Porous composite and method for producing porous composite
The porous composite with a dense foam-like network structure and specific material properties addresses the trade-off between pressure loss and collection efficiency in particulate filters, achieving high efficiency and low pressure loss for both gasoline and diesel engines.
Patent Information
- Application Number
- PCT/JP2024/011001
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-29
- Filing Date
- 2024-03-21
- Publication Date
- 2024-10-03
AI Technical Summary
Existing particulate filters face a trade-off between reducing pressure loss and maintaining high collection efficiency, making it challenging to meet stricter regulations for fuel efficiency and emissions control.
A porous composite is developed, comprising a porous sintered base material with a dense foam-like network structure collection layer, where the collection layer has a porosity of 75-95% and an average pore diameter of 0.3-1.5 μm, and is formed using alumina or silicon carbide, deposited on a cordierite base material using a method involving pore-forming materials and pre-firing to achieve high collection efficiency with low pressure loss.
The porous composite achieves high particulate matter collection efficiency while minimizing pressure loss, effectively addressing the trade-off between efficiency and pressure drop, and can be used in both gasoline and diesel engine exhaust systems.
Smart Images

Figure JP2024011001_03102024_PF_FP_ABST
Abstract
Description
Porous composite and method for producing the porous composite
[0001] The present invention relates to a porous composite and a method for manufacturing the same. [Reference to Related Applications] This application claims the benefit of priority from Japanese Patent Application JP2023-53027, filed on March 29, 2023, the entire disclosure of which is incorporated herein by reference.
[0002] Vehicles equipped with diesel or gasoline engines are equipped with filters to capture particulate matter in exhaust gases. One such filter is a honeycomb filter in which, among a plurality of cells in a porous honeycomb substrate, plugging portions are provided at the outlet openings of some of the cells and at the inlet openings of the remaining cells.
[0003] For example, in the honeycomb filter of Japanese Patent Laid-Open No. 2012-200642 (Document 1), a porous trapping layer is provided on the surface inside cells that have plugging portions at the outlet openings. The trapping layer is formed by a plurality of particles that are bonded or entangled with each other, and the plurality of particles includes flat, plate-like particles. The honeycomb filter of Document 1 can suppress an increase in initial pressure loss and an increase in pressure loss when particulate matter accumulates.
[0004] Furthermore, in the honeycomb filter of International Publication No. 2020 / 194681 (Document 2), the arithmetic mean height, which indicates the surface roughness, of the trapping layer provided in a predetermined cell is set to 0.1 μm or more and 12 μm or less, and the average film thickness of the trapping layer is set to 10 μm or more and 40 μm or less, thereby reducing pressure loss and improving the particulate matter collection efficiency.
[0005] As mentioned above, for the porous composites that make up honeycomb filters, technologies have been proposed to improve the collection efficiency of particulate matter and the like while reducing pressure loss in order to improve fuel efficiency. Because there is a trade-off between the two, it is not easy to achieve high collection efficiency while also reducing pressure loss. However, due to stricter regulations in recent years, there is a demand for both reduced pressure loss and improved collection efficiency.
[0006] An object of the present invention is to provide a porous composite having high collection efficiency and low pressure loss.
[0007] Aspect 1 of the present invention is a porous composite comprising a substrate which is a porous sintered body having air permeability, and a collection layer which is a sintered body having air permeability and is provided on the substrate, and which exhibits a dense foam-like network structure in longitudinal cross section.
[0008] According to the first aspect of the present invention, a porous composite having high collection efficiency and low pressure loss can be provided.
[0009] A second aspect of the present invention is the porous composite of the first aspect, wherein the porosity of the trapping layer is 75% or more and 95% or less, and the average pore size of the trapping layer is 0.3 μm or more and 1.5 μm or less.
[0010] A third aspect of the present invention is the porous composite of the first aspect (which may be either the first or second aspect), wherein the average pore size of the substrate is 10 μm or more and 30 μm or less.
[0011] A fourth aspect of the present invention is the porous composite of the first aspect (which may be any one of the first to third aspects), in which the average thickness of the trapping layer is 20 μm or more and 45 μm or less.
[0012] A fifth aspect of the present invention is the porous composite of the first aspect (which may be any one of the first to fourth aspects), in which the collection layer is formed of alumina.
[0013] A sixth aspect of the present invention is the porous composite of the first aspect (which may be any one of the first to fifth aspects), wherein the trapping layer includes silicon carbide and the substrate is cordierite.
[0014] A seventh aspect of the present invention is a particulate filter comprising the porous composite of any one of Aspects 1 to 6, for trapping particulate matter in exhaust gas emitted from a gasoline engine or a diesel engine.
[0015] Aspect 8 of the present invention is a method for manufacturing a porous composite, comprising the steps of: a) drying droplets containing a pore-forming material and material particles smaller than the pore-forming material to generate a collection of intermediate particles in which the material particles are present among densely packed pore-forming material; b) pre-firing the collection of intermediate particles to form a porous intermediate; c) crushing the porous intermediate to obtain porous particles; d) preparing a substrate which is a porous sintered body having air permeability; e) depositing the porous particles on the substrate; and f) firing the porous particles to form a collection layer on the substrate.
[0016] A ninth aspect of the present invention is the method for producing a porous composite according to the eighth aspect, wherein the average particle size of the pore-forming material is 500 nm or more and 10 μm or less, and the specific surface area of the material particles is 150 m 2 / g or more 400m 2 / g or less, or the average particle size is 10 nm or more and 50 nm or less.
[0017] Aspect 10 of the present invention is a method for producing a porous composite according to Aspect 8 (which may be Aspect 8 or 9), wherein the average pore size of the substrate is 10 μm or more and 30 μm or less, and the average particle size of the porous particles is 15 μm or more and 40 μm or less.
[0018] Aspect 11 of the present invention is the method for producing a porous composite according to aspect 10, wherein the porous particles are deposited on the substrate to a size of 25 μm or more and 50 μm or less by the step e).
[0019] A twelfth aspect of the present invention is the method for producing a porous composite according to any one of the eighth to eleventh aspects, wherein the material particles are alumina particles.
[0020] The above and other objects, features, aspects and advantages will become more apparent from the following detailed description of the invention which proceeds with reference to the accompanying drawings.
[0021] 1 is a simplified plan view of a porous composite; FIG. 2 is a cross-sectional view of a portion of the porous composite; FIG. 3 is an SEM image of a longitudinal section of a porous composite provided with a trapping layer; FIG. 4 is an enlarged view of a portion of FIG. 3; FIG. 5 is a simplified view of the structure of FIG. 3; FIG. 6 is an enlarged SEM image of a longitudinal section of a trapping layer of a comparative example; FIG. 7 is an SEM image showing the penetration of a trapping layer into a substrate; FIG. 8 is a diagram showing the flow of manufacturing a porous composite; FIG. 9 is a diagram showing droplets containing material particles and a pore-forming material; FIG. 10 is a diagram showing intermediate particles; FIG. 11 is a diagram showing a porous intermediate; FIG. 12 is a diagram showing the configuration of a dry film-forming apparatus; FIG. 13 is a diagram for explaining the deposition of porous particles on a substrate; and FIG. 14 is a diagram for explaining how the average film thickness is determined.
[0022] Fig. 1 is a simplified plan view of a porous composite 1 according to one embodiment of the present invention. The porous composite 1 is a tubular member that is long in one direction, and Fig. 1 shows one end face of the porous composite 1 in the longitudinal direction. Fig. 2 is a cross-sectional view of a portion of the porous composite 1. Fig. 2 shows a portion of the cross section along the longitudinal direction, and the direction perpendicular to the plane of Fig. 1 corresponds to the left-right direction in Fig. 2. The porous composite 1 is used, for example, as a gasoline particulate filter (GPF) that captures particulate matter (i.e., fine particles) such as soot in exhaust gas emitted from a gasoline engine of an automobile or the like.
[0023] The porous composite 1 includes a substrate 2 that is a porous sintered body, and a trapping layer 3 (see FIG. 2 ) that is also a porous sintered body. In the example shown in FIGS. 1 and 2 , the substrate 2 is a member having a honeycomb structure. The substrate 2 includes a cylindrical outer wall 21 and partition walls 22. The cylindrical outer wall 21 is a cylindrical portion that extends in the longitudinal direction (i.e., the left-right direction in FIG. 2 ). The cross-sectional shape of the cylindrical outer wall 21 perpendicular to the longitudinal direction is, for example, substantially circular. The cross-sectional shape may be other shapes, such as a polygon.
[0024] The partition walls 22 are provided inside the cylindrical outer wall 21 and are lattice-shaped sections that divide the interior into multiple cells. As described below, the multiple cells include multiple first cells 231 and multiple second cells 232. In the following description, when the first cells 231 and the second cells 232 are not distinguished from each other, the first cells 231 and the second cells 232 are simply referred to as "cells 23." Each of the multiple cells 23 is a space extending in the longitudinal direction. The cross-sectional shape of each cell 23 perpendicular to the longitudinal direction is, for example, approximately square. The cross-sectional shape may be other shapes such as polygonal or circular. In principle, the multiple cells 23 have the same cross-sectional shape. The multiple cells 23 may include cells 23 with different cross-sectional shapes. The substrate 2 is a cell structure whose interior is divided into multiple cells 23 by partition walls 22.
[0025] The cylindrical outer wall 21 and the partition walls 22 are each a porous portion. The cylindrical outer wall 21 and the partition walls 22 are formed of a ceramic such as cordierite. The material of the cylindrical outer wall 21 and the partition walls 22 may be a ceramic other than cordierite, or may be a material other than ceramics.
[0026] The longitudinal length of the cylindrical outer wall 21 is, for example, 50 mm or more and 300 mm or less. The outer diameter of the cylindrical outer wall 21 is, for example, 50 mm or more and 300 mm or less. The thickness of the cylindrical outer wall 21 is, for example, 30 μm or more, and preferably 50 μm or more. The thickness of the cylindrical outer wall 21 is, for example, 1000 μm or less, preferably 500 μm or less, and more preferably 350 μm or less. The longitudinal length of the partition wall 22 is approximately the same as that of the cylindrical outer wall 21. The thickness of the partition wall 22 is, for example, 30 μm or more, and preferably 50 μm or more. The thickness of the partition wall 22 is, for example, 1000 μm or less, preferably 500 μm or less, and more preferably 350 μm or less.
[0027] The porosity of the substrate 2 including the cylindrical outer wall 21 and the partition walls 22 is, for example, 20% or more, and preferably 30% or more. The porosity of the substrate 2 is, for example, 80% or less, and preferably 70% or less. The open porosity of the substrate 2 is, for example, 40% or more, and preferably 55% or more. The open porosity of the substrate 2 is, for example, 65% or less. The porosity and open porosity of the substrate 2 can be measured by Archimedes' method.
[0028] The average pore diameter of the substrate 2 (the arithmetic mean value obtained by dividing the sum of the diameters of all pores by the number of pores, or a value equivalent thereto; the same applies hereinafter) is, for example, 10 μm or more, preferably 15 μm or more. The average pore diameter of the substrate 2 is, for example, 30 μm or less, preferably 25 μm or less. The average pore diameter can be measured using a mercury porosimeter. The surface opening ratio of the substrate 2 is, for example, 20% or more, preferably 25% or more. The surface opening ratio of the substrate 2 is, for example, 60% or less, preferably 50% or less. The surface opening ratio is the proportion of the area of the surface of the substrate 2 where pores are open, and can be determined by image analysis of an SEM (scanning electron microscope) image of the surface. The SEM image is taken at, for example, 500x magnification. The image analysis is performed, for example, using image analysis software "Image-Pro ver. 9.3.2" manufactured by Nippon Roper Co., Ltd.
[0029] The cell density of the substrate 2 (i.e., the number of cells 23 per unit area in a cross section perpendicular to the longitudinal direction) is, for example, 10 cells / cm 2 or more, preferably 20 cells / cm 2 More preferably, 30 cells / cm or more. 2 The cell density is, for example, 200 cells / cm 2 and preferably 150 cells / cm or less. 2 1, the size of the cells 23 is drawn larger than in reality, and the number of the cells 23 is drawn smaller than in reality. The size and number of the cells 23 may be variously changed.
[0030] When the porous composite 1 is used as a GPF, one end side of the porous composite 1 in the longitudinal direction (i.e., the left side in FIG. 2 ) serves as an inlet, and the other end side serves as an outlet, and gas such as exhaust gas flows inside the porous composite 1. Furthermore, among the plurality of cells 23 of the porous composite 1, some of the plurality of cells 23 are provided with plugging portions 24 at their inlet-side ends, and the remaining plurality of cells 23 are provided with plugging portions 24 at their outlet-side ends.
[0031] Fig. 1 depicts the inlet side of the porous composite 1. To facilitate understanding of the drawing, the plugging portions 24 on the inlet side are indicated by diagonal lines in Fig. 1. In the example shown in Fig. 1, cells 23 provided with plugging portions 24 on the inlet side and cells 23 not provided with plugging portions 24 on the inlet side (i.e., cells 23 provided with plugging portions 24 on the outlet side) are alternately arranged in the vertical and horizontal directions in Fig. 1.
[0032] The first cell 231 is a cell 23 provided with a plugging portion 24 on the outlet side. The second cell 232 is a cell 23 provided with a plugging portion 24 on the inlet side. In the porous composite 1, a plurality of first cells 231 each having one plugged end in the longitudinal direction and a plurality of second cells 232 each having the other plugged end in the longitudinal direction are arranged alternately.
[0033] The trapping layer 3 is formed on the substrate 2. In the example shown in FIG. 2 , the trapping layer 3 is provided in a plurality of first cells 231 that have plugging portions 24 provided on the outlet side, and covers the inner surfaces of the plurality of first cells 231 (i.e., the surfaces of the partition walls 22). In FIG. 2 , the trapping layer 3 is indicated by a thick dashed line. The trapping layer 3 may also be provided on the inner surfaces of the outlet-side plugging portions 24 in the plurality of first cells 231. On the other hand, the trapping layer 3 is not present in a plurality of second cells 232 that have plugging portions 24 provided on the inlet side. In other words, the inner surfaces of the plurality of second cells 232 are not covered by the trapping layer 3 and are exposed.
[0034] In the porous composite 1 shown in Figures 1 and 2, as indicated by arrow A1 in Figure 2, gas flowing into the porous composite 1 flows into the first cells 231 from the inlets of the first cells 231, whose inlet sides are not sealed, and then moves from the first cells 231 through the porous trapping layer 3 and the partition walls 22 to the second cells 232, whose outlet sides are not sealed. At this time, substances to be trapped (here, particulate matter) in the gas are efficiently trapped in the trapping layer 3. Furthermore, if the trapping layer 3 contains catalyst particles, which will be described later, combustion (i.e., oxidative removal) of the trapped particulate matter is promoted. In the following description, the inner surfaces of the multiple first cells 231 on which the trapping layer 3 is provided will also be referred to as the "trapping surface."
[0035] Figure 3 is an SEM image of a longitudinal section of porous composite 1 provided with trapping layer 3. A "longitudinal section" is a plane perpendicular to the surface of substrate 2, and Figure 3 shows a longitudinal section parallel to the longitudinal direction of cell 23. In Figure 3, the area indicated by reference numeral 2 represents the range of substrate 2, and the gray area indicated by reference numeral 3 represents the range of trapping layer 3. The gray shadows visible above trapping layer 3 are those that were separated from trapping layer 3 during preparation of the observation sample and do not constitute trapping layer 3. Figure 4 is an SEM image showing an enlarged view of the portion indicated by reference numeral 51 of trapping layer 3 in Figure 3. Figure 5 is a simplified view of the longitudinal section structure of Figure 3.
[0036] As shown in Figures 3 and 5, the substrate 2 has large pores 20, and the pores 20 are connected to each other, providing breathability. A trapping layer 3 is formed on the substrate 2. As shown in Figure 4, the trapping layer 3 has a dense, foam-like network structure in a vertical cross section. The network structure is made of alumina (Al 2 O 3) form a three-dimensional network-like structure. The continuous alumina forms a continuous space in which numerous roughly spherical spaces 30 are partially connected. Such spaces can also be considered as spaces within a sponge-like structure. In Figure 5, the numerous spaces 30 are represented by bold circles. Because both the substrate 2 and the trapping layer 3 are breathable, the porous composite 1 is also breathable. The average pore diameter of the trapping layer 3 is smaller than that of the substrate 2. The method for forming the trapping layer 3 will be described later. However, if a trapping layer is formed by simply adhering alumina particles to the substrate 2 and firing it, the network structure shown in Figure 4 is not observed, as shown in Figure 6. Note that Figure 3 corresponds to Example 1, which will be described later, and Figure 6 corresponds to Comparative Example 1.
[0037] As shown in Figures 3 and 5, the trapping layer 3 covers the openings of the pores 20 in the substrate 2 but does not penetrate into the pores 20. Conventionally, to improve the trapping efficiency, it was necessary to make the material particles of the trapping layer smaller. However, in this case, as shown in Figure 7, the material particles of the trapping layer 3 enter the pores 20, significantly increasing pressure loss. If the trapping layer is made thinner to suppress the increase in pressure loss, the trapping efficiency decreases. In contrast, in Figure 3, the trapping layer 3 does not penetrate into the pores 20, and sufficient trapping efficiency is achieved while suppressing the increase in pressure loss.
[0038] Trapping layer 3 may contain catalyst particles to promote the oxidative removal of the trapped materials. The catalyst particles become part of trapping layer 3, for example, by adhering the catalyst particles to trapping layer 3 and baking it. The catalyst particles are typically oxides, and preferably CeO 2 (ceria), lanthanum (La)-cerium (Ce) composite oxide, lanthanum-manganese (Mn)-cerium composite oxide, lanthanum-cobalt (Co)-cerium composite oxide, lanthanum-iron (Fe)-cerium composite oxide, or lanthanum-praseodymium (Pr)-cerium composite oxide. In other words, the particles of the trapping layer 3 are CeO 2 , lanthanum-cerium composite oxide, lanthanum-manganese-cerium composite oxide, lanthanum-cobalt-cerium composite oxide, lanthanum-iron-cerium composite oxide, and lanthanum-praseodymium-cerium composite oxide.
[0039] Lanthanum-cerium composite oxide is an oxide containing La and Ce, and is also expressed as "La-Ce-O". Lanthanum-manganese-cerium composite oxide is an oxide containing La, Mn, and Ce, and is also expressed as "La-Mn-Ce-O". Lanthanum-cobalt-cerium composite oxide is an oxide containing La, Co, and Ce, and is also expressed as "La-Co-Ce-O". Lanthanum-iron-cerium composite oxide is an oxide containing La, Fe, and Ce, and is also expressed as "La-Fe-Ce-O". Lanthanum-praseodymium-cerium composite oxide is an oxide containing La, Pr, and Ce, and is also expressed as "La-Pr-Ce-O".
[0040] The composite oxide particles are produced, for example, by the citric acid method. The composite oxide particles may also be produced by an impregnation method, a complex polymerization method, or the like.
[0041] Next, an example of the production of the porous composite 1 will be described. FIG. 8 is a diagram showing the flow of the production of the porous composite 1. The production process of the porous composite 1 is divided into the production of porous particles (steps S11 to S13) and the formation of the trapping layer 3 (steps S21 to S23). In the production of the porous particles, first, an alumina sol containing alumina particles (or silica (SiO 2 A pore former, for example, polyethylene, is mixed with the colloidal silica containing the intermediate particles, and an aggregate of intermediate particles, i.e., a dry powder, is obtained using a spray dryer (step S11).
[0042] 9A and 9B are schematic diagrams illustrating step S11. As shown in FIG. 9A, minute droplets 40 containing alumina particles 41 (or silica particles; the same applies hereinafter in steps S11 and S12) and particles of a pore-forming material 42 (hereinafter simply referred to as "pore-forming material") in a solvent (e.g., water) are sprayed into hot air by a sprayer, and the droplets 40 are dried. Because the alumina particles 41 are sufficiently smaller than the pore-forming material 42, intermediate particles 44 are generated in which the alumina particles 41 adhere to the periphery of densely packed pore-forming material 42, as shown in FIG. 9B. It is believed that multiple pore-forming materials 42 gather in the intermediate particles 44, with the alumina particles 41 present in the gaps between the multiple pore-forming materials 42 (and even on the surface of the pore-forming material 42). A collection of intermediate particles 44 is obtained by spray drying.
[0043] The material particles for forming the trapping layer 3 are preferably the above-mentioned alumina particles or silica particles. The material particles may be particles other than alumina particles or silica particles, and may be cordierite (2MgO.2Al 2 O 3 5SiO 2 ) particles, mullite (3Al 2 O 3 2SiO 2 ) particles, etc. can be used. The particle size of the material particles is preferably sufficiently smaller than the particle size of the pore-forming material. Specifically, the average particle size of the material particles is preferably 1 / 10 or less and 1 / 1000 or more of the average particle size of the pore-forming material. The average particle size of the pore-forming material is preferably 500 nm or more and 10 μm or less. When the size of the material particles is specified by the specific surface area, the specific surface area is 150 m 2 / g or more, 400m 2 When the size of the material particles is specified by the average particle size, the average particle size is preferably 10 nm or more and 50 nm or less.
[0044] The aggregate of intermediate particles 44 is pre-fired (step S12). That is, the aggregate of intermediate particles 44 is heated, the pore-forming material 42 is removed by combustion, and the alumina particles 41 are bonded to a certain extent, thereby forming a porous intermediate body 45 shown in Fig. 9C. The porous intermediate body 45 is crushed and classified to obtain porous particles of a desired size (step S13).
[0045] Next, a porous sintered body having air permeability is prepared as the substrate 2 (step S21). Various known methods may be used to manufacture the substrate 2. A step of depositing porous particles on the substrate 2 by a dry film formation method is carried out (step S22). Fig. 10 is a diagram showing the configuration of a dry film formation apparatus 8. Fig. 11 is a diagram for explaining how porous particles 46 are deposited on the substrate 2, and schematically shows a portion of a cross section of the substrate 2 along the longitudinal direction.
[0046] 10 includes a first cylindrical portion 81, a second cylindrical portion 82, and a particle supply portion 83. The first cylindrical portion 81 and the second cylindrical portion 82 are both cylindrical members, and the cross-sectional shape perpendicular to the central axis thereof is substantially the same as the cross-sectional shape of the outer surface (the outer surface of the cylindrical outer wall 21) of the substrate 2. As described above, the substrate 2 is a member extending in the longitudinal direction, and one end of the substrate 2 in the longitudinal direction is inserted into the end of the first cylindrical portion 81, and the other end of the substrate 2 is inserted into the end of the second cylindrical portion 82. In the present embodiment, the end of the substrate 2 where the first cells 231 (see FIG. 11 ) (more precisely, the first cells 231 before the formation of the lower layer 31) are open (i.e., the end where the plugging portions 24 are provided on the second cells 232 (more precisely, the second cells 232 before the formation of the lower layer 31)) is inserted into the first cylindrical portion 81, and the end of the substrate 2 where the second cells 232 are open is inserted into the second cylindrical portion 82. The outer surface of the substrate 2 may be in contact with the first cylindrical portion 81 or the second cylindrical portion 82 via an O-ring or the like. Gas and liquid are substantially impermeable between the outer surface of the substrate 2 and the inner surface of the first cylindrical portion 81, and between the outer surface of the substrate 2 and the inner surface of the second cylindrical portion 82.
[0047] A particle supply unit 83 is connected to the end of the first cylindrical portion 81 opposite the substrate 2. The particle supply unit 83 supplies an aerosol in which porous particles are dispersed in a gas into the first cylindrical portion 81. The dispersion medium of the aerosol is, for example, air. The dispersion medium of the aerosol may be a gas other than air. A pressure reduction mechanism (not shown) is connected to the end of the second cylindrical portion 82 opposite the substrate 2, and the pressure inside the second cylindrical portion 82 is reduced. As a result, the aerosol supplied into the first cylindrical portion 81 flows into the substrate 2.
[0048] As shown by arrow A2 in FIG. 11 , the aerosol flows into the first cells 231. The gas contained in the aerosol enters the partition walls 22 through pores opening on the inner surfaces of the first cells 231 and moves to the second cells 232 adjacent to the first cells 231. The gas that moves to the second cells 232 is discharged to the outside of the substrate 2 through the openings of the second cells 232. This causes porous particles 46 to deposit on the inner surface. At this time, the average particle size of the porous particles 46 is preferably equal to or greater than the average pore size of the substrate 2 so that most of the porous particles 46 do not enter the pores on the inner surface. The average pore size of the substrate 2 is preferably 10 μm to 30 μm, and the average particle size of the porous particles 46 is preferably 15 μm to 40 μm. The average particle size is the arithmetic mean value (the arithmetic mean value obtained by dividing the sum of the particle diameters by the number of particles, or a value equivalent thereto; the same applies hereinafter) and is determined from the particle size distribution of the particles obtained by laser diffraction.
[0049] Preferably, the density of the porous particles in the aerosol is 0.2 g / cm 3 1.2g / cm or more 3 The aerosol suction rate is 8.0 L / (min / cm 2 ) or more 15L / (min / cm 2 ) or less ("L" stands for liters). The thickness of the deposited layer of the porous particles is preferably 25 μm or more and 50 μm or less. The thickness of the deposited layer is determined as the difference between the average height position of the surface of the deposited layer measured with a laser three-dimensional shape measuring device and the average height position of the surface of the substrate.
[0050] The substrate 2 on which the porous particles 46 have been deposited is removed from the dry film-forming apparatus 8 and fired (step S23). When the material particles are alumina particles, the heating temperature during firing is preferably 800°C or higher and 1500°C or lower. The heating time during firing is preferably 0.5 hours or higher and 5 hours or lower. When the material particles are silica particles, the heating temperature during firing is preferably 600°C or higher and 1200°C or lower. The heating time during firing is preferably 0.5 hours or higher and 5 hours or lower. By firing, a trapping layer 3 is formed on the substrate 2, and a porous composite 1 is obtained. The average thickness of the trapping layer 3 is preferably 20 μm or higher and 45 μm or lower.
[0051] In step S22, silicon carbide (SiC) particles may be mixed into the aerosol. This can improve the adhesion between the porous particles 46 and the substrate 2 during the firing in step S23. The average particle size of the silicon carbide particles is preferably 0.1 μm or more and 10 μm or less, and the mixed amount is preferably 3 wt % or more and 30 wt % or less with respect to the weight of the porous particles.
[0052] Next, with reference to Tables 1 to 3, Examples 1 to 7 of the porous composite according to the present invention and Comparative Examples 1 and 2 for comparison with the porous composite will be described.
[0053]
[0054]
[0055]
[0056] (Example 1) In the production of porous particles in Example 1, alumina particles were used as inorganic material particles, and commercially available polyethylene particles were used as a pore-forming material. The alumina particles were obtained in the form of a commercially available alumina sol. The specific surface area of the alumina particles in the sol was 300 m 2 / g (catalog value measured with a mercury porosimeter after heat treatment at 500°C for 1 hour), and the average particle size of the polyethylene particles was 1 μm (catalog value). An aggregate of intermediate particles was generated by spray drying in an environment of 80°C, and pre-baked at 600°C for 1 hour to obtain a porous intermediate. The porous intermediate was crushed and classified to obtain a porous intermediate having an average particle size of 20 μm and a specific surface area of 300 m. 2 The specific surface area of the porous particles is a BET specific surface area (the same applies hereinafter).
[0057] Next, a substrate made of cordierite and having a honeycomb filter shape (honeycomb structure) was prepared. The porosity of the substrate was 48%, and the average pore diameter (the arithmetic mean value obtained by dividing the total diameter of all pores by the number of pores, or an equivalent value; the same applies hereinafter) was 12 μm. The porosity was measured by the Archimedes method using pure water as a medium. The average pore diameter was measured using a mercury porosimeter.
[0058] The porous particles were deposited on a cordierite substrate by a dry film-forming method. During deposition, the flow rate was 8.2 L / (min cm 2 ) (unit surface area 1 cm within the first cell 231 of the substrate 2 2 Suction was performed at a rate of 1 minute (suction amount per unit time). At this time, silicon carbide (SiC) powder was mixed with the porous particles. After that, firing was performed at a temperature of 1150°C for 2 hours to form a collection layer.
[0059] In the produced porous composite, the penetration depth of the alumina trapping layer into the pores of the substrate in a longitudinal section, i.e., a cross section of the porous composite taken along a plane perpendicular to the surface of the substrate, was 5 μm, the porosity of the trapping layer was 76%, the average pore diameter of the trapping layer was 0.5 μm, the average pore diameter of the trapping layer was 1.5 μm, and the average film thickness of the trapping layer (i.e., the average layer thickness) was 35 μm. The silicon carbide content of the trapping layer was 5 wt %.
[0060] These measurements were obtained from 1000x SEM (scanning electron microscope) images of a cross section of a porous composite fragment embedded in resin and mirror-polished. Specifically, the "penetration depth of the trapping layer into the pores of the substrate" was determined by drawing a curve that represents the surface of the substrate in the SEM image, determining the straight line that most closely follows this curve using the least squares method or the like, and calculating the average depth to which the trapping layer penetrated into the pores relative to this straight line. The "porosity of the trapping layer" was obtained from the SEM image by image analysis using the above-mentioned Image-Pro. This image analysis is performed, for example, using a method similar to that described in WO 2020 / 194681. Specifically, in the region where the trapping layer is present in the SEM image, the area of the bright region where the bright portion (i.e., the skeletal portion of the trapping layer) appears and the area of the dark region where the dark portion (i.e., the pores of the trapping layer) appears are calculated. The porosity of the trapping layer is then calculated by dividing the total area of the dark regions by the sum of the total area of the bright regions and the total area of the dark regions.
[0061] The "average pore diameter of the trapping layer" was determined by binarizing the SEM image using Image-Pro at a threshold value sufficient to distinguish the network structure from the cross-section of the pores. The outlines of numerous pores were obtained from this image, and the "average pore diameter of the trapping layer" was calculated as the arithmetic mean of the major axes of the ellipses that best fit each outline (the ellipses with the smallest difference area relative to the outline). As shown in Figure 12, the "average film thickness of the trapping layer" was calculated by obtaining a curve 61 that traces the boundary between the surface of the substrate 2 and the trapping layer 3, and a curve 62 that traces the surface of the trapping layer 3, and then dividing the image into six equal parts horizontally. The horizontal direction of the image is the direction along the surface of the substrate 2. It should be noted that the sample does not necessarily need to be embedded in resin for various measurements; observation and measurement are possible even without embedding in resin.
[0062] The methods for obtaining the above-mentioned measurements for the substrate and trapping layer are the same in the following examples and comparative examples unless otherwise specified.
[0063] The collection efficiency of the porous composite in Example 1 was 99.9%, and the rate of increase in initial pressure loss was 55%.
[0064] The filtering efficiency of the porous composite was determined as follows. First, the porous composite was installed as a GPF in the exhaust system of a passenger vehicle equipped with a 2-liter direct-injection gasoline engine, and a vehicle test was conducted using a chassis dynamometer. In this vehicle test, the number of particulate matter particles emitted in the exhaust gas when the vehicle was driven in a European regulation driving mode (RTS95) was measured using a measurement method in accordance with PMP (European regulation particulate measurement protocol). In addition, a similar vehicle test was conducted without a GPF installed in the exhaust system, and the number of particulate matter particles emitted in the exhaust gas was measured using the same measurement method. The number of particulate matter particles emitted without a GPF was defined as the "reference emission number," and the difference between the number of particulate matter particles measured with the porous composite installed and the reference emission number was divided by the reference emission number to obtain the "filtering efficiency (%)."
[0065] To evaluate the initial pressure loss of the porous composite, first, air at room temperature was blown into the porous composite at a pressure of 10 Nm 3 / min to measure the pressure difference across the porous composite (i.e., the pressure difference between the air inlet and outlet sides). The pressure difference across the substrate alone was used as the reference pressure difference, and the rate of increase in the pressure difference across the porous composite relative to the reference pressure difference was used as the rate of increase in initial pressure loss. The rate of increase in initial pressure loss (%) was calculated as (A-B) / B x 100, where A is the pressure difference across the porous composite and B is the reference pressure difference across the substrate. The methods for calculating the collection efficiency and initial pressure loss were the same in the following Examples 2 to 7 and Comparative Examples 1 and 2.
[0066] (Example 2) The conditions for producing porous particles in Example 2 were as follows: the average particle size of the obtained porous particles was 25 μm, and the specific surface area was 300 m 2 This is the same as Example 1 except that the saturation temperature is 100°C / g.
[0067] Regarding the baking of porous particles onto the substrate, the suction exhaust volume during deposition of porous particles onto the substrate was 11.0 L / (min cm 2 ) is the same as in Example 1.
[0068] In the produced porous composite, the penetration depth of the alumina trapping layer into the pores of the substrate in the longitudinal section was 5 μm, the porosity of the trapping layer was 78%, the average pore size of the trapping layer was 0.7 μm, the average pore size of the trapping layer was 1.7 μm, and the average film thickness of the trapping layer was 35 μm. The silicon carbide content of the trapping layer was 10 wt %.
[0069] The collection efficiency of the porous composite in Example 2 was 99.7%, and the rate of increase in initial pressure loss was 53%.
[0070] Example 3 The conditions for producing porous particles and the measurement results of the porous particles in Example 3 are the same as those in Example 2.
[0071] The firing of the porous particles onto the substrate was the same as in Example 2, except that no silicon carbide powder was mixed with the porous particles when they were deposited onto the substrate.
[0072] In the produced porous composite, the penetration depth of the alumina trapping layer into the pores of the substrate in the longitudinal section of the trapping layer was 0 μm, the porosity of the trapping layer was 82%, the average pore diameter of the trapping layer was 0.9 μm, the average pore diameter of the trapping layer was 2.7 μm, the average film thickness of the trapping layer was 40 μm, and the silicon carbide content of the trapping layer was 0 wt %.
[0073] The collection efficiency of the porous composite in Example 3 was 99.2%, and the rate of increase in initial pressure loss was 42%.
[0074] (Example 4) The conditions for producing porous particles in Example 4 were as follows: the average particle size of the obtained porous particles was 30 μm, and the specific surface area was 280 m 2 This is the same as Example 1 except that the saturation temperature is 100°C / g.
[0075] The conditions for baking the porous particles onto the substrate were the same as those in Example 2, except that the baking temperature was 1100°C.
[0076] In the produced porous composite, the penetration depth of the alumina trapping layer into the pores of the substrate in the longitudinal section of the trapping layer was 0 μm, the porosity of the trapping layer was 82%, the average pore diameter of the trapping layer was 0.9 μm, the average pore diameter of the trapping layer was 2.7 μm, and the average film thickness of the trapping layer was 36 μm. The silicon carbide content of the trapping layer was 10 wt %.
[0077] The collection efficiency of the porous composite in Example 4 was 99.3%, and the rate of increase in initial pressure loss was 40%.
[0078] Example 5 The conditions for producing the porous particles and the measurement results of the porous particles in Example 5 are the same as those in Example 4. The conditions for baking the porous particles onto the substrate are also the same as those in Example 4.
[0079] In the produced porous composite, the penetration depth of the alumina trapping layer into the pores of the substrate in the longitudinal cross section was 0 μm, the porosity of the trapping layer was 90%, the average pore size of the trapping layer was 1.1 μm, the average pore size of the trapping layer was 3.0 μm, and the average film thickness of the trapping layer was 36 μm. The silicon carbide content of the trapping layer was 10 wt %.
[0080] The collection efficiency of the porous composite in Example 5 was 98.5%, and the rate of increase in initial pressure loss was 30%.
[0081] (Example 6) The conditions for producing porous particles in Example 6 were as follows: the average particle size of the obtained porous particles was 30 μm, and the specific surface area was 320 m 2 The conditions for baking the porous particles onto the substrate were the same as those in Example 4, except that the baking temperature was 1000°C.
[0082] In the produced porous composite, the penetration depth of the alumina trapping layer into the pores of the substrate in the longitudinal section was 5 μm, the porosity of the trapping layer was 92%, the average pore size of the trapping layer was 1.3 μm, the average pore size of the trapping layer was 4.0 μm, the average film thickness of the trapping layer was 35 μm, and the silicon carbide content of the trapping layer was 15 wt %.
[0083] The collection efficiency of the porous composite in Example 6 was 98.0%, and the rate of increase in initial pressure loss was 29%.
[0084] (Example 7) In the production of porous particles in Example 7, silica particles were used as inorganic material particles, and commercially available polyethylene particles were used as a pore-forming material. The silica particles were obtained in the form of commercially available colloidal silica. The average particle size of the silica particles in the colloidal silica was 15 nm (catalog value, determined, for example, from a TEM (transmission electron microscope) image after drying the colloidal silica), and the average particle size of the polyethylene particles was 3.5 μm (catalog value). An aggregate of intermediate particles was produced by spray drying, and pre-baked at 600°C for 1 hour to obtain a porous intermediate. The porous intermediate was crushed to obtain a porous intermediate with an average particle size of 30 μm and a specific surface area of 80 m. 2 The specific surface area of the porous particles is a BET specific surface area.
[0085] Next, a cordierite substrate similar to that of Example 1 was prepared, and the porous particles were deposited on the substrate by a dry film-forming method. During deposition, the flow rate was 11 L / (min cm 2 ) and suction was performed. At this time, the silicon carbide powder was not mixed with the porous particles. Thereafter, the mixture was fired at a temperature of 1000°C for 1.5 hours to form a collection layer.
[0086] In the produced porous composite, the penetration depth of the silica trapping layer into the pores of the substrate in the longitudinal section of the trapping layer was 0 μm, the porosity of the trapping layer was 82%, the average pore diameter of the trapping layer was 1.0 μm, the average pore diameter of the trapping layer was 3.0 μm, and the average film thickness of the trapping layer was 40 μm. The silicon carbide content of the trapping layer was 0 wt %.
[0087] The collection efficiency of the porous composite in Example 7 was 99.5%, and the rate of increase in initial pressure loss was 40%.
[0088] (Comparative Example 1) In the production of a porous composite according to Comparative Example 1, solid particles of alumina were used instead of the porous particles of Example 1. The material, porosity, and average pore diameter of the substrate were the same as those of Example 1. The average particle diameter of the alumina particles was 0.1 μm (catalog value), and when the alumina particles were deposited on the substrate by the dry film-forming method, a flow rate of 13.7 L / (min cm 2 ) and suction was performed. At this time, the silicon carbide powder was not mixed with the alumina particles. Thereafter, the mixture was fired at a temperature of 1100°C for 1.5 hours to form a collection layer.
[0089] In the produced porous composite, the penetration depth of the alumina trapping layer into the pores of the substrate in the longitudinal section was 20 μm, the porosity of the trapping layer was 86%, the average pore size of the trapping layer was 1.7 μm, the average film thickness of the trapping layer was 14 μm, and the silicon carbide content of the trapping layer was 0 wt %.
[0090] The collection efficiency of the porous composite in Comparative Example 1 was 99.8%, and the rate of increase in initial pressure loss was 100%.
[0091] Comparative Example 2 The porous composite according to Comparative Example 1 was prepared in the same manner as Comparative Example 1, except that silicon carbide powder was mixed with the alumina particles when the alumina particles were deposited on the substrate.
[0092] In the produced porous composite, the penetration depth of the alumina trapping layer into the pores of the substrate in the longitudinal section was 20 μm, the porosity of the trapping layer was 86%, the average pore size of the trapping layer was 0.8 μm, the average pore size of the trapping layer was 2.5 μm, and the average film thickness of the trapping layer was 50 μm. The silicon carbide content of the trapping layer was 10 wt %.
[0093] The porous composite of Comparative Example 2 had a collection efficiency of 99.8% and an increase rate of the initial pressure loss of 95%.
[0094] As is clear from the above examples and comparative examples, the porous composite according to the present invention suppresses an increase in pressure drop by having a trapping layer with a dense, foam-like network structure. When a trapping layer is formed by simply baking alumina particles onto a substrate, as in comparative examples 1 and 2, the trapping layer penetrates into the pores, resulting in a high initial pressure drop. Furthermore, the reduction in initial pressure drop shown in the examples also reduces pressure drop when particulate matter is trapped in the trapping layer.
[0095] In the present invention, the "air permeability" of the porous composite 1 refers to the property of gas flowing from one surface of the porous composite 1 to the other surface via the internal pores when a pressure difference is applied between the two surfaces of the porous composite 1. Naturally, therefore, the substrate 2 and the trapping layer 3 also have air permeability. Both the substrate 2 and the trapping layer 3 are porous sintered bodies. The substrate 2 is not limited to cordierite, and may be, for example, Si-bonded SiC, Cd-bonded SiC, Si 3 N 4 Bonded SiC, silicon carbide, silicon nitride (Si 3 N 4 ), alumina, mullite, etc. From the viewpoint of high heat resistance, trapping layer 3 is preferably made of alumina, but is not limited to alumina and may be made of, for example, the above-mentioned silica, cordierite, silicon carbide, mullite, etc. However, in order for trapping layer 3 to exhibit its function of trapping particulate matter, the average pore diameter of trapping layer 3 is smaller than the average pore diameter of substrate 2.
[0096] The average pore diameter of the substrate 2 is preferably 10 μm or more and 30 μm or less, particularly when the porous composite 1 is used as a particle filter for exhaust gases, etc. This makes it possible to suppress penetration of particles into the pores of the trapping layer 3 while maintaining sufficient breathability. On the other hand, in Examples 1 to 7 above, the porosity of the trapping layer 3 having a mesh structure is 76% or more and 92% or less, and the average pore diameter is 0.5 μm or more and 1.3 μm or less. From these values, in order to maintain breathability and the particulate matter collection efficiency, the porosity of the trapping layer 3 is preferably 75% or more and 95% or less, and the average pore diameter is 0.3 μm or more and 1.5 μm or less, and more preferably, the porosity is 80% or more and 90% or less, and the average pore diameter is 0.8 μm or more and 1.2 μm or less. Note that the "average pore diameter of the trapping layer 3" refers to the arithmetic mean value of the pore diameters of the trapping layer 3 or a value equivalent thereto. The same applies to the substrate 2.
[0097] Furthermore, in order to prevent the trapping layer 3 from penetrating the pores of the substrate 2, the average particle size of the porous particles 46 deposited on the substrate 2 during the formation of the trapping layer 3 is preferably equal to or greater than the average pore size of the substrate 2. However, even if the average particle size of the porous particles 46 is less than the average pore size of the substrate 2, the porous particles 46 do not necessarily penetrate into the pores of the substrate 2, and even if the average particle size of the porous particles 46 is about half the average pore size of the substrate 2, the porous particles 46 are prevented from penetrating into the pores. Therefore, the average particle size of the porous particles 46 needs only to be 15 μm or greater. If the average particle size of the porous particles 46 is too large, large gaps will form between the porous particles 46 during deposition, reducing the uniformity of the trapping layer 3. Therefore, the average particle size of the porous particles 46 is preferably 40 μm or less.
[0098] The penetration depth of the trapping layer 3 into the substrate 2 is preferably 10 μm or less. In order to suppress a decrease in the trapping efficiency while suppressing an increase in pressure loss, the average film thickness of the trapping layer 3 is preferably 20 μm or more and 45 μm or less.
[0099] The trapping layer 3 provided on the substrate 2 exhibits a dense, foam-like network structure in a longitudinal cross section. The "dense, foam-like network structure" means that traces of the pore-forming material 42 that existed densely before the calcination remain, and the continuous spaces connecting the spaces where the pore-forming material 42 existed are formed by a series of thin skeletons. This structure can also be considered a (non-flexible) sponge-like or foam-like structure. Note that the trapping layer 3 "exhibits" a dense, foam-like network structure "in a longitudinal cross section," and the expression "dense, foam-like network structure" is merely used to describe the actual structure.
[0100] In the intermediate particles 44 generated before the porous particles 46 are generated, material particles for forming the trapping layer 3 (alumina particles 41 in the case of FIG. 9B ) are present between densely packed pore-forming materials 42. "Densely packed pore-forming materials" refers to a state in which the distance between multiple pore-forming materials 42 is shorter than the diameter of the pore-forming materials 42, or the pore-forming materials 42 are in contact with each other, and in the intermediate particles 44, material particles are present at least between the pore-forming materials 42. Of course, material particles may also be present in areas other than between the pore-forming materials 42. The collection of intermediate particles 44 before pre-baking refers to intermediate particles 44 deposited in a predetermined position by, for example, spray drying. The collection of intermediate particles 44 may also be further gathered and placed in a mold.
[0101] The term "pre-baking" means baking the intermediate particles 44 at a temperature equal to or lower than the temperature at which the porous particles 46 are baked onto the substrate 2. It is known that baking the intermediate particles 44 at a temperature higher than necessary will deteriorate the network structure.
[0102] The average particle size of the pore-forming material 42 directly affects the density of the mesh structure of the trapping layer 3, and thus influences the collection efficiency and pressure loss. Since the average particle sizes of the pore-forming material in the examples are 1 μm and 3.5 μm, in order to obtain a favorable relationship between collection efficiency and pressure loss, the average particle size of the pore-forming material 42 is preferably 500 nm or more and 10 μm or less. A mixture of pore-forming materials with different average particle sizes may also be used as the pore-forming material 42. The material of the pore-forming material 42 may be, in addition to polyethylene, starch, polymethyl methacrylate resin, phenolic resin, etc. Furthermore, the shape of the pore-forming material 42 is not limited to spherical, and may be granular, fibrous, plate-like, etc.
[0103] On the other hand, with regard to the material particles, the specific surface area of the alumina particles in Examples 1 to 6 was 300 m 2 / g, the preferred range of the specific surface area of the material particles is at least 150 m 2 / g or more 400m 2 Since the average particle size of the silica particles in Example 7 is 15 nm and the average particle size of the material particles only needs to be sufficiently smaller than the average particle size of the pore-forming material, it is considered that the preferable range of the average particle size of the material particles is at least 10 nm or more and 50 nm or less.
[0104] The "deposition" of porous particles 46 on substrate 2 during the formation of trapping layer 3 means that the particles are simply piled up without the use of a binder or the like. To deposit porous particles 46, methods other than the method using the dry film-forming apparatus 8 may be employed. For example, porous particles 46 may be deposited on substrate 2 simply by utilizing gravity or centrifugal force, or deposition may be performed by other physical forces. The amount of deposited porous particles 46 directly affects the average film thickness of trapping layer 3. Considering that the porous particles 46 are pre-baked and therefore do not change volume significantly during baking, it is preferable that the porous particles 46 be deposited on substrate 2 to a thickness of 25 μm to 50 μm.
[0105] It should be noted that the various "preferred" numerical ranges in the above description do not limit the present invention.
[0106] The use of the porous composite 1 is not limited to gasoline particulate filters that capture particulate matter in exhaust gases emitted from gasoline engines. For example, it may be used in diesel particulate filters (DPFs) that capture particulate matter in exhaust gases emitted from diesel engines. It can also be used for other applications for capturing particulate matter in gases. Note that, since capturing particulate matter means separating gases from particulate matter, it can also be used for various applications for separating gases from particulate matter. Furthermore, the characteristic structure of the trapping layer of the present invention has the potential for use in various applications other than capturing and separating particulate matter.
[0107] The structure of the porous composite 1 may be modified in various ways. For example, the plugging portions 24 may be omitted from the substrate 2. Alternatively, the inner surfaces of all the cells 23 may be used as collection surfaces, and the collection layers 3 may be provided. Furthermore, the substrate 2 does not necessarily have a honeycomb structure, and may have other shapes, such as a simple cylindrical or flat plate shape whose interior is not divided by partition walls. The porous composite 1 does not necessarily have to be a single independent component, but may be part of a single component.
[0108] The configurations in the above-described embodiment and each modification may be combined as appropriate as long as they are not mutually contradictory.
[0109] While the invention has been particularly illustrated and described, it should be understood that the foregoing description is illustrative and not restrictive, and that numerous modifications and variations are possible without departing from the scope of the invention.
[0110] REFERENCE SIGNS LIST 1 porous composite 2 substrate 3 collection layer 40 droplet 41 alumina particle (material particle) 42 pore-forming material 44 intermediate particle 45 porous intermediate 46 porous particle S11 to S13, S21 to S23 steps
Claims
1. A porous composite comprising: a substrate which is a porous sintered body having air permeability; and a collection layer which is a sintered body having air permeability and is provided on the substrate, and which exhibits a dense bubble-like mesh structure in longitudinal cross section.
2. A porous composite according to claim 1, wherein the porosity of the collection layer is 75% or more and 95% or less, and the average pore diameter of the collection layer is 0.3 μm or more and 1.5 μm or less.
3. A porous composite according to claim 1, wherein the average pore size of the substrate is 10 μm or more and 30 μm or less.
4. A porous composite according to claim 1, wherein the average thickness of the collection layer is 20 μm or more and 45 μm or less.
5. A porous composite according to claim 1, wherein the collection layer is made of alumina.
6. The porous composite of claim 1, wherein said collection layer comprises silicon carbide, and said substrate is cordierite.
7. A porous composite material according to any one of claims 1 to 6, which is a particulate filter for collecting particulate matter in exhaust gas discharged from a gasoline engine or a diesel engine.
8. A method for producing a porous composite, comprising the steps of: a) drying droplets containing a pore-forming material and material particles smaller than the pore-forming material to generate a collection of intermediate particles in which the material particles are present among densely packed pore-forming materials; b) pre-firing the collection of intermediate particles to form a porous intermediate body; c) crushing the porous intermediate body to obtain porous particles; d) preparing a substrate which is a porous sintered body having air permeability; e) depositing the porous particles on the substrate; and f) firing the porous particles to form a collection layer on the substrate.
9. The method for producing a porous composite according to claim 8, wherein the average particle size of the pore-forming material is 500 nm or more and 10 μm or less, and the specific surface area of the material particles is 150 m2 / g or more 400m 2 / g or less, or a method for producing a porous composite having an average particle size of 10 nm or more and 50 nm or less.
10. A method for producing a porous composite as described in claim 8, wherein the average pore diameter of the substrate is 10 μm or more and 30 μm or less, and the average particle diameter of the porous particles is 15 μm or more and 40 μm or less.
11. A method for producing a porous composite according to claim 10, wherein the porous particles are deposited on the substrate to a thickness of 25 μm or more and 50 μm or less by step e).
12. A method for producing a porous composite according to any one of claims 8 to 11, wherein the material particles are alumina particles.
Citation Information
Patent Citations
Filter for purifying exhaust gas and its manufacture
JP1996332329A
Method for producing calcined powder
JP2006264990A
Porous body having two or more skeleton layers, and method for producing the same
JP2008088461A
Honeycomb filter
JP2020001032A
Honeycomb filter
JP2023002191A