Additive manufacturing metal powder and method for producing additive manufacturing metal powder
By attaching laser-absorbing powders like TiB2 or Y2O3 to copper-containing particles, the additive manufacturing process overcomes the low laser absorption issue of copper powders, resulting in high-density, high-conductivity objects.
Patent Information
- Application Number
- PCT/JP2023/045134
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-27
- Filing Date
- 2023-12-15
- Publication Date
- 2024-10-03
AI Technical Summary
Copper and copper alloy powders used in additive manufacturing have low laser absorption rates, leading to inefficient melting or sintering and resulting in objects with low density and conductivity due to the difficulty in absorbing the laser beam effectively.
A method involving the attachment of laser-absorbing powders such as TiB2 or Y2O3 to the surface of copper-containing particles to enhance the laser absorption rate, promoting efficient melting and sintering, and improving the electrical conductivity of the produced objects.
The enhanced laser absorption rate results in the production of high-density objects with improved electrical conductivity, achieving conductivity levels of 90% IACS or higher after aging treatment.
Smart Images

Figure JP2023045134_03102024_PF_FP_ABST
Abstract
Description
Metal powder for additive manufacturing and method for manufacturing metal powder for additive manufacturing
[0001] This specification discloses metal powders for use in additive manufacturing and methods for their production.
[0002] In metal additive manufacturing, which is one of the additive manufacturing (so-called AM) technologies, for example, a laser beam or electron beam is irradiated onto a thin layer of metal powder based on cross-sectional data of the object to be manufactured, and a layer is formed by melting and solidifying or sintering part of the powder, and then the metal powder is deposited on top of that and the laser beam or the like is irradiated repeatedly to stack the layers and manufacture the object.
[0003] In order to manufacture a copper or copper alloy object, which has excellent electrical and thermal conductivity, by such additive manufacturing, copper powder or copper alloy powder is used as the metal powder.
[0004] Here, copper and copper alloys not only have low laser absorptivity, but also have high thermal conductivity, which means that heat from the laser beam easily escapes. For this reason, copper powder and copper alloy powder cannot be sufficiently melted or sintered unless they are irradiated with a laser beam of higher power than normal for a relatively long period of time, which may make it difficult to efficiently perform additive manufacturing. In response to this, for example, Patent Document 1 aims to "provide copper powder for 3D printers that has high absorptivity during laser irradiation and can be fused and bonded with a low-energy laser by enabling efficient heat input, and a method for manufacturing the same." It proposes a copper powder having an absorptivity of 18.9% to 65.0% for light with a wavelength λ = 1060 nm, and an index represented by the absorptivity / oxygen concentration for light with a wavelength λ = 1060 nm of 3.0 or more.
[0005] Furthermore, with regard to copper alloy powder, Patent Document 2 describes "a metal powder for additive manufacturing, which contains 0.10% by mass or more and 1.00% by mass or less of at least one of chromium and silicon, the total amount of the chromium and the silicon being 1.00% by mass or less, and the remainder being copper." Patent Document 2 states that such a "metal powder" "provides an additive manufacturing product made of a copper alloy that can achieve both mechanical strength and electrical conductivity."
[0006] JP 2018-178239 A JP 2016-211062 A
[0007] However, copper powder or copper alloy powder has low laser absorption rate, and therefore when it is used for additive manufacturing, the laser beam is hardly absorbed in the copper powder or copper alloy powder, which results in insufficient melting or sintering of the copper powder or copper alloy powder, resulting in a molded product with low density and electrical conductivity.
[0008] This specification provides a metal powder for additive manufacturing that has a relatively high laser absorption rate and can contribute to improving the conductivity of the object produced when additive manufacturing is performed, and a method for manufacturing the metal powder for additive manufacturing.
[0009] The metal powder for additive manufacturing disclosed in this specification comprises copper-containing particles containing copper, and laser-absorbing powder adhered to the surfaces of the copper-containing particles.
[0010] The method for producing a metal powder for additive manufacturing disclosed in this specification includes the steps of mixing copper powder or copper alloy powder with a laser-absorbing powder and adhering the laser-absorbing powder to the surfaces of copper-containing particles of the copper powder or copper alloy powder.
[0011] The above-mentioned metal powder for additive manufacturing has a relatively high laser absorptivity, which can contribute to improving the electrical conductivity of the object produced by additive manufacturing.
[0012] FIG. 2 is a cross-sectional view schematically showing a powder adhesion particle contained in the metal powder for additive manufacturing of one embodiment.
[0013] Hereinafter, embodiments of the metal powder for additive manufacturing and a method for manufacturing the same will be described in detail with reference to the drawings. Note that, although reference numerals will be used as needed in the description, reference numerals may be omitted when not needed.
[0014] (Metal Powder) One embodiment of the metal powder for additive manufacturing (hereinafter also simply referred to as "metal powder") includes, as schematically shown in FIG. 1 , powder-adhered particles 3 each including a copper-containing particle 1 containing copper and a laser-absorbing powder 2 attached thereto.
[0015] The copper-containing particle 1 is made of copper or a copper alloy containing copper. In the case of a copper-containing particle 1 made of copper, the copper content of the metal powder is, for example, 99.9% by mass or more. In the case of a copper-containing particle 1 made of a copper alloy, the metal powder contains, for example, 90% by mass to 99.9% by mass of copper and, as alloying elements, one or more selected from the group consisting of Al, Cr, Fe, Ni, Nb, P, Si, Ti, Zn, and Zr, and when multiple elements are included, the total content of these elements may be 0.1% by mass to 10% by mass. The copper and alloying element contents of the metal powder can be measured by inductively coupled plasma optical emission spectroscopy (ICP-OES).
[0016] Laser-absorbing powder 2 adheres to the periphery of copper-containing particle 1. As a result, when the metal powder is used for additive manufacturing, absorption of the laser beam by copper-containing particle 1 is promoted by laser-absorbing powder 2 around copper-containing particle 1, making it easier to melt or sinter copper-containing particle 1. As a result, a high-density molded object can be produced, and it is expected that the conductivity of the molded object will be high.
[0017] The laser-absorbing powder 2 is preferably a substance with a higher melting point than copper. Furthermore, the laser-absorbing powder 2 preferably contains an element or compound that does not easily react with copper. This is because if the laser-absorbing powder 2 contains an element or compound that can dissolve in copper, the resulting product may not have a very high electrical conductivity due to the element or compound dissolving in copper during additive manufacturing. Furthermore, if the copper-containing particles 1 are made of a copper alloy, the substance contained in the laser-absorbing powder 2 is preferably a substance that reacts with and precipitates an alloying element that is dissolved in copper. When this substance reacts with the alloying element and precipitates, the parent phase becomes substantially pure copper, improving electrical conductivity.
[0018] Specific examples of the material for the laser absorbing powder 2 include simple boron (B), borides such as TiB2, and oxides such as Y2O3.
[0019] When the laser-absorbing powder 2 contains B, the B in the laser-absorbing powder 2 may be in the form of a simple substance, or TiB2. For example, the laser-absorbing powder 2 to be attached to the surface of a copper-containing particle 1 made of copper may contain TiB2. Alternatively, the laser-absorbing powder 2 to be attached to the surface of a copper-containing particle 1 made of a copper alloy (Cu-Ti alloy, etc.) may contain simple substance B. The B in the laser-absorbing powder 2 attached to the surface of the copper-containing particle 1 made of a copper alloy reacts with the alloy element and precipitates during additive manufacturing, turning the matrix into substantially pure copper and improving electrical conductivity.
[0020] When the laser-absorbing powder 2 adhered to the periphery of the copper-containing particle 1 contains TiB, the metal powder containing such powder-adhered particles 3 contains Ti and B. The Ti content of the metal powder is preferably 1 mass% or less, more preferably 0.5 mass% or less, relative to the total mass of the metal powder. By reducing the Ti content to a certain level, the electrical conductivity of the shaped object can be effectively improved. The Ti content may be, for example, 0.01 mass% or more, and typically 0.1 mass% to 0.5 mass%. When the laser-absorbing powder 2 contains TiB, it is desirable to change the B content depending on the Ti content. The mass-based ratio of B content / (Ti content + B content) is preferably 0.1 or more and less than 0.5, and more preferably 0.2 or more and less than 0.4. When the B content / (Ti content + B content) is within this range, TiB can be expected to be formed in the shaped object. When TiB2 is formed in the molded product, the matrix becomes almost pure copper, improving electrical conductivity.
[0021] The Ti content and B content of the metal powder can be measured by inductively coupled plasma optical emission spectroscopy (ICP-OES).
[0022] When the laser-absorbing powder 2 adhering to the periphery of the copper-containing particle 1 contains YO, the metal powder containing such powder-adhered particles 3 contains Y. The Y content of the metal powder is preferably 1% by mass or less, more preferably 0.5% by mass or less, relative to the total mass of the metal powder. If the Y content is too high, the electrical conductivity of the shaped object will not be improved. The Y content may be, for example, 0.01% by mass or more, and typically 0.1% to 0.5% by mass. The oxygen content is desirably varied depending on the Y content, and the mass-based oxygen content / (Y content + oxygen content) is preferably 0.1 or more and less than 1, more preferably 0.2 or more and less than 0.4. When the oxygen content / (Y content + oxygen content) is within this range, it is expected that YO will be formed within the shaped object. When YO is formed within the shaped object, the matrix becomes substantially pure copper, improving electrical conductivity.
[0023] The Y content of the metal powder can be measured by inductively coupled plasma optical emission spectroscopy (ICP-OES). The oxygen content of the metal powder can be measured by inert gas fusion. Here, using a TCH600 manufactured by LECO Corporation, two measurements are taken for a 1 g sample of the metal powder, and the average value is used as the oxygen content.
[0024] As described above, it can be confirmed by X-ray photoelectron spectroscopy (XPS) that the laser absorbing powder 2 attached to the periphery of the copper-containing particle 1 contains TiB2 and Y2O3.
[0025] The average particle diameter D50 of the metal powder is preferably 10 μm to 150 μm. By not making the average particle diameter D50 too small, the metal powder is less likely to fly around during molding, making it easier to handle, and the required fluidity is exerted, allowing it to be spread in the intended location, improving moldability. By keeping the average particle diameter D50 at a certain size, the energy required to melt or sinter the metal powder with a laser beam can be reduced, and the precision of the molding can be improved.
[0026] The average particle diameter D50 is the particle diameter at which the cumulative volume-based frequency of the metal powder reaches 50% in the particle diameter histogram (particle diameter distribution graph) obtained by measuring the particle diameter of the metal powder using a laser diffraction / scattering particle diameter distribution analyzer, and is measured in accordance with JIS Z8825 (2013). More specifically, the average particle diameter D50 can be measured using an MT3300EXII manufactured by Microtrac-Bell, with pure water as the solvent and a refractive index of 1.33.
[0027] Since typical laser-based additive manufacturing uses a fiber laser with a wavelength of about 1060 nm, the laser absorptance of metal powder is calculated by measuring the reflectance at a wavelength of 1060 nm using the following equipment and conditions. The laser absorptance of metal powder is preferably 15% or higher, and more preferably 25% or higher. Manufacturer: Shimadzu Corporation Equipment name: Spectrophotometer (MPC-3100, powder holder used) Measurement wavelength: 300-1500 mm Slit width: 20 nm Reference: BaSO4 Measured physical property: Reflectance Absorbance (%) = 1 - (Reflectance (%))
[0028] (Manufacturing Method) To manufacture the metal powder described above, for example, copper powder or copper alloy powder is first prepared. The copper powder or copper alloy powder may be prepared by purchasing already manufactured powder or by other methods, such as atomization.
[0029] The copper powder mainly contains copper-containing particles containing copper, and preferably has a copper content of 99.9% by mass or more (purity of 3N or more). The copper alloy powder mainly contains copper-containing particles containing a copper alloy. The copper alloy powder may have a copper content of 80% by mass or more, more preferably 85% by mass or more, even more preferably 90% by mass or more, or even more preferably 99% by mass or more, and may contain, in addition to copper, one or more alloy elements selected from the group consisting of Al, Cr, Fe, Ti, Ni, Nb, P, Si, Zn, and Zr.
[0030] The copper powder or copper alloy powder preferably has an average particle diameter D50 of 10 μm to 150 μm, the particle size of which is adjusted by sieving or the like as necessary. This average particle diameter D50 is the same as the average particle diameter D50 described above for metal powders, and can be measured by the same method.
[0031] By mixing the copper powder or copper alloy powder with a laser-absorbing powder, the laser-absorbing powder adheres to the surfaces of the copper-containing particles, thereby producing a metal powder.
[0032] The laser-absorbing powder to be mixed with the copper-containing particles of the copper powder or copper alloy powder is preferably a powder with a fine particle size. The average particle size D50 of the laser-absorbing powder is preferably 10 μm or less. This average particle size D50 is the same as the average particle size D50 described above.
[0033] However, fine laser-absorbing powders, for example, having an average particle size D50 of 10 μm or less, may be agglomerated. If the laser-absorbing powder is highly agglomerated, the agglomerations can be easily eliminated by mixing the powder with copper powder or copper alloy powder and then sieving the powder together with the copper powder or copper alloy powder.
[0034] Any mixing method can be used, such as mixing with a ball mill or a mixer. For example, copper powder or copper alloy powder is charged into a ball mill, and then a laser-absorbing powder such as TiB powder, B powder, or YO powder is charged, and the ball mill is rotated at 50 rpm or more for about 10 to 90 minutes, to obtain a metal powder containing powder-adhered particles 3 as shown in FIG.
[0035] By carrying out the above-described steps, it is possible to produce a metal powder containing copper-containing particles and laser-absorbing powder.
[0036] Next, the metal powder for additive manufacturing described above was prototyped and its effects were confirmed, which will be described below. However, the description here is for illustrative purposes only and is not intended to be limiting.
[0037] Pure copper powder or copper alloy powder having an average particle size D50 of approximately 30 μm to 45 μm was prepared. The pure copper powder had a copper content of 99.9 mass %, and the copper alloy powder contained 0.3 mass % Ti.
[0038] Example 1 The above copper powder was mixed with TiB2 powder (laser absorbing powder) for 30 minutes using a ball mill to prepare a metal powder in which the laser absorbing powder adhered to the surfaces of the copper-containing particles.
[0039] Example 2 The above copper powder was mixed with Y2O3 powder (laser absorbing powder) for 30 minutes using a ball mill to prepare a metal powder in which the laser absorbing powder adhered to the surfaces of copper-containing particles.
[0040] Example 3 The above copper alloy powder was mixed with powder B (laser absorbing powder) for 30 minutes using a ball mill to prepare a metal powder in which the laser absorbing powder adhered to the surfaces of copper-containing particles.
[0041] Comparative Example 1 The above copper powder was used as it was as a metal powder.
[0042] (Evaluation) The average particle size D50 and the contents of the constituent components of the laser-absorbing powder were confirmed for each of the above metal powders by the method described above, and the results were as shown in Table 1. The metal powders of Examples 1 and 2 were analyzed by the method described above, and it was confirmed that laser-absorbing powders of predetermined materials were present in each of them.
[0043] To confirm the effect of each metal powder, a 20 mm cube was fabricated using a Renishaw AM400 molding machine with an output of 400 W and a scanning speed of 400 mm / sec.
[0044] The density of the above-mentioned molded object was determined by measuring the proportion of the area occupied by voids in an image observed with an optical microscope. The relative density was calculated using the formula: relative density = ((area of molded object - area of voids) / area of molded object) x 100 (%). Note that the same calculation was also performed when a molded object was produced using a metal powder produced using a copper alloy powder.
[0045] The electrical conductivity was calculated from the current value of the eddy current generated by passing an eddy current through the molded object. Furthermore, the molded object was subjected to an aging treatment in an Ar atmosphere at 1000°C for two hours in Example 1, and at 700°C for two hours in Example 3, to confirm whether the electrical conductivity could be increased.
[0046] The results are shown in Table 1.
[0047]
[0048] The conductivity of Comparative Example 1 was less than 80%, while the objects of Examples 1 and 3, which were fabricated under the same conditions, achieved a conductivity of 90% IACS or higher after aging treatment. Example 2 achieved a conductivity of 95% IACS or higher even without aging treatment. This confirmed the effectiveness of the laser-absorbing powder.
[0049] From the above, it was found that the metal powder described above has improved laser absorption rate and is effective for manufacturing objects with high conductivity.
[0050] 1 Copper-containing particles 2 Laser-absorbing powder 3 Powder-adhered particles
Claims
1. A metal powder for use in additive manufacturing, comprising copper-containing particles containing copper and laser-absorbing powder adhered to the surfaces of the copper-containing particles.
2. The metal powder for additive manufacturing according to claim 1, wherein the laser-absorbing powder contains B.
3. The metal powder for additive manufacturing according to claim 2, wherein the laser absorbing powder contains TiB2.
4. The metal powder for additive manufacturing according to claim 3, wherein the Ti content is 0.1% by mass to 0.5% by mass relative to the total mass of the metal powder.
5. The metal powder for additive manufacturing according to claim 1, wherein the laser-absorbing powder contains an oxide.
6. The metal powder for additive manufacturing according to claim 5, wherein the oxide is Y2O3.
7. The metal powder for additive manufacturing according to claim 6, wherein the Y content is 0.1% by mass to 0.5% by mass relative to the total mass of the metal powder.
8. The metal powder for additive manufacturing according to any one of claims 1 to 7, wherein the average particle size D50 is 10 μm to 150 μm.
9. A method for producing metal powder for use in additive manufacturing, comprising the steps of mixing copper powder or copper alloy powder with a laser-absorbing powder and adhering the laser-absorbing powder to the surfaces of copper-containing particles of the copper powder or copper alloy powder.
10. A method for producing a metal powder for additive manufacturing as described in claim 9, wherein the laser absorbing powder used is a laser absorbing powder containing TiB2 or Y2O3.
Citation Information
Patent Citations
Copper alloy powder, manufacturing method of laminate molded article and laminate molded article
JP2016211062A
Copper powder, manufacturing method therefor, and manufacturing method of solid molded article
JP2018178239A
Method for manufacturing quasicrystal-nanocrystalline modified gradient composite in laser additive mode
CN107723511A
Surface modified metal powder with high laser reflectivity and 3D printing method
CN109746435A
An additional manufacturing method of parts by melting or sintering powder particles, using a powder suitable for the target method / material combination together with a high-energy beam
JP2016532773A
Cited By
Powder for additive manufacturing
WO2026069891A1