Optical laminate and image display device

The optical laminate structure with specific adhesive and optical film layers addresses the issue of display defects in image display devices by dispersing pressure and reducing stress on the optical films, ensuring robustness against minor collisions or narrow contact pressures.

WO2024203043A1PCT designated stage expired Publication Date: 2024-10-03NITTO DENKO CORP
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/008361
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-31
Filing Date
2024-03-05
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Image display devices using optical laminates are prone to display defects when subjected to pressure from small objects colliding with the screen or pressing with a narrow contact area, due to damage to the optical films within the laminate.

Method used

An optical laminate structure comprising a first optical film, a first adhesive sheet with a thickness of 30 μm to 1000 μm and elongation at break of 500% or less, a second optical film, and a second adhesive sheet, where the first adhesive sheet is formed from a photocurable or solvent-based adhesive composition, and the second optical film includes multiple layers with a polarizer and at least one film having a photoelastic coefficient of 4×10^-11 m^2/N or less.

Benefits of technology

This configuration effectively disperses pressure and reduces stress on the second optical film, thereby suppressing display defects and appearance issues in image display devices, even under conditions of minor collisions or narrow contact pressures.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024008361_03102024_PF_FP_ABST
    Figure JP2024008361_03102024_PF_FP_ABST
Patent Text Reader

Abstract

Provided is an image display device produced using an optical laminate. The optical laminate is suitable for preventing display failure, even if a small object impacts a screen or presses against the screen, the surface-area of contact being narrow. The optical laminate has a configuration in which the following are laminated in the order given: a first optical film; a first adhesive sheet; a second optical film; and a second adhesive sheet. The thickness T1 of the first adhesive sheet is 30 μm to 1000 μm. In addition, the elongation-to-break of the first adhesive sheet is 500% or less.
Need to check novelty before this filing date? Find Prior Art

Description

Optical laminate and image display device

[0001] The present invention relates to an optical laminate and an image display device.

[0002] In recent years, image display devices, such as liquid crystal display devices and electroluminescence (EL) display devices (e.g., organic EL display devices and inorganic EL display devices), have rapidly become popular. These various image display devices have a laminated structure of, for example, an image display cell, such as a liquid crystal cell or an EL light-emitting element, and an optical laminate. The optical laminate includes an optical film, such as a retardation film and a polarizing film, and a pressure-sensitive adhesive sheet. The pressure-sensitive adhesive sheet is mainly used to bond between films included in the optical laminate, or to bond the image display cell and the optical laminate.

[0003] Patent Document 1 discloses a pressure-sensitive adhesive composition for optical films, and an optical film having a pressure-sensitive adhesive layer obtained from this composition on at least one surface thereof.

[0004] JP 2012-158702 A

[0005] When an image display device is used or transported, a large load may be applied to the image display device due to a small object colliding with or pressing against the screen over a small contact area. When such a load is applied to an image display device manufactured using an optical laminate, damage may occur to the optical film included in the optical laminate. Damage to the optical laminate may cause display defects in the image display device.

[0006] Therefore, an object of the present invention is to provide an optical laminate that is suitable for suppressing display defects in an image display device manufactured using the optical laminate, even when a small object collides with or presses the screen over a small contact area.

[0007] The present invention provides an optical laminate comprising a first optical film, a first adhesive sheet, a second optical film, and a second adhesive sheet laminated in this order, wherein the thickness T1 of the first adhesive sheet is 30 μm or more and 1000 μm or less, and the breaking elongation of the first adhesive sheet is 500% or less.

[0008] The present invention further provides an image display device comprising the above optical laminate.

[0009] According to the present invention, an optical laminate can be provided that is suitable for suppressing display defects in an image display device manufactured using an optical laminate, even when a small object collides with or presses the screen with a small contact area.

[0010] FIG. 1 is a cross-sectional view schematically showing an example of an optical laminate according to the present embodiment. FIG. 2 is a schematic view illustrating an example of a method for manufacturing a first pressure-sensitive adhesive sheet. FIG. 3 is a schematic view illustrating another example of a method for manufacturing a first pressure-sensitive adhesive sheet. FIG. 4A is a cross-sectional view schematically showing an example of a second optical film. FIG. 4B is a cross-sectional view schematically showing another example of a second optical film. FIG. 5 is a cross-sectional view schematically showing another example of an optical laminate according to the present embodiment. FIG. 6 is a cross-sectional view schematically showing an example of an image display device according to the present embodiment. FIG. 7 is a cross-sectional view schematically showing optical laminates according to Examples 1 to 4 and 6, and Comparative Examples 1 to 4. FIG. 8 is a cross-sectional view schematically showing an optical laminate according to Example 5.

[0011] The optical laminate according to a first aspect of the present invention is an optical laminate in which a first optical film, a first adhesive sheet, a second optical film, and a second adhesive sheet are laminated in this order, wherein the thickness T1 of the first adhesive sheet is 30 μm or more and 1000 μm or less, and the breaking elongation of the first adhesive sheet is 500% or less.

[0012] In a second aspect of the present invention, for example, in the optical laminate according to the first aspect, the first adhesive sheet is formed from a photocurable adhesive composition (I) containing a monomer group and / or a partial polymer of the monomer group.

[0013] In a third aspect of the present invention, for example, in the optical laminate according to the second aspect, the photocurable pressure-sensitive adhesive composition (I) contains a crosslinking agent, and the amount of the crosslinking agent in the photocurable pressure-sensitive adhesive composition (I) is 0.4 parts by weight or more and 20 parts by weight or less, relative to 100 parts by weight in total of the monomer group and the partially polymerized product.

[0014] In a fourth aspect of the present invention, for example, in the optical laminate according to any one of the first to third aspects, the thickness T of the optical laminate is 200 μm or more.

[0015] In a fifth aspect of the present invention, for example, in the optical laminate according to any one of the first to fourth aspects, the second optical film includes a plurality of layers, the plurality of layers include a polarizer and at least one film disposed between the polarizer and the second pressure-sensitive adhesive sheet, and the photoelastic coefficient of the at least one film is 4×10 -11 m 2 / N or less.

[0016] An image display device according to a sixth aspect of the present invention includes the optical laminate according to any one of the first to fifth aspects.

[0017] The present invention will be described in detail below, but the present invention is not limited to the following embodiments and can be implemented in any modified form without departing from the gist of the present invention.

[0018] First, the meanings of terms used in this specification will be explained. "Main surface" refers to the surface of a film or layer having the largest area. "(Meth)acrylic" refers to acrylic and methacrylic. For example, "(meth)acrylate" refers to acrylate and methacrylate. "Main component" refers to the component with the largest content in a composition. "Substantially free" means that the content of a substance such as a compound, polymer, or solvent is, for example, 0.1 wt% or less, preferably 0.05 wt% or less, and more preferably 0.01 wt% or less. "Main unit" refers to a unit that accounts for 50 wt% or more, preferably 60 wt% or more, more preferably 70 wt% or more, and even more preferably 80 wt% or more of all structural units contained in a polymer. "Long-chain alkyl group" refers to an alkyl group having 6 to 30 carbon atoms. "Substantially parallel" means that the angle between two directions is 0°±7°, preferably 0°±5°, and more preferably 0°±3°. "Substantially perpendicular" means that the angle between the two directions is 90°±7°, preferably 90°±5°, and more preferably 90°±3°.

[0019] [Embodiment of Optical Laminate] The optical laminate according to this embodiment includes a first optical film, a first pressure-sensitive adhesive sheet, a second optical film, and a second pressure-sensitive adhesive sheet laminated in this order. The thickness T1 of the first pressure-sensitive adhesive sheet is 30 μm or more and 1000 μm or less. In addition, the breaking elongation of the first pressure-sensitive adhesive sheet is 500% or less.

[0020] 1 is a cross-sectional view schematically illustrating an example of an optical laminate according to the present embodiment. The optical laminate 10A includes a first optical film 1, a first adhesive sheet 2, a second optical film 3, and a second adhesive sheet 4. The optical laminate 10A has a structure in which the first optical film 1, the first adhesive sheet 2, the second optical film 3, and the second adhesive sheet 4 are laminated in this order.

[0021] The first optical film 1 is in contact with the first pressure-sensitive adhesive sheet 2. The first optical film 1 is disposed in contact with one main surface of the first pressure-sensitive adhesive sheet 2. In FIG. 1 , the first optical film 1 is in contact with the entire one main surface of the first pressure-sensitive adhesive sheet. However, the first optical film 1 may be in contact with only a portion of one main surface of the first pressure-sensitive adhesive sheet 2.

[0022] The first adhesive sheet 2 is formed on the second optical film 3. The first adhesive sheet 2 is formed on one main surface of the second optical film 3. In FIG. 1 , the first adhesive sheet 2 is formed on the entire one main surface of the second optical film 3. However, the first adhesive sheet 2 may be formed on only a portion of one main surface of the second optical film 3.

[0023] The second adhesive sheet 4 is formed on the second optical film 3. Specifically, the second adhesive sheet 4 is formed on the main surface of the second optical film 3 opposite to the main surface on which the first adhesive sheet 2 is formed. In Fig. 1 , the second adhesive sheet 4 is formed on the entire one main surface of the second optical film 3. However, the second adhesive sheet 4 may be formed on only a portion of one main surface of the second optical film 3.

[0024] (First Pressure-Sensitive Adhesive Sheet) As described above, the thickness T1 of the first pressure-sensitive adhesive sheet 2 is 30 μm or more and 1000 μm or less, preferably 40 μm or more and 800 μm or less, more preferably 45 μm or more and 700 μm or less, even more preferably 50 μm or more and 500 μm or less, and particularly preferably 80 μm or more and 300 μm or less. By having the thickness T1 of the first pressure-sensitive adhesive sheet 2 be 30 μm or more and 1000 μm or less, even if strong pressure is applied in the thickness direction of the optical laminate 10A, this pressure can be dispersed. Therefore, the stress applied to the second optical film 3 is less likely to be large, and damage to the second optical film 3 can be further suppressed. As a result, the optical laminate 10A can suppress display defects.

[0025] As described above, the breaking elongation of the first adhesive sheet 2 is 500% or less, preferably 400% or less, more preferably 350% or less, even more preferably 200% or less, and particularly preferably 100% or less. The lower limit of the breaking elongation of the first adhesive sheet 2 is, for example, 10%. When the breaking elongation of the first adhesive sheet 2 is 500% or less, the first adhesive sheet 2 is less likely to deform even when strong pressure is applied in the thickness direction of the optical laminate 10A. As a result, damage to the second optical film 3 can be further suppressed.

[0026] The first adhesive sheet 2 is formed from a photocurable pressure-sensitive adhesive composition (I) or a solvent-based pressure-sensitive adhesive composition (II). The photocurable pressure-sensitive adhesive composition (I) is a pressure-sensitive adhesive composition that forms the first adhesive sheet 2 by being irradiated with light. The solvent-based pressure-sensitive adhesive composition (II) is, for example, a pressure-sensitive adhesive composition containing a polymer and a solvent. The photocurable pressure-sensitive adhesive composition (I) and the solvent-based pressure-sensitive adhesive composition (II) are described in detail below.

[0027] (Photocurable Pressure-Sensitive Adhesive Composition) The photocurable pressure-sensitive adhesive composition (I) contains, for example, a group of monomers and / or a partial polymer of the monomers. The group of monomers in the photocurable pressure-sensitive adhesive composition (I) preferably contains a (meth)acrylic monomer. The photocurable pressure-sensitive adhesive composition (I) may contain a (meth)acrylic component, i.e., a (meth)acrylic monomer and its polymer, as a main component. That is, the content of the (meth)acrylic monomer and its partial polymer in the photocurable pressure-sensitive adhesive composition (I) may be 50% by weight or more, 60% by weight or more, 70% by weight or more, or even 80% by weight or more. In this case, a (meth)acrylic first pressure-sensitive adhesive sheet 2 containing a (meth)acrylic polymer and its crosslinked product as a main component can be formed. However, the photocurable pressure-sensitive adhesive composition (I) is not limited to the above examples.

[0028] An example of the (meth)acrylic monomer is a (meth)acrylic acid alkyl ester having an alkyl group having 1 to 20 carbon atoms on the side chain. The number of carbon atoms in the alkyl group may be 7 or less, 6 or less, 5 or less, or even 4 or less. The alkyl group may be linear or branched. Examples of the (meth)acrylic acid alkyl ester include methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, isopropyl (meth)acrylate, n-butyl (meth)acrylate, s-butyl (meth)acrylate, t-butyl (meth)acrylate, isobutyl (meth)acrylate, n-pentyl (meth)acrylate, isopentyl (meth)acrylate, n-hexyl (meth)acrylate, isohexyl (meth)acrylate, isoheptyl (meth)acrylate, and 2-ethylhexyl (meth)acrylate. acrylate, n-octyl(meth)acrylate, isooctyl(meth)acrylate, n-nonyl(meth)acrylate, isononyl(meth)acrylate, n-decyl(meth)acrylate, isodecyl(meth)acrylate, n-dodecyl(meth)acrylate (lauryl(meth)acrylate), n-tridecyl(meth)acrylate, n-tetradecyl(meth)acrylate, pentadecyl(meth)acrylate, hexadecyl(meth)acrylate, heptadecyl(meth)acrylate, and octadecyl(meth)acrylate. The (meth)acrylic acid alkyl ester may be n-butyl(meth)acrylate.

[0029] The amount of the (meth)acrylic acid alkyl ester blended per 100 parts by weight of the monomer group may be, for example, 40 parts by weight or more, 50 parts by weight or more, 60 parts by weight or more, 70 parts by weight or more, 80 parts by weight or more, 85 parts by weight or more, 90 parts by weight or more, or even 95 parts by weight or more. In calculating the blending amount of a specific monomer, the weight of the partially polymerized product is converted into the weight of each monomer before polymerization.

[0030] The monomer group may include a carboxyl group-containing monomer. The carboxyl group-containing monomer may be a (meth)acrylic monomer; in other words, the (meth)acrylic monomer may include a carboxyl group-containing monomer. Examples of carboxyl group-containing monomers include (meth)acrylic acid, carboxyethyl (meth)acrylate, carboxypentyl (meth)acrylate, itaconic acid, maleic acid, fumaric acid, and crotonic acid. The amount of the carboxyl group-containing monomer per 100 parts by weight of the monomer group may be, for example, 10 parts by weight or less, 9 parts by weight or less, 8 parts by weight or less, 7 parts by weight or less, 6 parts by weight or less, 5 parts by weight or less, 4.8 parts by weight or less, 4 parts by weight or less, 3 parts by weight or less, 2 parts by weight or less, 1 part by weight or less, or even 0.5 parts by weight or less. The lower limit of the amount may be, for example, 0.1 parts by weight or more, and in some cases, 0.5 parts by weight or more. The monomer group may not contain a carboxyl group-containing monomer.

[0031] The monomer group may contain a hydroxy group-containing monomer. The hydroxy group-containing monomer may be a (meth)acrylic monomer, in other words, the (meth)acrylic monomer may contain a hydroxy group-containing monomer. The hydroxy group-containing monomer may contribute to improving the cohesive strength of the PSA sheet. Examples of hydroxy group-containing monomers are 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, 6-hydroxyhexyl (meth)acrylate, 8-hydroxyoctyl (meth)acrylate, 10-hydroxydecyl (meth)acrylate, 12-hydroxylauryl (meth)acrylate, and (4-hydroxymethylcyclohexyl)-methyl acrylate. The hydroxy group-containing monomer is preferably 2-hydroxyethyl (meth)acrylate or 4-hydroxybutyl (meth)acrylate. The amount of the hydroxy group-containing monomer blended per 100 parts by weight of the monomer group may be, for example, 20 parts by weight or less, 15 parts by weight or less, 10 parts by weight or less, 7.5 parts by weight or less, 5 parts by weight or less, 4 parts by weight or less, 3 parts by weight or less, 2 parts by weight or less, 1 part by weight or less, or even 0.5 parts by weight or less. The lower limit of the blended amount may be, for example, 0.01 parts by weight or more, 0.03 parts by weight or more, or even 0.05 parts by weight or more. The monomer group may not contain a hydroxy group-containing monomer.

[0032] The monomer group may include an ether group-containing monomer. The ether group-containing monomer may be a (meth)acrylic monomer, in other words, the (meth)acrylic monomer may include an ether group-containing monomer. The ether group-containing monomer can contribute to improving the adhesive strength between the first optical film 1 and the first pressure-sensitive adhesive sheet 2.

[0033] The ether group-containing monomer is preferably an alkoxy group-containing monomer. Examples of the alkoxy group-containing monomer include alkylene oxide adducts represented by the following chemical formula (1): R in formula (1) 1 is a hydrogen atom or a methyl group. 2 is an alkyl group. The alkyl group may be linear or branched. 2is preferably a linear alkyl group. 2 Examples of n are a methyl group and an ethyl group. In formula (1), n ​​is an integer of 1 to 30, preferably an integer of 1 to 12, and more preferably an integer of 1 to 5.

[0034] Examples of the alkylene oxide adduct represented by formula (1) are 2-methoxyethyl (meth)acrylate, 2-ethoxyethyl (meth)acrylate, 2-(2-ethoxyethoxy)ethyl (meth)acrylate, methoxytriethylene glycol (meth)acrylate, and methoxypolyethylene glycol (meth)acrylate, and preferably 2-methoxyethyl acrylate (MEA).

[0035] The ether group-containing monomer is not limited to the alkylene oxide adduct. The ether group-containing monomer may have a ring structure, and the ring structure may have an ether group. Examples of the ring structure having an ether group include a tetrahydrofuran ring and a dioxane ring. Examples of the ether group-containing monomer having a ring structure include cyclic trimethylolpropane formal (meth)acrylate and tetrahydrofurfuryl (meth)acrylate.

[0036] The amount of the ether group-containing monomer blended per 100 parts by weight of the monomer group is, for example, 1 part by weight or more, and may be 5 parts by weight or more, 10 parts by weight or more, 20 parts by weight or more, 25 parts by weight or more, 30 parts by weight or more, 40 parts by weight or more, 50 parts by weight or more, 60 parts by weight or more, 70 parts by weight or more, 80 parts by weight or more, or even 90 parts by weight or more. The upper limit of the blended amount is, for example, 99 parts by weight or less, and in some cases may be 50 parts by weight or less. The monomer group may not contain an ether group-containing monomer.

[0037] In the photocurable pressure-sensitive adhesive composition (I), each of the above-mentioned monomers may be contained as a partial polymer. The partial polymer may be either a homopolymer or a copolymer. The partial polymer can appropriately increase the viscosity of the photocurable pressure-sensitive adhesive composition (I), thereby contributing to the stable formation of a coating layer, which will be described later.

[0038] The photocurable pressure-sensitive adhesive composition (I) usually contains a photopolymerization initiator. Examples of the photopolymerization initiator include a photoradical generator that generates radicals when exposed to visible light and / or ultraviolet light having a wavelength shorter than 450 nm.

[0039] Examples of the photopolymerization initiator include benzoin ethers such as benzoin methyl ether, benzoin isopropyl ether, and benzil dimethyl ketal; substituted benzoin ethers such as anisole methyl ether; substituted acetophenones such as 2,2-diethoxyacetophenone and 2,2-dimethoxy-2-phenylacetophenone; α-hydroxyalkylphenones such as 1-hydroxycyclohexyl-phenyl ketone; substituted alpha-ketol such as 2-methyl-2-hydroxypropiophenone; aromatic sulfonyl chlorides such as 2-naphthalenesulfonyl chloride; photoactive oximes such as 1-phenyl-1,1-propanedione-2-(o-ethoxycarbonyl)-oxime; and benzophenone compounds such as benzophenone, benzoylbenzoic acid, methyl benzoylbenzoate, 4-phenylbenzophenone, hydroxybenzophenone, acrylated benzophenone, 4-benzoyl-4'-methyldiphenyl sulfide, and 3,3',4,4'-tetra(t-butylperoxycarbonyl)benzophenone. Thioxanthone compounds such as thioxanthone, 2-chlorothioxanthone, 2-methylthioxanthone, isopropylthioxanthone, 2,4-diisopropylthioxanthone, and 2,4-diethylthioxanthone; 2,4,6-trichloro-s-triazine, 2-phenyl-4,6-bis(trichloromethyl)-s-triazine, 2-(p-methoxyphenyl)-4,6-bis(trichloromethyl)-s-triazine, and 2-(p-tolyl)-4,6-bis(trichloromethyl)-s-triazine , 2-piperonyl-4,6-bis(trichloromethyl)-s-triazine, 2,4-bis(trichloromethyl)-6-styryl-s-triazine, 2-(naphth-1-yl)-4,6-bis(trichloromethyl)-s-triazine, 2-(4-methoxy-naphth-1-yl)-4,6-bis(trichloromethyl)-s-triazine, 2,4-trichloromethyl-(piperonyl)-6-triazine, 2,4-trichloromethyl-(4'-methoxystyryl)-6-triazine and other triazine-based compounds;Oxime ester compounds such as 1,2-octanedione, 1-[4-(phenylthio)-, 2-(O-benzoyloxime)], O-(acetyl)-N-(1-phenyl-2-oxo-2-(4'-methoxy-naphthyl)ethylidene)hydroxylamine; phosphine compounds such as bis(2,4,6-trimethylbenzoyl)phenylphosphine oxide and 2,4,6-trimethylbenzoyldiphenylphosphine oxide; quinone compounds such as 9,10-phenanthrenequinone, camphorquinone, and ethylanthraquinone; borate compounds; carbazole compounds; imidazole compounds; and titanocene compounds. The photocurable pressure-sensitive adhesive composition (I) may contain one or more photopolymerization initiators.

[0040] The amount of the photopolymerization initiator in the photocurable pressure-sensitive adhesive composition (I) is, for example, 0.02 to 10 parts by weight, and may be 0.05 to 5 parts by weight, relative to 100 parts by weight of the total of the monomer group and its partial polymer.

[0041] The photocurable pressure-sensitive adhesive composition (I) may contain a crosslinking agent. An example of the crosslinking agent is a polyfunctional monomer having two or more polymerizable functional groups in one molecule. The polyfunctional monomer may be a (meth)acrylic monomer. Examples of the polyfunctional monomer are a monomer having two or more C=C bonds in one molecule, and a monomer having one or more C=C bonds and one or more polymerizable functional groups such as epoxy groups, aziridine groups, oxazoline groups, hydrazine groups, or methylol groups in one molecule. The polyfunctional monomer is preferably a monomer having two or more C=C bonds in one molecule.

[0042] Examples of the polyfunctional monomer include (poly)ethylene glycol di(meth)acrylate, (poly)propylene glycol di(meth)acrylate, neopentyl glycol di(meth)acrylate, pentaerythritol di(meth)acrylate, pentaerythritol tri(meth)acrylate, dipentaerythritol hexa(meth)acrylate, 1,2-ethylene glycol di(meth)acrylate, 1,6-hexanediol di(meth)acrylate, 1,9-nonanediol diacrylate (N Polyfunctional acrylates (such as ester compounds of polyhydric alcohols and (meth)acrylic acid) such as 1,12-dodecanediol di(meth)acrylate, trimethylolpropane tri(meth)acrylate, and tetramethylolmethane tri(meth)acrylate; allyl (meth)acrylate, vinyl (meth)acrylate, divinylbenzene, epoxy acrylate, polyester acrylate, urethane acrylate, butyl di(meth)acrylate, and hexyl di(meth)acrylate. The polyfunctional monomer is preferably a polyfunctional acrylate, and more preferably trimethylolpropane tri(meth)acrylate, hexanediol di(meth)acrylate, or dipentaerythritol hexa(meth)acrylate.

[0043] The crosslinking agent may contain a crosslinking agent other than the above-mentioned polyfunctional monomer. Examples of the other crosslinking agent include an isocyanate-based crosslinking agent. The photocurable pressure-sensitive adhesive composition (I) may contain an isocyanate-based crosslinking agent as the crosslinking agent, and preferably contains both the above-mentioned polyfunctional monomer and an isocyanate-based crosslinking agent. The isocyanate-based crosslinking agent can contribute to improving the adhesive strength between the first optical film 1 and the first pressure-sensitive adhesive sheet 2.

[0044] As the isocyanate-based crosslinking agent, a compound having at least two isocyanate groups (isocyanate compound) can be used. The number of isocyanate groups contained in the isocyanate compound is preferably 3 or more. The upper limit of the number of isocyanate groups is not particularly limited, and is, for example, 5. Examples of the isocyanate compound include aromatic isocyanate compounds, alicyclic isocyanate compounds, and aliphatic isocyanate compounds.

[0045] Examples of aromatic isocyanate compounds include phenylene diisocyanate, 2,4-tolylene diisocyanate, 2,6-tolylene diisocyanate, 2,2'-diphenylmethane diisocyanate, 4,4'-diphenylmethane diisocyanate, 4,4'-toluidine diisocyanate, 4,4'-diphenyl ether diisocyanate, 4,4'-diphenyl diisocyanate, 1,5-naphthalene diisocyanate, and xylylene diisocyanate.

[0046] Examples of alicyclic isocyanate compounds include 1,3-cyclopentene diisocyanate, 1,3-cyclohexane diisocyanate, 1,4-cyclohexane diisocyanate, isophorone diisocyanate, hydrogenated diphenylmethane diisocyanate, hydrogenated xylylene diisocyanate, hydrogenated tolylene diisocyanate, and hydrogenated tetramethylxylylene diisocyanate.

[0047] Examples of the aliphatic isocyanate compound include trimethylene diisocyanate, tetramethylene diisocyanate, hexamethylene diisocyanate (HDI), pentamethylene diisocyanate (PDI), 1,2-propylene diisocyanate, 1,3-butylene diisocyanate, dodecamethylene diisocyanate, and 2,4,4-trimethylhexamethylene diisocyanate.

[0048] Examples of the isocyanate-based crosslinking agent include polymers (dimers, trimers, pentamers, etc.) of the above-mentioned isocyanate compounds, adducts obtained by adding them to polyhydric alcohols such as trimethylolpropane, urea-modified products, biuret-modified products, allophanate-modified products, isocyanurate-modified products, carbodiimide-modified products, and urethane prepolymers obtained by adding them to polyether polyols, polyester polyols, acrylic polyols, polybutadiene polyols, polyisoprene polyols, etc.

[0049] The isocyanate-based crosslinking agent preferably includes an aliphatic isocyanate compound and / or a derivative of an aliphatic isocyanate compound. It is particularly preferable that the isocyanate-based crosslinking agent is at least one selected from the group consisting of pentamethylene diisocyanate (PDI)-based crosslinking agents (PDI and its derivatives) and hexamethylene diisocyanate (HDI)-based crosslinking agents (HDI and its derivatives). Specific examples of PDI-based crosslinking agents include isocyanurate-modified PDI. Specific examples of HDI-based crosslinking agents include isocyanurate-modified HDI and biuret-modified HDI.

[0050] The amount of crosslinking agent in the photocurable pressure-sensitive adhesive composition (I) varies depending on the molecular weight, number of functional groups, etc., but is preferably 0.4 parts by weight or more and 20 parts by weight or less, more preferably 0.4 parts by weight or more and 10 parts by weight or less, and even more preferably 0.5 parts by weight or more and 5 parts by weight or less, relative to 100 parts by weight of the total of the monomer group and its partial polymer. By appropriately adjusting the amount of crosslinking agent in the photocurable pressure-sensitive adhesive composition (I), display defects in image display devices can be further suppressed. In addition, by appropriately adjusting the amount of crosslinking agent in the photocurable pressure-sensitive adhesive composition (I), the adhesive strength between the first pressure-sensitive adhesive sheet 2 and the first optical film 1 and / or the second optical film 3 can be improved.

[0051] When the photocurable pressure-sensitive adhesive composition (I) contains an isocyanate-based crosslinking agent, the amount of the isocyanate-based crosslinking agent blended is, for example, 0.02 parts by weight or more, and may be 0.05 parts by weight or more, 0.1 parts by weight or more, 0.5 parts by weight or more, or even 1 part by weight or more, relative to 100 parts by weight in total of the monomer group and its partial polymer.

[0052] When an isocyanate-based crosslinking agent is added, the pressure-sensitive adhesive sheet may harden, especially in a high-temperature environment. In such a case, the stress relaxation property of the pressure-sensitive adhesive sheet is impaired, so that the expansion or contraction stress of the optical film is easily transmitted to the interface between the pressure-sensitive adhesive sheet and the adherend, and peeling tends to occur. When the adhesive strength between the pressure-sensitive adhesive sheet and the optical film can be ensured by means other than the addition of an isocyanate-based crosslinking agent, it is desirable that the photocurable pressure-sensitive adhesive composition (I) does not contain an isocyanate-based crosslinking agent.

[0053] The photocurable pressure-sensitive adhesive composition (I) may contain additives other than those described above, such as a chain transfer agent, a silane coupling agent, a viscosity modifier, a tackifier, a plasticizer, a softener, an antioxidant, a filler, a colorant, an antioxidant, a surfactant, an antistatic agent, and an ultraviolet absorber.

[0054] The solvent content in the photocurable pressure-sensitive adhesive composition (I) is, for example, 5 wt % or less, and may be 4 wt % or less, 3 wt % or less, 2 wt % or less, 1 wt % or less, or even 0.5 wt % or less. The photocurable pressure-sensitive adhesive composition (I) may be substantially free of a solvent.

[0055] The viscosity of the photocurable pressure-sensitive adhesive composition (I) is preferably 5 to 150 poise. The photocurable pressure-sensitive adhesive composition (I) having a viscosity in the above range is particularly suitable for forming a coating layer, which will be described later.

[0056] The polymerization rate of the monomer group in the first pressure-sensitive adhesive sheet 2 is preferably 90% or more, and may be 95% or more, 98% or more, or even 99% or more.

[0057] The gel fraction of the first adhesive sheet 2 is, for example, 50% or more, and may be 75% or more, 80% or more, or even 85% or more.

[0058] [Method for manufacturing first pressure-sensitive adhesive sheet] When the first pressure-sensitive adhesive sheet 2 is formed from the photocurable pressure-sensitive adhesive composition (I), the first pressure-sensitive adhesive sheet 2 can be manufactured, for example, by the following method. FIG. 2 is a schematic diagram illustrating one example of a method for manufacturing a first pressure-sensitive adhesive sheet. As shown in FIG. 2( a), a first laminate 15 is prepared, which includes, in this order, a base sheet 21, a coating layer 22 containing the photocurable pressure-sensitive adhesive composition (I), and a release liner 23. Next, light 14 is irradiated onto the first laminate 15. At this time, the light 14 transmits through the base sheet 21 to reach the coating layer 22, curing the coating layer 22. The first laminate 15 is typically irradiated with light 14 from the side of the base sheet 21. However, light 14 may also be irradiated from the side of the release liner 23. As a result, the first pressure-sensitive adhesive sheet 2 is formed from the coating layer 22, as shown in FIG. 2( b). That is, a second laminate 16 is obtained that includes a base sheet 21, a first pressure-sensitive adhesive sheet 2, and a release liner 23 in this order.

[0059] When the first PSA sheet 2 is formed from the photocurable PSA composition (I), the first PSA sheet 2 can be produced by, for example, another method. FIG. 3 is a schematic diagram illustrating another example of a method for producing a first PSA sheet. As shown in FIG. 3( a), a first laminate 15 is produced, which includes, in this order, a base sheet 21, a coating layer 22 containing the photocurable PSA composition (I), and a release liner 23. Next, light 14 is irradiated onto the first laminate 15. As shown in FIG. 3( a), light 14 is irradiated from both the release liner 23 and base sheet 21 sides. As a result, a first PSA sheet 2 is formed from the coating layer 22, as shown in FIG. 3( b). That is, a second laminate 16 is obtained, which includes, in this order, the base sheet 21, the first PSA sheet 2, and the release liner 23.

[0060] The first adhesive sheet 2 formed from the coating layer 22 may be sandwiched between the base sheet 21 and the release liner 23 until the release liner 23 is peeled off, and may form part of the second laminate 16.

[0061] An example of the substrate of the release liner 23 (hereinafter referred to as "liner substrate") is a resin film. Examples of resins that can be contained in the liner substrate include polyesters such as polyethylene terephthalate and polyethylene naphthalate, acetate resins, polyethersulfone, polycarbonate, polyamide, polyimide, polyolefin, (meth)acrylic resins, polyvinyl chloride, polyvinylidene chloride, polystyrene, polyvinyl alcohol, polyarylate, and polyphenylene sulfide. The resin is preferably a polyester such as polyethylene terephthalate.

[0062] The release liner 23 may have light 14 transparency, or may have light 14 transparency of the same order as that of the base sheet 21 .

[0063] The thickness of the release liner 23 is, for example, 10 to 200 μm, and may be 25 to 150 μm.

[0064] The release liner 23 may include a layer other than the liner substrate. The release liner 23 may include a release layer. The release liner 23 may include, for example, a liner substrate and a release layer formed on one surface of the liner substrate. This release liner 23 can be used such that the release layer is on the coating layer 22 side.

[0065] The release layer is typically a cured layer of a release agent composition containing a release agent. Various types of release agents can be used as the release agent, such as silicone-based release agents, fluorine-based release agents, long-chain alkyl-based release agents, fatty acid amide-based release agents, and silica powder. The release liner 23 may be provided with a cured layer of a release agent composition containing a silicone-based release agent as a main component (hereinafter referred to as the "silicone release layer"). The silicone release layer is particularly suitable for achieving both good adhesion to the first adhesive sheet 2 and good releasability.

[0066] The silicone-based release agent is, for example, a variety of curable silicone materials such as addition reaction type, condensation reaction type, ultraviolet curable type, electron beam curable type, and solventless type, with addition reaction curable silicone materials being preferred. Addition reaction curable silicone materials are particularly suitable for forming a release layer that has both good adhesion to and releasability from the first adhesive sheet 2. The curable silicone material may be a silicone-modified resin in which reactive silicone is introduced into an organic resin such as a urethane, epoxy, or alkyd resin by graft polymerization or the like.

[0067] An example of an addition reaction curable silicone material is a polyorganosiloxane having a vinyl group or an alkenyl group in the molecule. The addition reaction curable silicone material may not have a hydrosilyl group. Examples of alkenyl groups include 3-butenyl, 4-pentenyl, 5-hexenyl, 6-heptenyl, 7-octenyl, 8-nonenyl, 9-decenyl, 10-undecenyl, and 11-dodecenyl groups. Examples of polyorganosiloxanes include polyalkylalkylsiloxanes such as polydimethylsiloxane, polydiethylsiloxane, and polymethylethylsiloxane, polyalkylarylsiloxanes, and copolymers of multiple Si atom-containing monomers such as poly(dimethylsiloxane-diethylsiloxane). The polyorganosiloxane is preferably polydimethylsiloxane.

[0068] A release agent composition containing a silicone-based release agent as a main component (hereinafter referred to as "silicone release agent composition") usually contains a crosslinking agent. An example of the crosslinking agent is a polyorganosiloxane having a hydrosilyl group. The crosslinking agent may have two or more hydrosilyl groups in one molecule.

[0069] The silicone release agent composition may contain a curing catalyst. An example of the curing catalyst is a platinum-based catalyst. Examples of the platinum-based catalyst are chloroplatinic acid, platinum olefin complexes, and chloroplatinic acid olefin complexes. The amount of the platinum-based catalyst used is, for example, 10 to 1,000 ppm (by weight, platinum equivalent) based on the total solids content of the composition.

[0070] The silicone release agent composition may contain additives. Examples of additives are release control agents and adhesion promoters. Examples of release control agents are unreactive silicone resins, and more specific examples are organosiloxanes such as octamethylcyclotetrasiloxane, and MQ resins. The amount of the release control agent and adhesion promoter used is, for example, 1 to 30% by weight in total, based on the total solids content of the composition. Further examples of additives are fillers, antistatic agents, antioxidants, UV absorbers, plasticizers, and colorants. The amount of the additional additives used is, for example, 10% by weight or less in total, based on the total solids content of the composition.

[0071] The silicone release agent composition may contain an organic solvent. Examples of organic solvents include hydrocarbon solvents such as cyclohexane, n-hexane, and n-heptane; aromatic solvents such as toluene and xylene; ester solvents such as ethyl acetate and methyl acetate; ketone solvents such as acetone and methyl ethyl ketone; and alcohol solvents such as methanol, ethanol, and butanol. Two or more organic solvents may be contained. The amount of organic solvent used is preferably 80 to 99.9% by weight of the silicone release agent composition.

[0072] The release layer can be formed, for example, by heating and drying a coating film containing the release agent composition formed on a liner substrate. Various coating methods can be used to apply the release agent composition, such as roll coating, kiss roll coating, gravure coating, reverse coating, roll brushing, spray coating, dip roll coating, bar coating, knife coating, air knife coating, curtain coating, lip coating, and die coating. For heating and drying, for example, hot air drying can be used. The heating temperature and time vary depending on the heat resistance of the liner substrate, but are typically 80 to 150°C and about 10 seconds to 10 minutes. If necessary, irradiation with active energy rays such as ultraviolet rays may be used in combination.

[0073] The thickness of the release layer is, for example, 10 to 300 nm. The upper limit of the thickness may be 200 nm or less, 150 nm or less, 120 nm or less, 110 nm or less, 100 nm or less, less than 100 nm, 90 nm or less, 80 nm or less, 70 nm or less, less than 70 nm, or even 65 nm or less. The lower limit of the thickness may be 15 nm or more, 20 nm or more, 25 nm or more, 30 nm or more, 35 nm or more, 40 nm or more, 45 nm or more, or even 50 nm or more.

[0074] The release liner 23 may be in the form of a sheet or a continuous piece.

[0075] An example of the base sheet 21 is a resin film. Examples of the resin contained in the base sheet 21 are the same as the examples of the resin that can be contained in the liner base material.

[0076] The base sheet 21 preferably has excellent light 14 transmittance.

[0077] The thickness of the base sheet 21 is, for example, 10 to 200 μm, and may be 25 to 150 μm.

[0078] The base sheet 21 may have a release layer on the surface facing the coating layer 22. Examples of the release layer that the base sheet 21 may have and the manufacturing method thereof are the same as the examples of the release layer that the release liner 23 may have and the manufacturing method thereof. Both the release liner 23 and the base sheet 21 may have a release layer. In this case, both release layers may be formed from a release agent composition containing the same release agent as a main component. Furthermore, the thicknesses of both release layers may be different; for example, the release layer provided on the base sheet 21 may be thicker.

[0079] For the base sheet 21 , a sheet having a greater peel strength from the first PSA sheet 2 than the release liner 23 can usually be selected.

[0080] The base sheet 21 may be in the form of a sheet or a continuous sheet.

[0081] The first laminate 15 can be formed, for example, by forming a coating layer 22 on a base sheet 21 (or a release liner 23), and then placing the release liner 23 (or base sheet 21) on the formed coating layer 22. Alternatively, the first laminate 15 may be formed by applying the photocurable pressure-sensitive adhesive composition (I) in a pouring manner into the space between the base sheet 21 and the release liner 23, which are held at a predetermined distance so that their main surfaces face each other.

[0082] The coating layer 22 can be formed by various coating methods such as roll coating, kiss roll coating, gravure coating, reverse coating, roll brush, spray coating, dip roll coating, bar coating, knife coating, air knife coating, curtain coating, lip coating, and die coating.

[0083] The thickness of the coating layer 22 can be adjusted according to the desired thickness of the first adhesive sheet 2, and may be, for example, 5 to 500 μm, 5 to 250 μm, 5 to 150 μm, 5 to 100 μm, 5 to 50 μm, 5 to 30 μm, 5 to 25 μm, or even 5 to 20 μm.

[0084] The light 14 irradiated onto the first laminate 15 is, for example, visible light or ultraviolet light having a wavelength shorter than 450 nm. The light 14 may include light having a wavelength in the same range as the absorption wavelength of the photopolymerization initiator contained in the photocurable pressure-sensitive adhesive composition. Light 14 may be irradiated with light having a wavelength of 300 nm or less, filtered out using a filter or the like. Cutting out short-wavelength light is suitable for suppressing deterioration of the base sheet 21 due to the light 14. The light source of the light 14 is, for example, a light irradiation device equipped with an ultraviolet irradiation lamp. Examples of ultraviolet irradiation lamps include ultraviolet LEDs, low-pressure mercury lamps, medium-pressure mercury lamps, high-pressure mercury lamps, ultra-high-pressure mercury lamps, metal halide lamps, xenon lamps, microwave-excited mercury lamps, black light lamps, chemical lamps, germicidal lamps, low-pressure discharge mercury lamps, and excimer lasers. Two or more ultraviolet irradiation lamps may be combined.

[0085] The irradiation with light 14 may be continuous or intermittent.

[0086] The illuminance of the light 14 is, for example, 1 to 20 mW / cm 2The irradiation time of the light 14 is, for example, 5 minutes to 5 hours. The integrated light amount of the light 14 on the first laminate 15 is, for example, 100 to 5000 mJ / cm. 2 is.

[0087] (Solvent-Based Pressure-Sensitive Adhesive Composition) As described above, the solvent-based pressure-sensitive adhesive composition (II) is, for example, a pressure-sensitive adhesive composition containing a polymer and a solvent. When the first pressure-sensitive adhesive sheet 2 is formed from the solvent-based pressure-sensitive adhesive composition (II), examples of the pressure-sensitive adhesive constituting the first pressure-sensitive adhesive sheet 2 include acrylic pressure-sensitive adhesives, rubber pressure-sensitive adhesives, vinyl alkyl ether pressure-sensitive adhesives, silicone pressure-sensitive adhesives, polyester pressure-sensitive adhesives, polyamide pressure-sensitive adhesives, urethane pressure-sensitive adhesives, fluorine-based pressure-sensitive adhesives, epoxy pressure-sensitive adhesives, and polyether pressure-sensitive adhesives. The pressure-sensitive adhesives constituting the first pressure-sensitive adhesive sheet 2 are used alone or in combination of two or more types. However, from the viewpoints of transparency, processability, durability, adhesion, etc., it is preferable to use an acrylic pressure-sensitive adhesive (composition) containing a (meth)acrylic polymer alone. In other words, it is preferable that the first pressure-sensitive adhesive sheet 2 contains a (meth)acrylic polymer as the polymer.

[0088] [(Meth)acrylic Polymer (A)] The (meth)acrylic polymer (A) preferably has, as a main unit, a structural unit derived from a (meth)acrylic monomer (A1) having an alkyl group having 1 to 30 carbon atoms on its side chain. The alkyl group may be linear or branched. The (meth)acrylic polymer (A) may have one or more structural units derived from the (meth)acrylic monomer (A1). Examples of the (meth)acrylic monomer (A1) include methyl (meth)acrylate, ethyl (meth)acrylate, n-butyl (meth)acrylate, s-butyl (meth)acrylate, t-butyl (meth)acrylate, isobutyl (meth)acrylate, n-pentyl (meth)acrylate, isopentyl (meth)acrylate, n-hexyl (meth)acrylate, isohexyl (meth)acrylate, and isoheptyl (meth)acrylate. acrylate, 2-ethylhexyl(meth)acrylate, n-octyl(meth)acrylate, isooctyl(meth)acrylate, n-nonyl(meth)acrylate, isononyl(meth)acrylate, n-decyl(meth)acrylate, isodecyl(meth)acrylate, n-dodecyl(meth)acrylate (lauryl(meth)acrylate), n-tridecyl(meth)acrylate, and n-tetradecyl(meth)acrylate.

[0089] The (meth)acrylic polymer (A) may have a structural unit derived from a (meth)acrylic monomer (A1) having a long-chain alkyl group on the side chain. An example of the monomer (A1) is n-dodecyl (meth)acrylate (lauryl (meth)acrylate).

[0090] The (meth)acrylic polymer (A) may have a structural unit derived from a (meth)acrylic monomer (A1) which, when made into a homopolymer, has a glass transition temperature (Tg) in the range of −70 to −20° C. An example of the monomer (A1) is n-butyl acrylate.

[0091] The (meth)acrylic polymer (A) may have a structural unit other than the structural unit derived from the (meth)acrylic monomer (A1). The structural unit is derived from a monomer (A2) copolymerizable with the (meth)acrylic monomer (A1). The (meth)acrylic polymer (A) may have one or more types of the structural unit.

[0092] An example of the monomer (A2) is an aromatic ring-containing monomer. The aromatic ring-containing monomer may be an aromatic ring-containing (meth)acrylic monomer. Examples of the aromatic ring-containing monomer include phenyl(meth)acrylate, phenoxyethyl(meth)acrylate, benzyl(meth)acrylate, phenoxydiethylene glycol(meth)acrylate, ethylene oxide-modified nonylphenol(meth)acrylate, hydroxyethylated β-naphthol(meth)acrylate, and biphenyl(meth)acrylate. The content of the structural unit derived from the aromatic ring-containing monomer in the (meth)acrylic polymer (A) is, for example, 0 to 50% by weight, and may be 1 to 30% by weight, 5 to 25% by weight, 8 to 20% by weight, 10 to 18% by weight, 12 to 16% by weight, or even 12 to 16% by weight. The (meth)acrylic polymer (A) having a structural unit derived from an aromatic ring-containing monomer can contribute to improving the compatibility of the (meth)acrylic polymer (A) with the crosslinking agent (B) and its self-polymer.

[0093] Another example of the monomer (A2) is a hydroxyl group-containing monomer. The hydroxyl group-containing monomer may be a hydroxyl group-containing (meth)acrylic monomer. Examples of the hydroxyl group-containing monomer include hydroxyalkyl (meth)acrylates such as 2-hydroxyethyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, 6-hydroxyhexyl (meth)acrylate, 8-hydroxyoctyl (meth)acrylate, 10-hydroxydecyl (meth)acrylate, and 12-hydroxylauryl (meth)acrylate, as well as (4-hydroxymethylcyclohexyl)-methyl acrylate. The hydroxyl group can react with various crosslinking agents. From the viewpoint of increasing the uniformity of the crosslinked structure to be formed, the content of the structural unit derived from the hydroxyl group-containing monomer in the (meth)acrylic polymer (A) may be 1% by weight or less, 0.5% by weight or less, or even 0.1% by weight or less, or may even be 0% by weight (no such structural unit may be contained).

[0094] The monomer (A2) may be a carboxyl group-containing monomer, an amino group-containing monomer, or an amide group-containing monomer. Examples of the carboxyl group-containing monomer are (meth)acrylic acid, carboxyethyl (meth)acrylate, carboxypentyl (meth)acrylate, itaconic acid, maleic acid, fumaric acid, and crotonic acid. Examples of the amino group-containing monomer are N,N-dimethylaminoethyl (meth)acrylate and N,N-dimethylaminopropyl (meth)acrylate. Examples of the amide group-containing monomer include acrylamide-based monomers such as (meth)acrylamide, N,N-dimethyl(meth)acrylamide, N,N-diethyl(meth)acrylamide, N-isopropylacrylamide, N-methyl(meth)acrylamide, N-butyl(meth)acrylamide, N-hexyl(meth)acrylamide, N-methylol(meth)acrylamide, N-methylol-N-propane(meth)acrylamide, aminomethyl(meth)acrylamide, aminoethyl(meth)acrylamide, mercaptomethyl(meth)acrylamide, and mercaptoethyl(meth)acrylamide; N-acryloyl heterocyclic monomers such as N-(meth)acryloylmorpholine, N-(meth)acryloylpiperidine, and N-(meth)acryloylpyrrolidine; and N-vinyl group-containing lactam-based monomers such as N-vinylpyrrolidone and N-vinyl-ε-caprolactam.

[0095] Monomer (A2) may be a polyfunctional monomer. Examples of the polyfunctional monomer include polyfunctional acrylates such as hexanediol di(meth)acrylate (1,6-hexanediol di(meth)acrylate), butanediol di(meth)acrylate, (poly)ethylene glycol di(meth)acrylate, (poly)propylene glycol di(meth)acrylate, neopentyl glycol di(meth)acrylate, pentaerythritol di(meth)acrylate, pentaerythritol tri(meth)acrylate, dipentaerythritol hexa(meth)acrylate, trimethylolpropane tri(meth)acrylate, tetramethylolmethane tri(meth)acrylate, allyl (meth)acrylate, vinyl (meth)acrylate, epoxy acrylate, polyester acrylate, and urethane acrylate; and divinylbenzene. The polyfunctional acrylate is preferably 1,6-hexanediol diacrylate or dipentaerythritol hexa(meth)acrylate.

[0096] The total content of structural units derived from carboxyl group-containing monomers, amino group-containing monomers, amide group-containing monomers, and polyfunctional monomers in the (meth)acrylic polymer (A) is preferably 20% by weight or less, more preferably 10% by weight or less, and even more preferably 8% by weight or less. When the (meth)acrylic polymer (A) contains such structural units, the total content is, for example, 0.01% by weight or more, and may even be 0.05% by weight or more. The (meth)acrylic polymer (A) may not contain structural units derived from polyfunctional monomers. When the (meth)acrylic polymer (A) contains structural units derived from carboxyl group-containing monomers, particularly acrylic acid, and / or structural units derived from amide group-containing monomers, the self-polymerization of the crosslinking agent (B), for example, can be enhanced. The improvement in the self-polymerization property of the crosslinking agent (B) can particularly contribute to suppressing peeling of the PSA sheet in a humid environment and stabilizing the physical properties of the PSA sheet in a system with a high content of the crosslinking agent (B).

[0097] Examples of the other monomer (A2) include (meth)acrylic acid alkoxyalkyl esters such as 2-methoxyethyl (meth)acrylate, 2-ethoxyethyl (meth)acrylate, methoxytriethylene glycol (meth)acrylate, 3-methoxypropyl (meth)acrylate, 3-ethoxypropyl (meth)acrylate, 4-methoxybutyl (meth)acrylate, and 4-ethoxybutyl (meth)acrylate; epoxy group-containing monomers such as glycidyl (meth)acrylate and methylglycidyl (meth)acrylate; vinyl sulfonate; (meth)acrylic acid esters having an alicyclic hydrocarbon group, such as cyclopentyl (meth)acrylate, cyclohexyl (meth)acrylate, and isobornyl (meth)acrylate; vinyl esters, such as vinyl acetate and vinyl propionate; aromatic vinyl compounds, such as styrene and vinyltoluene; olefins or dienes, such as ethylene, propylene, butadiene, isoprene, and isobutylene; vinyl ethers, such as vinyl alkyl ether; and vinyl chloride.

[0098] The total content of the structural units derived from the other monomer (A2) in the (meth)acrylic polymer (A) is, for example, 30% by weight or less, and may be 10% by weight or less, and is preferably 0% by weight (not including such structural units).

[0099] The (meth)acrylic polymer (A) can be formed by polymerizing one or more of the above-mentioned monomers using a known method. A monomer and a partial polymer of the monomer may also be polymerized. The polymerization can be carried out, for example, by solution polymerization, emulsion polymerization, bulk polymerization, thermal polymerization, or active energy ray polymerization. Solution polymerization and active energy ray polymerization are preferred because they allow the formation of a pressure-sensitive adhesive sheet with excellent optical transparency. The polymerization is preferably carried out while avoiding contact between the monomer and / or the partial polymer and oxygen. For this purpose, for example, polymerization can be carried out in an inert gas atmosphere such as nitrogen, or polymerization in a state where oxygen is blocked by a resin film or the like. The (meth)acrylic polymer (A) formed may be in any form, such as a random copolymer, a block copolymer, or a graft copolymer.

[0100] The polymerization system for forming the (meth)acrylic polymer (A) may contain one or more polymerization initiators. The type of polymerization initiator can be selected depending on the polymerization reaction, and may be, for example, a thermal polymerization initiator or a photopolymerization initiator.

[0101] Examples of solvents used in solution polymerization include esters such as ethyl acetate and n-butyl acetate; aromatic hydrocarbons such as toluene and benzene; aliphatic hydrocarbons such as n-hexane and n-heptane; alicyclic hydrocarbons such as cyclohexane and methylcyclohexane; and ketones such as methyl ethyl ketone and methyl isobutyl ketone. However, the solvent is not limited to the above examples. The solvent may be a mixed solvent of two or more solvents.

[0102] Examples of polymerization initiators used in solution polymerization include azo polymerization initiators, peroxide polymerization initiators, and redox polymerization initiators. Examples of peroxide polymerization initiators include dibenzoyl peroxide and t-butyl permaleate. Among these, the azo polymerization initiators disclosed in JP-A-2002-69411 are preferred. Examples of such azo polymerization initiators include 2,2'-azobisisobutyronitrile (AIBN), 2,2'-azobis-2-methylbutyronitrile, 2,2'-azobis(2-methylpropionate)dimethyl, and 4,4'-azobis-4-cyanovaleric acid. However, the polymerization initiator is not limited to the above examples. The amount of the azo polymerization initiator used is, for example, 0.05 to 0.5 parts by weight, or may be 0.1 to 0.3 parts by weight, per 100 parts by weight of the total amount of monomers.

[0103] The active energy rays used in the active energy ray polymerization include, for example, ionizing radiation such as α rays, β rays, γ rays, neutron rays, and electron beams, as well as ultraviolet rays. The active energy rays are preferably ultraviolet rays. Polymerization by irradiation with ultraviolet rays is also called photopolymerization. The polymerization system for the active energy ray polymerization typically contains a photopolymerization initiator. The polymerization conditions for the active energy polymerization are not limited as long as a (meth)acrylic polymer (A) is formed.

[0104] Examples of the photopolymerization initiator include a benzoin ether-based photopolymerization initiator, an acetophenone-based photopolymerization initiator, an α-ketol-based photopolymerization initiator, an aromatic sulfonyl chloride-based photopolymerization initiator, a photoactive oxime-based photopolymerization initiator, a benzoin-based photopolymerization initiator, a benzyl-based photopolymerization initiator, a benzophenone-based photopolymerization initiator, a ketal-based photopolymerization initiator, and a thioxanthone-based photopolymerization initiator, although the photopolymerization initiator is not limited to the above examples.

[0105] Examples of benzoin ether-based photopolymerization initiators include benzoin methyl ether, benzoin ethyl ether, benzoin propyl ether, benzoin isopropyl ether, benzoin isobutyl ether, 2,2-dimethoxy-1,2-diphenylethan-1-one, and anisole methyl ether. Examples of acetophenone-based photopolymerization initiators include 2,2-diethoxyacetophenone, 2,2-dimethoxy-2-phenylacetophenone, 1-hydroxycyclohexyl phenyl ketone, 4-phenoxydichloroacetophenone, and 4-(t-butyl)dichloroacetophenone. Examples of α-ketol-based photopolymerization initiators include 2-methyl-2-hydroxypropiophenone and 1-[4-(2-hydroxyethyl)phenyl]-2-methylpropan-1-one. Examples of aromatic sulfonyl chloride-based photopolymerization initiators include 2-naphthalenesulfonyl chloride. An example of a photoactive oxime-based photopolymerization initiator is 1-phenyl-1,1-propanedione-2-(o-ethoxycarbonyl)-oxime. An example of a benzoin-based photopolymerization initiator is benzoin. An example of a benzyl-based photopolymerization initiator is benzil. An example of a benzophenone-based photopolymerization initiator is benzophenone, benzoylbenzoic acid, 3,3'-dimethyl-4-methoxybenzophenone, polyvinylbenzophenone, or α-hydroxycyclohexyl phenyl ketone. An example of a ketal-based photopolymerization initiator is benzil dimethyl ketal. An example of a thioxanthone-based photopolymerization initiator is thioxanthone, 2-chlorothioxanthone, 2-methylthioxanthone, 2,4-dimethylthioxanthone, isopropylthioxanthone, 2,4-diisopropylthioxanthone, or dodecylthioxanthone.

[0106] The amount of the photopolymerization initiator used is, for example, 0.01 to 1 part by weight, and may be 0.05 to 0.5 parts by weight, relative to 100 parts by weight of the total amount of the monomers.

[0107] The weight average molecular weight (Mw) of the (meth)acrylic polymer (A) is, for example, 1,000,000 to 2,800,000, and from the viewpoint of the durability and heat resistance of the PSA sheet, may be 1,200,000 or more, or even 1,400,000 or more. The weight average molecular weight (Mw) of the polymer and oligomer in this specification is a value (polystyrene equivalent) based on measurement by GPC (gel permeation chromatography).

[0108] The content of the (meth)acrylic polymer (A) in the pressure-sensitive adhesive composition (II) is, for example, 50% by weight or more, 60% by weight or more, 70% by weight or more, or even 80% by weight or more, in terms of solid content. The upper limit of the content is, for example, 99% by weight or less, 97% by weight or less, 95% by weight or less, 93% by weight or less, or even 90% by weight or less.

[0109] [Crosslinking agent (B)] The crosslinking agent (B) is typically a polyfunctional crosslinking agent having two or more crosslinking reactive groups per molecule. The crosslinking agent (B) may be a trifunctional or higher crosslinking agent having three or more crosslinking reactive groups per molecule. A trifunctional or higher crosslinking agent (B) is likely to form a self-polymer. The upper limit of the number of crosslinking reactive groups per molecule is, for example, 5.

[0110] The crosslinking agent (B) is, for example, an isocyanate-based crosslinking agent. The isocyanate-based crosslinking agent contains an isocyanate group as a crosslinking reactive group. The isocyanate-based crosslinking agent (B) may be an aromatic isocyanate compound, an alicyclic isocyanate compound, or an aliphatic isocyanate compound.

[0111] Examples of aromatic isocyanate compounds that can be used in the crosslinking agent (B) include phenylene diisocyanate, 2,4-tolylene diisocyanate, 2,6-tolylene diisocyanate, 2,2'-diphenylmethane diisocyanate, 4,4'-diphenylmethane diisocyanate, 4,4'-toluidine diisocyanate, 4,4'-diphenyl ether diisocyanate, 4,4'-diphenyl diisocyanate, 1,5-naphthalene diisocyanate, and xylylene diisocyanate.

[0112] Examples of the alicyclic isocyanate compound that can be used in the crosslinking agent (B) include 1,3-cyclopentene diisocyanate, 1,3-cyclohexane diisocyanate, 1,4-cyclohexane diisocyanate, isophorone diisocyanate, hydrogenated diphenylmethane diisocyanate, hydrogenated xylylene diisocyanate, hydrogenated tolylene diisocyanate, and hydrogenated tetramethylxylylene diisocyanate.

[0113] Examples of aliphatic isocyanate compounds that can be used in the crosslinking agent (B) are trimethylene diisocyanate, tetramethylene diisocyanate, hexamethylene diisocyanate, pentamethylene diisocyanate, 1,2-propylene diisocyanate, 1,3-butylene diisocyanate, dodecamethylene diisocyanate, and 2,4,4-trimethylhexamethylene diisocyanate.

[0114] The crosslinking agent (B) may be a derivative of the isocyanate compound. Examples of the derivative include multimers (dimers, trimers, pentamers, etc.), adducts obtained by addition to polyhydric alcohols such as trimethylolpropane, urea-modified products, biuret-modified products, allophanate-modified products, isocyanurate-modified products, carbodiimide-modified products, and urethane prepolymers obtained by addition to polyether polyols, polyester polyols, acrylic polyols, polybutadiene polyols, polyisoprene polyols, etc.

[0115] The crosslinking agent (B) is preferably an aromatic isocyanate compound or a derivative thereof, more preferably tolylene diisocyanate or a derivative thereof (in other words, a tolylene diisocyanate-based (TDI-based) crosslinking agent). TDI-based crosslinking agents have better reaction uniformity than xylylene diisocyanate or a derivative thereof (in other words, a xylylene diisocyanate-based (XDI-based) crosslinking agent). An example of a TDI-based crosslinking agent is an adduct of tolylene diisocyanate and a polyfunctional alcohol, and a more specific example is a trimethylolpropane / tolylene diisocyanate trimer adduct.

[0116] Commercially available products can be used as the crosslinking agent (B). Examples of commercially available products include Millionate MT, Millionate MTL, Millionate MR-200, Millionate MR-400, Coronate L, Coronate HL, and Coronate HX (all manufactured by Tosoh Corporation; all trade names), and Takenate D-102, Takenate D-103, Takenate D-110N, Takenate D-120N, Takenate D-140N, Takenate D-160N, Takenate D-165N, Takenate D-170HN, Takenate D-178N, Takenate 500, and Takenate 600 (all manufactured by Mitsui Chemicals; all trade names). As the crosslinking agent (B), Coronate L, Takenate D-102 and Takenate D-103 (all of which are trimethylolpropane / tolylene diisocyanate trimer adducts) can be preferably used.

[0117] The amount of the crosslinking agent (B) in the pressure-sensitive adhesive composition (I) may be 5 parts by weight or more, 6 parts by weight or more, 7 parts by weight or more, 8 parts by weight or more, 9 parts by weight or more, 10 parts by weight or more, more than 10 parts by weight, or even 11 parts by weight or more, relative to 100 parts by weight of the (meth)acrylic polymer (A). The upper limit of the amount may be, for example, 30 parts by weight or less, 28 parts by weight or less, 25 parts by weight or less, 23 parts by weight or less, 20 parts by weight or less, 19 parts by weight or less, 18 parts by weight or less, or even 15 parts by weight or less.

[0118] The pressure-sensitive adhesive composition (I) may contain one or more crosslinking agents (B).

[0119] The pressure-sensitive adhesive sheet formed from the pressure-sensitive adhesive composition (II) may have an interpenetrating network (IPN) structure of the crosslinked product of the (meth)acrylic polymer (A) and the self-polymer of the crosslinking agent (B). The IPN structure is suitable for improving the durability of the pressure-sensitive adhesive sheet.

[0120] Other examples of the crosslinking agent (B) include peroxide-based crosslinking agents, epoxy-based crosslinking agents, imine-based crosslinking agents, and polyfunctional metal chelates. However, the crosslinking agent (B) is preferably an isocyanate-based crosslinking agent. When the pressure-sensitive adhesive composition (II) contains a crosslinking agent (B) other than an isocyanate-based crosslinking agent, the total amount of the crosslinking agent (B) is preferably 0.1 to 5 parts by weight, more preferably 0.1 to 3 parts by weight, 0.1 to 2 parts by weight, and 0.1 to 1 part by weight, in that order. The pressure-sensitive adhesive composition (II) does not necessarily need to contain a crosslinking agent (B) other than an isocyanate-based crosslinking agent, such as an epoxy-based crosslinking agent.

[0121] [Additives] The pressure-sensitive adhesive composition (II) may contain other additives. Examples of additives include silane coupling agents, polyfunctional alcohols, colorants such as pigments and dyes, surfactants, plasticizers, tackifiers, surface lubricants, leveling agents, rework improvers, softeners, antioxidants, antiaging agents, light stabilizers, UV absorbers, polymerization inhibitors, antistatic agents (alkali metal salts, ionic liquids, ionic solids, etc., which are ionic compounds), inorganic fillers, organic fillers, powders such as metal powders, particles, and foil-like materials. The additives can be blended in an amount of, for example, 10 parts by weight or less, preferably 5 parts by weight or less, more preferably 1.5 parts by weight or less, relative to 100 parts by weight of the (meth)acrylic polymer (A).

[0122] Examples of the silane coupling agent include epoxy group-containing silane coupling agents such as 3-glycidoxypropyltrimethoxysilane, 3-glycidoxypropyltriethoxysilane, 3-glycidoxypropylmethyldiethoxysilane, and 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane; amino group-containing silane coupling agents such as 3-aminopropyltrimethoxysilane, N-2-(aminoethyl)-3-aminopropylmethyldimethoxysilane, 3-triethoxysilyl-N-(1,3-dimethylbutylidene)propylamine, and N-phenyl-γ-aminopropyltrimethoxysilane; (meth)acrylic group-containing silane coupling agents such as 3-acryloxypropyltrimethoxysilane and 3-methacryloxypropyltriethoxysilane; and isocyanate group-containing silane coupling agents such as 3-isocyanatepropyltriethoxysilane.

[0123] When the pressure-sensitive adhesive composition (II) contains a silane coupling agent, the blending amount thereof is, for example, 5 parts by weight or less, and may be 3 parts by weight or less, 1 part by weight or less, 0.5 parts by weight or less, 0.2 parts by weight or less, 0.1 parts by weight or less, or even 0.05 parts by weight or less, relative to 100 parts by weight of the (meth)acrylic polymer (A). The pressure-sensitive adhesive composition (I) does not need to contain a silane coupling agent.

[0124] The pressure-sensitive adhesive composition (II) may contain a polyfunctional alcohol. The molecular weight of the polyfunctional alcohol is, for example, 240 or less, or may be 230 or less, 220 or less, 210 or less, 200 or less, 190 or less, 180 or less, 170 or less, 160 or less, or even 150 or less. The lower limit of the molecular weight is, for example, 60 or more, 80 or more, 90 or more, or even 100 or more.

[0125] Examples of polyfunctional alcohols include alkylene glycols such as ethylene glycol and propylene glycol and polymers thereof, ether glycols such as diethylene glycol and polymers thereof, trimethylolethane, trimethylolpropane, glycerin, and sugar alcohols such as pentaerythritol and sorbitol. The polyfunctional alcohol is preferably trimethylolpropane, glycerin, or diethylene glycol and polymers thereof, more preferably trimethylolpropane.

[0126] The polyfunctional alcohol may be trifunctional or higher. Examples of trifunctional polyfunctional alcohols are trimethylolpropane and glycerin.

[0127] The polyfunctional alcohol may have no reactive group other than the hydroxyl group that is reactive with the crosslinking agent (B). The reactive group is, for example, at least one selected from an amino group, a carboxyl group, and an epoxy group, and is particularly an amino group.

[0128] The amount of the polyfunctional alcohol in the pressure-sensitive adhesive composition (II) is, for example, 0.5 parts by weight or more and 20 parts by weight or less, relative to 100 parts by weight of the (meth)acrylic polymer (A). The upper limit of the amount may be 15 parts by weight or less, 10 parts by weight or less, 8 parts by weight or less, 5 parts by weight or less, 4 parts by weight or less, or even 3 parts by weight or less.

[0129] The pressure-sensitive adhesive composition (II) may not contain a crosslinking accelerator such as a catalyst. Examples of crosslinking accelerators include polyethers, polyether polyols, and phosphate esters having a reactive group reactive with the crosslinking agent (B). The reactive group is, for example, at least one selected from a hydroxyl group, an amino group, a carboxyl group, and an epoxy group, and is particularly a hydroxyl group or an amino group. The pressure-sensitive adhesive composition (II) may not contain a polyether polyol having an amino group, or a phosphate ester having a hydroxyl group. The solvent-based pressure-sensitive adhesive (II) may not contain a photocuring agent such as an ultraviolet curing agent.

[0130] [Method for producing first pressure-sensitive adhesive sheet] When the first pressure-sensitive adhesive sheet 2 is formed from the solvent-based pressure-sensitive adhesive composition (II), the first pressure-sensitive adhesive sheet 2 contains, for example, a crosslinked product of the (meth)acrylic polymer (A). The first pressure-sensitive adhesive sheet 2 can be formed from the solvent-based pressure-sensitive adhesive composition (II) by the following method.

[0131] The method for producing the first adhesive sheet 2 includes, for example, applying a solvent-based adhesive composition (II) containing a (meth)acrylic polymer (A) and a crosslinking agent to a substrate to form a coating film, and drying the resulting coating film.

[0132] The substrate can be, for example, a release film. The first pressure-sensitive adhesive sheet 2 formed on the release film can be transferred to, for example, an optical film. The substrate may be the first optical film 1 or the second optical film 3. In this case, the first pressure-sensitive adhesive sheet 2 can be formed on the first optical film 1 or the second optical film 3, and an optical film with the first pressure-sensitive adhesive sheet can be obtained.

[0133] After the first adhesive sheet 2 is transferred to the first optical film 1 or the second optical film 3, the release film can be used as a release liner until the first adhesive sheet 2 is put to practical use, thereby simplifying the process.

[0134] Examples of materials constituting the release film include suitable thin sheets such as porous materials such as plastic film, paper, cloth, and nonwoven fabric, nets, foam sheets, metal foils, and laminates thereof, but plastic film is preferably used because of its excellent surface smoothness.

[0135] The plastic film is not particularly limited, and examples thereof include polyethylene film, polypropylene film, polybutene film, polybutadiene film, polymethylpentene film, polyvinyl chloride film, vinyl chloride copolymer film, polyethylene terephthalate film, polybutylene terephthalate film, polyurethane film, and ethylene-vinyl acetate copolymer film.

[0136] The thickness of the release film is usually 5 to 200 μm, and preferably about 5 to 100 μm. The release film is subjected to a release treatment such as a silicone-based, fluorine-based, or long-chain alkyl-based treatment. The release film may be subjected to a release and antifouling treatment using a fatty acid amide-based release agent, silica powder, or the like, or an antistatic treatment such as a coating-type, kneading-type, or vapor deposition-type.

[0137] A solution (adhesive solution) containing a solvent-based pressure-sensitive adhesive composition (II) may be applied to the substrate. The solids concentration of the pressure-sensitive adhesive solution is, for example, 5 to 50 wt %, preferably 10 to 40 wt %. The pressure-sensitive adhesive solution can be prepared by appropriately adding the same solvent as the polymerization solvent or a different solvent to the solvent-based pressure-sensitive adhesive composition (II), depending on the polymerization form of the (meth)acrylic polymer (A).

[0138] Various methods can be used to apply the solvent-based pressure-sensitive adhesive composition (II) to the substrate, including, for example, roll coating, kiss roll coating, gravure coating, reverse coating, roll brushing, spray coating, dip roll coating, bar coating, knife coating, air knife coating, curtain coating, lip coating, and extrusion coating using a die coater, etc. The amount of solvent-based pressure-sensitive adhesive composition (II) to be applied can be adjusted appropriately depending on the desired thickness of the first pressure-sensitive adhesive sheet 2.

[0139] The coating film is dried to harden the coating film, thereby forming the first adhesive sheet 2. The drying temperature for the coating film is, for example, 130°C or lower, preferably 125°C or lower, more preferably 120°C or lower, even more preferably 110°C or lower, and particularly preferably 100°C or lower. The drying temperature for the coating film may be 60°C or higher, or may be 80°C or higher. When the drying temperature is 60°C or higher, for example, the reaction of the isocyanate-based crosslinking agent proceeds smoothly, which can improve the cohesive strength of the first adhesive sheet 2 and tend to reduce display unevenness in the image display device. When the drying temperature is 130°C or lower, for example, the reaction rate of the isocyanate-based crosslinking agent can be appropriately adjusted, which tends to ensure transparency.

[0140] The drying time of the coating film can be appropriately adjusted depending on the composition of the solvent-based pressure-sensitive adhesive composition (II), and is preferably 30 to 300 seconds, more preferably 40 to 240 seconds, and particularly preferably 60 to 180 seconds.

[0141] As described above, the first pressure-sensitive adhesive sheet 2 is formed from the photocurable pressure-sensitive adhesive composition (I) or the solvent-based pressure-sensitive adhesive composition (II). In other words, the first pressure-sensitive adhesive sheet 2 is a cured product of the photocurable pressure-sensitive adhesive composition (I) or a cured product of the solvent-based pressure-sensitive adhesive composition (II). The first pressure-sensitive adhesive sheet 2 is preferably formed from the photocurable pressure-sensitive adhesive composition (I). That is, the first pressure-sensitive adhesive sheet 2 is preferably formed from the photocurable pressure-sensitive adhesive composition (I) containing a monomer group and / or a partial polymer of the monomer group. The first pressure-sensitive adhesive sheet 2 formed from the photocurable pressure-sensitive adhesive composition (I) tends to have excellent surface smoothness. The smoothness of the first pressure-sensitive adhesive sheet 2 can improve the adhesion between the first pressure-sensitive adhesive sheet 2 and the first optical film 1 and / or the second optical film 3. In addition, a smooth first pressure-sensitive adhesive sheet 2 tends to suppress the occurrence of appearance defects such as color unevenness. That is, by using the first adhesive sheet 2 formed from the photocurable adhesive composition (I), the image display device can achieve the effect of suppressing display defects even when a small object collides with or presses against the screen over a small contact area, as well as the effect of suppressing the occurrence of appearance defects such as color unevenness.

[0142] (Second Pressure-Sensitive Adhesive Sheet) The thickness T2 of the second pressure-sensitive adhesive sheet 4 is, for example, 5 μm or more and 100 μm or less, preferably 8 μm or more and 80 μm or less, more preferably 10 μm or more and 50 μm or less, and even more preferably 12 μm or more and 30 μm or less. By appropriately adjusting the thickness of the second pressure-sensitive adhesive sheet 4, the adhesion between the second optical film 3 and the second pressure-sensitive adhesive sheet 4 can be improved.

[0143] The breaking elongation of the second pressure-sensitive adhesive sheet 4 is, for example, 500% or more. The breaking elongation of the second pressure-sensitive adhesive sheet 4 is preferably 700% or more, more preferably 800% or more, and even more preferably 1000% or more. The upper limit of the breaking elongation of the second pressure-sensitive adhesive sheet 4 is, for example, 2000%.

[0144] A known pressure-sensitive adhesive can be used for the second pressure-sensitive adhesive sheet 4. The second pressure-sensitive adhesive sheet 4 may be a pressure-sensitive adhesive sheet formed from a photocurable pressure-sensitive adhesive composition (I), or may be a pressure-sensitive adhesive sheet formed from a solvent-based pressure-sensitive adhesive composition (II). The first pressure-sensitive adhesive sheet 2 may be used for the second pressure-sensitive adhesive sheet 4. The second pressure-sensitive adhesive sheet 4 is preferably a pressure-sensitive adhesive sheet formed from a photocurable pressure-sensitive adhesive composition (I).

[0145] 1, the first optical film 1 has two main surfaces facing each other. One main surface is exposed to the outside of the optical laminate 10A, for example. The other main surface of the first optical film 1 faces the first pressure-sensitive adhesive sheet 2 and is the surface of the first optical film 1 on which the first pressure-sensitive adhesive sheet is laminated.

[0146] The first optical film 1 may be composed of a single layer or a laminate of multiple layers. In other words, the first optical film 1 may be composed of a single film or a laminate of multiple films. The films constituting the first optical film 1 may be bonded together via any adhesive and any pressure-sensitive adhesive sheet. The first optical film 1 includes, for example, at least one selected from the group consisting of a polarizing film and a retardation film. The first optical film 1 may include a polarizing film. The first optical film 1 may be a laminate film including a polarizing film and / or a retardation film.

[0147] The polarizing film includes a polarizer. The polarizing film typically includes a polarizer and a protective film (transparent protective film). The protective film is, for example, disposed in contact with a main surface of the polarizer. The polarizer may be disposed between two protective films. The protective film may be disposed on at least one surface of the polarizer.

[0148] Examples of polarizers include those obtained by uniaxially stretching a hydrophilic polymer film, such as a polyvinyl alcohol film, a partially formalized polyvinyl alcohol film, or a partially saponified ethylene-vinyl acetate copolymer film, after adsorbing a dichroic substance, such as iodine or a dichroic dye; and polyene-based oriented films, such as a dehydrated polyvinyl alcohol film or a dehydrochlorinated polyvinyl chloride film. Polarizers typically consist of a polyvinyl alcohol film (polyvinyl alcohol films include partially saponified ethylene-vinyl acetate copolymer films) and a dichroic substance, such as iodine.

[0149] The thickness of the polarizer is, for example, 80 μm or less, and may be 50 μm or less, 30 μm or less, 25 μm or less, or even 20 μm or less. The lower limit of the polarizer thickness is not particularly limited, and may be, for example, 1 μm or more, 5 μm or more, 10 μm or more, or even 15 μm or more. A thin polarizer (for example, a thickness of 20 μm or less) is suppressed in dimensional change, and can contribute to improving the durability of the optical laminate, particularly durability at high temperatures.

[0150] The material for the protective film may be, for example, a thermoplastic resin having excellent transparency, mechanical strength, thermal stability, moisture-blocking properties, isotropy, etc. Specific examples of such thermoplastic resins include cellulose resins such as triacetyl cellulose, polyester resins, polyethersulfone resins, polysulfone resins, polycarbonate resins, polyamide resins, polyimide resins, polyolefin resins, (meth)acrylic resins, cyclic polyolefin resins (norbornene-based resins), polyarylate resins, polystyrene resins, polyvinyl alcohol resins, and mixtures thereof. The material for the protective film may be a thermosetting resin or an ultraviolet-curable resin such as a (meth)acrylic, urethane, acrylic urethane, epoxy, or silicone-based resin. When the polarizing film has two protective films, the materials of the two protective films may be the same or different. For example, a protective film made of a thermoplastic resin may be bonded to one main surface of the polarizer via an adhesive, and a protective film made of a thermosetting resin or an ultraviolet-curable resin may be bonded to the other main surface of the polarizer. The protective film may contain one or more optional additives, such as ultraviolet absorbers, antioxidants, lubricants, plasticizers, release agents, color inhibitors, flame retardants, nucleating agents, antistatic agents, pigments, and colorants.

[0151] The thickness of the protective film can be determined as appropriate, but is generally about 10 to 200 μm in view of strength, workability such as handling, thinness, and the like.

[0152] The polarizer and the protective film are usually adhered to each other via an aqueous adhesive or the like. Examples of aqueous adhesives include isocyanate-based adhesives, polyvinyl alcohol-based adhesives, gelatin-based adhesives, vinyl latex, aqueous polyurethane, and aqueous polyester. Examples of adhesives other than the above-mentioned adhesives include ultraviolet-curable adhesives and electron beam-curable adhesives. Electron beam-curable polarizing plate adhesives exhibit suitable adhesive properties for various protective films. The adhesive may contain a metal compound filler.

[0153] In the polarizing film, a retardation film or the like can be formed on the polarizer instead of the protective film. Another protective film or a retardation film or the like can be further provided on the protective film.

[0154] The protective film may have a hard coat layer on the surface opposite to the surface bonded to the polarizer, and may also be subjected to treatments for purposes such as anti-reflection, anti-sticking, diffusion, and anti-glare.

[0155] The polarizing film may be a circular polarizing film.

[0156] The retardation film may be a film obtained by stretching a polymer film or a film obtained by aligning and fixing a liquid crystal material. The retardation film has birefringence, for example, in the in-plane and / or thickness direction.

[0157] Examples of the retardation film include anti-reflection retardation films (see JP 2012-133303 A,

[0221] ,

[0222] ,

[0228] ), viewing angle compensation retardation films (see JP 2012-133303 A,

[0225] ,

[0226] ), and tilted orientation retardation films for viewing angle compensation (see JP 2012-133303 A,

[0227] ).

[0158] The retardation film is not particularly limited in terms of, for example, retardation value, arrangement angle, three-dimensional birefringence, whether it is a single layer or a multilayer, etc., as long as it substantially has the above-mentioned functions, and a known retardation film can be used.

[0159] The thickness of the retardation film is preferably 20 μm or less, more preferably 10 μm or less, still more preferably 1 to 9 μm, and particularly preferably 3 to 8 μm.

[0160] The retardation film is composed of, for example, two layers of a quarter wave plate and a half wave plate in which a liquid crystal material is oriented and fixed.

[0161] 1 , the second optical film 3 has two main surfaces facing each other. One main surface faces the first pressure-sensitive adhesive sheet 2 and is the surface of the second optical film 3 on which the first pressure-sensitive adhesive sheet 2 is laminated. The other main surface of the second optical film 3 faces the second pressure-sensitive adhesive sheet 4 and is the surface of the second optical film 3 on which the second pressure-sensitive adhesive sheet 4 is laminated.

[0162] The second optical film 3 may be composed of a single layer or a laminate of multiple layers. In other words, the second optical film 3 may be composed of a single film or a laminate of multiple films. The films constituting the second optical film 3 may be bonded together via any adhesive and any pressure-sensitive adhesive sheet. When the second optical film 3 is a laminate of multiple films, the second optical film 3 includes, for example, at least one selected from the group consisting of a polarizing film and a retardation film. The second optical film 3 may be a laminate including a polarizing film and / or a retardation film.

[0163] The second optical film 3 may include a laminate of a plurality of retardation films. The second optical film 3 may include a laminate of a first retardation film and a second retardation film. The first retardation film may be bonded to the second retardation film via any adhesive and any pressure-sensitive adhesive sheet.

[0164] The second optical film 3 includes, for example, multiple layers. The multiple layers are, for example, a laminate including a polarizer and at least one film. The at least one film included in the second optical film 3 may be disposed between the polarizer and the second pressure-sensitive adhesive sheet. That is, the second optical film 3 may include at least one film disposed at a position closer to the second pressure-sensitive adhesive sheet than the polarizer.

[0165] Fig. 4A is a cross-sectional view schematically illustrating an example of the second optical film. As shown in Fig. 4A, the second optical film 3A includes a film A31, a polarizer 32, a film B33, and a film C34 laminated in this order. The films A31 and B33 may be protective films for the polarizer. The film C34 may be a retardation film. However, the films A to C may also have functions other than those described above. For example, the film A and / or the film B may have the function of a retardation film.

[0166] The photoelastic coefficients of the films B33 and C34 disposed between the polarizer 32 and the second adhesive sheet 4 are each 4×10 -11 m 2 The photoelastic coefficient is preferably 2×10 -11 m 2 / N or less, and more preferably 1×10 -11 m 2 / N or less, and more preferably 5×10 -12 m 2 The lower limit of the photoelastic coefficient is not particularly limited, but is, for example, 2×10 -13 m 2 / N or more, preferably 5×10 -13 m 2 / N or more, and more preferably 1×10 -12 m 2 / N or more. At least one retardation film may be disposed between the polarizer 32 and the second adhesive sheet 4.

[0167] In the following description, in the case where both the film B33 and the film C34 function as retardation films, the film B33 may be referred to as the first retardation film 33 and the film C34 as the second retardation film 34.

[0168] (Polarizing Plate) The polarizing plate 30 is, for example, a laminate of a polarizer 32 and a protective film 31 arranged on the viewing side of the polarizer 32. The protective film 31 is typically attached to the viewing side of the polarizer 32 via any appropriate adhesive sheet. The protective film 31 is located between the polarizer 32 and the first adhesive sheet 2 and is in contact with the first adhesive sheet 2. The polarizing plate 30 may be a laminate further including a second protective film on the side opposite the viewing side of the polarizer 32.

[0169] (Polarizer) Any appropriate polarizer can be adopted as the polarizer 32. For example, the resin film forming the polarizer 32 may be a single-layer resin film or a laminate of two or more layers.

[0170] A specific example of a polarizer composed of a single-layer resin film is a PVA-based resin film that has been subjected to a dyeing treatment with iodine and a stretching treatment (typically, uniaxial stretching). The dyeing with iodine is performed, for example, by immersing the PVA-based film in an iodine aqueous solution. The stretching ratio of the uniaxial stretching is preferably 3 to 7 times. The stretching may be performed after the dyeing treatment or while dyeing. Alternatively, the stretching may be performed before dyeing. If necessary, the PVA-based resin film may be subjected to a swelling treatment, a crosslinking treatment, a washing treatment, a drying treatment, or the like. For example, by immersing the PVA-based resin film in water and washing it before dyeing, it is possible to clean off stains and antiblocking agents on the surface of the PVA-based resin film and also to swell the PVA-based resin film, thereby preventing uneven dyeing and the like.

[0171] Specific examples of polarizers obtained using laminates include a laminate of a resin substrate and a PVA-based resin layer (PVA-based resin film) laminated on the resin substrate, or a polarizer obtained using a laminate of a resin substrate and a PVA-based resin layer coated on the resin substrate. A polarizer obtained using a laminate of a resin substrate and a PVA-based resin layer coated on the resin substrate can be produced, for example, by applying a PVA-based resin solution to the resin substrate and drying the solution to form a PVA-based resin layer on the resin substrate to obtain a laminate of the resin substrate and the PVA-based resin layer, and then stretching and dyeing the laminate to convert the PVA-based resin layer into a polarizer. A polarizer obtained using a laminate of a resin substrate and a PVA-based resin layer coated on the resin substrate preferably has a polyvinyl alcohol-based resin layer containing a halide and a polyvinyl alcohol-based resin formed on one side of the resin substrate. Stretching typically involves immersing the laminate in an aqueous boric acid solution to stretch it. Furthermore, the stretching may optionally include in-air stretching of the laminate at a high temperature (e.g., 95°C or higher) before stretching in the boric acid aqueous solution. In addition, the laminate is preferably subjected to a drying shrinkage treatment in which the laminate is heated while being transported in the longitudinal direction, thereby shrinking the laminate by 2% or more in the width direction. Typically, a polarizer manufacturing method includes subjecting the laminate to an auxiliary in-air stretching treatment, a dyeing treatment, an underwater stretching treatment, and a drying shrinkage treatment, in this order. By introducing auxiliary stretching, it is possible to increase the crystallinity of the PVA, even when the PVA is coated on a thermoplastic resin, thereby achieving high optical properties. Furthermore, by simultaneously increasing the orientation of the PVA in advance, problems such as a decrease in orientation or dissolution of the PVA when immersed in water in the subsequent dyeing or stretching steps can be prevented, thereby achieving high optical properties. Furthermore, when the PVA-based resin layer is immersed in a liquid, the disordering of the polyvinyl alcohol molecules and the decrease in orientation can be suppressed compared to when the PVA-based resin layer does not contain a halide. This can improve the optical properties of a polarizer obtained through a treatment step in which the laminate is immersed in a liquid, such as a dyeing treatment and an underwater stretching treatment.Furthermore, by shrinking the laminate in the width direction through a drying shrinkage treatment, the optical properties can be improved.The obtained resin substrate / polarizer laminate may be used as is (i.e., the resin substrate may be used as a protective layer for the polarizer), or the resin substrate may be peeled off from the resin substrate / polarizer laminate and any appropriate protective layer depending on the purpose may be laminated on the peeled surface. Details of such a method for producing a polarizer are described in, for example, JP-A-2012-73580 and Japanese Patent No. 6,470,455. The entire disclosures of these publications are incorporated herein by reference.

[0172] The polarizer 32 is preferably made up of a laminate of two or more layers, and more preferably made up of a laminate of a resin substrate and a PVA-based resin layer formed by coating on the resin substrate.

[0173] The thickness of the polarizer 32 is preferably 15 μm or less, more preferably 12 μm or less, even more preferably 10 μm or less, and particularly preferably 8 μm or less, and is typically 1 μm or more, preferably 3 μm or more. When the thickness of the polarizer 32 is in this range, warping of the optical laminate in a high-humidity environment can be more stably suppressed.

[0174] The polarizer 32 preferably exhibits absorptive dichroism at any wavelength between 380 nm and 780 nm. The polarizer 32 has a single transmittance of, for example, 41.5% to 46.0%, preferably 43.0% to 46.0%, and more preferably 44.5% to 46.0%. The polarizer 32 has a degree of polarization of preferably 97.0% or more, more preferably 99.0% or more, and even more preferably 99.9% or more.

[0175] (Protective Film) The protective film 31 is formed of any appropriate film that can be used as a protective layer for the polarizer 32. Specific examples of materials that can be the main component of the film include cellulose-based resins such as triacetyl cellulose (TAC), and transparent resins such as polyesters, polyvinyl alcohols, polycarbonates, polyamides, polyimides, polyethersulfones, polysulfones, polystyrenes, polynorbornenes, polyolefins, (meth)acrylics, and acetates. Other examples include thermosetting resins or ultraviolet-curable resins such as (meth)acrylics, urethanes, (meth)acrylic urethanes, epoxy resins, and silicone resins. Other examples include glassy polymers such as siloxane polymers. Polymer films described in JP 2001-343529 A (WO 01 / 37007) can also be used. Examples of materials that can be used for this film include a resin composition containing a thermoplastic resin having a substituted or unsubstituted imide group in its side chain and a thermoplastic resin having a substituted or unsubstituted phenyl group and a nitrile group in its side chain, such as a resin composition containing an alternating copolymer of isobutene and N-methylmaleimide and an acrylonitrile-styrene copolymer. The polymer film can be, for example, an extrusion molded product of the above resin composition.

[0176] The protective film 31 contains, for example, a (meth)acrylic resin. For example, a (meth)acrylic resin having a glutarimide structure is used as the (meth)acrylic resin. Examples of (meth)acrylic resins having a glutarimide structure are described in JP 2006-309033 A, JP 2006-317560 A, JP 2006-328329 A, JP 2006-328334 A, JP 2006-337491 A, JP 2006-337492 A, JP 2006-337493 A, JP 2006-337569 A, JP 2007-009182 A, JP 2009-161744 A, and JP 2010-284840 A. These descriptions are incorporated herein by reference.

[0177] The thickness of the protective film 31 is typically 300 μm or less, preferably 100 μm or less, more preferably 5 μm to 80 μm, and even more preferably 10 μm to 60 μm.

[0178] (First Retardation Film) When the film B33 functions as a retardation film, the first retardation film 33 may be composed of a retardation film having any appropriate optical and / or mechanical properties depending on the purpose. The first retardation film 33 is composed of, for example, a single layer. The first retardation film 33 is located on the side opposite the viewing side of the polarizing plate 30 described above. Specifically, the first retardation film 33 is attached to the side opposite the viewing side of the polarizer 32 via any appropriate adhesive sheet. In this case, the first retardation film 33 is disposed between the polarizer 32 and the second adhesive sheet 4. That is, the first retardation film 33 is provided closer to the second adhesive sheet 4 than the polarizer 32. The first retardation film 33 may also serve as a protective layer on the side opposite the viewing side of the polarizer 32.

[0179] The thickness of the first retardation film 33 is preferably 10 μm to 60 μm, and more preferably 20 μm to 50 μm.

[0180] The in-plane retardation Re(550) of the first retardation film 33 is preferably 80 nm to 150 nm, more preferably 90 nm to 140 nm, and even more preferably 100 nm to 130 nm.

[0181] The refractive index characteristics of the first retardation film 33 preferably satisfy the relationship nx>ny>nz. The Nz coefficient of the first retardation film 33 is preferably 1.1 to 3.0, and more preferably 1.3 to 2.7.

[0182] The first retardation film 33 can be preferably disposed so that its slow axis is substantially parallel to the absorption axis of the polarizer.

[0183] The photoelastic coefficient of the first retardation film 33 is, for example, as described above. By appropriately adjusting the photoelastic coefficient of the first retardation film 33, it is possible to obtain an optical laminate 10A that is more suitable for suppressing display defects even when a small object collides with or presses the screen over a small contact area. In addition, by appropriately adjusting the photoelastic coefficient of the first retardation film 33, phase difference changes are less likely to occur when shrinkage stress occurs during heating. Therefore, by appropriately adjusting the photoelastic coefficient of the first retardation film 33, thermal unevenness can be effectively prevented when the optical laminate 10A is applied to an image display device.

[0184] The first retardation film 33 may exhibit a reverse wavelength dispersion characteristic in which the retardation value increases with the wavelength of the measurement light, a positive wavelength dispersion characteristic in which the retardation value decreases with the wavelength of the measurement light, or a flat wavelength dispersion characteristic in which the retardation value changes little with the wavelength of the measurement light. The first retardation film 33 preferably exhibits a flat wavelength dispersion characteristic. Specifically, the Re(450) / Re(550) of the first retardation film 33 is preferably 0.99 to 1.03, and the Re(650) / Re(550) is preferably 0.98 to 1.02. By arranging a λ / 2 plate and a λ / 4 plate having flat wavelength dispersion characteristics at a predetermined axial angle, it is possible to obtain characteristics close to ideal reverse wavelength dispersion characteristics, resulting in excellent antireflection properties.

[0185] The first retardation film 33 may be made of any appropriate resin film that can satisfy the above-mentioned characteristics. Examples of such resins include cyclic olefin-based resins, polycarbonate-based resins, cellulose-based resins, polyester-based resins, polyvinyl alcohol-based resins, polyamide-based resins, polyimide-based resins, polyether-based resins, polystyrene-based resins, and acrylic-based resins. A cyclic olefin-based resin may be suitably used for the first retardation film 33. The first retardation film 33 may be obtained, for example, by appropriately stretching a film formed from the above-mentioned resin.

[0186] (Second Retardation Film) When the film C34 functions as a retardation film, the second retardation film 34 may be composed of a retardation film having any appropriate optical and / or mechanical properties depending on the purpose. The second retardation film 34 is composed of, for example, a single layer. The second retardation film 34 is located on the side opposite the viewing side of the first retardation film 33. The second retardation film 34 is disposed between the polarizer 32 and the second adhesive sheet 4. That is, the second retardation film 34 is provided in a position closer to the second adhesive sheet 4 than the polarizer 32. The second retardation film 34 is preferably disposed between the first retardation film 33 and the second adhesive sheet 4.

[0187] The thickness of the second retardation film 34 is preferably 5 μm to 50 μm, and more preferably 5 μm to 40 μm.

[0188] The in-plane retardation Re(550) of the second retardation film 34 is preferably 10 nm to 60 nm, more preferably 20 nm to 50 nm, and even more preferably 30 nm to 40 nm.

[0189] The refractive index characteristics of the second retardation film 34 preferably satisfy the relationship nz>nx>ny. The Nz coefficient of the second retardation film 34 is preferably −10 to −0.1, and more preferably −5 to −1.

[0190] The second retardation film 34 can be preferably disposed so that its slow axis is substantially perpendicular to the absorption axis of the polarizer.

[0191] The second retardation film 34 may be composed of any appropriate resin film that can satisfy the above-mentioned characteristics. An example of such a resin may be a polymer having negative intrinsic birefringence. A polymer having negative intrinsic birefringence is a polymer in which, when oriented by stretching or the like, the refractive index in the orientation direction becomes relatively small. Examples of polymers having negative intrinsic birefringence include those in which chemical bonds and functional groups with large polarization anisotropy, such as aromatic or carbonyl groups, are introduced into the side chains of the polymer. Specific examples of polymers having negative intrinsic birefringence include modified polyolefin-based resins (e.g., modified polyethylene-based resins), acrylic-based resins, styrene-based resins, maleimide-based resins, and fumaric acid ester-based resins. The second retardation film may be obtained, for example, by appropriately stretching a film formed from the above-mentioned resin.

[0192] The optical laminate 10A may include at least one selected from the group consisting of a first retardation film and a second retardation film as the second optical film 3, and the optical laminate 10A may not include the first retardation film and / or the second retardation film.

[0193] 4B is a cross-sectional view schematically showing another example of the second optical film. As shown in FIG. 4B, the second optical film 3B has a film A31, a polarizer 32, and a film D35 laminated in this order. The film A31 may be a protective film for the polarizer. The film D35 may be a retardation film or a protective film for the polarizer. When the film D35 is a protective film for the polarizer, the films A31 and D35 may be the same type of protective film or different types of protective films. The film A may be a film that performs a function other than the above. For example, the film A may have a function as a retardation film.

[0194] The photoelastic coefficient of the film D35 disposed between the polarizer 32 and the second adhesive sheet 4 is 4×10 -11 m 2 The photoelastic coefficient is preferably 2×10 -11 m2 / N or less, and more preferably 1×10 -11 m 2 / N or less, and more preferably 5×10 -12 m 2 The lower limit of the photoelastic coefficient is not particularly limited, but is, for example, 2×10 -13 m 2 / N or more, preferably 5×10 -13 m 2 / N or more, and more preferably 1×10 -12 m 2 / N or more. At least one retardation film may be disposed between the polarizer 32 and the second adhesive sheet 4.

[0195] The following describes an embodiment in which the film D35 functions as a protective film for a polarizer.

[0196] 4B , the second optical film 3B includes a polarizer 32. In addition, the second optical film 3B has a configuration in which a protective film 35 is disposed between the polarizer 32 and the second adhesive sheet 4. That is, in the second optical film 3B, the protective film 35 is provided at a position closer to the second adhesive sheet 4 than the polarizer 32.

[0197] The photoelastic coefficient of the protective film 35 is, for example, as described above. By appropriately adjusting the photoelastic coefficient of the protective film 35, it is possible to obtain the optical laminate 10A that is more suitable for suppressing display defects even when a small object collides with or presses the screen over a small contact area.

[0198] (Optical laminate) The thickness T of the optical laminate 10A is, for example, 200 μm or more. The thickness of the optical laminate 10A is preferably 250 μm or more, more preferably 500 μm or more, even more preferably 1000 μm or more, and particularly preferably 1500 μm or more. The upper limit of the thickness of the optical laminate 10A is, for example, 5000 μm or less, preferably 3000 μm or less, more preferably 2000 μm or less, and even more preferably 1000 μm or less.

[0199] The optical laminate 10A may not include a cover glass on the surface opposite to the side on which the first adhesive sheet 2 is formed of the first optical film 1. Even with this configuration, the optical laminate 10A includes the first adhesive sheet 2, and therefore, in an image display device including the optical laminate 10A, even when a small object collides with or presses the screen over a small contact area, display defects of the image display device can be further suppressed.

[0200] Fig. 5 is a cross-sectional view schematically showing another example of an optical laminate. As shown in Fig. 5, the optical laminate 10B is a laminate including the optical laminate 10A, a third optical film 5, and a third adhesive sheet 6. In detail, the optical laminate 10B has a laminate structure in which a first optical film 1, a first adhesive sheet 2, a second optical film 3, a second adhesive sheet 4, a third optical film 5, and a third adhesive sheet 6 are laminated in this order. The optical laminate 10B can be used, for example, by being attached to an image forming layer via the third adhesive sheet 6.

[0201] The thickness of the optical laminate 10B is, for example, 200 μm or more. The thickness of the optical laminate 10B is preferably 250 μm or more, and more preferably 300 μm or more. The upper limit of the thickness of the optical laminate 10B is, for example, 6000 μm or less, preferably 5000 μm or less, more preferably 3000 μm or less, even more preferably 2000 μm or less, and particularly preferably 1000 μm or less.

[0202] (Third Adhesive Sheet) The third adhesive sheet 6 is formed on the third optical film 5. The third adhesive sheet 6 is formed on one main surface of the third optical film 5. In Fig. 5 , the third adhesive sheet 6 is formed on the entire one main surface of the third optical film 5. However, the third adhesive sheet 6 may be formed on only a part of one main surface of the third optical film 5.

[0203] The thickness T3 of the third pressure-sensitive adhesive sheet 6 is, for example, 5 μm or more and 100 μm or less, preferably 8 μm or more and 80 μm or less, more preferably 10 μm or more and 50 μm or less, and even more preferably 12 μm or more and 30 μm or less. By appropriately adjusting the thickness of the third pressure-sensitive adhesive sheet 6, the adhesion between the third optical film 5 and the third pressure-sensitive adhesive sheet 6 can be improved.

[0204] A known pressure-sensitive adhesive can be used for the third pressure-sensitive adhesive sheet 6. The third pressure-sensitive adhesive sheet 6 may be a pressure-sensitive adhesive sheet formed from a photocurable pressure-sensitive adhesive composition (I) or a solvent-based pressure-sensitive adhesive composition (II). The first pressure-sensitive adhesive sheet 2 or the second pressure-sensitive adhesive sheet 4 may be used for the third pressure-sensitive adhesive sheet 6.

[0205] 5 , the third optical film 5 has two main surfaces facing each other. One main surface faces the second pressure-sensitive adhesive sheet 4 and is the surface of the third optical film 5 on which the second pressure-sensitive adhesive sheet 4 is laminated. The other main surface of the third optical film 5 faces the third pressure-sensitive adhesive sheet 6 and is the surface of the third optical film 5 on which the third pressure-sensitive adhesive sheet 6 is laminated.

[0206] The third optical film 5 includes, for example, at least one selected from the group consisting of a polarizing film and a retardation film. The third optical film 5 may be a laminated film including a polarizing film and / or a retardation film.

[0207] [Embodiment of Image Display Device] An example of an image display device of this embodiment is shown in Figure 6. The image display device 11 of Figure 6 has a layered structure in which an optical laminate 10A, an image forming layer (e.g., an organic EL layer or liquid crystal layer) 7, and a substrate 8 are layered in this order. That is, the image display device 11 of Figure 6 has a layered structure in which a first optical film 1, a first pressure-sensitive adhesive sheet 2, a second optical film 3, a second pressure-sensitive adhesive sheet 4, the image forming layer 7, and a substrate 8 are layered in this order. The image display device 11 may have the optical laminate 10B of Figure 5 instead of the optical laminate 10A. The image forming layer 7 and the substrate 8 may have the same configurations as the image forming layer and the substrate, respectively, provided in known image display devices.

[0208] The image display device 11 in Fig. 6 may be an organic EL display or a liquid crystal display. However, the image display device 11 is not limited to this example. The image display device 11 may also be an electroluminescence (EL) display, a plasma display (PD), a field emission display (FED), or the like. The image display device 11 can be used for home appliances, in-vehicle applications, public information displays (PID), and the like.

[0209] The image display device of this embodiment can have any configuration as long as it includes the optical laminate of this embodiment.

[0210] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to the examples shown below.

[0211] 7 is a cross-sectional view schematically illustrating optical laminates according to Examples 1 to 4 and 6 and Comparative Examples 1 to 4. As shown in FIG. 7, the optical laminates 40 according to Examples 1 to 4 and 6 and Comparative Examples 1 to 4 are laminates in which a first optical film 1, a first pressure-sensitive adhesive sheet 2, a second optical film 3A, and a second pressure-sensitive adhesive sheet 4 are laminated in this order. The second optical film 3A had a structure in which a protective film 31, a polarizer 32, a first retardation film 33, and a second retardation film 34 were laminated in this order. The first retardation film 33 and the second retardation film 34 were disposed between the polarizer 32 and the second pressure-sensitive adhesive sheet 4. That is, the first retardation film 33 and the second retardation film 34 were provided closer to the second pressure-sensitive adhesive sheet 4 than the polarizer 32.

[0212] Fig. 8 is a cross-sectional view schematically showing an optical laminate according to Example 5. As shown in Fig. 8, the optical laminate 41 according to Example 5 is a laminate in which a first optical film 1, a first pressure-sensitive adhesive sheet 2, a second optical film 3B, and a second pressure-sensitive adhesive sheet 4 are laminated in this order. The second optical film 3B had a structure in which a protective film 31, a polarizer 32, and a protective film 35 were laminated in this order. The protective film 35 was disposed between the polarizer 32 and the second pressure-sensitive adhesive sheet 4. That is, the protective film 35 was provided in a position closer to the second pressure-sensitive adhesive sheet 4 than the polarizer 32.

[0213] For convenience, the following description will be given based on the reference numerals given in FIGS.

[0214] [Evaluation Method] <Breaking Elongation> In Examples 1 to 5 and Comparative Examples 1 to 4, a laminate LX composed of a release liner A, a first PSA sheet 2 (thickness: 20 μm), and a release liner B was prepared using the same preparation method as for the laminate L1b described below, except that the thickness of the first PSA sheet 2 was 20 μm. This laminate LX was cut into a size of 3 cm wide x 10 cm long, and the release liner B was peeled off to prepare a test sample. In Example 6, a laminate LY in which a first PSA sheet 2 (thickness: 20 μm) was formed on the surface of a PET film was prepared using the same preparation method as for the laminate L6 described below, except that the thickness of the first PSA sheet 2 was 20 μm. This laminate LY was cut into a size of 3 cm wide x 10 cm long to prepare a test sample. For each test sample, a test piece was prepared by rolling the first PSA sheet 2 lengthwise on the release liner into a string-like shape. The release liner was peeled off from this test piece, and the string-like first adhesive sheet 2 was set in a tensile tester, and a tensile test was performed under conditions of an initial chuck distance of 10 mm and a tensile speed of 300 mm / min. The length of the test piece when it broke during the tensile test was measured and taken as L1 [mm]. The breaking elongation was calculated using the following formula: Breaking elongation [%] = {(L1 - L0) / L0} × 100

[0215] In the above formula, L0 [mm] represents the initial length of the test piece in the longitudinal direction (before the tensile test). The tensile tester used was an Autograph AG-10G tensile tester manufactured by Shimadzu Corporation. The tensile test was performed by pulling the test piece in the longitudinal direction.

[0216] The breaking elongation of the second pressure-sensitive adhesive sheet 4 was calculated by the same method as above, except that the laminate L2a was used.

[0217] <Puncture test> The optical laminates 40 and 41 according to the examples and comparative examples were cut into a size of 5 cm x 5 cm to prepare test samples. Next, the test samples were attached to a glass plate having a thickness of 1.2 mm via a second adhesive sheet 4 to prepare measurement samples.

[0218] The measurement samples according to the examples and comparative examples were placed on the stage of an Indenter CMS tester (manufactured by Instron, product name: 5581) equipped with a piercing jig. The piercing jig had a rounded, pointed tip. In addition, the radius of curvature R of the tip of the piercing jig was 550 μm. The piercing jig was pierced into the test sample on the stage at room temperature (23°C ± 3°C) with a load of 5 kg. The optical laminates 40 and 41 after the piercing test were arranged so that the polarizers 32 of the optical laminates 40 and 41 and a polarizer attached to a microscope were in a crossed Nicol configuration. Light leakage at this time was observed using a microscope (objective lens magnification: 5x). Evaluation was based on the following criteria: A: No light leakage was observed. B: Light leakage was observed, but had no practical impact. C: Light leakage was so significant that it was practically unacceptable.

[0219] <Photoelastic Coefficient> In the second optical films 3A and 3B used in the examples and comparative examples, the film (layer) disposed between the polarizer 32 and the second adhesive sheet 4 was cut into a size of 20 mm x 100 mm to prepare a sample. The sample was measured using an ellipsometer (manufactured by JASCO Corporation, M-150) with light having a wavelength of 550 nm to measure the photoelastic coefficient.

[0220] <Smoothness> Evaluation samples were prepared by attaching the optical laminates 40 and 41 according to the examples and comparative examples to a black plate via the second adhesive sheet 4. Whether or not the evaluation samples were smooth was visually confirmed from the first optical film 1 side of the evaluation sample, and evaluated according to the following criteria: A: There was an inconspicuous unevenness. B: There was a very noticeable unevenness.

[0221] <Weight-average molecular weight of (meth)acrylic polymer> The weight-average molecular weight (Mw) of the (meth)acrylic polymer was measured by GPC (gel permeation chromatography). Analytical device: HLC-8120GPC manufactured by Tosoh Corporation Column: G7000H manufactured by Tosoh Corporation XL +GMH XL +GMH XL Column size: 7.8 mm diameter x 30 cm, total 90 cm Column temperature: 40°C Flow rate: 0.8 mL / min Injection volume: 100 μL Eluent: tetrahydrofuran Detector: differential refractometer (RI) Standard sample: polystyrene

[0222] [First Optical Film 1 (Polarizing Film)] A long, amorphous isophthalic copolymerized polyethylene terephthalate film (thickness: 100 μm) having a Tg of approximately 75° C. was used as a thermoplastic resin substrate, and one side of the resin substrate was subjected to a corona treatment.

[0223] A PVA aqueous solution (coating solution) was prepared by adding 13 parts by weight of potassium iodide to 100 parts by weight of a PVA-based resin prepared by mixing polyvinyl alcohol (polymerization degree 4200, saponification degree 99.2 mol%) and acetoacetyl-modified PVA (manufactured by Nippon Synthetic Chemical Industry Co., Ltd., trade name "GOHSEFIRMER") in a ratio of 9:1. The resulting mixture was dissolved in water.

[0224] The above PVA aqueous solution was applied to the corona treated surface of the resin substrate and dried at 60° C. to form a PVA-based resin layer with a thickness of 13 μm, thereby producing a laminate.

[0225] The resulting laminate was uniaxially stretched 2.4 times in the machine direction (longitudinal direction) in an oven at 130°C (in-air auxiliary stretching treatment).

[0226] Next, the laminate after the auxiliary air-stretching treatment was immersed for 30 seconds in an insolubilizing bath at a liquid temperature of 40°C (insolubilizing treatment). The insolubilizing bath was an aqueous boric acid solution obtained by blending 4 parts by weight of boric acid with 100 parts by weight of water.

[0227] Next, the film was immersed in a dye bath at a liquid temperature of 30° C. for 60 seconds while adjusting the concentration so that the single transmittance (Ts) of the polarizer finally obtained would be a desired value (dyeing treatment). The dye bath was an aqueous iodine solution obtained by blending iodine and potassium iodide in a weight ratio of 1:7 with 100 parts by weight of water.

[0228] Next, the sample was immersed for 30 seconds in a crosslinking bath at a liquid temperature of 40° C. (crosslinking treatment). The crosslinking bath was an aqueous boric acid solution obtained by mixing 3 parts by weight of potassium iodide and 5 parts by weight of boric acid with 100 parts by weight of water.

[0229] Thereafter, the laminate was immersed in an aqueous boric acid solution at a liquid temperature of 70° C. and uniaxially stretched in the machine direction (longitudinal direction) between rolls with different peripheral speeds to a total stretch ratio of 5.5 (underwater stretching treatment). The aqueous boric acid solution was an aqueous solution containing 4% by weight of boric acid and 5% by weight of potassium iodide.

[0230] Thereafter, the laminate was immersed in a cleaning bath at a liquid temperature of 20° C. (cleaning treatment) The cleaning bath was an aqueous solution obtained by mixing 4 parts by weight of potassium iodide with 100 parts by weight of water.

[0231] Thereafter, the film was dried in an oven maintained at about 90° C., and brought into contact with a heated roll made of SUS whose surface temperature was maintained at about 75° C. (drying shrinkage treatment).

[0232] In this way, a polarizer having a thickness of about 5 μm was formed on the resin substrate.

[0233] An acrylic resin film (thickness: 40 μm) having a glutarimide structure as a protective layer was bonded to the surface of the obtained polarizer (the surface opposite to the resin substrate) via a UV-curable adhesive. Specifically, the curable adhesive was applied so that the total thickness was approximately 2.0 μm, and the films were bonded using a roller. The adhesive was then cured by irradiating it with UV light from the acrylic resin film side. The resin substrate was then peeled off to obtain a polarizing film (first optical film 1) having a configuration of acrylic resin film (protective layer) / polarizer.

[0234] [Second Optical Film] In Examples 1 to 4 and 6 and Comparative Examples 1 to 4 (see FIG. 7 ), a laminate X having a configuration in which a protective film 31, a polarizer 32, a first retardation film 33, and a second retardation film 34 were laminated in this order was used as the second optical film 3A. The polarizer prepared above was used as the polarizer 32. The protective film 31 was an acrylic resin film (manufactured by Kaneka Corporation, product name: HTX) (thickness: 40 μm) having a glutarimide structure. The protective film 31 and the polarizer 32 were bonded together via an ultraviolet-curable adhesive.

[0235] A cyclic olefin film (manufactured by Zeon Corporation, product name: Zeonorfilm ZT12-50135) was used as the first retardation film 33. The thickness of the first retardation film 33 was 18 μm.

[0236] The second retardation film 34 was prepared as follows.

[0237] [Polymer synthesis and dope preparation] 48 parts by weight of hydroxypropyl methylcellulose (manufactured by Shin-Etsu Chemical Co., Ltd., trade name: Metrose 60SH-50), 15,601 parts by weight of distilled water, 8,161 parts by weight of diisopropyl fumarate, 240 parts by weight of 3-ethyl-3-oxetanylmethyl acrylate, and 45 parts by weight of t-butyl peroxypivalate as a polymerization initiator were placed in an autoclave equipped with a stirrer, a cooling tube, a nitrogen inlet tube, and a thermometer. Nitrogen bubbling was performed for 1 hour, and then the mixture was maintained at 49°C for 24 hours with stirring, thereby carrying out radical suspension polymerization. The mixture was then cooled to room temperature, and the suspension containing the produced polymer particles was centrifuged. The resulting polymer was washed twice with distilled water and twice with methanol and then dried under reduced pressure to obtain a white fumarate ester-based resin.

[0238] The obtained fumaric acid ester-based resin was dissolved in methyl ethyl ketone to prepare a solution with a solid content of 20% by weight. Further, 5 parts by weight of tributyl trimellitate as a plasticizer was added to 100 parts by weight of the fumaric acid ester-based resin to prepare a dope.

[0239] A 75 μm-thick polyester film (biaxially stretched film of polyethylene-terephthalate / isophthalate copolymer) was used as the support film. The dope was applied to a film thickness of about 6 μm after drying and then dried to obtain a laminate A in which a coating film of a fumaric acid ester resin was tightly laminated on the support.

[0240] The laminate A was subjected to free-end uniaxial stretching to obtain a laminate B in which a second retardation film 34 (positive B plate) having a refractive index anisotropy of nz > nx > ny was closely laminated on the support. The support was peeled off from the laminate B to obtain a second retardation film 34 (positive B plate) having a refractive index anisotropy. The first retardation film 33 and the second retardation film 34 were bonded together via an ultraviolet-curable adhesive.

[0241] The photoelastic coefficient of the protective film 31 is 3×10 -12 m 2 The photoelastic coefficient of the first retardation film 33 was 1×10 -12 m 2 The photoelastic coefficient of the second retardation film 34 was 5×10 -11 m 2 / N.

[0242] In Example 5 (see FIG. 8 ), a laminate Y having a configuration in which a protective film 31, a polarizer 32, and a protective film 35 were laminated in this order was used as the second optical film 3B. The polarizer 32 prepared above was used as the polarizer 32. The protective films 31 and 35 were acrylic resin films having a glutarimide structure (manufactured by Kaneka Corporation, product name: HTX) (thickness: 40 μm).

[0243] [Release Liner A] A silicone-based release agent composition was obtained by mixing 30 parts by weight of an addition reaction curable silicone (LTC761 containing a hexenyl group-containing polyorganosiloxane, a 30 wt% toluene solution, manufactured by Dow Corning Toray), 0.9 parts by weight of a release control agent (BY24-850 containing an unreactive silicone resin, manufactured by Dow Corning Toray), and 2 parts by weight of a curing catalyst (SRX212 containing a platinum catalyst, manufactured by Dow Corning Toray), and a toluene / hexane mixed solvent (volume ratio 1:1) as a dilution solvent. The silicone solids concentration in the release agent composition was 1.0 wt%. Next, the release agent composition was applied with a wire bar to one side of a liner substrate (Lumirror XD500P, a polyester film, 75 μm thick), and heated at 130° C. for 1 minute to produce a release liner A having a release layer (thickness 60 nm) on one side.

[0244] [Release Liner B] Release liner B having a release layer (thickness 120 nm) on one side was prepared in the same manner as release liner A, except that the thickness of the release agent composition applied to the liner substrate was changed.

[0245] Monomer Syrup A1: 100 parts by weight of n-butyl acrylate (BA), 5 parts by weight of acrylic acid (AA), 0.16 parts by weight of 1-hydroxycyclohexylphenyl ketone (Omnirad 184, manufactured by IGM Resins BV) as a photopolymerization initiator, and 0.04 parts by weight of bis(2,4,6-trimethylbenzoyl)phenylphosphine oxide (Omnirad 819, manufactured by IGM Resins BV) were placed in a four-neck flask and irradiated with ultraviolet light under a nitrogen atmosphere to obtain a partially photopolymerized monomer syrup A1. UV irradiation was continued until the viscosity of the liquid in the flask reached approximately 20 Pa s (measurement conditions: BH viscometer No. 5 rotor, 10 rpm, measurement temperature 30°C).

[0246]

[0247] The abbreviations in Table 1 are as follows: BA: n-butyl acrylate AA: acrylic acid

[0248] [Photocurable Pressure-Sensitive Adhesive Compositions C1 to C6] Next, photocurable pressure-sensitive adhesive compositions C1 to C3 were obtained by mixing monomer syrups and crosslinking agents so as to obtain the compositions shown in Table 2. The abbreviation "NDDA" in Table 2 stands for 1,9-nonanediol diacrylate.

[0249]

[0250] (Example 1) See Figure 7. A photocurable pressure-sensitive adhesive composition C1 was applied to the surface of the release layer of release liner A using an applicator to form a coating layer (thickness: 50 µm). Next, the above-mentioned release liner B was placed on the formed coating layer to obtain laminate L1a. Release liner B was placed so that the release layer was in contact with the coating layer. Next, an illuminance of 9 mW / cm was applied from the side of release liner A in laminate L1a. 2 Conditions (integrated light amount 868 mJ cm 2 ) was irradiated with light. This photocured the coating layer, forming a laminate L1b composed of release liner A, first pressure-sensitive adhesive sheet 2 (thickness 50 μm), and release liner B. A combination of a black light source and an LED was used as the light source. The peak wavelength of the light irradiated by the LED was 340 nm. The cumulative light amount was the sum of the cumulative light amounts from both light sources.

[0251] Next, the release liner B was peeled off from the laminate L1b, and the above-mentioned polarizing film (first optical film 1) was placed on the exposed surface of the first adhesive sheet 2, thereby obtaining a laminate L1c in which the release liner A, the first adhesive sheet 2, and the polarizing film were laminated in this order. The polarizing film was placed so that the surface on the side of the transparent protective film made of a modified acrylic polymer was in contact with the first adhesive sheet 2.

[0252] Separately, a photocurable pressure-sensitive adhesive composition C3 was applied to the surface of the release layer of release liner A using an applicator to form a coating layer (thickness 15 μm). Next, the above-mentioned release liner B was placed on top of the formed coating layer to obtain laminate L2a. Release liner B was placed so that the release layer was in contact with the coating layer. Next, light was irradiated from the side of release liner A in laminate L2a. This photocured the coating layer, forming laminate L2b composed of release liner A, second PSA sheet 4 (thickness 15 μm), and release liner B. The light irradiation conditions were the same as those used when first PSA sheet 2 was produced.

[0253] Next, the release liner B was peeled off from the laminate L2b, and the laminate X described above as the second optical film 3A was placed on the exposed surface of the second pressure-sensitive adhesive sheet 4 so that the second retardation film 34 was in contact with the second pressure-sensitive adhesive sheet 4, thereby obtaining a laminate L2c in which the release liner A, the second pressure-sensitive adhesive sheet 4, and the second optical film 3A were laminated in this order. The laminate X was placed so that the second retardation film 34 was in contact with the second pressure-sensitive adhesive sheet 4.

[0254] The release liner A was peeled off from the laminate L1c to obtain a laminate L1d. The first pressure-sensitive adhesive sheet 2 of the laminate L1d was transferred to the protective film 31 of the laminate L2c to obtain a laminate L3 in which a polarizing film (first optical film 1), a first pressure-sensitive adhesive sheet 2, a second optical film 3A, a second pressure-sensitive adhesive sheet 4, and a release liner A were laminated in this order. The release liner A was peeled off from the laminate L3 to obtain an optical laminate 40 according to Example 1.

[0255] Example 2 An optical laminate 40 according to Example 2 was obtained in the same manner as in Example 1, except that the thickness of the first pressure-sensitive adhesive sheet 2 was changed to 100 μm.

[0256] Example 3 An optical laminate 40 according to Example 3 was obtained in the same manner as in Example 1, except that the photocurable pressure-sensitive adhesive composition C2 was used instead of the photocurable pressure-sensitive adhesive composition C1.

[0257] Example 4 An optical laminate 40 according to Example 4 was obtained in the same manner as in Example 3, except that the thickness of the first pressure-sensitive adhesive sheet 2 was changed to 100 μm.

[0258] Example 5 See Fig. 8. An optical laminate 41 according to Example 5 was obtained in the same manner as in Example 4, except that laminate Y was used instead of laminate X as the second optical film.

[0259] Example 6 [Preparation of (Meth)acrylic Polymer B1] A monomer mixture containing 79.9 parts by weight of n-butyl acrylate (BA), 5 parts by weight of acrylic acid (AA), 0.1 parts by weight of 4-hydroxybutyl acrylate (HBA), and 15 parts by weight of benzyl acrylate was charged into a four-neck flask equipped with a stirring blade, a thermometer, a nitrogen gas inlet tube, and a condenser. Furthermore, 0.1 parts by weight of 2,2'-azobisisobutyronitrile (AIBN; manufactured by Kishida Chemical Co., Ltd.) as a polymerization initiator was charged together with ethyl acetate per 100 parts by weight of the monomer mixture to prepare a mixture. While gently stirring the mixture, nitrogen gas was introduced into the flask to replace the atmosphere with nitrogen. The liquid temperature in the flask was maintained at around 55°C, and a polymerization reaction was carried out for 7 hours. Ethyl acetate was then added to the resulting reaction solution to adjust the solids concentration to 30%, thereby preparing a solution of (meth)acrylic polymer B1 with a weight-average molecular weight (Mw) of 2,200,000.

[0260] [Adhesive Sheet] A solution of (meth)acrylic adhesive composition D1 (solvent-based adhesive composition) of Example 6 was prepared by further blending 12 parts by weight of a crosslinker (manufactured by Mitsui Chemicals, Inc., product name: Takenate D-101E), 0.1 parts by weight of a silane coupling agent (manufactured by Shin-Etsu Chemical Co., Ltd., product name: KBM-403), and 1 part by weight of a polyether compound having an alkoxysilyl group (manufactured by Kaneka Corporation, product name: Silyl SAT10) with 100 parts by weight of the solids content of the solution of (meth)acrylic polymer B1. Takenate D-101E is a trimethylolpropane / tolylene diisocyanate trimer adduct. KBM-403 is 3-glycidoxypropyltrimethoxysilane.

[0261] (Meth)acrylic pressure-sensitive adhesive composition D1 was applied to the surface of a PET film, which was a base film (release liner), so that the thickness of the pressure-sensitive adhesive sheet after drying would be 100 μm. A fountain coater was used to apply (meth)acrylic pressure-sensitive adhesive composition D1. The coating film formed by application was dried in an air-circulating constant-temperature oven at 90°C for 1 minute to obtain a laminate L6 in which a first pressure-sensitive adhesive sheet 2 was formed on the surface of the PET film. The thickness of the pressure-sensitive adhesive sheet was 100 μm.

[0262] [Optical laminate] See Fig. 7. The first pressure-sensitive adhesive sheet 2 of the obtained laminate L6 was transferred to the above-mentioned polarizing film (first optical film 1), thereby producing a laminate L7 in which the polarizing film (first optical film 1), the first pressure-sensitive adhesive sheet 2, and the base film were laminated in this order.

[0263] The base film was peeled off from the laminate L7 and the exposed surface of the first adhesive sheet 2 was transferred to the protective film 31 of the above-mentioned laminate L2c, thereby obtaining a laminate L8 in which a polarizing film (first optical film 1), a first adhesive sheet 2, a second optical film 3A, a second adhesive sheet 4, and a release liner A were laminated in this order.

[0264] The release liner A was peeled off from the laminate L8 to obtain the optical laminate 40 according to Example 6.

[0265] (Comparative Example 1) An optical laminate 40 according to Comparative Example 1 was obtained by the same method as in Example 1, except that a photocurable pressure-sensitive adhesive composition C3 was used instead of the photocurable pressure-sensitive adhesive composition C1 and the thickness of the first pressure-sensitive adhesive sheet 2 was changed to 12 μm.

[0266] Comparative Example 2 An optical laminate 40 according to Comparative Example 2 was obtained by the same method as in Comparative Example 1, except that the thickness of the first pressure-sensitive adhesive sheet 2 was changed to 50 μm.

[0267] Comparative Example 3 An optical laminate 40 according to Comparative Example 3 was obtained by the same method as in Comparative Example 1, except that the thickness of the first pressure-sensitive adhesive sheet 2 was changed to 100 μm.

[0268] Comparative Example 4 An optical laminate 40 according to Comparative Example 4 was obtained in the same manner as in Example 3, except that the thickness of the first pressure-sensitive adhesive sheet 2 was changed to 12 μm.

[0269]

[0270]

[0271]

[0272] As shown in Table 3, the results of the piercing test were good in each example. The optical laminates according to the examples are suitable for suppressing display defects.

[0273] The optical layered body of the present invention can be used, for example, in an image display device.

Claims

1. An optical laminate comprising a first optical film, a first adhesive sheet, a second optical film, and a second adhesive sheet laminated in this order, wherein the thickness T1 of the first adhesive sheet is 30 μm or more and 1000 μm or less, and the breaking elongation of the first adhesive sheet is 500% or less.

2. The optical laminate according to claim 1, wherein the first adhesive sheet is formed from a photocurable adhesive composition (I) containing a monomer group and / or a partial polymer of the monomer group.

3. The optical laminate according to claim 2, wherein the photocurable pressure-sensitive adhesive composition (I) contains a crosslinking agent, and the amount of the crosslinking agent in the photocurable pressure-sensitive adhesive composition (I) is 0.4 parts by weight or more and 20 parts by weight or less per 100 parts by weight of the total of the monomer group and the partial polymer.

4. The optical laminate according to claim 1, wherein the thickness T of the optical laminate is 200 μm or more.

5. The second optical film includes a plurality of layers, the plurality of layers including a polarizer and at least one film disposed between the polarizer and the second adhesive sheet, and the photoelastic coefficient of the at least one film is 4×10 -11 m 2 The optical laminate according to claim 1, wherein the optical density is 1 / N or less.

6. An image display device comprising the optical laminate according to claim 1.

Citation Information

Patent Citations

  • Roll of optical sheet material and continuous manufacturing method of liquid crystal display device

    WO2011001834A1

  • Layered body for flexible image display device, and flexible image display device

    WO2019026753A1

  • Adhesive sheet used for laminate within flexible image display device, laminate used for flexible image display device, and flexible image display device

    WO2021187278A1

  • Adhesive sheet used in layered product in flexible image display device, layered product used in flexible image display device, and flexible image display device

    WO2021256331A1

  • Adhesive composition, adhesive sheet, optical laminate, and image display device

    WO2022244557A1