Rail and method for manufacturing same
The rail steel composition and controlled cooling process address the issue of rail breakage by achieving optimal 0.2% proof stress and fracture toughness, enhancing the rail's resistance to mechanical loads and preventing crack formation, thus improving rail durability.
Patent Information
- Application Number
- PCT/JP2024/001011
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-24
- Filing Date
- 2024-01-16
- Publication Date
- 2024-10-03
AI Technical Summary
Rail transportation efficiency improvements lead to increased stress on rails, causing frequent breakage from the bottom due to inadequate resistance to tensile and compressive stresses, despite previous attempts to enhance rail bottom strength through composition and cooling methods.
A rail steel composition with specific elemental ranges (C: 0.60-0.90%, Si: 0.10-1.20%, Mn: 0.10-1.50%, Cr: 0.05-2.00%, and others) is used, combined with a controlled cooling process (average rate of 0.4°C/sec to 6.0°C/sec from 650°C to 400°C/600°C) to achieve a 0.2% proof stress of 500-1100 MPa and fracture toughness of 26MPa m^1/2 at -20°C, suppressing crack occurrence and enhancing resistance to mechanical loads.
The solution effectively prevents rail breakage by controlling crack formation and increasing resistance to mechanical loads, ensuring the rail's durability under increased usage conditions.
Smart Images

Figure JP2024001011_03102024_PF_FP_ABST
Abstract
Description
Rail and manufacturing method thereof
[0001] The present invention relates to a rail and a method for manufacturing the same.
[0002] Compared to other modes of transport, rail transport is highly efficient and environmentally friendly, and efforts are being made to increase transport capacity through measures such as increasing operating speeds, increasing freight car loads, and congested timetables. As a result, the number of wheels passing over rails is also increasing, and repeated tensile and compressive stresses are applied to the rails, causing them to break from the bottom, and the frequency of rail replacement is gradually increasing, becoming a problem. Therefore, there is a growing demand for rail steel that can reduce breakage from the bottom.
[0003] Therefore, various studies have been conducted with the aim of further improving the prevention of breakage from the rail bottom. For example, Patent Document 1 describes a steel rail with a pearlite structure containing 0.65 to 1.40% C, in which pearlite blocks with grain sizes of 1 to 15 μm are present in an area of 0.2 mm2 at least in a region extending from the bottom surface to a depth of 10 mm. 2 More than 200 rails have been disclosed.
[0004] Patent Document 2 discloses a rail in which, after rail rolling, the rail head is accelerated cooled from the austenite region while the rail bottom surface is accelerated cooled between 800 and 450°C at a cooling rate of 1 to 5°C / sec, resulting in an average hardness of pearlite at the rail bottom surface of HB 320 or more.
[0005] Patent Document 3 discloses a rail containing, by mass%, 0.65 to 1.20% C, 0.05 to 2.00% Si, and 0.05 to 2.00% Mn, with the remainder being Fe and unavoidable impurities, in which 97% or more of the head surface and bottom surface are pearlite structures, the surface hardness of the pearlite structure is in the range of Hv 320 to 500, the maximum surface roughness is 180 μm or less, and the ratio of the surface hardness to the maximum surface roughness is 3.5 or more.
[0006] JP 2006-57127 A JP 1-139724 A International Publication No. 2011 / 021582
[0007] The rails described in Patent Documents 1 to 3 can control the structure of the rail bottom portion and increase the strength of the rail bottom portion, but this alone is insufficient to suppress the occurrence of cracks in the rail bottom portion or to control resistance to fracture when a mechanical load is applied to the rail bottom portion if a crack exists in the rail bottom portion, which may result in breakage from the rail bottom portion.
[0008] To prevent breakage from the rail bottom, it is effective to prevent cracks from occurring at the rail bottom and, if cracks exist at the rail bottom, to increase resistance to fracture when a mechanical load is applied. The present invention was made to solve this problem, and provides a rail, together with a manufacturing method thereof, that can prevent cracks from occurring at the rail bottom and increase resistance to cracks by controlling the chemical composition of the rail and controlling the 0.2% proof stress and fracture toughness of the rail bottom within predetermined ranges.
[0009] The gist of the present invention is as follows: [1] In mass%, C: 0.60% or more and less than 0.90%, Si: 0.10 to 1.20%, Mn: 0.10 to 1.50%, Cr: 0.05 to 2.00%, Al: 0.0002 to 0.005%, P: 0 to 0.035%, S: 0 to 0.020%, V: 0 to 0.30%, Cu: 0 to 1.0%, Ni: 0 to 1.0%, Nb: 0 to 0.05%, Mo: 0 to 0.5%, B: 0 to 0.0050%, Ti: 0 to 0.01%, Mg: 0 to 0.01%, Ca: 0 to 0.02%, W: 0 to 0.10%, Sb: 0 to 0.05%, Sn: 0 to 0.05%, and Co: 0 to 1.0% The 0.2% proof stress of the rail bottom portion is more than 500 MPa and less than 1100 MPa, and the fracture toughness of the rail bottom portion at -20°C is 26.0 MPa m 1 / 2[2] The rail according to [1], wherein the chemical composition contains, in mass%, one or more elements selected from the group consisting of V: 0.001 to 0.30%, Cu: 0.001 to 1.0%, Ni: 0.001 to 1.0%, Nb: 0.001 to 0.05%, Mo: 0.001 to 0.5%, B: 0.0001 to 0.0050%, Ti: 0.001 to 0.01%, Mg: 0.0005 to 0.01%, Ca: 0.0005 to 0.02%, W: 0.001 to 0.10%, Sb: 0.001 to 0.05%, Sn: 0.001 to 0.05%, and Co: 0.001 to 1.0%. [3] A method for manufacturing a rail as set forth in [1] or [2], comprising hot rolling a steel bloom having the chemical composition as set forth in [1] or [2], followed by cooling the center of the bottom of the rail from a cooling start point T1 to a cooling end point T2 at an average cooling rate of 0.4°C / sec to 6.0°C / sec, wherein T1 is a temperature in the range of 650°C to 800°C, and T2 is a temperature in the range of 400°C to 600°C.
[0010] Here, the 0.2% proof stress at the rail bottom and the stress intensity factor range ΔK at the rail bottom are 15 MPa m 1/2 The fatigue crack propagation rates at these times are values measured by the method described in the Examples.
[0011] According to the present invention, it is possible to provide a rail, together with a manufacturing method thereof, that can suppress the occurrence of cracks at the rail bottom, and, if a crack exists at the rail bottom, increase resistance to fracture when a mechanical load is applied, thereby suppressing breakage from the rail bottom.
[0012] FIG. 1 is a cross-sectional view of a rail; FIG. 2 is a diagram showing the cross-sectional area and thickness of the bottom of the rail; FIG. 3 is a diagram showing the position where a tensile test specimen was taken; FIG. 4 is a diagram showing the dimensions of the tensile test specimen; FIG. 5 is a diagram showing the position where a fracture toughness test specimen was taken; and FIG. 6 is a diagram showing the dimensions of the fracture toughness test specimen.
[0013] <Rail parts> The designations of the various rail parts in the present invention will be explained with reference to the rail cross-sectional view in Figure 1. In the rail 1 shown in Figure 1, 11 is the head, 12 is the web, and 13 is the bottom (foot). The bottom center refers to the center in the width direction of the back surface of the bottom.
[0014] <Composition of Rail> The composition of the steel of the rail of the present invention will be described. In the following description, "%" represents "mass %" unless otherwise specified.
[0015] C: 0.60% or more but less than 0.90% C is an essential element for forming cementite in pearlite structures and ensuring 0.2% yield strength. The 0.2% yield strength improves with increasing C content. If the C content is less than 0.60%, it is difficult to obtain excellent 0.2% yield strength and fracture toughness. Therefore, the C content is set to 0.60% or more, preferably 0.63% or more, and more preferably 0.70% or more. Furthermore, if the C content is 0.90% or more, pro-eutectoid cementite forms at austenite grain boundaries during transformation after hot rolling, reducing the rail's fracture toughness. As a result, the fracture toughness value significantly decreases. Therefore, the C content is set to less than 0.90%, preferably 0.89% or less, and more preferably 0.85% or less.
[0016] Si: 0.10-1.20% Si is a deoxidizing agent and a strengthening element for the pearlite structure, and 0.10% or more is required to fully obtain this effect. The Si content is preferably 0.15% or more, and more preferably 0.20% or more. If the Si content exceeds 1.20%, martensite structure is more likely to form, which increases the 0.2% proof stress and increases the amount of Si oxide, resulting in a decrease in fracture toughness. The Si content is 1.20% or less, preferably 1.10% or less, and more preferably 1.00% or less.
[0017] Mn: 0.10 to 1.50% Mn is an element that strengthens the pearlite structure, and 0.10% or more is required to fully obtain this effect. The Mn content is preferably 0.20% or more, and more preferably 0.30% or more. If the Mn content exceeds 1.50%, the high hardenability of Mn makes it more likely that a martensite structure will form, which may result in an excessive increase in 0.2% proof stress and a decrease in fracture toughness. Therefore, the Mn content is set to 1.50% or less, preferably 1.40% or less, and more preferably 1.30% or less.
[0018] P: 0 to 0.035% If P is contained in an amount exceeding 0.035%, the ductility, which is a characteristic of the rail itself, deteriorates. Therefore, the P content is set to 0.035% or less, and preferably 0.020% or less. The lower limit of the P content is not particularly limited and may be 0%, but setting it to less than 0.001% would inevitably increase steelmaking costs, so the P content can be set to 0.001% or more.
[0019] S: 0 to 0.020% S is an element present in steel mainly in the form of A-type inclusions. If the S content exceeds 0.020%, the amount of these inclusions increases significantly, and at the same time, coarse inclusions are formed, which deteriorates the cleanliness of the rail steel and reduces the fracture toughness of the rail. Therefore, the S content is set to 0.020% or less, preferably 0.015% or less, and more preferably 0.010% or less. The lower limit of the S content is not particularly limited and may be 0%, but setting it to less than 0.0005% would necessitate an increase in steelmaking costs, so the S content can be set to 0.0005% or more.
[0020] Cr: 0.05% or more and 2.00% or less. Cr is an element that increases the pearlite equilibrium transformation temperature and contributes to refinement of lamellar spacing. At the same time, the inclusion of Cr can further increase the 0.2% yield strength through solid solution strengthening. Since a Cr content of less than 0.05% does not provide sufficient 0.2% yield strength, the Cr content is set to 0.05% or more, preferably 0.10% or more, and more preferably 0.15% or more. If the Cr content exceeds 2.00%, the hardenability increases and martensite structure is more likely to form, resulting in an increase in 0.2% yield strength and a decrease in fracture toughness. Therefore, the Cr content is set to 2.00% or less, preferably 1.60% or less, and more preferably 1.40% or less.
[0021] Al: 0.0002 to 0.005% Al is a deoxidizer and strengthens the pearlite structure, and 0.0002% or more is required to fully obtain this effect. If the Al content exceeds 0.005%, the 0.2% proof stress increases and the amount of Al oxide increases, resulting in a decrease in fracture toughness. Therefore, the Al content is set to 0.0002 to 0.005%.
[0022] In addition to the basic components described above, the chemical composition of the rail of the present invention may optionally contain one or more elements selected from the following: V: 0-0.30%, Cu: 0-1.0%, Ni: 0-1.0%, Nb: 0-0.05%, Mo: 0-0.5%, B: 0-0.0050%, Ti: 0-0.01%, Mg: 0-0.01%, Ca: 0-0.02%, W: 0-0.10%, Sb: 0-0.05%, Sn: 0-0.05%, and Co: 0-1.0%. These are optional elements and do not necessarily need to be included, so their lower limit is 0%. However, if these elements are included, the preferred contents are as follows:
[0023] V: 0.001 to 0.30% V forms carbonitrides in steel, disperses and precipitates in the matrix, and improves fracture toughness by increasing 0.2% proof stress. This effect is achieved when the V content is 0.001% or more. Therefore, when V is added, the V content is preferably 0.001% or more, and more preferably 0.005% or more. On the other hand, if the V content exceeds 0.30%, the 0.2% proof stress increases excessively, which may actually decrease fracture toughness. Furthermore, the alloy cost increases, which increases the cost of the rail steel. Therefore, when V is added, the V content is preferably 0.30% or less, and more preferably 0.29% or less.
[0024] Cu: 0.001 to 1.0% Like Cr, Cu is an element that can further increase strength through solid solution strengthening. If the Cu content is less than 0.001%, this effect is small, while if it exceeds 1.0%, Cu cracking becomes more likely to occur. Therefore, if Cu is added, the Cu content is preferably 0.001 to 1.0%.
[0025] Ni: 0.001-1.0% Ni is an element that can increase strength without degrading ductility. Furthermore, adding Ni in combination with Cu suppresses Cu cracking, so it is desirable to add Ni when Cu is added. A Ni content of less than 0.001% is ineffective, while a Ni content of more than 1.0% increases hardenability, martensite is formed, and fracture toughness tends to decrease. Therefore, if Ni is added, the Ni content is preferably 0.001-1.0%.
[0026] Nb: 0.001 to 0.05% Nb is an element that combines with C in steel to precipitate as carbides during and after rolling, improving the 0.2% proof stress and thereby improving fracture toughness, but if the Nb content is less than 0.001%, this effect is small, and if it is contained in excess of 0.05%, no effect commensurate with the content can be obtained. Therefore, if Nb is contained, the Nb content is preferably 0.001 to 0.05%.
[0027] Mo: 0.001 to 0.5% Mo is an element that can further increase strength through solid solution strengthening, but at less than 0.001%, this effect is minimal, while at more than 0.5%, hardenability increases, martensite begins to form, and fracture toughness tends to decrease. Therefore, if Mo is added, the Mo content is preferably 0.001 to 0.5%.
[0028] B: 0.0001 to 0.0050% B is an element that precipitates as a nitride and can further increase the strength of rails through precipitation strengthening. If the B content is less than 0.0001%, this effect is small, while if it exceeds 0.0050%, the alloy cost increases. Therefore, if B is added, the B content is preferably 0.0001 to 0.0050%.
[0029] Ti: 0.001 to 0.01% Ti is an element that precipitates as carbide, nitride, or carbonitride, and can further increase the strength of rails through precipitation strengthening. If the Ti content is less than 0.001%, this effect is small, while if it exceeds 0.01%, the alloy cost increases. Therefore, if Ti is added, the Ti content is preferably 0.001 to 0.01%.
[0030] Mg: 0.0005 to 0.01% Mg is an element that combines with oxygen to precipitate MgO, further increasing strength. If the Mg content is less than 0.0005%, this effect is small, while if it exceeds 0.01%, the increase in MgO tends to cause a decrease in fracture toughness. Therefore, if Mg is added, the Mg content is preferably 0.0005 to 0.01%.
[0031] Ca: 0.0005 to 0.02% Ca is an element that combines with oxygen to precipitate CaO, further increasing strength. If the Ca content is less than 0.0005%, this effect is small, while if it exceeds 0.02%, the increase in CaO makes it more likely that fracture toughness will increase. Therefore, if Ca is added, the Ca content is preferably 0.0005 to 0.02%.
[0032] W: 0.001 to 0.10% W is an element that precipitates as carbides and can further increase the strength of rails through precipitation strengthening. If the W content is less than 0.001%, this effect is small, while if it exceeds 0.10%, it will increase the alloy cost. Therefore, if W is added, the W content is preferably 0.001 to 0.10%.
[0033] Sb: 0.001 to 0.05% Sb is an element that has a significant effect of preventing decarburization of steel during reheating of rail billets in a heating furnace before hot rolling. If the Sb content exceeds 0.05%, it has a negative effect on the ductility and toughness of the steel. Therefore, if Sb is contained, the Sb content is preferably 0.05% or less. On the other hand, if Sb is contained, the Sb content is preferably 0.001% or more in order to exert the effect of reducing the decarburized layer.
[0034] Sn: 0.001 to 0.05% Sn is an element that has a significant effect of preventing decarburization of steel during reheating of rail billets in a heating furnace before hot rolling. If the Sn content exceeds 0.05%, it has a negative effect on the ductility and toughness of the steel. Therefore, if Sn is contained, the Sn content is preferably 0.05% or less. On the other hand, if Sn is contained, the Sn content is preferably 0.001% or more in order to exert the effect of reducing the decarburized layer.
[0035] Co: 0.001 to 1.0% Co is an element that increases the pearlite equilibrium transformation temperature and refines lamellar spacing, thereby further increasing the strength of steel. Co also has the effect of suppressing the precipitation of proeutectoid cementite. If the Co content exceeds 1.0%, martensite forms in the steel, resulting in a decrease in ductility. For these reasons, if the composition contains Co, the Co content is preferably 1.0% or less. There is no particular lower limit for the Co content, but for high strength, it is preferably 0.001% or more. A more preferred range for the Co content is 0.001 to 0.5%.
[0036] The chemical composition of the steel for rails of the present invention, other than the above-mentioned essential and optional elements, consists of Fe and unavoidable impurities. Examples of unavoidable impurities include N and O, with N content up to 0.008% and O content up to 0.004%. Depending on the raw materials, materials, and manufacturing equipment, impurities other than N and O may be unavoidably mixed into the steel. Examples of raw materials include iron ore, reduced iron, and scrap. The above impurities are also acceptable within the scope of the present invention, provided they do not impair the objectives of the present invention. Examples of impurities other than N and O include Pb, Zr, Bi, Zn, Se, As, Te, Tl, Cd, Hf, Ag, Hg, Ga, Ge, and REM.
[0037] <Rail Microstructure> In the microstructure of the rail of the present invention, 95% or more of the area of the rail bottom is pearlite. The remaining structure other than pearlite is permissible as long as its total area is 5% or less, as this does not significantly affect the properties of the present invention. Examples of the remaining structure include ferrite and bainite. The microstructure can be identified by the method described in the Examples.
[0038] <0.2% Yield Strength of Rail Bottom More Than 500 MPa and Less Than 1100 MPa> The rail of the present invention has a 0.2% yield strength in the range of more than 500 MPa and less than 1100 MPa. If the 0.2% yield strength is 500 MPa or less, crack resistance is weak when a wheel passes over the rail, making cracks more likely to occur at the rail bottom due to stress generated within the rail. On the other hand, if the 0.2% yield strength is 1100 MPa or more, the rail bottom becomes stronger, which actually increases sensitivity to cracks after they have occurred and makes the rail more likely to break. Therefore, the 0.2% yield strength of the rail bottom is set to more than 500 MPa, preferably 501 MPa or more, and more preferably 570 MPa or more. Furthermore, the 0.2% yield strength of the rail bottom is set to less than 1100 MPa, preferably 1099 MPa or less, and more preferably 1060 MPa or less.
[0039] <Fracture toughness of the rail base at -20°C is 26 MPa m 1 / 2 The rail of the present invention has a strength of 26 MPa m 1 / 2 The rail bottom has a fracture toughness value of 26 MPa m at -20°C or higher. The fracture toughness value is the resistance to fracture when a mechanical load is applied to the rail bottom if a crack is present. 1 / 2 If the fracture toughness is less than 26 MPa m, the resistance to fracture is low, making the rail particularly susceptible to breakage under assumed operating conditions, including use in cold climates. 1 / 2 or more, preferably 27 Pa m 1 / 2 The upper limit of the fracture toughness value is not particularly limited, but is, for example, 50 Pa m 1 / 2 Here, taking into consideration that the material will be used in cold climates, the fracture toughness value was set to a value at -20°C.
[0040] <Rail Shape> The shape of the rail in the present invention is not particularly limited, and may be any of the rail shapes described in JIS E 1101:2001, BS EN13674-1:2011, American Railway Engineering and Maintenance-of-Way Association (AREMA), etc.
[0041] <Rail Manufacturing Method> A method for manufacturing a rail of the present invention will now be described. The rail of the present invention can be manufactured by hot rolling a steel bloom having the above-described chemical composition, followed by cooling at the center of the rail bottom from the cooling start point T1 to the cooling stop point T2 at an average cooling rate of 0.4°C / sec to 6.0°C / sec. The cooling start point T1 is a temperature in the range of 650°C to 800°C. The cooling start point T1 and the cooling stop point T2 are surface temperatures at the center of the rail bottom measured with a radiation thermometer, and the average cooling rate is the difference between the cooling start point T1 and the cooling stop point T2 at the center of the rail bottom divided by the time required for cooling.
[0042] (Hot Rolling) The blooms used as rail materials have the chemical composition of the rails described above and can be produced by any method. They can be produced by casting, particularly continuous casting. For example, steel can be melted in a converter or electric furnace, and if necessary, subjected to secondary refining such as degassing to adjust the chemical composition of the steel to the above ranges. The melted steel can then be continuously cast into a bloom.
[0043] It is preferable to heat the slab before subjecting it to hot rolling. For example, the slab can be heated to 1200°C or higher and 1350°C or lower in a heating furnace and then hot rolled. In the hot rolling process, hot rolling can be performed using a breakdown rolling mill, a roughing rolling mill, or a finishing rolling mill. In this hot rolling process, the austenite grains that have become coarse due to heating can be refined by rolling and recrystallization in the recrystallization temperature range, or by introducing strain in the non-recrystallization temperature range, thereby refining the structure after pearlite transformation.
[0044] In order to refine the structure after pearlite transformation, the rolling end temperature of the bottom (foot) portion in hot rolling is preferably set to 800°C or higher and 1000°C or lower.
[0045] Furthermore, hot rolling is preferably performed so that the area reduction rate of the bottom portion when rolling at 1050°C or below is 11% or more, more preferably 13% or more. The area reduction rate can be 20% or less, preferably 18% or less. Here, the area reduction rate at 1050°C or below is a value calculated by the equation area reduction rate (%) = {(S0 - S1) / S0} × 100, where S0 is the cross-sectional area of the bottom portion when the temperature drops to 1050°C or below and S1 is the cross-sectional area of the bottom portion after finish rolling. The difference between the thickness reduction rate at 1050°C or below and the area reduction rate at 1050°C or below (thickness reduction rate - area reduction rate) is preferably 4% to 8%, more preferably 5% to 7%. Here, the thickness reduction rate at 1050°C or below is calculated as follows: Thickness reduction rate (%) = {(H0-H1) / H0} × 100, where H0 is the thickness of the bottom portion at 1050°C or below and H1 is the cross-sectional area of the bottom portion after finish rolling. In particular, in the final rolling pass, the reduction rate (thickness reduction rate) in the thickness direction of the bottom portion is preferably equal to or greater than the area reduction rate of that pass. Finish rolling here refers to one final rolling pass performed using the final rolling groove of a single final rolling mill. For example, if the area reduction rate is 11%, the thickness reduction rate at the center of the bottom portion should be 15% or more. This allows for the introduction of large shear strain into the bottom portion, further promoting the refinement of the structure after pearlite transformation and effectively improving the toughness of the back surface of the bottom portion. By designing the groove so that the width dimension of the bottom part is widened in this finish rolling, it is possible to stably perform rolling with a relatively large thickness reduction rate relative to the area reduction rate. By performing finish rolling under these conditions, the 0.2% proof stress of the bottom part is more than 500 MPa and less than 1100 MPa, and the fracture toughness value of the bottom part at -20°C is 26 MPa m 1/2Here, the cross-sectional area of the bottom of the rail is the area of the shaded portion marked with S in the cross-sectional view of the rail in Figure 2, and the thickness of the bottom of the rail is the height marked with H in the same figure.
[0046] Other hot rolling conditions are not particularly limited.
[0047] (Accelerated Cooling) In the manufacturing method of the present invention, accelerated cooling is performed at a predetermined average cooling rate for the center of the rail bottom after hot rolling.
[0048] The cooling start point T1 of accelerated cooling is a temperature in the range of 650°C to 800°C. If the cooling start point is below 650°C, the pearlite transformation temperature will be high and the 0.2% proof stress will decrease. On the other hand, if cooling is performed from above 800°C, martensite tends to form at the bottom of the rail, increasing the 0.2% proof stress and tending to decrease the fracture toughness value. For this reason, the cooling start point is set to 650°C to 800°C.
[0049] The cooling stop point T2 is a temperature in the range of 400°C to 600°C. If the cooling stop point is below 400°C, cooling will continue even after pearlite transformation is complete, increasing the cooling time and reducing productivity. On the other hand, if the cooling stop point is above 600°C, cooling will be stopped before pearlite transformation is complete, resulting in a decrease in 0.2% yield strength. Therefore, the cooling stop point is set to 400°C to 600°C.
[0050] The average cooling rate from the cooling start point T1 to the cooling end point T2 is 0.4°C / sec or more and 6.0°C / sec or less. If the average cooling rate is less than 0.4°C / sec, the 0.2% proof stress of the rail bottom decreases, resulting in a decrease in fracture toughness. On the other hand, if the average cooling rate exceeds 6.0°C / sec, the 0.2% proof stress of the rail bottom increases, resulting in a decrease in fracture toughness. Therefore, the average cooling rate during accelerated cooling is preferably 0.4°C / sec or more and 6.0°C / sec or less, and 0.9°C / sec or more and less than 3.0°C / sec.
[0051] The accelerated cooling method is not particularly limited, and can be, for example, a cooling method using online heat treatment equipment. The cooling medium is not particularly limited, and can be one or more selected from air, spray water, mist, etc., but air is preferably used.
[0052] In the manufacturing method of the present invention, it is important to apply accelerated cooling to the center of the rail base after hot rolling so as to satisfy a predetermined average cooling rate within a predetermined temperature range (between T1 and T2), and as long as this condition is satisfied, there are no particular restrictions on other temperature ranges or cooling of other parts of the rail (e.g., the rail head, etc.). For example, the base (foot) may be accelerated cooled with air to control the average cooling rate of the center of the rail base, while other parts of the rail (e.g., the rail head, etc.) may be allowed to cool naturally or may be accelerated cooled in the same way as the base (foot).
[0053] (Others) After cooling, the rail material may be subjected to known treatments, for example, cold roller straightening.
[0054] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples.
[0055] A billet having the chemical composition shown in Table 1 was heated to 1250°C and then hot rolled into a rail shape (60 kg rail as specified in JIS E 1101:2001) at the finishing rolling temperature shown in Table 2. The area reduction rate at the bottom during rolling at 1050°C or below and the thickness reduction rate at the bottom center during the final rolling pass (finish rolling) were adjusted to satisfy the values shown in Table 2. The rail was then transported to an online heat treatment facility, where the center of the rail bottom was cooled under the cooling conditions shown in Table 2. Cooling was performed by air injection using an air injection device. The rail was then transported to a cooling bed and allowed to cool to room temperature. The cooling start and stop points in Table 2 are the surface temperatures measured at those points using a two-dimensional radiation thermometer capable of measuring the temperature distribution at the center of the rail bottom. The average cooling rate is the average cooling rate between these temperatures.
[0056]
[0057]
[0058] The rails obtained as described above were subjected to a tensile test and evaluated for fracture toughness in the following manner.
[0059] <Tensile test> Tensile test specimens were taken from the rail positions shown in Figure 3 and subjected to tensile tests in accordance with JIS Z2241. The shape of the test specimen is shown in Figure 4. After the tensile test, the 0.2% yield strength and tensile strength were determined.
[0060] <Fracture toughness test> Test specimens according to ASTM E1820-09 were taken from the rail positions shown in Figure 5. The shape of the test specimens is shown in Figure 6. The test specimens were subjected to a test at a test temperature of -20°C using a 250KN autograph tester manufactured by Shimadzu Corporation in accordance with ASTM E1820-09 to determine the fracture toughness values.
[0061] <Microstructure> Test specimens for microstructure observation were cut from the manufactured rails at a depth of 1 mm from the surface of the center of the sole of the rail bottom, mirror-polished, and etched with 1% nitric acid alcohol (1% Nital). The specimens were then microstructure observed at 100x magnification (1200 μm × 950 μm field of view, 10 fields of view) using an optical microscope. If any structures other than pearlite were present, they were photographed, and the structures other than pearlite were traced on the photographed structure. The image analysis software Image-Pro (Nippon Roper Co., Ltd.) was used to calculate the fraction of structures other than pearlite according to the following formula: Fraction of structures other than pearlite = {(area other than pearlite) / (area of pearlite + area of structures other than pearlite)} × 100
[0062] <Drop weight test> A 1500mm long rail was taken from the manufactured rail, and a hole with a diameter of 1.0mm and a depth of 1.0mm was drilled in the center of the bottom of the rail, 750mm from the end. A drop weight test was conducted with the rail head facing up, with a weight dropped from a height of 300mm. All other test conditions were in accordance with JIS E1101. The drop weight test was used to check for the presence or absence of rail breakage, and the rail was judged to be in good condition if no breakage was found.
[0063] From Table 2, it can be seen that the rails of the invention examples all have a 0.2% yield strength of more than 500 MPa and less than 1100 MPa, and a fracture toughness value of 26 MPa m at -20°C. 1 / 2As mentioned above, it can be seen that the results of the drop weight test were also good.
[0064] The present invention makes it possible to provide a rail, together with a manufacturing method thereof, that can suppress the occurrence of cracks at the rail bottom and, in the event that a crack exists at the rail bottom, increase resistance to fracture when a mechanical load is applied, thereby suppressing breakage from the rail bottom, and is therefore highly useful industrially.
[0065] 1 Rail 11 Head 12 Body 13 Bottom (foot)
Claims
1. By mass, C: 0.60% or more but less than 0.90%, Si: 0.10-1.20%, Mn: 0.10-1.50%, Cr: 0.05-2.00%, Al: 0.0002-0.005%, P: 0-0.035%, S: 0-0.020%, V: 0-0.30%, Cu: 0-1.0%, Ni: 0-1.0%, Nb: 0-0.05%, Mo: 0-0.5%, B: 0-0.0050%, Ti: 0-0.01%, Mg: 0-0.01%, Ca: 0-0.02%, W: 0-0.10%, Sb: 0-0.05%, Sn: 0-0.05%, and Co: 0-1.0%. The composition of the steel sheet is such that the 0.2% proof stress of the rail bottom portion is more than 500 MPa and less than 1,100 MPa, and the fracture toughness value of the rail bottom portion at -20°C is 26.0 MPa m 1 / 2 That's it, rails.
2. A rail as set forth in claim 1, wherein the chemical composition contains, by mass, one or more elements selected from the group consisting of V: 0.001-0.30%, Cu: 0.001-1.0%, Ni: 0.001-1.0%, Nb: 0.001-0.05%, Mo: 0.001-0.5%, B: 0.0001-0.0050%, Ti: 0.001-0.01%, Mg: 0.0005-0.01%, Ca: 0.0005-0.02%, W: 0.001-0.10%, Sb: 0.001-0.05%, Sn: 0.001-0.05%, and Co: 0.001-1.0%.
3. A method for manufacturing a rail as claimed in claim 1 or 2, comprising the steps of hot rolling a steel slab having the chemical composition as claimed in claim 1 or 2, and then cooling the slab at the center of the bottom of the rail from a cooling start point T1 to a cooling end point T2 at an average cooling rate of 0.4°C / sec to 6.0°C / sec, wherein T1 is a temperature in the range of 650°C to 800°C, and T2 is a temperature in the range of 400°C to 600°C.
Citation Information
Patent Citations
High-ductility and alpine-cold railway steel rail and production method thereof
CN112239831A
Manufacturing method for improving low-temperature toughness of hot-rolled U75V steel rail through rare earth elements
CN114855082A
Pearlite rail and method for manufacturing pearlite rail
WO2014157252A1
Rail manufacturing method and rail manufacturing apparatus
WO2016047076A1
rail
WO2016117692A1