Core-shell type upconverting microparticle, upconverting micro precursor particle, sensitizing core-shell type upconverting microparticle, tio2-coated core-shell type upconverting microparticle, near-infrared detector, photoelectric conversion element, and method for producing core-shell type upconverting microparticle

Core-shell upconversion microparticles with specific structural features and rare earth compositions address the low sensitivity of conventional photoelectric conversion elements to near-infrared light, achieving efficient conversion and cost-effective production, thereby enhancing detection sensitivity and efficiency.

WO2024202598A1PCT designated stage expired Publication Date: 2024-10-03THE JAPAN SCI & TECH AGENCY
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/004677
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-31
Filing Date
2024-02-09
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Conventional photoelectric conversion elements, such as solar cells and photodiodes, have lower detection sensitivity for near-infrared light compared to visible light, limiting their photoelectric conversion efficiency. There is a need for upconversion particles that can efficiently convert low-energy near-infrared light into high-energy visible light, especially under low excitation conditions like sunlight, and require a more cost-effective production method than traditional hydrothermal methods.

Method used

The development of core-shell type upconversion microparticles with a hexagonal columnar shape, where the core is formed using a sol-gel method under 50°C to 500°C conditions, and a shell is grown using the same method, allowing for efficient upconversion light emission even under low excitation. These particles have a specific size and aspect ratio, with a shell-to-core ratio that enhances luminescence quantum yield and suppresses energy deactivation, using rare earth atoms like Yb, Nd, Tm, and Er for sensitization and emission.

Benefits of technology

The core-shell upconversion microparticles achieve high sensitization characteristics for weak near-infrared light, enabling improved photoelectric conversion efficiency and cost-effective production, with the ability to emit light in the visible range, enhancing detection sensitivity and reducing production costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024004677_03102024_PF_FP_ABST
    Figure JP2024004677_03102024_PF_FP_ABST
Patent Text Reader

Abstract

This core-shell type upconverting microparticle is an upconverting particle comprising a core section and a shell section covering the core section. The core-shell type upconverting microparticle has a hexagonal columnar particle shape, a particle diameter of 300 nm or more, a thickness of 100 nm or more, and an aspect ratio, defined as the particle diameter / particle thickness, of at least 1.2 and not more than 5.0.
Need to check novelty before this filing date? Find Prior Art

Description

Core-shell upconversion microparticles, upconversion microprecursor particles, sensitized core-shell upconversion microparticles, TiO2-coated core-shell upconversion microparticles, near-infrared detectors, photoelectric conversion elements, and methods for producing core-shell upconversion microparticles

[0001] The present invention relates to core-shell upconversion microparticles, upconversion microprecursor particles, sensitized core-shell upconversion microparticles, TiO 2 This application claims priority to Japanese Patent Application No. 2023-058703, filed on March 31, 2023, the contents of which are incorporated herein by reference.

[0002] Photoelectric conversion elements such as solar cells and photodiodes are widely used in various fields. However, conventional photoelectric conversion elements have a problem in that they have lower detection sensitivity for light in the near-infrared region than for light in the visible region. If the detection sensitivity for light in the near-infrared region could be increased to the same level as for visible light, the photoelectric conversion efficiency of, for example, solar cells could be improved. Therefore, there is a demand for photoelectric conversion elements that have high detection sensitivity for light in the near-infrared region as well as for visible light.

[0003] Patent Document 1 discloses a technology using upconversion particles as an inorganic porous material for supporting an organic-inorganic composite perovskite compound, which is a power generation layer. Here, upconversion refers to the phenomenon of converting low-energy light (long-wavelength light, e.g., infrared light) into high-energy light (short-wavelength light, e.g., visible light, ultraviolet light, etc.). Upconversion particles refer to particles that have the function of converting long-wavelength light, such as infrared light, into short-wavelength light, such as visible light or ultraviolet light (upconversion emission). This technology converts long-wavelength light, such as near-infrared light, absorbed by inorganic core-shell particles into short-wavelength light, such as visible light or ultraviolet light, and then reabsorbs this into an organic-inorganic composite perovskite crystal, thereby exciting the light and generating an electromotive force.

[0004] Japanese Patent Application Publication No. 2015-92563

[0005] Currently, there is a demand for upconversion particles that exhibit upconversion luminescence even under low-energy excitation light such as sunlight and that exhibit high sensitization properties to weak light of long wavelengths. While many upconversion particles have been conventionally produced by hydrothermal methods, this method requires synthesis under high-temperature and high-pressure conditions, and therefore, there is a demand for easier, lower-cost production methods.

[0006] Under these circumstances, the inventors of the present invention have employed a sol-gel method and made extensive efforts while focusing on the size and shape of the crystal particles and the core-shell structure, thereby discovering upconversion microprecursor particles that exhibit high luminescence quantum yields. They have also discovered a method that enables the construction of a defect-free crystal structure and the suppression of energy deactivation due to shell formation, thereby arriving at the present invention.

[0007] The present invention has been made in consideration of the above circumstances, and provides core-shell upconversion microparticles, sensitized core-shell upconversion microparticles, TiO, and the like that are capable of upconversion emission even under low excitation light such as sunlight irradiation, can achieve higher sensitization properties using weak light with long wavelengths, and can be manufactured at low cost. 2The present invention aims to provide coated core-shell upconversion microparticles, upconversion microprecursor particles, near-infrared detectors, photoelectric conversion elements, and methods for producing core-shell upconversion microparticles. In the following description, the above-mentioned "core-shell upconversion microparticles" may also be referred to simply as "upconversion particles."

[0008] In order to solve the above problems, the present invention proposes the following means. <1> A core-shell upconversion microparticle of Aspect 1 of the present invention is an upconversion particle comprising a core portion and a shell portion covering the core portion, the particle shape being a hexagonal pillar, the particle diameter being 300 nm or more, the thickness being 100 nm or more, and the aspect ratio (particle diameter / thickness) being 1.2 or more and 5.0 or less. <2> Aspect 2 of the present invention is the core-shell upconversion microparticle of Aspect 1, wherein the particle diameter is 500 nm or more and the thickness is 300 nm or more. <3> Aspect 3 of the present invention is the core-shell upconversion microparticle of Aspect 1 or Aspect 2, wherein the aspect ratio is 1.2 or more and 3.0 or less. <4> Aspect 4 of the present invention is the core-shell upconversion microparticle of any one of Aspects 1 to 3, wherein the aspect ratio is 1.5 or more and 2.0 or less. <5> Aspect 5 of the present invention relates to the core-shell upconversion microparticle of any one of Aspects 1 to 4, wherein the shell / core ratio, which is the ratio of the width of the shell portion of the upconversion particle to the diameter of the core portion, may be 0.01 or more and 10.00 or less. <6> Aspect 6 of the present invention relates to the core-shell upconversion microparticle of Aspect 5, wherein the shell / core ratio may be 0.10 or more and 2.00 or less. <7> Aspect 7 of the present invention relates to the core-shell upconversion microparticle of any one of Aspects 1 to 6, wherein the crystal lattice hosting the core portion and the crystal lattice hosting the shell portion are composed of the same component, and the core portion contains a doped rare earth atom as a guest, while the shell portion does not contain a doped rare earth atom. <8> Aspect 8 of the present invention relates to the core-shell upconversion microparticle of Aspect 7, wherein the shell portion does not cause energy transfer. <9> A ninth aspect of the present invention relates to the core-shell upconversion microparticle of the seventh aspect, wherein the core portion may contain both a light absorption sensitizing atom and a light emission activating atom as the doped rare earth atoms.<10> Aspect 10 of the present invention relates to the core-shell upconversion microparticle of aspect 9, wherein the light-absorption sensitizing atom is a trivalent rare earth atom having an f-orbital energy level and absorbing near-infrared light to excite ground-state electrons to the f-orbital energy level, and the luminescence-activating atom has multiple energy levels and undergoes multiphoton multistep excitation by transferring energy at the f-orbital energy level of the excited light-absorption sensitizing atom, resulting in electrons being excited to a high energy level corresponding to an energy level equal to or higher than the f-orbital energy level, which is necessary for emitting light in the visible light region, by the multiphoton multistep excitation, and then the electrons excited to the high energy level emit light upon returning to the ground state, thereby causing emission of light in the visible light region as light with an energy level equal to or higher than the f-orbital energy level. <11> Aspect 11 of the present invention relates to the core-shell upconversion microparticle of aspect 9, wherein the crystal lattice is NaYF. 4wherein the light absorption sensitizing atoms are one or more selected from the group consisting of Yb and Nd, and the luminescence activating atoms are one or more selected from the group consisting of Tm, Er, and Ho. <12> Aspect 12 of the present invention relates to the core-shell upconversion microparticle of Aspect 7, wherein the doped rare earth atoms may be Nd. <13> Aspect 13 of the present invention relates to the core-shell upconversion microparticle of Aspect 7, wherein the doped rare earth atoms may be either one pair of Nd and Yb atoms or one pair of Tm and Yb atoms. <14> Aspect 14 of the present invention relates to the core-shell upconversion microparticle of Aspect 1, wherein the crystal lattice serving as a host for the core portion and the crystal lattice serving as a host for the shell portion are made of the same component, the core portion contains a first doped rare earth atom as a guest, and the shell portion contains a second doped rare earth atom as a guest that is different from the first doped rare earth atom in the core portion. <15> Aspect 15 of the present invention relates to the core-shell upconversion microparticle of Aspect 14, wherein the shell portion may cause energy transfer. <16> Aspect 16 of the present invention relates to the core-shell upconversion microparticle of Aspect 14, wherein the first doped rare earth atom or the second doped rare earth atom may include both a light-absorption sensitizing atom and a light-emission activating atom. <17> Aspect 17 of the present invention relates to the core-shell upconversion microparticle of Aspect 16, wherein the light-absorption sensitizing atom is one or more atoms selected from the group consisting of Yb and Nd, and the light-emission activating atom includes one or more atoms selected from the group consisting of Tm, Er, and Ho. <18> Aspect 18 of the present invention relates to the core-shell upconversion microparticle of Aspect 14, wherein the first doped rare earth atom or the second doped rare earth atom includes Nd. <19> Aspect 19 of the present invention relates to the core-shell upconversion microparticle of Aspect 14, wherein the crystal lattice is NaYF 4and the first doped rare earth atoms may be a pair of either Nd and Yb atoms or Tm and Yb atoms, and the second doped rare earth atoms may be a pair of either Nd and Yb atoms or Tm and Yb atoms, which is different from the pair of the first doped rare earth atoms. <20> Aspect 20 of the present invention relates to the core-shell upconversion microparticle of Aspect 14, wherein a first energy level that is an energy level of the first doped rare earth atoms may be different from a second energy level that is an energy level of the second doped rare earth atoms, in order to cause energy transfer from the first doped rare earth atoms to the second doped rare earth atoms. <21> Aspect 21 of the present invention relates to the core-shell upconversion microparticle of Aspect 20, wherein a third doped rare earth atom, which is a doped rare earth atom different from the first doped rare earth atom and the second doped rare earth atom, may further be present as a guest in at least one of the core portion and the shell portion, and a third energy level of the third doped rare earth atom may be located between the energy level of the first doped rare earth atom and the energy level of the second doped rare earth atom. <22> Aspect 22 of the present invention relates to the core-shell upconversion microparticle of Aspect 21, wherein the second doped rare earth atom has a plurality of post-excitation energy levels higher than an energy level before excitation at which the second doped rare earth atom has received energy transferred from the first doped rare earth atom or the third doped rare earth atom, and an energy gap between the pre-excitation energy level and one of the post-excitation energy levels may be equal to the transferred energy.<23> Aspect 23 of the present invention relates to the core-shell upconversion microparticle of aspect 1, which comprises a doped rare earth atom, and the doped rare earth atom is both a light-absorption sensitizer atom and a light-emission activator atom. The light-absorption sensitizer atom is a trivalent rare earth atom that has an f-orbital energy level and absorbs near-infrared light, thereby exciting an electron in a ground state to the energy level of the f-orbital. The light-emission activator atom has a plurality of energy levels and undergoes multiphoton multistep excitation by transferring energy at the energy level of the f-orbital of the excited light-absorption sensitizer atom, so that electrons are excited to a high energy level corresponding to an energy level equal to or higher than the energy level of the f-orbital, which is necessary for emitting light in the visible light region, by the multiphoton multistep excitation. Then, the electrons excited to the high energy level emit light when returning to the ground state, thereby causing light emission in the visible light region as light with an energy equal to or higher than the energy level of the f-orbital. <24> Aspect 24 of the present invention relates to the core-shell upconversion microparticle of aspect 23, wherein the light-absorption sensitizing atom is Yb, the light-emitting activated atom is Er, and the multiphoton multi-step excitation is two-photon two-step excitation. <25> Aspect 25 of the present invention relates to the core-shell upconversion microparticle of aspect 23, wherein the light-absorption sensitizing atom is Yb, the light-emitting activated atom is Tm, and the multiphoton multi-step excitation is three-photon three-step excitation. <26> Aspect 26 of the present invention relates to the core-shell upconversion microparticle of aspect 23, wherein the light-absorption sensitizing atom is Yb, the light-emitting activated atom is Tm, and the multiphoton multi-step excitation is two-photon two-step excitation. <27> Aspect 27 of the present invention relates to the core-shell upconversion microparticle of aspect 23, wherein one of the light-absorption sensitizing atoms is Nd, and the other light-absorption sensitizing atom is one or more selected from the group consisting of Er, Tm, and Ho.<28> A sensitized core-shell upconversion microparticle of Aspect 28 of the present invention is an upconversion particle comprising a core portion and a shell portion covering the core portion, wherein the particle shape is a hexagonal pillar, the particle diameter is 500 nm or more, the thickness is 300 nm or more, and an aspect ratio (particle diameter / thickness) is 1.2 to 3.0, the core portion contains one pair of either Nd and Yb atoms or Tm and Yb atoms, and the shell portion contains a pair of Nd and Yb atoms or Tm and Yb atoms different from the pair contained in the core portion. <29> Aspect 29 of the present invention is the sensitized core-shell upconversion particle of Aspect 28, wherein the core portion contains both Nd and Yb atoms, and the shell portion may contain both Tm and Yb atoms. <30> A 30th aspect of the present invention relates to the sensitized core-shell upconversion microparticles of Aspect 28, wherein the core portion may contain both Tm and Yb atoms, and the shell portion may contain both Nd and Yb atoms. <31> A 31st aspect of the present invention relates to a photoelectric conversion element comprising a transparent conductive film as a cathode and TiO comprising the sensitized core-shell upconversion microparticles of Aspect 28. 2 A TiO layer, an electrolyte layer, a hole transport layer, and an Ag layer serving as an anode are laminated in this order. 2 The coated core-shell upconversion microparticles are the sensitized core-shell upconversion microparticles of Aspect 28 or the core-shell upconversion microparticles of Aspect 1, the outermost layer of which is TiO 2 TiO consisting of 2 <33> The near-infrared detector of aspect 33 of the present invention is a TiO layer of aspect 32. 2 The near-infrared detector of aspect 34 of the present invention comprises a TiO sensitized core-shell upconversion microparticle containing either the sensitized core-shell upconversion microparticle of aspect 28 or the core-shell upconversion microparticle of aspect 1 in the photoelectric conversion layer. 2<35> The photoelectric conversion element of aspect 35 of the present invention comprises a transparent conductive film as a cathode and the TiO layer of aspect 32. 2The core-shell upconversion microparticles of the present invention are formed by laminating, in this order, a layer of coated core-shell upconversion microparticles, an electrolyte layer or a hole transport layer, and an Ag layer serving as an anode. <36> A method for producing core-shell upconversion microparticles of Aspect 36 of the present invention is the method for producing core-shell upconversion microparticles of Aspect 1, comprising: a first step of forming the core portion by crystal growth under conditions ranging from 50°C to 500°C using a sol-gel method; and a second step of growing crystals constituting the shell portion on the surface of the core portion by the sol-gel method under conditions ranging from 50°C to 500°C. <37> Aspect 37 of the present invention is the method for producing core-shell upconversion microparticles of Aspect 36, wherein the crystal growth in the first step may be performed by a heating operation that includes the formation of cubic crystals and a phase transition from cubic crystals to hexagonal crystals. <38> Aspect 38 of the present invention relates to the method for producing core-shell upconversion microparticles of Aspect 37, wherein the heating operation in the first step may be performed until an accumulated temperature as a heating condition for the phase transition exceeds an accumulated temperature as a heating condition for forming the cubic crystal. <39> Aspect 39 of the present invention relates to the method for producing core-shell upconversion microparticles of Aspect 37, wherein the heating operation in the first step may be performed while a degassing operation is performed to maintain a predetermined vacuum level. <40> Aspect 40 of the present invention relates to the method for producing core-shell upconversion microparticles of Aspect 36, wherein the crystal lattice constituting the core portion and the crystal lattice constituting the shell portion may be made of the same component. <41> An upconversion micro precursor particle of Aspect 41 of the present invention is a central particle capable of becoming the core contained in the core-shell upconversion microparticle of Aspect 1, the particle shape being a hexagonal pillar, the particle diameter being 300 nm or more, the thickness being 100 nm or more, and the aspect ratio (particle diameter / thickness) being 1.2 or more and 5.0 or less. <42> Aspect 42 of the present invention is the upconversion micro precursor particle of Aspect 41, which may be obtained by crystal growth under conditions in the range of 50°C to 500°C by a sol-gel method.<43> In aspect 43 of the present invention, in the upconversion microprecursor particles of aspect 42, the long-chain organic molecules used as a gelling agent in the sol-gel method may remain or be attached to the surface of the particles even after crystal growth by a heating operation.

[0009] According to the above-described aspects of the present invention, upconversion particles, upconversion microprecursor particles, sensitized core-shell type upconversion particles, TiO, and the like are capable of upconversion emission even under low excitation light such as sunlight irradiation, and can achieve higher sensitization properties using weak light with long wavelengths, and can be manufactured at low cost. 2 It is possible to provide coated core-shell upconversion particles, near-infrared detectors, photoelectric conversion elements, and methods for producing upconversion particles.

[0010] 11 is a schematic diagram of a core-shell upconversion microparticle according to the first embodiment; FIG. 12 is a schematic cross-sectional view of the core-shell upconversion microparticle of FIG. 1 taken along line A-A; FIG. 13 is a flowchart of a method for manufacturing a core-shell upconversion microparticle according to the first embodiment; FIG. 14 is a cross-sectional view of a photoelectric conversion element including a core-shell upconversion microparticle according to the first embodiment; FIG. 15 is a diagram showing the energy band structure of each layer during operation of a photoelectric conversion element 100 including a core-shell upconversion microparticle according to the first embodiment; FIG. 16 is a cross-sectional view of a modified example of a photoelectric conversion element including a core-shell upconversion microparticle according to the first embodiment; FIG. 17 is a schematic cross-sectional view of the core-shell upconversion microparticle of FIG. 7 taken along line B-B; FIG. 18 is a flowchart of a method for manufacturing a core-shell upconversion microparticle according to the second embodiment; FIG. 19 is a cross-sectional view of a photoelectric conversion element including a core-shell upconversion microparticle according to the third embodiment; FIG. 19 is a schematic cross-sectional view of the core-shell upconversion microparticle of FIG. 11 taken along line CC. 1 is a flowchart of a method for producing core-shell upconversion microparticles according to a third embodiment; FIG. 2 is a cross-sectional view of a photoelectric conversion element of the present invention including core-shell upconversion microparticles according to the third embodiment; FIG. 3 is an XRD pattern of the core portion (i.e., the upconversion microprecursor particle serving as the central particle) contained in the core-shell upconversion microparticles of Example 3-2 and the cubic (α-phase) particles of Comparative Example 2; FIG. 4 is an SEM image of Example 1 (upconversion microprecursor particles), Comparative Example 1-1 (nanoparticles), and Comparative Example 1-2 (cubic (α-phase) particles); FIG. 5 is an FT-IR spectrum of Example 1 (upconversion microprecursor particles) and Comparative Example 1-2 (cubic (α-phase) particles); FIG. 6 is an emission spectrum of Example 1 (upconversion microprecursor particles) and Comparative Example 1-2 (cubic (α-phase) particles).1 shows XRD patterns of the core portion (i.e., upconversion micro precursor particle serving as the central particle) contained in the core-shell upconversion microparticles of Example 2-2 and the cubic (α-phase) particles of Comparative Example 2.

[0034] FIG. 1 shows SEM images of Example 2-1 (core) and Comparative Example 2 (cubic (α-phase) particles).

[0035] FIG. 1 shows FT-IR spectra of Example 2-1 (core) and Comparative Example 2 (cubic (α-phase) particles).

[0036] FIG. 1 shows emission spectra of Example 2-1 (core) and Comparative Example 2 (cubic (α-phase) particles).

[0037] FIG. 1 shows XRD patterns of the core and core-shell of Example 3-1.

[0038] FIG. 1 shows XRD patterns of the core and core-shell of Example 3-2.

[0039] FIG. 1 shows SEM images of the core and core-shell of Example 3-1.

[0040] FIG. 1 shows SEM images of the core and core-shell of Example 3-2.

[0041] FIG. 1 shows emission spectra of the upconversion particles of the core-shell upconversion microparticles of Examples 3-1 and 3-2.

[0042] FIG. 1 shows SEM images of Example 4. 10 is a graph showing the response speed of the photocurrent obtained in the photoelectric conversion element of Example 5.

[0011] Hereinafter, core-shell type upconversion microparticles, upconversion microprecursor particles, sensitized core-shell type upconversion microparticles, TiO 2 The coated core-shell upconversion microparticles, near-infrared detectors, photoelectric conversion elements, and methods for manufacturing core-shell upconversion microparticles are described in detail with reference to the drawings. Note that the drawings used in the following description may show characteristic portions enlarged for ease of understanding, and the dimensional ratios of each component may not necessarily be the same as those in reality. Furthermore, the materials, dimensions, etc. exemplified in the following description are merely examples, and the present invention is not limited thereto. Appropriate modifications can be made within the scope of the present invention.

[0012] First Embodiment (Upconversion Particle 10) Fig. 1 is a schematic diagram of an upconversion particle 10 according to a first embodiment. Fig. 2 is a schematic cross-sectional view of the upconversion particle 10 of Fig. 1 taken along line A-A. The upconversion particle 10 comprises a core portion (upconversion microprecursor particle serving as the central particle) 11 and a shell portion (coating layer) 12 that coats the core portion 11. The upconversion particle 10 of the present disclosure is a particle having a core-shell structure. The particle shape of the upconversion particle 10 is a hexagonal pillar.

[0013] "Particle Diameter of Upconversion Particles 10" The particle diameter L1 of the upconversion particles 10 is 300 nm or more. The particle diameter L1 of the upconversion particles 10 is preferably increased while maintaining the aspect ratio described below, in order to obtain particles that are micronized to at least several hundred nanometers in size (i.e., so-called "microparticles"), rather than particles that are nanosized to several tens of nanometers or less (i.e., so-called "nanoparticles"), but is preferably 500 nm or more, for example. The particle diameter L1 of the upconversion particles 10 is more preferably 550 nm or more. The particle diameter L1 of the upconversion particles 10 is particularly preferably 600 nm or more. The particle diameter L1 of the upconversion particles 10 is preferably 2000 nm or less. This is because defects are more likely to occur in the crystal structure of the particles when the particle diameter is greater than 2000 nm. The particle diameter L1 of the upconversion particles 10 is more preferably 1500 nm or less. The particle diameter of the core portion 11 is preferably 300 nm or more. Here, the particle diameter L1 of the upconversion particle 10 is the diameter of the smallest encompassing circle that encloses the hexagonal base of the upconversion particle 10 (in the in-plane direction).

[0014] "Thickness of Upconversion Particles 10" The thickness t1 of the upconversion particles 10 is 100 nm or more. By making the thickness t1 of the upconversion particles 10 100 nm or more, the amount of organic molecules adhering to the upconversion particles 10 is reduced, and thermal deactivation can be suppressed. The thickness t1 of the upconversion particles 10 is more preferably 300 nm or more. The thickness t1A of the upconversion particles 10 is 600 nm or less. Here, the thickness t1 of the upconversion particles 10 is the length in the height direction of the hexagonal pillar. Similarly, the thickness of the core portion 11 is preferably 100 nm or more.

[0015] "Particle diameter L1 of upconversion particle 10 / Thickness t1 of upconversion particle 10" The aspect ratio of the particle diameter of upconversion particle 10 / thickness of upconversion particle 10 is 1.2 or more and 5.0 or less. The particle diameter of upconversion particle 10 / thickness of upconversion particle 10 is preferably 1.5 or more. Similarly, the particle diameter of core portion 11 / thickness of core portion 11 is preferably 1.2 or more and 5.0 or less.

[0016] "Method for Measuring Particle Diameter and Thickness of Upconversion Particles 10" The particle diameter and thickness of the upconversion particles 10 can be measured by the following method. For example, the upconversion particles 10 are placed on a flat substrate and observed at 15,000 to 30,000 magnifications using a scanning electron microscope (SEM). Fifteen upconversion particles 10 obtained through observation are randomly selected, and the particle diameters of the upconversion particles 10 are measured from the diameter of the smallest encompassing circle enclosing the hexagonal base. The five highest values ​​in descending order from the highest value and the five lowest values ​​in ascending order from the lowest value are excluded, and the average value of the five intermediate values ​​remaining is taken as the particle diameter of the upconversion particles 10. Similarly, 15 upconversion particles 10 obtained through observation are randomly selected, and the height of the hexagonal prism is measured. The five highest values ​​in descending order from the highest value and the five lowest values ​​in ascending order from the lowest value are excluded, and the average value of the five intermediate values ​​remaining is taken as the thickness of the upconversion particles 10.

[0017] "Core portion 11" The core portion 11 has the ability to convert the wavelength of light. Preferably, the core portion 11 is formed by crystal growth using a sol-gel method under conditions ranging from 50°C to 500°C. Growth in this manner improves luminous efficiency. Long-chain organic molecules used as gelling agents in the sol-gel method may remain or adhere to the particle surface even after crystal growth by heating. The core portion 11 is a particle (an upconversion microprecursor particle serving as the central particle) that forms the core of the core-shell particle. Here, the light wavelength conversion ability refers to the ability to convert the wavelength of incident light and emit light with a wavelength different from that of the incident light. In this embodiment, an example will be described in which incident near-infrared light is wavelength-converted and emitted as visible light.

[0018] Examples of materials for the core 11 include rare earth metals capable of emitting excitation light in the visible or ultraviolet region, such as erbium (Er), thulium (Tm), ytterbium (Yb), neodymium (Nd), holmium (Ho), praseodymium (Pr), gadolinium (Gd), europium (Eu), terbium (Tb), samarium (Sm), cerium (Ce), and dysprosium (Dy), as well as compounds containing at least one of these. Light in the visible or ultraviolet region refers to light with a wavelength of less than 700 nm. Examples of materials for the core 11 include NaErF 4、 Tm 2 O 3 , TmCl 3 , TmF 3 , Er 2 O 3 , ErCl 3 , ErF 3 , Ho 2 O 3 , HoCl 3 , HoF 3and inorganic fine particles containing rare earth atoms doped as guests in a crystal lattice serving as a host (hereinafter, sometimes referred to as doped rare earth atoms). The core portion 11 is preferably an inorganic fine particle containing doped rare earth atoms as guests in a crystal lattice serving as a host. By using inorganic fine particles containing doped rare earth atoms as guests in a crystal lattice serving as a host for the core portion 11, the efficiency of upconversion light emission can be improved.

[0019] When the core portion 11 is an inorganic fine particle containing a doped rare earth atom as a guest in a crystal lattice as a host, the crystal lattice as a host may be, for example, CeO 3 , Y 2 O 3 Simple oxides such as NaYF 4 Complex halides such as Gd 2 O 2 S, CaAl 12 O 19 , YTa 7 O 19 , GdTa 7 O 19 , M.T.a. 7 O 11 Examples of the host crystal lattice include complex oxides such as NaYF (where M=Ca, Sr, Ba). 4 Preferred are complex halides having low phonon energy such as those mentioned above, which can suppress loss of excitation energy due to non-radiative transition in which energy is lost to heat without emitting light in the excited state.

[0020] When the core portion 11 is an inorganic microparticle containing a doped rare earth atom as a guest in a crystal lattice as a host, examples of the doped rare earth element include rare earth elements capable of emitting excitation light in the visible or ultraviolet region, such as erbium (Er), thulium (Tm), ytterbium (Yb), neodymium (Nd), holmium (Ho), praseodymium (Pr), gadolinium (Gd), europium (Eu), terbium (Tb), samarium (Sm), cerium (Ce), and dysprosium (Dy). The total content of the doped rare earth atoms is preferably 0.5% to 40% by mass relative to the total mass of the core portion 11. In the case of luminescence-activating atoms, the total content of the luminescence-activating atoms is preferably 0.5% to 2.0% by mass relative to the total mass of the core portion 11. In the case of light-absorption-sensitizing atoms, the total content of the luminescence-activating atoms is preferably 10% to 40% by mass relative to the total mass of the core portion 11. By setting the total content of doped rare earth atoms to 0.5 mass % to 40 mass % with respect to the total mass of the core 11, it is possible to suppress collapse of the crystal structure and improve the efficiency of upconversion light emission.

[0021] The core region 11 preferably contains both a light-absorbing sensitizing atom and a light-emitting activating atom as doped rare earth atoms. The light-absorbing sensitizing atom is an atom that receives energy from outside the light-absorbing sensitizing atom and mediates the energy to another atom (e.g., a light-emitting activating atom). The light-emitting activating atom is an atom that receives energy from outside the light-absorbing activating atom and emits light at a predetermined wavelength. The light-absorbing sensitizing atom is, for example, one or more atoms selected from the group consisting of Yb and Nd. The light-absorbing sensitizing atom is, for example, Yb or both Yb and Nd atoms. The core region 11 may contain only one rare earth atom, such as Yb or Nd, but containing two or more rare earth atoms is preferable because it can further improve the luminous efficiency. The light-absorbing sensitizing atom is preferably a trivalent rare earth atom that has an f-orbital energy level, absorbs near-infrared light (wavelength 800 nm to 2500 nm), and has ground-state electrons excited to the f-orbital energy level. The luminescence-activating atom is preferably a trivalent rare earth atom having multiple energy levels, and is capable of undergoing multiphoton multistep excitation by transferring energy at the energy levels of the orbitals of the sensitized atom after the sensitized atom absorbs near-infrared light and is excited to the energy level of the f orbital, resulting in electrons being excited to a high energy level corresponding to an energy level equal to or higher than the energy level of the f orbital, which is necessary for emitting light in the visible light region. The electrons excited to the high energy level then emit light when returning to the ground state, resulting in light emission in the visible light region as light with an energy level equal to or higher than the energy level of the f orbital of the sensitized atom. Multiphoton multistep excitation refers to a phenomenon in which a molecule or the like absorbs multiple photons almost simultaneously, causing further excitation from the excited level or a level relaxed after excitation. The luminescence-activating atom is, for example, one or more selected from the group consisting of Tm, Er, and Ho. Preferably, the optical absorption sensitizing atom is Yb, the luminescence activating atom is Er, and the multiphoton multistep excitation is two-photon two-step excitation. Preferably, the optical absorption sensitizing atom is Yb, the luminescence activating atom is Tm, and the multiphoton multistep excitation is three-photon three-step excitation or two-photon two-step excitation.It is preferable that one of the light absorption sensitizing atoms is Nd and the other light absorption sensitizing atoms is one or more selected from the group consisting of Er, Tm and Ho. As such a core portion 11, Yb is preferable. 3+ and Er 3+ Gd doped with 2 O 2 S (hereinafter referred to as “Gd 2 O 2 S: Er, Yb), Yb 3+ and Er 3+ NaYF doped with 4 (hereinafter referred to as "NaYF 4 : Er, Yb), Tm 3+ and Yb 3+ NaYF doped with 4 (hereinafter referred to as "NaYF 4 Examples of inorganic fine particles include those made of NaYF 4 It is particularly preferred that the core region 11 contains both a light-absorption-sensitizing atom and a light-emission-activating atom as guests, the light-absorption-sensitizing atom being Yb or both Yb and Nd atoms, and the light-emission-activating atom being one or more atoms selected from the group consisting of Tm, Er, and Ho. As the doped rare earth atom, the core region 11 preferably contains Nd.

[0022] When the light absorption sensitizing atom is Yb, the light emission activating atom is Er, and the multiphoton multistep excitation is two-photon two-step excitation, (a1) Yb 3+ (b1) After the energy transition due to the light absorption, Yb 3+ From Er 3+ Energy transfer to (c1) Yb 3+ From Er 3+ After energy transfer to Er 3+ (d1) Energy transfer by multiphoton multistep excitation at Er 3+ It is preferable that light emission occurs through the steps (a1) to (d1), that is, light emission at Yb 3+ of 2 F 7/2 From the level of2 F 5/2 In the process of (b1), the energy transition to the level of Yb 3+ of 2 F 5/2 From the level of Er 3+ of 4 I 11/2 In the process of (c1), the energy transfer to the level of Er 3+ of 4 I 11/2 From the level of 4 F 7/2 In the process of (d1), the energy transition to the level of Er 3+ accompanied by red light emission from 4 F 9/2 From the level of 4 I 15/2 Energy transition to the level of Er 3+ accompanied by green light emission 4 S 3/2 From the level of 4 I 15/2 Energy transition to the level of Er 3+ accompanied by green light emission 2 H 11/2 From the level of 4 I 15/2 This results in an energy transition to the level of

[0023] When the light absorption sensitizing atom is Yb, the light emission activating atom is Tm, and the multiphoton multistep excitation is four-photon four-step excitation, (a2) Yb 3+ (b2) After the energy transition due to the light absorption, Yb 3+ From Tm 3+ Energy transfer to (c2) Yb 3+ From Tm 3+ After energy transfer to Tm 3+ (d2) Energy transfer by multiphoton multistep excitation at Tm 3+ It is preferable that light emission occurs through the steps (a2) to (d2), that is, light emission at Yb 3+ of 2 F 7/2 From the level of 2 F 5/2In the process of (b2), the energy transition to the level of Yb 3+ of 2 F 5/2 From the level of Tm 3+ of 3 In the process of (c2), the energy transfer occurs to the level of Tm 3+ of 3 From the level of H5 3 F 4 energy relaxation to the level of 3 F 4 From the level of 3 F 2 or 3 F 3 energy transition to the level of 3 H 4 From the level of 1 G 4 energy transition to the level of 1 G 4 From the level of 1 D 2 In the process of (d2), the energy transition to the level of Tm 3+ The blue light emitted by 1 D 2 From the level of 3 H 6 Energy transition to the level of Tm 3+ The blue light emitted by 1 G 4 From the level of 3 H 6 Energy transition to the level of Tm 3+ accompanied by red light emission from 3 H 4 From the level of 3 H 6 This results in an energy transition to the level of

[0024] When the light-absorbing sensitizing atoms are Nd and Yb and the other light-absorbing sensitizing atoms are one or more selected from the group consisting of Er, Tm, and Ho, (a4) Nd 3+ (b4) After the energy transition due to the light absorption, Nd 3+ From Yb 3+ Energy transfer to (c4) Nd 3+ From Yb 3+ After energy transfer to Yb 3+It is preferable to go through the processes (a4) to (c4) in which the energy transition occurs at Nd 3+ of 4 I 9/2 From the level of 4 F 5/2 In the process of (b4), the energy transition to the level of Nd 3+ of 4 F 3/2 From the level of Yb 3+ of 2 F 5/2 In the process of (c4), the energy transfer to the level of Yb 3+ of 2 F 7/2 From the level of 2 F 5/2 This results in an energy transition to the level of

[0025] When the light absorption sensitizing atoms are Nd and Yb and the emission activating atom is Tm, (a4) Nd 3+ (b4) After the energy transition due to the light absorption, Nd 3+ From Yb 3+ Energy transfer to (c4) Nd 3+ From Yb 3+ After energy transfer to Yb 3+ From Tm 3+ Energy transfer to (d4) Yb 3+ From Tm 3+ After energy transfer to Tm 3+ (e5) Energy transition by multiphoton multistep excitation at Tm 3+ It is preferable that light emission occurs through the steps (a4) to (e5), that is, light emission at Nd 3+ of 4 I 9/2 From the level of 4 F 5/2 In the process of (b4), the energy transition to the level of Nd 3+ of 4 F 3/2 From the level of Yb 3+ of 2 F 5/2 In the process of (c4), the energy transfer to the level of Yb3+ of 2 F 7/2 From the level of 2 F 5/2 In the process of (d4), the energy transition to the level of Yb 3+ of 2 F 5/2 From the level of Tm 3+ of 3 In the process of (c2), the energy transfer occurs to the level of Tm 3+ of 3 From the level of H5 1 G 4 energy transition to the level of 1 G 4 From the level of 3 F 2 or 3 F 3 energy relaxation to the level of 3 F 2 or 3 F 3 From the level of 1 D 2 energy transition to the level of 1 D 2 From junior 3 P 2 In the process of (d2), the energy transition to the level of Tm 3+ Accompanied by ultraviolet emission of 1 I 6 From the level of 3 H 6 Energy transition to the level of Tm 3+ The blue light emitted by 1 D 2 From the level of 3 H 6 Energy transition to the level of Tm 3+ The blue light emitted by 1 G 4 From the level of 3 H 6 Energy transition to the level of Tm 3+ accompanied by red light emission from 3 H 4 From the level of 3 H 6 This results in an energy transition to the level of

[0026] When the core region 11 contains both light absorption sensitizing atoms and light emission activating atoms as doped rare earth atoms, the doped rare earth atoms contained as guests in the core region 11 are preferably one pair of either Nd and Yb atoms or Tm and Yb atoms. That is, the core region 11 preferably contains both Nd and Yb atoms as guests, or both Tm and Yb atoms as guests. When the core region contains Tm and Yb as doped rare earth atoms, the molar ratio of Tm to Yb is preferably 10:30 to 30:10. More preferably, the molar ratio of Tm to Yb is 15:25 to 25:15. When the core region contains Nd and Yb as doped rare earth atoms, the molar ratio of Nd to Yb is preferably 10:30 to 30:10. More preferably, the molar ratio of Nd to Yb is 15:25 to 25:15.

[0027] The particle diameter (diameter length) C1 of the core portion 11 is preferably 500 nm to 1500 nm, and is the diameter of the smallest inclusive circle that encloses the hexagon on a plane perpendicular to the height direction of the hexagonal column.

[0028] (Shell 12) The shell 12 is a coating layer that coats the core 11. The crystal lattice constituting the shell 12 is preferably made of the same component as the crystal lattice serving as the host of the core 11. For example, if the crystal lattice of the host of the core 11 is NaYF 4 In this case, the crystal lattice of the shell portion 12 is also NaYF 4 It is preferable that:

[0029] In the first embodiment, the shell portion 12 does not contain doped rare earth atoms, and the shell portion 12 does not undergo energy transfer. Since the shell portion 12 of the first embodiment does not contain doped rare earth atoms, the doped rare earth atoms are unevenly distributed in the core portion 11. By doing so, for example, even if long-chain organic molecules adhere to the surface during the production of the upconversion particle 10, the long-chain organic molecules can be separated from the core portion 11, and vibrational deactivation due to the long-chain organic molecules can be suppressed.

[0030] The thickness (width) Sh1 of the shell portion 12 is preferably, for example, 100 nm to 500 nm. As described below, the shell / core ratio (the width of the shell portion to the diameter of the core portion) of the upconversion particle 10 is preferably 0.01 or more and 10.00 or less. Therefore, for example, when the shell / core ratio is 0.01, the thickness (width) Sh1 of the shell portion 12 can be set to be smaller than the lower limit of the above-mentioned preferred range depending on the particle diameter (diameter) C1 of the core portion 11. Specifically, for example, if the particle diameter (diameter) C1 of the core portion 11 is 500 nm, the thickness (width) Sh1 of the shell portion 12 may be 5 nm, and if the particle diameter (diameter) C1 of the core portion 11 is 100 nm, the thickness (width) Sh1 of the shell portion 12 may be 1 nm. The thickness (width) Sh1 of the shell portion 12 is the length of the shell portion 12 in a direction perpendicular to the interface between the core portion 11 and the shell portion 12 on a plane perpendicular to the height direction of the hexagonal prism.

[0031] The coverage of the surface of the core portion 11 with the shell portion 12 is preferably 50% or more, and more preferably 100%.

[0032] The shell portion 12 may be a single layer or may have two or more layers. By increasing the number of layers, even if long-chain organic molecules used as a gelling agent during the production of the upconversion particles 10, specifically after crystal growth by heating in a sol-gel process, remain or adhere to the surface of the particles, the long-chain organic molecules can be separated from the core portion 11, thereby suppressing vibrational deactivation caused by the long-chain organic molecules. This improves the luminous efficiency of the upconversion particles 10. Incidentally, even if the shell portion 12 has two or more layers in terms of the production process, for example, if the first and second shell layers have the same composition and are integrated into one shell layer without a clear interface between them, the first and second shell layers can be considered together as a single layer. In such cases, for example, the presence of an interface between the first and second shell layers cannot be observed even when observed using a transmission electron microscope.

[0033] The particle diameter (diameter length) C1 of the core region 11 and the thickness (width length) Sh1 of the shell region 12 can be measured by the following method. Fifteen upconversion particles 10 are randomly selected through observation using a scanning electron microscope (SEM) or a transmission electron microscope (TEM). The particle diameters of the core region 11 and the thicknesses of the shell region 12 of the selected upconversion particles 10 are measured, and the five particles with the highest values ​​in descending order from the highest to the fifth highest value and the five particles with the lowest values ​​in ascending order from the lowest to the fifth highest value are excluded. The average particle diameters and thicknesses (width lengths) of the remaining five particles with intermediate values ​​are defined as the particle diameter of the core region 11 and the thickness (width length) of the shell region 12, respectively.

[0034] (Shell / core ratio, which is the width of the shell portion 12 of the upconversion particle 10 divided by the diameter of the core portion 11) The shell / core ratio, which is the width of the shell portion of the upconversion particle 10 divided by the diameter of the core portion, is preferably 0.01 or more and 10.00 or less. A more preferred shell / core ratio is 0.10 or more and 2.00 or less. An even more particularly preferred shell / core ratio is 0.10 or more and 1.00 or less. For example, in the case of the upconversion particle shown in FIG. 2, the width of the shell portion of the upconversion particle is the value of Sh1, and the diameter of the core portion is the value of C1. Furthermore, in the case of the upconversion particle shown in FIG. 8, the width of the shell portion of the upconversion particle is the value of Sh1A, and the diameter of the core portion is the value of C1A. Note that when the shell portion is made up of multiple layers, the width of the shell portion corresponds to the width diameter of the multiple layers. For example, in the case of the upconversion particle shown in Figure 12, the width of the shell portion of the upconversion particle is the sum of the values ​​of Sh1A and T1B, and the diameter of the core portion is the value of C1A. By setting the shell / core ratio of upconversion particle 10 to be 0.01 or more and 10.00 or less, even if long-chain organic molecules used as a gelling agent during the production of upconversion particle 10, specifically after crystal growth by heating in a sol-gel process, remain or adhere to the surface of the particle, the long-chain organic molecules can be separated from core portion 11, thereby suppressing vibrational deactivation caused by the long-chain organic molecules. This improves the luminous efficiency of upconversion particle 10.

[0035] The upconversion particle 10 has an outermost layer of TiO 2 TiO consisting of 2 That is, the upconversion particle 10 may have a TiO layer on the surface of the shell portion 12. 2 TiO consisting of 2 It may also comprise a layer.

[0036] (Method for Producing Upconversion Particles 10) Next, a method for producing upconversion particles 10 according to the present disclosure will be described. As shown in Fig. 3, the method for producing upconversion particles 10 according to the present disclosure includes a first step S1 in which a core portion 11 is formed by crystal growth using a sol-gel method under conditions in the range of 50°C to 500°C, and a second step S2 in which crystals constituting a shell portion 12 are grown on the surface of the core portion 11 after the first step S1 by the sol-gel method under conditions in the range of 50°C to 500°C. Conventional upconversion particles have been produced by a hydrothermal method, which requires high-temperature and high-pressure conditions. However, the method for producing upconversion particles according to the present disclosure does not require high-temperature and high-pressure conditions, and therefore allows upconversion particles to be produced easily and at low cost.

[0037] "First Step S1" In the first step S1, the core portion 11 is formed by crystal growth under conditions ranging from 50°C to 500°C by a sol-gel method. Specifically, the main raw material is, for example, Y 2 O 3 , Er 2 O 3 , Nd 2 O 3 , Tm 2 O 3 , Ho 2 O 3 , Gd 2 O 3 and Yb 2 O 3 rare earth oxides such as YCl 3 , Y.F. 3 , ErCl 3 , ErF 3 , TmCl 3 , TmF 3 , HoCl 3 , HoF 3 , GdCl 3 , GdF 3Trifluoroacetate is synthesized using rare earth atom halides such as the above. The ratio of each material is determined depending on the target composition ratio. Furthermore, sodium trifluoroacetate and an organic molecule having 1 to 3 long-chain hydrocarbon groups with approximately 8 to 24 carbon atoms, such as 1-octadecene, oleic acid, oleylamine, trioctylphosphine oxide, linoleic acid, or octylamine, or a long-chain organic molecule such as its carboxylic acid, are used as a gelling agent, and N 2 Alternatively, the reaction is carried out under low temperature conditions (50°C to 500°C) in an Ar atmosphere. After the reaction, the solution is cooled, and an organic solvent such as ethanol is added as needed, followed by centrifugation to separate the central particles that form the core portion 11. The main raw material for the core portion 11 is appropriately adjusted so as to contain a crystal lattice as a host and a doped rare earth atom as a guest. For example, when the crystal lattice as a host is NaYF 4 and when the doped rare earth atoms are Nd and Yb, Y 2 O 3 , Nd 2 O 3 , Yb 2 O 2 and the ratio is determined according to the desired composition ratio of the core region 11.

[0038] The crystal growth in the first step S1 is performed by a heating operation including (a) the formation of an α phase (cubic crystal) and (b) a phase transition from the α phase (cubic crystal) to a β phase (hexagonal crystal). For example, the heating operation for forming the α phase is performed by raising the temperature from room temperature to a temperature range (first temperature range) of 80°C to 150°C at a heating rate of approximately 100°C / 4 minutes to 100°C / 10 minutes, and performing heat treatment in the first temperature range for approximately 10 to 40 minutes. The heating operation for the phase transition from the α phase to the β phase is performed by raising the temperature from the first temperature range to a temperature range (second temperature range) of 200°C to 500°C at a heating rate of approximately 100°C to 300°C / 10 minutes to 15 minutes, and performing heat treatment in the second temperature range for 20 to 80 minutes. By performing heat treatment in the second temperature range for 60 minutes or more, it is possible to obtain only the β phase.

[0039] In the above-described heating operation in the first step S1, it is preferable to perform the heating operation until the cumulative temperature as a heating condition for the phase transition from the α phase to the β phase exceeds the cumulative temperature as a heating condition for the formation of cubic crystals. This facilitates the formation of upconversion particles 10 having a particle diameter of 500 nm or more, a thickness of 300 nm or more, and an aspect ratio (particle diameter / thickness) of 1.2 to 3.0. The cumulative temperature is the sum of the treatment temperatures for a predetermined period of time. For example, if a 30-minute heat treatment is performed at a heating temperature (100°C) every 5 minutes during the heat treatment, the cumulative temperature is 100°C x 30 / 5 = 600°C. The cumulative temperature calculation method is the same for the cumulative temperature as a heating condition for the phase transition from the α phase to the β phase and the cumulative temperature as a heating condition for the formation of cubic crystals. The heating temperature is, for example, the set temperature of the heating furnace used for heating.

[0040] The heating operation in the first step S1 is performed while degassing to maintain a predetermined degree of vacuum, for example, 0.1 MPa to 0.01 MPa. This facilitates the formation of upconversion particles 10 having a particle diameter of 500 nm or more, a thickness of 300 nm or more, and an aspect ratio (particle diameter / thickness) of 1.2 to 5.0.

[0041] "Second Step S2" Next, in the second step S2, crystals constituting the shell portion 12 are grown on the surface of the core portion 11 formed in the first step S1 by a sol-gel method under conditions ranging from 50°C to 500°C. A rare earth atom oxide or rare earth atom halide is selected so that the components of the crystal lattice constituting the shell portion 12 are the same as those of the crystal lattice serving as the host for the core portion 11, and a trifluoroacetate is synthesized in the same manner as in the first step. Next, the core portion 11 obtained in the first step S1, sodium trifluoroacetate, and an organic molecule having one to three long-chain hydrocarbon groups having about 8 to 24 carbon atoms, such as 1-octadecene, oleic acid, oleylamine, trioctylphosphine oxide, linoleic acid, or octylamine, or a long-chain organic molecule such as its carboxylic acid, are used as a gelling agent, and N 2Alternatively, the reaction is carried out under low-temperature conditions (50°C to 500°C) in an Ar atmosphere for 30 minutes or less. The solution after the reaction is cooled, and an organic solvent such as ethanol is added as needed, followed by centrifugation to separate the upconversion particles 10. When a shell 12 consisting of multiple layers is formed around the core 11, the above steps can be repeated to obtain upconversion particles 10 consisting of multiple layers. It is preferable that the crystal lattice of the core 11 formed in the first step S1 and the crystal lattice of the shell 12 formed in the second step S2 are made of the same component. As described above, if the crystal lattice of the core 11 formed in the first step S1 and the crystal lattice of the shell 12 formed in the second step S2 are made of the same component, even if long-chain organic molecules adhere to the surface of the upconversion particles 10 during production, the long-chain organic molecules can be separated from the core 11, which is expected to suppress vibrational deactivation caused by the long-chain organic molecules.

[0042] 4 is a cross-sectional view of a photoelectric conversion element 100 including upconversion particles 10. The photoelectric conversion element 100 is mainly composed of a positive electrode layer (positive electrode member) 101, a negative electrode layer (negative electrode member) 102, and a photoelectric conversion layer 103 sandwiched therebetween.

[0043] "Negative electrode layer 102" Between the negative electrode layer 102 and the photoelectric conversion layer 103, there is provided a layer having an E cb is the lowest energy level of the conduction band between the negative electrode layer 102 and the photoelectric conversion layer 103. c2 and E c3 (i.e., E c2 <E cb <E c3 The buffer layer 107 may be made of, for example, europium oxide (Eu 2 O 3 ), titanium oxide, tin oxide, etc. Examples of the structure of the buffer layer 107 include a structure in which one or more of the above-mentioned constituent materials are laminated on the surface of the photoelectric conversion layer 103 on the negative electrode layer 102 side.

[0044] In order to capture light into the photoelectric conversion layer 103, the anode layer 102 is preferably made of a transparent conductive material such as antimony-doped indium oxide (ATO), indium tin oxide (ITO), zinc oxide, tin oxide, or fluorine-doped indium oxide (FTO). ATO, which has heat resistance, is preferred as the anode layer 102.

[0045] "Positive electrode layer 101" The positive electrode layer 101 does not need to be transparent, and metals, conductive polymers, etc. can be used as the electrode material of the electrode. Specific examples of electrode materials include metals such as gold (Au), silver (Ag), aluminum (Al), and zinc (Zn), as well as alloys of two or more of these metals, graphite, graphite intercalation compounds, polyaniline and its derivatives, and polythiophene and its derivatives. An example of a material for the transparent positive electrode layer 101 is ITO.

[0046] 4, the photoelectric conversion layer 103 preferably includes a first layer (electron transport layer) 104 mainly composed of a plurality of particles (hereinafter sometimes referred to as "inorganic semiconductor particles") 20 containing an inorganic semiconductor as a primary component. The photoelectric conversion layer 103 may be formed by stacking a second layer 105 formed on the surface of the first layer 104 and composed of an aggregate or thin film (composite) containing an inorganic perovskite-type material 17 as a primary component and further containing upconversion particles 10, and a third layer 106 composed of a plurality of particles or aggregates or thin films containing an organic or inorganic semiconductor (including a metal complex) as a primary component. In other words, the photoelectric conversion element 100 may be configured such that the positive electrode layer 101, the third layer 106, the second layer 105, the first layer 104, and the negative electrode layer 102 are arranged in this order, and a current path is formed at least from the positive electrode layer 101 to the negative electrode layer 102. The photoelectric conversion layer 103 contains upconversion particles 10 and an inorganic perovskite material 17. Here, "containing an inorganic semiconductor as a main component" means that the inorganic semiconductor particles 20 contain an amount of inorganic semiconductor capable of exhibiting the function of the present invention, specifically, for example, that the content of inorganic semiconductor is greater than 50% by volume. Preferably, it is greater than 90% by volume, and more preferably, it is essentially composed of an inorganic semiconductor. "containing an inorganic perovskite material 17 as a main component" means that the inorganic perovskite material 17 is contained in an amount capable of exhibiting the function of the present invention, relative to the total mass of the second layer 105, specifically, for example, that the content of inorganic perovskite material 17 is greater than 50% by volume. Preferably, it is 70% by volume or more. Furthermore, "containing an organic or inorganic semiconductor (including a metal complex) as a main component" means that the aggregates or thin films (composites) containing the upconversion particles 10 are contained in an amount sufficient to exhibit the function of the present invention relative to the total mass of the third layer 106. Specifically, for example, the content of the aggregates or thin films (composites) containing the upconversion particles 10 is greater than 50 mass%. Preferably, it is greater than 90 volume%, and more preferably, it is substantially composed of an organic or inorganic semiconductor (including a metal complex). The more current paths formed, the better, but adjacent current paths may or may not be electrically connected to each other.In this embodiment, the term "layer" refers to a film formed by one or more film-forming processes, and is not limited to being flat, and does not necessarily have to be integral.

[0047] Furthermore, the materials and compositions of the three layers 104 to 106 are determined so that the energy levels of the lowest conduction bands or the energy levels of the Lowest Unoccupied Molecular Orbital (LUMO) increase in the order of the first layer 104, the second layer 105, and the third layer 106. For example, for the first layer 104, the highest valence band energy level can be set to −8 eV or higher, and the lowest conduction band energy level can be set to −4 eV or lower. In this case, for the second layer 105, the highest valence band energy level can be set to −6.0 eV or higher, and the lowest conduction band energy level can be set to −3 eV or lower. Furthermore, for the third layer 106, it is preferable that the lowest conduction band energy level be set to −2 eV or lower.

[0048] The first layer 104 is an aggregate of a plurality of inorganic semiconductor particles 20 formed on the negative electrode layer 102, and is preferably a porous film having a plurality of voids between the inorganic semiconductor particles 20. The inorganic semiconductor particles 20 in contact with the second layer 105 are in direct contact with the negative electrode layer 102 or indirectly via other inorganic semiconductor particles 20 so as to be electrically connected to the negative electrode layer 102. The presence of the first layer 104, which is a porous film, can increase the contact area with the second layer 105.

[0049] The inorganic semiconductor contained in the inorganic semiconductor particles 20 preferably has an absorption wavelength in the ultraviolet region, such as titanium oxide (IV) (TiO 2 ), zinc oxide, etc. Examples of the inorganic semiconductor particles 20 include titanium(IV) oxide. In this case, the photoelectric conversion element 100 includes an electron transport layer made of titanium(IV) oxide. The thickness of the first layer 104 is preferably about 10 nm or more and 1000 nm or less, and more preferably about 50 nm or more and 500 nm or less.

[0050] The second layer 105 is a thin film that covers the exposed portion of the surface of the inorganic semiconductor particles 20 during the manufacturing process, i.e., the portion that is not in contact with either the negative electrode layer 102 or the inorganic semiconductor particles 20. The second layer 105 does not need to cover the entire exposed portion, but it preferably covers at least the positive electrode layer 101 side in order to form the current path.

[0051] The inorganic perovskite-type substance 17 constituting the second layer 105 is Pb 2+ , Sn 2+ metal cations such as I - , Cl - ,Br - halide anions such as CH 3 NH 3 + (MA), NH=CHNH 2 + (FA), C s + The inorganic perovskite material 17 is composed of multiple molecules consisting of metal cations, halide anions, and organic cations. The size and shape of the band gap can be changed by selecting the number of ions from each of the metal cations, halide anions, and organic cations. Adding tin to the inorganic perovskite material 17 narrows the band gap and makes it responsive to long-wavelength light such as near-infrared light, but it is easily oxidized in the atmosphere, resulting in degradation of its characteristics. In each molecule constituting the inorganic perovskite material 17, the halide anions are arranged at the vertices of a regular octahedron centered on the metal ion, and the organic cations are arranged near a cube centered on the metal ion and containing the regular octahedron. Specifically, the regular octahedrons formed by the metal ions and halide anions form a three-dimensional lattice, with the organic cations filling the gaps. Light converted to visible light by the upconversion particles 10 is absorbed by the inorganic perovskite material 17. This improves the light conversion efficiency of the photoelectric conversion element 100 in the near-infrared region.

[0052] It is preferable that the content of the upconversion particles 10 in the second layer 105 is 5 wt % or more, since this improves the sensitivity to light in the near-infrared region.If the content of the upconversion particles 10 in the second layer 105 exceeds 30 wt %, it becomes difficult to form a perovskite-type substance, so it is preferable that the content be 30 wt % or less.

[0053] Furthermore, it is preferable that the highest energy level of the valence band of the second layer 105 is lower than the highest energy level of the valence band of the third layer 106 and is intermittently connected to the same energy level. The composition of the second layer 105 (inorganic perovskite-type material 17) that satisfies these conditions is, for example, CH 3 NH 3 Pbl 3 , NH=CHNH 2 PbI 3 , CsPbI 3 Other examples include halide anions in which the composition ratio of I to Cl or Br is changed.

[0054] The third layer 106 is preferably a thin film covering the surface (exposed surface) of the inorganic perovskite material 17 contained in the second layer of the photoelectric conversion element precursor constituted by the first layer 104 and the second layer 105. The third layer 106 is formed of any one of a p-type organic semiconductor, an inorganic semiconductor, and an organometallic complex. The thickness of the third layer 106 is preferably, for example, 1 nm or more and 100 nm or less.

[0055] Examples of p-type organic semiconductors that constitute the third layer include bathocuproine (BCP), 2,2',7,7'-tetrakis(N,N'-di-p-methoxyphenylamine)-9,9'-spirobifluorene (Spiro-OMeTAD), poly(3,4-ethylenedioxythiophene):poly(styrenesulfonate) (PEDOT:PSS), and N,N,N',N'-tetrakis(4-methoxyphenyl)-benzidine (TPD).

[0056] Examples of p-type inorganic semiconductors that form the third layer 106 include CuI and CuSCN.

[0057] The photoelectric conversion element 100 may include a hole transport layer and an electron transport layer, and the member for a photoelectric conversion element according to the present disclosure may be disposed between the hole transport layer and the electron transport layer.

[0058] (Energy Band Structure) FIGS. 5A to 5C show the energy band structure of each layer during operation of the photoelectric conversion element 100 according to this embodiment.

[0059] In the absence of light irradiation, the energy level of the lowest conduction band of the third layer 106 is higher than the Fermi level of the positive electrode layer 101 on the positive electrode layer 101 side, and as shown in FIG. 5( a), current flowing from the positive electrode layer 101 to the negative electrode layer 102 is blocked.

[0060] When light having a wavelength of 700 nm or more is irradiated onto the photoelectric conversion element 100, the upconversion particles 10 constituting the second layer 105 absorb the light and convert the wavelength into visible light. Next, the inorganic perovskite-type material 17 absorbs the wavelength-converted light (FIG. 5(b)). Note that the dashed arrow and the solid arrow of the upconversion particles 10 in FIG. 5(b) indicate the same energy level. By absorbing light, the inorganic perovskite-type material 17 generates electrons e and holes h, and the electrons e enter the conduction band E c1 and the hole h moves to the valence band E v3 (FIG. 5(c)).

[0061] The photoelectric conversion element is not limited to the above configuration. Figure 6 is a cross-sectional view of a modified example 100x of the photoelectric conversion element having the upconversion particles 10 of Figure 1. The photoelectric conversion element 100x is composed of a positive electrode layer (positive electrode member) 101, a negative electrode layer (negative electrode member) 102, and a photoelectric conversion layer 103x sandwiched therebetween. The photoelectric conversion layer 103x is composed of a layered second layer 105 and a layered third layer 106. As in the photoelectric conversion element 100x, the second layer 105 and the third layer 106 may be formed as uniform films.

[0062] (Method for manufacturing photoelectric conversion element 100) There are no particular limitations on the method for manufacturing the photoelectric conversion element 100. The photoelectric conversion element 100 can be manufactured by forming each layer using a known method such as a vacuum deposition method, a spin coating method, or a dipping method.

[0063] The upconversion particle 10 according to the first embodiment, the core 11 (i.e., the upconversion microprecursor particle serving as the central particle) contained in the upconversion particle 10 according to the first embodiment, and the photoelectric conversion element 100 have been described above. The upconversion particle 10 has a hexagonal columnar shape, a particle diameter of 300 nm or more, a thickness of 100 nm or more, and an aspect ratio (particle diameter / thickness) of 1.2 or more and 5.0 or less, thereby providing high upconversion luminescence efficiency. Therefore, the photoelectric conversion element 100 using the upconversion particle 10 has high photoelectric conversion characteristics. Furthermore, the core 11 has a hexagonal columnar shape, a particle diameter of 300 nm or more, a thickness of 100 nm or more, and an aspect ratio (particle diameter / thickness) of 1.2 or more and 5.0 or less, thereby providing high luminescence quantum yield. Therefore, the upconversion particle 10 including the core 11 has high upconversion luminescence efficiency.

[0064] Second Embodiment (Upconversion particle 10A) Fig. 7 is a schematic diagram of an upconversion particle 10A according to one embodiment of the present invention. Fig. 8 is a schematic cross-sectional view of the upconversion particle 10A of Fig. 7 taken along line B-B. The upconversion particle 10A comprises a core portion (central particle) 11A and a shell portion (coating layer) 12A that coats the core portion 11A. The upconversion particle 10A of the present disclosure is a particle having a core-shell structure. The particle shape of the upconversion particle 10A is a hexagonal pillar.

[0065] "Particle diameter of upconversion particles 10A" The particle diameter L1A of the upconversion particles 10A is 300 nm or more. The particle diameter L1A of the upconversion particles 10A is preferably 500 nm or more. The particle diameter L1A of the upconversion particles 10A is more preferably 550 nm or more. The particle diameter L1 of the upconversion particles 10A is particularly preferably 600 nm or more. The particle diameter L1A of the upconversion particles 10A is preferably 2000 nm or less. The particle diameter L1 of the upconversion particles 10A is more preferably 1500 nm or less. Here, the particle diameter L1A of the upconversion particles 10A is the diameter of the smallest encompassing circle that encloses the hexagonal base of the upconversion particle 10.

[0066] "Thickness of Upconversion Particle 10A" The thickness t1A of the upconversion particle 10A is 100 nm or more. The thickness t1A of the upconversion particle 10 is more preferably 300 nm or more. The thickness t1A of the upconversion particle 10 is 600 nm or less. Here, the thickness t1A of the upconversion particle 10 is the length of the hexagonal column in the thickness direction.

[0067] "Particle diameter L1A of upconversion particles 10A / Thickness t1A of upconversion particles 10A" The aspect ratio of the particle diameter of upconversion particles 10A to the thickness of upconversion particles 10A is 1.2 or more and 5.0 or less. It is preferable that the particle diameter L1A of upconversion particles 10A / thickness t1A of upconversion particles 10A is 1.5 or more. By having the aspect ratio of the particle diameter L1A of upconversion particles 10A to the thickness t1A of upconversion particles 10A be 1.2 or more and 5.0 or less, the brightness of visible light or ultraviolet light after conversion of long-wavelength light can be increased. The particle diameter and thickness of upconversion particles 10A can be measured using the same method as for upconversion particles 10.

[0068] "Core portion 11A" The core portion 11A is a particle (upconversion micro precursor particle serving as the central particle) that serves as the core of the upconversion particle (core-shell particle) 10A. The core portion 11A includes at least one of rare earth metals capable of emitting excitation light in the visible or ultraviolet region, such as erbium (Er), thulium (Tm), ytterbium (Yb), neodymium (Nd), holmium (Ho), praseodymium (Pr), gadolinium (Gd), europium (Eu), terbium (Tb), samarium (Sm), cerium (Ce), and dysprosium (Dy), or a compound thereof. The core portion 11A may be, for example, NaErF 4、 Tm 2 O 3 , TmCl 3 , TmF 3 , Er 2 O 3 , ErCl 3 , ErF 3 , Ho 2 O 3 , HoCl 3 , HoF 3 Examples of the inorganic fine particles include inorganic fine particles such as those containing rare earth atoms doped as guests in a host crystal lattice (hereinafter, sometimes referred to as first doped rare earth atoms). The core portion 11A is preferably an inorganic fine particle containing a first doped rare earth atom as a guest in a host crystal lattice. By using inorganic fine particles containing a first doped rare earth atom as a guest in a host crystal lattice as the core portion 11A, the efficiency of upconversion light emission can be improved.

[0069] When the core portion 11A is an inorganic fine particle containing a host crystal lattice containing a doped rare earth atom as a guest, the host crystal lattice of the core portion 11 is, for example, NaYF 4 , Gd 2 O 2 Examples of the crystal lattice serving as the host for the core portion 11 include NaYF 4 The crystal lattice of the core portion 11A is preferably a dielectric.

[0070] When the core portion 11A is an inorganic microparticle containing a doped rare earth atom as a guest in a crystal lattice as a host, examples of the first doped rare earth element include rare earth elements capable of emitting excitation light in the visible or ultraviolet region, such as erbium (Er), thulium (Tm), ytterbium (Yb), neodymium (Nd), holmium (Ho), praseodymium (Pr), gadolinium (Gd), europium (Eu), terbium (Tb), samarium (Sm), cerium (Ce), and dysprosium (Dy). The total content of the first doped rare earth atoms in the core portion 11A is preferably 0.5% to 40% by mass. By having the total content of the first doped rare earth atoms in the core portion 11A be 0.5% to 40% by mass, the collapse of the crystal structure can be suppressed, and the efficiency of upconversion light emission can be improved.

[0071] The core region 11A preferably contains both a light-absorption sensitizing atom and a light-emission activating atom as the first doped rare earth atom. The light-absorption sensitizing atom is, for example, one or more atoms selected from the group consisting of Yb and Nd. The light-absorption sensitizing atom is, for example, Yb or both Yb and Nd atoms. The light-emission activating atom is, for example, one or more atoms selected from the group consisting of Tm, Er, and Ho. The core region 11A may be a Gd doped with Yb and Er. 2 O 2 S (i.e., "Gd 2 O 2 S: Er, Yb"), Yb 3+ and Er 3+ NaYF doped with 4 (i.e., "NaYF 4 :Er, Yb), NaYF doped with Tm and Yb 4 (i.e., "NaYF 4 :Tm, Yb"), NaYF doped with Nd and Yb 4 (i.e., "NaYF 4 The core portion 11A may be an inorganic fine particle made of a host crystal lattice such as NaYF 4It is particularly preferable that the core region 11A contains both a light-absorption-sensitizing atom and a light-emission-activating atom as guests, the light-absorption-sensitizing atom being Yb or both Yb and Nd atoms, and the light-emission-activating atom being one or more atoms selected from the group consisting of Tm, Er, and Ho. It is preferable that the core region 11A contains Nd as the first doped rare earth atom.

[0072] When the core region 11A contains both a light absorption sensitizing atom and a light emission activating atom as the first doped rare earth atom, the doped rare earth atoms contained as guests in the core region 11A are preferably either a pair of Nd and Yb atoms or a pair of Tm and Yb atoms. That is, the core region 11A preferably contains both Nd and Yb atoms as guests, or both Tm and Yb atoms as guests. When the core region contains both Tm and Yb atoms as doped rare earth atoms, the molar ratio of Tm to Yb is preferably 10:30 to 30:10. More preferably, the molar ratio of Tm to Yb is 15:25 to 25:15. When the core region contains Nd and Yb as doped rare earth atoms, the molar ratio of Nd to Yb is preferably 10:30 to 30:10. More preferably, the molar ratio of Nd to Yb is 15:25 to 25:15.

[0073] The particle diameter (diameter length) C1A of the core portion 11A is preferably 500 nm to 1500 nm, and is the diameter of the smallest inclusive circle that encloses the hexagon on a plane perpendicular to the height direction of the hexagonal column.

[0074] (Shell portion 12A) The shell portion 12 is a coating layer that coats the core portion 11A. Examples of materials for the shell portion 12A include rare earth metals that can emit excitation light in the visible or ultraviolet region, such as erbium (Er), thulium (Tm), ytterbium (Yb), neodymium (Nd), holmium (Ho), praseodymium (Pr), gadolinium (Gd), europium (Eu), terbium (Tb), samarium (Sm), cerium (Ce), and dysprosium (Dy), as well as compounds containing at least one of these elements. Examples of materials for the shell portion 12A include NaErF 4、 Tm 2 O 3 , TmCl 3 , TmF 3 , Er 2 O 3 , ErCl 3 , ErF 3 , Ho 2 O 3 , HoCl 3 , HoF 3 Examples of suitable inorganic particles include inorganic fine particles such as those mentioned above, and a coating layer containing rare earth atoms (hereinafter sometimes referred to as second-doped rare earth atoms) doped as guests into a crystal lattice serving as a host. The shell portion 12A is preferably a coating layer containing second-doped rare earth atoms as guests in a crystal lattice serving as a host. The rare earth atoms (e.g., second-doped rare earth atoms) contained in the shell portion 12A are different from the rare earth atoms (e.g., first-doped rare earth atoms) contained in the core portion 11A. By differentiating the rare earth atoms (e.g., second-doped rare earth atoms) contained in the shell portion 12A from the rare earth atoms (e.g., first-doped rare earth atoms) contained in the core portion 11A, energy transfer is more likely to occur, improving the upconversion emission characteristics. It is preferable that energy transfer occurs between the shell portion 12A and the core portion 11A. Specifically, it is preferable that energy transfer occurs between the second doped rare earth atoms in the shell portion 12A and the first doped rare earth atoms in the core portion 11A.

[0075] When the shell portion 12A is a coating layer containing a second doped rare earth atom as a guest in a crystal lattice as a host, the crystal lattice as a host of the shell portion 12A may be, for example, CeO3 , Y 2 O 3 Simple oxides such as NaYF 4 Complex halides such as Gd 2 O 2 S, CaAl 12 O 19 , YTa 7 O 19 , GdTa 7 O 19 , M.T.a. 7 O 11 Examples of suitable crystal lattices for the shell portion 12A include composite oxides such as M (M=Ca, Sr, Ba). The crystal lattice of the shell portion 12A is preferably a dielectric. Examples of suitable crystal lattices for the shell portion 12A include NaYF 4 Preferred are complex halides having low phonon energy such as those mentioned above, which can suppress loss of excitation energy due to non-radiative transition in which energy is lost to heat without emitting light in the excited state.

[0076] When the shell portion 12A is a coating layer containing a second doped rare earth atom as a guest in a crystal lattice as a host, examples of the second doped rare earth element include rare earth elements capable of emitting excitation light in the visible or ultraviolet region, such as erbium (Er), thulium (Tm), ytterbium (Yb), neodymium (Nd), holmium (Ho), praseodymium (Pr), gadolinium (Gd), europium (Eu), terbium (Tb), samarium (Sm), cerium (Ce), and dysprosium (Dy). The total content of the second doped rare earth atoms is preferably 0.5% to 40% by mass relative to the total mass of the shell portion 12A.

[0077] The shell portion 12A preferably contains both a light-absorption sensitizing atom and a light-emission activating atom as the second doped rare earth atom. The light-absorption sensitizing atom is, for example, one or more atoms selected from the group consisting of Yb and Nd. The light-absorption sensitizing atom is, for example, Yb or both Yb and Nd atoms. The light-emission activating atom is, for example, one or more atoms selected from the group consisting of Tm, Er, and Ho. Examples of such a shell portion 12A include Yb 3+ and Er 3+ NaYF doped with4 (i.e., "NaYF 4 :Er, Yb"), Tm 3+ and Yb 3+ NaYF doped with 4 (i.e., "NaYF 4 :Tm, Yb''), Nd 3+ and Yb 3+ NaYF doped with 4 (i.e., "NaYF 4 The shell portion 12A may have a crystal lattice structure made of NaYF 4 It is particularly preferred that the shell portion 12A contains both a light-absorption-sensitizing atom and a light-emission-activating atom as guests, the light-absorption-sensitizing atom being Yb or both Yb and Nd atoms, and the light-emission-activating atom being one or more atoms selected from the group consisting of Tm, Er, and Ho. It is preferred that the shell portion 12A contains Nd as the second doped rare earth atom.

[0078] When the shell portion 12A contains both a light absorption sensitizing atom and a light emission activating atom as the second doped rare earth atom, the second doped rare earth atom contained as a guest in the shell portion 12A is preferably a pair of either Nd and Yb atoms or Tm and Yb atoms. That is, the shell portion 12A preferably contains both Nd and Yb atoms as guests, or both Tm and Yb atoms as guests. When the shell portion 12A contains both Tm and Yb atoms as the second doped rare earth atom, the molar ratio of Tm to Yb is preferably 10:30 to 30:10. More preferably, the molar ratio of Tm to Yb is 15:25 to 25:15. When the shell portion 12A contains Nd and Yb as the second doped rare earth atoms, the molar ratio of Nd to Yb is preferably 10:30 to 30:10, and more preferably 15:25 to 25:15.

[0079] The thickness (width) Sh1A of the shell portion 12A is preferably, for example, 100 nm to 500 nm. As described below, the shell / core ratio (the width of the shell portion to the diameter of the core portion) of the upconversion particle 10 is preferably 0.01 or more and 10.00 or less. Therefore, for example, when the shell / core ratio is 0.01, the thickness (width) Sh1A of the shell portion 12 can be smaller than the lower limit of the above-mentioned preferred range depending on the particle diameter (diameter) C1 of the core portion 11. Specifically, for example, if the particle diameter (diameter) C1 of the core portion 11 is 500 nm, the thickness (width) Sh1A of the shell portion 12 may be 5 nm, and if it is 100 nm, the thickness (width) Sh1A of the shell portion 12 may be 1 nm. The thickness (width) Sh1A of the shell portion 12A is the length of the shell portion 12A in a direction perpendicular to the interface between the core portion 11A and the shell portion 12A on a plane perpendicular to the height direction of the hexagonal prism.

[0080] The coverage of the surface of the core portion 11A with the shell portion 12A is preferably 50% or more, and more preferably 100%.

[0081] The shell portion 12A may be a single layer or may have two or more layers. By increasing the number of layers, even if long-chain organic molecules used as a gelling agent during the production of the upconversion particles 10, specifically after crystal growth by heating in a sol-gel method, remain or adhere to the surface of the particles, the long-chain organic molecules can be separated from the core portion 11, and vibrational deactivation caused by the long-chain organic molecules can be suppressed. This can improve the luminous efficiency of the upconversion particles 10A. For example, when the shell portion 12A has multiple layers, the outermost layer of the shell portion 12A can be made of NaNdF 4 , NaYF 4In this way, the effects of light absorption sensitization and suppression of energy deactivation can be obtained. Incidentally, even if the shell portion 12 has two or more layers in the manufacturing process, for example, if the first shell layer and the second shell layer have the same composition and are integrally formed without a clear interface between the first shell layer and the second shell layer, the first shell layer and the second shell layer can be regarded as a single layer. In such a case, for example, the existence of an interface between the first shell layer and the second shell layer cannot be observed even when observed with an electron microscope.

[0082] (Shell / core ratio, i.e., width of shell 12 / diameter of core 11 of upconversion particle 10A) The shell / core ratio, i.e., width of shell 12 / diameter of core 11 of upconversion particle 10A, is preferably 0.01 or more and 10.00 or less, and more preferably 0.10 or more and 2.00 or less.

[0083] (Relationship between the first doped rare earth atom contained in the core portion 11 and the second doped rare earth atom contained in the shell portion 12A) In order to cause energy transfer from the first doped rare earth atom to the second doped rare earth atom, it is preferable that the first energy level, which is the energy level of the first doped rare earth atom, is different from the second energy level, which is the energy level of the second doped rare earth atom. Specifically, when the second doped rare earth atom emits light, in order to cause energy transfer from the first doped rare earth atom to the second doped rare earth atom, it is preferable that the first energy level, which is the energy level of the first doped rare earth atom in an excited state after being excited by irradiation of external energy such as infrared light (first energy level after excitation), is higher than the second energy level, which is the energy level the second doped rare earth atom receives to emit light (second energy level for emission). When the first doped rare earth atom emits light, in order to cause energy transfer from the second doped rare earth atom to the first doped rare earth atom, it is preferable that the second energy level (second energy level after excitation), which is the energy level of the second doped rare earth atom in an excited state after being excited by external energy irradiation such as infrared light, is higher than the first energy level (first energy level for emission), which is the energy level that the first doped rare earth atom receives to emit light. By doing so, energy transfer (energy transfer) occurs, and the efficiency of upconversion light emission can be improved.

[0084] Preferably, a third doped rare earth atom, which is a doped rare earth atom different from the first doped rare earth atom and the second doped rare earth atom, is further present as a guest in at least one of the core portion 11A and the shell portion 12A. Preferably, the third energy level of the third doped rare earth atom is located between the energy level of the first doped rare earth atom and the energy level of the second doped rare earth atom.

[0085] Specifically, when the core portion 11A or the shell portion 12A contains a third doped rare earth atom and the second doped rare earth atom emits light, in order to cause energy transfer from the first doped rare earth atom to the second doped rare earth atom, it is preferable that the first energy level (first energy level after excitation), which is the energy level of the first doped rare earth atom in an excited state after being excited by irradiation of external energy such as infrared light, is higher than the second energy level (second energy level for emission), which is the energy level the second doped rare earth atom receives in order to emit light, and that the third energy level (third energy level), which is the energy level mediating the energy transfer of the third doped rare earth atom, is located between the energy level of the first doped rare earth atom (first energy level after excitation) and the energy level of the second doped rare earth atom (second energy level for emission). If the energy difference between the first energy level and the third energy level after excitation is 0.3 eV and the energy difference between the third energy level and the second energy level for light emission is 0.3 eV or less, energy transfer occurs, enabling more efficient light emission.

[0086] When the core portion 11A or the shell portion 12A contains a third doped rare earth atom and the first doped rare earth atom emits light, in order to cause energy transfer from the second doped rare earth atom to the first doped rare earth atom, it is preferable that the second energy level (second energy level after excitation), which is the energy level of the second doped rare earth atom in an excited state after being excited by irradiation of external energy such as infrared light, is higher than the first energy level (first energy level for light emission), which is the energy level the first doped rare earth atom receives in order to emit light, and that the third energy level, which is the energy level mediating the energy transfer of the third doped rare earth atom, is located between the energy level of the first doped rare earth atom (first energy level for light emission) and the energy level of the second doped rare earth atom (second energy level after excitation). If the energy difference between the second energy level and the third energy level after excitation is 0.3 eV and the energy difference between the third energy level and the first energy level for light emission is 0.3 eV or less, energy transfer occurs, enabling more efficient light emission.

[0087] It is preferable that the first doped rare earth atoms in the core region 11A are a pair of either Nd and Yb atoms or Tm and Yb atoms, and the second doped rare earth atoms in the shell region 12A are a pair of Nd and Yb atoms or Tm and Yb atoms, which is different from the first doped rare earth atoms. Specifically, when the first doped rare earth atoms in the core region 11A are Nd and Yb, the second doped rare earth atoms in the shell region 12A are Tm and Yb. That is, in this case, the core region 11A contains both Nd and Yb atoms, and the shell region 12A contains both Tm and Yb atoms. When the first doped rare earth atoms in the core region 11A are Tm and Yb, the second doped rare earth atoms in the shell region 12A are Nd and Yb. That is, in this case, the core portion 11A contains both Tm and Yb atoms, and the shell portion 12A contains both Nd and Yb atoms. 2 The upconversion particles coated with the coating were 2 They may also be called coated core-shell type up-conversion particles.

[0088] This section describes upconversion emission in the case where the first doped rare earth atoms in the core section 11A are either a pair of Nd and Yb atoms or a pair of Tm and Yb atoms, and the second doped rare earth atoms in the shell section 12A are either a pair of Nd and Yb atoms or a pair of Tm and Yb atoms that is different from the first doped rare earth atoms. When irradiated with light from the outside, Nd in the core section 11A or the shell section 12A is excited. Energy transfer occurs from the excited Nd to the Yb contained in the core section 11A and the shell section 12A. Next, energy transfer occurs from the Yb to Tm. The Tm that has received the energy emits ultraviolet light, enabling upconversion emission to ultraviolet light. In this case, Nd 2 H 9/2 From Yb 2 F 5/2 Energy transfer occurs to Yb 2 F 5/2 From Tm 3 H 5 Energy transfer occurs between these two molecules, resulting in ultraviolet emission.

[0089] When the second doped rare earth atom emits light, the second doped rare earth atom preferably has a plurality of post-excitation energy levels (post-excitation second energy levels) at positions higher than the pre-excitation energy level (pre-excitation second energy level) at which the second doped rare earth atom has received energy (transition energy) transferred from the first doped rare earth atom or the third doped rare earth atom, and the energy gap (i.e., transition energy) between the pre-excitation energy level and one of the post-excitation energy levels is equal to the transition energy.

[0090] When the first doped rare earth atom emits light, it is preferable that the first doped rare earth atom has a plurality of post-excitation energy levels (post-excitation first energy levels) at positions higher than the pre-excitation energy level (pre-excitation first energy level) at which the first doped rare earth atom has received energy (transition energy) transferred from the second doped rare earth atom or the third doped rare earth atom, and that the energy gap (i.e., transition energy) between the pre-excitation energy level and one of the post-excitation energy levels is equal to the transition energy.

[0091] In the above description, the first doped rare earth atoms are a pair of Nd and Yb or a pair of Tm and Yb, and the second doped rare earth atoms are a pair of Nd and Yb or a pair of Tm and Yb, which is different from the pair of first doped rare earth atoms. The upconversion particle 10A described above can also be understood as an upconversion particle 10A in which the core 11A contains Nd or Tm as the first rare earth atom and Yb as the third rare earth atom, and the shell 12A contains an atom of Nd or Tm as the second rare earth atom different from the first rare earth atom and Yb as the third rare earth atom.

[0092] (Method for Manufacturing Upconversion Particle 10A) Next, a method for manufacturing upconversion particle 10A according to the present disclosure will be described. As shown in Fig. 9, the method for manufacturing upconversion particle 10A according to the present disclosure includes a first step S1 in which core portion 11A is formed by crystal growth using a sol-gel method under conditions ranging from 50°C to 500°C, and a second step S2A in which crystals constituting shell portion 12 are grown on the surface of core portion 11A after first step S1 using a sol-gel method under conditions ranging from 50°C to 500°C.

[0093] "First Step S1" In the first step S1, the core portion 11 is formed by crystal growth under conditions ranging from 50°C to 500°C by a sol-gel method. Specifically, the main raw material is, for example, Y 2 O 3 , Er 2 O 3 , Nd 2 O 3, Tm 2 O 3 , Ho 2 O 3 , Yb 2 O 3 rare earth oxides such as YCl 3 , ErCl 3 , ErF 3 , TmCl 3 , TmF 3 , HoCl 3 , HoF 3 Trifluoroacetate is synthesized using rare earth atom halides such as the above. The ratio of each material is determined depending on the target composition ratio. Furthermore, sodium trifluoroacetate and an organic molecule having 1 to 3 long-chain hydrocarbon groups with approximately 8 to 24 carbon atoms, such as 1-octadecene, oleic acid, oleylamine, trioctylphosphine oxide, linoleic acid, or octylamine, or a long-chain organic molecule such as its carboxylic acid, are used as a gelling agent, and N 2 Alternatively, the reaction is carried out under low temperature conditions (50°C to 500°C) in an Ar atmosphere. After the reaction, the solution is cooled, and an organic solvent such as ethanol is added as needed, followed by centrifugation to separate the central particles that form the core portion 11. The main raw material for the core portion 11 is appropriately adjusted so as to contain a crystal lattice as a host and a doped rare earth atom as a guest. For example, when the crystal lattice as a host is NaYF 4 and when the doped rare earth atoms are Nd and Yb, Y 2 O 3 , Nd 2 O 3 , Yb 2 O 2 and the ratio is determined according to the desired composition ratio of the core region 11.

[0094] The crystal growth in the first step S1 is performed by a heating operation including (a) the formation of an α phase (cubic crystal) and (b) a phase transition from the α phase (cubic crystal) to a β phase (hexagonal crystal). For example, the heating operation for forming the α phase is performed by raising the temperature from room temperature to a temperature range (first temperature range) of 80°C to 150°C at a heating rate of approximately 100°C / 4 minutes to 100°C / 10 minutes, and performing heat treatment in the first temperature range for approximately 10 to 40 minutes. The heating operation for the phase transition from the α phase to the β phase is performed by raising the temperature from the first temperature range to a temperature range (second temperature range) of 200°C to 500°C at a heating rate of approximately 100°C to 300°C / 10 minutes to 15 minutes, and performing heat treatment in the second temperature range for 20 to 80 minutes. By performing heat treatment in the second temperature range for 60 minutes or more, it is possible to obtain only the β phase.

[0095] The heating operation in the first step S1 is preferably performed until the cumulative temperature, which is a heating condition for the phase transition from the α phase to the β phase, exceeds the cumulative temperature, which is a heating condition for the formation of cubic crystals. This facilitates the formation of upconversion particles 10A having a particle diameter of 500 nm or more, a thickness of 300 nm or more, and an aspect ratio (particle diameter / thickness) of 1.2 to 3.0.

[0096] The heating operation in the first step S1 is performed while a degassing operation is performed to maintain a preset degree of vacuum, for example, 0.1 Pa to 0.01 Pa. This facilitates the formation of upconversion particles 10A having a particle diameter of 500 nm or more, a thickness of 300 nm or more, and an aspect ratio (particle diameter / thickness) of 1.2 to 3.0.

[0097] "Second Step S2A" Next, in the second step S2A, crystals constituting the shell portion 12 are grown on the surface of the core portion 11A formed in the first step S1 by a sol-gel method under conditions ranging from 50°C to 500°C. A rare earth atom oxide or rare earth atom halide is selected so that the components of the crystal lattice constituting the shell portion 12A are the same as those of the crystal lattice serving as the host of the core portion 11 described above, but the second doped rare earth atom serving as the guest is different, and a trifluoroacetate salt is synthesized in the same manner as in the first step. The main raw material of the shell portion 12A is appropriately adjusted to include a crystal lattice serving as the host and a second doped rare earth atom serving as the guest. The second doped rare earth atom is adjusted so as to be different from the first rare earth atom of the core portion 11A. For example, if the crystal lattice serving as the host of the core portion 11A is NaYF 4 The first doped rare earth atoms are Nd and Yb, and the crystal lattice serving as the host of the shell portion 12A is NaYF 4 and when the doped rare earth atoms are Tm and Yb, Y 2 O 3 , Tm 2 O 2 , Yb 2 O 2 Next, the core 11 obtained in the first step S1, sodium trifluoroacetate, and an organic molecule having 1 to 3 long-chain hydrocarbon groups with about 8 to 24 carbon atoms, such as 1-octadecene, oleic acid, oleylamine, trioctylphosphine oxide, linoleic acid, or octylamine, or a long-chain organic molecule such as its carboxylic acid, are used as a gelling agent, and N 2Alternatively, the reaction is carried out under low-temperature conditions (50°C to 500°C) in an Ar atmosphere. The solution after the reaction is cooled, and an organic solvent such as ethanol is added as needed, followed by centrifugation to separate the upconversion particles 10A. When a shell portion 12A consisting of multiple layers is formed around the core portion 11, the above steps can be repeated to obtain upconversion particles 10A consisting of multiple layers. It is preferable that the crystal lattice of the core portion 11A formed in the first step S1 and the crystal lattice of the shell portion 12A formed in the second step S2A are of the same composition, and that the second doped rare earth atom in the shell portion 12A is different from the first doped rare earth atom in the core portion 11A.

[0098] (Photoelectric Conversion Element) In the following description, an example will be described in which the upconversion particles 10A emit ultraviolet light. Fig. 10 is a cross-sectional view of a photoelectric conversion element 100A including the upconversion particles 10A. The photoelectric conversion element 100 is mainly composed of a positive electrode layer (positive electrode member) 101, a negative electrode layer (negative electrode member) 102, a photoelectric conversion layer 103A sandwiched therebetween, and an intermediate layer 111 sandwiched between the photoelectric conversion layer 103A and the positive electrode layer 101.

[0099] "Negative electrode layer 102" In order to capture light into the photoelectric conversion layer 103, the negative electrode layer 102 is preferably made of a transparent conductive material such as antimony-doped indium oxide (ATO), indium tin oxide (ITO), zinc oxide, tin oxide, or fluorine-doped indium oxide (FTO). As the negative electrode layer 102, ATO, which has heat resistance, is preferred.

[0100] "Positive electrode layer 101" The positive electrode layer 101 does not need to be transparent, and metals, conductive polymers, etc. can be used as the electrode material of the electrode. Specific examples of electrode materials include metals such as gold (Au), silver (Ag), aluminum (Al), zinc (Zn), and platinum (Pt), as well as alloys of two or more of these metals, graphite, graphite intercalation compounds, polyaniline and its derivatives, and polythiophene and its derivatives. The positive electrode layer 101 is preferably Pt (particularly when the electrolyte is a solution), or Au or Ag (particularly when the electrolyte is a solid).

[0101] "Photoelectric Conversion Layer 103A" As shown in FIG. 10, the photoelectric conversion layer 103A is a TiO 3 film containing upconversion particles 10A. 2 The photoelectric conversion element 100A according to the second embodiment includes a TiO 2 The photoelectric conversion layer 103A includes inorganic semiconductor particles 30 made of the above and up-conversion particles 10A.

[0102] The content of the upconversion particles 10A is preferably 10% by mass to 90% by mass with respect to the total mass of the photoelectric conversion layer 103A. When the content of the upconversion particles 10A is 10% by mass to 90% by mass with respect to the total mass of the photoelectric conversion layer 103A, the photoelectric conversion characteristics of the photoelectric conversion element 100A are improved.

[0103] The content of the inorganic semiconductor particles 30 is preferably 10% by mass to 90% by mass relative to the total mass of the photoelectric conversion layer 103 A. When the content of the inorganic semiconductor particles 30 is 10% by mass to 90% by mass relative to the total mass of the photoelectric conversion layer 103 A, the photoelectric conversion characteristics of the photoelectric conversion element 100 A are improved. The average particle diameter of the inorganic semiconductor particles 30 is 10 nm to 1000 nm.

[0104] The total content of the upconversion particles 10A and the inorganic semiconductor particles 30 is 90% by mass to 100% by mass. In addition to the upconversion particles 10A and the inorganic semiconductor particles 30, the photoelectric conversion layer 103A may contain materials such as a binder.

[0105] Although the number of current paths formed in the photoelectric conversion layer 103A is preferably as large as possible, adjacent current paths may or may not be electrically connected to each other. Note that the "layer" in this embodiment refers to a film formed by one or more film formation processes, and is not limited to being flat, and does not have to be integral.

[0106] "Intermediate layer 111" The intermediate layer 111 is disposed between the photoelectric conversion layer 103A and the positive electrode layer 101. The intermediate layer is, for example, an electrolyte or a hole transport layer. In the case of an electrolyte layer, the material of the intermediate layer 111 is iodine. In the case of a hole transport layer, the material of the intermediate layer 111 is Spiro-OMeTAD or a triphenylamine derivative. The presence of the intermediate layer 111 has the effect of contributing to higher photoelectric conversion efficiency and longer life of the photoelectric conversion element.

[0107] The upconversion particle 10A according to the second embodiment, the core portion 11A (i.e., the upconversion microprecursor particle serving as the central particle) contained in the upconversion particle 10A according to the second embodiment, and the photoelectric conversion element 100A have been described above. The upconversion particle 10A has a hexagonal columnar particle shape, a particle diameter of 300 nm or more, a thickness of 100 nm or more, and an aspect ratio (particle diameter / thickness) of 1.2 or more and 5.0 or less, thereby providing high upconversion luminescence efficiency. Therefore, the photoelectric conversion element 100A using the upconversion particle 10 has high photoelectric conversion characteristics. Furthermore, the core portion 11A has a hexagonal columnar particle shape, a particle diameter of 300 nm or more, a thickness of 100 nm or more, and an aspect ratio (particle diameter / thickness) of 1.2 or more and 5.0 or less, thereby providing high luminescence quantum yield. Therefore, the upconversion particle 10A including the core portion 11A has high upconversion luminescence efficiency.

[0108] In the photoelectric conversion element 100A, when near-infrared light is irradiated, the upconversion particles 10A emit ultraviolet light. 2 In the photoelectric conversion element 100A, by using the upconversion particles 10A, the photoelectric conversion element 100A can generate an electromotive force by using an inorganic semiconductor (TiO 2 ) can be directly absorbed by the electrons. Therefore, it has excellent photoelectric conversion properties.

[0109] Third Embodiment (Upconversion particle 10B) Hereinafter, an upconversion particle 10B according to a third embodiment will be described. The upconversion particle 10B further includes TiO 2 on the surface of the shell layer 12A of the upconversion particle 10A according to the second embodiment. 2 The same elements as those of the upconversion particle 10A are denoted by the same reference numerals, and the description thereof will be omitted.

[0110] Fig. 11 is a schematic diagram of an upconversion particle 10B according to one embodiment of the present invention. Fig. 12 is a schematic cross-sectional view of the upconversion particle 10B taken along line CC of Fig. 11. The upconversion particle 10B comprises a core portion (an upconversion microprecursor particle serving as a central particle) 11B, a shell portion (coating layer) 12B that coats the core portion 11B, and a TiO 2 and a layer 13. Upconversion particle 10B of the present disclosure is a particle having a core-shell structure. Upconversion particle 10B has a particle shape of a hexagonal pillar. Upconversion particle 10A is an upconversion particle that emits upconversion light when exposed to ultraviolet light.

[0111] "TiO 2 layer”TiO 2 Layer 13 is TiO 2 The light emitted from the core portion 11A or the shell portion 12A is converted into TiO 2 The light is absorbed in the layer 13. This allows direct photoelectric conversion.

[0112] TiO 2 The thickness T1B of the layer 13 is, for example, 1 nm to 100 nm.

[0113] TiO on the surface of the shell portion 12A 2 The coverage of the layer 13 is preferably 50% or more. 2 More preferably, the coverage of layer 13 is 100%.

[0114] (Method for Manufacturing Upconversion Particle 10B) Next, a method for manufacturing upconversion particle 10B according to the present disclosure will be described. As shown in Fig. 13, the method for manufacturing upconversion particle 10B according to the present disclosure includes a first step S1 in which core portion 11A is formed by crystal growth using a sol-gel method under conditions ranging from 50°C to 500°C, a second step S2A in which crystals constituting shell portion 12 are grown on the surface of core portion 11A after first step S1 using a sol-gel method under conditions ranging from 50°C to 500°C, and a second step S2A in which TiO 2 The method includes a third step S3 of forming a layer 13. The same steps as those in the method for producing the upconversion particles 10A are denoted by the same reference numerals, and the description thereof will be omitted.

[0115] "Third step S3" In the third step S3, TiO is applied to the surface of the shell portion 12A. 2 The layer 13 is formed on the surface of the shell portion 12A. 2 The method for forming the layer 13 is not particularly limited. For example, a Ti compound (e.g., titanium diisopropylpropoxide bis(acetylacetonate) ([(CH 3 ) 2 CHO] 2 Ti(C 5 H 7 O 2 ) 2 ), or titanium chloride (TiCl 4 ) under a predetermined temperature condition (for example, 70°C for 60 minutes), and then sintered at 450°C for 1 hour to obtain TiO 2 A layer 13 may be formed.

[0116] (Photoelectric Conversion Element) In the following description, an example will be described in which the upconversion particles 10B emit ultraviolet light. FIG. 14 is a cross-sectional view of a photoelectric conversion element 100B including the upconversion particles 10B. The photoelectric conversion element 100 is mainly composed of a positive electrode layer (positive electrode member) 101, a negative electrode layer (negative electrode member) 102, a photoelectric conversion layer 103B sandwiched therebetween, and an intermediate layer 111 sandwiched between the photoelectric conversion layer 103A and the positive electrode layer 101. Elements having the same functions as those of the photoelectric conversion layer 103A are designated by the same reference numerals, and description thereof will be omitted.

[0117] "Photoelectric conversion layer 103B" As shown in FIG. 14, the photoelectric conversion layer 103B includes a layer containing upconversion particles 10B. The content of the upconversion particles 10B is preferably 10% by mass to 90% by mass with respect to the total mass of the photoelectric conversion layer 103B. By having the content of the upconversion particles 10B be 10% by mass to 90% by mass with respect to the total mass of the photoelectric conversion layer 103B, the photoelectric conversion characteristics of the photoelectric conversion element 100B are improved. The photoelectric conversion layer 103B may contain materials such as a binder in addition to the upconversion particles 10B.

[0118] The more current paths formed in the photoelectric conversion layer 103B, the more preferable it is, but adjacent current paths may or may not be electrically connected to each other. Note that the "layer" in this embodiment means a film formed by one or more film formation processes, and is not limited to being flat, and does not have to be integral.

[0119] The upconversion particle 10B according to the third embodiment, the core portion 11A (i.e., the upconversion microprecursor particle serving as the central particle) contained in the upconversion particle 10B according to the third embodiment, and the photoelectric conversion element 100B have been described above. The upconversion particle 10B has a hexagonal columnar particle shape, a particle diameter of 300 nm or more, a thickness of 100 nm or more, and an aspect ratio (particle diameter / thickness) of 1.2 or more and 5.0 or less, thereby providing high upconversion luminescence efficiency. Therefore, the photoelectric conversion element 100B using the upconversion particle 10B has high photoelectric conversion characteristics. Furthermore, the core portion 11A has a hexagonal columnar particle shape, a particle diameter of 300 nm or more, a thickness of 100 nm or more, and an aspect ratio (particle diameter / thickness) of 1.2 or more and 5.0 or less, thereby providing high luminescence quantum yield. Therefore, the upconversion particle 10B including the core portion 11A has high upconversion luminescence efficiency.

[0120] In the photoelectric conversion element 100B, when irradiated with near-infrared light, the core portion 11A or the shell portion 12A in the upconversion particle 10B emits ultraviolet light. 2 The photoelectric conversion element 100B uses upconversion particles 10B, which allows direct absorption into the inorganic semiconductor without dye sensitization. This provides excellent photoelectric conversion characteristics. In addition, the ultraviolet light generated in the core portion 11A or the shell portion 12A is absorbed by the TiO 2 Since the light is absorbed in the layer 13, the photoelectric conversion characteristics are higher than those of the photoelectric conversion element 100A.

[0121] As described above, the upconversion particles 10, 10A, and 10B and photoelectric conversion elements 100, 100A, and 100B according to this embodiment are capable of upconversion emission even under low excitation light such as sunlight irradiation, can obtain higher sensitization characteristics using weak light with long wavelengths, and can be manufactured inexpensively.

[0122] The upconversion particles 10, 10A, and 10B according to the present embodiment can be used in liquid crystal displays, solid-state lasers, sensors, solar cells, biomarkers, etc. The photoelectric conversion elements 100, 100A, and 100B according to the present embodiment can be used in solar cells and near-infrared detectors.

[0123] In the upconversion particle according to this embodiment, the core 11 has a structure containing doped rare earth atoms (for example, ErYF 4 ), and the shell portion 12 is a two-layer structure of a perovskite structure (for example, CsPbI 3 / CsPbI 3 ) By making the shell portion 12 a perovskite structure, the light wavelength-converted in the core portion 11 can be directly absorbed by the perovskite structure. Furthermore, since the above-mentioned upconversion particles have the specific particle size, particle shape, and core-shell structure of the core-shell type upconversion microparticles of the present invention, they can exhibit excellent visible light (internal) quantum efficiency and near-infrared light quantum yield.

[0124] The upconversion particle according to this embodiment may further include a second shell portion on the surface of the shell portion 12, the second shell portion being an organic compound having light absorption in the near-infrared or infrared region and containing a multidentate organic ligand having at least two or more coordination sites. Furthermore, the surface of the second shell portion may further include a third shell portion containing a coordination metal capable of forming a coordination bond with the multidentate organic ligand of the second shell portion. This can improve detection sensitivity. Furthermore, since the upconversion particle has the specific particle size, particle shape, and core-shell structure of the core-shell upconversion microparticles of the present invention, it can exhibit excellent visible light (internal) quantum efficiency and near-infrared light quantum yield.

[0125] In the upconversion particle according to this embodiment, the core 11 is Er 3+ The core 11 may contain Er, and the shell 12 may be composed of a plurality of layers. 3+ and the layer (adjacent layer) of the shell portion 12 adjacent to the core portion 11 contains Yb 3+ and the layer provided on the surface of the adjacent layer contains Er. 3+ The upconversion particles may contain a compound having a specific particle size, particle shape, and core-shell structure, which are characteristic of the core-shell upconversion microparticles of the present invention.

[0126] Within the scope of the present invention, the components in the above-described embodiments may be replaced with known components as appropriate, and the above-described components may be combined as appropriate.

[0127] The effects of the present invention will be made clearer by the following examples. Note that the present invention is not limited to the following examples and can be practiced with appropriate modifications within the scope of the present invention.

[0128] (Production of Upconversion Particles) Upconversion particles were produced according to the above-described method for producing upconversion particles, specifically under the following conditions.

[0129] (Example 1) (Upconversion microparticle precursor serving as the central particle of the present invention) The core of the core-shell type upconversion microparticle (i.e., the upconversion microparticle precursor serving as the central particle) was synthesized by a sol-gel method. 2 O 3 ) 0.975 mmol, Yb oxide (Yb 2 O 3 ) 0.25 mmol, Er oxide (Er 2 O 3 0.025 mmol of sodium trifluoroacetate (NaCOOCF) was mixed with 10 mL of trifluoroacetic acid and 10 mL of water. The resulting mixture was heated and stirred at 80°C under reduced pressure. The powder obtained by evaporation to dryness was treated with sodium trifluoroacetate (NaCOOCF 3 ) 2.5 mmol was added. This was mixed with 7.5 mL of oleic acid and 7.5 mL of 1-octadecene. The resulting mixture was stirred at 100°C under reduced pressure for 30 minutes (formation of the α phase), and then stirred at 330°C under reduced pressure for 60 minutes to cause a phase transition from the α phase to the β phase. The pressure was reduced to a predetermined pressure (0.01 Pa) or less by degassing using a vacuum pump. After stirring, the mixture was cooled to 80°C, and 20 mL of ethanol was added to it. Upconversion microprecursor particles (NaYF) that would become the central particles of Example 1 were extracted from the resulting mixture by centrifugation. 4 The upconversion micro-precursor particles had a particle size of 600 nm and a thickness of 150 nm.

[0130] (Comparative Example 1-1) (Nanoparticles) Y oxide (Y 2 O 3 ) 0.975 mmol, Yb oxide (Yb 2 O 3 ) 0.25 mmol, Er oxide (Er 2 O 30.025 mmol of sodium trifluoroacetate (NaCOOCF) was mixed with 10 mL of trifluoroacetic acid and 10 mL of water. The resulting mixture was heated and stirred at 80°C under reduced pressure. The powder obtained by evaporation to dryness was treated with sodium trifluoroacetate (NaCOOCF 3 ) 5.0 mmol was added. This was mixed with 7.5 mL of oleic acid and 7.5 mL of 1-octadecene. The resulting mixture was stirred at 100°C under reduced pressure for 30 minutes (formation of the α phase), and then stirred at 330°C under reduced pressure for 15 minutes to cause a phase transition from the α phase to the β phase. The pressure was reduced to a predetermined pressure (0.01 Pa) or less by degassing using a vacuum pump. After stirring, the mixture was cooled to 80°C, and 20 mL of ethanol was added thereto. The nanoparticles of Comparative Example 1-1 (NaYF 4 The nanoparticles were separated into 100 nm diameter and 50 nm thickness.

[0131] (Comparative Example 1-2) (Cubic (α phase) particles) No. 1 Y oxide (Y 2 O 3 ) 0.975 mmol, Yb oxide (Yb 2 O 3 ) 0.25 mmol, Er oxide (Er 2 O 3 0.025 mmol of sodium trifluoroacetate (NaCOOCF) was mixed with 10 mL of trifluoroacetic acid and 10 mL of water. The resulting mixture was heated and stirred at 80°C under reduced pressure. The powder obtained by evaporation to dryness was treated with sodium trifluoroacetate (NaCOOCF 3 ) 2.5 mmol was added. This was mixed with 7.5 mL of oleic acid and 7.5 mL of 1-octadecene. The resulting mixture was stirred at 100°C under reduced pressure for 30 minutes (formation of the α-phase), and then the mixture was stirred at 330°C under reduced pressure for 10 minutes. The reduced pressure was degassed using a vacuum pump to a predetermined pressure (0.01 Pa) or less. After stirring, the mixture was cooled to 80°C, and 20 mL of ethanol was added thereto. Cubic (α-phase) particles (NaYF 4 : Yb, Er) was separated.

[0132] (Example 2-1) Core-shell type upconversion microparticles of the present invention (No. 1: formation of first shell, No. 2: formation of second shell) are prepared by using Y oxide (Y) as the core of the upconversion microparticle precursor. 2 O 3 ) 0.7375 mmol, Yb oxide (Yb 2 O 3 ) 0.50 mmol, Tm oxide (Tm 2 O 3 0.0125 mmol of sodium trifluoroacetate (NaCOOCF) was mixed with 10 mL of trifluoroacetic acid and 10 mL of water. The resulting mixture was heated and stirred at 80°C under reduced pressure. The powder obtained by evaporation to dryness was treated with sodium trifluoroacetate (NaCOOCF 3 2.65 mmol of NaYF4:Yb,Tm (core) was added to the mixture. This was mixed with 7.5 mL of oleic acid and 7.5 mL of 1-octadecene. The resulting mixture was stirred at 100°C under reduced pressure for 30 minutes (forming the α phase), and then stirred at 330°C under reduced pressure for 60 minutes to induce a phase transition from the α phase to the β phase. The pressure was reduced to a predetermined pressure (0.01 Pa) or less by degassing using a vacuum pump. After stirring, the mixture was cooled to 80°C, and 20 mL of ethanol was added. Upconversion microprecursor particles (NaYF4:Yb,Tm (core)), which would become the central particles of Example 2-1, were separated from the resulting mixture by centrifugation. The particle size of the upconversion microparticles was 850 nm and the thickness was 570 nm.

[0133] (Example 2-2) Core-shell type upconversion microparticle No. 1 of the present invention The first coating layer was formed on the upconversion microparticle precursor, which was the central particle of Example 2-1, separated above, by a sol-gel method. Specifically, a Y oxide (Y 2 O 3 0.5 mmol of the above-mentioned core particle 1 was mixed with 5 mL of trifluoroacetic acid and 5 mL of water. The mixture was heated and stirred at 80° C. under reduced pressure. The powder obtained by evaporation to dryness was mixed with 1.0 mmol of the above-mentioned core particle 1 and sodium trifluoroacetate (NaCOOCF 32.0 mmol of NaYF was added to the resulting mixture, which was then mixed with 7.5 mL of oleic acid and 7.5 mL of 1-octadecene. The resulting mixture was stirred at 100°C under reduced pressure for 30 minutes, and then stirred at 300°C under reduced pressure for 60 minutes. After stirring, the mixture was cooled to 80°C, and 20 mL of ethanol was added to the mixture. The core-shell upconversion microparticles (NaYF) of Example 2-2 were extracted from the resulting mixture by centrifugation. 4 : Yb, Tm (core), NaYF 4 (shell) × 1) was separated. The reduced pressure was achieved by degassing using a vacuum pump to a predetermined pressure (0.01 Pa) or less. The particle size and thickness of the core-shell upconversion microparticles of Example 2-2 were obtained by analyzing SEM images obtained by SEM observation according to the above-mentioned measurement method. The particle size and thickness of the core-shell upconversion microparticles of Example 2-2 were 1000 nm and 590 nm, respectively. The shell / core ratio was 5.7.

[0134] Example 2-3 Core-shell upconversion microparticles No. 2 of the present invention The second coating layer was formed on the core-shell upconversion microparticles of Example 2-2 containing the first coating layer separated above by a sol-gel method. 2 O 3 0.5 mmol of the above-mentioned core particle 1 was mixed with 5 mL of trifluoroacetic acid and 5 mL of water. The mixture was heated and stirred at 80° C. under reduced pressure. The powder obtained by evaporation to dryness was mixed with 1.0 mmol of the above-mentioned core particle 1 and sodium trifluoroacetate (NaCOOCF 3 2.0 mmol of NaYF was added to the resulting mixture, which was then mixed with 7.5 mL of oleic acid and 7.5 mL of 1-octadecene. The resulting mixture was stirred at 100°C under reduced pressure for 30 minutes, and then stirred at 300°C under reduced pressure for 60 minutes. After stirring, the mixture was cooled to 80°C, and 20 mL of ethanol was added to the mixture. The core-shell upconversion microparticles (NaYF) of Example 2-3 were extracted from the resulting mixture by centrifugation. 4 : Yb, Tm (core), NaYF 4(shell) × 2) were separated. The pressure was reduced by degassing using a vacuum pump to a predetermined pressure (0.01 Pa) or less. The particle size and thickness of the core-shell upconversion microparticles of Example 2-3 were obtained by analyzing SEM images obtained by SEM observation according to the above-mentioned measurement method. The particle size and thickness of the core-shell upconversion microparticles of Example 2-3 were 1100 nm and 600 nm, respectively. The shell / core ratio was 3.4.

[0135] (Comparative Example 2) α cubic crystal (α phase) particle No. 2 Y oxide (Y 2 O 3 ) 0.7375 mmol, Yb oxide (Yb 2 O 3 ) 0.50 mmol, Tm oxide (Tm 2 O 3 0.0125 mmol of sodium trifluoroacetate (NaCOOCF) was mixed with 10 mL of trifluoroacetic acid and 10 mL of water. The resulting mixture was heated and stirred at 80°C under reduced pressure. The powder obtained by evaporation to dryness was treated with sodium trifluoroacetate (NaCOOCF 3 ) 2.65 mmol was added. This was mixed with 7.5 mL of oleic acid and 7.5 mL of 1-octadecene. The resulting mixture was stirred at 100°C under reduced pressure for 30 minutes (formation of the α-phase), and then the mixture was stirred at 330°C under reduced pressure for 10 minutes. The reduced pressure was degassed using a vacuum pump to a predetermined pressure (0.01 Pa) or less. After stirring, the mixture was cooled to 80°C, and 20 mL of ethanol was added thereto. Cubic (α-phase) particles (NaYF 4 : Yb, Er) was separated.

[0136] (Example 3-1) Core-shell type upconversion microparticle No. 3 of the present invention The core part of the core-shell type upconversion microparticle (i.e., the upconversion micro precursor particle that becomes the central particle) was synthesized by the sol-gel method. Specifically, Y oxide (Y 2 O 3 ) 0.744 mmol, Yb oxide (Yb 2 O 3 ) 0.50 mmol, Tm oxide (Tm 2 O3 0.00625 mmol of sodium trifluoroacetate (NaCOOCF) was mixed with 10 mL of trifluoroacetic acid and 10 mL of water. The resulting mixture was heated and stirred at 80°C under reduced pressure. The powder obtained by evaporation to dryness was treated with sodium trifluoroacetate (NaCOOCF 3 2.65 mmol of ethanol was added. This was mixed with 7.5 mL of oleic acid and 7.5 mL of 1-octadecene. The resulting mixture was stirred at 100°C under reduced pressure for 30 minutes (forming the α phase), and then stirred at 330°C under reduced pressure for 60 minutes to induce a phase transition from the α phase to the β phase. The reduced pressure was degassed using a vacuum pump to a predetermined pressure (0.01 Pa) or less. After stirring, the mixture was cooled to 80°C, and 20 mL of ethanol was added. Upconversion microprecursor particles, which would become the central particles of Example 3-1, were separated from the resulting mixture by centrifugation. The particle size of the upconversion microprecursor particles was 630 nm and the thickness was 420 nm.

[0137] The first coating layer was formed on the upconversion micro-precursor particles, which were the central particles of Example 3-1, by a sol-gel method. 2 O 3 ) 0.30 mmol, Yb oxide (Yb 2 O 3 ) 0.15 mmol, Nd oxide (Nd 2 O 3 0.05 mmol of sodium trifluoroacetate (NaCOOCF) was mixed with 5 mL of trifluoroacetic acid and 5 mL of water. The resulting mixture was heated and stirred at 80°C under reduced pressure. The powder obtained by evaporation to dryness was treated with sodium trifluoroacetate (NaCOOCF 3) 2.65 mmol was added. This was mixed with 7.5 mL of oleic acid and 7.5 mL of 1-octadecene. The resulting mixture was stirred at 100°C under reduced pressure for 30 minutes (formation of the α phase), and then stirred at 330°C under reduced pressure for 60 minutes to cause a phase transition from the α phase to the β phase. The reduced pressure was degassed using a vacuum pump to a predetermined pressure (0.01 Pa) or less. After stirring, the mixture was cooled to 80°C, and 20 mL of ethanol was added to it. The core-shell upconversion microparticles (NaYF) of Example 3-1 were extracted from the resulting mixture by centrifugation. 4 : Yb, Tm (core), NaYF 4 : Yb, Nd (shell)) were separated. The particle size of the core-shell upconversion microparticles including the first coating layer was 850 nm, and the shell thickness was 500 nm.

[0138] (Example 3-2) Core-shell type upconversion microparticle No. 4 of the present invention The core part of the core-shell type upconversion microparticle (i.e., the upconversion micro precursor particle that becomes the central particle) was synthesized by the sol-gel method. Specifically, Y oxide (Y 2 O 3 ) 0.75 mmol, Yb oxide (Yb 2 O 3 ) 0.375 mmol, Nd oxide (Nd 2 O 3 0.125 mmol of sodium trifluoroacetate (NaCOOCF) was mixed with 10 mL of trifluoroacetic acid and 10 mL of water. The resulting mixture was heated and stirred at 80°C under reduced pressure. The powder obtained by evaporation to dryness was treated with sodium trifluoroacetate (NaCOOCF 32.65 mmol of ethanol was added. This was mixed with 7.5 mL of oleic acid and 7.5 mL of 1-octadecene. The resulting mixture was stirred at 100°C under reduced pressure for 30 minutes (forming the α phase), and then stirred at 330°C under reduced pressure for 60 minutes to induce a phase transition from the α phase to the β phase. The reduced pressure was degassed using a vacuum pump to a predetermined pressure (0.01 Pa) or less. After stirring, the mixture was cooled to 80°C, and 20 mL of ethanol was added. Upconversion microprecursor particles, which would become the central particles of Example 3-2, were separated from the resulting mixture by centrifugation. The particle size of the upconversion microprecursor particles was 300 nm and the thickness was 170 nm.

[0139] The first coating layer was formed on the upconversion micro-precursor particles, which were the central particles of Example 3-2, by a sol-gel method. 2 O 3 ) 0.295 mmol, Yb oxide (Yb 2 O 3 ) 0.20 mmol, Tm oxide (Tm 2 O 3 0.005 mmol of sodium trifluoroacetate (NaCOOCF) was mixed with 5 mL of trifluoroacetic acid and 5 mL of water. The resulting mixture was heated and stirred at 80°C under reduced pressure. The powder obtained by evaporation to dryness was treated with sodium trifluoroacetate (NaCOOCF 3 ) 2.65 mmol was added. This was mixed with 7.5 mL of oleic acid and 7.5 mL of 1-octadecene. The resulting mixture was stirred at 100°C under reduced pressure for 30 minutes (formation of the α phase), and then stirred at 330°C under reduced pressure for 60 minutes to cause a phase transition from the α phase to the β phase. The reduced pressure was degassed using a vacuum pump to a predetermined pressure (0.01 Pa) or less. After stirring, the mixture was cooled to 80°C, and 20 mL of ethanol was added to it. The core-shell type upconversion microparticles (NaYF) of Example 3-2 were extracted from the resulting mixture by centrifugation. 4 : Yb, Nd (core), NaYF 4 : Yb, Tm (core)) was separated. The core-shell upconversion microparticles including the first coating layer had a particle size of 400 nm and a thickness of 220 nm.

[0140] (Example 4) TiO of the present invention 2 Coated Core-Shell Upconversion Microparticles The core of the core-shell upconversion microparticles (i.e., the upconversion microparticle precursor serving as the central particle) was synthesized by the sol-gel method. 2 O 3 ) 0.744 mmol, Yb oxide (Yb 2 O 3 ) 0.50 mmol, Tm oxide (Tm 2 O 3 0.00625 mmol of sodium trifluoroacetate (NaCOOCF) was mixed with 10 mL of trifluoroacetic acid and 10 mL of water. The resulting mixture was heated and stirred at 80°C under reduced pressure. The powder obtained by evaporation to dryness was treated with sodium trifluoroacetate (NaCOOCF 3 2.65 mmol of ethanol was added. This was mixed with 7.5 mL of oleic acid and 7.5 mL of 1-octadecene. The resulting mixture was stirred at 100°C under reduced pressure for 30 minutes (forming the α phase), and then stirred at 330°C under reduced pressure for 60 minutes to induce a phase transition from the α phase to the β phase. The pressure was reduced to a predetermined pressure (0.01 Pa) or less by degassing using a vacuum pump. After stirring, the mixture was cooled to 80°C, and 20 mL of ethanol was added. Upconversion microprecursor particles, which would become the central particles of Example 4, were separated from the resulting mixture by centrifugation. The particle size of the upconversion microprecursor particles was 630 nm and the thickness was 420 nm.

[0141] The first coating layer was formed on the upconversion micro-precursor particles, which were separated as described above and which were to become the central particles of Example 4, by a sol-gel method. 2 O 3 ) 0.30 mmol, Yb oxide (Yb 2 O 3 ) 0.15 mmol, Nd oxide (Nd 2 O 30.05 mmol of sodium trifluoroacetate (NaCOOCF) was mixed with 5 mL of trifluoroacetic acid and 5 mL of water. The resulting mixture was heated and stirred at 80°C under reduced pressure. The powder obtained by evaporation to dryness was treated with sodium trifluoroacetate (NaCOOCF 3 ) 2.65 mmol was added. This was mixed with 7.5 mL of oleic acid and 7.5 mL of 1-octadecene. The resulting mixture was stirred at 100°C under reduced pressure for 30 minutes (formation of the α phase), and then stirred at 330°C under reduced pressure for 60 minutes to cause a phase transition from the α phase to the β phase. The pressure was reduced to a predetermined pressure (0.01 Pa) or less by degassing with a vacuum pump. After stirring, the mixture was cooled to 80°C, and 20 mL of ethanol was added to it. The core-shell type upconversion microparticles (NaYF) of Example 4 were extracted from the resulting mixture by centrifugation. 4 : Yb, Tm (core), NaYF 4 : Yb, Nd (shell)) was separated. The core-shell upconversion microparticles including the first coating layer had a particle size of 850 nm and a thickness of 500 nm.

[0142] The outermost layer of the core-shell type upconversion microparticles of Example 4 separated above was coated with TiO 2 Specifically, a layer of titanium diisopropoxide bis(acetylacetonate) [(CH 3 ) 2 CHO] 2 Ti(C 5 H 7 O 2 ) 2 1 mmol of the coated particles was mixed with a 20 mmol / L ethanol solution. The resulting mixture was stirred at 70°C for 1 hour. After stirring, the resulting solid was heated at 450°C for 1 hour to obtain the TiO 2 Coated core-shell type upconversion microparticles were obtained. 2 The particle size of the coated core-shell upconversion microparticles was 860 nm and the thickness was 520 nm. 2 The shell (excluding TiO 2 The (including layer) / core ratio was 0.365.2 The thickness was 10 nm.

[0143] (Example 5) Preparation of a photoelectric conversion element of the present invention A conductive substrate was prepared in which fluorine-doped tin oxide (FTO) was provided on a glass substrate. 2 A dispersion containing coated core-shell upconversion microparticles and titanium oxide powder (particle diameter 1 μm or less) was spin-coated onto the substrate and heated at 400°C to obtain a cathode substrate. 0.026 g of iodine and 0.166 g of potassium iodide were dissolved in 2 mL of ethylene glycol to prepare an electrolyte solution. Next, a Pt film was formed on a glass substrate by vacuum deposition to obtain an anode substrate. The anode substrate and the cathode substrate were arranged so that the FTO and Ag faced each other, and an electrolyte solution (electrolyte: I, solvent: ethylene glycol) was filled between the anode substrate and the cathode substrate to produce a photoelectric conversion element.

[0144] Using an X-ray diffraction device, measurements were performed on the upconversion microprecursor particles that serve as the central particles in Example 1, the core-shell type upconversion microparticles in Example 2-2, the cubic crystal (α-phase) particles in Comparative Example 1-2, and the cubic crystal (α-phase) particles in Comparative Example 2.

[0145] (Test Example 1) Emission spectrum of each particle The upconversion microparticles serving as the central particles in Example 1, the upconversion microparticles serving as the central particles in Example 2-1, the core-shell upconversion microparticles in Example 2-2, the core-shell upconversion microparticles in Example 2-3, and the nanoparticles in Comparative Example 1-1, the cubic (α-phase) particles in Comparative Example 1-2, and the cubic (α-phase) particles in Comparative Example 2 were irradiated with near-infrared light having a wavelength of 980 nm. The emission spectra were measured using an absolute PL quantum yield measurement device manufactured by Hamamatsu Photonics, and the quantum efficiencies were determined from the obtained emission spectra. Similarly, the core-shell upconversion microparticles in Example 3-1 and the core-shell upconversion microparticles in Example 3-2 were irradiated with near-infrared light having a wavelength of 790 nm. The emission spectra were measured using an absolute PL quantum yield measurement device manufactured by Hamamatsu Photonics, and the quantum efficiencies were determined from the obtained emission spectra.

[0146] (Test Example 2) SEM Observation of Each Particle Using a scanning electron microscope manufactured by Hitachi High-Technologies Corporation at a magnification of 150,000 times, each particle of Example 1, Example 2-1, Example 3-1 (core, core-shell), Example 3-2 (core, core-shell), and Comparative Examples 1-1, 1-2, and 2 was observed to obtain an SEM image.

[0147] Test Example 3: FT-IR measurement of each particle Using a Fourier transform infrared spectrophotometer (FT-IR), FT-IR measurement was carried out on each particle (particles of Example 1, Example 2-1, Comparative Examples 1-2, and Comparative Example 2). The measurement was carried out by a transmission method, in which KBr and each particle were mixed to prepare a pellet, and the measurement was carried out.

[0148] (Test Example 4) Photocurrent response characteristics of the photoelectric conversion element of the present invention The photoresponse characteristics were measured for the photoelectric conversion element of Example 5. The voltage applied between the positive electrode layer and the negative electrode layer of the photoelectric conversion element was set to -0.5 V. The wavelength and irradiance of the light irradiating the photoelectric conversion element were 808 nm and 10 mW / cm, respectively. 2 It was decided.

[0149] FIG. 15 shows XRD patterns of Example 1 and Comparative Example 1-2. The horizontal axis of FIG. 15 is 2θ (degrees), and the vertical axis of FIG. 15 is intensity (arbitrary). FIG. 15(a) is an XRD pattern of the upconversion microparticle that serves as the central particle of Example 1, and FIG. 15(b) is an XRD pattern of the cubic (α-phase) particle of Comparative Example 1-2. From FIG. 15, it was confirmed that the upconversion microparticle that serves as the central particle of Example 1 is the β-phase, and the cubic (α-phase) particle of Comparative Example 1-2 is the α-phase.

[0150] Figure 16(a) is an SEM image of Example 1, Figure 16(b) is an SEM image of nanoparticles of Comparative Example 1-1, and Figure 16(c) is an SEM image of cubic particles of Comparative Example 1-2. The particle size of the upconversion microprecursor particles estimated from the SEM image was 600 nm and the thickness was 150 nm. The particle size of the cubic (α phase) particles of Comparative Example 2 estimated from the SEM image was 100 nm and the thickness was 50 nm.

[0151] 17 shows FT-IR spectra of Example 1 (upconversion micro precursor particles) and Comparative Example 1-2 (cubic (α-phase) particles). The horizontal axis shows wave numbers (cm -1 ), and the vertical axis is absorbance (arbitrary). FIG. 17(a) is the FT-IR spectrum of Example 1, and FIG. 17(b) is the FT-IR spectrum of Comparative Example 1-2. As shown in FIG. 17, in the FT-IR spectrum of Example 1, -1 ~2800cm -1 and approximately 1700 cm -1 ~1400cm -1 A decrease in absorbance was confirmed.

[0152] 18 shows the emission spectra of Example 1 and Comparative Examples 1 and 2. The horizontal axis of FIG. 18 shows the wavelength (cm -1 ), and the vertical axis represents intensity (arbitrary). The solid line represents the emission spectrum of Example 1, and the dotted line represents the emission spectrum of Comparative Example 1-2. As shown in FIG. 18, the particles of Example 1, which had a larger particle size, had a higher emission intensity than the particles of Comparative Example 1-2. The luminescence quantum efficiency (%) of each particle of Example 1, Comparative Example 1-1, and Comparative Example 1-2 obtained based on these results is shown in Table 1 (excitation wavelength 980 nm). The upconversion microparticles, which are the central particles of Example 1, had a particle diameter of 300 nm or more, a thickness of 100 nm or more, and an aspect ratio (particle diameter / thickness) of 1.2 or more and 5.0 or less, and therefore had a significantly higher luminescence quantum efficiency than the nanoparticles of Comparative Example 1-1 and the cubic (α-phase) particles of Comparative Example 1-2.

[0153]

[0154] FIG. 19 shows XRD patterns of the core portion (i.e., the upconversion micro precursor particle that serves as the central particle) contained in the core-shell upconversion microparticle of Example 2-2 and the cubic (α-phase) particle of Comparative Example 2. The horizontal axis of FIG. 19 is 2θ (degrees), and the vertical axis of FIG. 19 is intensity (arbitrary). FIG. 19(a) is the XRD pattern of the core portion (i.e., the upconversion micro precursor particle that serves as the central particle) contained in the core-shell upconversion microparticle of Example 2-2, and FIG. 19(b) is the XRD pattern of the cubic (α-phase) particle of Comparative Example 2. It was confirmed from FIG. 19 that the core portion of the core-shell upconversion microparticle of Example 2-2 is the β-phase, and the cubic (α-phase) particle of Comparative Example 2 is the α-phase.

[0155] Figure 20(a) is an SEM image of Example 2-1, and Figure 20(b) is an SEM image of cubic crystal particles of Comparative Example 2. The particle size of the upconversion microprecursor particles of Example 2-1 estimated from the SEM image was 850 nm, and the thickness was 570 nm. The particle size of the cubic crystal (α phase) particles of Comparative Example 2 estimated from the SEM image was 100 nm, and the thickness was 50 nm.

[0156] 21 shows FT-IR spectra of Example 2-1 (upconversion micro precursor particles) and Comparative Example 2 (cubic (α-phase) particles). The horizontal axis shows wave numbers (cm -1 ), and the vertical axis is absorbance (arbitrary). FIG. 21(a) is the FT-IR spectrum of Example 2-1, and FIG. 21(b) is the FT-IR spectrum of Comparative Example 2. As shown in FIG. 21, in the FT-IR spectrum of Example 2-1, -1 ~2800cm -1 and approximately 1700 cm -1 ~1400cm -1 A decrease in absorbance was confirmed.

[0157] 22 shows the emission spectra of Example 2-1 and Comparative Example 2. The horizontal axis of FIG. 22 shows the wavelength (cm -122 ), and the vertical axis represents intensity (arbitrary). The solid line represents the emission spectrum of Example 2-1, and the dotted line represents the emission spectrum of Comparative Example 2. As shown in FIG. 22 , the particles of Example 2-1, which had a larger particle size, had a higher emission intensity than the particles of Comparative Example 2.

[0158] Table 2 shows the luminescence quantum efficiency (%) of each particle of Examples 2-1, 2-2, 2-3, and Comparative Example 2 (excitation wavelength 980 nm). Each particle of Examples 2-1, 2-2, and 2-3 had a particle diameter of 300 nm or more, a thickness of 100 nm or more, and an aspect ratio (particle diameter / thickness) of 1.2 or more and 5.0 or less, and therefore had a significantly higher luminescence quantum efficiency than the cubic crystal (α-phase) particles of Comparative Example 2 and the cubic crystal (α-phase) particles of Comparative Example 1-2. Furthermore, the core-shell upconversion microparticles of Examples 2-1 and 2-2 had a shell portion, and therefore further improved luminescence quantum efficiency.

[0159]

[0160] FIG. 23 shows the XRD pattern of the core and the XRD pattern of the core-shell of Example 3-1. That is, the XRD patterns are of the core portion contained in the core-shell upconversion microparticle (i.e., the upconversion micro precursor particle that serves as the central particle) and the core-shell upconversion microparticle. The horizontal axis of FIG. 23 is 2θ (degrees), and the vertical axis of FIG. 23 is intensity (arbitrary). FIG. 23(a) is the XRD pattern of the core portion contained in the core-shell upconversion microparticle of Example 3-1 (i.e., the upconversion microparticle of Example 3-1 that serves as the central particle), and FIG. 23(b) is the XRD pattern of the core-shell upconversion microparticle of Example 3-2. It was confirmed from FIG. 23 that the core-shell upconversion microparticle of Example 3-1 and its core portion were both in the β phase.

[0161] FIG. 24 shows the XRD pattern of the core and the XRD pattern of the core-shell of Example 3-2. That is, the XRD patterns are of the core portion contained in the core-shell upconversion microparticle (i.e., the upconversion micro precursor particle that serves as the central particle) and the core-shell upconversion microparticle. The horizontal axis of FIG. 24 is 2θ (degrees), and the vertical axis of FIG. 24 is intensity (arbitrary). FIG. 24(a) is the XRD pattern of the core portion contained in the core-shell upconversion microparticle of Example 3-2 (i.e., the upconversion microparticle of Example 3-2 that serves as the central particle), and FIG. 24(b) is the XRD pattern of the core-shell upconversion microparticle of Example 3-2. It was confirmed from FIG. 24 that the core-shell upconversion microparticle of Example 3-2 and its core portion were both in the β phase.

[0162] Fig. 25(a) is an SEM image of the core of the core-shell upconversion microparticle of Example 3-1, and Fig. 25(b) is an SEM image of the core-shell upconversion microparticle of Example 3-1. The particle size of the core-shell upconversion microparticle including the first coating layer estimated from the SEM images of Fig. 25(a) and Fig. 25(b) was 850 nm, and the thickness was 500 nm.

[0163] Figure 26(a) is an SEM image of the core of the core-shell upconversion microparticle of Example 3-2, and Figure 26(b) is an SEM image of the core-shell upconversion microparticle of Example 3-2. The particle size of the core-shell upconversion microparticle including the first coating layer estimated from the SEM images of Figure 26(a) and Figure 26(b) was 400 nm, and the thickness was 220 nm.

[0164] FIG. 27 shows the emission spectra of the core-shell upconversion microparticles of Examples 3-1 and 3-2. The horizontal axis of FIG. 27 represents wavelength, and the vertical axis represents intensity. In FIG. 27, the solid line represents the emission spectrum of the core-shell upconversion microparticles of Example 3-1 containing Nd in the shell portion. In FIG. 27, the dotted line represents the emission spectrum of the core-shell upconversion microparticles of Example 3-2 containing Nd in the core portion. Both Examples 3-1 and 3-2 were confirmed to emit ultraviolet light. Furthermore, the luminescence quantum efficiency of Example 3-1 was 0.06%, and the external quantum efficiency of Example 3-2 was 0.01%. It was confirmed that ultraviolet light emission with high quantum efficiency was possible by containing Nd and Tm and Yb in the core and shell portions. Furthermore, the luminescence quantum efficiency was higher when the shell portion contained Nd and the core portion contained Tm.

[0165]

[0166] 28 is an SEM image of Example 4. TiO estimated from the obtained SEM image of Example 4, etc. 2 The particle size of the coated core-shell upconversion microparticles was 860 nm, and the thickness was 520 nm. 2 The shell (excluding TiO 2 The (including layer) / core ratio was 0.365. 2 The thickness was 10 nm.

[0167] 29 is a graph showing the response speed of the photocurrent obtained by irradiating the photoelectric conversion element of Example 5 with light at a predetermined timing. The horizontal axis of the graph represents the elapsed time (s), and the vertical axis of the graph represents the photocurrent (mA / cm 2 The photocurrent shows instantaneous rise and fall in response to the on / off of the voltage, demonstrating that a sufficient response speed can be achieved.

[0168] Core-shell upconversion microparticles, upconversion microprecursor particles, sensitized core-shell upconversion microparticles, TiO 2 The coated core-shell upconversion microparticles, near-infrared detectors, photoelectric conversion elements, and methods for producing core-shell upconversion microparticles are highly industrially applicable because they are capable of upconversion emission even under low excitation light such as sunlight irradiation, and can achieve higher sensitization properties using weak light with long wavelengths.

[0169] 10 Core-shell upconversion microparticle, 11 Core portion, 12 Shell portion, 100 Photoelectric conversion element, 101 Positive electrode layer, 102 Negative electrode layer, 103 Photoelectric conversion layer, 104 First layer, 105 Second layer, 106 Third layer

Claims

1. An upconversion particle having a core portion and a shell portion covering the core portion, characterized in that the particle shape is a hexagonal column, the particle diameter is 300 nm or more, the thickness is 100 nm or more, and the aspect ratio (particle diameter / thickness) is 1.2 or more and 5.0 or less.

2. The core-shell type upconversion microparticle according to claim 1, characterized in that the particle diameter is 500 nm or more and the thickness is 300 nm or more.

3. The core-shell type upconversion microparticle according to claim 1, wherein the aspect ratio is 1.2 or more and 3.0 or less.

4. The core-shell type upconversion microparticle according to claim 1, wherein the aspect ratio is 1.5 or more and 2.0 or less.

5. A core-shell type upconversion microparticle according to claim 1, characterized in that the shell / core ratio, which is the width of the shell part of the upconversion particle divided by the diameter of the core part, is 0.01 or more and 10.00 or less.

6. The core-shell upconversion microparticle according to claim 5, wherein the shell / core ratio is 0.10 or more and 2.00 or less.

7. A core-shell upconversion microparticle as described in claim 1, characterized in that the crystal lattice as a host of the core portion and the crystal lattice as a host of the shell portion are made of the same component, the core portion contains doped rare earth atoms as guests, and the shell portion does not contain doped rare earth atoms.

8. The core-shell upconversion microparticle according to claim 7, characterized in that the shell portion does not cause energy transfer.

9. The core-shell type upconversion microparticle according to claim 7, characterized in that the core portion contains both light absorption sensitizing atoms and light emission activating atoms as the doped rare earth atoms.

10. The core-shell upconversion microparticle according to claim 9, characterized in that the light absorption sensitizing atom is a trivalent rare earth atom having an energy level of an f orbital, and absorbing near-infrared light, and an electron in the ground state is excited to the energy level of the f orbital, and the light emission activating atom is a trivalent rare earth atom having a plurality of energy levels, and undergoes multi-photon multi-step excitation by transferring energy at the energy level of the f orbital of the light absorption sensitizing atom after the excitation, so that electrons are excited to a high energy level corresponding to an energy level equal to or higher than the energy level of the f orbital by the multi-photon multi-step excitation, which is necessary for emitting light in the visible light region, and then, when the electrons excited to the high energy level return to the ground state, they emit light, thereby causing emission in the visible light region as light with an energy level equal to or higher than the energy level of the f orbital.

11. The crystal lattice is NaYF 4 The core-shell upconversion microparticle according to claim 9, characterized in that the light absorption sensitizing atom is one or more selected from the group consisting of Yb and Nd, and the light emission activating atom is one or more selected from the group consisting of Tm, Er, and Ho.

12. The core-shell upconversion microparticle according to claim 7, characterized in that the doped rare earth atoms include Nd.

13. The core-shell upconversion microparticle according to claim 7, wherein the doped rare earth atoms are one pair of either Nd and Yb atoms or Tm and Yb atoms.

14. A core-shell upconversion microparticle as described in claim 1, characterized in that the crystal lattice as a host of the core portion and the crystal lattice as a host of the shell portion are made of the same component, the core portion contains a first doped rare earth atom as a guest, and the shell portion contains a second doped rare earth atom as a guest that is different from the first doped rare earth atom of the core portion.

15. The core-shell upconversion microparticle according to claim 14, wherein the shell portion effects energy transfer.

16. The core-shell upconversion microparticle according to claim 14, characterized in that the first doped rare earth atoms or the second doped rare earth atoms include both light absorption sensitizing atoms and light emission activating atoms.

17. The core-shell upconversion microparticle of claim 16, characterized in that the light absorption sensitizing atoms are one or more selected from the group consisting of Yb and Nd, and the light emission activating atoms include one or more selected from the group consisting of Tm, Er, and Ho.

18. The core-shell upconversion microparticle of claim 14, wherein the first doped rare earth atom or the second doped rare earth atom comprises Nd.

19. The crystal lattice is NaYF 4 15. The core-shell upconversion microparticle according to claim 14, characterized in that the first doped rare earth atoms are one pair of either Nd and Yb atoms or Tm and Yb atoms, and the second doped rare earth atoms are one pair of either Nd and Yb atoms or Tm and Yb atoms, which is different from the first doped rare earth atoms.

20. The core-shell upconversion microparticle of claim 14, wherein a first energy level, which is an energy level of the first doped rare earth atom, is different from a second energy level, which is an energy level of the second doped rare earth atom, to effect an energy transfer from the first doped rare earth atom to the second doped rare earth atom.

21. The core-shell upconversion microparticle according to claim 20, characterized in that a third doped rare earth atom, which is a doped rare earth atom different from the first doped rare earth atom and the second doped rare earth atom, is further present as a guest in at least one of the core portion and the shell portion, and a third energy level, which is the energy level of the third doped rare earth atom, is located between the energy level of the first doped rare earth atom and the energy level of the second doped rare earth atom.

22. The core-shell upconversion microparticle of claim 21, characterized in that the second doped rare earth atom has a plurality of post-excitation energy levels at a position higher than a pre-excitation energy level at which the second doped rare earth atom has received energy transferred from the first doped rare earth atom or the third doped rare earth atom, and an energy gap between the pre-excitation energy level and one of the post-excitation energy levels is equal to the transferred energy.

23. A core-shell upconversion microparticle according to claim 1, characterized in that it comprises a doped rare earth atom, the doped rare earth atom being both a light absorption sensitizer atom and a light emission activator atom, the light absorption sensitizer atom being a trivalent rare earth atom having an energy level of an f orbital and absorbing near-infrared light, and an electron in a ground state being excited to the energy level of the f orbital, the light emission activator atom being a trivalent rare earth atom having a plurality of energy levels and undergoing multiphoton multistep excitation by the transfer of energy at the energy level of the f orbital of the light absorption sensitizer atom after the excitation, as a result of which electrons are excited to a high energy level corresponding to an energy level equal to or higher than the energy level of the f orbital by the multiphoton multistep excitation, which is necessary for emission in the visible light region, and then the electrons excited to the high energy level emit light when returning to the ground state, thereby causing emission in the visible light region as light with an energy level equal to or higher than the energy level of the f orbital.

24. The core-shell upconversion microparticle of claim 23, wherein the light absorption sensitizing atom is Yb, the light emission activating atom is Er, and the multiphoton multi-step excitation is two-photon two-step excitation.

25. The core-shell upconversion microparticle of claim 23, wherein the light absorption sensitizing atom is Yb, the light emission activating atom is Tm, and the multiphoton multistep excitation is a three-photon three-step excitation.

26. The core-shell upconversion microparticle of claim 23, wherein the light absorption sensitizing atom is Yb, the light emission activating atom is Tm, and the multiphoton multi-step excitation is two-photon two-step excitation.

27. The core-shell upconversion microparticle according to claim 23, characterized in that one of the light-absorbing sensitizing atoms is Nd and the other light-absorbing sensitizing atom is one or more selected from the group consisting of Er, Tm and Ho.

28. A sensitized core-shell upconversion microparticle comprising a core portion and a shell portion covering the core portion, the particle shape being a hexagonal column, the particle diameter being 500 nm or more, the thickness being 300 nm or more, the aspect ratio (particle diameter / thickness) being 1.2 or more and 3.0 or less, the core portion containing one pair of either Nd and Yb atoms or Tm and Yb atoms, and the shell portion containing a pair of Nd and Yb atoms or Tm and Yb atoms different from the pair contained in the core portion.

29. The sensitized core-shell upconversion microparticle of claim 28, wherein the core portion contains both Nd and Yb atoms, and the shell portion contains both Tm and Yb atoms.

30. The sensitized core-shell upconversion microparticle of claim 28, wherein the core portion contains both Tm and Yb atoms, and the shell portion contains both Nd and Yb atoms.

31. A transparent conductive film as a cathode and a TiO 2 1. A photoelectric conversion element comprising: a cathode layer, an electrolyte layer, a hole transport layer, and an Ag layer serving as an anode, laminated in this order.

32. The sensitized core-shell type upconversion microparticles according to claim 28 or the core-shell type upconversion microparticles according to claim 1, wherein the outermost layer is TiO 2 TiO 2 A TiO 2 Coated core-shell upconversion microparticles.

33. The TiO of claim 32. 2A near-infrared detector comprising a layer of coated core-shell type upconversion microparticles in a photoelectric conversion layer.

34. A TiO2-containing particle comprising either the sensitized core-shell type upconversion microparticles according to claim 28 or the core-shell type upconversion microparticles according to claim 1. 2 A near-infrared detector comprising a layer in a photoelectric conversion layer.

35. A transparent conductive film as a cathode and the TiO of claim 32. 2 A photoelectric conversion element comprising a layer of coated core-shell type upconversion microparticles, an electrolyte layer or a hole transport layer, and an Ag layer serving as an anode, laminated in this order.

36. A method for producing core-shell upconversion microparticles as described in claim 1, comprising: a first step of forming the core portion by crystal growth under conditions ranging from 50°C to 500°C using a sol-gel method; and a second step of growing crystals constituting the shell portion on the surface of the core portion by a sol-gel method under conditions ranging from 50°C to 500°C.

37. The method for producing core-shell upconversion microparticles according to claim 36, characterized in that the crystal growth in the first step is performed by a heating operation which involves the formation of cubic crystals and a phase transition from cubic to hexagonal crystals.

38. A method for producing core-shell upconversion microparticles as described in claim 37, characterized in that the heating operation in the first step is performed until the accumulated temperature as a heating condition for the phase transition exceeds the accumulated temperature as a heating condition for the formation of the cubic crystals.

39. The method for producing core-shell upconversion microparticles according to claim 37, characterized in that the heating operation in the first step is carried out while a degassing operation is performed to maintain a preset vacuum level.

40. The method for producing core-shell upconversion microparticles according to claim 36, characterized in that the crystal lattice constituting the core portion and the crystal lattice constituting the shell portion are of the same component.

41. An upconversion micro precursor particle, characterized in that the central particle capable of becoming the core portion contained in the core-shell type upconversion microparticle described in claim 1 has a particle shape of a hexagonal column, a particle diameter of 300 nm or more, a thickness of 100 nm or more, and an aspect ratio of the particle diameter / thickness of 1.2 or more and 5.0 or less.

42. The upconversion micro precursor particles according to claim 41, characterized in that they are crystal-grown by a sol-gel method under conditions ranging from 50°C to 500°C.

43. The upconversion micro precursor particle described in claim 42, characterized in that the long-chain organic molecule used as a gelling agent in the sol-gel method remains or adheres to the surface of the particle even after crystal growth by a heating operation.

Citation Information

Patent Citations

  • Organic-inorganic composite thin-film solar cell

    JP2015092563A

  • Wooden window structure

    JP2023058703A

  • Bioluminescent nanoparticle with 800-nanometer strong near infrared up-conversion emission characteristic and application thereof

    CN102618284A

  • Red light enhanced core-shell upconversion luminescent nano-carrier and preparation method therefor

    CN105385448A

  • Up-conversion nanometer material with greatly enhanced red light and preparation method thereof

    CN111139063A