Two-dimensional particle, and electroconductive film and method for producing same
By integrating a hydrocarbon compound on MXene layers to prevent oxidation, the conductivity stability of MXene materials is enhanced, addressing the temperature-induced instability in MXene-based films.
Patent Information
- Application Number
- PCT/JP2024/010284
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-24
- Filing Date
- 2024-03-15
- Publication Date
- 2024-10-03
AI Technical Summary
MXene materials exhibit unstable electrical conductivity, particularly at high temperatures, due to oxidation issues.
Incorporating a hydrocarbon compound on the surface of MXene layers, which can be physically or chemically bonded, to suppress oxidation and maintain conductivity stability even in high-temperature environments.
The method effectively stabilizes the electrical conductivity of MXene-based films, ensuring high conductivity is maintained across varying temperatures.
Smart Images

Figure JP2024010284_03102024_PF_FP_ABST
Abstract
Description
Two-dimensional particles, conductive film and method for producing the same
[0001] The present disclosure relates to two-dimensional particles, conductive films, and methods for producing the same.
[0002] In recent years, MXene has attracted attention as a novel electrically conductive material. MXene is a type of so-called two-dimensional material, and as described below, it is a layered material having the form of one or more layers. MXene generally has the form of particles of such layered materials (which may include powders, flakes, nanosheets, etc.).
[0003] In Patent Document 1, Ti 2 By immersing the AlC-TiC mixture in a HF solution, Ti 3 C 2 (OH) 2 It is described that MXene represented by the formula:
[0004] Non-Patent Document 1 shows that delamination of multilayer MXene was achieved by handshaking using TMAOH (tetramethylammonium hydroxide), and by using DMSO (dimethyl sulfoxide) and further ultrasonic treatment.
[0005] U.S. Patent Publication No. 2014 / 0162130
[0006] Guidelines for Synthesis and Processing of Two-Dimensional Titanium Carbide (Ti3C2Tx MXene) Chem. Mater. 2017, 29, 7633-7644
[0007] Although MXene described in Patent Document 1 and Non-Patent Document 1 exhibits electrical conductivity, the stability of the electrical conductivity is not fully satisfactory.
[0008] The present disclosure aims to provide two-dimensional particles capable of realizing a conductive film with good stability of conductivity, preferably two-dimensional particles capable of realizing a conductive film with good stability of conductivity even in a high-temperature environment. The present disclosure also aims to provide a conductive film including such two-dimensional particles and a method for producing such two-dimensional particles.
[0009] The two-dimensional particles of the present disclosure comprise one or more layers and a hydrocarbon compound, wherein the layers have the following formula: M m X n (wherein M is at least one Group 3, 4, 5, 6, or 7 metal; X is a carbon atom, a nitrogen atom, or a combination thereof; n is 1 or more and 4 or less; and m is greater than n and 5 or less). The hydrocarbon compound is present on the layer.
[0010] The method for producing two-dimensional particles of the present disclosure includes heating precursor particles in the presence of an organic compound under conditions of an absolute pressure of less than 1,013 hPa and a temperature equal to or higher than the boiling point of the organic compound to obtain two-dimensional particles, wherein the precursor particles include one or more layers, and the layers are represented by the following formula: M m X n (wherein M is at least one metal of Group 3, 4, 5, 6 or 7; X is a carbon atom, a nitrogen atom or a combination thereof; n is 1 or more and 4 or less; and m is greater than n and 5 or less), and a modification or termination T (T is at least one selected from the group consisting of a hydroxyl group, a fluorine atom, a chlorine atom, an iodine atom, an oxygen atom, a chlorine atom, a phosphorus atom and a hydrogen atom) present on the surface of the layer body, and the melting point of the organic compound is 20°C or less.
[0011] According to the present disclosure, it is possible to provide two-dimensional particles capable of realizing a film in which the decrease in conductivity is suppressed, preferably two-dimensional particles capable of realizing a conductive film in which the decrease in conductivity is suppressed even in a high-temperature environment. The present disclosure can also provide a conductive film including such two-dimensional particles and a method for producing such two-dimensional particles.
[0012] 1A and 1B are schematic cross-sectional views of layered MXene particles according to one embodiment of the present disclosure, where (a) shows a single-layer MXene particle and (b) shows a multi-layer (exemplarily two-layer) MXene particle.
[0013] First Embodiment: Two-Dimensional Particles Hereinafter, two-dimensional particles according to one embodiment of the present disclosure will be described.
[0014] The two-dimensional particles of the present disclosure comprise one or more layers and a hydrocarbon compound, wherein the layers have the following formula: M m X n (wherein M is at least one metal of Group 3, 4, 5, 6 or 7; X is a carbon atom, a nitrogen atom or a combination thereof; n is 1 or more and 4 or less; and m is greater than n and 5 or less), and a modified or terminated T (T is at least one selected from the group consisting of a hydroxyl group, a fluorine atom, a chlorine atom, an iodine atom, an oxygen atom, a chlorine atom, a phosphorus atom and a hydrogen atom) present on the surface of the layer body, and the hydrocarbon compound is present on the layer.
[0015] According to the present disclosure, it is possible to provide two-dimensional particles capable of realizing a film in which a decrease in conductivity is suppressed, and preferably two-dimensional particles capable of realizing a conductive film in which a decrease in conductivity is suppressed even in a high-temperature environment. Although the present disclosure should not be interpreted as being limited to a particular theory, the reason why the two-dimensional particles of the present disclosure exhibit the above-mentioned effects is thought to be as follows.
[0016] Although the present disclosure should not be interpreted as being limited to any particular theory, oxidation of MXene is one of the causes of the decrease in conductivity of MXene. In the two-dimensional particles of the present disclosure, the presence of a hydrocarbon compound on the MXene layer is thought to suppress oxidation of the MXene layer even in high-temperature environments. As a result, it is thought that it is possible to realize a film with a suppressed decrease in conductivity, particularly a conductive film with a suppressed decrease in conductivity even in high-temperature environments.
[0017] In the present disclosure, the phrase "a hydrocarbon compound is present on a layer" includes both a case where the hydrocarbon compound is physically or chemically bound to the layer and a case where the hydrocarbon compound is not bound to the layer, and may also include a case where the hydrocarbon compound is not bound to the layer, a case where the hydrocarbon compound is in contact with the layer, and a case where the hydrocarbon compound is not in contact with the layer.
[0018] In the present disclosure, when an "atom" refers to a certain element, the oxidation number of the element is not limited to 0, but may be any number within the range of possible oxidation numbers of the element.
[0019] In this disclosure, "hydrocarbon compound" means a compound consisting of carbon atoms and hydrogen atoms, and may include aromatic hydrocarbon compounds, saturated or unsaturated aliphatic hydrocarbon compounds, and saturated or unsaturated alicyclic hydrocarbon compounds.
[0020] In this disclosure, the term "aromatic hydrocarbon compound" refers to a hydrocarbon compound containing an aromatic hydrocarbon group. In addition, in this disclosure, the term "alicyclic hydrocarbon compound" refers to a hydrocarbon compound containing an alicyclic hydrocarbon group.
[0021] In this disclosure, the layer may be referred to as an MXene layer, and the two-dimensional particles may be referred to as MXene two-dimensional particles or MXene particles.
[0022] The above M m X n In a layer body represented by the formula: wherein each X is located within an octahedral array of M, the layer body may have a crystal lattice.
[0023] The modification or terminal T may be m X n The modified or terminal T may be present on the surface of the layer body represented by the formula (I), for example, on at least one of the two surfaces of the layer body that face each other. The modified or terminal T is preferably a hydroxyl group, a fluorine atom, a chlorine atom, an iodine atom, SO 4 2- and P.O. 4 3- and more preferably, a chlorine atom, an iodine atom, or SO 42- and P.O. 4 3- It may contain one or more selected from:
[0024] In the present disclosure, the two-dimensional particles may be understood as layered materials or layered compounds, and are referred to as "M m X n T s ", where s is any number, and conventionally, x or z may be used instead of s. Typically, n can be 1, 2, 3, or 4, but is not limited thereto.
[0025] In the above formula for MXene, M is preferably at least one selected from the group consisting of Ti, Zr, Hf, V, Nb, Ta, Cr, Mo, and Mn, more preferably at least one selected from the group consisting of Ti, V, Cr, and Mo, and even more preferably at least one selected from the group consisting of Ti and V.
[0026] MXene is a compound represented by the formula: M m X n However, it is known that it can be expressed as follows: Sc 2 C, Ti 2 C, Ti 2 N, Zr 2 C, Zr 2 N, Hf 2 C, Hf 2 N.V. 2 C.V. 2 N, Nb 2 C, Ta 2 C, Cr 2 C, Cr 2 N, Mo 2 C, Mo 1.3 C, Cr 1.3 C, (Ti, V) 2 C, (Ti, Nb) 2 C.W. 2 C.W. 1.3 C, Mo 2 N, Nb 1.3 C, Mo 1.3 Y 0.6 C (in the above formula, "1.3" and "0.6" mean approximately 1.3 (= 4 / 3) and approximately 0.6 (= 2 / 3), respectively), Ti 3C 2 、Ti 3 N 2 、Ti 3 (CN)、Zr 3 C 2 、(Ti,V) 3 C 2 、(Ti 2 Nb)C 2 、(Ti 2 Ta)C 2 、(Ti 2 Mn)C 2 、Hf 3 C 2 、(Hf 2 V)C 2 、(Hf 2 Mn)C 2 、(V 2 Ti)C 2 、(Cr 2 Ti)C 2 、(Cr 2 V)C 2 、(Cr 2 Nb)C 2 、(Cr 2 Ta)C 2 、(Mo 2 Sc)C 2 、(Mo 2 Ti)C 2 、(Mo 2 Zr)C 2 、(Mo 2 Hf)C 2 、(Mo 2 V)C 2 、(Mo 2 Nb)C 2 、(Mo 2 Ta)C 2 、(W 2 Ti)C 2 、(W 2 Zr)C 2 、(W 2 Hf)C 2 、 Ti 4 N 3 、V 4 C 3 、Nb 4 C 3 、Ta 4 C 3 、(Ti,Nb) 4 C 3 、(Nb,Zr)4 C 3 , (Ti 2 Nb 2 )C 3 , (Ti 2 Yes 2 )C 3 , (V 2 Ti 2 )C 3 , (V 2 Nb 2 )C 3 , (V 2 Yes 2 )C 3 , (Nb) 2 Yes 2 )C 3 , (Cr 2 Ti 2 )C 3 , (Cr 2 V 2 )C 3 , (Cr 2 Nb 2 )C 3 , (Cr 2 Yes 2 )C 3 , (Mo) 2 Ti 2 )C 3 , (Mo) 2 Zr 2 )C 3 , (Mo) 2 Hf 2 )C 3 , (Mo) 2 V 2 )C 3 , (Mo) 2 Nb 2 )C 3 , (Mo) 2 Yes 2 )C 3 , (W 2 Ti 2 )C 3 , (W 2 Zr 2 )C 3 , (W 2 Hf 2 )C 3 , (Mo) 2.7 V 1.3 )C 3(In the above formula, "2.7" and "1.3" mean approximately 2.7 (= 8 / 3) and approximately 1.3 (= 4 / 3), respectively.)
[0027] Representatively, M m X n But Ti 2 C, Ti 3 C 2 , Ti 3 (CN), (Cr 2 Ti)C 2 , (Mo 2 Ti)C 2 , (Mo 2 Ti 2 ) C 3 , (Mo 2.7 V 1.3 ) C 3 and V 4 C 3 and preferably, M m X n But Ti 2 C, Ti 3 C 2 , Ti 3 (CN), (Cr 2 Ti)C 2 , (Mo 2 Ti)C 2 , (Mo 2 Ti 2 ) C 3 , and (Mo 2.7 V 1.3 ) C 3 The compound is represented by at least one selected from the group consisting of:
[0028] Typically, in the above formula, M can be titanium or vanadium, and X can be a carbon atom or a nitrogen atom. For example, the MAX phase can be Ti 3 AlC 2 or V 4 AlC 3 and the layer body is Ti 3 C 2 or V 4 C 3 and MXene is Ti 3 C 2 T s or V 4 C 3 Ts (In other words, M is Ti or V, X is C, n is 2 or 3, and m is 3 or 4). In particular, M m X n is Ti 3 C 2 or V 4 C 3 In one embodiment, the MAX phase may be Ti 3 AlC 2 and the layer body is Ti 3 C 2 and MXene is Ti 3 C 2 T s (In other words, M is TiV, X is C, n is 2, and m is 3). In particular, M m X n is Ti 3 C 2 In another aspect, the MAX phase can be V 4 AlC 3 and the layer body is V 4 C 3 and MXene is V 4 C 3 T s (in other words, M is V, X is C, n is 3, and m is 4). In particular, M m X n is V 4 C 3 It could be.
[0029] In the present disclosure, MXene may contain a relatively small amount of A atoms derived from the MAX phase of the precursor, for example, 10 mass% or less, relative to 100 mass% of the total amount of A atoms contained in the MAX phase of the precursor. The residual amount of A atoms may be preferably 0 mass% or more and 8 mass% or less, more preferably 0 mass% or more and 6 mass% or less, relative to 100 mass% of the total amount of A atoms contained in the MAX phase of the precursor. However, even if the residual amount of A atoms exceeds 10 mass%, this may not be a problem depending on the application and use conditions of the two-dimensional particles.
[0030] The two-dimensional particle is an aggregate including one layer of MXene particles (hereinafter simply referred to as "MXene particles") 10a (single-layer MXene particles) as shown in Fig. 1(a). More specifically, the MXene particles 10a are m X n The layer body (M m X n The MXene layer 7a has a main layer 1a and modifications or terminations T3a, 5a present on the surface of the main layer 1a (more specifically, on at least one of the two opposing surfaces of each layer). m X n T s ", where s is an arbitrary number. Note that hydrocarbon compounds are not shown in FIG. 1(a).
[0031] The two-dimensional particles may contain one or more layers. Examples of MXene particles with multiple layers (multilayer MXene particles) include, but are not limited to, two-layer MXene particles 10b, as shown schematically in Figure 1(b). 1b, 3b, 5b, and 7b in Figure 1(b) are the same as 1a, 3a, 5a, and 7a in Figure 1(a). Two adjacent MXene layers (e.g., 7a and 7b) in a multilayer MXene particle do not necessarily need to be completely separated and may be partially in contact. The MXene particle 10a may consist of the multilayer MXene particles 10b separated into a single layer, or may contain unseparated multilayer MXene particles 10b, resulting in a mixture of the single-layer MXene particles 10a and multilayer MXene particles 10b. Hydrocarbon compounds are not shown in Figure 1(b).
[0032] Although this embodiment is not limited thereto, the thickness of each layer (corresponding to the above-described MXene layers 7a and 7b) contained in the MXene particle is, for example, 0.8 nm to 5 nm, particularly 0.8 nm to 3 nm (this may vary mainly depending on the number of M atomic layers contained in each layer). The interlayer distance (or gap dimension, shown as Δd in FIG. 1(b)) of each stack of the multilayer MXene particle that may be contained may be, for example, 0.8 nm to 10 nm, particularly 0.8 nm to 5 nm, more particularly 0.8 nm to 1.5 nm. The total number of layers may be 2 to 20,000.
[0033] In one aspect, the two-dimensional particles of this embodiment preferably include multilayer MXene particles having a small number of layers obtained through a delamination process. The term "small number of layers" refers to, for example, six or fewer MXene layers. Furthermore, the thickness of the multilayer MXene particles having a small number of layers in the stacking direction is preferably 15 nm or less, more preferably 10 nm or less. Hereinafter, these "multilayer MXene particles having a small number of layers" may be referred to as "small-layer MXene particles." Furthermore, single-layer MXene particles and small-layer MXene particles may be collectively referred to as "single-layer / small-layer MXene particles." The inclusion of single-layer / small-layer MXene particles can enhance the conductivity of the resulting film.
[0034] The two-dimensional particles of this embodiment preferably contain single-layered MXene particles and few-layered MXene particles, i.e., single-layered and few-layered MXene particles. The two-dimensional particles of this embodiment preferably contain single-layered and few-layered MXene particles with a thickness of 15 nm or less in an amount of 90% by volume or more, more preferably 95% by volume or more.
[0035] In one embodiment, the ratio of (average major axis length of the two-dimensional surfaces of the two-dimensional particles) / (average thickness length of the two-dimensional particles) is, for example, 1.2 or more, preferably 1.5 or more, and more preferably 2 or more. The average major axis length of the two-dimensional surfaces of the two-dimensional particles and the average thickness length of the two-dimensional particles may be determined by the method described below.
[0036] (Average value of major axes of two-dimensional surfaces of two-dimensional particles) The average value of major axes of two-dimensional surfaces of the two-dimensional particles of this embodiment is, for example, 1 μm or more and 20 μm or less. Hereinafter, the average value of major axes of the two-dimensional surfaces may be referred to as the "average flake size."
[0037] The larger the average flake size, the higher the conductivity of the film. The two-dimensional particles of this embodiment have a large average flake size of 1.0 μm or more. Therefore, a film formed using these two-dimensional particles, for example, a film obtained by laminating these two-dimensional particles, can achieve a conductivity of 2000 S / cm or more. The average long diameter of the two-dimensional surface is preferably 1.5 μm or more, more preferably 2.5 μm or more. When MXene is delaminate-treated by ultrasonic treatment, the majority of the MXene is reduced in diameter to approximately several hundred nanometers in long diameter, and therefore, a film formed from a single layer of MXene delaminated by ultrasonic treatment is considered to have low conductivity.
[0038] The average value of the major axis of the two-dimensional surface is, for example, 20 μm or less, preferably 15 μm or less, and more preferably 10 μm or less, from the viewpoint of dispersibility in the dispersion medium.
[0039] The longest diameter of the two-dimensional plane refers to the longest diameter when each MXene particle is approximated to an ellipse in an electron microscope photograph, and the average longest diameter of the two-dimensional plane refers to the number average of the longest diameters of 80 or more particles. As the electron microscope, a scanning electron microscope (SEM) or a transmission electron microscope (TEM) can be used.
[0040] The average major axis of the two-dimensional particles of this embodiment may be measured by dissolving a film containing the two-dimensional particles in a solvent and dispersing the two-dimensional particles in the solvent, or by measuring the average major axis from an SEM image of the film.
[0041] (Average Thickness of Two-Dimensional Particles) The average thickness of the two-dimensional particles of this embodiment is preferably 1 nm or more and 15 nm or less. The thickness is preferably 10 nm or less, more preferably 7 nm or less, and even more preferably 5 nm or less. On the other hand, considering the thickness of the monolayer MXene particles, the lower limit of the thickness of the two-dimensional particles can be 1 nm.
[0042] The average thickness of the two-dimensional particles is determined as a number-average size (for example, a number-average of at least 40 particles) based on atomic force microscope (AFM) or transmission electron microscope (TEM) photographs.
[0043] The two-dimensional particles contain a hydrocarbon compound. The hydrocarbon compound is considered to be present on the layer because the interatomic distance between the hydrocarbon compound and the layer is greater than the interatomic distance between the atoms in the layer body. As described above, in the present disclosure, the phrase "a hydrocarbon compound is present on the layer" includes both cases where the hydrocarbon compound is physically or chemically bonded to the layer and cases where the hydrocarbon compound and the layer are not bonded, and also includes cases where the hydrocarbon compound and the layer are not bonded, where the hydrocarbon compound and the layer are in contact, and where the hydrocarbon compound and the layer are not in contact. The inclusion of the hydrocarbon compound in such a manner is considered to suppress oxidation of the layer, and to contribute to suppressing a decrease in electrical conductivity, and further to suppressing a decrease in electrical conductivity in a high-temperature environment.
[0044] The hydrocarbon compound is typically a compound consisting of carbon atoms and hydrogen atoms, and may include aromatic hydrocarbon compounds, saturated or unsaturated aliphatic hydrocarbon compounds, and saturated or unsaturated alicyclic hydrocarbon compounds. The hydrocarbon compound preferably includes one or more compounds selected from aromatic hydrocarbon compounds and saturated or unsaturated aliphatic hydrocarbon compounds, and more preferably includes one or more compounds selected from saturated or unsaturated aliphatic hydrocarbon compounds.
[0045] The aromatic hydrocarbon compound may be preferably an aromatic hydrocarbon compound having 6 to 20 carbon atoms, more preferably an aromatic hydrocarbon compound having 6 to 10 carbon atoms, and specific examples thereof include toluene and xylene.
[0046] The saturated aliphatic hydrocarbon compound may be preferably a saturated aliphatic hydrocarbon compound having 1 to 20 carbon atoms, more preferably a saturated aliphatic hydrocarbon compound having 4 to 10 carbon atoms, and specific examples thereof include butane, isobutane, 2-methylbutane, 2-methylpentane, 2,4-dimethylpentane, 2-methylheptane, and octane.
[0047] The unsaturated aliphatic hydrocarbon compound may be an unsaturated aliphatic hydrocarbon compound preferably having 2 to 20 carbon atoms, more preferably having 3 to 10 carbon atoms, and specific examples thereof include propene, isobutene, pentene, 2-methylbutene, 2-methylpentene, 2-methylhexene, and octene.
[0048] The saturated or unsaturated alicyclic hydrocarbon compound may be a saturated or unsaturated alicyclic hydrocarbon compound preferably having 3 to 20 carbon atoms, more preferably having 6 to 10 carbon atoms, and specific examples thereof include cyclohexane, methylcyclohexane, cyclohexene, and methylcyclohexene.
[0049] The types of hydrocarbon compounds contained in the two-dimensional particles can be identified by gas chromatography-mass spectrometry (GC-MS), which is typically performed using a gas chromatography-mass spectrometry (GC-MS) device equipped with a vibrolyzer.
[0050] The content of carbon atoms derived from the hydrocarbon compound is preferably 0.5% by mass or more, more preferably 0.5% by mass or more and 5% by mass or less, and even more preferably 0.7% by mass or more and 3% by mass or less, based on 100% by mass of the total amount of the two-dimensional particles. When the content of carbon atoms derived from the hydrocarbon compound is within this range, it can be easy to improve the stability of the electrical conductivity while maintaining it.
[0051] The content of carbon atoms derived from the hydrocarbon compound can be measured by carbon-sulfur analysis (CS analysis). m X n is Ti 3 C 2 In this case, the content of carbon atoms derived from the hydrocarbon compound is determined based on the total amount of carbon atoms measured by carbon-sulfur analysis (CS analysis), and the total amount of carbon atoms in the layer of the two-dimensional particle (the layer body and modified or terminated T) is determined based on the total amount of carbon atoms measured by carbon-sulfur analysis (CS analysis). 3 C 2 O 2 The amount of carbon atoms calculated assuming that the carbon number is expressed as
[0052] The interlayer distance in the two-dimensional particles may be preferably 0.8 nm or more and 1.1 nm or less. The interlayer distance can be determined by X-ray diffraction measurement (XRD) as follows: 002 It can be measured as:
[0053] Second Embodiment: Method for Producing Two-Dimensional Particles Hereinafter, a method for producing two-dimensional particles according to one embodiment of the present disclosure will be described in detail, but the present disclosure is not limited to this embodiment.
[0054] The two-dimensional particles of this embodiment include a step of heating precursor particles in the presence of an organic compound under conditions of an absolute pressure of less than 1,013 hPa and a temperature equal to or higher than the boiling point of the organic compound to obtain two-dimensional particles, wherein the precursor particles include one or more layers, and the layers are represented by the following formula: M m X n (wherein M is at least one metal of Group 3, 4, 5, 6 or 7; X is a carbon atom, a nitrogen atom or a combination thereof; n is 1 or more and 4 or less; and m is greater than n and 5 or less), and a modification or termination T (T is at least one selected from the group consisting of a hydroxyl group, a fluorine atom, a chlorine atom, an iodine atom, an oxygen atom, a chlorine atom, a phosphorus atom and a hydrogen atom) present on the surface of the layer body, and the melting point of the organic compound is 20°C or less.
[0055] According to the method for producing two-dimensional particles of the present disclosure, it is possible to provide two-dimensional particles that can realize a conductive film with good stability of conductivity. Although the present disclosure should not be interpreted as being limited to a particular theory, the reason why the production method of the present disclosure exhibits the above-mentioned effects is thought to be as follows.
[0056] That is, in the method for producing two-dimensional particles disclosed herein, precursor particles are heated under reduced pressure in the presence of a liquid organic compound at a temperature equal to or higher than the boiling point of the organic compound. Heating under these conditions is thought to produce hydrocarbon compounds on the layers contained in the precursor particles, and the hydrocarbon compounds suppress oxidation of the layers, thereby improving the stability of electrical conductivity. While the reason for the production of hydrocarbon compounds is unclear, it is thought that the MXene layers are close to each other, and that modified or terminated T groups are present on the surface of the layers, resulting in a highly active state between the MXene layers. The coexistence of an organic compound in this state is thought to promote the production of hydrocarbon compounds.
[0057] The organic compound has a melting point of 20°C or lower at 1 atmosphere (1,013 hPa). When the melting point of the organic compound is 20°C or lower, the organic compound can penetrate into the interior of the precursor particles, making it easier to obtain two-dimensional particles containing a hydrocarbon compound. The melting point of the organic compound may be preferably 10°C or lower, more preferably -50°C or higher and 5°C or lower, and even more preferably -20°C or higher and 0°C or lower.
[0058] The boiling point of the organic compound is, for example, 285°C or lower, preferably 240°C or lower, more preferably 200°C or lower, and is, for example, 50°C or higher.
[0059] The dielectric constant of the organic compound may be preferably 60 or more, more preferably 60 or more and 300 or less, and even more preferably 60 or more and 250 or less. When the dielectric constant of the organic compound is in this range, it is thought that the hydrocarbon compound is more likely to precipitate.
[0060] The organic compound is soluble or miscible in water. The solubility of the organic compound in water is 5 g / 100 g H at 25° C. 2 0 or more, more preferably 10 g / 100 gH 2 In this specification, the solubility when miscible with water is treated as infinite.
[0061] The organic compound is preferably a compound with high polarity. In this specification, a compound with high polarity is a concept that includes not only compounds that exhibit clear charge separation but also compounds with high hydrophilicity. The polarity of a compound can be evaluated using the solubility parameter as an index. The Hildebrand solubility parameter (also referred to as the "SP value") of the organic compound is 19.0 MPa. 1/2 The SP value of the organic compound is preferably equal to or less than the SP value of water, and is 47.8 MPa or more. 1/2 The SP value is a value that serves as an index of the polarity of a compound, and the larger the SP value, the higher the polarity, and compounds with similar SP values tend to be more compatible with each other.
[0062] The molecular weight of the organic compound is, for example, 500 or less, preferably 300 or less, more preferably 200 or less, and is, for example, 30 or more.
[0063] Examples of the organic compound include organic compounds having one or more of a carbonyl group, an ester group, an amide group, a formamide group, a carbamoyl group, a carbonate group, an aldehyde group, an ether group, a sulfonyl group, a sulfinyl group, a hydroxyl group, a cyano group, and a nitro group, and preferably organic compounds having an amide group. Specific examples of the organic compound include alcohols such as methanol (MeOH), ethanol (EtOH), and 2-propanol; sulfone compounds such as sulfolane; sulfoxides such as dimethyl sulfoxide (DMSO); carbonates such as propylene carbonate (PC); amides such as N-methylformamide (NMF), N,N-dimethylformamide, N-methylpyrrolidone (NMP), and dimethylacetamide (DMAc); ketones such as acetone and methyl ethyl ketone (MEK); and tetrahydrofuran (THF), and preferably amides.
[0064] The pressure during heating is, in absolute terms, less than 1,013 hPa, preferably 1,000 hPa or less, more preferably 50 hPa to 1,000 hPa, and even more preferably 100 hPa to 1,000 hPa. By maintaining the pressure in this range, it is believed that the MXene layer can be maintained and hydrocarbon compounds can be easily produced.
[0065] The heating temperature is equal to or higher than the boiling point of the organic compound, preferably equal to or higher than 200° C., more preferably from 200° C. to 400° C., and even more preferably from 200° C. to 350° C. By maintaining the temperature in this range, it is believed that the layer structure of MXene can be maintained and hydrocarbon compounds can be more easily produced.
[0066] The heating time is preferably 1 hour or more and 30 hours or less, and more preferably 5 hours or more and 20 hours or less.
[0067] Pre-drying may be carried out before the heating. Such pre-drying may be carried out under normal pressure at 80 ° C or less. The pressure during pre-drying may be preferably 900 hPa or more and 1,200 hPa or less as an absolute pressure, and further may be 950 hPa or more and 1,160 hPa or less as an absolute pressure. The temperature during pre-drying may be 10 ° C or less, preferably 10 ° C or more and 80 ° C or less, more preferably 20 ° C or more and 70 ° C or less, and even more preferably 30 ° C or more and 70 ° C or less. The pre-drying time is, for example, 30 minutes to 10 hours, preferably 1 hour to 5 hours.
[0068] The amount of the organic compound may be, but is not limited to, preferably 5 parts by mass or more and 100 parts by mass or less, more preferably 10 parts by mass or more and 99 parts by mass or less, relative to 1 part by mass of the precursor particles.
[0069] The precursor particles can be produced by a production method including, but not limited to, typically: (a) preparing a predetermined precursor; (b) using an etching solution to remove at least a portion of the A atoms from the precursor to obtain an etched product; (c) washing the etched product to obtain an etched-washed product; (d) mixing the etched-washed product with an intercalator to obtain an intercalation product; and (e) stirring the intercalation product to obtain a delamination product containing the precursor particles.
[0070] The method for causing the precursor particles and the organic compound to coexist is not particularly limited, and may be, for example, one or more operations selected from the following (d1), (f), and (g): (d1) using an organic compound as an intercalator, (f) mixing the delamination-treated product with the organic compound, or (g) drying the delamination-treated product and then mixing it with the organic compound, but is not limited thereto.
[0071] Each step will be described in detail below.
[0072] Step (a) First, a predetermined precursor is prepared. The predetermined precursor that can be used in this embodiment is a MAX phase, which is a precursor of MXene, and is represented by the following formula: M m AX n (wherein M is at least one metal of Groups 3, 4, 5, 6, and 7, including at least Ti; X is a carbon atom, a nitrogen atom, or a combination thereof; A is at least one element of Groups 12, 13, 14, 15, and 16; n is 1 or more and 4 or less; and m is greater than n and 5 or less).
[0073] The above M, X, n and m are as described above.
[0074] A is at least one Group 12, 13, 14, 15, or 16 element, and is usually a Group A element, typically Group IIIA or Group IVA, and more particularly may include at least one element selected from the group consisting of Al, Ga, In, Tl, Si, Ge, Sn, Pb, P, As, S, and Cd, and is preferably Al.
[0075] The MAX phase is M m X n It has a crystal structure in which a layer composed of A atoms is located between two layers represented by M m X n The two layers represented by the formula (x, y, y) may have a crystal lattice in which each X is located in an octahedral array of M. The MAX phase is typically formed when m=n+1, with one layer of X atoms between each of the n+1 layers of M atoms (collectively referred to as "M m X n The repeating unit has a layer of A atoms (also referred to as an "A atom layer") arranged as the next layer after the n+1th layer of M atoms, but is not limited thereto.
[0076] The MAX phase can be produced by a known method. For example, TiC powder, Ti powder, and Al powder are mixed in a ball mill, and the resulting mixed powder is sintered in an Ar atmosphere to obtain a sintered body (a block of the MAX phase). The sintered body is then pulverized with an end mill to obtain the powdered MAX phase for the next step.
[0077] Step (b) In step (b), the M of the precursor is removed using an etching solution. m AX n An etching treatment is performed to remove at least a part of the A atoms from the precursor by etching. m X n The treated product is obtained in which at least a part of the layer constituted by A atoms has been removed while the layer represented by the formula (I) is maintained.
[0078] The etching solution may contain an acid such as HF, HCl, HBr, HI, sulfuric acid, phosphoric acid, or nitric acid, and typically, an etching solution containing F atoms can be used. Examples of such etching solutions include a mixture of LiF and hydrochloric acid, a mixture of hydrofluoric acid and hydrochloric acid, and a mixture containing hydrofluoric acid, and these mixtures may further contain phosphoric acid or the like. Typically, the etching solution may be an aqueous solution.
[0079] As the etching procedure and other conditions using the above etching solution, conditions conventionally used can be adopted.
[0080] Step (c) In step (c), the etched product obtained by the etching treatment is washed to obtain an etching-washed product. By performing washing, the acid used in the etching treatment and the like can be sufficiently removed.
[0081] The cleaning can be performed using a cleaning solution, typically by mixing the etched material with the cleaning solution. Such a cleaning solution typically contains water, preferably pure water. Alternatively, a small amount of hydrochloric acid or the like may be further contained in addition to pure water. The amount of cleaning solution to be mixed with the etched material and the method for mixing the etched material with the cleaning solution are not particularly limited. For example, such a mixing method may involve coexisting the etched material with the cleaning solution and then stirring, centrifuging, or the like. Examples of the stirring method include stirring using a hand shake, an automatic shaker, a shear mixer, a pot mill, or the like. The degree of stirring, such as the stirring speed and stirring time, may be adjusted depending on the amount and concentration of the etched material to be treated. Washing with the above cleaning solution may be performed one or more times, and it is preferable to perform washing with the cleaning solution multiple times. Specifically, for example, washing with the washing solution may be carried out by sequentially carrying out the following steps: step (i) adding the washing solution (to the treated product or the remaining precipitate obtained in (iii) below) and stirring; step (ii) centrifuging the stirred product; and step (iii) discarding the supernatant after centrifugation. Steps (i) to (iii) may be repeated two or more times, for example, 15 or less times.
[0082] Step (d) In step (d), an intercalation treatment is carried out using an intercalator to obtain an intercalation-treated product.
[0083] The intercalators include metal compounds containing metal cations, the organic compounds and organic salts described above.
[0084] The metal cations may be the same as the metal cations contained in the two-dimensional particles.
[0085] Examples of the metal compound include ionic compounds in which the metal cation and anion are bonded. Examples include sulfide salts including iodides, phosphates, and sulfates of the metal cations, nitrates, acetates, and carboxylates. The metal cation is preferably an alkali metal ion or an alkaline earth metal cation, and more preferably a lithium ion. The metal compound is preferably a metal compound containing an alkali metal ion or an alkaline earth metal ion, more preferably a metal compound containing lithium ion, and even more preferably an ionic compound of lithium ion, and particularly preferably one or more of iodides, phosphates, and sulfides of lithium ion. If lithium ion is used as the metal ion, it is thought that water hydrated with lithium ion has the most negative dielectric constant, making it easier to form a monolayer.
[0086] When a metal compound containing a metal cation is used as an intercalator, the metal cation can be intercalated into the etching and cleaning treatment product. As a result, the metal cation can be intercalated into two adjacent M m X n An intercalated product is obtained in which the intercalation occurs between the layers.
[0087] The organic compound is the same as the organic compound that is allowed to coexist when the precursor particles are heated.
[0088] When an organic compound is used as an intercalator, the organic compound is intercalated into the etching and cleaning treatment product. As a result, the organic compound is intercalated into two adjacent M m X n An intercalated product is obtained in which the intercalation occurs between the layers.
[0089] Examples of the organic salt include organic salts containing an organic cation and an anion. Examples of the organic cation include ammonium cations, and examples of the anions include hydroxide ions and chloride ions. Examples of the organic salt include ammonium salts. Specific examples of the organic salt include tetramethylammonium hydroxide (TMAOH), tetraethylammonium hydroxide (TEAOH), and tetrabutylammonium chloride.
[0090] When an organic salt is used as an intercalator, the organic cations constituting the organic salt can be intercalated into the etching and cleaning treatment product. m X n An intercalated product is obtained in which the intercalation occurs between the layers.
[0091] The intercalation treatment may be carried out in a dispersion medium. The specific method of the intercalation treatment is not particularly limited. For example, the etched and washed product may be mixed with a metal compound and stirred or allowed to stand. For example, stirring at room temperature may be used. Examples of the stirring method include a method using a stirring bar such as a stirrer, a method using a stirring blade, a method using a mixer, and a method using a centrifugal device. The stirring time can be set depending on the production scale of the single-layer / few-layer MXene particles, and can be set, for example, between 12 and 24 hours.
[0092] The intercalation treatment may be carried out in the presence of a dispersion medium, such as water, or an organic medium such as N-methylpyrrolidone, N-methylformamide, N,N-dimethylformamide, methanol, ethanol, dimethyl sulfoxide, ethylene glycol, or acetic acid.
[0093] The order of mixing the dispersion medium, the etching-cleaned product, and the metal compound is not particularly limited, but in one embodiment, the dispersion medium and the etching-cleaned product may be mixed together, and then the metal compound may be mixed in. Typically, the etching liquid after the etching treatment may be used as the dispersion medium.
[0094] The intercalation treatment is typically carried out on the etching-cleaned product, but in another embodiment, it may be carried out on the precursor simultaneously with the etching treatment. Specifically, the etching and intercalation treatment include mixing the precursor, an etching solution, and a metal compound containing a metal cation to remove at least a part of the A atoms from the precursor, and intercalating the metal cation into the precursor from which the A atoms have been removed, thereby obtaining an intercalation-treated product. As a result, at least a part of the A atoms are removed from the precursor (MAX), and the M in the precursor is removed. m X n The layer remains, and multiple adjacent M m X n An intercalation product is obtained in which metal cations are intercalated between the layers.
[0095] The etching solution and metal compound used in the etching and intercalation treatment may be the same as the etching solution and metal compound used in step (b), respectively.
[0096] Step (d1) In the step (d), the organic compound is used as an intercalator, so that the obtained precursor particles can coexist with the organic compound. Step (d1) can be carried out in the same manner as the step (d), except that the organic compound is used as an intercalator.
[0097] Step (e): In step (e), the intercalation-treated product is stirred to perform a delamination process for delaminating the intercalation-treated product, thereby obtaining a delamination-treated product. By this stirring, shear stress is applied to the intercalation-treated product, and two adjacent M mX n At least a portion of the space between the layers can be peeled off, and the MXene particles can be divided into a single layer or a few layers.
[0098] The conditions for the delamination treatment are not particularly limited and can be performed by known methods. For example, one method of applying shear stress to the intercalation-treated product is to disperse the intercalation-treated product in a dispersion medium and stir the mixture. Examples of stirring methods include stirring using a mechanical shaker, vortex mixer, homogenizer, ultrasonic treatment, hand shake, automatic shaker, etc. The degree of stirring, such as stirring speed and stirring time, can be adjusted depending on the amount and concentration of the product to be treated. For example, the above-mentioned intercalation-treated slurry can be centrifuged and the supernatant discarded, followed by adding pure water to the remaining precipitate and stirring using, for example, a hand shake or automatic shaker to perform layer separation (delamination). Removal of unexfoliated material can be achieved by centrifuging, discarding the supernatant, and then washing the remaining precipitate with water. For example, (i) pure water can be added to the remaining precipitate after discarding the supernatant, followed by stirring, (ii) centrifuging, and (iii) recovering the supernatant. The steps (i) to (iii) can be repeated at least once, preferably at least twice, but not more than 10 times to obtain a supernatant containing single- and few-layered MXene particles as a delamination-treated product. Alternatively, the supernatant can be centrifuged and discarded to obtain a clay containing single- and few-layered MXene particles as a delamination-treated product.
[0099] The delamination-treated product may be further washed before being subjected to the next step.
[0100] In one embodiment, the cleaning can be performed using a cleaning solution, typically by mixing the delamination-treated product with the cleaning solution. In another embodiment, the cleaning can be performed by acid-treating the delamination-treated product and then mixing the acid-treated product with the cleaning solution. The acid used in the acid treatment can be inorganic acids such as hydrochloric acid, sulfuric acid, nitric acid, phosphoric acid, perchloric acid, hydroiodic acid, hydrobromic acid, or hydrofluoric acid; or organic acids such as acetic acid, citric acid, oxalic acid, benzoic acid, or sorbic acid. The acid concentration in the acid solution can be adjusted appropriately depending on the delamination-treated product. The cleaning with the cleaning solution can be performed sequentially by: step (i) adding the cleaning solution to the treated product or the remaining precipitate obtained in (iii) below and stirring; step (ii) centrifuging the stirred product; and step (iii) discarding the supernatant after centrifugation. Steps (i) to (iii) can be repeated two or more times, for example, up to 15 times. The stirring can be carried out using a handshake, an automatic shaker, a shear mixer, a pot mill, or the like. The acid treatment may be carried out at least once, and if necessary, the operation of mixing with a fresh acid solution (an acid solution not used in the acid treatment) and stirring may be carried out at least twice, for example, at most 10 times. The washing liquid can be the same as the washing liquid in step (c). For example, water may be used as the washing liquid, and pure water is preferred. The mixing can be carried out by the same method as the mixing method in step (c), for example, by stirring, centrifugation, or the like. Stirring methods include stirring methods using a handshake, an automatic shaker, a shear mixer, a pot mill, or the like.
[0101] Step (f): In step (f), the delamination-treated product is mixed with the organic compound. This allows the organic compound to be inserted between the layers. In step (f), mixing the delamination-treated product with the organic compound means that the delamination-treated product and the organic compound are mixed from a state in which they are completely separated to a state in which the organic compound can be present in the delamination-treated product.
[0102] The method for mixing the delamination-treated product and the organic compound is not particularly limited and can be performed by a known method. For example, a method of stirring and dispersing the organic compound and the delamination-treated product can be used. Examples of stirring methods include stirring using a mechanical shaker, a vortex mixer, a homogenizer, ultrasonic treatment, hand shaking, an automatic shaker, etc. The degree of stirring, such as the stirring speed and stirring time, can be adjusted depending on the amount and concentration of the product to be treated. In one embodiment, the content of the delamination-treated product in a mixture containing the delamination-treated product and the organic compound can be, for example, 0.5% by mass or more and 10% by mass or less, or even 1% by mass or more and 5% by mass or less.
[0103] When the delamination-treated product and the organic compound are mixed, another dispersion medium may be present. A specific example of the other dispersion medium is water. The organic compound and the other dispersion medium may be mixed so that the volume ratio of the organic compound to the other dispersion medium (organic compound / other dispersion medium) is, for example, 50 / 50 or more, preferably 55 / 45 or more.
[0104] When the delamination treatment product and the organic compound are mixed, a resin may be further mixed, if necessary, to obtain a conductive film containing two-dimensional particles and a resin.
[0105] Step (g): In step (g), the delamination-treated product is dried and then mixed with the organic compound. By drying the delamination-treated product, moisture contained in the delamination-treated product can be removed. Hereinafter, the material obtained by drying the delamination-treated product is also referred to as the dried product.
[0106] The drying method may be carried out under mild conditions such as natural drying (typically, placing the product in an air atmosphere at room temperature and normal pressure) or air drying (blowing air), or under relatively active conditions such as hot air drying (blowing heated air), heat drying, vacuum drying, and / or freeze drying. In step (g), it is preferable to remove as much water as possible from the delamination-treated product. From this perspective, drying under active conditions is preferred. Furthermore, it is preferable to remove water without heating to a high temperature in step (g). For example, the drying temperature in step (g) may be preferably 190°C or less, more preferably 150°C or less, even 140°C or less, and particularly 120°C or less. In one embodiment, it may be less than 20°C, even 10°C or less. From this perspective, vacuum drying and / or freeze drying are preferred as the drying method, and freeze drying is even more preferred.
[0107] In the drying step, the dispersion medium can be removed from the delamination treatment product, and a dried product in the form of a film is typically obtained.
[0108] The mixing of the dried material with the organic compound can be carried out by any method, for example, by impregnating the dried material with the organic compound or by immersing the dried material in the organic compound.
[0109] In such an embodiment, the amount of the dried product may be, for example, 0.5 parts by mass or more and 10 parts by mass or less, or even 1 part by mass or more and 5 parts by mass or less, relative to 100 parts by mass of the organic compound.
[0110] (Third embodiment: conductive film)
[0111] Hereinafter, a conductive film according to one embodiment of the present disclosure will be described in detail, but the present disclosure is not limited to such an embodiment.
[0112] The conductive film of this embodiment contains the two-dimensional particles and has a conductivity of 2,000 S / cm or more.
[0113] This makes it possible to provide a conductive film with good conductivity stability. While the present disclosure should not be interpreted as being limited to a particular theory, the reason why the conductive film of the present disclosure can achieve this effect is believed to be as follows. That is, the conductive film of the present disclosure contains the above-mentioned two-dimensional particles, and in these two-dimensional particles, a hydrocarbon compound is present on the MXene layer. Therefore, it is believed that oxidation of the MXene layer can be suppressed even in high-temperature environments, and a conductive film with good conductivity stability, particularly in high-temperature environments, can be provided.
[0114] The conductivity of the conductive film is preferably 2,000 S / cm or more, more preferably 5,000 S / cm or more, and even more preferably 7,000 S / cm or more, and may usually be 25,000 S / cm or less.
[0115] When the conductive film is analyzed by X-ray photoelectron spectroscopy (XPS), the ratio of the area of the peaks attributable to divalent and trivalent Ti to the total area of the peaks attributable to Ti2p (hereinafter also referred to as the "Ti2p area ratio") is preferably 80% to 100%, more preferably 85% to 100%, and even more preferably 90% to 100%. The higher the Ti2p area ratio, the more suppressed the oxidation of the MXene layer surface and the more stable the conductivity. As oxidation progresses, the peak area attributable to tetravalent Ti increases and the Ti2p area ratio decreases.
[0116] When the conductive film is heat-treated at 300° C. for 2 hours under normal pressure, the Ti2p area ratio before the heat treatment is A 0 , the Ti2p area ratio after heat treatment is A 1 In this case, A 0 A against 1 Ratio A 1 / A 0 The ratio A is preferably 80% or more and 100% or less, more preferably 85% or more and 100% or less, and even more preferably 90% or more and 100% or less. 1 / A 0 When the temperature is in this range, oxidation of the surface of the MXene layer can be suppressed, and the stability of the electrical conductivity can be good.
[0117] The content of the two-dimensional particles in the conductive film may be preferably 70% by volume or more and 100% by volume or less, more preferably 90% by volume or more and 100% by volume or less, and even more preferably 95% by volume or more and 100% by volume or less.
[0118] The conductive film may further contain a resin in addition to the two-dimensional particles, and the resin may be one or more selected from the group consisting of a thermosetting resin, a thermoplastic resin, and a conductive polymer.
[0119] Examples of the thermosetting resin include epoxy resin, epoxy acrylate resin, phenol novolac type epoxy resin, phenol resin, urethane resin, silicone resin, polyamide resin, polyimide resin, polyamideimide resin, etc. The thermosetting resin may be used alone or in combination of two or more kinds.
[0120] Examples of the thermoplastic resin include polyolefin resins (e.g., polyethylene resins, polypropylene resins), polyvinyl chloride, polystyrene resins, polyvinyl acetate, acrylic resins, polyester resins, polylactic acid, polyurethane resins, polycarbonate resins, polyvinyl acetal resins, polyvinyl butyral resins, fluorine-based resins, liquid crystal polymers, polyacrylic acid, polyether resins, polyphenyl sulfide resins, diallyl phthalate resins, polyvinyl alcohol resins (e.g., cation-modified polyvinyl alcohol), epoxy resins to which no curing agent has been added, and phenoxy resins to which no curing agent has been added. Only one type of thermoplastic resin may be used, or two or more types may be used in combination.
[0121] Examples of the conductive polymer include poly(3,4-ethylenedioxythiophene):polystyrenesulfonic acid (PEDOT:PSS), polyaniline, polypyrrole, and polythiophene. The conductive polymer may be used alone or in combination of two or more.
[0122] As the resin, polyurethane resin, polyacrylic acid, and poly(3,4-ethylenedioxythiophene):polystyrene sulfonic acid (PEDOT:PSS) are preferred.
[0123] The film may further contain other additives.
[0124] The method for producing a conductive film according to this embodiment includes forming a conductive film using the two-dimensional particles, and in one aspect, heating a precursor film containing the precursor particles in the presence of an organic compound at an absolute pressure of less than 1,013 hPa and above the boiling point of the organic compound to obtain a conductive film. This produces hydrocarbon compounds on the MXene layer, suppressing oxidation of the MXene layer and resulting in a conductive film with excellent conductivity stability.
[0125] The pressure during heating is, in absolute terms, less than 1,013 hPa, preferably 1,000 hPa or less, more preferably 50 hPa to 1,000 hPa, and even more preferably 100 hPa to 1,000 hPa. By maintaining the pressure in this range, it is believed that the MXene layer can be maintained and hydrocarbon compounds can be easily produced.
[0126] The heating temperature is equal to or higher than the boiling point of the organic compound, preferably equal to or higher than 200° C., more preferably from 200° C. to 400° C., and even more preferably from 200° C. to 350° C. By maintaining the temperature in this range, it is believed that the layer structure of MXene can be maintained and hydrocarbon compounds can be more easily produced.
[0127] The heating time is preferably 1 hour or more and 30 hours or less, and more preferably 5 hours or more and 20 hours or less.
[0128] Pre-drying may be carried out before the heating. Such pre-drying may be carried out under normal pressure at 80 ° C or less. The pressure during pre-drying may be preferably 900 hPa or more and 1,200 hPa or less as an absolute pressure, and further may be 950 hPa or more and 1,160 hPa or less as an absolute pressure. The temperature during pre-drying may be 10 ° C or less, preferably 10 ° C or more and 80 ° C or less, more preferably 20 ° C or more and 70 ° C or less, and even more preferably 30 ° C or more and 70 ° C or less. The pre-drying time is, for example, 30 minutes to 10 hours, preferably 1 hour to 5 hours.
[0129] The precursor film can be produced by one selected from the following steps (h) and (f1): (h) forming a precursor film using a mixed liquid containing the precursor particles and the organic compound, or (f1) forming a dry film using a dispersion liquid containing the precursor particles, and permeating the dry film with the organic compound.
[0130] Each step will be described below.
[0131] Step (h) The mixed liquid containing the precursor particles and the organic compound may be a mixture of the delamination-treated product obtained by step (f) and the organic compound as is, or a mixed liquid obtained by mixing precursor particles that can be produced by any method with the organic compound may be used.
[0132] In the mixed liquid, the content of the precursor particles can be, for example, 0.5% by mass or more and 10% by mass or less, or even 1% by mass or more and 5% by mass or less, relative to 100% by mass of the total amount of the mixed liquid.
[0133] The mixed solution may contain another dispersion medium in addition to the organic compound. A specific example of the other dispersion medium is water. The organic compound and the other dispersion medium may be mixed so that the volume ratio of the organic compound to the other dispersion medium (organic compound / other dispersion medium) is, for example, 50 / 50 or more, preferably 55 / 45 or more.
[0134] The mixed liquid may further contain the resin as required.
[0135] The precursor film can be formed, for example, by suction filtering the mixed liquid, or by coating the mixed liquid and drying it under normal pressure, once or twice or more times.
[0136] The method for applying the mixed liquid may be, for example, spraying. The spraying method may be, for example, an airless spraying method or an air spraying method, and specific examples thereof include spraying using a nozzle such as a one-fluid nozzle, a two-fluid nozzle, or an airbrush.
[0137] Step (f1) As the dispersion liquid containing the precursor particles, the delamination-treated product obtained by the step (f) may be used as it is, or a dispersion liquid in which precursor particles that can be produced by any method are dispersed in a dispersion medium may be used.
[0138] Examples of the dispersion medium include water; and organic media such as N-methylpyrrolidone, N-methylformamide, N,N-dimethylformamide, methanol, ethanol, dimethyl sulfoxide, ethylene glycol, and acetic acid.
[0139] The content of the precursor particles may be, for example, 0.5% by mass or more and 10% by mass or less, or even 1% by mass or more and 5% by mass or less, relative to 100% by mass of the total amount of the dispersion.
[0140] The formation of the dried film can be carried out by suction filtering the dispersion, or by coating the dispersion and drying it under normal pressure once or twice or more times. The method for coating the dispersion can be a spray coating method. The spray method can be, for example, an airless spray method or an air spray method, and specifically, can be a method of spraying using a nozzle such as a one-fluid nozzle, a two-fluid nozzle, or an airbrush.
[0141] The permeation of the organic compound into the dry film can be typically carried out by immersing the dry film in the organic compound.
[0142] An example of an application of the membrane of this embodiment is an electrode. Such an electrode is not limited to a specific form as long as it includes the conductive membrane. Examples of the electrode include solid electrodes and flexible soft electrodes.
[0143] In the electrode of this embodiment, the film may be exposed to the outside air so as to be in direct contact with the object to be measured, or may be covered with a substrate and / or a protective film or the like.
[0144] When the electrode of this embodiment has a substrate, the film and the substrate may be in direct contact. The material of the substrate is not particularly limited and may be, for example, an inorganic material such as ceramic or glass, or an organic material. Examples of such organic materials include flexible organic materials, specifically thermoplastic polyurethane elastomer (TPU), PET film, polyimide film, etc. Furthermore, the material of the substrate may be a fibrous material such as paper or cloth (e.g., a sheet-like fibrous material).
[0145] The protective layer may be a layer that covers at least a part or all of the film, and preferably a layer that covers at least a part of the film. The protective layer may be made of an organic material, specifically, a resin such as an acrylic resin, a polyester resin, a polyamide resin, a polyimide resin, a polyamideimide resin, a polyolefin resin, a polycarbonate resin, a polyurethane resin, a polystyrene resin, a polyether resin, polylactic acid, or polyvinyl alcohol.
[0146] The electrodes can be used for any suitable application. Examples include counter electrodes and reference electrodes for electrochemical measurements, electrodes for electrochemical capacitors, electrodes for batteries, bioelectrodes, electrodes for sensors, electrodes for antennas, and electrodes for electrical stimulation. They can also be used for applications requiring high conductivity (reducing the decrease in initial conductivity and preventing oxidation), such as electromagnetic shielding (EMI shielding). Details of these applications are described below.
[0147] The electrodes are not particularly limited, and may be, for example, capacitor electrodes, battery electrodes, biosignal sensing electrodes, sensor electrodes, antenna electrodes, electrical stimulation electrodes, etc. By using the above-mentioned membrane, it is possible to obtain large-capacity capacitors and batteries, low-impedance biosignal sensing electrodes, and highly sensitive sensors and antennas even in a smaller volume (volume occupied by the device).
[0148] The capacitor may be an electrochemical capacitor. An electrochemical capacitor is a capacitor that utilizes capacitance generated by a physicochemical reaction between an electrode (electrode active material) and ions (electrolyte ions) in an electrolyte solution, and can be used as a device for storing electrical energy (electrical storage device). The battery may be a chemical battery that can be repeatedly charged and discharged. The battery may be, for example, a lithium-ion battery, a magnesium-ion battery, a lithium-sulfur battery, a sodium-ion battery, or the like, but is not limited to these.
[0149] The biosignal sensing electrode is an electrode for acquiring a biosignal, and may be, for example, an electrode for measuring EEG (electroencephalogram), ECG (electrocardiogram), EMG (electromyogram), or EIT (electrical impedance tomography), but is not limited to these.
[0150] A sensor electrode is an electrode for detecting a target substance, state, abnormality, etc. The sensor may be, for example, a gas sensor, a biosensor (a chemical sensor that utilizes a molecular recognition mechanism of biological origin), etc., but is not limited to these.
[0151] The antenna electrode is an electrode for emitting electromagnetic waves into space and / or receiving electromagnetic waves in space. The antenna formed by the antenna electrode is not particularly limited to an antenna for mobile communication such as a mobile phone (so-called 3G, 4G, or 5G antenna), an antenna for RFID, or an antenna for NFC (Near Field Communication).
[0152] An electrical stimulation electrode is an electrode for applying electrical stimulation to a living body, and such electrical stimulation can be applied to a living body, particularly to biological tissues such as, but not limited to, the spinal cord, brain, nerve tissue, muscle tissue, etc.
[0153] Although the two-dimensional particles, the manufacturing method thereof, and the conductive film according to one embodiment of the present disclosure have been described above in detail, various modifications are possible. Note that the two-dimensional particles and the conductive film according to the present disclosure may be manufactured by a method different from the manufacturing method according to the above embodiment, and that the manufacturing method of the two-dimensional particles and the conductive film according to the present disclosure is not limited to only those that provide the two-dimensional particles and the conductive film according to the above embodiment.
[0154] The present disclosure includes the following: <1> A polymerizable composition comprising one or more layers and a hydrocarbon compound, wherein the layer is represented by the following formula: M m X n (wherein M is at least one kind of Group 3, 4, 5, 6 or 7 metal; X is a carbon atom, a nitrogen atom or a combination thereof; n is 1 or more and 4 or less; and m is greater than n and 5 or less), and a modified or terminated T (T is at least one kind selected from the group consisting of a hydroxyl group, a fluorine atom, a chlorine atom, an iodine atom, an oxygen atom, a chlorine atom, a phosphorus atom and a hydrogen atom) present on the surface of the layer body, and the hydrocarbon compound is present on the layer. <2> The two-dimensional particle according to <1>, wherein the hydrocarbon compound includes a hydrocarbon compound having 3 to 10 carbon atoms. <3> The two-dimensional particle according to <1> or <2>, wherein a content of carbon atoms derived from the hydrocarbon compound is 0.5 mass% or more with respect to 100 mass% of the total amount of the two-dimensional particle. <4> The two-dimensional particle according to any one of <1> to <3>, further comprising one or more metal atoms selected from Li, K, Na, Mg, Mn, Ca, Fe, Zn, Al, and Cu. <5> A conductive film comprising the two-dimensional particle according to any one of <1> to <4>, and having a conductivity of 2,000 S / cm or more. <6> A method for producing two-dimensional particles by heating precursor particles in the presence of an organic compound under conditions of an absolute pressure of less than 1,013 hPa and a temperature equal to or higher than the boiling point of the organic compound, wherein the precursor particles comprise one or more layers, and the layers are represented by the following formula: M m X n(wherein M is at least one Group 3, 4, 5, 6, or 7 metal; X is a carbon atom, a nitrogen atom, or a combination thereof; n is 1 or more and 4 or less; and m is greater than n and 5 or less), and a modified or terminated T (T is at least one selected from the group consisting of a hydroxyl group, a fluorine atom, a chlorine atom, an iodine atom, an oxygen atom, a chlorine atom, a phosphorus atom, and a hydrogen atom) present on the surface of the layer body, wherein the melting point of the organic compound is 20°C or less. <7> A method for producing two-dimensional particles according to <6>, wherein the organic compound includes an organic compound having one or more of a carbonyl group, an ester group, an amide group, a formamide group, a carbamoyl group, a carbonate group, an aldehyde group, an ether group, a sulfonyl group, a sulfinyl group, a hydroxyl group, a cyano group, and a nitro group. <8> A method for producing two-dimensional particles according to <6> or <7>, wherein the organic compound has a relative dielectric constant of 60 or more. <9> The precursor particles are: (a) a compound represented by the following formula: M m AX n (wherein M is at least one metal of Group 3, 4, 5, 6, or 7; X is a carbon atom, a nitrogen atom, or a combination thereof; A is at least one element of Group 12, 13, 14, 15, or 16; n is 1 or more and 4 or less; and m is greater than n and 5 or less); (b) using an etching solution to remove at least some A atoms from the precursor to obtain an etched product; (c) mixing the etched product with an intercalator to obtain an intercalation product; and (d) stirring the intercalation product to obtain a delamination product containing precursor particles.
[0155] The present invention will be explained in more detail with reference to the following examples, but the present invention is not limited to these examples.
[0156] Example 1 Fabrication of Two-Dimensional Particles In Example 1, a conductive film containing two-dimensional particles was fabricated by sequentially carrying out the following steps, as detailed below: (1) preparation of a precursor (MAX), (2) etching of the precursor, (3) washing, (4) intercalation, (5) delamination and washing, (6) mixing with N-methylformamide, and (7) preparation and heating of a precursor film.
[0157] (1) Preparation of Precursor (MAX) TiC powder, Ti powder, and Al powder (all manufactured by Kojundo Chemical Laboratory Co., Ltd.) were mixed in a molar ratio of 2:1:1 in a ball mill containing zirconia balls for 24 hours. The resulting mixed powder was sintered at 1350°C for 2 hours in an Ar atmosphere. The resulting sintered body (block) was then pulverized with an end mill to a maximum size of 40 μm or less. As a result, TiC powder was obtained as MAX particles. 3 AlC 2 particles were obtained.
[0158] (2) Etching of precursor (ACID method) Ti prepared by the above method 3 AlC 2 Using particles (powder), etching was performed under the following etching conditions to remove Ti 3 AlC 2 A solid-liquid mixture (slurry) containing solid components derived from the powder was obtained. (Etching conditions) Precursor: Ti 3 AlC 2 (Sieved through a 45 μm mesh) Etching solution composition: 49% HF 6 mL H 2 O 18 mL HCl (12 M) 36 mL Precursor input amount: 3.0 g Etching container: 100 mL Eye Boy Etching temperature: 35°C Etching time: 24 h Stirrer rotation speed: 400 rpm
[0159] (3) Washing The slurry was divided into two parts and placed in two 50 mL centrifuge tubes, respectively. After centrifuging at 3500 G using a centrifuge, the supernatant was discarded. 40 mL of pure water was added to the remaining precipitate in each centrifuge tube, and the tubes were centrifuged again at 3500 G to separate and remove the supernatant. This procedure was repeated 11 times. After the final centrifugation, the supernatant was discarded, and Ti3 C 2 T x - Water medium clay was obtained.
[0160] (4) Intercalation The above Ti 3 C 2 T s The clay containing Ti and a water medium was stirred at 20°C to 25°C for 12 hours using LiCl as a Li-containing compound under the following conditions to perform Li intercalation. (Li intercalation conditions) 3 C 2 T x - Water medium clay (MXene after washing): solid content 0.75 g LiCl: 0.75 g Pure water: 37.2 g Intercalation container: 100 mL Eye Boy Temperature: 20 ° C or higher and 25 ° C or lower (room temperature) Time: 10 h Stirrer rotation speed: 800 rpm
[0161] (5) Delamination and cleaning 3 C 2 T x (i) 40 mL of pure water was added to the clay, which was then stirred for 15 minutes on a shaker. (ii) The mixture was centrifuged at 3,500 G, and (iii) the supernatant was collected as a solution containing monolayer MXene. These steps (i) to (iii) were repeated four times to obtain a solution containing monolayer MXene. This supernatant was then centrifuged at 4,300 G for two hours using a centrifuge, after which the supernatant was discarded, yielding a clay containing delamination.
[0162] (6) Mixing with N-methylformamide: 55 parts by volume of N-methylformamide and 45 parts by volume of water were mixed to prepare a mixed dispersion medium, and the delamination-treated product and the mixed dispersion medium were mixed so that the content of the delamination-treated product in the mixed mixture after mixing was 1.5% by mass. This mixture was then dispersed for 15 minutes using an ultrasonic cleaner (AS ONE Corporation, AS482) to obtain a slurry containing two-dimensional particles.
[0163] (7) Preparation and heating of precursor film A predetermined amount of the slurry containing the above two-dimensional particles was placed in a 50 mL centrifuge tube, and pure water was added. At this time, the amount of pure water added was adjusted so that the concentration of the delamination-treated material in the mixture was 1.5 mass%. Then, the mixture was stirred with a shaker for 15 minutes to obtain a slurry.
[0164] The slurry was suction filtered to prepare a filtration membrane. A membrane filter (Merck, Durapore, pore size 0.45 μm) was used as the suction filtration filter. The filtration membrane was dried in a vacuum oven at 150° C. for 16 hours to prepare a precursor membrane.
[0165] The obtained precursor film was placed in a vacuum oven and heated at 200° C. for 12 hours under an absolute pressure of 912 hPa (gauge pressure −0.1 MPa) to produce a film.
[0166] Example 2 Preparation of Two-Dimensional Particles In Example 2, a two-dimensional particle-containing composition (MXene-containing composition) was prepared by sequentially carrying out the following steps, as detailed below: (1) preparation of a precursor (MAX), (2) etching of the precursor and Li intercalation, (3) washing with water, (4) intercalation of a high-dielectric-constant dispersion medium (N-methylformamide), and (5) delamination.
[0167] (1) Preparation of Precursor (MAX) VC powder, V powder, and Al powder (all manufactured by Kojundo Chemical Laboratory Co., Ltd.) were mixed in a molar ratio of 3:1:1 in a ball mill containing zirconia balls for 24 hours. The resulting mixed powder was sintered at 1600°C for 2 hours in an Ar atmosphere. The resulting sintered body (block-shaped MAX) was pulverized with an end mill to a maximum size of 40 μm or less. As a result, V was prepared as a precursor (powdered MAX). 4 AlC 3 particles were obtained.
[0168] (2) Precursor etching and Li intercalation V prepared by the above method 4 AlC 3 Etching was performed using particles (powder) under the following etching conditions. 4 AlC 3A solid-liquid mixture (slurry) containing solid components derived from the powder was obtained. (Etching conditions) Precursor: V 4 AlC 3 (Passed through a 45 μm sieve) Etching solution composition: 49% HF 60 mL Metal salt: LiCl 3 g Precursor input amount: 3.0 g Reaction vessel: 100 mL Eye Boy Etching temperature: 50° C. Etching time: 48 hours Stirrer rotation speed: 400 rpm
[0169] (3) Water washing The above slurry was divided into two equal parts and placed in two 50 mL centrifuge tubes. Then, after centrifuging at 3,500 G for 5 minutes using a centrifuge, the supernatant was discarded. Thereafter, (i) 35 mL of pure water was added to the remaining precipitate in each centrifuge tube, (ii) the mixture was stirred by hand shaking, (iii) the mixture was centrifuged at 3,500 G for 5 minutes, and (iv) the supernatant was removed. These steps (i) to (iv) were repeated a total of 11 times. Finally, after centrifuging at 3,500 G for 5 minutes using a centrifuge, the supernatant was discarded and the V 4 C 3 T s - Water medium clay was obtained.
[0170] (4) Intercalation of the dispersion medium by mixing with a high dielectric constant dispersion medium (N-methylformamide) V prepared by the above method 4 C 3 T s The clay was mixed with N-methylformamide (NMF) as a high dielectric constant dispersion medium under the following conditions to perform intercalation of NMF. (Mixing conditions with high dielectric constant dispersion medium (N-methylformamide)) V 4 C 3 T s - Water medium clay (MXene after washing): solid content 0.5 g Dispersion medium: NMF 20 mL Reaction vessel: 100 mL Eye Boy Temperature: 20 to 25°C (room temperature) Stirring time: 11 hours Stirring rotation speed: 700 rpm
[0171] (5) Delamination: The slurry obtained by mixing with the NMF was transferred to a 50 mL centrifuge tube, and 20 mL of NMF was added. The mixture was then centrifuged at 3,500 G for 5 minutes using a centrifuge, and the supernatant was recovered. (i) 35 mL of NMF was then added to the supernatant, (ii) the mixture was stirred on a shaker for 15 minutes, (iii) the mixture was centrifuged at 3,500 G for 5 minutes, and (iv) the supernatant containing the monolayered MXene was recovered. These steps (i) to (iv) were repeated four times to recover the entire supernatant. The resulting supernatant was then centrifuged at 4,300 G for 2 hours using a centrifuge to precipitate the MXene, and the supernatant was discarded. The precipitate was then obtained as a two-dimensional particle-containing composition.
[0172] [Comparative Example 1] [Preparation of Two-Dimensional Particles] In Comparative Example 1, (1) preparation of a precursor (MAX), (2) etching of the precursor, (3) cleaning, (4) intercalation, and (5) delamination and cleaning were performed in the same manner as in Example 1 to obtain a delamination-treated product, and then the following step (7) was performed to prepare two-dimensional particles. A precursor film was prepared and heated in this order to produce a conductive film containing two-dimensional particles. (7) Preparation and Heating of Precursor Film: A predetermined amount of the delamination-treated product was placed in a 50 mL centrifuge tube, and pure water was added. The amount of pure water added was adjusted so that the concentration of the delamination-treated product in the mixture was 1.5% by mass. The mixture was then stirred with a shaker for 15 minutes to obtain a slurry.
[0173] The slurry was suction filtered to prepare a filtration membrane. A membrane filter (Merck, Durapore, pore size 0.45 μm) was used as the suction filtration filter. The filtration membrane was dried in a vacuum oven at 150° C. for 16 hours to prepare a precursor membrane.
[0174] The obtained membrane was placed in a vacuum oven and heated at 200° C. for 12 hours under an absolute pressure of 912 hPa (gauge pressure −0.1 MPa) to produce a membrane.
[0175] [Gas Chromatography-Mass Spectrometry] The two-dimensional particles obtained in the examples and comparative examples were heated to 450°C using a virolyzer ("PY-2020i" manufactured by Frontier Labs) to desorb the gas adsorbed on the surface of the two-dimensional particle layer. Mass analysis of the gas desorbed from the two-dimensional particles was performed using a gas chromatography-mass spectrometer ("7890A / 5975C" manufactured by Agilent Technologies, Inc.).
[0176] [Carbon and Sulfur Analysis] Using a carbon and sulfur analyzer (Horiba, Ltd., "EMIA-920V2 / FA"), the CO and CO generated when the two-dimensional particles obtained in the examples and comparative examples were heated together with combustion improvers (metal W, metal Sn) in an oxygen stream were analyzed. 2 The total content of carbon atoms contained in the two-dimensional particles was calculated by qualitatively and quantitatively analyzing the two-dimensional particles. 3 C 2 O 2 The value obtained by dividing by the formula weight of C2 and multiplying the result by the formula weight of C2 was taken as the content of carbon atoms derived from the layer of the two-dimensional particles. The content of carbon atoms derived from hydrocarbon compounds contained in the two-dimensional particles was calculated by subtracting the content of carbon atoms derived from the layer of the two-dimensional particles from the total content of carbon atoms contained in the two-dimensional particles.
[0177] [X-ray Photoelectron Spectroscopy] X-ray photoelectron spectroscopy was performed on the conductive films obtained in the examples and comparative examples using an X-ray photoelectron spectroscopy analyzer ("PHI Quantes" manufactured by ULVAC-PHI, Inc.) under the following conditions. Next, based on the obtained spectrum, the ratio of the area of the peaks attributable to divalent and trivalent Ti to the total area of the peaks attributable to Ti2p was calculated. [X-ray Photoelectron Spectroscopy Measurement Conditions] X-ray source: Al monochromator Kα (25 W, 15 kV) Analysis range: 100 μmφ Photoelectron take-off angle: 45° relative to the sample surface
[0178] [Measurement of Conductivity] The conductivity of the obtained conductive film was determined. Resistivity (Ω) and thickness (μm) were measured at three locations per sample, and the conductivity (S / cm) was calculated from these measurements. The average of the three resulting conductivities was used. Resistivity was measured by measuring the surface resistance of the film using a simple low resistivity meter (Loresta AX MCP-T370, manufactured by Mitsubishi Chemical Analytical Corporation) using the four-terminal method. Thickness was measured using a micrometer (MDH-25MB, manufactured by Mitutoyo Corporation). Volume resistivity was calculated from the obtained surface resistance and film thickness, and the conductivity was calculated by taking the reciprocal of this value.
[0179] [Heat Treatment] The two-dimensional particles obtained in the examples and comparative examples were subjected to heat treatment at 300° C. for 2 hours under normal pressure in the air.
[0180]
[0181] Examples 1 and 2 are examples of the present disclosure, and it was confirmed that the two-dimensional particles contained a hydrocarbon compound. Furthermore, it was confirmed that the conductivity of a conductive film obtained using such two-dimensional particles was increased before and after heat treatment at 300°C, and in particular, that the decrease in conductivity was suppressed even in a high-temperature environment, and in some cases the conductivity could be increased.
[0182] Comparative Example 1 is an example in which two-dimensional particles and a conductive film were produced without using N-methylformamide, and it was confirmed that the conductivity was easily reduced, particularly in a high-temperature environment.
[0183] 1a, 1b Layer body (M m X n Layer) 3a, 5a, 3b, 5b Modified or terminated T 7a, 7b MXene layer 10, 10a, 10b MXene particle (2D particle of layered material)
Claims
1. A method for preparing a polymerizable composition comprising one or more layers and a hydrocarbon compound, the layers being represented by the following formula: M m X n (wherein M is at least one type of Group 3, 4, 5, 6 or 7 metal; X is a carbon atom, a nitrogen atom or a combination thereof; n is 1 or more and 4 or less; and m is greater than n and 5 or less), and a modification or termination T (T is at least one type selected from the group consisting of a hydroxyl group, a fluorine atom, a chlorine atom, an iodine atom, an oxygen atom, a chlorine atom, a phosphorus atom and a hydrogen atom) present on a surface of the layer body, and the hydrocarbon compound is present on the layer.
2. The two-dimensional particle according to claim 1, wherein the hydrocarbon compound includes a hydrocarbon compound having 3 to 10 carbon atoms.
3. The two-dimensional particle according to claim 1 or 2, wherein the content of carbon atoms derived from the hydrocarbon compound is 0.5 mass% or more in 100 mass% of the total amount of the two-dimensional particle.
4. The two-dimensional particle according to any one of claims 1 to 3, further comprising one or more metal atoms selected from Li, K, Na, Mg, Mn, Ca, Fe, Zn, Al and Cu.
5. A conductive film comprising the two-dimensional particles according to any one of claims 1 to 4 and having a conductivity of 2,000 S / cm or more.
6. Heating the precursor particles in the presence of an organic compound under conditions of an absolute pressure of less than 1,013 hPa and a temperature equal to or higher than the boiling point of the organic compound to obtain two-dimensional particles, the precursor particles comprising one or more layers, the layers being represented by the following formula: M m X n(wherein M is at least one Group 3, 4, 5, 6 or 7 metal; X is a carbon atom, a nitrogen atom or a combination thereof; n is 1 or more and 4 or less; and m is greater than n and 5 or less), and a modification or termination T (T is at least one selected from the group consisting of a hydroxyl group, a fluorine atom, a chlorine atom, an iodine atom, an oxygen atom, a chlorine atom, a phosphorus atom and a hydrogen atom) present on a surface of the layer body, wherein the melting point of the organic compound is 20° C. or less.
7. The method for producing two-dimensional particles according to claim 6, wherein the organic compound includes an organic compound having one or more of a carbonyl group, an ester group, an amide group, a formamide group, a carbamoyl group, a carbonate group, an aldehyde group, an ether group, a sulfonyl group, a sulfinyl group, a hydroxyl group, a cyano group, and a nitro group.
8. The method for producing two-dimensional particles according to claim 6 or 7, wherein the organic compound has a relative dielectric constant of 60 or more.
9. The precursor particles are: (a) a metal complex having the following formula: M m A.X. n (wherein M is at least one metal of Group 3, 4, 5, 6, or 7; X is a carbon atom, a nitrogen atom, or a combination thereof; A is at least one element of Group 12, 13, 14, 15, or 16; n is 1 or more and 4 or less; and m is greater than n and 5 or less); (b) removing at least a part of A atoms from the precursor using an etching solution to obtain an etched product; (c) mixing the etched product with an intercalator to obtain an intercalation product; and (d) stirring the intercalation product to obtain a delamination product containing precursor particles. The method for producing two-dimensional particles according to any one of claims 6 to 8,
Citation Information
Patent Citations
2-dimensional mxene particle surface-modified with functional group containing saturated or unsaturated hydrocarbon, preparation method thereof and use thereof
JP2020093971A
Fuel cell membrane handling equipment
JP2020518982A
2-dimensional mxene surface-modified with catechol derivative, method for preparing the same, and mxene organic ink including the same
US20210269664A1