raw material is 25 parts by mass or more and 70 parts by mass or less, the other raw materials contain at least one selected from the group consisting of boron compounds, tungsten compounds, titanium compounds, bismuth compounds, and fluorine compounds, and the content of the other raw materials relative to 100 parts by mass of the aluminum raw material is 0.05 parts by mass or more and 20 parts by mass or less, and the thermally conductive particles satisfy the following conditions: (1) A thermally conductive particle having 50 g of the thermally conductive particles and an epoxy equivalent of 200 g / eq or more and 1000 g / eq or less, measured by an E-type viscometer at a measurement temperature of 25°C, a cone rotor (3° x R9.7), and a rotation speed of 100 s -1 The resin composition for viscosity measurement obtained by the above method was kneaded for 1 minute at 1,000 rpm and 1 minute at 2,000 rpm using an E-type viscometer at a measurement temperature of 25° C., a cone rotor (3°×R9.7), and a rotation speed of 100 s. -1(2) 500 parts by mass of SUS304 steel balls having a diameter of 5 mm and 100 parts by mass of the thermally conductive particles are placed in a 250 mL wide-mouthed cylindrical container, and rotated at 80 rpm for 3 hours with the central axis of the cylinder of the cylindrical container as the rotation axis, and then the steel balls and the thermally conductive particles are separated using a sieve with a mesh size of 1 mm to obtain thermally conductive particles after the abrasion test, and 4 parts by mass of the thermally conductive particles before and after the abrasion test and 8 parts by mass of lithium borate are mixed and ground in a mortar for 5 minutes. The strength of the iron element is measured using a fluorescent X-ray analyzer, and the abrasion degree calculated by the following formula for the fluorescent X-ray strength (kcps) of the iron element before and after the abrasion test is 4 kcps or less. Abrasion degree = (fluorescent X-ray intensity of iron element after abrasion test) - (fluorescent X-ray intensity of iron element before abrasion test) (3) A resin composition obtained by kneading 30 parts of a mixed liquid obtained by mixing an epoxy resin having an epoxy equivalent of 200 g / eq or more and 1000 g / eq or less and an amine-based curing agent having an amine value of 100 mgKOH / g or more and 500 mgKOH / g or less in a ratio of 3:1 to 4:1 with 70 parts of thermally conductive particles is pressed into a mold into a circular sheet molded product having a diameter of 100 mm or more and a thickness of 4 mm or more, heat-cured at a set temperature of 120°C for 1 hour, and cut into four equal parts so as to form a sector shape with a central angle of 90° after cooling. The thermal conductivity of the test piece measured by hot disk thermophysical property measurement is 0.80 W / m·K or more.

2. The thermally conductive particles according to claim 1, wherein the other raw materials (excluding fluorine compounds) are at least one selected from the group consisting of oxides, oxoacid salts, hydroxides, carbonates, and basic carbonates.

3. The thermally conductive particles according to claim 1, which contain at least one element selected from the group consisting of iron, cobalt, copper, manganese, nickel, and chromium and are colored.

4. A mixture obtained by mixing the thermally conductive particles according to any one of claims 1 to 3 with a thermally conductive filler.

5. The mixture of claim 4, wherein the thermally conductive filler is at least one selected from the group consisting of barium sulfate, talc, boron nitride, and magnesium oxide.

6. A method for producing thermally conductive particles according to any one of claims 1 to 3, comprising firing a raw material mixture containing an aluminum raw material, a zinc raw material, and raw materials other than the aluminum raw material and the zinc raw material, wherein the aluminum raw material is at least one selected from the group consisting of boehmite, aluminum hydroxide, and alumina, and the zinc raw material is at least one selected from the group consisting of zinc oxide and basic carbonate.

7. A method for producing thermally conductive particles, comprising firing the raw material mixture according to claim 6 at a temperature of 1,000°C or higher and 1,600°C or lower.

8. An article containing the thermally conductive particles according to any one of claims 1 to 3.

9. The article according to claim 8, which is any one of a gravure ink, a coating liquid, a resin composition, and an adhesive composition.

10. A resin composition used to form a thermally conductive resin composition, comprising the mixture according to claim 4 and a forming resin.

11. The resin composition according to claim 10, wherein the content of the mixture relative to the entire molding resin is 5% by mass or more and 95% by mass or less.

12. A thermally conductive thin film formed by coating the article according to claim 9.

13. The article according to claim 8, which is used as a heat dissipation member in any one of an electronic device part, an electronic device housing, an EV motor, and a lithium battery.

Citation Information

Patent Citations

  • Spherical zinc oxide particle powder and high thermal conductivity composition

    JP2009249226A

  • Alumina-based thermally conductive rounded discoid particles and their manufacturing method, thermally conductive compositions, articles, liquid compositions, thermally conductive thin films, and electronic device components

    JP7185798B1

  • Package for accommodating semiconductor device

    JP2003100932A

  • Thermally conductive complex oxide, production method therefor, thermally conductive complex oxide-containing composition, and use therefor

    WO2015137468A1

  • Alumina-based thermally conductive oxide and method for producing same

    WO2018159608A1