Nitride semiconductor device and method for manufacturing nitride semiconductor device
The nitride semiconductor device addresses the challenge of uniform gate layer thickness by using a silicon substrate with a specific surface orientation and epitaxial growth to form a gate layer with a ridge and extension portion, resulting in improved uniformity and gate breakdown voltage.
Patent Information
- Application Number
- PCT/JP2024/008740
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-30
- Filing Date
- 2024-03-07
- Publication Date
- 2024-10-03
AI Technical Summary
Existing nitride semiconductor devices face challenges in achieving uniform thickness of the gate layer's extending portion, leading to potential defects and reduced gate breakdown voltage due to thickness unevenness.
A nitride semiconductor device with a silicon substrate having a specific (111) plane surface and an off-angle of 0 degrees or more and 0.08 degrees or less, where the gate layer includes a ridge portion and an extension portion formed by epitaxial growth and selective etching, ensuring uniform thickness of the extension portion.
This configuration improves the uniformity of the gate layer's thickness, reduces defective portions, and maintains or enhances the gate breakdown voltage, thereby improving the yield and performance of the nitride semiconductor device.
Smart Images

Figure JP2024008740_03102024_PF_FP_ABST
Abstract
Description
NITRIDE SEMICONDUCTOR DEVICE AND METHOD FOR MANUFACTURING NITRIDE SEMICONDUCTOR DEVICE
[0001] The present disclosure relates to a nitride semiconductor device and a method for manufacturing a nitride semiconductor device.
[0002] Currently, high electron mobility transistors (HEMTs) using group III nitride semiconductors (hereinafter sometimes simply referred to as "nitride semiconductors") such as gallium nitride (GaN) are being commercialized. HEMTs use two-dimensional electron gas (2DEG) formed near the interface of a semiconductor heterojunction as a conductive path (channel). Power devices using HEMTs are recognized as devices that enable lower on-resistance and higher speed / frequency operation compared to typical silicon (Si) power devices.
[0003] For example, a nitride semiconductor device described in Patent Document 1 includes an electron transit layer formed of a gallium nitride (GaN) layer and an electron supply layer formed of an aluminum gallium nitride (AlGaN) layer. A 2DEG is formed in the electron transit layer near the heterojunction interface between the electron transit layer and the electron supply layer. Furthermore, in the nitride semiconductor device described in Patent Document 1, a gate layer (e.g., a p-type GaN layer) containing acceptor impurities is provided on the electron transit layer and directly below the gate electrode. In this configuration, the gate layer increases the band energy of the conduction band near the heterojunction interface between the electron transit layer and the electron supply layer in the region directly below the gate layer, thereby eliminating the channel directly below the gate layer and achieving a normally-off mode.
[0004] Japanese Patent Application Laid-Open No. 2017-73506
[0005] In a nitride semiconductor device in which a nitride semiconductor layer containing acceptor-type impurities is provided as a gate layer directly below a gate electrode, a structure in which an extension portion is provided in the gate layer to improve gate breakdown voltage can be adopted. In this structure, it is required that the extension portion be formed with a uniform thickness.
[0006] a gate electrode formed on the gate layer; and a source electrode and a drain electrode formed on the electron supply layer, wherein the gate layer, the source electrode, and the drain electrode are aligned in a first direction on the top surface of the electron supply layer, the gate layer including a ridge portion in contact with the electron supply layer, and an extension portion extending from the ridge portion in the first direction and having a smaller thickness than the ridge portion; the top surface of the silicon substrate is a plane including a first plane formed by a (111) plane, and an off-angle between a reference plane perpendicular to a thickness direction of the silicon substrate and the first plane is greater than or equal to 0 degrees and less than 0.08 degrees.
[0007] A method for manufacturing a nitride semiconductor device according to one aspect of the present disclosure includes forming an electron transit layer made of a nitride semiconductor on an upper surface of a silicon substrate by epitaxial growth, forming an electron supply layer made of a nitride semiconductor having a band gap larger than that of the electron transit layer by epitaxial growth on the electron transit layer, forming a gate layer made of a nitride semiconductor containing acceptor-type impurities on the electron supply layer, forming a gate electrode on the gate layer, and forming a source electrode and a drain electrode on the electron supply layer, wherein the gate layer, the source electrode, and the drain electrode are the gate layer includes a ridge portion in contact with the electron supply layer and an extension portion that extends from the ridge portion in the first direction and is thinner than the ridge portion; forming the gate layer includes forming a nitride semiconductor layer that constitutes the gate layer by epitaxial growth and selectively etching the nitride semiconductor layer to form the ridge portion and the extension portion; the silicon substrate has an upper surface that includes a first plane that is a (111) plane, and an off angle between the first plane and a reference plane that is orthogonal to a thickness direction of the silicon substrate is equal to or greater than 0 degrees and equal to or less than 0.08 degrees.
[0008] According to the nitride semiconductor device and method for manufacturing the nitride semiconductor device of the present disclosure, the uniformity of the thickness of the extension portion of the gate layer can be improved.
[0009] FIG. 1 is an exemplary schematic plan view of a nitride semiconductor device. FIG. 2 is a cross-sectional view taken along line 2-2 of FIG. 1. FIG. 3 is a schematic diagram of the crystal structure of a silicon substrate. FIG. 4 is a schematic cross-sectional view showing an exemplary manufacturing process for the nitride semiconductor device of FIG. 1. FIG. 5 is a schematic cross-sectional view showing an example of the shape of the upper surface of a drain-side extension portion. FIG. 6 is a schematic cross-sectional view showing an example of the shape of the upper surface of a drain-side extension portion of a reference example. FIG. 7 is a graph showing the relationship between the off-angle of a first plane of the upper surface of a silicon substrate and the thickness unevenness of the extension portion.
[0010] Hereinafter, embodiments of nitride semiconductor devices according to the present disclosure will be described with reference to the accompanying drawings. Note that for simplicity and clarity of description, components shown in the drawings are not necessarily drawn to scale. Also, for ease of understanding, hatching lines may be omitted in cross-sectional views. The accompanying drawings merely illustrate embodiments of the present disclosure and should not be considered as limiting the present disclosure.
[0011] The following detailed description includes devices, systems, and methods embodying exemplary embodiments of the present disclosure. This detailed description is merely illustrative in nature and is not intended to limit the embodiments of the present disclosure or the application and uses of such embodiments.
[0012] [Schematic Structure of Nitride Semiconductor Device] FIG. 1 is a schematic plan view of an exemplary nitride semiconductor device 10 according to an embodiment. FIG. 2 is a schematic cross-sectional view of the nitride semiconductor device 10, taken along line 2-2 in FIG. 1. In one example, the nitride semiconductor device 10 may be a HEMT using GaN. Below, the cross-sectional structure of the nitride semiconductor device 10 will be described with reference to FIG. 2, and then the planar structure of the nitride semiconductor device 10 will be described with reference to FIG. 1.
[0013] As shown in FIG. 2 , the nitride semiconductor device 10 includes a silicon substrate 12, a buffer layer 14 formed on the silicon substrate 12, an electron transit layer 16 formed on the buffer layer 14, and an electron supply layer 18 formed on the electron transit layer 16.
[0014] The silicon substrate 12 is a substrate made of silicon. The thickness of the silicon substrate 12 may be, for example, 200 μm or more and 1500 μm or less. The silicon substrate 12 has a substrate upper surface 12A with a specific shape. The shape of the substrate upper surface 12A will be described in detail later.
[0015] 1 and 2, the Z-axis direction of the mutually orthogonal X, Y, and Z axes is the thickness direction of the silicon substrate 12. Note that the term "plan view" used in this specification refers to viewing the nitride semiconductor device 10 from above along the Z-axis direction, unless explicitly stated otherwise.
[0016] The buffer layer 14 is formed on the substrate upper surface 12A of the silicon substrate 12. The buffer layer 14 may be located between the silicon substrate 12 and the electron transit layer 16. In one example, the buffer layer 14 may be made of any material that can facilitate epitaxial growth of the electron transit layer 16. The buffer layer 14 may include one or more nitride semiconductor layers.
[0017] In one example, the buffer layer 14 may include at least one of an aluminum nitride (AlN) layer, an aluminum gallium nitride (AlGaN) layer, and a graded AlGaN layer having different aluminum (Al) compositions. For example, the buffer layer 14 may be composed of a single AlN layer, a single AlGaN layer, a layer having an AlGaN / GaN superlattice structure, a layer having an AlN / AlGaN superlattice structure, or a layer having an AlN / GaN superlattice structure. To suppress leakage current in the buffer layer 14, impurities may be introduced into a portion of the buffer layer 14 to make the buffer layer 14 semi-insulating. In this case, the impurity may be, for example, carbon (C) or iron (Fe), and the impurity concentration may be, for example, 4×10 16 cm -3 It can be more than that.
[0018] The electron transit layer 16 is made of a nitride semiconductor. The electron transit layer 16 is, for example, a GaN layer. The thickness of the electron transit layer 16 is, for example, 0.5 μm or more and 2 μm or less. In order to suppress leakage current in the electron transit layer 16, an impurity may be introduced into a part of the electron transit layer 16 to make the electron transit layer 16 semi-insulating except for the surface region. In this case, the impurity may be, for example, C, and the peak concentration of the impurity in the electron transit layer 16 may be, for example, 1×10 19 cm -3 That's all.
[0019] The electron supply layer 18 is made of a nitride semiconductor having a larger band gap than the electron transit layer 16. The electron supply layer 18 is, for example, an AlGaN layer. In this case, the band gap increases as the Al composition increases, so the electron supply layer 18, which is an AlGaN layer, has a larger band gap than the electron transit layer 16, which is a GaN layer. In one example, the electron supply layer 18 is made of Al x Ga 1-x The electron supply layer 18 is made of N, where x satisfies 0.1<x<0.4, and more preferably 0.2<x<0.3. The thickness of the electron supply layer 18 is, for example, not less than 5 nm and not more than 20 nm.
[0020] The electron transit layer 16 and the electron supply layer 18 are made of nitride semiconductors with different lattice constants. Therefore, the nitride semiconductor (e.g., GaN) that constitutes the electron transit layer 16 and the nitride semiconductor (e.g., AlGaN) that constitutes the electron supply layer 18 form a lattice-mismatched heterojunction. Due to spontaneous polarization in the electron transit layer 16 and the electron supply layer 18 and piezoelectric polarization caused by stress applied to the electron supply layer 18 near the heterojunction interface, the energy level of the conduction band of the electron transit layer 16 near the heterojunction interface is lower than the Fermi level. As a result, a two-dimensional electron gas (2DEG) 20 spreads within the electron transit layer 16 near the heterojunction interface between the electron transit layer 16 and the electron supply layer 18 (e.g., within a range of several nanometers from the interface).
[0021] The nitride semiconductor device 10 further includes a gate layer 22 formed on the electron supply layer 18, a gate electrode 24 formed on the gate layer 22, and a passivation layer 26. The passivation layer 26 is formed on the electron supply layer 18, the gate layer 22, and the gate electrode 24, and includes a first opening 26A and a second opening 26B. The nitride semiconductor device 10 also includes a source electrode 28 in contact with the upper surface 18A of the electron supply layer 18 through the first opening 26A, and a drain electrode 30 in contact with the upper surface 18A of the electron supply layer 18 through the second opening 26B.
[0022] The gate layer 22 is located between the first opening 26A and the second opening 26B of the passivation layer 26 and is spaced apart from each of the first opening 26A and the second opening 26B. The gate layer 22 is located closer to the first opening 26A than to the second opening 26B. The detailed structure of the gate layer 22 will be described later.
[0023] The gate layer 22 has a band gap smaller than that of the electron supply layer 18 and is made of a nitride semiconductor containing acceptor-type impurities. The gate layer 22 can be made of any material having a band gap smaller than that of the electron supply layer 18, which is, for example, an AlGaN layer. In one example, the gate layer 22 is a GaN layer doped with acceptor-type impurities (a p-type GaN layer).
[0024] The acceptor-type impurities may include at least one of magnesium (Mg), zinc (Zn), and C. An example of the acceptor-type impurity is Mg. The maximum concentration of the acceptor-type impurity in the gate layer 22 is, for example, 1×10 18 cm -3 or more, or 1 x 10 19 cm -3 The maximum concentration of the acceptor-type impurity in the gate layer 22 is, for example, 1×10 20 cm -3 The following is the result.
[0025] As described above, the energy levels of the electron transit layer 16 and the electron supply layer 18 are raised by including acceptor-type impurities in the gate layer 22. Therefore, in the region immediately below the gate layer 22, the energy level of the conduction band of the electron transit layer 16 near the heterojunction interface between the electron transit layer 16 and the electron supply layer 18 is approximately the same as or higher than the Fermi level. Therefore, at zero bias when no voltage is applied to the gate electrode 24, no 2DEG 20 is formed in the region of the electron transit layer 16 immediately below the gate layer 22. On the other hand, 2DEG 20 is formed in the region of the electron transit layer 16 other than the region immediately below the gate layer 22.
[0026] In this way, the presence of the gate layer 22 doped with acceptor-type impurities causes the 2DEG 20 to disappear in the region directly below the gate layer 22. As a result, normally-off operation of the transistor is achieved. When an appropriate on-voltage is applied to the gate electrode 24, a channel is formed by the 2DEG 20 in the electron transit layer 16 in the region directly below the gate electrode 24, thereby establishing conduction between the source and drain.
[0027] The gate electrode 24 is composed of one or more metal layers. One example of the gate electrode 24 is a titanium nitride (TiN) layer. Alternatively, the gate electrode 24 may be composed of a first metal layer made of a material containing Ti and a second metal layer made of a material containing TiN and stacked on the first metal layer. The gate electrode 24 can form a Schottky junction with the gate layer 22. The gate electrode 24 can be formed in an area smaller than the gate layer 22 in a plan view. The thickness of the gate electrode 24 is, for example, 50 nm or more and 200 nm or less.
[0028] The passivation layer 26 is formed on the electron supply layer 18. It can also be said that the passivation layer 26 covers the upper surface 18A of the electron supply layer 18. The passivation layer 26 is made of, for example, silicon nitride (SiN), silicon dioxide (SiO 2 ), silicon oxynitride (SiON), alumina (Al 2 O 3 The passivation layer 26 may be made of a material containing one of silicon nitride (SiN), aluminum nitride (AlN), and aluminum oxynitride (AlON). In one example, the passivation layer 26 is made of a material containing silicon nitride (SiN). The portion of the passivation layer 26 covering the gate layer 22 and the gate electrode 24 is formed along the surfaces of the gate layer 22 and the gate electrode 24, and therefore has an uneven surface. The passivation layer 26 has a thickness of, for example, 200 nm or less. Here, the thickness of the passivation layer 26 may be, for example, the thickness of the portion in contact with the electron supply layer 18 or the thickness of the portion in contact with the upper surface of the gate electrode 24.
[0029] The source electrode 28 and the drain electrode 30 are disposed on the upper surface 18A of the electron supply layer 18 so as to sandwich the gate layer 22. Hereinafter, the direction in which the gate layer 22, the source electrode 28, and the drain electrode 30 are aligned on the upper surface 18A of the electron supply layer 18 will be referred to as a first direction. In this embodiment, the first direction corresponds to the X-axis direction.
[0030] The source electrode 28 and the drain electrode 30 may be composed of one or more metal layers. For example, the source electrode 28 and the drain electrode 30 may be composed of a combination of two or more metal layers selected from a group including a Ti layer, a TiN layer, an Al layer, an AlSiCu layer, and an AlCu layer. At least a portion of the source electrode 28 is filled in the first opening 26A and makes ohmic contact with the 2DEG 20 immediately below the electron supply layer 18 through the first opening 26A. Similarly, at least a portion of the drain electrode 30 is filled in the second opening 26B and makes ohmic contact with the 2DEG 20 immediately below the electron supply layer 18 through the second opening 26B.
[0031] In one example, the source electrode 28 may include a source contact portion 28A filled in the first opening 26A and a source field plate portion 28B formed on the passivation layer 26. The source field plate portion 28B is continuous with the source contact portion 28A and is formed integrally with the source contact portion 28A. The source field plate portion 28B includes an end portion 28C located between the second opening 26B and the gate layer 22 in a plan view. The source field plate portion 28B is spaced apart from the drain electrode 30. The source field plate portion 28B serves to reduce electric field concentration near the end portion of the gate electrode 24 and the end portion of the gate layer 22 when a drain voltage is applied to the drain electrode 30 in a zero-bias state where no gate voltage is applied to the gate electrode 24.
[0032] [Planar Structure of Nitride Semiconductor Device] Next, the planar structure of the nitride semiconductor device 10 will be described with reference to Fig. 1. In Fig. 1, the passivation layer 26 and the source electrode 28 are not shown, and the first opening 26A and the second opening 26B of the passivation layer 26 and the end 28C of the source electrode 28 are depicted by dashed lines.
[0033] The nitride semiconductor device 10 has, for example, active regions that contribute to transistor operation and inactive regions (not shown) that do not contribute to transistor operation. In one example, the active regions and inactive regions are arranged alternately in the Y-axis direction.
[0034] In the active region of the nitride semiconductor device 10, the source electrode 28 (see FIG. 2), the gate electrode 24, and the drain electrode 30 are arranged adjacent to each other in a first direction (X-axis direction) on the electron supply layer 18 (see FIG. 2). A combination of the source electrode 28, the gate electrode 24, and the drain electrode 30 adjacent to each other in the first direction constitutes one HEMT cell 10HC. In the example of FIG. 1, two HEMT cells 10HC are arranged in the X-direction in the active region. In practice, more HEMT cells 10HC may be arranged in each active region.
[0035] [Detailed Structure of Gate Layer (Step Structure)] The gate layer 22 has a step structure. Details of the gate layer 22 having the step structure will be described below with reference to FIG.
[0036] 2, the gate layer 22 includes a ridge portion 42 and an extension portion 43 that is thinner than the ridge portion 42. The extension portion 43 extends in the X-axis direction from each of the side surfaces 42C of the ridge portion 42 in the X-axis direction.
[0037] The ridge portion 42 corresponds to a relatively thick portion of the gate layer 22. The gate electrode 24 is in contact with the ridge portion 42. The ridge portion 42 may have a rectangular or trapezoidal shape in a cross section taken along the XZ plane in FIG. 2. The ridge portion 42 may have a thickness T1 of, for example, 100 nm or more and 200 nm or less. The thickness T1 of the ridge portion 42 refers to the distance from the upper surface 42A to the lower surface 42B of the ridge portion 42. The thickness T1 of the ridge portion 42 may be determined in consideration of various parameters such as the gate breakdown voltage.
[0038] The extension portion 43 includes a source-side extension portion 44 and a drain-side extension portion 46. The source-side extension portion 44 and the drain-side extension portion 46 extend in opposite directions in the X-axis direction. More specifically, the source-side extension portion 44 extends from the ridge portion 42 toward the first opening 26A of the passivation layer 26. The drain-side extension portion 46 extends from the ridge portion 42 toward the second opening 26B of the passivation layer 26. The source-side extension portion 44 and the drain-side extension portion 46 may have the same length or different lengths.
[0039] The thickness T2 of each extension portion 43 is, for example, 30 nm or less, 25 nm or less, 20 nm or less, or 15 nm or less. The thickness T2 of the extension portion 43 is, for example, 5 nm or more. More specifically, the thickness T2A of the source side extension portion 44 is, for example, 30 nm or less, 25 nm or less, or 20 nm or less. The thickness T2A of the source side extension portion 44 is, for example, 5 nm or more. The thickness T2A of the source side extension portion 44 refers to the average value of the distance from the upper surface 44A to the lower surface 44B of the source side extension portion 44. The thickness T2B of the drain side extension portion 46 is, for example, 30 nm or less, 25 nm or less, or 20 nm or less. The thickness T2B of the drain side extension portion 46 is, for example, 5 nm or more. The thickness T2B of the drain side extension portion 46 refers to the average value of the distance from the upper surface 46A to the lower surface 46B of the drain side extension portion 46.
[0040] In one example, the thickness T2A of the source-side extension portion 44 is equal to the thickness T2B of the drain-side extension portion 46. Here, if the difference between the thickness T2A of the source-side extension portion 44 and the thickness T2B of the drain-side extension portion 46 is, for example, within 10% of the thickness of the source-side extension portion 44, it can be said that the thickness T2A of the source-side extension portion 44 and the thickness T2B of the drain-side extension portion 46 are equal to each other.
[0041] The source side extension 44 may have a first direction length L1 of, for example, 100 nm or more in the direction from the ridge 42 toward the first opening 26A. The first direction length L1 of the source side extension 44 is, for example, 200 nm or more and 300 nm or less. The drain side extension 46 may have a first direction length L2 of, for example, 200 nm or more and 600 nm or less in the direction from the ridge 42 toward the second opening 26B. In one example, the first direction length L2 of the drain side extension 46 is longer than the first direction length L1 of the source side extension 44.
[0042] The gate layer 22 has an upper surface and a lower surface. The lower surface of the gate layer 22 is the surface of the gate layer 22 facing the upper surface 18A of the electron supply layer 18. The upper surface of the gate layer 22 is the surface of the gate layer 22 located opposite the lower surface. The upper surface of the gate layer 22 having a step structure refers to the surface including the upper surface 42A of the ridge portion 42 and the upper surfaces of the extension portions 43 (the upper surface 44A of the source-side extension portion 44 and the upper surface 46A of the drain-side extension portion 46). The lower surface of the gate layer 22 having a step structure refers to the surface including the lower surface 42B of the ridge portion 42, the lower surface 44B of the source-side extension portion 44, and the lower surface 46B of the drain-side extension portion 46.
[0043] The cross-sectional shape of the gate layer 22 having the step structure is not limited to the above shape. For example, the thickness T2A of the source-side extension 44 and the thickness T2B of the drain-side extension 46 may be different. Also, either the source-side extension 44 or the drain-side extension 46 may be omitted.
[0044] [Detailed Structure of Silicon Substrate] Fig. 3 is a schematic diagram showing the crystalline structure of the substrate upper surface 12A of the silicon substrate 12. For ease of explanation, Fig. 3 shows a schematic view of an example of an atomic-level surface structure in the case where the silicon substrate 12 has an ideal crystalline structure.
[0045] As shown in FIG. 3 , the substrate upper surface 12A of the silicon substrate 12 is a surface including a first plane 60. Furthermore, the substrate upper surface 12A of the silicon substrate 12 may be a surface having a plurality of first planes 60 aligned in a specific direction D1 via one or more step portions 61 in a plan view. The specific direction D1 is not particularly limited. The specific direction D1 may be, for example, the X-axis direction (first direction) or a direction intersecting the X-axis direction (Y-axis direction). In the example shown in FIG. 3 , the specific direction D1 is the X-axis direction.
[0046] The first plane 60 is a plane formed by the (111) plane of a cubic Si crystal and is flat at the atomic level. The dashed line in the figure represents a virtual (111) plane. Here, the angle between the first plane 60 and a reference plane BP perpendicular to the thickness direction of the silicon substrate 12 on the substrate upper surface 12A is defined as the off-angle θ. In FIG. 3 , the off-angle θ and the dimensions of the step portion 61 and the like are exaggerated for ease of understanding.
[0047] The off-angle θ of the first plane 60 is equal to or greater than 0 degrees and equal to or less than 0.08 degrees. The off-angle θ of the first plane 60 may be equal to or less than 0.06 degrees or equal to or less than 0.04 degrees. An off-angle θ of 0 degrees means that the first plane 60 is parallel to the reference plane BP. In this case, the substrate upper surface 12A is a flat surface at the atomic level that does not include the step portion 61. Furthermore, an off-angle θ of more than 0 degrees means that the first plane 60 is inclined with respect to the reference plane BP.
[0048] When the off angle θ exceeds 0 degrees, the substrate upper surface 12A is preferably formed so that the width dimension W of the first plane 60 is long. The width dimension W is, for example, 200 nm or more, and preferably 224 nm or more. The width dimension W is, for example, 1800 nm or less. The width dimension W tends to become longer as the off angle θ becomes smaller.
[0049] The step portion 61 connecting the first planes 60 can have a height H corresponding to one or more crystal lattice layers. The height H is, for example, 0.314 nm or an integer multiple of 0.314 nm. The substrate upper surface 12A is preferably formed so that the height H of the step portion 61 is small. The height H tends to decrease as the off-angle θ decreases. The height H is, for example, 0.314 nm or greater.
[0050] [Method of Manufacturing Nitride Semiconductor Device] Next, an example of a method of manufacturing the nitride semiconductor device 10 will be described briefly. Figure 4 is a schematic cross-sectional view showing an exemplary manufacturing process of the nitride semiconductor device 10. For ease of understanding, in Figure 4, components similar to those in Figure 1 may be assigned the same reference numerals.
[0051] 4 , the method for manufacturing the nitride semiconductor device 10 includes forming a buffer layer 50, a first nitride semiconductor layer 51, a second nitride semiconductor layer 52, and a third nitride semiconductor layer 53 on a silicon substrate 12. The first nitride semiconductor layer 51 is a layer that forms the electron transit layer 16 of the nitride semiconductor device 10. The second nitride semiconductor layer 52 is a layer that forms the electron supply layer 18 of the nitride semiconductor device 10. The third nitride semiconductor layer 53 is a layer that forms the gate layer 22 of the nitride semiconductor device 10.
[0052] A substrate having a substrate upper surface 12A with a specific shape is prepared as the silicon substrate 12. The specific shape means that the substrate upper surface 12A includes a first plane 60 formed by a (111) plane, and the off-angle, which is the angle of the first plane 60 with respect to the reference plane BP, is between 0 degrees and 0.08 degrees. The silicon substrate 12 having the substrate upper surface 12A with the specific shape can be obtained, for example, as follows. First, bulk-grown silicon is cut along a plane parallel to the (111) plane, and the off-angle θ of the cut plane is measured. Then, a substrate having a measured off-angle θ between 0 degrees and 0.08 degrees is selected and used as the silicon substrate 12. The off-angle θ can be measured, for example, using an X-ray diffraction (XRD) device.
[0053] The buffer layer 50, the first nitride semiconductor layer 51, the second nitride semiconductor layer 52, and the third nitride semiconductor layer 53 can be epitaxially grown on the silicon substrate 12 by using a metal organic chemical vapor deposition (MOCVD) method. These layers are formed from nitride semiconductors with relatively similar lattice constants, and therefore can be epitaxially grown successively.
[0054] In one example, the buffer layer 50 is a multi-layer buffer layer, in which an AlN layer (first buffer layer) is formed on the silicon substrate 12, and then a graded AlGaN layer (second buffer layer) is formed on the AlN layer. The graded AlGaN layer is formed, for example, by stacking three AlGaN layers with Al compositions of 75%, 50%, and 25%, in that order from the side closest to the AlN layer.
[0055] The first nitride semiconductor layer 51 and the second nitride semiconductor layer 52 are formed by being sequentially stacked on the buffer layer 50. During the epitaxial growth of each of the first nitride semiconductor layer 51 and the second nitride semiconductor layer 52, a doping gas may be introduced into the growth chamber as needed. This allows the desired layer to be doped with an impurity. For example, during the epitaxial growth of the second nitride semiconductor layer 52, Si is doped as an n-type impurity. This allows the second nitride semiconductor layer 52 containing an n-type impurity to be formed.
[0056] The third nitride semiconductor layer 53 is formed by being stacked on the second nitride semiconductor layer 52. During the epitaxial growth of the third nitride semiconductor layer 53, a doping gas is introduced into the growth chamber. For example, during the epitaxial growth of the third nitride semiconductor layer 53, Mg is doped as an acceptor-type impurity. This allows the third nitride semiconductor layer 53 containing the acceptor-type impurity to be formed.
[0057] The method for manufacturing the nitride semiconductor device 10 includes forming the gate electrode 24. The gate electrode 24 is formed by selectively removing a metal layer formed on the third nitride semiconductor layer 53 by lithography and etching.
[0058] The method for manufacturing the nitride semiconductor device 10 includes forming the gate layer 22 including the extensions 43 (the source-side extension 44 and the drain-side extension 46). The extensions 43 of the gate layer 22 are formed by selectively removing the third nitride semiconductor layer 53 by lithography and etching. The portions of the third nitride semiconductor layer 53 that are masked during the etching are left as the ridge portion 42 of the gate layer 22.
[0059] The manufacturing method of nitride semiconductor device 10 may include measuring the thickness of the formed extension portion 43 and sorting the extension portion 43 based on the measured value. For example, as a result of the measurement, an extension portion 43 that does not include a portion having a thickness equal to or less than a specific thickness is sorted as a non-defective product, and an extension portion 43 that includes a portion having a thickness equal to or less than the specific thickness is sorted as a defective product. The specific thickness may be, for example, 1 nm, 3 nm, or 5 nm. The specific thickness may be a thickness that is equal to or less than a specific percentage (for example, 20% or less) of the design value (target thickness) of extension portion 43. The thickness of extension portion 43 can be measured using, for example, an atomic force microscope (AFM).
[0060] [Function] Next, the function of the nitride semiconductor device 10 will be described. The nitride semiconductor device 10 includes a gate layer 22 provided on the electron supply layer 18 and made of a nitride semiconductor containing acceptor-type impurities. The gate layer 22 includes a ridge portion 42 and an extension portion 43 that is thinner than the ridge portion 42. An etching process is used to form the extension portion 43. When the extension portion 43 is formed by etching, an uneven shape is formed on the upper surface of the extension portion 43 due to the etching. The extension portion 43 has thickness variations due to the uneven shape of the upper surface.
[0061] 5, thickness unevenness of the extension portion 43 will be described below using the drain-side extension portion 46 as an example. Fig. 5 is a schematic cross-sectional view showing an example of the uneven shape of the upper surface 46A of the drain-side extension portion 46. In Fig. 5, the uneven shape of the upper surface 46A of the drain-side extension portion 46 is exaggerated for ease of understanding.
[0062] 5 , the upper surface 46A of the drain-side extension 46 has an uneven shape including one or more recesses 70 recessed toward the lower surface of the gate layer 22 and one or more protrusions 71 protruding to the side opposite the lower surface of the gate layer 22. The recesses 70 do not reach the lower surface 46B of the drain-side extension 46. That is, the drain-side extension 46 includes a portion located between the bottom of the recess 70 and the lower surface 46B. In one example, the deepest recess 70A of the recesses 70 is formed along the side surface 42C of the ridge portion 42. In this case, the portion along the side surface 42C of the ridge portion 42 where the recess 70A is located is the thinnest portion of the drain-side extension 46.
[0063] The thickness variation R of the extension portion 43 can be defined as the difference between the thickness of the thickest portion of the extension portion 43 and the thickness of the thinnest portion of the extension portion 43. In the case of the drain-side extension portion 46, the thickness variation R is the maximum thickness T2B, which is the thickness of the thickest portion of the drain-side extension portion 46. max and a minimum thickness T2B, which is the thickness of the thinnest portion of the drain-side extension portion 46. min Difference with (T2B max -T2B min ) Although detailed description will be omitted, similar to the drain-side extension portion 46, the source-side extension portion 44 also has an upper surface 44A having an uneven shape and a thickness unevenness R. Note that, when the extension portion 43 includes both the source-side extension portion 44 and the drain-side extension portion 46, the thickness unevenness R of the extension portion 43 is defined for each of the source-side extension portion 44 and the drain-side extension portion 46.
[0064] The thickness unevenness R of the extension portion 43 occurs during the manufacturing process of the nitride semiconductor device 10 as follows. As shown in FIG. 4 , the extension portion 43 of the gate layer 22 is formed by etching a third nitride semiconductor layer 53 formed by epitaxial growth on the second nitride semiconductor layer 52 constituting the electron supply layer 18. The third nitride semiconductor layer 53 contains a higher concentration of impurities such as Mg than the second nitride semiconductor layer 52. Therefore, when the third nitride semiconductor layer 53 is formed by epitaxial growth on the upper surface 52A of the second nitride semiconductor layer 52, the roughness of the upper surface 53A of the formed third nitride semiconductor layer 53 becomes greater than that of the upper surface 52A of the second nitride semiconductor layer 52. Then, when the third nitride semiconductor layer 53 is etched to form the extension portion 43, the roughness of the upper surface 53A of the third nitride semiconductor layer 53 is inherited by the upper surfaces (44A, 46A) of the extension portion 43. As a result, the roughness of the upper surface of the extension portion 43 is greater than the roughness of the lower surfaces (44B, 46B) of the extension portion 43. As a result, thickness unevenness R occurs in the extension portion 43. It is preferable that such thickness unevenness R of the extension portion 43 is small.
[0065] 6 is a cross-sectional view, as a reference example, schematically illustrating a drain-side extension portion 46 having an excessively large thickness unevenness R. For ease of understanding, in this reference example, the same names and symbols will be used for components corresponding to those in the nitride semiconductor device 10 of the embodiment.
[0066] As shown in FIG. 6 , if the thickness variation R of the drain-side extension portion 46 is excessively large, for example, if the thickness variation R is greater than the thickness T2B of the drain-side extension portion 46, a recess 70 reaching the lower surface 46B of the drain-side extension portion 46 may be formed. This recess 70 can also be referred to as a recess 70 reaching the upper surface 18A of the electron supply layer 18. The recess 70 reaching the lower surface 46B becomes a defect 46C where the drain-side extension portion 46 is locally absent within the formation range of the drain-side extension portion 46 in a planar view. In this case, a gate leakage current flows through the defect 46C in the drain-side extension portion 46, resulting in a problem of not being able to obtain the desired gate breakdown voltage. Therefore, by reducing the thickness variation R of the extension portion 43, the occurrence of the defect 46C in the extension portion 43 can be suppressed, and a decrease in the gate breakdown voltage due to the defect 46C can be suppressed.
[0067] In the above-described method for manufacturing the nitride semiconductor device 10, those having the recesses 70 reaching the electron supply layer 18 are removed by measuring the thickness of the formed extension portion 43 and selecting them based on the measurement value. Therefore, reducing the thickness unevenness R of the extension portion 43 also contributes to improving the yield when manufacturing the nitride semiconductor device 10.
[0068] In the nitride semiconductor device 10, the thickness unevenness R of the extension portion 43 is reduced by using a silicon substrate 12 having a substrate upper surface 12A with a specific shape. More specifically, the substrate upper surface 12A of the silicon substrate 12 is a surface including a first plane 60 configured by a (111) plane. In addition, on the substrate upper surface 12A, the off angle θ formed between a reference plane BP orthogonal to the thickness direction of the silicon substrate 12 and the first plane 60 is equal to or greater than 0 degrees and equal to or less than 0.08 degrees.
[0069] When a silicon substrate 12 having the substrate upper surface 12A of the above-described specific shape is used, the thickness variation of the extension portion 43 is, for example, less than 100%, 90% or less, or 80% or less of the thickness T2 of the extension portion 43. In the case of the thickness variation R of the drain-side extension portion 46, the length is less than 100%, 90% or less, or 80% or less of the thickness T2B of the drain-side extension portion 46. In the case of the thickness variation R of the source-side extension portion 44, the length is less than 100%, 90% or less, or 80% or less of the thickness T2A of the source-side extension portion 44.
[0070] FIG. 7 is a graph showing the relationship between the off-angle θ of the substrate upper surface 12A of the silicon substrate 12 and the thickness unevenness R of the extension portion 43. The graph in FIG. 7 is based on the results of actually performing the above-described steps of manufacturing the nitride semiconductor device 10 in sequence using multiple types of silicon substrates 12 with different off-angles θ, and measuring the thickness unevenness R of the gate layer 22 at the timing when the gate layer 22 was formed. The off-angle θ was measured using an XRD device. The thickness unevenness R of the extension portion 43 was calculated by measuring the thickness of the extension portion 43 in a predetermined specific range using an AFM device, and then calculating the difference between the maximum and minimum thickness values of the extension portion 43 obtained from the measurement results. In addition, in the manufacturing of the nitride semiconductor device 10, the design value of the thickness of the extension portion 43 was set to 15 nm.
[0071] As shown in FIG. 7 , the thickness variation R of the extension portion 43 tends to decrease as the off angle θ decreases. This tendency is particularly pronounced when the off angle θ is 0.08 or less. That is, compared to when the off angle θ exceeds 0.08, the degree of decrease in the thickness variation R of the extension portion 43 with decreasing off angle θ is significantly greater when the off angle θ is 0.08 or less. From this result, it can be seen that by using a silicon substrate 12 having a substrate upper surface 12A with an off angle θ of 0.08 or less, the thickness variation R of the extension portion 43 can be significantly reduced, i.e., the extension portion 43 can be formed with a uniform thickness. Furthermore, when the off angle θ is 0.08 or less, the thickness variation R of the extension portion 43 is less than the design value (15 nm) of the thickness of the extension portion 43. Therefore, by setting the off angle θ to 0.08 or less, the thickness variation R of the extension portion 43 can be suppressed to less than the design value of the thickness of the extension portion 43.
[0072] [Effects] The nitride semiconductor device 10 according to the embodiment provides the following effects. (1) The nitride semiconductor device 10 includes a silicon substrate 12 having a substrate upper surface 12A, an electron supply layer 18 formed on the substrate upper surface 12A of the silicon substrate 12 and made of a nitride semiconductor having a larger band gap than an electron transit layer 16 made of a nitride semiconductor, a gate layer 22 formed on the electron supply layer 18 and made of a nitride semiconductor containing acceptor-type impurities, a gate electrode 24 formed on the gate layer 22, and a source electrode 28 and a drain electrode 30 formed on the electron supply layer 18. The gate layer 22, the source electrode 28, and the drain electrode 30 are arranged on the upper surface 18A of the electron supply layer 18 so as to be aligned in a first direction (X-axis direction). The gate layer 22 includes a ridge portion 42 in contact with the electron supply layer 18 and an extension portion 43 extending from the ridge portion 42 in the first direction and thinner than the ridge portion 42. The substrate upper surface 12A of the silicon substrate 12 is a surface including a first plane 60 configured of a (111) plane. An off angle θ between a reference plane BP perpendicular to the thickness direction of the silicon substrate 12 and the first plane 60 is equal to or greater than 0 degrees and equal to or less than 0.08 degrees.
[0073] In this case, it is possible to reduce the thickness unevenness R of the extension portion 43, i.e., to improve the thickness uniformity of the extension portion 43. This makes it possible to suppress the occurrence of the defect portion 46C in the extension portion 43 and to suppress the decrease in gate breakdown voltage caused by the occurrence of the defect portion 46C. Furthermore, it is possible to improve the yield when manufacturing the nitride semiconductor device 10.
[0074] (2) The upper surface 12A of the silicon substrate 12 has a plurality of first planes 60 arranged in the specific direction D1 via step portions 61. The width W of each of the first planes 60 in the specific direction D1 is 224 nm or more.
[0075] In this case, the substrate upper surface 12A has a small number of step portions 61, i.e., the substrate upper surface 12A has a low frequency of occurrence of step portions 61. On the substrate upper surface 12A of the silicon substrate 12, the edge E (see FIG. 3 ) formed by the first plane 60 and the step portion 61 is a site where nitride semiconductor crystal nuclei are likely to form when a nitride semiconductor layer is formed on the substrate upper surface 12A by epitaxial growth. Therefore, when a silicon substrate 12 having a substrate upper surface 12A with a small number of step portions 61 is used, fewer crystal nuclei are generated during layer formation, thereby improving the flatness of the electron transit layer 16 and the electron supply layer 18 formed on the substrate upper surface 12A. In other words, the roughness of the upper surface 18A of the electron supply layer 18 can be reduced.
[0076] The small roughness of upper surface 18A of electron supply layer 18 can prevent the roughness of upper surface 53A of third nitride semiconductor layer 53 formed on upper surface 18A from increasing. As a result, the roughness of the upper surface of extension portion 43 formed by inheriting the roughness of upper surface 53A of third nitride semiconductor layer 53 also becomes small, and the thickness unevenness R of extension portion 43 can be further reduced.
[0077] (3) The thickness T2 of the extension portion 43 is 5 nm or more and 30 nm or less. The thinner the thickness T2 of the extension portion 43, the more likely the defect portion 46C caused by the thickness unevenness R of the extension portion 43 is to occur. Therefore, the configuration that reduces the thickness unevenness R of the extension portion 43 of the gate layer 22 by using the silicon substrate 12 having the substrate upper surface 12A of the specific shape described in (1) above is particularly effective in terms of suppressing the defect portion 46C when the thickness T2 of the extension portion 43 is thin.
[0078] (4) The concentration of the acceptor-type impurity in the gate layer 22 is 1×10 18 cm -3 That's all. As described above, the thickness unevenness R of the extension portion 43 is caused by the fact that when the third nitride semiconductor layer 53, which is a layer constituting the gate layer 22 and contains a high concentration of impurities, is formed, the roughness of the upper surface 53A of the third nitride semiconductor layer 53 increases, and the large roughness of the upper surface 53A is inherited by the upper surface of the extension portion 43. The higher the concentration of the acceptor-type impurities contained in the third nitride semiconductor layer 53, the greater the roughness of the upper surface 53A of the third nitride semiconductor layer 53, and as a result, the thickness unevenness R of the extension portion 43 also increases. Therefore, the configuration in which the thickness unevenness R of the extension portion 43 of the gate layer 22 is reduced by using the silicon substrate 12 having the substrate upper surface 12A of the specific shape described in (1) above is used is particularly effective when the concentration of the acceptor-type impurities in the gate layer 22 is high.
[0079] (5) The extension portion 43 includes a recess 70 that is formed from the upper surface of the extension portion 43 along the side surface 42C of the ridge portion 42 and does not reach the lower surface of the extension portion 43. The recess 70 that is formed from the upper surface of the extension portion 43 along the side surface 42C of the ridge portion 42 tends to be the deepest recess among the recesses 70 that the extension portion 43 has. Therefore, by forming the extension portion 43 so that the recess 70 does not reach the lower surface of the extension portion 43, the occurrence of a missing portion 46C in the extension portion 43 can be suppressed.
[0080] <Modifications> The above embodiment can be modified, for example, as follows. The above embodiment and each of the following modifications can be combined with each other as long as no technical contradiction occurs. In the following modifications, parts that are common to the above embodiment will be assigned the same reference numerals as in the above embodiment, and their description will be omitted.
[0081] Regarding the manufacturing method of the nitride semiconductor device 10, when measuring the thickness of the formed extension portion 43 and selecting the extension portion 43 based on the measured value, the target range for measuring the thickness of the extension portion 43 is not particularly limited. For example, the thickness of the extension portion 43 may be measured for the entire extension portion 43, or for a portion of the extension portion 43. From the viewpoint of improving manufacturing efficiency, it is preferable to limit the target range for measuring the thickness of the extension portion 43 to a specific location. As an example, the thickness of the extension portion 43 may be measured for a portion where a recess 70 formed from the upper surface of the extension portion 43 along the side surface 42C of the ridge portion 42 is located. The recess 70 formed from the upper surface of the extension portion 43 along the side surface 42C of the ridge portion 42 tends to be the deepest recess among the recesses 70 of the extension portion 43. Therefore, if the thickness of the portion where the recess 70 is located is not equal to or less than the specific thickness, it can be determined that the extension portion 43 does not include a portion equal to or less than the specific thickness.
[0082] In the method for manufacturing the nitride semiconductor device 10, it is possible to omit measuring the thickness of the formed extension portion 43 and selecting the nitride semiconductor device 10 based on the measured value. In the above embodiment, the nitride semiconductor device 10 is configured as a nitride semiconductor HEMT, but is not limited to a nitride semiconductor HEMT and may be configured as a nitride semiconductor diode.
[0083] The term "on" as used in this disclosure includes both the meanings of "on" and "above," unless the context clearly indicates otherwise. Thus, the phrase "a first layer is formed on a second layer" is intended to mean that in some embodiments, the first layer may be disposed directly on the second layer in contact with the second layer, while in other embodiments, the first layer may be disposed above the second layer without contacting the second layer. In other words, the term "on" does not exclude a structure in which another layer is formed between the first and second layers.
[0084] The Z direction used in this disclosure does not necessarily have to be the vertical direction, nor does it have to completely coincide with the vertical direction. Therefore, various structures according to this disclosure are not limited to the "up" and "down" in the Z direction described herein being "up" and "down" in the vertical direction. For example, the X axis direction may be the vertical direction, or the Y axis direction may be the vertical direction.
[0085] In this disclosure, terms such as "first," "second," and "third" are used merely to distinguish between objects and do not rank the objects. In this specification, "at least one of A and B" should be understood to mean "A only, or B only, or both A and B."
[0086] <Supplementary Notes> The technical ideas that can be understood from the present disclosure are described below. Note that, for the purpose of aiding understanding and not intending to be limiting, the components described in the supplementary notes are given the reference symbols of the corresponding components in the embodiments. The reference symbols are shown as examples to aid understanding, and the components described in each supplementary note should not be limited to the components indicated by the reference symbols.
[0087] [Supplementary Note 1] A semiconductor device comprising: a silicon substrate (12) having a substrate upper surface (12A); an electron transit layer (16) formed on the substrate upper surface (12A) of the silicon substrate (12) and made of a nitride semiconductor; an electron supply layer (18) formed on the electron transit layer (16) and made of a nitride semiconductor having a larger band gap than the electron transit layer (16); a gate layer (22) formed on the electron supply layer (18) and made of a nitride semiconductor containing acceptor-type impurities; a gate electrode (24) formed on the gate layer (22); and a source electrode (28) and a drain electrode (30) formed on the electron supply layer (18), wherein the gate layer (22), the source electrode (28), and the drain electrode (30) are arranged to be aligned in a first direction (X-axis direction) on the upper surface (18A) of the electron supply layer (18), and the gate layer (22) a nitride semiconductor device (10) including: a ridge portion (42) in contact with the electron supply layer (18); and an extension portion (43) extending from the ridge portion (42) in the first direction and thinner than the ridge portion (42), wherein the substrate upper surface (12A) of the silicon substrate (12) is a surface including a first plane (60) configured by a (111) plane, and an off angle (θ) between a reference plane (BP) perpendicular to a thickness direction of the silicon substrate (12) and the first plane (60) is equal to or greater than 0 degrees and equal to or less than 0.08 degrees.
[0088] [Supplementary Note 2] The nitride semiconductor device (10) according to Supplementary Note 1, wherein the substrate upper surface (12A) of the silicon substrate (12) has a plurality of the first planes (60) arranged in a specific direction (D1) via step portions (61), and a width dimension (W) of the first planes (60) along the specific direction (D1) is 224 nm or more.
[0089] [Supplementary Note 3] The nitride semiconductor device (10) according to Supplementary Note 1 or Supplementary Note 2, wherein the thickness (T2) of the extension portion (43) is 5 nm or more and 30 nm or less.
[0090] [Supplementary Note 4] The concentration of the acceptor-type impurity in the gate layer (22) is 1×10 18 cm -3The nitride semiconductor device (10) according to any one of appendices 1 to 3 is as described above.
[0091] [Appendix 5] The nitride semiconductor device (10) according to any one of Appendices 1 to 4, wherein the extension portion (43) is formed from an upper surface of the extension portion (43) along a side surface (42C) of the ridge portion (42), and includes a recess (70) that does not reach a lower surface of the extension portion (43).
[0092] [Appendix 6] The nitride semiconductor device (10) according to any one of Appendices 1 to 4, wherein the extension portion (43) includes a recess (70) formed from an upper surface of the extension portion (43) along a side surface (42C) of the ridge portion (42).
[0093] [Supplementary Note 7] The nitride semiconductor device (10) according to any one of Supplementary Notes 1 to 6, wherein the electron transit layer (16) is a GaN layer, the electron supply layer (18) is an AlGaN layer, and the gate layer (22) is a GaN layer containing the acceptor-type impurity.
[0094] [Supplementary Note 8] The method includes forming an electron transit layer (16) made of a nitride semiconductor on a substrate upper surface (12A) of a silicon substrate (12) by epitaxial growth, forming an electron supply layer (18) made of a nitride semiconductor having a band gap larger than that of the electron transit layer (16) on the electron transit layer (16) by epitaxial growth, forming a gate layer (22) made of a nitride semiconductor containing acceptor-type impurities on the electron supply layer (18), forming a gate electrode (24) on the gate layer (22), and forming a source electrode (28) and a drain electrode (30) on the electron supply layer (18), wherein the gate layer (22), the source electrode (28), and the drain electrode (30) are arranged to be aligned in a first direction (X-axis direction) on the upper surface (18A) of the electron supply layer (18), and the gate layer (22) has: a ridge portion (42) in contact with the electron supply layer (18); and an extension portion (43) that is thinner than the ridge portion (42) and extends from the ridge portion (42) in the first direction, wherein forming the gate layer (22) includes forming a nitride semiconductor layer (53) that constitutes the gate layer (22) by epitaxial growth, and selectively etching the nitride semiconductor layer (53) to form the ridge portion (42) and the extension portion (43), wherein the silicon substrate (12) has an upper surface (12A) that includes a first plane (60) that is a (111) plane, and an off angle (θ) between a reference plane (BP) that is orthogonal to a thickness direction of the silicon substrate (12) and the first plane (60) is between 0 degrees and 0.08 degrees.
[0095] [Supplementary Note 9] The method for manufacturing the nitride semiconductor device (10) according to Supplementary Note 8, further comprising measuring the thickness of the formed extension portion 43 and selecting based on the measured value.
[0096] [Appendix 10] A method for manufacturing a nitride semiconductor device (10) according to Appendix 9, wherein the extension portion (43) includes a recess (70) formed from an upper surface of the extension portion (43) along a side surface (42C) of the ridge portion (42), and the method includes measuring a thickness of the extension portion (43) at a portion where the recess (70) is located, and selecting based on the measurement value.
[0097] θ...off angle BP...reference plane D1...specific direction H...height dimension L1, L2...length in first direction R...thickness variation T1, T2, T2A, T2B...thickness T2Bmax...maximum thickness T2Bmin...minimum thickness W...width dimension 10...nitride semiconductor device 10HC...HEMT cell 12...silicon substrate 12A...substrate upper surface 14...buffer layer 16...electron transit layer 18...electron supply layer 18A...upper surface 20...two-dimensional electron gas 22...gate layer 24...gate electrode 26...passivation layer 26A...first opening 26B...second opening 28...source electrode 28A...source contact portion 28B...source field plate portion 28C...edge 30...drain electrode 42...ridge portion 42A...upper surface 42B...lower surface 42C...side surface 43: Extension portion 44: Source-side extension portion 44A: Upper surface 44B: Lower surface 46: Drain-side extension portion 46A: Upper surface 46B: Lower surface 46C: Defect portion 50: Buffer layer 51: First nitride semiconductor layer 52: Second nitride semiconductor layer 52A: Upper surface 53: Third nitride semiconductor layer 53A: Upper surface 60: First plane 61: Step portion 70, 70A: Recessed portion 71: Protruding portion
Claims
a gate electrode formed on the gate layer; and a source electrode and a drain electrode formed on the electron supply layer, wherein the gate layer, the source electrode, and the drain electrode are arranged to be aligned in a first direction on an upper surface of the electron supply layer, the gate layer including: a ridge portion in contact with the electron supply layer; and an extension portion extending from the ridge portion in the first direction and being thinner than the ridge portion, the upper surface of the silicon substrate being a plane including a first plane formed by a (111) plane, and an off angle between a reference plane perpendicular to a thickness direction of the silicon substrate and the first plane is greater than or equal to 0 degrees and is less than 0.08 degrees.
2. The nitride semiconductor device according to claim 1, wherein the upper surface of the silicon substrate has a plurality of the first planes arranged in a specific direction via step portions, and a width dimension of the first planes in the specific direction is 224 nm or more.
3. The nitride semiconductor device according to claim 1 or 2, wherein the extension portion has a thickness of 5 nm or more and 30 nm or less.
4. The concentration of the acceptor-type impurity in the gate layer is 1×10 18 cm -3 The nitride semiconductor device according to any one of claims 1 to 3, wherein:
5. The nitride semiconductor device according to any one of claims 1 to 4, wherein the extension portion is formed from the upper surface of the extension portion along a side surface of the ridge portion and includes a recess that does not reach the lower surface of the extension portion.
6. The nitride semiconductor device according to any one of claims 1 to 5, wherein the electron transit layer is a GaN layer, the electron supply layer is an AlGaN layer, and the gate layer is a GaN layer containing the acceptor-type impurity.
7. A method for fabricating a silicon substrate comprising: forming an electron transport layer made of a nitride semiconductor by epitaxial growth on an upper surface of the substrate of a silicon substrate; forming an electron supply layer made of a nitride semiconductor having a band gap larger than that of the electron transport layer by epitaxial growth on the electron transport layer; forming a gate layer made of a nitride semiconductor containing acceptor-type impurities on the electron supply layer; forming a gate electrode on the gate layer; and forming a source electrode and a drain electrode on the electron supply layer, wherein the gate layer, the source electrode, and the drain electrode are arranged to be aligned in a first direction on the upper surface of the electron supply layer, and the gate layer includes a ridge portion in contact with the electron supply layer, and an extension portion extending from the ridge portion in the first direction and being thinner than the ridge portion, and forming the gate layer includes forming a nitride semiconductor layer constituting the gate layer by epitaxial growth, and selectively etching the nitride semiconductor layer to form the ridge portion and the extension portion, and the silicon substrate comprises a top surface of the substrate including a first plane constituted by a (111) plane, and an off angle between a reference plane perpendicular to a thickness direction of the silicon substrate and the first plane is equal to or greater than 0 degrees and equal to or less than 0.08 degrees.
Citation Information
Patent Citations
Electronic element structure body and manufacture thereof
JP1999111963A
Semiconductor device
JP2012015304A
Epitaxial wafer, manufacturing method thereof and ultraviolet light emitting device
JP2014053412A
High electron mobility transistor and manufacturing method for the same
JP2021174987A
Nitride semiconductor laminate, method for producing same and nitride semiconductor device