Decorative sheet and decorative board

The decorative sheet with a cross-linked curable resin surface protective layer addresses adhesion, hardness, and processability issues, offering enhanced performance for decorative and protective applications.

WO2024202869A1PCT designated stage expired Publication Date: 2024-10-03DAI NIPPON PRINTING CO LTD

Patent Information

Application Number
PCT/JP2024/007302
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-24
Filing Date
2024-02-28
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Decorative sheets used for surface protection and decoration lack sufficient adhesion to underlying layers, surface hardness, scratch resistance, and processability, particularly when attached to wooden or plastic boards, and existing hard coat films do not adequately address these requirements.

Method used

A decorative sheet with a surface protective layer containing a cross-linked curable resin, characterized by specific peak height ratios in infrared spectroscopy measurements, which enhances adhesion, surface hardness, and processability, and may include ionizing radiation-curable resins, antibacterial agents, and biomass-derived components.

Benefits of technology

The decorative sheet achieves excellent adhesion to underlying layers, superior surface hardness and scratch resistance, and improved processability, making it suitable for various applications in building materials and furniture.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024007302_03102024_PF_FP_ABST
    Figure JP2024007302_03102024_PF_FP_ABST
Patent Text Reader

Abstract

The present invention provides a decorative sheet in which a surface protective layer exhibits excellent adhesion to a lower layer and which exhibits excellent surface hardness, scratch resistance, and processability. The present invention provides a decorative sheet comprising at least a surface protective layer, said decorative sheet being characterized in that: the surface protective layer contains a crosslinkable and curable resin; in an infrared spectroscopic measurement of the surface protective layer, when the height of a peak appearing at 855-1325 cm-1 is regarded as A and the height of a peak appearing at 1650-1800 cm-1 is regarded as B, the peak height ratio between A and B ((A / B)×100 (%)) is 105-400%; and, in the infrared spectroscopic measurement of the surface protective layer, when the height of a peak appearing at 3200-3500 cm-1 is regarded as C, the peak height ratio between B and C ((B / C)×100 (%)) is 1000-6000%.
Need to check novelty before this filing date? Find Prior Art

Description

Decorative sheets and decorative panels

[0001] The present invention relates to a decorative sheet and a decorative board.

[0002] Decorative sheets are used by being attached to the surface of wood boards, plastic boards, etc. for the purpose of surface protection, decoration, etc. The decorative boards obtained in this way are used in a variety of applications such as decorative items, building materials, furniture, etc.

[0003] Decorative sheets used in the above applications are required to have a surface protective layer that exhibits adhesion to the underlying layer. In particular, a film with a small number of polar groups may be used on the surface of the underlying layer, and the surface protective layer of the decorative sheet is required to exhibit adhesion to such a film.

[0004] As a decorative sheet having a surface protective layer that exhibits adhesion to a film, a hard-coated film in which a hard-coat layer is provided on at least one surface of a substrate film has been proposed (see Patent Document 1).

[0005] However, the hard coat film provided with the hard coat layer of Patent Document 1 does not have sufficient adhesion between the substrate film and the hard coat film when used in various applications, and there is room for improvement.

[0006] Furthermore, since decorative sheets are used by being attached to the surface of wood boards, plastic boards, etc., they are subject to being hit by objects, and therefore the surface of the decorative sheet is required to have surface hardness and scratch resistance.

[0007] Furthermore, since decorative sheets are used by being attached to the surface of an article for decorative purposes, they need to conform to the shape of the article. Therefore, decorative sheets are required to have processability that allows them to be processed to conform to the shape of the article. The hard coat film described in Patent Document 1 has a problem in that processability is not considered, and therefore it has poor processability.

[0008] Therefore, there is a need for the development of a decorative sheet that has excellent adhesion to the underlying layer, excellent surface hardness and scratch resistance, and excellent processability.

[0009] Japanese Patent Application Laid-Open No. 2017-177667

[0010] An object of the present invention is to provide a decorative sheet in which the surface protective layer has excellent adhesion to the underlying layer, excellent surface hardness and scratch resistance, and excellent processability.

[0011] As a result of extensive research, the present inventors have discovered a decorative sheet having at least a surface protective layer, wherein the surface protective layer contains a cross-linked curable resin, and in infrared spectroscopy measurement of the surface protective layer, the wavelength range of the cross-linked curable resin is 855 to 1325 cm -1 The height of the peak appearing at 1650 to 1800 cm is defined as A. -1 The peak height ratio ((A / B)×100(%)) of A to B, where B is the height of the peak appearing in the -1 The present inventors have found that the above object can be achieved by a decorative sheet in which the peak height ratio of B to C ((B / C) x 100(%)) is 1000% or more and 6000% or less, where C is the height of the peak appearing in the graph.

[0012] That is, the present invention relates to the following decorative sheet and decorative board: 1. A decorative sheet having at least a surface protective layer, wherein the surface protective layer contains a cross-linked curable resin, and wherein infrared spectroscopy of the surface protective layer shows a wavelength range of 855 to 1325 cm -1 The height of the peak appearing at 1650 to 1800 cm is defined as A. -1 the peak height ratio of A to B ((A / B)×100(%)) is 105% or more and 400% or less, where B is the height of the peak appearing in the -11. A decorative sheet characterized in that, when the height of the peak appearing in (A) is defined as C, the peak height ratio of B to C ((B / C) x 100(%)) is 1000% or more and 6000% or less. 2. The decorative sheet according to item 1, wherein the peak height ratio of A to B is 110% or more and 300% or less, and the peak height ratio of B to C is 1300% or more and 5500% or less. 3. The decorative sheet according to item 1 or 2, wherein the cross-linking curable resin comprises an ionizing radiation curable resin. 4. The decorative sheet according to item 3, wherein the ionizing radiation curable resin comprises an acrylic resin having a (meth)acryloyl group. 5. The decorative sheet according to any one of items 1 to 4, wherein the surface protective layer comprises at least one agent selected from the group consisting of an antibacterial agent, an antiviral agent, and an antiallergen agent. 6. The decorative sheet according to any one of items 1 to 5, comprising a picture pattern layer, a transparent resin layer, and the surface protective layer on a base sheet, in this order. 7. Item 6. The decorative sheet according to Item 6, wherein at least one layer selected from the group consisting of the base sheet and the transparent resin layer contains a flame retardant. 8. The decorative sheet according to Item 6 or 7, wherein at least one layer selected from the group consisting of the base sheet, the picture pattern layer, the transparent resin layer, and the surface protective layer contains a biomass-derived component. 9. A decorative board having the decorative sheet according to any one of Items 1 to 8 on a substrate.

[0013] The decorative sheet of the present invention has a surface protective layer that has excellent adhesion to the underlying layer, excellent surface hardness and scratch resistance, and excellent processability. Therefore, a decorative board laminated with the decorative sheet of the present invention can be used for various building materials, furniture, etc.

[0014] FIG. 1 is a diagram showing an example of the results of infrared spectroscopy measurement of the surface protective layer of the decorative sheet of the present invention. FIG. 2 is a diagram explaining a method for determining peak heights in infrared spectroscopy measurement of the surface protective layer of the decorative sheet of the present invention. FIG. 3 is a diagram explaining a method for determining peak heights in infrared spectroscopy measurement of the surface protective layer of the decorative sheet of the present invention. FIG. 4 is a diagram showing an example of the layer structure of the decorative sheet of the present invention. FIG. 5 is a diagram showing an example of the layer structure of the decorative board of the present invention. FIG. 6 is a diagram showing an example of hydrogen bonding between molecules of a cross-linked curable resin. FIG. 7 is a schematic diagram showing a method for testing fire spread resistance. FIG. 8 is a schematic diagram showing a method for testing fire spread resistance.

[0015] 1. Decorative Sheet The decorative sheet of the present invention is a decorative sheet having at least a surface protective layer, said surface protective layer containing a cross-linked curable resin, and in infrared spectroscopy measurement of said surface protective layer, -1 The height of the peak appearing at 1650 to 1800 cm is defined as A. -1 The peak height ratio ((A / B)×100(%)) of A to B, where B is the height of the peak appearing in the -1 The decorative sheet is characterized in that the peak height ratio of B to C ((B / C) x 100(%)) is 1000% or more and 6000% or less, where C is the height of the peak appearing in the decorative sheet. Because the decorative sheet of the present invention has the above characteristics, the surface protective layer of the decorative sheet has excellent adhesion to the underlying layer, excellent surface hardness and scratch resistance, and excellent processability. Therefore, decorative boards laminated with the decorative sheet of the present invention can be used for a variety of applications, such as various building materials and furniture.

[0016] As described above, the decorative sheet of the present invention has a wavelength of 855 to 1325 cm in infrared spectroscopy measurement of the surface protective layer. -1 The height of the peak appearing at 1650 to 1800 cm is defined as A. -1 The peak height ratio ((A / B)×100(%)) of A to B, where B is the height of the peak appearing in the -1 When the height of the peak appearing in the graph is defined as C, the peak height ratio between B and C ((B / C)×100(%)) is 1000% or more and 6000% or less. This will be explained below with reference to the drawings.

[0017] 1 is a diagram showing an example of the results of infrared spectroscopy (hereinafter also referred to as "IR") measurement of the surface protective layer of the decorative sheet of the present invention. In FIG. 1, A indicates a peak due to an ether bond, B indicates a peak due to an ester bond, and C indicates a peak due to a urethane bond.

[0018] In this specification, the height of each peak is measured as follows. That is, as shown in Figure 2, two base points b1 and b2 of each peak are taken, and a baseline bL is drawn by connecting the base points with a straight line. Next, a vertical line is drawn downward from the peak top position p, and the intersection point bp with the baseline bL is designated. The length h between p and bp is defined as the height of the peak.

[0019] Furthermore, when peak A exhibits multiple peaks, as shown in FIG. 3, the peak heights are measured as follows. That is, when two adjacent peaks exist as shown in FIG. 3, if the heights h1-1 and h2-1 from the valley between the two peaks to the peak apex are 0.10 Abs or more, the two peak heights h1 and h2 are summed to determine the peak height. Note that in FIG. 3, a peak whose peak top is p2 has adjacent peaks on both sides, and there are two heights from the valley between the two peaks to the peak apex, h2-1 and h2-2. In this case, the shorter height h2-1 is used to determine whether or not the height is 0.10 Abs or more.

[0020] In this specification, the infrared spectroscopy of the surface protective layer can be measured using a commercially available infrared spectroscopy measuring device.

[0021] The decorative sheet of the present invention has a surface protective layer having a wavelength of 855 to 1325 cm in infrared spectroscopy measurement. -1 The height of the peak appearing at 1650 to 1800 cm is defined as A. -1 When the height of the peak appearing in is defined as B, the peak height ratio of A to B ((A / B) x 100(%)) is 105% or more and 400% or less. If the peak height ratio of A to B is less than 105%, the surface protective layer contains too many ester bonds, making the surface protective layer too hard and reducing the processability of the decorative sheet. If the peak height ratio of A to B exceeds 400%, the surface protective layer contains too many ether bonds, making the surface protective layer too soft and reducing the surface hardness and scratch resistance of the decorative sheet. The peak height ratio of A to B is preferably 110% or more and 300% or less, and more preferably 150% or more and 250% or less.

[0022] The decorative sheet of the present invention has a surface protective layer having a wavelength of 3200 to 3500 cm in infrared spectroscopy measurement. -1 When the height of the peak appearing in the graph is defined as C, the peak height ratio of B to C ((B / C) x 100(%)) is 1000% or more and 6000% or less. If the peak height ratio of B to C is less than 1000%, the surface protective layer contains too many urethane bonds, and the hydrogen bonds between the -N-H groups and the -C=O groups in the urethane bonds as shown in Figure 6 increase excessively, making the surface protective layer too hard and reducing the processability of the decorative sheet. If the peak height ratio of B to C exceeds 6000%, the surface protective layer contains too few urethane bonds, making the surface protective layer too soft and reducing the surface hardness and scratch resistance of the decorative sheet. The peak height ratio of B to C is preferably 1300% or more and 5500% or less, and more preferably 1500% or more and 5200% or less.

[0023] An example of a method for adjusting the peak height ratio between A and B and the peak height ratio between B and C within the above ranges is to change the formulation of the cross-linking curable resin used to form the surface protective layer. When the cross-linking curable resin contains a large amount of ether bonds and a small amount of ester bonds, the peak height ratio between A and B becomes large. Conversely, when the cross-linking curable resin contains a small amount of ether bonds and a large amount of ester bonds, the peak height ratio between A and B becomes small. Furthermore, when the cross-linking curable resin contains a large amount of ester bonds and a small amount of urethane bonds, the peak height ratio between B and C becomes large. Conversely, when the cross-linking curable resin contains a small amount of ester bonds and a large amount of urethane bonds, the peak height ratio between B and C becomes small.

[0024] Each layer of the decorative sheet of the present invention will be described in detail below. In the decorative sheet of the present invention, the surface is the so-called "front side," which is the side opposite to the side that comes into contact with the substrate when the decorative sheet of the present invention is laminated to a substrate or the like, and is the side that is visible after lamination. In this specification, the direction of the surface of the decorative sheet of the present invention will sometimes be referred to as the "front" or "top," and the opposite side as the "back" or "bottom." In the following description, the lower and upper limits of numerical ranges expressed by "to" mean "greater than or equal to" (for example, if α to β, it means greater than or equal to α and less than or equal to β).

[0025] The layer thickness in this specification is a value measured at a location on the decorative sheet where there are no irregularities such as embossments or protruding fine particle heads.

[0026] (Layer structure of the decorative sheet of the present invention) The decorative sheet of the present invention is sufficient as long as it has at least a surface protective layer, and it is preferable that the surface protective layer be the above-mentioned surface protective layer on the outermost surface of the decorative sheet. The specific structure may be appropriately set depending on the application of the decorative sheet, etc. For example, as shown in Figure 4, a layer structure having, in order, a base sheet 11, a picture pattern layer 12 (solid ink layer and / or patterned ink layer), an adhesive layer (not shown), a transparent resin layer 13, and a surface protective layer 14 is exemplified. A decorative sheet having such a layer structure will be specifically described below as a representative example.

[0027] (Surface Protective Layer) The decorative sheet of the present invention has at least a surface protective layer. In this specification, the surface protective layer contains a cross-linked curable resin.

[0028] Examples of cross-linking curable resins include thermosetting resins, ionizing radiation curable resins (e.g., electron beam curable resins), etc. In particular, from the viewpoints of scratch resistance due to high surface hardness, convex shape retention, productivity, etc., it is preferable that the surface protective layer contains an ionizing radiation curable resin, and it is more preferable that the resin constituting the surface protective layer is an ionizing radiation curable resin.

[0029] Examples of thermosetting resins include unsaturated polyester resins, polyurethane resins (including two-component curing polyurethanes), epoxy resins, aminoalkyd resins, phenolic resins, urea resins, diallyl phthalate resins, melamine resins, guanamine resins, melamine-urea co-condensation resins, silicon resins, and polysiloxane resins.

[0030] The resin may contain a crosslinking agent, a curing agent such as a polymerization initiator, a polymerization accelerator, etc. For example, curing agents such as isocyanate and organic sulfonate may be added to unsaturated polyester resins and polyurethane resins, organic amines may be added to epoxy resins, and peroxides such as methyl ethyl ketone peroxide and radical initiators such as azoisobutylnitrile may be added to unsaturated polyester resins.

[0031] The surface protection layer can be formed from a thermosetting resin by, for example, applying a solution of the thermosetting resin by a coating method such as roll coating or gravure coating, followed by drying and curing.

[0032] The ionizing radiation curable resin is not limited as long as it undergoes a crosslinking polymerization reaction upon irradiation with ionizing radiation and changes into a three-dimensional polymer structure. For example, one or more prepolymers, oligomers, and monomers having a polymerizable unsaturated bond or an epoxy group in the molecule that can be crosslinked upon irradiation with ionizing radiation can be used. Examples include acrylate resins such as urethane acrylate, polyester acrylate, and epoxy acrylate; silicon resins such as siloxane; polyester resins; and epoxy resins.

[0033] The ionizing radiation curable resin preferably contains an acrylic resin having a (meth)acryloyl group. By including an acrylic resin having a (meth)acryloyl group as the ionizing radiation curable resin, hydrogen bonds are formed between the molecules of the ionizing radiation curable resin, thereby further improving the surface hardness and scratch resistance of the surface protective layer.

[0034] Ionizing radiation includes visible light, ultraviolet light (near ultraviolet light, vacuum ultraviolet light, etc.), X-rays, electron beams, ion beams, etc., and among these, ultraviolet light and / or electron beams are preferred.

[0035] The ultraviolet light source may be an ultra-high pressure mercury lamp, a high pressure mercury lamp, a low pressure mercury lamp, a carbon arc lamp, a black light fluorescent lamp, or a metal halide lamp. The wavelength of the ultraviolet light is about 190 to 380 nm.

[0036] As the electron beam source, various electron beam accelerators can be used, such as Cockcroft-Waldt type, Van de Graaf type, resonant transformer type, insulating core transformer type, linear type, dynamitron type, and high frequency type. The energy of the electron beam is preferably about 100 to 1000 keV, more preferably about 100 to 300 keV. The dose of the electron beam is preferably about 2 to 15 Mrad.

[0037] Ionizing radiation curable resins are sufficiently cured by irradiation with electron beams, but when curing is performed by irradiation with ultraviolet rays, it is preferable to add a photopolymerization initiator (sensitizer).

[0038] In the case of a resin system having a radically polymerizable unsaturated group, the photopolymerization initiator may be, for example, at least one of acetophenones, benzophenones, thioxanthones, benzoin, benzoin methyl ether, Michler's benzoyl benzoate, Michler's ketone, diphenyl sulfide, dibenzyl disulfide, diethyl oxide, triphenylbiimidazole, isopropyl-N,N-dimethylaminobenzoate, etc. In the case of a resin system having a cationically polymerizable functional group, the photopolymerization initiator may be, for example, at least one of aromatic diazonium salts, aromatic sulfonium salts, metallocene compounds, benzoin sulfonate esters, furyloxysulfoxonium diallyliodosyl salts, etc.

[0039] The amount of the photopolymerization initiator added is not particularly limited, but is generally about 0.1 to 10 parts by mass per 100 parts by mass of the ionizing radiation curable resin.

[0040] Furthermore, in recent years, the use of biomass-derived resins, which have a low environmental impact, has been studied in many areas, and the resin forming the surface protective layer of the decorative sheet of the present invention can also contain components derived from biomass; specifically, biomass polyolefins and the like can be used.

[0041] The surface protective layer may be a single layer or may be a multi-layer structure of two or more layers. In the present invention, when the surface protective layer is a multi-layer structure, each layer contains a cross-linked curable resin. When the surface protective layer is a multi-layer structure, the infrared spectroscopy of the surface protective layer is measured by measuring the infrared spectroscopy of the laminated surface protective layers from the outermost surface protective layer side.

[0042] The thickness of the surface protective layer is not particularly limited as long as it does not impede the effects of the present invention, but is preferably 1 to 200 μm, more preferably 1 to 100 μm, even more preferably 3 to 50 μm, and particularly preferably 4 to 40 μm.

[0043] The surface protective layer may contain fine particles. Examples of the fine particles include inorganic fillers such as silica, aluminum oxide, silicon carbide, silicon dioxide, calcium titanate, barium titanate, magnesium pyroborate, zinc oxide, silicon nitride, zirconium oxide, chromium oxide, iron oxide, boron nitride, diamond, emery, and glass fiber; and organic material powders or beads such as acrylic, crosslinked alkyl, crosslinked styrene, benzoguanamine resin, urea-formaldehyde resin, phenolic resin, polyethylene, and nylon. One or more types of the fine particles can be used.

[0044] The average particle size of the fine particles is preferably equal to or greater than the thickness of the surface protective layer, and in order to exhibit scratch resistance, it is preferably less than "the thickness of the surface protective layer + 40 μm", and more preferably equal to or less than "the thickness of the surface protective layer + 30 μm".

[0045] The average particle size of the fine particles can be measured by known methods such as laser diffraction, Coulter counter method, sedimentation method, etc. The average particle size means the mode diameter.

[0046] The content of the fine particles in the surface protective layer is preferably 3 to 50 parts by mass, and more preferably 5 to 30 parts by mass, based on 100 parts by mass of the resin component that forms the surface protective layer.

[0047] Silicone may be added to the surface protective layer. When silicone is added to the surface protective layer, the amount of silicone added is preferably 0.1 to 1 part by mass, and more preferably 0.1 to 0.5 parts by mass, per 100 parts by mass of the resin (resin component) constituting the surface protective layer, from the viewpoint of achieving both ease of wiping and non-slip properties.

[0048] The surface protective layer may contain various additives, such as a solvent, a colorant such as a dye or a pigment, a filler such as an inorganic filler, an antifoaming agent, a leveling agent, a thixotropy-imparting agent, a flame retardant, an antibacterial agent, an antiviral agent, or an antiallergen, as needed.

[0049] The inorganic filler can be used as a means for imparting predetermined surface properties to the surface protective layer by incorporating an inorganic filler having a thickness greater than that of the surface protective layer. The inorganic filler can also be used as a matting agent, and incorporating the inorganic filler in the surface protective layer is expected to have the effect of suppressing the cure shrinkage of the surface protective layer. Therefore, in the present invention, it is preferable that the inorganic filler has been surface-treated (hydrophobized). Furthermore, among these additives, it is preferable that at least one selected from the group consisting of antibacterial agents, antiviral agents, and antiallergen agents be incorporated into the surface protective layer, which is the outermost layer, in order to facilitate the attainment of the desired effect.

[0050] Examples of inorganic fillers include silica, aluminum oxide, silicon carbide, silicon dioxide, calcium titanate, barium titanate, magnesium pyroborate, zinc oxide, silicon nitride, zirconium oxide, chromium oxide, iron oxide, boron nitride, diamond, emery sand, and glass fiber.

[0051] The method of surface treatment (hydrophobic treatment) of inorganic filler is not particularly limited, and can be carried out by known method.For example, the method of hydrophobic treatment of inorganic filler by silicone oil-based treatment agent; the method of hydrophobic treatment of inorganic filler by alkylsilazane-based treatment agent, trimethylsilylating agent and / or alkoxysilane after treating inorganic filler by above-mentioned silicone oil-based treatment agent; the method of hydrophobic treatment of inorganic filler by silicone oil-based treatment agent, and then further treatment by trimethylsilylating agent or alkylsilazane-based treatment agent; the method of hydrophobic treatment of inorganic filler by alkoxysilane; the method of treating inorganic filler by alkoxysilane, and then further treatment by silicone oil-based treatment agent, or silicone oil-based treatment agent and alkoxysilane; the method of treating inorganic filler by dimer diol siloxane and / or trimethylsilanol or cyclic siloxane. In addition to the above-mentioned hydrophobic treatment methods, other examples of hydrophobic treatment methods include treatment with various coupling agents such as silane coupling agents, titanate coupling agents, and aluminate coupling agents; surfactants such as phosphoric acid and fatty acid surfactants; oils and fats, stearic acid, etc. Hereinafter, the above-mentioned products for hydrophobizing untreated inorganic fillers (for example, all of the treatment agents such as silicone oil treatment agents, silane coupling agents, surfactants, etc.) are collectively referred to as hydrophobic treatment agents.

[0052] The method for hydrophobizing an inorganic filler with a hydrophobic treatment agent is not particularly limited and can be carried out by a known method. For example, a method (dry treatment method) in which a stock solution of the hydrophobic treatment agent or a hydrophobic treatment agent diluted in water or an organic solvent is added (e.g., sprayed) to an untreated inorganic filler; a method (wet treatment method) in which an untreated inorganic filler is treated (e.g., immersed) in a stock solution of the hydrophobic treatment agent, an aqueous solution containing the hydrophobic treatment agent, or an organic solvent containing the hydrophobic treatment agent, and then dried; etc. are mentioned. By such treatment, a part or all of the surface of the inorganic filler is (a) coated with the hydrophobic treatment agent, (b) adsorbs the hydrophobic treatment agent, or (c) is coated with and adsorbs the hydrophobic treatment agent (a combination of (a) and (b)), etc. As a result, a hydrophobized inorganic filler is obtained. The hydrophobic treatment agent may be used alone or in combination of two or more types.

[0053] The antibacterial agent includes inorganic antibacterial agents and organic antibacterial agents. In particular, inorganic antibacterial agents are desirable because they are generally safer than organic antibacterial agents and have excellent durability and heat resistance. Inorganic antibacterial agents are antibacterial metals such as silver, copper, and zinc supported on various inorganic carriers. When contained in the surface protective layer, the amount of antibacterial agent added is preferably 0.1 to 10 parts by mass per 100 parts by mass of the resin component of the surface protective layer, but the details can be adjusted appropriately depending on the type of antibacterial agent.

[0054] The antiviral agents can generally be broadly divided into organic and inorganic types. Organic antiviral agents include quaternary ammonium salts, quaternary phosphonium salts, pyridines, pyrithiones, benzimidazoles, organic iodines, isothiazolinones, anions, and ethers. Inorganic antiviral agents include those in which metal ions such as silver, copper, and zinc are supported on a carrier such as zeolite, apatite, zirconia, glass, or molybdenum oxide. When contained in the surface protective layer, the amount of the antiviral agent added is preferably 0.1 to 10 parts by mass per 100 parts by mass of the resin component of the surface protective layer, but the details can be adjusted appropriately depending on the type of antiviral agent.

[0055] Among the organic antiviral agents, benzimidazole-based antiviral agents, anionic-based antiviral agents, or ether-based antiviral agents that maintain a particle shape are particularly preferred. "Maintaining a particle shape" here means that the agent exists in a particle state without dissolving in the composition (ink before curing) that becomes the curable resin of the surface protective layer. Therefore, during the process of forming the surface protective layer, particles of imidazole-based compounds, particles of anionic compounds, or particles of ether-based compounds tend to float up, making it easier to unevenly distribute the particles of imidazole-based compounds, anionic compounds, or particles of ether-based compounds on the outermost surface side of the surface protective layer. Furthermore, unevenly distributing the particles of imidazole-based compounds, particles of anionic compounds, or particles of ether-based compounds on the outermost surface side of the surface protective layer can reduce the amount of antiviral agent added necessary to achieve a predetermined antiviral property, thereby making it easier to prevent a decrease in the scratch resistance of the surface protective layer.

[0056] The anionic antiviral agent preferably contains, for example, a styrene resin, a styrene polymer derivative compound, and an unsaturated carboxylic acid derivative compound. Furthermore, the styrene polymer derivative compound and the unsaturated carboxylic acid derivative compound preferably contain at least one structure selected from the groups consisting of styrene, sodium sulfonate, acrylic acid, maleic acid, and fumaric acid, and more preferably contain all of these structures. This is because viruses are broadly classified into two types, those with and without envelopes, and it is believed that the structures of antiviral agents that can effectively inhibit the activity of each type differ. Therefore, for example, if effectiveness against only influenza viruses, which are non-enveloped viruses, is desired, it is sufficient to contain only a styrene polymer derivative compound, and in some cases, sufficient effectiveness can be obtained by containing only a simple styrene resin.

[0057] As the inorganic antiviral agent, a silver-based antiviral agent is preferable from the viewpoint of being non-toxic to living organisms and excellent in safety, and among these, a phosphate glass-supported silver compound or a silver zeolite compound, and a molybdenum oxide-silver double salt compound are more preferable because they exhibit antiviral activity even in small amounts and therefore the amount added can be reduced.

[0058] When the silver-based antiviral agent is contained in the surface protective layer, discoloration may occur depending on the surface protective layer (the discoloration may occur due to heat or light in the paint state to which the agent is added, or may occur due to heat or light after the surface protective layer is formed), but in this case, it is possible to improve the situation by appropriately adding an ultraviolet inhibitor, a light stabilizer, etc. For example, the use of a benzotriazole-based compound for the molybdenum oxide silver double salt compound can be expected to have an effect of improving discoloration.

[0059] The antiallergen agent contains either an inorganic compound or an organic compound, and may be used alone or in combination of two or more different compounds. The inorganic compound is preferably a metal-supported material. When contained in the surface protective layer, the amount of the antiallergen agent added is preferably 0.1 to 10 parts by mass per 100 parts by mass of the resin component of the surface protective layer, but the details can be adjusted appropriately depending on the type of antiallergen agent.

[0060] Examples of methods for forming a surface protective layer containing an ionizing radiation curable resin include a method in which a solution (resin composition for forming a surface protective layer) containing (1) a resin such as an ionizing radiation curable resin, and (2) as necessary, other resins, fine particles, an ultraviolet absorber, an antibacterial agent, the various additives described above, etc. is applied by a coating method such as gravure coating or roll coating, and then the ionizing radiation curable resin is cured to form the surface protective layer.

[0061] (Base Sheet) The base sheet is a layer on whose surface (front surface) a picture pattern layer and the like are sequentially laminated.

[0062] Suitable substrate sheets include, for example, sheets (films) made of thermoplastic resins. Specific examples include olefin-based resins such as polyethylene, ethylene-α-olefin copolymers, polypropylene, polymethylpentene, polybutene, ethylene-propylene copolymers, propylene-butene copolymers, ethylene-vinyl acetate copolymers, saponified ethylene-vinyl acetate copolymers, ethylene-(meth)acrylic acid copolymers, and ethylene-(meth)acrylic acid ester copolymers; polyvinyl chloride, polyethylene terephthalate, polybutylene terephthalate, polyamides, polycarbonates, polyethylene naphthalate, ionomers, acrylic acid ester polymers, and methacrylic acid ester polymers. In recent years, the use of biomass-derived resins, which have a low environmental impact, has been widely investigated. The resin forming the substrate sheet of the decorative sheet of the present invention can also contain biomass-derived components; specifically, biomass polyolefins can be used. The substrate sheet can be formed using these resins alone or in combination of two or more.

[0063] In this specification, "(meth)acrylic acid" means acrylic acid and / or methacrylic acid, and the same applies to other moieties written as (meth).

[0064] The substrate sheet may be colored. In this case, a colorant (pigment or dye) can be added to the thermoplastic resin as described above to color it. Examples of colorants that can be used include inorganic pigments such as titanium dioxide, carbon black, and iron oxide, organic pigments such as phthalocyanine blue, and various dyes. One or more of these can be selected from known or commercially available colorants. The amount of colorant added can also be appropriately determined depending on the desired color tone, etc.

[0065] The substrate sheet may contain various additives such as fillers, matting agents, foaming agents, flame retardants, lubricants, antistatic agents, antioxidants, ultraviolet absorbers, and light stabilizers, as required.

[0066] In the substrate sheet, the above ultraviolet absorbers, light stabilizers, and flame retardants can be the same as those used in the transparent resin layer described below, and can be added in the same amounts.

[0067] The thickness of the substrate sheet can be appropriately set depending on the application and method of use of the final product, but is generally preferably 20 to 300 μm.

[0068] If necessary, the surface (front surface) of the substrate sheet may be subjected to a corona discharge treatment in order to improve the adhesion of the ink that forms the picture pattern layer. The corona discharge treatment may be carried out by a known method and under known conditions. If necessary, the back surface of the substrate sheet may be subjected to a corona discharge treatment or a back surface primer layer may be formed.

[0069] (Picture / Design Layer) The decorative sheet of the present invention may have a picture / design layer.

[0070] The picture pattern layer imparts a desired pattern (design) to the decorative sheet, and the type of pattern is not limited, and examples include wood grain patterns, leather patterns, stone grain patterns, sand grain patterns, tile patterns, brickwork patterns, fabric patterns, geometric shapes, letters, symbols, and abstract patterns.

[0071] The method for forming the picture pattern layer is not particularly limited, and for example, the picture pattern layer may be formed on the surface of the substrate sheet by a printing method using an ink obtained by dissolving (or dispersing) a known colorant (dye or pigment) together with a binder resin in a solvent (or dispersion medium). From the viewpoint of reducing VOCs in the decorative sheet, an aqueous composition can also be used as the ink.

[0072] Examples of colorants include inorganic pigments such as carbon black, titanium white, zinc white, red iron oxide, iron blue, and cadmium red; organic pigments such as azo pigments, lake pigments, anthraquinone pigments, quinacridone pigments, phthalocyanine pigments, isoindolinone pigments, and dioxazine pigments; metal powder pigments such as aluminum powder and bronze powder; pearlescent pigments such as titanium oxide-coated mica and bismuth oxide chloride; fluorescent pigments; and luminous pigments. These colorants can be used alone or in combination. These colorants may be used together with fillers such as silica, extender pigments such as organic beads, neutralizers, surfactants, and the like.

[0073] As binder resins, in addition to hydrophilically treated polyester-based urethane resins, polyesters, polyacrylates, polyvinyl acetates, polybutadiene, polyvinyl chloride, chlorinated polypropylenes, polyethylene, polystyrene, polystyrene-acrylate copolymers, rosin derivatives, alcohol adducts of styrene-maleic anhydride copolymers, cellulose-based resins, etc. can also be used. More specifically, for example, polyacrylamide-based resins, poly(meth)acrylic acid-based resins, polyethylene oxide-based resins, poly(N-vinylpyrrolidone)-based resins, water-soluble polyester-based resins, water-soluble polyamide-based resins, water-soluble amino-based resins, water-soluble phenol-based resins, other water-soluble synthetic resins, water-soluble natural polymers such as polynucleotides, polypeptides, and polysaccharides, etc., can also be used. Furthermore, for example, modified natural rubber, synthetic rubber, polyvinyl acetate-based resins, (meth)acrylic resins, polyvinyl chloride-based resins, polyurethane-polyacrylic resins, etc., mixtures of the above natural rubbers, and other resins can also be used. The above binder resins can be used alone or in combination of two or more.

[0074] Examples of the solvent (or dispersion medium) include petroleum-based organic solvents such as hexane, heptane, octane, toluene, xylene, ethylbenzene, cyclohexane, and methylcyclohexane; ester-based organic solvents such as ethyl acetate, butyl acetate, 2-methoxyethyl acetate, and 2-ethoxyethyl acetate; alcohol-based organic solvents such as methyl alcohol, ethyl alcohol, normal propyl alcohol, isopropyl alcohol, isobutyl alcohol, ethylene glycol, and propylene glycol; ketone-based organic solvents such as acetone, methyl ethyl ketone, methyl isobutyl ketone, and cyclohexanone; ether-based organic solvents such as diethyl ether, dioxane, and tetrahydrofuran; chlorine-based organic solvents such as dichloromethane, carbon tetrachloride, trichloroethylene, and tetrachloroethylene; and inorganic solvents such as water. These solvents (or dispersion media) can be used alone or in combination of two or more.

[0075] Furthermore, in recent years, the use of biomass-derived resins, which have a small environmental impact, has been studied in many fields, and the binder resin that forms the picture pattern layer of the decorative sheet of the present invention can also contain a biomass-derived component. For example, a biomass-derived urethane (meth)acrylate or the like can be used, and specific examples include binder resins that contain a urethane (meth)acrylate containing at least a polyol, an isocyanate compound, and a hydroxy (meth) acrylate, and at least one selected from the group consisting of the polyol, the isocyanate compound, and the hydroxy (meth) acrylate contains a biomass-derived component.

[0076] Examples of printing methods used to form the picture pattern layer include gravure printing, offset printing, screen printing, flexographic printing, electrostatic printing, and inkjet printing. When forming a solid picture pattern layer over the entire surface, examples of coating methods include roll coating, knife coating, air knife coating, die coating, lip coating, comma coating, kiss coating, flow coating, and dip coating. Other methods that may be used include hand-drawing, ink-flowing, photography, transfer printing, laser beam writing, electron beam writing, partial vapor deposition of metals or the like, and etching, or may be used in combination with other forming methods.

[0077] The thickness of the picture pattern layer is not particularly limited and can be set appropriately depending on the product characteristics, but the layer thickness is about 0.1 to 10 μm.

[0078] (Colored Concealing Layer) In the decorative sheet of the present invention, a colored concealing layer may be further formed between the substrate sheet and the picture pattern layer.

[0079] The colored concealing layer is only required to be able to conceal the base color of the adherend when the decorative sheet and the adherend are joined together, and is usually formed so as to cover the base sheet.

[0080] The colored concealing layer can be formed by the above-mentioned known printing methods, and the ink used to form the picture pattern layer can be used as it is.

[0081] The coating amount is 2 to 30 g / m 2The thickness of the colored concealing layer is usually about 0.1 to 20 μm, preferably about 1 to 10 μm.

[0082] (Adhesive Layer) In order to improve adhesion between the transparent resin layer and the picture pattern layer described below, an adhesive layer may be formed on the picture pattern layer. The adhesive layer is preferably a transparent adhesive layer, and examples of the transparent adhesive layer include colorless transparent, colored transparent, and translucent adhesive layers.

[0083] The adhesive is not particularly limited, and any adhesive known in the field of decorative sheets can be used.

[0084] Examples of adhesives known in the field of decorative sheets include thermoplastic resins such as polyamide resins, acrylic resins, and vinyl acetate resins, and thermosetting resins such as urethane resins. These adhesives can be used alone or in combination of two or more. Two-component curing polyurethane resins or polyester resins using isocyanate as a curing agent can also be used.

[0085] The transparent adhesive layer can be formed by the above-mentioned known printing method.

[0086] The thickness of the transparent adhesive layer is not particularly limited, but the thickness after drying is about 0.1 to 30 μm, preferably about 1 to 20 μm.

[0087] (Transparent Resin Layer) The decorative floor sheet of the present invention may have a transparent resin layer.

[0088] The transparent resin layer is not particularly limited as long as it is transparent, and includes colorless and transparent, colored and transparent, translucent, etc. Examples of resins constituting the transparent resin layer include polyethylene, ethylene-α-olefin copolymer, polypropylene such as homopolypropylene and random polypropylene, polymethylpentene, polybutene, ethylene-propylene copolymer, propylene-butene copolymer, ethylene-vinyl acetate copolymer, saponified ethylene-vinyl acetate copolymer, ethylene-(meth)acrylic acid copolymer, ethylene-(meth)acrylic acid ester copolymer, olefin-based resins such as olefin-based elastomers, polyethylene terephthalate, polybutylene terephthalate, polyamide, ionomer, acrylic acid ester polymer, methacrylic acid ester polymer, polycarbonate, cellulose triacetate, etc. In recent years, the use of biomass-derived resins, which have a low environmental impact, has been widely investigated. The resin forming the transparent resin layer of the decorative sheet of the present invention can also contain a biomass-derived component; specifically, biomass polyolefin, etc. can be used. For the transparent resin layer, these resins can be used alone or in combination of two or more.

[0089] The transparent resin layer is preferably a transparent thermoplastic resin layer, more preferably contains an olefin-based resin such as a polypropylene resin or a polyethylene resin, and it is even more preferable that the resin constituting the transparent resin layer is the above-mentioned olefin-based resin or ionomer-based resin.

[0090] The transparent resin layer may be colored as long as it has transparency, but it is preferable not to blend any colorant therein.

[0091] The transparent resin layer may further contain various additives as necessary. Examples include lubricants such as silicone resins, waxes, and fluororesins; colorants such as dyes and pigments; antioxidants; ultraviolet absorbers; light stabilizers; and flame retardants. The content of the additives is not particularly limited and is, for example, 0.1% by mass or more and 10% by mass or less, with the transparent resin layer being 100% by mass.

[0092] The transparent resin layer preferably contains an ultraviolet absorber from the viewpoint of imparting weather resistance.

[0093] Examples of the ultraviolet absorber include benzotriazole-based ultraviolet absorbers, benzophenone-based ultraviolet absorbers, and triazine-based ultraviolet absorbers. Among these, triazine-based ultraviolet absorbers are preferred. One or more types of ultraviolet absorbers can be used.

[0094] Among the triazine-based ultraviolet absorbers, hydroxyphenyltriazine-based ultraviolet absorbers in which at least three organic groups selected from hydroxyphenyl groups, alkoxyphenyl groups, and organic groups containing these groups are linked to a triazine ring are more preferred, and hydroxyphenyltriazine-based ultraviolet absorbers represented by the following general formula (A) are even more preferred: Because the hydroxyphenyltriazine-based ultraviolet absorber has a branched structure, it is expected that it will be less likely to bleed out from the transparent resin layer, and excellent weather resistance can be obtained over a longer period of time.

[0095]

[0096] In general formula (A), R 11 is a divalent organic group, and R 12 is -C(=O)OR 15 and R 13 , R 14 and R 15 are each independently a monovalent organic group, and n 11 and n 12 are each independently an integer of 1 to 5.

[0097] R 11 Examples of the divalent organic group include aliphatic hydrocarbon groups such as alkylene groups and alkenylene groups, and from the viewpoint of weather resistance, alkylene groups are preferred, and the number of carbon atoms therein is preferably 1 to 20, more preferably 1 to 12, still more preferably 1 to 8, and particularly preferably 1 to 4. The alkylene group and alkenylene group may be linear, branched, or cyclic, but linear or branched groups are preferred.

[0098] Examples of alkylene groups having 1 to 20 carbon atoms include methylene, 1,1-ethylene, 1,2-ethylene, 1,3-propylene, 1,2-propylene, 2,2-propylene, and other various propylene groups (hereinafter, "various" refers to linear, branched, and isomeric forms thereof), various butylene groups, various pentylene groups, various hexylene groups, various heptylene groups, various octylene groups, various nonylene groups, various decylene groups, various undecylene groups, various dodecylene groups, various tridecylene groups, various tetradecylene groups, various pentadecylene groups, various hexadecylene groups, various heptadecylene groups, various octadecylene groups, various nonadecylene groups, and various icosylene groups.

[0099] R 13 and R 14 Examples of the monovalent organic group include an alkyl group, an alkenyl group, a cycloalkyl group, an aryl group, and an arylalkyl group. Of these, aromatic hydrocarbon groups such as an aryl group and an arylalkyl group are preferred, and an aryl group is more preferred. 13 and R 14 The monovalent organic group is preferably a phenyl group.

[0100] The aryl group preferably has from 6 to 20 carbon atoms, more preferably from 6 to 12 carbon atoms, and even more preferably from 6 to 10 carbon atoms, such as a phenyl group, various methylphenyl groups, various ethylphenyl groups, various dimethylphenyl groups, various propylphenyl groups, various trimethylphenyl groups, various butylphenyl groups, and various naphthyl groups. The arylalkyl group preferably has from 7 to 20 carbon atoms, more preferably from 7 to 12 carbon atoms, and even more preferably from 7 to 10 carbon atoms, such as a benzyl group, a phenethyl group, various phenylpropyl groups, various phenylbutyl groups, various methylbenzyl groups, various ethylbenzyl groups, various propylbenzyl groups, various butylbenzyl groups, and various hexylbenzyl groups.

[0101] R 15Examples of the monovalent organic group include an alkyl group, an alkenyl group, a cycloalkyl group, an aryl group, and an arylalkyl group. An aliphatic hydrocarbon group such as an alkyl group or an alkenyl group is preferred, and an alkyl group is more preferred. That is, R 12 As the alkyl ester group, an alkyl ester group or an alkenyl ester group is preferred, and an alkyl ester group is more preferred.

[0102] The alkyl group is preferably an alkyl group having 1 to 20 carbon atoms, more preferably 2 to 16 carbon atoms, and even more preferably 6 to 12 carbon atoms, such as a methyl group, an ethyl group, various propyl groups, various butyl groups, various pentyl groups, various hexyl groups, various octyl groups, various nonyl groups, various decyl groups, various undecyl groups, various dodecyl groups, various tridecyl groups, various tetradecyl groups, various pentadecyl groups, various hexadecyl groups, various heptadecyl groups, various octadecyl groups, various nonadecyl groups, and various icosyl groups.

[0103] The alkenyl group is preferably an alkenyl group having from 2 to 20 carbon atoms, more preferably from 3 to 16 carbon atoms, and even more preferably from 6 to 12 carbon atoms, such as a vinyl group, various propenyl groups, various butenyl groups, various pentenyl groups, various hexenyl groups, various octenyl groups, various nonenyl groups, various decenyl groups, various undecenyl groups, various dodecenyl groups, various tridecenyl groups, various tetradecenyl groups, various pentadecenyl groups, various hexadecenyl groups, various heptadecenyl groups, various octadecenyl groups, various nonadecenyl groups, and various icosenyl groups.

[0104] More specifically, the hydroxyphenyltriazine compound represented by the general formula (A) is R 11 is an alkylene group having 1 to 20 carbon atoms, and R 12 and R 15 is an alkyl ester group which is an alkyl group having 1 to 20 carbon atoms, and R 13 and R 14 is an aryl group having 6 to 20 carbon atoms, and n 11 and n 12 Hydroxyphenyltriazine compounds in which R is 1 are preferred, 11is an alkylene group having 1 to 12 carbon atoms, and R 12 and R 15 is an alkyl ester group which is an alkyl group having from 2 to 16 carbon atoms, and R 13 and R 14 is an aryl group having 6 to 12 carbon atoms, and n 11 and n 12 Hydroxyphenyltriazine compounds in which R is 1 are more preferred, 11 is an alkylene group having 1 to 8 carbon atoms, and R 12 is R 15 and an alkyl ester group, which is an alkyl group having 6 to 12 carbon atoms, R 13 and R 14 is an aryl group having 6 to 10 carbon atoms, and n 11 and n 12 More preferred are hydroxyphenyltriazine compounds in which R 11 is an alkylene group having 1 to 4 carbon atoms, and R 12 and R 15 is an ester group which is an alkyl group having 8 carbon atoms, and R 13 and R 14 is a phenyl group, and n 11 and n 12 Hydroxyphenyltriazine compounds having a molar ratio of 1 are particularly preferred.

[0105] Examples of the hydroxyphenyltriazine compound include 2-(4,6-diphenyl-1,3,5-triazin-2-yl)-5-[2-(2-ethylhexanoyloxy)ethoxy]phenol, 2-(2hydroxy-4-[1-octyloxycarbonylethoxy]phenyl)-4,6-bis(4-phenylphenyl)-1,3,5-triazine, and 2-(4,6-diphenyl-1,3,5-triazin-2-yl)-5 -[(hexyl)oxy]-phenol, 2-[4-[(2-hydroxy-3-tridecyloxypropyl)oxy]-2-hydroxyphenyl]-4,6-bis(2,4-dimethylphenyl)-1,3,5-triazine, 2-ethyl-hexanoic acid-2-[4-(4,6-diphenyl-[1,3,5]triazin-2-yl)-3-hydroxy-phenoxy]-ethyl ester, octanoic acid-2-[4- (4,6-diphenyl-[1,3,5]triazin-2-yl)-3-hydroxy-phenoxy]-ethyl ester, 2,4,6-tris{2-(2-hydroxy-4-[1-octyloxycarbonylethoxy]phenyl)}-1,3,5-triazine, 2,4-bis(2-hydroxy-4-butyloxyphenyl)-6-(2,4-bis-butyloxyphenyl)-1,3,5-triazine, 2,4-bis(2,4-dimethyl 2,4-bis(2,4-dimethylphenyl)-6-(2-hydroxy-4-n-octyloxyphenyl)-s-triazine, 2,4-bis(2,4-dimethylphenyl)-6-(2-hydroxy-4-n-octyloxyphenyl)-1-3-5-triazine, 2,4-bis(2-hydroxy-4-butyloxyphenyl)-6-(2,4-bis-butyloxyphenyl)-1,3,5-triazine, and the like, as well as mixtures, modified products, polymers, and derivatives thereof.

[0106] The content of the ultraviolet absorber is preferably 0.2 to 10.0 parts by mass, more preferably 0.5 to 5.0 parts by mass, and even more preferably 1.0 to 4.0 parts by mass, per 100 parts by mass of the resin component constituting the transparent resin layer.

[0107] Examples of light stabilizers include aromatic compounds, amine compounds, organic acid compounds, catechin compounds, and hindered amine compounds, and among these, hindered amine compounds are preferred. Hindered amine compounds have a structure containing a 2,2,6,6-tetramethylpiperidine skeleton in the molecule.

[0108] The content of the light stabilizer is preferably 0.1 to 10 parts by mass, more preferably 0.3 to 8.0 parts by mass, and even more preferably 1.0 to 5.0 parts by mass, relative to 100 parts by mass of the resin components constituting the transparent resin layer. Note that it is preferable to include a hindered amine compound as the light stabilizer in the above range.

[0109] Examples of the flame retardant include halogen-based flame retardants, phosphorus-based flame retardants, nitrogen-based flame retardants, aluminum-based flame retardants, antimony-based flame retardants, magnesium-based flame retardants, boron-based flame retardants, and zirconium-based flame retardants. From an environmental perspective, non-halogen-based flame retardants are more preferably used. The flame retardants can be used alone or in combination of two or more.

[0110] Examples of phosphorus-based flame retardants include metal phosphinate flame retardants and phosphazene flame retardants. The content of the flame retardant is not limited to its type, and is preferably 3 parts by mass or more and 30 parts by mass or less per 100 parts by mass of the resin components that make up the transparent resin layer. By keeping the content within the above range, the flame retardancy of the decorative sheet is improved while preventing any impairment of the performance required for the decorative sheet.

[0111] The thickness of the transparent resin layer is usually about 20 to 200 μm, but may exceed this range depending on the intended use of the decorative floor sheet.

[0112] (Primer Layer) A primer layer may be provided on the transparent resin layer. The primer layer can be formed by applying a known primer agent to the surface of the transparent resin layer. Examples of primer agents include urethane resin-based primer agents made from acrylic-modified urethane resin (acrylic urethane-based resin), primer agents made from urethane-cellulose-based resin (e.g., a resin obtained by adding hexamethylene diisocyanate to a mixture of urethane and soluble nitrocellulose), and resin-based primer agents made from a block copolymer of acrylic and urethane. Additives may be blended into the primer agent as needed. Examples of additives include fillers such as calcium carbonate and clay, flame retardants such as magnesium hydroxide, antioxidants, lubricants, foaming agents, ultraviolet absorbers, and light stabilizers. The amount of additives blended can be appropriately determined depending on the product characteristics.

[0113] The amount of primer applied is not particularly limited, but is usually 0.1 to 100 g / m 2 , preferably 0.1 to 50 g / m 2 That's about it.

[0114] The thickness of the primer layer is not particularly limited, but is usually about 0.01 to 10 μm, preferably about 0.1 to 1 μm.

[0115] (Back primer layer) If necessary, a back primer layer may be provided on the back surface of the substrate sheet (the surface opposite to the surface on which the picture pattern layer is laminated). For example, this is effective when laminating a decorative sheet and a substrate (adherend) to produce a decorative board.

[0116] The back primer layer can be formed by applying a known primer agent to the substrate sheet. Examples of primer agents include urethane resin-based primer agents made from acrylic-modified urethane resin (acrylic urethane-based resin), primer agents made from urethane-cellulose-based resin (e.g., a resin obtained by adding hexamethylene diisocyanate to a mixture of urethane and soluble nitrocellulose), and resin-based primer agents made from an acrylic-urethane block copolymer. Additives may be blended into the primer agent as needed. Examples of additives include fillers such as calcium carbonate and clay, flame retardants such as magnesium hydroxide, antioxidants, lubricants, foaming agents, ultraviolet absorbers, and light stabilizers. The amount of additives blended can be appropriately determined depending on the product characteristics.

[0117] The amount of primer applied is not particularly limited, but is usually 0.1 to 100 g / m 2 , preferably 0.1 to 50 g / m 2 That's about it.

[0118] The thickness of the back primer layer is not particularly limited, but is usually about 0.01 to 10 μm, preferably about 0.1 to 1 μm.

[0119] (Synthetic Resin Backer Layer) A synthetic resin backer layer (hereinafter simply referred to as "backer layer"; a synthetic resin layer for improving scratch resistance and mitigating the effects of the substrate (adherend)) may be provided on the back surface of the base sheet. Note that the scratch resistance particularly refers to resistance to dents when a partial load is applied. The decorative sheet of the present invention has sufficient scratch resistance even without a backer layer, but providing a backer layer can further improve various performance properties such as scratch resistance.

[0120] The backer layer is preferably formed by extrusion molding of a molten resin, for example, by extrusion molding using a T-die.

[0121] Methods for bonding the back surface of the substrate sheet to the backing layer include a method of bonding the substrate sheet to the backing layer obtained by extrusion molding of molten resin by heat fusion, and a method of bonding by providing an adhesive layer (and optionally a primer layer) between the substrate sheet and the backing layer.

[0122] Resins constituting the backer layer include, but are not limited to, thermoplastic resins such as polyethylene, polypropylene (PP), polyvinyl alcohol, ethylene-vinyl alcohol copolymer, polymethylene, polymethylpentene, polyethylene terephthalate, amorphous polyethylene terephthalate (A-PET), highly heat-resistant polyalkylene terephthalates (e.g., polyethylene terephthalate in which part of the ethylene glycol is substituted with 1,4-cyclohexanedimethanol or diethylene glycol, known as PET-G (manufactured by Eastman Chemical Company)), polybutylene terephthalate (PBT), polycarbonate, polyarylate, polyethylene naphthalate, polyethylene naphthalate-isophthalate copolymer, polyimide, polystyrene, polyamide, and ABS (acrylonitrile-butadiene-styrene copolymer). In recent years, the use of biomass-derived resins, which have a low environmental impact, has been widely investigated. The resins constituting the backer layer of the decorative sheet of the present invention can also contain biomass-derived components; specifically, biomass polyolefins can be used. These resins can be used alone or in combination of two or more.

[0123] The thickness of the backer layer can be appropriately set depending on the application and method of use of the final product, and is generally preferably 100 to 800 μm, more preferably 100 to 600 μm.

[0124] If necessary, the adhesive surface of the backing layer may be subjected to a known adhesion-facilitating treatment such as corona discharge treatment, plasma treatment, degreasing treatment, surface roughening treatment, etc. In addition, a primer layer may be further provided on the back surface in consideration of adhesion to the adherend.

[0125] (Vesiculation of Various Additives Contained in Each Layer of the Decorative Sheet) The various additives added to the above-mentioned layers of the decorative sheet of the present invention (such as inorganic fillers added to the primer layer or surface protective layer) are preferably vesiculated. The method for vesiculating the various additives is not particularly limited, and they can be vesiculated by any known method, among which supercritical reverse phase evaporation is preferred.

[0126] In addition to supercritical reverse-phase evaporation, other vesicle-forming methods include the Bangham method, extrusion, hydration, reverse-phase evaporation, and freeze-thawing. Briefly, the Bangham method involves placing chloroform or a chloroform / methanol mixed solvent in a flask or other container, followed by dissolving phospholipids. The solvent is then removed using an evaporator to form a thin lipid film, and a dispersion of additives is added. The resulting solution is then hydrated and dispersed in a vortex mixer to obtain vesicles. The extrusion method involves preparing a thin phospholipid solution and passing it through a filter, replacing the mixer used as an external perturbation in the Bangham method, to obtain vesicles. The hydration method is a preparation method similar to the Bangham method, but does not use a mixer; instead, vesicles are obtained by gently stirring and dispersing the solution. The reverse phase evaporation method involves dissolving phospholipids in diethyl ether or chloroform, adding a solution containing an additive to form a W / O emulsion, removing the organic solvent from the emulsion under reduced pressure, and then adding water to obtain vesicles.The freeze-thaw method uses cooling and heating as external perturbations, and obtains vesicles by repeating this cooling and heating process.

[0127] Supercritical reverse-phase evaporation is described in detail below. Supercritical reverse-phase evaporation is a method in which a substance forming the outer membrane of a vesicle is uniformly dissolved in carbon dioxide in a supercritical state or at a temperature or pressure above the supercritical point, and an aqueous phase containing various additives as water-soluble or hydrophilic encapsulation substances is added to the mixture to form a capsule-like vesicle encapsulating the various additives as encapsulation substances in a single layer. Carbon dioxide in a supercritical state refers to carbon dioxide in a supercritical state at or above its critical temperature (30.98°C) and critical pressure (7.3773±0.0030 MPa). Carbon dioxide under a temperature or pressure above its critical point refers to carbon dioxide under conditions in which only the critical temperature or only the critical pressure exceeds the critical conditions. This method can produce unilamellar vesicles with a diameter of 50 to 800 nm. Generally, a vesicle is a general term for a small vesicle having a spherical, closed membrane structure and containing a liquid phase inside, and in particular, a liposome is one whose outer membrane is composed of biological lipids such as phospholipids.

[0128] Examples of the phospholipids include glycerophospholipids such as phosphatidylcholine, phosphatidylethanolamine, phosphatidylserine, phosphatidic acid, phosphatidylglycerol, phosphatidylinositol, cardiolipin, egg yolk lecithin, hydrogenated egg yolk lecithin, soybean lecithin, and hydrogenated soybean lecithin; and sphingophospholipids such as sphingomyelin, ceramide phosphorylethanolamine, and ceramide phosphorylglycerol.

[0129] The substance that can be used to form the outer membrane may also be a dispersant such as a nonionic surfactant or a mixture of a nonionic surfactant with cholesterol or triacylglycerol.

[0130] As the nonionic surfactant, one or more of polyglycerin ether, dialkylglycerin, polyoxyethylene hydrogenated castor oil, polyoxyethylene alkyl ether, polyoxyethylene sorbitan fatty acid ester, sorbitan fatty acid ester, polyoxyethylene polyoxypropylene copolymer, polybutadiene-polyoxyethylene copolymer, polybutadiene-poly2-vinylpyridine, polystyrene-polyacrylic acid copolymer, polyethylene oxide-polyethylethylene copolymer, polyoxyethylene-polycaprolactam copolymer, etc. can be used.

[0131] As the cholesterols, one or more of cholesterol, α-cholestanol, β-cholestanol, cholestane, desmosterol (5,24-cholestadien-3β-ol), sodium cholate, cholecalciferol, and the like can be used.

[0132] The outer membrane of the liposome may be formed from a mixture of a phospholipid and a dispersant. In the decorative sheet of the present invention, by using a liposome whose outer membrane is formed from a phospholipid, it is possible to improve the compatibility between the resin composition, which is the main component of each layer, and various additives.

[0133] (Method for manufacturing decorative sheet) The decorative sheet of the present invention can be obtained by forming at least a surface protective layer on the outermost surface, for example, by laminating a picture pattern layer, a transparent adhesive layer, a transparent resin layer, and a primer layer on a base sheet, and then forming a surface protective layer on the outermost surface.

[0134] Furthermore, when the decorative sheet is embossed, it may be after the formation of the surface protective layer or before the formation of the surface protective layer. For example, as a specific embodiment, 1) a picture pattern layer, a transparent resin layer, and a primer layer may be formed in this order on the substrate sheet, and then the surface protective layer may be formed, and finally the embossing may be performed. As another specific embodiment, 2) a picture pattern layer, a transparent resin layer, and a primer layer may be formed in this order on the substrate sheet, and then the embossing may be performed, and finally the surface protective layer may be formed. As yet another specific embodiment, 3) a picture pattern layer and a transparent resin layer may be formed in this order on the substrate sheet, and then the embossing may be performed, and then a primer layer may be provided, and finally the surface protective layer may be formed. When the Sm, Rz, and area ratio of the portion up to a depth of 30 μm from the surface of the surface protective layer are adjusted by embossing, it is preferable to perform embossing after the formation of the surface protective layer.

[0135] The embossing is carried out, for example, at a sheet temperature of 120°C to 160°C and 10 to 40 kg / cm 2 The concave-convex pattern can be transferred to the printed surface of the decorative sheet with a pressure of 1000 psi.

[0136] 2. Decorative Board The decorative board of the present invention is a decorative board having the above-mentioned decorative sheet on a substrate. The decorative sheet may be laminated on the substrate so that the surface protective layer of the decorative sheet is the outermost layer.

[0137] The substrate (adherend) is not limited, and the same materials as known decorative sheets can be used. Examples include wood, metal, ceramics, plastics, and glass. In particular, the decorative sheet of the present invention is suitable for use with wood. Specific examples of wood include veneers, wood veneers, wood plywood, wood fiberboards, particle boards, and medium-density fiberboards (MDF) made from various materials such as cedar, cypress, zelkova, pine, lauan, teak, and melapy.

[0138] The lamination method is not limited, and can be, for example, a method of attaching the decorative sheet to the substrate using an adhesive. The adhesive can be appropriately selected from known adhesives depending on the type of substrate, etc. Examples include polyvinyl acetate, polyvinyl chloride, vinyl chloride-vinyl acetate copolymer, ethylene-acrylic acid copolymer, ionomer, butadiene-acrylonitrile rubber, neoprene rubber, natural rubber, etc. These adhesives can be used alone or in combination of two or more types.

[0139] The decorative board produced in this manner can be used, for example, as interior materials for buildings such as walls, ceilings, and floors, as surface decorative boards for fittings such as window frames, doors, and handrails, and as surface decorative boards for furniture or cabinets for low-voltage electrical appliances and office automation equipment, etc. In particular, the decorative board of the present invention can be suitably used as a decorative material for floors.

[0140] The present invention will be described in more detail below with reference to examples and comparative examples, but the present invention is not limited to these examples.

[0141] Example 1 (Preparation of Decorative Sheet) A primer layer (back primer layer) was provided on the back surface of a substrate sheet made of a 60 μm thick colored polypropylene film. Next, a picture pattern layer was formed on the surface of the substrate sheet by printing, and an adhesive layer was further formed on the picture pattern layer. An 80 μm thick transparent polypropylene resin (transparent random polypropylene resin) sheet was laminated on the adhesive layer by extrusion lamination to form a transparent resin layer. Next, the surface of the transparent random polypropylene resin sheet was subjected to corona discharge treatment, and then a two-component curing urethane resin was applied to form a primer layer.

[0142] An ionizing radiation curable resin containing a urethane acrylate oligomer was applied to the entire surface of the primer layer by gravure coating to a coating weight of 15 μm, and then an electron beam was irradiated using an electron irradiation device under conditions of an acceleration voltage of 165 KeV and 5 Mrad in an environment with an oxygen concentration of 200 ppm or less to form a surface protective layer. Further, the surface protective layer side was heated with an infrared non-contact heater to soften the substrate sheet and the transparent resin layer, and then embossed by heat and pressure.

[0143] The urethane acrylate oligomer contained in the ionizing radiation curable resin forming the surface protective layer was a mixture of the following urethane acrylate oligomers in the following formulation: Bifunctional urethane acrylate oligomer A (polyol component is polyester diol, Tg: 25°C, molecular weight: 1500) Hexafunctional aliphatic urethane acrylate oligomer B (Tg: 200°C or higher, molecular weight: 1500, UA306H manufactured by Kyoeisha Chemical Co., Ltd.) Blending ratio (mass ratio) A:B = 80:20

[0144] (Preparation of decorative board) A water-based emulsion adhesive (manufactured by Japan Coating Resin Co., Ltd., BA-10L (main agent):BA-11B (hardener) = 100:2.5 (mass ratio)) was applied at 80 g / m on a medium-density wood fiberboard (MDF) having a thickness of 2.5 mm. 2 The resulting laminate was attached to the primer layer side of the back surface of the decorative sheet obtained above, and left to cure at room temperature for 3 days to prepare a decorative board.

[0145] Example 2 (Nanoization of Nucleating Agent Using Supercritical Reverse Phase Evaporation) Nanoization of a nucleating agent using supercritical reverse phase evaporation was carried out as follows. First, 100 parts by mass of methanol, 82 parts by mass of a phosphate ester metal salt nucleating agent (ADK STAB NA-11, manufactured by ADEKA Corporation), and 5 parts by mass of phosphatidylcholine were placed in a high-pressure stainless steel container maintained at 60°C and sealed, and carbon dioxide was injected to a pressure of 20 MPa to create a supercritical state. Next, 100 parts by mass of ion-exchanged water was injected while vigorously stirring and mixing. After stirring for 15 minutes while maintaining the temperature and pressure inside the container, the carbon dioxide was discharged and the pressure was returned to atmospheric pressure, yielding nucleating agent vesicles having an outer membrane made of phospholipids encapsulating the nucleating agent.

[0146] (Formation of Transparent Resin Layer, Picture Pattern Layer, and Colored Concealing Layer) The polypropylene resin (transparent random polypropylene resin) containing nucleating agent vesicles obtained as described above was extruded to a thickness of 80 μm to form a transparent resin layer. A pattern was printed on one side of the transparent resin layer using a two-component curing urethane ink (V351: manufactured by Toyo Ink Mfg. Co., Ltd.) to form a picture pattern layer. Next, a two-component curing urethane ink (V351: manufactured by Toyo Ink Mfg. Co., Ltd.) having concealing properties was applied on top of the picture pattern layer in an amount of 6 g / m. 2 A colored hiding layer was formed by coating with the above.

[0147] (Formation of Primer Layer) A two-component curing urethane ink (PET-E, Regiuser: manufactured by Dainichiseika Color & Chemicals Co., Ltd.) was applied as a primer on the colored concealing layer in an amount of 1 g / m. 2 was applied to form a back primer layer.

[0148] (Formation of Embossed Pattern) Next, an embossed pattern was formed on the other surface of the transparent resin layer by pressing using an embossing mold roll.

[0149] (Formation of Surface Protective Layer) The following surface protective layer-forming composition 1 (coating amount after drying (described as film thickness after drying; the same applies hereinafter) 5 μm) and surface protective layer-forming composition 2 (coating amount after drying 10 μm) were sequentially laminated on the surface of the embossed pattern to form a surface protective layer consisting of surface protective layer 1 (lower layer) and surface protective layer 2 (upper layer).

[0150] [Surface protection layer forming composition 1] The following additives were added in the following amounts to 100 parts by mass of the main agent to prepare a surface protection layer forming composition 1. Main agent: acrylic polyol (acrylic polyol containing urethane bonds, curing agent (forming urethane bonds via bonds with isocyanate containing NH groups) (glass transition temperature approximately 100°C, weight average molecular weight Mw approximately 40,000, hydroxyl value 12) (additives) UV absorber: Tinuvin 479 (manufactured by BASF Corporation) 5 parts by mass Light stabilizer: Tinuvin 123 (manufactured by BASF Corporation) 3 parts by mass Dilution solvent: ethyl acetate 50 parts by mass Gloss adjuster: inorganic filler L-121 (manufactured by AGC Si-Tech Co., Ltd.) 15 parts by mass Curing agent: Duranate TAP-100 (manufactured by Asahi Kasei Corporation) 5 parts by mass

[0151] [Surface protective layer forming composition 2] The following resins were blended in a mass ratio of A:B:C = 40:40:20 to prepare a mixed resin. The following additives were added in the following amounts to 100 parts by mass of the mixed resin to prepare surface protective layer forming composition 2. Resin A: Polyfunctional urethane acrylate oligomer having 3 to 15 functional groups Resin B: Polyfunctional urethane acrylate oligomer having 2 to 9 functional groups Resin C: 5 parts by mass of curing agent Duranate TAP-100 (manufactured by Asahi Kasei Corporation) per 100 parts by mass of acrylic polyol having a glass transition temperature of about 100°C, a weight average molecular weight Mw of about 50,000, and a hydroxyl value of 15 (additive) Ultraviolet absorber: 5 parts by mass of Tinuvin 479 (manufactured by BASF Corporation) Light stabilizer: 3 parts by mass of Tinuvin 123 (manufactured by BASF Corporation) Dilution solvent: 50 parts by mass of ethyl acetate

[0152] (Preparation of decorative board) A water-based emulsion adhesive (manufactured by Japan Coating Resin Co., Ltd., BA-10L (main agent):BA-11B (hardener) = 100:2.5 (mass ratio)) was applied at 80 g / m on a medium-density wood fiberboard (MDF) having a thickness of 2.5 mm. 2 The resulting laminate was attached to the primer layer side of the back surface of the decorative sheet obtained above, and left to cure at room temperature for 3 days to prepare a decorative board.

[0153] Example 3 A decorative sheet and decorative board of Example 3 were produced in the same manner as in Example 1, except that the following urethane acrylate oligomers were used in the following blend as the urethane acrylate oligomer contained in the ionizing radiation curable resin that forms the surface protective layer: Bifunctional urethane acrylate oligomer A (polyol component is polyester diol, Tg: 25°C, molecular weight 1500) Bifunctional urethane acrylate oligomer B (polyol component is polyester diol, Tg: -55°C, molecular weight 5000) Hexafunctional urethane acrylate oligomer C (Tg: 200°C or higher, molecular weight 1500, UA306H manufactured by Kyoeisha Chemical Co., Ltd.) Blending ratio (mass ratio) A:B:C = 60:10:30

[0154] Example 4 Decorative sheets and decorative boards were produced in the same manner as in Example 1, except that the urethane acrylate oligomers contained in the ionizing radiation curable resin forming the surface protective layer were a mixture of the following urethane acrylate oligomers in the following formulation: Bifunctional urethane acrylate oligomer A (polyol component is polyester diol, Tg: 25°C, molecular weight 1500) Hexafunctional urethane acrylate oligomer C (Tg: 200°C or higher, molecular weight 1500, UA306H manufactured by Kyoeisha Chemical Co., Ltd.) Blend ratio (mass ratio) A:B = 65:35

[0155] Comparative Example 1 As the resin for forming a surface protective layer, a urethane acrylate ultraviolet-curable resin composition "TOMAX FA-3246" (solid content 40%, manufactured by Nippon Kako Toryo Co., Ltd.) and a urethane acrylate ultraviolet-curable resin "ART RESIN UN-904" (solid content 100%, number of (meth)acryloyloxy groups: 10, manufactured by Negami Chemical Industrial Co., Ltd.) were used as the main components, and the solid content blending ratio (mass ratio) of TOMAX FA-3246 to UN-904 was 80 / 20. Irgacure 184 (photopolymerization initiator, manufactured by BASF) was added in an amount of 3 parts by mass relative to the solid content of the resin composition, and then the mixture was diluted with butyl acetate until the solid content concentration in the paint for forming a surface protective layer was 30%, and the mixture was thoroughly stirred to prepare a paint for forming a surface protective layer. The prepared coating material for forming a surface protective layer was applied to the surface of the primer layer using a bar coater, and then dried with hot air in a drying oven at 80°C for 1 minute to form a coating layer with a coating thickness of 5.0 µm. Next, using a UV irradiation device set at a height of 60 mm from the coated surface of the coating layer, a UV irradiation dose of 250 mJ / cm was applied. 2 The coating was cured by UV irradiation under the conditions of 1.0 to 1.5° C., and a surface protective layer was formed. Except for this, the decorative sheet and decorative board of Comparative Example 1 were produced in the same manner as in Example 1.

[0156] The decorative sheets produced in the examples and comparative examples were subjected to the following measurements.

[0157] [IR Peak Height Ratio] The infrared spectrum of the surface of the surface protective layer of the decorative sheet was measured using an infrared spectrophotometer (IR Affinity-1A, manufactured by Shimadzu Corporation). -1 The height of the peak appearing at 1650-1800 cm is A. -1 The height of the peak appearing at B is 3200-3500 cm -1 The height of the peak appearing in the graph was defined as C, and the ratios (A / B)×100 and (B / C)×100 were defined as the peak height ratios.

[0158] The peak height was measured by drawing a baseline for each wavelength range and measuring the length from the peak to the baseline so that it was horizontal to the vertical axis. When there were multiple peaks within each wavelength range, if the difference between the peak and valley of adjacent peaks was 0.010 Abs or more, they were considered to be "two peaks," and the sum of the heights of the peaks was taken as the "peak height."

[0159] [Adhesion] A checkerboard peel test was performed on the surface protective layer of the decorative sheet under the conditions of 25°C and 50% RH in a JIS environment using a test method conforming to JIS-K5600-5-6. Specifically, a total of 100 squares were cut into the surface protective layer of the decorative sheet using a cutter knife, with 11 vertical and 11 horizontal cuts spaced 1 mm apart in a checkerboard pattern. Sekisui Chemical Co., Ltd.'s adhesive tape No. 252 was then attached thereto, pressed evenly with a spatula, and peeled at a 60° angle. After five pressure-bonding and peeling tests at the same location, the number of remaining pieces of the surface protective layer was counted and evaluated according to the following evaluation criteria. When evaluating adhesion after the environmental test, the decorative sheet was left in a humid and hot environment of 60°C and 90% RH for three weeks, and then the adhesion was evaluated in a 25°C environment. The length of the decorative sheet refers to the winding direction of the original decorative sheet (MD direction in the manufacturing device), and the width of the decorative sheet refers to the width direction of the original decorative sheet (TD direction in the manufacturing device). (Evaluation criteria) ++: 100 pieces +: 95 to 99 pieces -: 80 to 94 pieces --: 79 pieces or less

[0160] [Abrasion Resistance] 300 g / m of steel wool (manufactured by Bonstar Co., Ltd. #0000) was applied to the surface protective layer of the decorative sheet. 2 The surface of the decorative sheet facing the surface protection layer was rubbed 100 times with steel wool #0000 under a load of 1 kg, and the degree of scratching was evaluated according to the following evaluation criteria. (Evaluation criteria) ++: No scratches occurred +: Slight scratches occurred -: Large amounts of scratches occurred

[0161] [Pencil hardness] The pencil hardness was measured by a test method in accordance with JIS K5600-5-4. The hardness at which no scratches were generated on the surface was taken as the pencil hardness.

[0162] [Whitening by bending] A decorative sheet was cut into a size of 10 cm x 10 cm to prepare a test piece. The test piece was suddenly bent 180 degrees in two directions, lengthwise and widthwise (both lengthwise and widthwise), so that the surface protective layer side formed a peak, and evaluated according to the following evaluation criteria. Note that the length of the decorative sheet refers to the direction in which the original decorative sheet is wound (MD direction in the manufacturing device), and the width of the decorative sheet refers to the width direction of the original decorative sheet (TD direction in the manufacturing device). Evaluation criteria ++: No whitening at all +: Partial whitening but not noticeable -: Whitening present and noticeable

[0163] The results are shown in Table 1.

[0164]

[0165] From the results in Table 1, it was found that in Examples 1 and 2, the peak height ratio of A to B was 221 or 116, and since the ester bonds were present in an appropriate amount, the surface protective layer had an appropriate hardness, and the evaluations of scratch resistance, pencil hardness, and flexural whitening were excellent, and all of these properties were achieved. Furthermore, in Examples 1 and 2, the peak height ratio of B to C was 1723 or 5057, and since the urethane bonds were present in an appropriate amount, it was thought that hydrogen bonds were formed with the ester bonds in the surface protective layer, as shown in Figure 6, and therefore the adhesion was rated ++, and furthermore, since hydrolysis was suppressed, the adhesion after the environmental test was rated ++.

[0166] Furthermore, the results in Table 1 show that the surface protective layer in Example 3 is relatively soft compared to the surface protective layers in Examples 1 and 2. That is, the peak height ratio of A to B is larger compared to Examples 1 and 2, and the surface protective layer contains fewer ester bonds, so it is softer, and although the scratch resistance and pencil hardness are slightly inferior compared to Examples 1 and 2, it is found that whitening on bending is more suppressed. Furthermore, the peak height ratio of B to C in Example 3 is larger compared to Examples 1 and 2, and the surface protective layer contains fewer urethane bonds, so it is slightly inferior in adhesion compared to Examples 1 and 2, and it is also more susceptible to hydrolysis, so it is found that the adhesion after the environmental test is slightly inferior.

[0167] Furthermore, Table 1 shows that the surface protective layer of Example 4 was relatively hard and brittle compared to the surface protective layers of Examples 1 and 2. That is, the peak height ratio of A to B was smaller compared to Examples 1 and 2, and the surface protective layer contained more ester bonds, making it harder, and the pencil hardness was rated H, but the bending whitening was rated +. Furthermore, the peak height ratio of B to C in Example 4 was smaller compared to Examples 1 and 2, and the urethane bonds contained more, which are thought to form hydrogen bonds with the ester bonds in the surface protective layer, as shown in Figure 6, so the adhesion was rated ++. Furthermore, it was found that the adhesion after the environmental test was rated ++ because hydrolysis was further suppressed.

[0168] Example 5 A decorative sheet and a decorative board were produced in the same manner as in Example 1, except that 3 parts by mass of a phosphate glass silver-supported compound (PG-711 manufactured by Koa Glass Co., Ltd.) was added as an antiviral agent to 100 parts by mass of the ionizing radiation-curable resin forming the surface protective layer. The peak height ratios of A and B and B and C in the surface protective layer were the same as in Example 1.

[0169] The decorative sheets produced in Examples 1 and 5 were used to carry out the following evaluations.

[0170] [Antiviral Properties] <Evaluation Method> The decorative sheets produced in Examples 1 and 5 were subjected to an antiviral performance test in accordance with the antiviral test method (ISO 21702), and the antiviral activity value against influenza virus was calculated and evaluated based on the following evaluation criteria. The results are shown in Table 2. A + rating indicates that there is no problem in practical use. In addition, the antiviral agent (parts by mass) in Table 2 refers to the amount (parts by mass) of antiviral agent used per 100 parts by mass of ionizing radiation curable resin. <Evaluation Criteria> +: Antiviral activity value was 2.0 or more -: Antiviral activity value was less than 2.0

[0171] The results are shown in Table 2.

[0172]

[0173] Example 6 Decorative sheets and decorative boards were produced in the same manner as in Example 1, except that the following resin composition was hot-melt extruded and laminated as a transparent polypropylene-based resin (transparent random polypropylene-based resin) to form an 80 μm transparent resin layer. The peak height ratios of A and B and B and C of the surface protective layer were the same as in Example 1. (Resin composition) Transparent polypropylene resin: 100 parts by mass Phosphinic acid metal salt flame retardant (product name: Pekoflam STC (manufactured by Archroma); aluminum phosphinate): 10 parts by mass

[0174] The decorative sheets produced in Examples 1 and 6 were used to carry out the following evaluations.

[0175] [Flame Retardancy Evaluation] The decorative panels prepared in Examples 1 and 6 were cut into 9 cm x 30 cm pieces to serve as test specimens. As shown in Figures 7 and 8, a rectangular metal stand 103 was placed on the stand 102 of a commercially available household heater 101 (Zaiguru Handsome SJ-100 (trade name)). A test specimen 105 was placed in a metal frame 104 set on the stand, and a fire spread resistance test was conducted under conditions of a heater angle of 45° and a heater output dial of 4. Specifically, the test specimen was preheated for 2 minutes using the household heater. Next, as shown in Figure 7, the heater-side end 106 of the test specimen in the longitudinal direction was heated with a lighter 107 for 1 minute to ignite the end, and the fire was allowed to spread longitudinally along the test specimen 105 as shown in Figure 8. The fire spread was then visually observed, and the burning distance (L1) and burning duration were evaluated as follows. This allowed for evaluation of horizontal flammability (fire spread resistance).

[0176] (Burning Distance (L1)) The test piece was ignited and the flame from the lighter was removed, and the flame spread distance (L1) was measured from the initial ignition and evaluated according to the following evaluation criteria. A rating of + or higher indicates that there is no problem in practical use. ++: L1 is less than 5 cm +: L1 is 5 cm or more but less than 10 cm -: L1 is 10 cm or more

[0177] (Burning duration) The burning duration from initial ignition to self-extinguishing, after the test piece was ignited and the lighter flame was removed, was measured and evaluated according to the following evaluation criteria. A rating of + or higher is considered acceptable for practical use. +++: Burning duration is less than 100 seconds or does not ignite ++: Burning duration is 100 seconds or more but less than 300 seconds +: Burning duration is 300 seconds or more but less than 600 seconds -: Burning duration is 600 seconds or more (does not self-extinguish in 600 seconds)

[0178] The results are shown in Table 3.

[0179]

[0180] 1: Decorative sheet 11: Base sheet 12: Design pattern layer 13: Transparent resin layer 14: Surface protective layer 2: Base 101. Household heater 102. Household heater base 103. Metal rectangular base 104. Metal frame 105. Test piece 106. Heater side end of test piece in the longitudinal direction 107. Lighter L1. Burning distance

Claims

1. A decorative sheet having at least a surface protective layer, the surface protective layer containing a cross-linked curable resin, and an infrared spectroscopy measurement of the surface protective layer shows a wavelength of 855 to 1325 cm -1 The height of the peak appearing at 1650 to 1800 cm is defined as A. -1 The peak height ratio ((A / B)×100(%)) of A to B is 105% or more and 400% or less, when the height of the peak appearing in the surface protective layer is B, and -1 a peak height ratio of B to C ((B / C)×100(%)) is 1000% or more and 6000% or less, when C is the height of a peak appearing in the decorative sheet.

2. The decorative sheet according to claim 1, wherein the peak height ratio between said A and B is 110% or more and 300% or less, and the peak height ratio between said B and C is 1300% or more and 5500% or less.

3. The decorative sheet according to claim 1, wherein the crosslinking curable resin includes an ionizing radiation curable resin.

4. The decorative sheet according to claim 3, wherein the ionizing radiation curable resin comprises an acrylic resin having a (meth)acryloyl group.

5. The decorative sheet according to claim 1, wherein the surface protective layer contains at least one agent selected from the group consisting of antibacterial agents, antiviral agents, and antiallergen agents.

6. The decorative sheet according to claim 1, comprising a picture pattern layer, a transparent resin layer and said surface protective layer on a base sheet in this order.

7. The decorative sheet according to claim 6, wherein at least one layer selected from the group consisting of the base sheet and the transparent resin layer contains a flame retardant.

8. The decorative sheet according to claim 6, wherein at least one layer selected from the group consisting of the base sheet, the picture pattern layer, the transparent resin layer, and the surface protective layer contains a component derived from biomass.

9. A decorative board having the decorative sheet according to any one of claims 1 to 8 on a substrate.

Citation Information

Patent Citations

  • Hard coat film

    JP2017177667A

  • Top clear sheet for decorating sheet

    JP1999116700A

  • Decorative sheet

    JP2017042917A

  • Decorative sheet and method for producing decorative sheet

    JP2018144437A

  • Decorative sheet and manufacturing method thereof

    JP2020075420A

Cited By

  • Transparent film and decorative plate

    WO2026063173A1