Composite comprising gallium nitride and diamond and production method for same
By using an intermediate layer with carbon, gallium, and oxygen to bond gallium nitride and diamond substrates through surface treatments, the method addresses crystallinity deterioration and vacuum requirements, achieving enhanced thermal and electrical properties for semiconductor devices.
Patent Information
- Application Number
- PCT/JP2024/010253
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-30
- Filing Date
- 2024-03-15
- Publication Date
- 2024-10-03
AI Technical Summary
Existing methods for bonding gallium nitride (GaN) and diamond substrates, such as those using argon beam irradiation, deteriorate the crystallinity of both materials, leading to poor heat dissipation and electrical insulation properties, and require a vacuum environment, which is impractical for semiconductor device manufacturing.
A composite material is created by bonding a gallium nitride layer with a diamond layer via an intermediate layer containing carbon, gallium, and oxygen, using surface treatments like oxidation, nitriding, and reduction processes to functionalize the surfaces and apply reaction energy for bonding, allowing for atmospheric bonding without crystallinity deterioration.
The method effectively suppresses crystallinity deterioration, enabling strong bonding between GaN and diamond layers with improved thermal conductivity and electrical insulation, and eliminates the need for a vacuum environment, facilitating the manufacturing of high-performance semiconductor devices.
Smart Images

Figure JP2024010253_03102024_PF_FP_ABST
Abstract
Description
Composite Comprising Gallium Nitride and Diamond and Method for Producing the Same
[0001] The present application relates to a composite in which gallium nitride and diamond are bonded via an intermediate layer containing carbon, gallium, and oxygen, and a method for producing the composite.
[0002] Gallium nitride (GaN) has been attracting attention as a substrate material for next-generation power semiconductors. To improve the heat dissipation performance of GaN, a semiconductor device in which a GaN-based semiconductor is directly bonded to a diamond substrate is known (Patent Document 1). Patent Document 1 describes a method for bonding GaN and diamond by irradiating each surface with an argon beam to remove natural oxide films and activate the surface. The method then heats the diamond substrate under a pressure of 1000 K. -6 GaN and diamond are directly bonded in a vacuum chamber at or below Pa.
[0003] In the bonding method of Patent Document 1, argon beam irradiation of the GaN surface deteriorates the crystallinity of the GaN. Deterioration of GaN crystallinity reduces the device characteristics of GaN-based semiconductors. Furthermore, argon beam irradiation of the diamond surface also deteriorates the crystallinity of the diamond. Diamond has a high electrical breakdown field and is suitable for ensuring the insulation of GaN-based semiconductors. However, diamond with deteriorated crystallinity has poor electrical insulation. Therefore, bonding diamond with deteriorated crystallinity to a GaN-based semiconductor adversely affects the operation of the GaN-based semiconductor. Furthermore, the bonding method of Patent Document 1 is performed in a high vacuum, requiring a vacuum bonding device.
[0004] Japanese Patent Application Laid-Open No. 2021-13007
[0005] The present application has been made in view of the above circumstances, and aims to provide a method for manufacturing a composite that can bond GaN and diamond even in the atmosphere while suppressing deterioration of the crystallinity of the two, and a composite in which diamond with suppressed deterioration of crystallinity is bonded, via an intermediate layer, to GaN with suppressed deterioration of crystallinity.
[0006] The composite of the present application has a gallium nitride layer, an intermediate layer formed on the surface of the gallium nitride layer and containing carbon, gallium, and oxygen, and a diamond layer bonded to the surface of the gallium nitride layer via the intermediate layer.
[0007] A method for producing a composite according to one embodiment of the present application comprises a first substrate treatment step of functionalizing the surface of the gallium oxide layer by subjecting the surface of the gallium oxide layer of a first substrate having a gallium nitride layer and an exposed gallium oxide layer formed on the gallium nitride layer to one or more of oxidation, nitridation and reduction treatment; a second substrate treatment step of functionalizing the surface of the diamond layer of a second substrate having a diamond layer whose surface is a (111) plane by subjecting the surface of the diamond layer to oxidation treatment; and a bonding step of bonding the first substrate and the second substrate by applying reaction energy to the contact portion while the surface of the gallium oxide layer that has undergone the first substrate treatment step and the surface of the diamond layer that has undergone the second substrate treatment step are in contact with each other.
[0008] Another aspect of the present application is a method for producing a composite, which comprises a first substrate treatment step of nitriding the surface of the gallium oxide layer of a first substrate comprising a gallium nitride layer and an exposed gallium oxide layer formed on the gallium nitride layer, thereby functionalizing the surface of the gallium oxide layer; a second substrate treatment step of oxidizing the surface of the diamond layer of a second substrate comprising a diamond layer whose surface is a (100) plane, thereby functionalizing the surface of the diamond layer; and a bonding step of bringing the surface of the gallium oxide layer that has undergone the first substrate treatment step into contact with the surface of the diamond layer that has undergone the second substrate treatment step, and applying reaction energy to this contact portion to bond the first substrate and the second substrate.
[0009] In the manufacturing method of the composite of the present application, the gallium oxide layer on the gallium nitride layer and the diamond layer are each subjected to a predetermined treatment that suppresses deterioration of crystallinity, thereby functionalizing and bonding them.Therefore, according to the manufacturing method of the composite of the present application, a composite is obtained in which the gallium nitride layer and the diamond layer are bonded together, with the deterioration of crystallinity being suppressed.In addition, in the composite of the present application, the gallium nitride layer and the diamond layer are bonded together via a predetermined intermediate layer.Therefore, according to the composite of the present application, a composite is obtained in which the gallium nitride layer and the diamond layer are bonded together, with the deterioration of crystallinity being suppressed.
[0010] 1. Planar image of composite 1 of Example 1 observed from the diamond substrate side. 2. Planar image of composite 2 of Example 1 observed from the GaN layer side. 3. Planar image of composite of Example 2 observed from the diamond substrate side. 4. Cross-sectional microscope image of the composite of Example 2. 5. Transmission electron microscope image of the bonding interface of the composite of Example 2. 6. Energy dispersive X-ray spectroscopy spectrum of the intermediate layer of the composite of Example 2. 7. Transmission electron microscope image and element map near the bonding interface of the composite of Example 2. 8. Electron energy loss spectroscopy spectrum of the intermediate layer of the composite of Example 2 and the diamond substrate. 9. Planar image of the attachment of Comparative Example 2 observed from the diamond substrate side. 10. Planar image of the attachment of Comparative Example 3 observed from the diamond substrate side. 11. Planar image of the composite of Example 3 observed from the diamond substrate side. 12. Planar image of the composite of Example 4 observed from the diamond wafer side. 13. Rocking curve of the GaN substrate of the reference example. 14. X-ray photoelectron spectroscopy spectrum of the surface of the GaN layer before and after reduction treatment of Example 2.
[0011] The composite of the present embodiment includes a gallium nitride layer, an intermediate layer, and a diamond layer. The intermediate layer is formed on the surface of the gallium nitride layer. The diamond layer is bonded to the surface of the gallium nitride layer via the intermediate layer. More specifically, a second substrate including a diamond layer is bonded to a first substrate including a gallium nitride layer via the intermediate layer. The intermediate layer contains carbon, gallium, and oxygen. The intermediate layer may also contain nitrogen. Examples of the first substrate include various substrates such as a single-crystal GaN substrate, a GaN / sapphire substrate having a GaN layer on a sapphire substrate surface, a GaN / Si substrate having a GaN layer on a Si substrate surface, and a GaN / SiC substrate having a GaN layer on a SiC substrate surface.
[0012] A natural oxide film, which is a gallium oxide film, is formed on the surface of these GaN layers, and in this embodiment, the intermediate layer is derived from this gallium oxide film. Note that the intermediate layer may be derived from a gallium oxide film other than the natural oxide film on the GaN layer. The fact that the intermediate layer contains gallium oxide can be determined by energy dispersive X-ray analysis. In order to suppress a decrease in thermal conductivity between the gallium nitride layer and the diamond layer, the thickness of the intermediate layer is preferably 4 nm or less. Since the thickness of the natural oxide film formed on the surface of the GaN layer is about 2 nm, the thickness of the intermediate layer is often 2 nm or more.
[0013] In the semiconductor device disclosed in Patent Document 1, the nitrogen content is higher than the oxygen content at the bonding interface between the GaN-based semiconductor and the diamond substrate, which are bonded after removing the native oxide film by sputtering in an ultra-high vacuum. However, sputtering the native oxide film deteriorates the crystallinity of the GaN. In this embodiment, the intermediate layer is derived from a gallium oxide film on the surface of the GaN layer. Therefore, the oxygen content of the intermediate layer is higher than the nitrogen content. In this way, by bonding the first substrate and the second substrate via an intermediate layer containing carbon, gallium, and oxygen and having a nitrogen content lower than the oxygen content, the shear strength between the first substrate and the second substrate is 0.1 MPa or more.
[0014] The second substrate may be a single crystal diamond substrate, a diamond / Si substrate having a diamond layer on the surface of a Si substrate, or a diamond / sapphire substrate having a diamond layer on the surface of a sapphire substrate.The diamond layer preferably has a (100) or (111) surface.The diamond layer may also be a mosaic crystal having a (100) or (111) surface.
[0015] The method for manufacturing a composite according to a first embodiment of the present application includes a first substrate treatment step, a second substrate treatment step, and a bonding step. The first substrate includes a gallium nitride layer and an exposed gallium oxide layer formed on the gallium nitride layer. In the first substrate treatment step, a predetermined treatment is performed on the surface of the gallium oxide layer of the first substrate to functionalize the surface of the gallium oxide layer. The predetermined treatment is one or more of an oxidation treatment, a nitridation treatment, and a reduction treatment.
[0016] The oxidation treatment is a treatment in which oxygen atoms are introduced into the surface of the gallium oxide layer to grow the gallium oxide layer. The nitridation treatment is a treatment in which nitrogen atoms are introduced into the surface of the gallium oxide layer. The reduction treatment is a treatment in which reactive functional groups are introduced into the surface while thinning the gallium oxide layer. Examples of the oxidation treatment include treatment with a liquid containing ammonia and hydrogen peroxide, and treatment with reactive oxygen plasma. Examples of the nitridation treatment include treatment with reactive nitrogen plasma. Examples of the reduction treatment include treatment with hydrochloric acid. This treatment with hydrochloric acid converts the surface of the gallium oxide layer into -OH groups, -NH 2 The amine group is functionalized with one or more of a -Cl group and a -C1 group.
[0017] These examples of various treatments are also applicable to the second substrate treatment step in the manufacturing method of the composite of the first embodiment, and the first substrate treatment step and the second substrate treatment step in the manufacturing method of the composite of the second embodiment. The chemical structure of the surface of the gallium oxide layer functionalized by the oxidation treatment or nitriding treatment in the first substrate treatment step is not necessarily clear. However, the surface of the functionalized gallium oxide layer has properties that make it easy to bond with the surface of the diamond layer functionalized in the second substrate treatment step. Moreover, these predetermined treatments, which do not involve the complete removal of the gallium oxide layer, suppress deterioration of the crystallinity of the GaN layer.
[0018] The second substrate is provided with a diamond layer whose surface is a (111) plane. In the second substrate treatment step, the surface of the diamond layer of the second substrate is subjected to an oxidation treatment to introduce oxygen atoms into the surface of the diamond layer and functionalize the surface of the diamond layer. By the oxidation treatment, C—O—C groups or —OH groups are formed on the surface of the diamond layer. The surface of this functionalized diamond layer has properties that make it easy to bond with the surface of the gallium oxide layer functionalized in the first substrate treatment step.
[0019] In the bonding step, the surface of the gallium oxide layer that has undergone the first substrate treatment step is brought into contact with the surface of the diamond layer that has undergone the second substrate treatment step, and reaction energy is applied to this contact portion to bond the first substrate and the second substrate. Examples of reaction energy include thermal energy, light energy, electrical energy, and chemical energy. In this embodiment, the contact portion between the first substrate and the second substrate is heated to a temperature of approximately 200°C.
[0020] The bonding step bonds the surfaces of the gallium oxide layer and the diamond layer together. According to the electron energy loss spectroscopy of the gallium oxide layer and the diamond layer after bonding, it is believed that the gallium oxide layer and the diamond layer are not bonded by the formation of a Ga-O-C bond, but are bonded by the diffusion of C atoms on the surface of the diamond layer into the gallium oxide layer. The bonding step can be carried out in a vacuum chamber, but can also be carried out in the atmosphere. Therefore, the bonding step in the manufacturing method of the composite of this embodiment does not require a vacuum bonding device.
[0021] A method for manufacturing a composite according to a second embodiment of the present application will be described. In the description of the method for manufacturing a composite according to this embodiment, overlapping with the method for manufacturing a composite according to the first embodiment will be omitted as appropriate. The method for manufacturing a composite according to this embodiment also includes a first substrate treatment step, a second substrate treatment step, and a bonding step. In the first substrate treatment step, a nitriding treatment is performed on the surface of the gallium oxide layer of a first substrate, which includes a gallium nitride layer and an exposed gallium oxide layer formed on the gallium nitride layer, to functionalize the surface of the gallium oxide layer. In the second substrate treatment step, an oxidation treatment is performed on the surface of the diamond layer of a second substrate, which includes a diamond layer whose surface is a (100) plane, to functionalize the surface of the diamond layer.
[0022] Diamonds with a (100) surface (hereinafter simply referred to as "(100) diamond") are commonly used in industry. However, bonding (100) diamond to GaN has been difficult. The present inventors have discovered that by nitriding a gallium oxide layer on a gallium nitride layer, rather than by oxidation and reduction, it becomes easier to bond to the oxidized (100) diamond surface. In the bonding step, similar to the bonding step in the manufacturing method of the composite of the first embodiment, the surface of the gallium oxide layer that has undergone the first substrate treatment step and the surface of the diamond layer that has undergone the second substrate treatment step are brought into contact with each other, and reaction energy is applied to this contact portion to bond the first substrate and the second substrate.
[0023] Example 1: A GaN / sapphire substrate (POWDEC, 0.635 mm thick) having a 2 μm-thick GaN layer on the sapphire substrate surface, with the (0001) surface polished, was cut into a parallelogram shape with one side approximately 8 mm and the adjacent side approximately 7 mm. The surface of the GaN layer of this GaN / sapphire substrate was treated using the following procedure. The surface of this GaN layer, i.e., the native GaN oxide layer, was immersed for 10 minutes in a treatment solution composed of 10 mL of 28% ammonia water, 10 mL of 35% hydrogen peroxide water, and 50 mL of pure water at a temperature of 75°C. The surface of this GaN layer was then washed with pure water for 5 minutes (oxidation treatment).
[0024] On the other hand, the surface of the diamond layer of a single crystal diamond substrate (EDP Corporation) with a surface of (111) plane, a thickness of 0.3 mm, and a square of 3 mm was treated under the same conditions as the surface treatment of the GaN layer (oxidation treatment). By these oxidation treatments, the surface of the GaN layer and the surface of the diamond layer were functionalized, making these surfaces easy to bond with each other. After leaving the surface of this GaN layer and the surface of this diamond layer in contact in the atmosphere for 1 day, they were heated at a temperature of 200 ° C for 2 hours, and obtained a composite 1 in which the GaN / sapphire substrate and the diamond substrate were bonded, that is, the GaN layer and the diamond layer were bonded.
[0025] Figure 1 is a planar image of composite 1 observed from the diamond substrate side. As shown in Figure 1, no bright areas indicating depletion between the substrates were observed. In other words, most of the surface of the GaN layer of the GaN / sapphire substrate and the surface of the diamond layer of the diamond substrate were bonded. From the sapphire substrate side of composite 1, a wavelength of 248 nm and an energy density of 1000 mJ / cm were used. 2 The GaN layer was peeled off from the GaN / sapphire substrate and transferred to the surface of the diamond layer of the diamond substrate, obtaining a composite 2 in which the diamond layer was bonded to the GaN layer. Figure 2 is a planar image of the composite 2 observed from the GaN layer side. As shown in Figure 2, multiple rectangular GaN layers measuring 0.3 mm x 0.15 mm were formed in the right region of the surface of the 3 mm square diamond substrate. The thickness of this GaN layer was 2 μm.
[0026] Example 2 A GaN / Si substrate (CoorsTek, thickness 0.635 mm) having a 2 μm-thick GaN layer on the surface of a Si substrate, the (0001) surface of which was polished, was cut into a 15 mm × 16 mm rectangle. The surface of the GaN layer of this GaN / Si substrate was treated using the following procedure. The surface of this GaN layer, i.e., the native GaN oxide layer, was immersed for 10 minutes in a treatment solution composed of 10 mL of 35% hydrochloric acid and 60 mL of pure water at a temperature of 70°C. The surface of this GaN layer was then washed with pure water for 5 minutes (reduction treatment).
[0027] FIG. 14 shows the X-ray photoelectron spectroscopy spectra of the surface of the GaN layer after this reduction treatment ("HCl treated" in the figure) and the surface of the GaN layer before this reduction treatment ("untreated" in the figure). As shown in FIG. 14, by treating the surface of the GaN layer with hydrochloric acid, the peak derived from the O1s orbital becomes smaller and the position of this peak shifts to the higher energy side. The reduction treatment of the surface of the GaN layer makes the native oxide layer on the surface of the GaN layer thinner, and the Ga 2 O 3 It can be seen that Ga—OH, which has a larger bond energy than -NH 2 The peak due to the Ga—NH group and the peak due to the —Cl group at around 200 eV became larger. 2 It can be seen that Ga—Cl is formed.
[0028] On the other hand, a surface-treated diamond substrate was obtained under the same conditions as in Example 1, except that the temperature of the treatment solution during immersion was changed to 70°C (oxidation treatment). It is known that C-O-C or C-OH is formed on the surface of a diamond layer that has been subjected to oxidation treatment. Thereafter, a composite in which the GaN layer of the GaN / Si substrate and the diamond layer of the diamond substrate were bonded was obtained by the same method as in Example 1. The -OH groups and -NH 2 This composite was obtained by the reaction at the interface between the -Cl groups and the C-O-C groups or -OH groups formed on the surface of the diamond layer.
[0029] Figure 3 is a planar image of this composite when observed from the diamond substrate side. As shown in Figure 3, this composite has the diamond layer surfaces of two small diamond substrates bonded to the GaN layer surface of a large GaN / Si substrate. Even though the GaN layer and diamond layer overlap, Newton's rings are observed in the areas where the GaN layer surface and the diamond layer surface are not bonded. As shown in Figure 3, the surface of the diamond layer of the diamond substrate in the upper right is bonded to the GaN layer surface over the entire surface, and the diamond layer surface of the diamond substrate in the lower center is bonded to approximately 70% of the GaN layer surface.
[0030] This composite was cut using laser light, passing through the diamond substrate, the GaN layer, and the Si substrate. Figure 4 is a microscope image of this cross section. As shown in Figure 4, no non-bonded areas were observed at the bonded interface between the diamond layer and the GaN layer of the diamond substrate. In addition, this composite was cut using laser light, and an ultrathin sample was prepared by irradiating the cross section with a focused ion beam. The bonded interface between the diamond layer and the GaN layer of this sample was observed using a transmission electron microscope. Figure 5 is a transmission electron microscope image of this bonded interface. As shown in Figure 5, an intermediate layer approximately 3 nm thick was observed at the bonded interface.
[0031] The composition of this intermediate layer was analyzed by energy dispersive X-ray spectroscopy. Figure 6 shows the energy dispersive X-ray spectrum of this intermediate layer. The elemental ratio of this intermediate layer was C: 59.8%, Ga: 28.0%, O: 9.4%, N: 2.8%, and Cl: 0.1%, with the O content being greater than the N content. Furthermore, elemental mapping was performed near the bonding interface of this sample using energy dispersive X-ray spectroscopy. Figure 7 shows a transmission electron microscope image of the bonding interface of this sample and elemental maps of C, Ga, O, N, and Cl. The GaN layer portion was composed of Ga and N, the diamond layer portion was composed of C, and small amounts of O and Cl were observed at the bonding interface.
[0032] The structures of the intermediate layer and the diamond layer of this sample were also evaluated by electron energy loss spectroscopy (EELS). Figure 8 shows electron energy loss spectroscopy spectra of the intermediate layer and the diamond layer of this sample for C, Ga, O, and N. In the region of high crystallinity of diamond, a carbon σ bond (sp 3 A peak due to σ bonds was observed inside the diamond layer of this sample (inside diamond in the figure), but a peak due to π bonds (sp 2 ) were observed. Furthermore, Ga and O peaks were detected inside the diamond layer and the intermediate layer (inside the interfacial intermediate layer in the figure), but no significant peak was detected for N. From these results, it can be seen that the intermediate layer is sp 2It is thought to be composed of bonded carbon, gallium, and oxygen.
[0033] Comparative Example 1 The surface of the GaN layer of the same GaN / sapphire substrate as in Example 1 and the surface of the diamond layer of the same single crystal diamond substrate as in Example 1 were washed with acetone, ethanol, and pure water, in that order, for 5 minutes each. The cleaned surfaces of these GaN / sapphire substrate and diamond substrate were left in contact with each other in the atmosphere for 1 day, and then heated at a temperature of 200 ° C for 2 hours. However, the GaN layer of the GaN / sapphire substrate and the diamond layer of the single crystal diamond substrate did not bond. Unlike Example 1, the surface treatments with acetone, ethanol, and pure water, which do not fall under the categories of oxidation treatment, nitridation treatment, and reduction treatment, did not change the properties of the surfaces of the GaN layer and the diamond substrate to make them easier to bond.
[0034] Comparative Example 2: The same GaN / sapphire substrate as in Example 1 was cut into a parallelogram with one side approximately 8 mm and the adjacent side approximately 7 mm. The surface of the GaN layer of this GaN / sapphire substrate was treated (reduction treatment) under the same conditions as the surface treatment of the GaN layer of the GaN / sapphire substrate in Example 2. Meanwhile, the surface of the diamond layer of a single-crystal diamond substrate (EDP Corporation) with a (100) surface, a thickness of 0.3 mm, and a size of 5 mm square was treated (oxidation treatment) under the same conditions as the surface treatment of the diamond layer of the diamond substrate in Example 1.
[0035] Thereafter, a bonded structure was obtained in which the GaN layer of the GaN / sapphire substrate and the diamond layer of the diamond substrate were bonded by the same method as in Example 1. Figure 9 is a planar image of this bonded structure observed from the diamond substrate side. As shown in Figure 9, the depletion between the GaN / sapphire substrate and the diamond substrate was bright, and Newton's rings were observed, indicating that the GaN layer and the diamond layer were not bonded completely.
[0036] Comparative Example 3: The same GaN / sapphire substrate as in Example 1 was cut into a parallelogram shape with one side approximately 8 mm and the adjacent side approximately 7 mm. The surface of the GaN layer of this GaN / sapphire substrate was treated (oxidation treatment) under the same conditions as the surface treatment of the GaN layer of the GaN / sapphire substrate in Example 1. Meanwhile, the surface of the diamond layer of the same diamond substrate as in Comparative Example 2 was subjected to reactive ion etching (oxidation treatment) using oxygen gas at a pressure of 40 Pa at a power of 200 W for 30 seconds.
[0037] Thereafter, the same method as in Example 1 was used to obtain an adhered body in which the GaN layer of the GaN / sapphire substrate and the diamond layer of the diamond substrate were adhered. Figure 10 is a planar image of this adhered body observed from the diamond substrate side. As shown in Figure 10, the depletion between the GaN / sapphire substrate and the diamond substrate was bright, and Newton's rings were observed, indicating that the GaN layer and the diamond layer were not completely bonded in this adhered body. Furthermore, this adhered body broke when a shear strength of 48 kPa was applied.
[0038] Example 3 The same GaN / sapphire substrate as in Example 1 was cut into a parallelogram shape with one side approximately 8 mm and the adjacent side approximately 7 mm. The surface of the GaN layer of this GaN / sapphire substrate was treated under the same conditions as the surface treatment of the GaN layer of the GaN / sapphire substrate in Example 1. Furthermore, the surface of this GaN layer was subjected to reactive ion etching treatment (nitriding treatment) using nitrogen gas at a pressure of 40 Pa and an output of 200 W for 30 seconds. Meanwhile, the surface of the diamond layer of the same diamond substrate as in Comparative Example 2 was treated under the same conditions as the surface treatment of the diamond layer of the diamond substrate in Example 1 (oxidation treatment).
[0039] Thereafter, a composite was obtained in which the GaN layer of the GaN / sapphire substrate and the diamond layer of the diamond substrate were bonded together using the same method as in Example 1. Figure 11 shows a planar image of this composite observed from the diamond substrate side. Darkness due to depletion between the substrates was only observed in a portion of the right side of the diamond substrate. In other words, in this composite, the substrates, i.e., the GaN layer and the diamond layer, were mostly bonded together. This composite broke when a shear strength of 2.8 MPa was applied.
[0040] Example 4 The same GaN / sapphire substrate as in Example 1 was cut into a 15 mm x 16 mm rectangle. The subsequent procedure was the same as in Example 3, resulting in a GaN / sapphire substrate in which the surface of the GaN layer was nitrided. Meanwhile, the surface of the diamond layer of a circular mosaic single-crystal diamond minimal wafer (EDP Corporation), with a (100) surface, a thickness of 0.3 mm, and a diameter of 12.5 mm, was treated (oxidation treatment) under the same conditions as those for the surface treatment of the diamond layer of the diamond substrate in Example 1.
[0041] Thereafter, a composite was obtained in which the GaN layer of the GaN / sapphire substrate and the diamond layer of the diamond wafer were bonded together using the same method as in Example 1. Figure 12 is a planar image of this composite observed from the diamond wafer side. Darkness due to depletion between the substrate and the wafer was only observed in a small area to the upper left of the center of the diamond wafer. In other words, in this composite, most of the GaN layer and the diamond layer were bonded together.
[0042] Reference Example: The surface of the GaN layer of the same GaN / sapphire substrate as in Example 1 was irradiated for 120 seconds with an Ar atomic beam accelerated at a voltage of 1.5 kV and a current of 100 mA, thereby obtaining a GaN substrate 1 in which the surface oxide film of the GaN layer had been sputter-removed. Furthermore, a GaN substrate 2 was obtained in which the surface of the GaN layer had been subjected to a reduction treatment in the same manner as in Example 2. Furthermore, a GaN substrate 3 was obtained in which the surface of the GaN layer had been subjected to a nitriding treatment in the same manner as in Example 3. The crystallinity of these GaN substrates was evaluated using XRD. Specifically, X-rays were incident on the surface of each GaN substrate at an incident angle of 0.3°, and the peak derived from the GaN (110) plane near 2Θ = 57.775 in a region approximately 8 nm away from the surface was evaluated.
[0043] FIG. 13 shows the results of rocking curve measurement of each GaN substrate by XRD. A larger half-width indicates a deterioration in the crystallinity of GaN. For GaN substrate 1, the half-width of the in-plane XRD was 0.333°, and the half-width of the rocking curve measurement was 0.418°. For GaN substrate 2, the half-width of the in-plane XRD was 0.331°, and the half-width of the rocking curve measurement was 0.395°. For GaN substrate 3, the half-width of the in-plane XRD was 0.330°, and the half-width of the rocking curve measurement was 0.387°.
[0044] That is, when the surface oxide film of the GaN layer was removed, as in GaN substrate 1, the crystallinity of the surface of the GaN layer was significantly deteriorated. In contrast, when the surface oxide film of the GaN layer was not completely removed but the surface was functionalized, as in GaN substrates 2 and 3, the deterioration of the crystallinity of the surface of the GaN layer could be suppressed. Therefore, it was found that by subjecting the surface oxide film of the GaN layer to the oxidation treatment, nitriding treatment, and reduction treatment of the present application, the surface of the GaN layer can be changed to a state that makes it easier to bond to the surface of a diamond layer while suppressing the deterioration of the crystallinity of the surface of the GaN layer.
Claims
1. A composite having a gallium nitride layer, an intermediate layer formed on a surface of the gallium nitride layer and containing carbon, gallium, and oxygen, and a diamond layer bonded to the surface of the gallium nitride layer via the intermediate layer.
2. A composite according to claim 1, wherein the diamond layer has a surface of a (100) or (111) plane, or is a mosaic crystal having a surface of a (100) or (111) plane.
3. The composite according to claim 2, wherein the thickness of the intermediate layer is 4 nm or less.
4. The composite of claim 3, wherein the nitrogen content of said intermediate layer is less than the oxygen content.
5. A composite according to any one of claims 1 to 4, wherein a second substrate containing the diamond layer is bonded to a first substrate containing the gallium nitride layer, and the shear strength between the first substrate and the second substrate is 0.1 MPa or more.
6. A method for producing a composite, comprising: a first substrate treatment step of subjecting a surface of a gallium oxide layer of a first substrate having a gallium nitride layer and an exposed gallium oxide layer formed on the gallium nitride layer to one or more of oxidation, nitridation and reduction treatments to functionalize the surface of the gallium oxide layer; a second substrate treatment step of subjecting a surface of a diamond layer of a second substrate having a diamond layer whose surface is a (111) plane to oxidation treatment to functionalize the surface of the diamond layer; and a joining step of bringing the surface of the gallium oxide layer that has been subjected to the first substrate treatment step into contact with the surface of the diamond layer that has been subjected to the second substrate treatment step into contact with each other, and applying reaction energy to the contact portion to join the first substrate and the second substrate.
7. A method for producing a composite, comprising: a first substrate treatment step of subjecting a surface of a gallium oxide layer of a first substrate having a gallium nitride layer and an exposed gallium oxide layer formed on the gallium nitride layer to a nitriding treatment to functionalize the surface of the gallium oxide layer; a second substrate treatment step of subjecting a surface of a diamond layer of a second substrate having a diamond layer whose surface is a (100) plane to an oxidation treatment to functionalize the surface of the diamond layer; and a joining step of bringing the surface of the gallium oxide layer that has undergone the first substrate treatment step into contact with the surface of the diamond layer that has undergone the second substrate treatment step, and applying reaction energy to the contact portion to join the first substrate and the second substrate.
8. The method for producing a composite according to claim 6, wherein the first substrate treatment step comprises carrying out an oxidation treatment, the oxidation treatment being treatment with a liquid containing ammonia and hydrogen peroxide.
9. The method for producing a composite according to claim 6, wherein the first substrate treatment step comprises a nitriding treatment, the nitriding treatment being a treatment with reactive nitrogen plasma.
10. The method for producing a composite according to claim 6, wherein the first substrate treatment step comprises carrying out a reduction treatment, the reduction treatment being a treatment with hydrochloric acid.
11. The method according to claim 10, wherein in the first substrate treatment step, the surface of the gallium oxide layer is treated with -OH groups, -NH 2 A method for preparing a composite functionalized with one or more of the -Cl and -Cl groups.
12. A method for producing a composite according to claim 7, wherein the nitriding treatment is a treatment with reactive nitrogen plasma.
13. A method for producing a composite according to any one of claims 6 to 12, wherein the joining step is carried out in the atmosphere.
Citation Information
Patent Citations
Manufacturing of gallium nitride devices with a diamond layer
JP2012513675A
Semiconductor stacked structure and semiconductor device
JP2018049868A
Composite body comprising silicon carbide and method for producing same
WO2022196241A1
Joined body comprising mosaic diamond wafer and semiconductor of different type, method for producing same, and mosaic diamond wafer for use in joined body with semiconductor of different type
WO2022255363A1