Joined body manufacturing method, processing liquid, and processing method
The method of using a treatment liquid with a reducing agent and low metal anticorrosive agent in the direct bonding of semiconductor elements addresses the issue of suboptimal bonding strength by maintaining the metal oxide film, resulting in improved bonding and reliability of semiconductor devices.
Patent Information
- Application Number
- PCT/JP2024/007535
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-30
- Filing Date
- 2024-02-29
- Publication Date
- 2024-10-03
AI Technical Summary
Current direct bonding techniques for semiconductor elements often result in suboptimal bonding strength due to the difficulty in bonding metal oxide films and the surface roughening that occurs during their removal, which compromises the electrical connection and reliability of semiconductor devices.
A method involving a treatment liquid with a reducing agent and a low concentration of metal anticorrosive agent is applied to the semiconductor elements, which helps maintain the metal oxide film on the surface, allowing for improved bonding strength without surface roughening, using a pretreatment step with a straight nozzle discharge to enhance the bonding process.
The method achieves a bonded body with enhanced bonding strength by maintaining the metal film on the surface, improving the electrical connection and reliability of semiconductor devices, while minimizing surface roughening and inhibiting corrosion.
Smart Images

Figure JP2024007535_03102024_PF_FP_ABST
Abstract
Description
Manufacturing method of bonded body, treatment solution and treatment method
[0001] The present invention relates to a method for manufacturing a bonded body, a treatment liquid used in the method for manufacturing a bonded body, and a method for treating a bonded member.
[0002] From the viewpoints of downsizing, improving performance, and reducing power consumption of semiconductor devices, a technique called direct bonding is known as a technique for connecting semiconductor elements together, in which semiconductor elements are bonded together and electrodes exposed on the surfaces of the semiconductor elements are directly bonded to form an electrical connection. In the direct bonding, the surfaces of the semiconductor elements are often planarized to form bonding surfaces where the electrodes are exposed, and then the semiconductor elements are bonded together so that the electrodes face each other.
[0003] For example, Patent Document 1 discloses a method for manufacturing a semiconductor device, which includes forming an electrode made of metal on a predetermined surface, forming a non-metallic region on the predetermined surface using an insulating film, forming an insulating film on the outermost surface of the predetermined surface including the electrode and the non-metallic region, forming a substrate having a structure that prevents diffusion of the metal in the non-metallic region so as to surround the electrode, and bonding two of the substrates together so that the electrodes face each other with their predetermined surfaces facing each other.
[0004] JP 2016-181531 A
[0005] The present inventors, with reference to the technology described in Patent Document 1, have studied direct bonding in which the surfaces of semiconductor elements are planarized and then the planarized surfaces are used as bonding surfaces to bond the semiconductor elements together, and have found that there is room for further improvement in the bonding strength of the resulting bonded body.
[0006] In view of the above circumstances, an object of the present invention is to provide a method for manufacturing a bonded body having excellent bonding strength, a treatment liquid used in the method for manufacturing a bonded body, and a method for treating a bonded member.
[0007] As a result of extensive research into solving the above problems, the present inventors have found that the above problems can be solved by the following configuration.
[0008] [1] A method for manufacturing a bonded body, the method including: a preparation step of preparing bonded members having a maximum surface height Rmax of 50 nm or less; a pretreatment step of contacting the surfaces of the bonded members with a treatment liquid; and a bonding step of bonding the bonded members that have been subjected to the pretreatment step to another bonded member, wherein a conductive portion and an insulating portion containing a metal are exposed on the surfaces of the bonded members, the treatment liquid contains a reducing agent, and the content of a metal corrosion inhibitor contained in the treatment liquid is 0.01 mass% or less relative to the total mass of the treatment liquid. [2] The method for manufacturing a bonded body according to [1], wherein in the pretreatment step, the treatment liquid is supplied to the surfaces of the bonded members by ejecting it from a straight nozzle. [3] The method for manufacturing a bonded body according to [1] or [2], further including a cleaning step of cleaning the surfaces of the bonded members after the preparation step and before the pretreatment step. [4] The method for manufacturing a bonded body according to [3], wherein the time elapsed between the completion of the cleaning step and the start of the pretreatment step is 1 minute or more. [5] The method for manufacturing a bonded body according to any one of [1] to [4], wherein the reducing agent includes at least one selected from the group consisting of an inorganic acid reducing agent, an organic acid reducing agent, and a sugar. [6] The method for manufacturing a bonded body according to any one of [1] to [5], wherein the surface of the bonding member has a maximum height Rmax of 10 nm or less. [7] The method for manufacturing a bonded body according to any one of [1] to [6], wherein the surface of the bonding member has a surface roughness Ra of 1 nm or less. [8] The method for manufacturing a bonded body according to any one of [1] to [7], wherein a surface region of the surface of the bonding member where the insulating portion is exposed has a water contact angle of 30 degrees or less. [9] The method for manufacturing a bonded body according to any one of [1] to [8], wherein the bonding member has a plurality of element regions, and further comprising, after the preparing step, a singulating step of singulating the bonding member into individual element regions.
[10] The method for manufacturing a bonded body according to any one of [1] to [9], wherein the reducing agent includes an inorganic acid reducing agent.
[11] The method for producing a joined body according to
[10] , wherein the inorganic acid reducing agent includes at least one selected from the group consisting of nitrous acid and salts thereof, sulfurous acid and salts thereof, and thiosulfuric acid and salts thereof.
[12] The method for producing a bonded body according to any one of [1] to [9], wherein the reducing agent includes an organic acid reducing agent.
[13] The method for producing a bonded body according to
[12] , wherein the organic acid reducing agent includes at least one selected from the group consisting of ascorbic acid, formic acid, oxalic acid, 3,4,5-trihydroxybenzoic acid, and salts thereof.
[14] The method for producing a bonded body according to any one of [1] to
[13] , wherein the treatment liquid further includes an antibacterial agent.
[15] The method for producing a bonded body according to
[14] , wherein the antibacterial agent is a compound having at least one quaternary ammonium cation group in the molecule or a salt thereof.
[16] The method for producing a bonded body according to any one of [1] to
[15] , wherein the conductive portion is made of copper or a copper alloy.
[17] A treatment liquid used for treatment to be brought into contact with the surface of a joined member, the treatment liquid containing a reducing agent, and a metal corrosion inhibitor content of 0.01 mass% or less relative to the total mass of the treatment liquid, the joined member being a joined member used to produce a joined body by joining a treated joined member obtained by performing the treatment with another joined member, a conductive portion and an insulating portion containing metal exposed on the surface of the joined member, and a maximum height Rmax of the surface of the joined member being 50 nm or less.
[18] The treatment liquid according to
[17] , wherein the reducing agent includes at least one selected from the group consisting of an inorganic acid-based reducing agent, an organic acid-based reducing agent, and a sugar.
[19] The treatment liquid according to
[18] , wherein the inorganic acid-based reducing agent includes at least one selected from the group consisting of nitrous acid and its salts, sulfurous acid and its salts, and thiosulfuric acid and its salts.
[20] The treatment solution according to
[18] or
[19] , wherein the organic acid reducing agent comprises at least one selected from the group consisting of ascorbic acid, formic acid, oxalic acid, 3,4,5-trihydroxybenzoic acid, and salts thereof.
[21] The treatment solution according to any one of
[17] to
[20] , further comprising an antibacterial agent.
[22] The treatment solution according to
[21] , wherein the antibacterial agent is a compound having at least one quaternary ammonium cation group in the molecule, or a salt thereof.
[23] A method for treating bonded members used to manufacture a bonded body, the bonded members having surfaces on which metal-containing conductive parts and insulating parts are exposed and which have a maximum height Rmax of 50 nm or less, the method comprising contacting the surfaces of the bonded members with a treatment liquid containing a reducing agent and having a metal corrosion inhibitor content of 0.01 mass % or less relative to the total mass.
[24] The method according to
[23] , wherein the treatment liquid is supplied to the surfaces of the bonded members by ejecting it from a straight nozzle.
[0009] According to the present invention, it is possible to provide a method for manufacturing a bonded body having excellent bonding strength. Furthermore, according to the present invention, it is possible to provide a treatment liquid used in the method for manufacturing a bonded body, and a method for treating a bonded member.
[0010] Fig. 3 is a schematic diagram showing an example of a bonded body manufactured by the method for manufacturing a bonded body of the present invention. Fig. 4 is a schematic cross-sectional view showing an example of a semiconductor element used in the method for manufacturing a bonded body of the present invention. Fig. 5 is a schematic cross-sectional view showing an example of a bonding step included in the method for manufacturing a bonded body of the present invention. Fig. 6 is a schematic cross-sectional view showing an example of a bonded body obtained by the bonding step shown in Fig. 3.
[0011] The method for producing a bonded body, a temporary fixing member, and a laminate of the present invention will be described in detail below based on preferred embodiments shown in the accompanying drawings. Note that the drawings described below are merely illustrative for explaining the present invention, and the present invention is not limited to the drawings shown below. Note that in the following, the term "to" indicating a range of values includes the values written on both sides. For example, ε 1 is the number α 1 ~Number β 1 That is, ε 1 The range of α 1 and the number β 1 The range includes α 1 ≦ε 1 ≦β 1In this specification, when two or more types of a component are present, the "content" of that component refers to the total content of those two or more components. Temperature and pressure include the tolerance range generally accepted in the relevant technical field. Temperature is 23°C unless otherwise specified in the specification. Furthermore, "same" includes the tolerance range generally accepted in the relevant technical field. Furthermore, "all" and "all over" and the like include the tolerance range generally accepted in the relevant technical field.
[0012] [Method for Manufacturing Bonded Body] The method for manufacturing a bonded body according to the present invention (hereinafter also referred to as "the present manufacturing method") includes a preparation step of preparing bonded members having a maximum surface height Rmax of 50 nm or less, a pretreatment step of bringing a treatment liquid into contact with the surfaces of the bonded members, and a joining step of bonding the pretreated bonded members to another bonded member. Here, the treatment liquid used in the pretreatment step of the present manufacturing method contains a reducing agent, and the content of a metal corrosion inhibitor contained in the treatment liquid is 0.01 mass % or less relative to the total mass of the treatment liquid.
[0013] Although the detailed mechanism by which the present manufacturing method achieves the effects of the present invention is unclear, the inventors speculate as follows: When a conductive portion is exposed on the surface of a joining member, a metal oxide film composed of an oxide of the metal contained in the conductive portion may form on the exposed conductive portion. Because metal oxide films are difficult to bond to other members such as metal films, a process of removing the metal oxide film from the surface of the joining member by wet etching or the like is performed before bonding. However, it is presumed that applying a wet etching removal process to a metal oxide film increases the surface roughness after the process, resulting in a decrease in the bond strength of the joined body obtained by bonding to another joining member. In contrast, the manufacturing method of the present invention is characterized by contacting the surface of a joining member having a maximum height Rmax of 50 nm or less with a treatment liquid containing a reducing agent. This allows the metal film to be exposed on the surface without removing the metal oxide film from the surface of the conductive portion, i.e., without roughening the surface of the joining member. It is presumed that bonding to another joining member in this exposed state of the metal film results in a joined body with improved bond strength. The manufacturing method of the present invention is also characterized by using a treatment solution containing 0.01 mass % or less of a metal corrosion inhibitor, which is presumably used to suppress the amount of components that may inhibit bonding near the surface of the metal film, thereby resulting in a bonded body with improved bonding strength.
[0014] In this specification, a bonded body refers to a member formed by bonding at least two bonding members that are electrically connected to each other and are bonded in a conductive state. In this specification, a bonding member refers to a member that constitutes a semiconductor device, and examples include semiconductor elements that perform a specific function by themselves, but also members that perform a specific function when multiple elements are assembled together. Bonding members also include members that only have the function of transmitting electrical signals, such as wiring members. In this specification, a "treated bonding member" refers to a bonding member that has been treated using the specific treatment liquid described above. In addition, bonding members at any stage, including treated bonding members, may be simply referred to as "bonding members" without distinction.
[0015] Fig. 1 is a schematic diagram showing an example of the configuration of a bonded body produced by this production method. The stacked device (bonded body) 10 shown in Fig. 1 is a member in which, for example, a semiconductor element 12 and a semiconductor element 14 are stacked and bonded in a stacking direction Ds, and the semiconductor element 12 and the semiconductor element 14 are directly electrically connected. In this specification, the term "stacked device" refers to an example of a bonded body formed by bonding at least two bonding members, and refers to a member that exhibits a specific function by itself.
[0016] [Bonding Member] First, the bonding member used in this manufacturing method will be described in more detail using a semiconductor element, which is one type of bonding member, as an example. Figure 2 is a schematic cross-sectional view showing an example of the configuration of a semiconductor element, which is one type of bonding member. The semiconductor elements (bonding members) 12 and 14 shown in Figure 2 each have a semiconductor layer 32, a redistribution layer 34, a passivation layer 36, and multiple terminals 30.
[0017] The semiconductor layer 32 is a layer made of a semiconductor. The type of semiconductor making up the semiconductor layer 32 is not particularly limited, but examples include silicon, silicon carbide, germanium, gallium arsenide, and gallium nitride. A plurality of terminals 30 are provided on a surface 32a of the semiconductor layer 32. Also, an element region (not shown) in which a circuit or the like that performs a specific function is formed is provided on the surface 32a of the semiconductor layer 32.
[0018] Semiconductor elements and semiconductor wafers (described later) have element regions. The element region is a region in which various element component circuits, such as capacitors, resistors, and coils, are formed to function as electronic elements. The element region may include, for example, a region in which a memory circuit such as a flash memory, a logic circuit such as a microprocessor and an FPGA (field-programmable gate array), or a region in which a communication module such as a wireless tag and wiring are formed. In addition to the above regions, a transmitter circuit or a MEMS (Micro Electro Mechanical Systems) may also be formed in the element region. Examples of MEMS include sensors, actuators, and antennas. Examples of sensors include various sensors for acceleration, sound, light, and the like.
[0019] The rewiring layer 34 is an electrically insulating layer provided on the surface 32a of the semiconductor layer 32. An example of an insulating material that forms the rewiring layer 34 is polyimide. The rewiring layer 34 is provided with wiring 37 that is electrically connected to the element region of the semiconductor layer 32. Pads 38 are provided on the wiring 37, and the wiring 37 and the pads 38 are electrically connected to each other. Furthermore, a portion of the rewiring layer 34 does not have wiring 37, and only has pads 38. The wiring 37 and the pads 38 are members made of a conductive material, such as copper, a copper alloy, aluminum, or an aluminum alloy.
[0020] The passivation layer 36 is an electrically insulating layer provided on the surface 34a of the redistribution layer 34. Examples of insulating materials that constitute the passivation layer 36 include silicon nitride (SiN) and polyimide. The passivation layer 36 is provided with terminals 30a at positions where the wiring 37 and pads 38 of the redistribution layer 34 are provided. The terminals 30a are electrically connected to the element region via the wiring 37 and pads 38, enabling the transmission and reception of signals with the element region and the supply of voltages and the like to the element region. In addition, the passivation layer 36 is provided with terminals 30b at positions where only the pads 38 of the redistribution layer 34 are provided. Unlike the terminals 30a, the terminals 30b are not electrically connected to the semiconductor layer 32.
[0021] The constituent material of terminals 30a and 30b is not particularly limited as long as it is a material that has conductivity, similar to wiring 37 and pad 38, and examples thereof include metals and alloys.In addition, materials used for components called terminals or electrode pads in the semiconductor element field can be used as appropriate.
[0022] As shown in the figure, the surfaces of the semiconductor elements 12 and 14 have end faces 30c where the terminals 30a and 30b, which are conductive portions, are exposed, and end faces 36a where the passivation layer 36, which is an insulating portion, is exposed. Thus, the bonding member has a conductive portion containing metal and an insulating portion that has electrical insulation properties. As described below, the bonding member has at least a surface where the conductive portion and the insulating portion containing metal are exposed, and where the maximum height Rmax is 50 nm or less. In this manufacturing method, a treatment is performed by contacting the surface with a specific treatment liquid.
[0023] Examples of metals and alloys that constitute the conductive portion of the joining member include copper, copper alloys, aluminum, and aluminum alloys. The conductive portion is preferably made of copper or a copper alloy. When the conductive portion is made of copper or a copper alloy, the metal oxide film contains an oxide of copper or a copper alloy.
[0024] The semiconductor elements used as joining members in this manufacturing method are not limited to the semiconductor elements 12 and 14 shown in FIG. 2, but may be selected appropriately depending on the desired laminated device. The semiconductor element is not particularly limited, and examples thereof include logic LSIs (Large Scale Integration) (e.g., ASICs (Application Specific Integrated Circuits), FPGAs (Field Programmable Gate Arrays), ASSPs (Application Specific Standard Products), etc.), microprocessors (e.g., CPUs (Central Processing Units), GPUs (Graphics Processing Units), etc.), memories (e.g., DRAMs (Dynamic Random Access Memory), HMCs (Hybrid Memory Cubes), MRAMs (Magnetic RAMs), PCMs (Phase-Change Memory), ReRAMs (Resistive RAMs), FeRAMs (Ferroelectric RAMs), flash memories (NAND (Not AND) flash), etc.), LEDs (Light Emitting Diodes), (e.g., microflash for mobile terminals, in-vehicle devices, projector light sources, LCD backlights, general lighting, etc.), power devices, analog ICs (Integrated Circuits), (e.g., DC (Direct Current)-DC (Direct Current) Current converters, insulated gate bipolar transistors (IGBTs), etc.), MEMS (Micro Electro Mechanical Systems) (for example, acceleration sensors, pressure sensors, vibrators, gyro sensors, etc.), wireless (for example, GPS (Global Positioning System), FM (Frequency Modulation), NFC (Nearfield communication), RFEM (RF Expansion Module), MMIC (Monolithic Microwave Integrated Circuit), WLAN (Wireless Local Area Network),Examples of semiconductor devices include a semiconductor device such as a power supply, a power amplifier, a power amplifier circuit, a power amplifier circuit (PFC), ...
[0025] Each step of this manufacturing method will be described in detail below.
[0026] [Preparation Step] This manufacturing method includes a preparation step of preparing a bonding member having a surface (hereinafter also referred to as a "specific surface") on which metal-containing conductive and insulating portions are exposed and whose maximum height Rmax is 50 nm or less. Examples of the preparation step include a planarization step of forming the specific surface by planarizing the surfaces on which the conductive and insulating portions of the bonding member are exposed. The preparation step also includes procuring the bonding member by purchasing or the like.
[0027] The maximum height Rmax of the specific surface of the joining member prepared in the preparation step is 50 nm or less. In terms of better bondability, the maximum height Rmax of the specific surface is preferably 10 nm or less, more preferably 5 nm or less. The lower limit of the maximum height Rmax is not particularly limited and may be, for example, 0.1 nm or more. The maximum height Rmax (arithmetic mean height) of the surface of the joining member is determined in accordance with JIS B 0601 by measuring the maximum height at any five points on the surface of the joining member using an atomic force microscope and arithmetically averaging the obtained measurements.
[0028] The surface roughness Ra of the specific surface of the joining member is not particularly limited, but is preferably 3 nm or less, more preferably 1 nm or less, in terms of better bondability. The lower limit of the surface roughness Ra is not particularly limited, and may be, for example, 0.2 nm or more. The surface roughness Ra (arithmetic mean height) of the surface of the joining member is determined in accordance with JIS B 0601 by measuring the surface roughness at any five points on the surface of the joining member using an atomic force microscope and arithmetically averaging the obtained measured values.
[0029] The water contact angle of the surface region of the specific surface of the joining member where the insulating portion is exposed (hereinafter also referred to as the "insulating surface region") is preferably 35 degrees or less, more preferably 30 degrees or less, and even more preferably 25 degrees or less, in terms of superior bonding properties. The lower limit is not particularly limited and may be, for example, 5 degrees or more. Methods for adjusting the contact angle of the insulating surface region include, for example, selecting the constituent material of the insulating portion and controlling the surface roughness by planarization treatment.
[0030] The contact angle of water on the insulating surface region can be obtained by planarizing the surface of a model system consisting only of the same constituent materials as the insulating portion of the joining member, and measuring the contact angle of the surface of the resulting model system using the sessile drop method. Specifically, water is dropped onto the exposed insulating surface region, and the angle between the insulating surface region and the water on the side containing the water is measured to determine the contact angle. A method for determining the contact angle using the sessile drop method is described, for example, in "Wettability and Control" (published by Technical Information Association, Inc., January 31, 2001). The contact angle of the liquid droplet on the insulating surface region can be measured using a known measuring device. An example of a contact angle measuring device is the fully automatic contact angle meter "DMo-901" (manufactured by Kyowa Interface Science Co., Ltd.).
[0031] <Planarization Step> As a preparatory step for the present manufacturing method, a planarization step for planarizing the surface of the joining member is preferably performed to form a specific surface. The planarization process can form a flat surface state in which the end faces 30 c of the terminals 30 a and 30 b and the surface 36 a of the passivation layer 36 form the same plane, as shown in the semiconductor elements 12 and 14 in FIG.
[0032] An example of a planarization process for planarizing the surface of the joining member is chemical mechanical polishing (CMP). CMP is a process for planarization by a combined action of chemical action and mechanical polishing using a polishing liquid (polishing slurry) containing abrasive particles (abrasive grains). Examples of CMP include, but are not limited to, the CMP process described in Journal of the Japan Society for Precision Engineering, Vol. 84, No. 3, 2018.
[0033] The polishing liquid used in CMP is not particularly limited as long as it contains abrasive particles. CMP may also be performed using a polishing liquid that does not contain abrasive particles. Examples of abrasive particles include inorganic abrasive particles such as silica, alumina, zirconia, ceria, titania, germania, and silicon carbide; and organic abrasive particles such as polystyrene, polyacrylic, and polyvinyl chloride. The polishing liquid preferably contains water and a metal corrosion inhibitor, and may also contain at least one additive selected from the group consisting of hydrogen peroxide, an organic solvent, a passivation film forming agent, and a surfactant. The polishing liquid is preferably a slurry containing abrasive particles. The polishing liquid used in CMP may be the polishing liquid described in International Publication No. 2018 / 159530, etc., and the contents thereof are incorporated herein by reference.
[0034] [Pretreatment Step] In this manufacturing method, the pretreatment step involves contacting a specific surface of the bonded members prepared in the preparation step with a specific treatment liquid, which will be described later. Another embodiment of the present invention is a method for treating bonded members used to manufacture a bonded body, in which a specific treatment liquid is brought into contact with the specific surface of the bonded members. Hereinafter, the pretreatment step of this manufacturing method and the above-described method for treating bonded members will be described without distinguishing between them.
[0035] By subjecting the joining member to the above treatment, a treated joined member is obtained. By joining such a treated joined member to another joining member (preferably a similarly treated joined member), a joined body with improved joining strength is obtained. This is presumably because, in the treated joined member, the metal oxide film formed on the surface of the conductive portion of the joining member is reduced by the treatment liquid, and a metal film with higher joining strength is formed on a specific surface of the joining member.
[0036] <Treatment Solution> The treatment solution used in the pretreatment step contains a reducing agent, and the content of a metal corrosion inhibitor contained in the treatment solution is 0.01 mass % or less based on the total mass of the treatment solution. Each component contained in the treatment solution will be described in detail below.
[0037] (Reducing Agent) The treatment liquid contains a reducing agent. The reducing agent is not particularly limited as long as it is a compound having a reducing function, and examples thereof include inorganic acid reducing agents, organic acid reducing agents, and other reducing agents such as sugars.
[0038] The inorganic acid reducing agent is a compound selected from inorganic acids having a reducing function and their salts. Examples of inorganic acid reducing agents include at least one compound selected from the group consisting of nitrous acid and its salts, sulfurous acid and its salts, and thiosulfuric acid and its salts. Among these, at least one compound selected from the group consisting of nitrous acid and its salts, and thiosulfuric acid and its salts is preferred, and thiosulfuric acid and its salts are more preferred in terms of superior bonding strength of the bonded body. When the inorganic acid reducing agent is in the form of a salt, examples of the salt include sodium salts, potassium salts, and ammonium salts.
[0039] The organic acid reducing agent is a compound selected from organic acids having a reducing function, organic acid derivatives, and salts thereof. Examples of organic acid derivatives include esters of organic acids and alcohol compounds, ethers of organic acids having a hydroxyl group and alcohol compounds, and esters of organic acids having a hydroxyl group and inorganic acids such as phosphoric acid and sulfuric acid. When the organic acid reducing agent is in the form of a salt, examples of the salt include sodium salts, potassium salts, and ammonium salts.
[0040] More specifically, the organic acid reducing agent may be at least one compound selected from the group consisting of ascorbic acid, formic acid, oxalic acid, 3,4,5-trihydroxybenzoic acid, derivatives thereof, and salts thereof. Ascorbic acid includes L-ascorbic acid, D-ascorbic acid, and isoascorbic acid. Examples of the derivatives include ascorbic acid derivatives such as alkylglyceryl ascorbic acid, glycerol ascorbate, alkyl ether ascorbate, alkyl ester ascorbate, ascorbic acid sulfate, and ascorbic acid phosphate. The organic acid reducing agent is preferably at least one selected from the group consisting of ascorbic acid, formic acid, oxalic acid, 3,4,5-trihydroxybenzoic acid, and salts thereof, with formic acid being more preferred in terms of superior bonding strength of the bonded structure.
[0041] Examples of reducing agents other than inorganic acid-based reducing agents and organic acid-based reducing agents include sugars such as fructose, glucose, and ribose, hydrogen peroxide, reducing sulfur compounds, and hydrazine compounds such as hydrazine and hydrazide compounds. Reducing sulfur compounds are compounds that contain a sulfur atom and function as reducing agents. Examples of reducing sulfur compounds include mercaptosuccinic acid, dithiodiglycerol, bis(2,3-dihydroxypropylthio)ethylene, sodium 3-(2,3-dihydroxypropylthio)-2-methyl-propylsulfonate, 1-thioglycerol, sodium 3-mercapto-1-propanesulfonate, 2-mercaptoethanol, thioglycolic acid, and 3-mercapto-1-propanol.
[0042] The reducing agent is preferably at least one selected from the group consisting of inorganic acid reducing agents, organic acid reducing agents, and sugars, more preferably nitrous acid, sulfurous acid, thiosulfuric acid, ascorbic acid, formic acid, oxalic acid, 3,4,5-trihydroxybenzoic acid, glucose, derivatives thereof, and salts thereof, and even more preferably nitrite, thiosulfate, ascorbic acid, formic acid, oxalic acid, 3,4,5-trihydroxybenzoic acid, or glucose.
[0043] The reducing agent may be used alone or in combination of two or more. The content of the reducing agent is preferably 0.1% by mass or more, more preferably 0.5% by mass or more, and even more preferably 1.0% by mass or more, relative to the total mass of the treatment liquid, from the viewpoint of obtaining a more excellent bonding strength of the bonded body. The upper limit is not particularly limited, but is preferably 10.0% by mass or less, more preferably 5.0% by mass or less, relative to the total mass of the treatment liquid, from the viewpoint of obtaining a more excellent bonding strength of the bonded body.
[0044] (Metal Corrosion Inhibitor) The treatment liquid may contain a metal corrosion inhibitor. However, when the treatment liquid contains a metal corrosion inhibitor, the content of the metal corrosion inhibitor is 0.01 mass % or less relative to the total mass of the treatment liquid. The metal corrosion inhibitor is a compound that has the function of preventing corrosion of the metal components that constitute the conductive portion of the joint member to be treated.
[0045] Examples of metal corrosion inhibitors include heterocyclic compounds. Examples of heterocyclic compounds include azole compounds, pyrrole compounds, pyridine compounds, pyrazine compounds, pyrimidine compounds, indole compounds, indolizine compounds, indazole compounds, quinoline compounds, and oxazole compounds. Examples of metal corrosion inhibitors include triazole compounds, tetrazole compounds, and pyrrole compounds, and more preferably triazole compounds. In this specification, azole compounds include their tautomers.
[0046] Examples of the azole compound include an imidazole compound in which one of the atoms constituting the azole ring is a nitrogen atom, a pyrazole compound in which two of the atoms constituting the azole ring are nitrogen atoms, a thiazole compound in which one of the atoms constituting the azole ring is a nitrogen atom and the other is a sulfur atom, a triazole compound in which three of the atoms constituting the azole ring are nitrogen atoms, and a tetrazole compound in which four of the atoms constituting the azole ring are nitrogen atoms, with triazole compounds or tetrazole compounds being preferred.
[0047] Examples of the triazole compound include benzotriazole compounds in which two adjacent substituents on a triazole ring are bonded to each other to form a benzene ring. Examples of the benzotriazole compound include benzotriazole, 5-methyl-1H-benzotriazole (CAS Registry Number: 136-85-6), tolyltriazole (CAS Registry Number: 29385-43-1), 5-aminobenzotriazole, 1-hydroxybenzotriazole, 4-carboxybenzotriazole, 5,6-dimethylbenzatriatriazole, 1-[N,N-bis(hydroxyethyl)aminoethyl]benzotriazole, 1-(1,2-dicarboxyethyl)benzotriazole, 1-[N,N-bis(2-ethylhexyl)aminomethyl]benzotriazole, 1-[N,N-bis(2-ethylhexyl)aminomethyl]methylbenzotriazole, 2,2'-{[(methyl-1H-benzotriazol-1-yl)methyl]imino}bisethanol, and carboxybenzotriazole. Examples of triazole compounds other than benzotriazole compounds include 1,2,3-triazole, 1,2,4-triazole, 3-methyl-1,2,4-triazole, 3-amino-1,2,4-triazole, and 1-methyl-1,2,3-triazole.
[0048] Examples of tetrazole compounds include 1H-tetrazole (1,2,3,4-tetrazole), 5-methyl-1,2,3,4-tetrazole, 5-amino-1,2,3,4-tetrazole, 1,5-pentamethylenetetrazole, 1-phenyl-5-mercaptotetrazole, and 1-(2-dimethylaminoethyl)-5-mercaptotetrazole.
[0049] The metal corrosion inhibitor may be used alone or in combination of two or more. In order to obtain a bonded body with superior bonding strength, the content of the metal corrosion inhibitor contained in the treatment liquid is preferably 0.01 mass% or less relative to the total mass of the treatment liquid, and it is preferable that the treatment liquid is substantially free of the metal corrosion inhibitor. Here, "substantially free of" a certain component means that the content of that component is 0.001 mass% or less relative to the total mass of the treatment liquid.
[0050] (Water) The treatment solution may contain water, and preferably contains water. The type of water used in the treatment solution may be any type that does not adversely affect the semiconductor substrate, and distilled water, deionized (DI) water, and pure water (ultrapure water) can be used. Pure water (ultrapure water) is preferred because it contains almost no impurities and has less of an effect on the semiconductor substrate during the semiconductor substrate manufacturing process. The water content may be the balance of the reducing agent, metal corrosion inhibitor, antibacterial agent, and other components described below, and is preferably 85% by mass or more, more preferably 90% by mass or more, and even more preferably 95% by mass or more, based on the total mass of the treatment solution. The upper limit is preferably 99.99% by mass or less, more preferably 99.9% by mass or less, and even more preferably 99% by mass or less, based on the total mass of the treatment solution. Furthermore, in the treatment liquid, it is preferable that the remainder excluding the reducing agent, the metal corrosion inhibitor, the optionally added antibacterial agent, and any unintentionally mixed impurities is water, and it is more preferable that the remainder excluding the reducing agent, the optionally added antibacterial agent, and any unintentionally mixed impurities is water.
[0051] (Antibacterial Agent) The treatment liquid may contain an antibacterial agent. The antibacterial agent is a compound that has an antibacterial effect against bacteria, and any compound that does not inhibit the reducing action of the treatment liquid can be used as appropriate. The antibacterial agent may be in the form of a salt (for example, a known salt).
[0052] Examples of antibacterial agents include quaternary ammonium compounds, alcohol-based antibacterial agents, phenol-based antibacterial agents, aldehyde-based antibacterial agents, carboxylic acid-based antibacterial agents, ester-based antibacterial agents, ether-based antibacterial agents, nitrile-based antibacterial agents, peroxide-based antibacterial agents, halogen-based antibacterial agents, pyridine-based antibacterial agents, triazine-based antibacterial agents, isothiazolin-based antibacterial agents, imidazole-based antibacterial agents, anilide-based antibacterial agents, biguanide-based antibacterial agents, disulfide-based antibacterial agents, thiocarbamate-based antibacterial agents, carbohydrate-based antibacterial agents, tropolone-based antibacterial agents, surfactant-based antibacterial agents, and organometallic compounds. Among these, quaternary ammonium compounds, phenol-based antibacterial agents, carboxylic acid-based antibacterial agents, isothiazolin-based antibacterial agents, and biguanide-based antibacterial agents are preferred, and quaternary ammonium compounds are more preferred.
[0053] Examples of quaternary ammonium compounds include compounds having at least one quaternary ammonium cation group in the molecule, or salts thereof, which have bactericidal activity. Among these, salts with anions containing halogen atoms, such as halide ions, are preferred, with quaternary ammonium chloride, quaternary ammonium fluoride, or quaternary ammonium bromide being more preferred. Specific examples of suitable quaternary ammonium compounds include salts of the above anions with quaternary ammonium cations selected from the group consisting of tetramethylammonium cation, tetraethylammonium cation, tetrapropylammonium cation, tetrabutylammonium cation, methyltripropylammonium cation, methyltributylammonium cation, ethyltrimethylammonium cation, dimethyldiethylammonium cation, benzyltrimethylammonium cation, hexadecyltrimethylammonium cation, (2-hydroxyethyl)trimethylammonium cation, and spiro-(1,1')-bipyrrolidinium cation. Other preferred specific examples of the quaternary ammonium compound include benzalkonium chloride, didecyldimethylammonium chloride (DDAC), hexadecylpyridinium chloride (CPC), 3,3'-(2,7-dioxaoctane)bis(1-dodecylpyridinium bromide) (Hygeria), benzethonium chloride, and domiphen bromide. As the quaternary ammonium compound, a salt of a cation selected from the group consisting of tetramethylammonium cation, tetraethylammonium cation, and tetrapropylammonium cation with an anion selected from the group consisting of chloride ion, fluoride ion, and bromide ion is preferred, and tetramethylammonium bromide, tetraethylammonium bromide, or tetrapropylammonium bromide is more preferred.
[0054] Examples of phenolic antibacterial agents include cresol, chlorothymol, dichloroxylenol, and hexachlorophene. Examples of carboxylic acid antibacterial agents include unsaturated carboxylic acids such as sorbic acid, and aromatic carboxylic acids such as benzoic acid and salicylic acid, with sorbic acid, benzoic acid, and salicylic acid being preferred. Examples of isothiazoline antibacterial agents include 5-chloro-2-methyl-4-isothiazolin-3-one and 2-methyl-4-isothiazolin-3-one. Examples of biguanide antibacterial agents include 1,1'-hexamethylenebis[5-(p-chlorophenyl)biguanide] dihydrochloride (chlorhexidine hydrochloride), bis(p-chlorophenyldiguanide)hexane digluconate (chlorhexidine gluconate), and poly(hexamethylenebiguanide) hydrochloride (hexamethylenebiguanidine hydrochloride).
[0055] The antibacterial agent may be used singly or in combination of two or more. When the treatment liquid contains an antibacterial agent, the content of the antibacterial agent is preferably 0.01 to 0.1 mass %, and more preferably 0.02 to 0.08 mass %, relative to the total mass of the treatment liquid.
[0056] (Other Components) The treatment liquid may contain components other than the reducing agent, metal corrosion inhibitor, water, and antibacterial agent. Examples of other components include surfactants, pH adjusters, complexing agents, and organic solvents. To achieve superior bonding strength of the bonded body, the content of other components in the treatment liquid other than the reducing agent, metal corrosion inhibitor, water, and antibacterial agent is preferably 10% by mass or less relative to the total mass of the treatment liquid, and it is more preferable that the treatment liquid is substantially free of other components other than the reducing agent, metal corrosion inhibitor, water, and antibacterial agent. To achieve superior bonding strength of the bonded body, the content of other components in the treatment liquid other than the reducing agent, water, and antibacterial agent is preferably 5% by mass or less relative to the total mass of the treatment liquid, and it is more preferable that the treatment liquid is substantially free of other components other than the reducing agent, water, and antibacterial agent. The other components are described below.
[0057] -Surfactant- A surfactant is a compound having a hydrophilic group and a hydrophobic group (lipophilic group) in one molecule. Examples of surfactants include nonionic surfactants, anionic surfactants, cationic surfactants, and amphoteric surfactants. Note that surfactants are different compounds from the metal corrosion inhibitors described above.
[0058] Surfactants often have at least one hydrophobic group selected from the group consisting of an aliphatic hydrocarbon group, an aromatic hydrocarbon group, and a combination thereof. When the hydrophobic group includes an aromatic hydrocarbon group, the number of carbon atoms in the hydrophobic group of the surfactant is preferably 6 or more, more preferably 10 or more. The total number of carbon atoms in the surfactant is preferably 16 to 100. As surfactants, for example, the compounds exemplified in paragraph
[0126] of WO 2022 / 044893 can also be used, the contents of which are incorporated herein by reference.
[0059] - pH Adjuster - The treatment liquid may contain a pH adjuster to adjust and maintain the pH of the treatment liquid. The pH adjuster is a basic compound or an acidic compound that is different from the components that may be contained in the treatment liquid. However, it is permissible to adjust the pH of the treatment liquid by adjusting the amount of each of the above components added.
[0060] A basic compound is a compound that exhibits alkaline properties (a pH greater than 7.0) in an aqueous solution. Examples of basic compounds include basic inorganic compounds, such as alkali metal hydroxides such as sodium hydroxide and potassium hydroxide, and alkaline earth metal hydroxides. An acidic compound is a compound that exhibits acidity (a pH less than 7.0) in an aqueous solution. Examples of acidic compounds include inorganic acids that do not have a reducing function, such as hydrochloric acid, sulfuric acid, sulfurous acid, and boric acid.
[0061] The content of each of the above components in the treatment liquid can be measured by known methods such as gas chromatography-mass spectrometry (GC-MS), liquid chromatography-mass spectrometry (LC-MS), and ion-exchange chromatography (IC).
[0062] (pH) The treatment liquid may be either alkaline or acidic. The pH of the treatment liquid is preferably 5 to 9, and more preferably 6 to 8. The pH of the treatment liquid can be measured using a known pH meter according to a method in accordance with JIS Z8802-1984. The pH is measured at 25°C.
[0063] (Method for preparing treatment liquid) The treatment liquid can be prepared, for example, by mixing the above-mentioned components. Examples of methods for preparing the treatment liquid include adding a reducing agent and, if necessary, optional components such as an antibacterial agent and a metal corrosion inhibitor to a container containing purified pure water, and then stirring to mix the components to prepare the treatment liquid. When adding the components to the container, they may be added all at once, or may be added in multiple portions. The order in which the components are added can be selected as appropriate.
[0064] The stirring device and stirring method used to prepare the treatment solution may be a known device such as a stirrer or disperser. Examples of the stirrer include an industrial mixer, a portable stirrer, a mechanical stirrer, and a magnetic stirrer. Examples of the disperser include an industrial disperser, a homogenizer, an ultrasonic disperser, and a bead mill.
[0065] The mixing of the components in the preparation step of the treatment solution, the purification treatment described below, and the storage of the produced treatment solution are preferably carried out at 5 to 40° C. Preparation, treatment, and / or storage of the treatment solution within the above temperature range allows the performance to be maintained stably for a long period of time.
[0066] It is preferable to perform a purification treatment in advance on one or more of the raw materials used to prepare the treatment solution. Examples of purification treatment include known methods such as distillation, ion exchange, and filtration. The degree of purification is preferably such that the raw material has a purity of 99% by mass or more, and more preferably such that the raw solution has a purity of 99.9% by mass or more. The upper limit is, for example, 99.9999% by mass or less.
[0067] Examples of purification methods include passing the raw material through an ion exchange resin or a reverse osmosis membrane (RO membrane), distilling the raw material, and filtering. The purification method may be a combination of the above purification methods. For example, the raw material may be subjected to primary purification by passing through an RO membrane, followed by secondary purification by passing through a purification device made of a cation exchange resin, an anion exchange resin, or a mixed-bed ion exchange resin. The purification process may also be performed multiple times. The filter used for filtering is not particularly limited as long as it is a filter conventionally used for filtration purposes. Examples include filters made of fluororesins such as polytetrafluoroethylene (PTFE) and tetrafluoroethylene perfluoroalkyl vinyl ether copolymer (PFA), polyamide resins such as nylon, polyallylsulfone (PAS), and polyolefin resins (including high-density or ultra-high molecular weight) such as polyethylene and polypropylene (PP).
[0068] (Dilution) The treatment liquid used in the pretreatment step may be a diluted liquid obtained by diluting a stock solution containing at least a reducing agent before use. The dilution ratio of the stock solution may be adjusted appropriately depending on the type and content of components contained in the stock solution, and for example, the ratio of the treatment liquid (diluted liquid) to the stock solution is preferably 10 to 1000 times, more preferably 15 to 500 times, and even more preferably 20 to 100 times, in volume ratio.
[0069] In the dilution treatment, it is preferable to dilute the stock solution with water. It is preferable to perform a purification treatment on the water used in the dilution treatment in advance. The purification treatment is not particularly limited, and examples thereof include a treatment to reduce ion components using an ion exchange resin or an RO membrane, etc., and a treatment to remove foreign matter using filtering, which are described above as purification treatments for the treatment solution, and it is preferable to perform any one of these treatments.
[0070] The content of the metal corrosion inhibitor in the undiluted stock solution is not particularly limited, as long as the content of the metal corrosion inhibitor in the diluted cleaning solution is 0.01% by mass or less. For example, it may be 0.1% by mass or less, preferably 0.01% by mass or less, relative to the total mass of the stock solution. The lower limit is not particularly limited, and it is preferable that the stock solution is substantially free of the metal corrosion inhibitor. The content of the reducing agent in the stock solution is not particularly limited, but is preferably 0.1 to 5% by mass, more preferably 0.2 to 2% by mass, relative to the total mass of the stock solution. When a treatment solution containing an antibacterial agent is used in the pretreatment step, the content of the antibacterial agent in the stock solution is preferably 0.1 to 5% by mass, more preferably 0.2 to 2% by mass, relative to the total mass of the stock solution. The content of components other than the reducing agent, metal corrosion inhibitor, water, and antibacterial agent in the stock solution is preferably 10% by mass or less, relative to the total mass of the stock solution. It is more preferable that the stock solution is substantially free of components other than the reducing agent, metal corrosion inhibitor, water, and antibacterial agent.
[0071] The pH of the stock solution at 25° C. is preferably 5 to 9, and more preferably 6 to 8. The change in pH before and after dilution (the difference between the pH of the stock solution before dilution and the pH of the diluted treatment solution) is preferably 1.0 or less, and more preferably 0.5 or less.
[0072] The specific method for diluting the stock solution is not particularly limited, and may be carried out in accordance with the above-mentioned method for preparing the treatment solution. The stirring device and stirring method used in the dilution step are also not particularly limited, and may be carried out using the known stirring device mentioned in the above-mentioned method for preparing the treatment solution.
[0073] (Container) The processing solution and the undiluted solution can be filled into any container for storage, transportation, and use, as long as corrosiveness and other issues are not a problem. For semiconductor applications, a container with a high level of cleanliness within the container and that inhibits the elution of impurities from the inner wall of the container into each solution is preferred. Examples of such containers include various containers commercially available as containers for semiconductor processing solutions, such as the "Clean Bottle" series manufactured by Aicello Chemical Co., Ltd. and the "Pure Bottle" manufactured by Kodama Resin Industry Co., Ltd., but are not limited to these. Furthermore, the containers exemplified in paragraphs
[0121] to
[0124] of International Publication No. 2022 / 004217 can also be used, and the contents of these containers are incorporated herein.
[0074] <Treatment Method> The pretreatment method using a treatment liquid is not particularly limited as long as it brings the specific surface of the bonded member, which is the object, into contact with the treatment liquid, and can be carried out by any known method. Examples of methods for bringing the specific surface of the bonded member into contact with the treatment liquid include immersing the bonded member in a container for a certain period of time, continuously supplying the treatment liquid to the specific surface of the bonded member using a discharge nozzle, and combinations of these. The type of discharge nozzle used to supply the treatment liquid is not particularly limited, and examples include a straight nozzle, a shower nozzle, and a spray nozzle. Discharging the treatment liquid from a straight nozzle onto the specific surface of the bonded member is preferred because it results in superior bonding strength of the bonded body. It is believed that discharging the treatment liquid from a straight nozzle can prevent a decrease in the metal component-reducing function of the treatment liquid. In addition, in the above-mentioned pretreatment by spraying or discharging, the treatment liquid may be applied while rotating the bonded member. In the pretreatment by immersion, ultrasonic treatment is preferably performed on the bonded member immersed in the treatment liquid.
[0075] The temperature of the treatment liquid used in the pretreatment step is not particularly limited, but is preferably 10 to 60°C, and more preferably 15 to 50°C. The contact time between the bonding member and the treatment liquid can be appropriately changed depending on the type and content of each component contained in the treatment liquid, but in practice, it is preferably 10 to 120 seconds, and more preferably 20 to 90 seconds. The supply amount (supply rate) when the treatment liquid is discharged is preferably 50 to 5,000 mL / min, and more preferably 200 to 2,000 mL / min.
[0076] In the pretreatment step, the contact of the bonding member with the treatment liquid may be carried out only once or may be carried out two or more times. When the contact is carried out two or more times, the same method may be repeated, or different methods may be combined.
[0077] After the pretreatment, the bonding members may be dried by a drying method such as spin drying, applying a dry gas to a specific surface of the bonding members, heating the bonding members with a heating means such as a hot plate or an infrared lamp, or any combination of these methods.
[0078] The treated bonded members obtained by the pretreatment step (including the drying treatment) are preferably subjected to the bonding step without undergoing any other steps. Between the completion of the pretreatment step including the drying treatment and the start of the bonding step, the treated bonded members are preferably stored and transported in an atmosphere of an inert gas such as nitrogen, or in a reduced pressure atmosphere including a vacuum.
[0079] [Bonding Process] The bonding process is a process of bonding a treated bonding member that has been subjected to a pretreatment process to another bonding member. The bonding process results in a bonded body in which two bonding members are fixed together while ensuring electrical connection between them. In the bonding process, a treated bonding member may be bonded to a bonding member that has not been subjected to a pretreatment process, but it is preferable that treated bonding members are bonded together. In other words, the bonded body is preferably a member in which treated bonding members are bonded together.
[0080] The bonding step will be described with reference to the drawings. Fig. 3 is a schematic cross-sectional view showing an example of the bonding step included in this manufacturing method, and Fig. 4 is a schematic cross-sectional view showing an example of a bonded body obtained by the bonding step shown in Fig. 3. In Figs. 3 and 4, the same components as those in the stacked device 10 and semiconductor element 12 or 14 shown in Fig. 1 or 2 are designated by the same reference numerals, and detailed description thereof will be omitted. However, the semiconductor elements 12 and 14 shown in Figs. 3 and 4 are bonded members that have been subjected to a pretreatment step.
[0081] In the bonding process, first, as shown in Fig. 3, the semiconductor elements 12 and 14 are arranged so that their terminals 30 face each other. More specifically, alignment marks (not shown) provided on the semiconductor elements 12 and 14 are used to align the positions of the terminals 30a and 30b of the semiconductor elements 12 and 14. The process of aligning the positions of the semiconductor elements described above is also called alignment. After alignment, the semiconductor elements 12 and 14 are brought close to each other and brought into contact while maintaining the aligned state.
[0082] Next, the semiconductor elements 12 and 14 are bonded together to obtain the stacked device 10 shown in Fig. 4. In the stacked device 10 shown in Fig. 4, the above-mentioned bonding process results in direct connection between the corresponding terminals 30a and the corresponding terminals 30b. Through the bonding process, the semiconductor elements 12 and 14 are electrically and physically connected to each other via the respective terminals 30a. However, the semiconductor elements 12 and 14 are not electrically connected to each other via the terminals 30b.
[0083] <Bonding Conditions> In the bonding process, two bonding members are bonded under predetermined bonding conditions. The conditions for the bonding process, such as the atmosphere, heating temperature, pressure (load), and processing time, can be appropriately selected depending on the device, such as a semiconductor element, that uses the bonded body to be manufactured. The temperature conditions for the bonding process are not particularly limited, but are preferably 150 to 350°C, more preferably 200 to 300°C. The pressure conditions for the bonding process are not particularly limited, but are preferably 30 MPa or less, more preferably 0.1 to 20 MPa. The duration of the bonding process is not particularly limited, but is preferably 1 second to 60 minutes, more preferably 5 seconds to 10 minutes. Examples of equipment used in the bonding process include wafer bonding equipment from Mitsubishi Heavy Industries Machine Tools, Bondtech, PMT Corporation, Ayumi Industries, Tokyo Electron (TEL), EVG, SUSS Microtec K.K. (SUSS), and Musashino Engineering. The atmosphere for the bonding process can be selected from air, an inert atmosphere such as a nitrogen atmosphere, and a reduced-pressure atmosphere, including a vacuum atmosphere.
[0084] The heating temperature is not particularly limited to the above-mentioned temperature range, and can be selected from various temperatures in the range of 100 to 400°C. The heating rate can also be appropriately selected within a range of 10°C / min to 10°C / sec, depending on the performance of the heating stage or the heating method. The same applies to the cooling temperature and cooling rate. Step heating is also possible, and joining can be performed by sequentially increasing the heating temperature in several stages. The pressure (load) is also not particularly limited to the above-mentioned range, and pressing conditions such as rapid pressing or stepwise pressing can be appropriately selected depending on the physical properties of the objects to be joined, such as the strength.
[0085] The atmosphere, heating, and pressure holding times, as well as the change times, in the bonding process can be set as appropriate. The order of these steps can also be changed as appropriate. For example, a procedure can be established in which a first pressurization step is performed after a vacuum is achieved, followed by heating and a second pressurization step after the temperature is raised, followed by holding the pressure for a certain period of time, unloading and cooling, and then returning to atmospheric pressure once the temperature drops below a certain level. This procedure can be rearranged in various ways, and after pressurization in atmospheric air, heating can be performed in a vacuum state, or vacuuming, pressurization, and heating can be performed simultaneously. In the bonding process, a mechanism for individually controlling the pressure distribution and heat distribution within the plane can be used, which can improve the yield of the bonded product. In the bonding process, ultrasonic waves can also be applied to the bonding surfaces.
[0086] The joining, transporting, picking, etc. of the joining members (semiconductor elements) in the joining step can be achieved by using known semiconductor manufacturing equipment.
[0087] [Other Steps] The present manufacturing method may include steps other than the preparation step, pretreatment step, and bonding step. Examples of the other steps include a cleaning step for cleaning a specific surface of the bonding member, and a singulation step for singulating a semiconductor element having multiple element regions into individual element regions. When the cleaning step is performed, it is preferable to perform the cleaning step after the preparation step and before the pretreatment step.
[0088] <Cleaning Process> Examples of the cleaning process include a method of cleaning a specific surface of the bonding member using a cleaning solution different from the treatment solution used in the pretreatment process. In particular, when the planarization process is performed as a preparatory process, impurities such as metal wiring and barrier metal removed in the planarization process, as well as abrasive particles (silica and alumina) used in the planarization process, may remain on the specific surface of the bonding member. These impurities may cause short circuits between wirings and degrade the electrical properties of the bonding member. In contrast, by performing a cleaning process on a bonding member that has been subjected to a planarization process such as CMP, the above impurities can be removed from the specific surface of the bonding member.
[0089] The cleaning liquid used in the cleaning step is not particularly limited as long as it is a known cleaning liquid (pCMP cleaning liquid) for semiconductor substrates that have been subjected to CMP processing, has a different composition and function from the treatment liquid used in the pretreatment step, and is capable of removing or dissolving the above-mentioned impurities. Examples of cleaning liquids that can be used include those described in JP 2007-269918 A, the contents of which are incorporated herein by reference.
[0090] The method for cleaning the specific surface of the bonded member using a cleaning liquid is not particularly limited as long as it is a method of contacting the specific surface of the bonded member with the cleaning liquid, and can be carried out by any known method. Examples of the method for contacting the specific surface of the bonded member with the cleaning liquid include the methods listed as the method for contacting the treatment liquid with the specific surface of the bonded member in the pretreatment step, including preferred embodiments. The specific surface of the bonded member may also be cleaned by scrubbing, in which a cleaning member such as a brush is physically brought into contact with the specific surface of the bonded member while supplying the cleaning liquid.
[0091] The temperature of the cleaning liquid used in the cleaning step is not particularly limited, but is preferably 10 to 60°C, more preferably 15 to 50°C. The contact time between the bonding members and the cleaning liquid can be appropriately changed depending on the type and content of each component contained in the cleaning liquid, but in practice, it is preferably 10 to 120 seconds, more preferably 20 to 90 seconds. The supply amount (supply rate) when supplying the cleaning liquid to the specific surface of the bonding members is preferably 50 to 5000 mL / min, more preferably 200 to 2000 mL / min.
[0092] After the cleaning, a rinse treatment may be performed in which the bonded members are brought into contact with a rinse liquid. By performing the rinse treatment, the bonded members cleaned in the cleaning step are washed with the rinse liquid, and impurities can be efficiently removed. The rinse treatment is a treatment in which specific surfaces of the bonded members are rinsed with the rinse liquid, and is preferably performed consecutively after the cleaning. The rinse treatment may be performed using the mechanical stirring method described above.
[0093] Examples of the rinse liquid include water (preferably deionized water), methanol, ethanol, isopropyl alcohol (IPA), N-methylpyrrolidinone, γ-butyrolactone, dimethyl sulfoxide, ethyl lactate, and propylene glycol monomethyl ether acetate.
[0094] The method of contacting the bonded members with the rinse liquid can be the same as the method of contacting the bonded members with the treatment liquid. The contact time between the bonded members and the rinse liquid can be changed appropriately depending on the type and content of each component contained in the cleaning liquid. In practice, the contact time is preferably 10 to 120 seconds, more preferably 20 to 90 seconds. The temperature of the rinse liquid is preferably 0 to 50°C, more preferably 15 to 35°C. After the rinse treatment, a drying treatment may be performed to dry the bonded members. The drying treatment performed in the pretreatment step can be similarly applied as the drying treatment.
[0095] The time elapsed from the completion of the cleaning process (including the rinsing and drying processes) for the bonding member to the start of the pretreatment process is preferably 30 seconds or more, more preferably 1 minute or more, and even more preferably 2 minutes or more. This is because if the elapsed time is equal to or greater than the lower limit, the semiconductor wafer can be easily transported. Although the upper limit is not particularly limited, 30 minutes or less is preferred from the viewpoint of shortening the manufacturing time.
[0096] <Bonding Step> When the semiconductor element used as the bonding member has multiple element regions, the manufacturing method may include a singulation step in which the bonding member is divided into individual element regions. The singulation step may be performed by a known method such as dicing or laser scribing. The singulation step may be performed, for example, after the preparation step or the cleaning step. The singulation step may also be performed at any stage before the pretreatment step, before the bonding step, or after the bonding step.
[0097] Although this manufacturing method has been described with reference to Figures 1 to 4, this manufacturing method is not limited to the above. For example, the manufacturing method for the stacked device 10 shown in Figures 2 to 4 is a chip-on-chip manufacturing method, but this manufacturing method may be a chip-on-wafer method in which a semiconductor element and a semiconductor wafer are used as bonding members, or a wafer-on-wafer method in which two semiconductor wafers are used as bonding members.
[0098] A manufacturing method using the chip-on-wafer method will now be described. A semiconductor element used in the chip-on-wafer method is, for example, a semiconductor element having one element region and at least two alignment marks on the surface that indicate the position of the element region. A semiconductor wafer used in the chip-on-wafer method is, for example, a semiconductor wafer having multiple element regions and at least two alignment marks on the surface that indicate the position of each element region.
[0099] First, the semiconductor element and the semiconductor wafer are subjected to the above-mentioned preparation step, the above-mentioned pretreatment step, and an optional cleaning step. Then, the element region of the semiconductor element is bonded to the element region of the semiconductor wafer. The bonding is performed according to the above-mentioned bonding step, but multiple semiconductor elements may be bonded together, or the semiconductor elements may be bonded to the semiconductor wafer one by one. Next, the semiconductor wafer with the bonded semiconductor elements is divided into individual element regions by, for example, dicing or laser scribing. This allows the manufacture of multiple stacked devices each formed by bonding two semiconductor elements. By manufacturing multiple stacked devices together as described above, the takt time can be reduced and productivity can be improved.
[0100] [Stacked Device] The stacked device manufactured by the present manufacturing method is not limited to the configuration shown in Fig. 1 or 4. For example, the stacked device may have a configuration in which three or more semiconductor elements are stacked and joined in the stacking direction Ds, and adjacent semiconductor elements are directly electrically connected to each other. The three or more semiconductor elements constituting the stacked device may have the same configuration or different configurations.
[0101] As described above, this manufacturing method can be used to manufacture a stacked device using a semiconductor element having an element region in which an element configuration circuit and the like are formed and a redistribution layer. Therefore, stacked devices manufactured by this manufacturing method include, for example, a stacked device having a combination of a semiconductor element having a logic circuit and a semiconductor element having a memory circuit, a stacked device in which all semiconductor elements have memory circuits, and a stacked device in which all semiconductor elements have logic circuits. All of these can be manufactured. Furthermore, the combination of semiconductor elements in a stacked device may be a combination of a sensor, actuator, antenna, etc. with a memory circuit and a logic circuit, and is determined appropriately depending on the application of the stacked device.
[0102] The stacked device manufactured by this manufacturing method may be a component that functions as an optical sensor. An example of a stacked device that functions as an optical sensor is a stack in which a semiconductor element and a sensor chip provided with a lens are stacked in the stacking direction Ds. In this case, the semiconductor element is not particularly limited in configuration as long as it has a logic circuit that can process signals obtained by the sensor chip. The sensor chip has an optical sensor that detects light. The optical sensor is not particularly limited as long as it can detect light, and for example, a CCD (Charge Coupled Device) image sensor or a CMOS (Complementary Metal Oxide Semiconductor) image sensor is used. The lens is not particularly limited in configuration as long as it can focus light on the sensor chip, and for example, a component called a microlens is used.
[0103] The method for manufacturing a bonded body of the present invention has been described in detail above, but the present invention is not limited to the above-described embodiment, and various improvements or modifications may be made within the scope of the gist of the present invention.
[0104] The features of the present invention will be explained in more detail below with reference to examples. The materials, reagents, amounts and proportions of substances, and procedures shown in the following examples can be changed as appropriate without departing from the spirit of the present invention. Therefore, the scope of the present invention is not limited to the following examples.
[0105] <Preparation of Treatment Solution> The following compounds were used to prepare the treatment solution. Note that all of the components used in the examples were classified as semiconductor grade or equivalent high purity grade.
[0106] (Water) ・Pure water (reducing agent) ・Ammonium thiosulfate ・Potassium nitrite ・Ascorbic acid ・Formic acid ・Oxalic acid ・3,4,5-trihydroxybenzoic acid ・Glucose ・Ammonium thiosulfate (antibacterial agent) ・TMAB (tetramethylammonium bromide) ・Sorbic acid ・CMI (5-chloro-2-methyl-4-isothiazolin-3-one) ・Chlorhexidine hydrochloride ・Benzalkonium chloride ・Cresol (metal corrosion inhibitor) ・Benzotriazole (other ingredients) ・Sulfuric acid
[0107] Ammonium thiosulfate and TMAB were added to pure water in amounts to give the composition shown in Table 1, and the resulting mixture was thoroughly stirred to obtain treatment solution 1. Treatment solutions 2 to 10 and treatment solutions C1 and C2, each having the composition shown in Table 1, were prepared according to the method described above, except that the type and amount of each component was changed to give the composition shown in Table 1.
[0108] Example 1 Preparation of Bonding Member A Ta film having a thickness of 20 nm was formed on the surface of an 8-inch diameter silicon wafer by sputtering. Subsequently, a copper film having a thickness of 50 nm was formed on the Ta film by sputtering, and then a copper film having a total thickness of 1000 nm was formed by plating, thereby producing a silicon wafer for evaluation having a Ta film and a copper film in this order on the silicon wafer.
[0109] (Planarization Step (Preparation Step)) A Kemet "ARW-681MSII" polishing apparatus was used, and a copper film provided on a silicon wafer was polished while supplying a slurry under the following conditions to perform a planarization step (CMP). Target substrate: silicon wafer with Ta film and copper film; Table rotation speed: 104 rpm; Head rotation speed: 105 rpm; Polishing pressure: 6.9 kPa; Polishing pad: Rohm and Haas "IC-1400 (K-grv)+(A21)"; Slurry supply rate: 200 mL / min. The metal polishing liquid described in Example 1 of JP 2009-260304 A was used as the slurry. The slurry was prepared by adding the following components in the amounts indicated below to water to make a total amount of 100% by mass, mixing and stirring, and adjusting the pH to 6.0 with ammonia gas. Colloidal silica (Fuso Chemical Co., Ltd.: PL-2H): 0.010% by mass Metal corrosion inhibitor (1-(1,2-dicarboxyethyl)benzothiazole): 0.050% by mass Surfactant (polyoxyethylene alkyl ether): 0.1% by mass Hydrogen peroxide solution: 1.0% by mass Glycine: 1.0% by mass
[0110] The maximum height of the surface was measured at any five points on the copper film surface planarized by the above-mentioned planarization process using an atomic force microscope in accordance with JIS B 0601. The maximum height Rmax of the surface where the conductive portion subjected to the planarization process was exposed was determined by arithmetically averaging the obtained measurements, and the maximum height Rmax was 4 nm. Furthermore, the surface roughness was measured at any five points on the surface of the copper film planarized by the above-mentioned planarization process using an atomic force microscope in accordance with JIS B 0601. The surface roughness Ra of the surface where the conductive portion subjected to the planarization process was exposed was determined by arithmetically averaging the obtained measurements, and the surface roughness Ra was 1 nm.
[0111] (Washing Step) A washing solution to be used in the washing step was prepared according to the method described in Example 1 of JP-A-2007-269918.
[0112] The planarized silicon wafer was subjected to scrubbing for 25 seconds by supplying the diluted cleaning solution while contacting the surface of the silicon wafer with a PVA roll brush connected to a scrubbing unit built into a Kemet wafer cleaner "ZAB-8S1M-ODW." The supply rate of the diluted cleaning solution to the planarized surface was 650 mL / min. The supply rate of the diluted cleaning solution to the surface opposite the planarized surface of the silicon wafer was 500 mL / min. After the scrubbing, the silicon wafer was rinsed for 35 seconds using pure water (deionized water). The supply rate of the pure water to the planarized surface of the silicon wafer was 650 mL / min, and the supply rate of the pure water to the surface opposite the planarized surface of the silicon wafer was 500 mL / min. The silicon wafer was then dried for 30 seconds using a spin dryer built into the cleaner.
[0113] (Pretreatment Step) A photolithography apparatus (manufactured by Takizawa Sangyo Co., Ltd., product name "ED-3000") was prepared, in which a straight nozzle (manufactured by Ikeuchi Co., Ltd., product name "CCP") was connected to a discharge port. The silicon wafer was placed in this apparatus, and while the silicon wafer was being rotated at 300 rpm, treatment liquid 1 was discharged from the straight nozzle onto the planarized surface of the silicon wafer, thereby performing a pretreatment step, thereby obtaining a treated wafer. In the pretreatment step, the discharge rate of treatment liquid 1 from the straight nozzle was 450 ml / min, and the time for which treatment liquid 1 was supplied was 1 minute. Furthermore, in the cleaning step, the time from the end of the drying process to the start of the pretreatment step was 1 minute.
[0114] (Bonding Step) The processed wafer obtained by the pretreatment step described above was diced to produce a first sample cut into a 10 mm square size and a second sample cut into a 4 mm square size. In a bonding device ("FC-3000" manufactured by Toray Engineering Co., Ltd.), the first sample and the second sample were placed one above the other, with the surfaces that had been subjected to the pretreatment step facing each other. The bonding step was carried out by applying heat and pressure for 10 minutes under conditions of a load of 800 N and a temperature of 250°C. Subsequently, an annealing treatment was carried out in an oven at 300°C for 2 hours in a nitrogen atmosphere, thereby obtaining the bonded body of Example 1.
[0115] Example 2 A bonded body of Example 2 was obtained by performing the pretreatment step under the same conditions as in Example 1, except that in the pretreatment step of Example 1, a spray nozzle (manufactured by IKEUCHI CO., LTD., product name "VP") was connected to the outlet of the photolithography device instead of the straight nozzle.
[0116] <Examples 3 to 11, Comparative Examples 1 and 2> The bonding members of Examples 3 to 11 and Comparative Examples 1 and 2 were each manufactured according to the method of Example 1, except that the pretreatment step was carried out using the treatment liquids shown in Table 1.
[0117] <Evaluation> The bond strength was measured for each of the bonded structures produced in the examples and comparative examples. The bond strength was evaluated by measuring the shear strength using a universal bond tester Dage-4000 (manufactured by Nordson Advanced Technologies Co., Ltd.). The bond strength per area of the semiconductor element was calculated from the obtained fracture load. The bond strength measurement results are shown in Table 1 below.
[0118]
[0119] As shown in Table 1, Examples 1 to 11 had superior bonding strengths of the resulting bonded bodies compared to Comparative Example 1, in which the pretreatment step was carried out using a treatment liquid containing no reducing agent, and Comparative Example 2, in which the pretreatment step was carried out using a treatment liquid containing 0.1 mass % of a metal corrosion inhibitor relative to the total mass of the treatment liquid.
[0120] It was confirmed that when the treatment liquid was ejected from a straight nozzle in the pretreatment step, the bonding strength of the resulting bonded body was superior to that when the treatment liquid was ejected from a spray nozzle (comparison between Example 1 and Example 2).
[0121] It was confirmed that when the treatment liquid used in the pretreatment step contained an antibacterial agent, the bonding strength of the resulting bonded body was superior compared to when the treatment liquid did not contain an antibacterial agent (comparison between Example 1 and Example 3).
[0122] It was confirmed that when the treatment liquid used in the pretreatment step did not contain a metal corrosion inhibitor, the bonding strength of the resulting bonded body was superior to that when the treatment liquid contained a metal corrosion inhibitor (comparison between Example 3 and Example 11).
[0123] REFERENCE SIGNS LIST 10 Stacked device (bonded body) 12, 14 Semiconductor element (bonded member) 30, 30a, 30b Terminal 30c End face 32 Semiconductor layer 32a, 34a, 36a Surface 34 Rewiring layer 36 Passivation layer 37 Wiring 38 Pad Ds Stacking direction
Claims
1. A method for producing a joined body, comprising: a preparation step of preparing a joining member having a maximum surface height Rmax of 50 nm or less; a pretreatment step of contacting a treatment liquid with the surface of the joining member; and a joining step of joining the treated joining member that has been subjected to the pretreatment step to another joining member, wherein a conductive part and an insulating part containing metal are exposed on the surface of the joining member, the treatment liquid contains a reducing agent, and the content of a metal corrosion inhibitor contained in the treatment liquid is 0.01 mass % or less relative to the total mass of the treatment liquid.
2. The method for manufacturing a bonded body according to claim 1, wherein in the pretreatment step, the treatment liquid is supplied to the surfaces of the bonded members by being discharged from a straight nozzle.
3. The method for producing a bonded body according to claim 1 or 2, further comprising a cleaning step of cleaning the surfaces of the bonding members after the preparation step and before the pretreatment step.
4. The method for producing a bonded body according to claim 3, wherein the time elapsed from the completion of the cleaning step until the start of the pretreatment step is one minute or more.
5. The method for producing a conjugate according to claim 1 or 2, wherein the reducing agent includes at least one selected from the group consisting of inorganic acid reducing agents, organic acid reducing agents, and sugars.
6. The method for producing a bonded body according to claim 1 or 2, wherein the maximum height Rmax of the surface of the bonding member is 10 nm or less.
7. The method for manufacturing a bonded body according to claim 1 or 2, wherein the surface roughness Ra of the surface of the bonding member is 1 nm or less.
8. The method for manufacturing a joint body according to claim 1 or 2, wherein the surface area of the joint member where the insulating portion is exposed has a contact angle with water of 30 degrees or less.
9. The method for producing a bonded body according to claim 1 or 2, wherein the bonding member comprises a plurality of element regions, and further comprising, after the preparation step, a singulation step of singulating the bonding member into individual pieces for each of the element regions.
10. The method for producing a joint body according to claim 1 or 2, wherein the reducing agent includes an inorganic acid reducing agent.
11. The method for producing a joint body according to claim 10, wherein the inorganic acid reducing agent comprises at least one selected from the group consisting of nitrous acid and its salts, sulfurous acid and its salts, and thiosulfuric acid and its salts.
12. The method for producing a joint body according to claim 1 or 2, wherein the reducing agent includes an organic acid-based reducing agent.
13. The method for producing a conjugate according to claim 12, wherein the organic acid reducing agent includes at least one selected from the group consisting of ascorbic acid, formic acid, oxalic acid, 3,4,5-trihydroxybenzoic acid, and salts thereof.
14. The method for producing a joint body according to claim 1 or 2, wherein the treatment liquid further contains an antibacterial agent.
15. The method for producing a conjugate according to claim 14, wherein the antibacterial agent is a compound having at least one quaternary ammonium cationic group in the molecule, or a salt thereof.
16. The method for producing a joint body according to claim 1 or 2, wherein the conductive portion is made of copper or a copper alloy.
17. A treatment liquid used for treatment in contact with a surface of a joining member, the treatment liquid containing a reducing agent, the content of a metal corrosion inhibitor being 0.01 mass% or less relative to the total mass of the treatment liquid, the joining member being a joining member used for manufacturing a joined body by joining a treated joining member obtained by carrying out the treatment to another joining member, a conductive part and an insulating part containing metal being exposed on the surface of the joining member, and the maximum height Rmax of the surface of the joining member being 50 nm or less.
18. The treatment liquid according to claim 17, wherein the reducing agent includes at least one selected from the group consisting of inorganic acid reducing agents, organic acid reducing agents, and sugars.
19. The treatment liquid according to claim 18, wherein the inorganic acid reducing agent comprises at least one selected from the group consisting of nitrous acid and its salts, sulfurous acid and its salts, and thiosulfuric acid and its salts.
20. The treatment liquid according to claim 18, wherein the organic acid reducing agent comprises at least one selected from the group consisting of ascorbic acid, formic acid, oxalic acid, 3,4,5-trihydroxybenzoic acid, and salts thereof.
21. The treatment solution according to any one of claims 17 to 20, further comprising an antibacterial agent.
22. The treatment solution according to claim 21, wherein the antibacterial agent is a compound having at least one quaternary ammonium cationic group in the molecule, or a salt thereof.
23. A method for treating a joining member used for producing a joined body, the joining member having a surface on which a conductive part and an insulating part containing metal are exposed and having a maximum height Rmax of 50 nm or less, the method comprising contacting the surface of the joining member with a treatment liquid containing a reducing agent and having a metal corrosion inhibitor content of 0.01 mass% or less relative to the total mass.
24. The method according to claim 23, wherein the treatment liquid is supplied to the surface of the joining member by being discharged from a straight nozzle.
Citation Information
Patent Citations
Semiconductor device, semiconductor device manufacturing method and electronic apparatus
JP2013038112A
Semiconductor device and manufacturing method for the same
JP2023177917A
Manufacturing method of the structure
JP7220796B2
Semiconductor device, laminate, semiconductor device manufacturing method, and laminate manufacturing method
WO2018159186A1
Composition for forming polyimide-containing part, joined body manufacturing method, joined body, device manufacturing method and device
WO2022244717A1
Cited By
Core substrate, substrate, and method for manufacturing substrate
WO2026216594A1