Solder ball

By adding specific elements to the Au-Sn alloy and using a uniform droplet spraying method, the sphericity of solder balls is enhanced, addressing the issues of uneven surfaces and clogging in ball mounters and solder jet devices, and improving the manufacturing process.

WO2024203746A1PCT designated stage expired Publication Date: 2024-10-03NIPPON STEEL CHEM & MATERIAL CO LTD +1
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/011090
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-31
Filing Date
2024-03-21
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Conventional solder balls made of Au-Sn alloys often have uneven surfaces and poor sphericity due to the formation of non-uniform Au-rich phases during cooling, leading to mounting defects and clogging issues in ball mounters and solder jet devices, especially when the diameter is 250 μm or less.

Method used

Incorporating Mg, Al, Si, Ti, V, Cr, Mn, and Ce in the Au-Sn alloy at concentrations between 0.01 ppm and 0.1 ppm by weight to create a uniform eutectic alloy, which suppresses the formation of non-uniform Au-rich phases and enhances sphericity, and using a uniform droplet spraying method for manufacturing.

Benefits of technology

The modified solder balls exhibit increased sphericity of 0.7% or less, reducing mounting defects and clogging, and maintaining good wettability by dissolving surface oxides, thereby improving productivity in ball mounting and solder jet processes.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JPOXMLDOC01-APPB-T000001
    Figure JPOXMLDOC01-APPB-T000001
  • Figure 00000017_0000
    Figure 00000017_0000
  • Figure 00000018_0000
    Figure 00000018_0000
Patent Text Reader

Abstract

Provided is a solder ball capable of having increased sphericity. The solder ball contains 19 to 25 mass% of Sn with Au being the main component of the remainder, and further contains any one additive element from among Mg, Al, Si, Ti, V, Cr, Mn, and Ce. The concentration of the additive element in relation to the overall solder ball is 0.01 to less than 0.1 ppm by weight. A uniform lamellar structure is formed by a first phase (also referred to as an Au-rich phase) mainly composed of Au5Sn and a second phase mainly composed of AuSn, and thereby the occurrence of unevenness and shrinkage cavities in the surface is suppressed and sphericity is increased.
Need to check novelty before this filing date? Find Prior Art

Description

solder ball

[0001] The present invention relates to solder balls.

[0002] BACKGROUND ART Solder pastes and sheet-like brazing filler metals formed from Au—Sn alloys are used as bonding materials for sealing packages that hermetically seal electronic devices such as semiconductor light-emitting devices in which semiconductor light-emitting elements are mounted on circuit boards, SAW (Surface Acoustic Wave) filters, FBAR (Film Bulk Acoustic Resonator) filters, and quartz crystal oscillators, from the viewpoints of high strength, high electrical conductivity, etc.

[0003] Patent Document 1 discloses an Au—Sn-containing alloy paste, which is characterized by mixing an Au—Sn alloy powder having a particle size of 10 μm or less, containing 20 to 25 wt % Sn and the remainder being Au, with 15 to 30 wt % of a flux containing at least an activator.

[0004] US Pat. No. 5,699,499 discloses a method for providing solder bumps for use in flip-chip bonding technology using a solder composed of 80% Au and 20% Sn.

[0005] Patent Document 3 discloses a solder ball containing 19% by mass or more and 25% by mass or less of Sn, with the remainder being mainly composed of Au, and containing one element of Fe, Cr, or Ni, wherein, when Fe is contained, the concentration of Fe is 0.1 ppm by mass or more and 10 ppm by mass or less, when Cr is contained, the concentration of Cr is 0.1 ppm by mass or more and 100 ppm by mass or less, and when Ni is contained, the concentration of Ni is 1 ppm by mass or more and 5000 ppm by mass or less, relative to the entire solder ball.

[0006] When solder balls formed from the Au—Sn alloy are mounted as a bonding material for the sealed package or other semiconductor devices, a large number of solder balls are processed using a ball mounter or a solder jet device (manufactured by PacTech). When mounting solder balls using a ball mounter, it is necessary to position each solder ball in an appropriate position to prevent mounting defects. Furthermore, when mounting solder balls using a solder jet device, it is necessary to process them without causing clogging.

[0007] JP 2014-54653 A JP 5-136152 A International Publication No. 2020 / 217833

[0008] However, if the sphericity of the solder balls is not sufficiently high, poor mounting occurs when a ball mounter is used, or clogging occurs when a solder jet device is used, resulting in reduced productivity. This effect is particularly pronounced when the diameter of the solder balls is 250 μm or less.

[0009] An object of the present invention is to provide a solder ball that can have improved sphericity.

[0010] The solder ball according to the present invention contains 19% by mass or more and 25% by mass or less of Sn, with the remainder being primarily composed of Au, and contains one additive element selected from Mg, Al, Si, Ti, V, Cr, Mn, and Ce, with the concentration of the additive element relative to the entire solder ball being 0.01 ppm by weight or more and less than 0.1 ppm by weight.

[0011] According to the present invention, a uniform eutectic alloy of Au and Sn can be obtained, and the sphericity of the solder ball can be improved.

[0012] FIG. 1 is a cross-sectional view schematically showing a USD manufacturing apparatus used when manufacturing solder balls using the uniform droplet spraying method. FIG. 2A is a plan view showing an example of solder balls arranged in a close-packed manner according to an embodiment. FIG. 2B is a plan view showing an example of solder balls arranged with a distance L according to an embodiment. FIG. 3A is a schematic end view showing a state of a solder ball before melting according to an embodiment. FIG. 3B is a schematic end view showing a state of a solder ball after melting according to an embodiment. FIG. 4A is a perspective view showing an example of solder ball arrangement at a corner according to an embodiment. FIG. 4B is a schematic view showing an example of a joint at a corner according to an embodiment. FIG. 5 is a schematic view showing an example of a linear joint according to an embodiment. FIG. 6 is a partial cross-sectional view schematically showing an LED package manufactured using solder balls according to an embodiment.

[0013] Hereinafter, an embodiment of the present invention will be described in detail with reference to the drawings. Similar components are designated by similar reference numerals, and the description thereof will be omitted as appropriate.

[0014] 1. Embodiment (1) Configuration of Solder Ball The solder ball 34 according to this embodiment is an Au—Sn-based alloy containing 19% by mass or more and 25% by mass or less of Sn, with the remainder being mainly Au, and is formed by adding one of the following additive elements: Mg, Al, Si, Ti, V, Cr, Mn, and Ce. 5 Sn 1 The concentration of the additive element in the entire solder ball 34 is 0.01 ppm by weight or more and less than 0.1 ppm by weight.

[0015] Conventional solder balls made of Au-Sn alloys have the problem of having uneven surfaces and, in some cases, poor appearance due to shrinkage cavities. This is thought to be due to the formation of a non-uniform Au-rich phase near the surface of the solder ball during cooling in the solder ball manufacturing process.

[0016] In the solder ball 34 of this embodiment, trace amounts of Mg, Al, Si, Ti, V, Cr, Mn, and Ce are dispersed in the AuSn, which provides many nucleation sites during solidification and suppresses the generation of non-uniform Au-rich phases during cooling. 5A uniform lamellar structure is formed by a first phase (also called an Au-rich phase) consisting of Sn and a second phase mainly consisting of AuSn. This suppresses the occurrence of surface irregularities and shrinkage cavities, and improves sphericity. The improved sphericity is preferably 0.7% or less. This can prevent mounting defects in ball mounters and clogging in solder jet machines.

[0017] If the concentration of the additive element relative to the entire solder ball 34 is less than 0.01 ppm by weight, the effect of increasing the sphericity of the solder ball is small, which is not preferable. Also, if the concentration of the additive element relative to the entire solder ball 34 is increased to 0.1 ppm by weight or more, the effect of increasing the sphericity is not achieved due to the influence of oxides, and the upper limit is 0.1 ppm by weight.

[0018] The diameter of the solder balls 34 in this embodiment is not limited as long as the effects of the present invention are exhibited, but is preferably 10 μm or more and 500 μm or less. This range allows for the production of solder balls with uniform diameter accuracy. A more preferred diameter range is 20 μm or more and 400 μm or less, and even more preferably 50 μm or more and 300 μm or less. In conventional technology, when the diameter of the solder ball is 500 μm or less, particularly 300 μm or less, poor sphericity of the solder balls can easily cause mounting failures in a ball mounter or clogging in a solder jet device, resulting in reduced productivity. The solder balls 34 in this embodiment have enhanced sphericity, which can prevent mounting failures in a ball mounter or clogging in a solder jet device.

[0019] In the solder ball 34 of this embodiment, when the concentration of the additive element is within the above range, the oxide film on the surface is reliably dissolved when melted, thereby obtaining good wettability. It is believed that the wettability is affected by the oxide film on the solder ball surface, and when the concentration of the additive element is outside the above range, the oxide film becomes difficult to dissolve, which may result in a decrease in wettability.

[0020] (2) Solder Ball Manufacturing Method To achieve uniform diameter accuracy, the solder balls 34 are preferably formed by the uniform droplet spray method (UDS). A manufacturing apparatus for solder balls 34 using the UDS method will be described with reference to FIG. 1 . The USD manufacturing apparatus 31 shown in FIG. 1 includes a nozzle 35 that ejects molten solder 33 downward, a vibration device 37 that vibrates the nozzle 35, a nozzle stand 39 that slidably holds the nozzle 35, and a solder reservoir 41. The nozzle 35 has an outlet 47 below it. The nozzle 35 is connected to the vibration device 37 via a steel connecting rod 49. In the solder reservoir 41, the molten solder 33 is maintained at a temperature a predetermined temperature higher than its melting point. The nozzle 35 includes a nozzle path 51. The tip of the nozzle path 51 is connected to the outlet 47 below the nozzle. The molten solder 33 stored in the solder reservoir 41 passes through the stand path 53 and the nozzle path 51 and flows out from the outlet 47. The USD manufacturing apparatus 31 separates the flowed-out molten solder 33 into droplets 55 by causing the nozzle 35 to vibrate using the vibration device 37 while causing the molten solder 33 to flow out from the outlet 47. With the exception of the above, the manufacturing method for solder balls can be the same as the method described in Patent Document 3. The manufacturing method for solder balls using the USD manufacturing apparatus 31 produces solder balls 34 with uniform droplet sizes and highly accurate spherical diameters.

[0021] (3) Concentration Analysis Method The method for analyzing element concentrations will be described. Element concentrations are analyzed using either ICP-MS or ICP-OES depending on the concentration range. When the concentration range is less than 100 ppm by mass, analysis can be performed using inductively coupled plasma mass spectrometry (ICP-MS). When the concentration range is 100 ppm by mass or more, analysis can be performed using inductively coupled plasma optical emission spectrometry (ICP-OES).

[0022] (Regarding ICP-MS) <Sample pretreatment method> The analytical equipment used is manufactured by Agilent Technologies (equipment model number: Agilent 8800). The pretreatment procedure is as follows: 0.1 g of solder balls are weighed out, 20 ml of aqua regia (composition: a 3:1 mixture of hydrochloric acid and nitric acid) is added, and the mixture is heated to approximately 200°C to dissolve. After cooling, the mixture is transferred to a polypropylene (hereinafter referred to as "PP") measuring flask (volume: 100 mL) and made to volume with ultrapure water. A quartz glass beaker is used as the decomposition vessel to avoid the inclusion of impurities.

[0023] <Analysis Method> The analysis method is the standard addition method. Specifically, 10 mL of the solution is placed in each of several PP measuring flasks (volume: 100 mL). 2 mL of a solution prepared by diluting a single-element standard solution of the target element (Mg, Al, Si, Ti, V, Cr, Mn, Ce) to 100 μg / L is added stepwise to the PP measuring flasks. The analytical values ​​of the target elements are then extrapolated based on the analytical values ​​of the respective solutions, assuming that the added amount is zero. Kanto Chemical reagents are used for the single-element standard solutions.

[0024] <Measurement> In ICP-MS analysis, polyatomic ions generated interfere with the measurement, increasing the background. Therefore, measurements are performed using cool plasma (output: 600 W) to suppress the effects of interfering ions.

[0025] (About ICP-OES) <Sample pretreatment method> The analytical equipment used is a Thermo Fisher Scientific (equipment model: iCAP6500). The pretreatment procedure is as follows: 1.0 g of solder balls are weighed out, and 20 mL of aqua regia (composition: a 3:1 mixture of hydrochloric acid and nitric acid) is added, and the mixture is heated to approximately 200°C to dissolve. After cooling, the mixture is transferred to a borosilicate glass (hereinafter referred to as "glass") measuring flask (volume: 100 mL) and the volume is adjusted to the constant volume with heated and degassed aqua regia.

[0026] <Analysis Method> The analysis method is the standard addition method. Specifically, 10 mL of the solution is placed in each of several glass measuring flasks (volume: 100 mL), and a single-element standard solution (1000 μg / L) of the target analyte element (Sn) is added to the glass measuring flasks in 0.1 mL increments. Based on the analytical values ​​of each solution, the analytical value of the target element is extrapolated assuming that the added amount is zero. A reagent manufactured by Kanto Chemical is used for the single-element standard solution.

[0027] <Measurement> Sn: Measure a wavelength of 226.8 nm using ICP-OES.

[0028] (4) Method for Mounting and Bonding Solder Balls The solder balls 34 of this embodiment can be used as a bonding material for sealing packages that hermetically seal electronic devices such as semiconductor light-emitting devices in which semiconductor light-emitting elements are mounted on a circuit board, SAW filters, FBAR filters, and quartz oscillators, or as a bonding material for other semiconductor devices.

[0029] When the solder balls 34 of this embodiment are mounted on a joining surface as a joining material for the above-mentioned sealed package or other semiconductor devices, they can be mounted using, for example, a ball mounter. The ball mounter may be, for example, that described in Japanese Patent Application Laid-Open No. 2012-256748. The ball mounter includes, for example, a ball array plate with suction holes at the mounting positions of the solder balls 34. After the solder balls 34 are suction-held on the ball array plate, the ball array plate is transported to the joining surface and placed on the joining surface coated with flux. The solder balls 34 are adhered to the joining surface by the adhesive force of the flux. Using the ball mounter, multiple solder balls can be mounted at once.

[0030] When mounting the solder balls 34 of this embodiment as a bonding material for the above-mentioned sealed package or other semiconductor devices, they can be mounted using, for example, a solder jetting device (manufactured by PacTech). The solder jetting device loads the solder balls 34 into microtubes such as capillaries, irradiates them with laser light to melt the solder balls 34, and simultaneously extrudes them with an inert gas or the like to temporarily fix the solder balls 34 to the bonding surface, and then positions and mounts the solder balls 34 on the bonding surface. Using a solder jetting device allows the solder balls 34 to be temporarily fixed directly to the bonding surface without using flux, thereby reducing defects caused by flux, such as the occurrence of voids and bonding defects. Mounting the solder balls 34 using a solder jetting device may also be applied in combination with bumps or the like formed on the bonding surface.

[0031] 2A is a plan view showing an example in which the solder balls 34 according to the embodiment are arranged in a closest packed manner. As shown in FIG. 2A, the solder balls 34 may be arranged in a closest packed manner.

[0032] 2B is a plan view showing an example in which solder balls 34 according to the embodiment are arranged at intervals L. As shown in FIG. 2B, the solder balls 34 may be arranged on the joining surface at intervals L expressed by the following formula (1): L=√(2R 1 3 / 3t) (1)

[0033] 3A is a schematic end view showing an example of the state of the solder ball 34 according to the embodiment before melting, and FIG. 3B is a schematic end view showing an example of the state of the solder ball 34 according to the embodiment after melting. Here, a case will be described in which the solder ball 34 is mounted on the joining surface of the substrate 16, and the solder ball 34 is melted and spread to form the joint 14. Before melting, the spherical diameter R 1 The solder balls 34 are arranged at intervals of L. When the solder balls 34 melt, they spread and their diameters become R. 2 , forming a joint 14 having a thickness t.

[0034] 4A is a perspective view showing an example of the arrangement of solder balls 34 in a corner portion according to an embodiment. In this example, solder balls 34 are mounted on a conductive layer 46 provided on a flange portion 44 of a substrate 36 having a corner portion using a solder jet device, and the solder balls 34 are melted to form joints 14, with the surface of the conductive layer 46 serving as the joint surface.

[0035] 4B is a schematic diagram showing an example of a joint 14 at a corner according to the embodiment. The joint 14 shown in FIG. 4B is formed by aligning a mating surface (not shown) with the joining surface of the substrate 36 carrying the solder balls 34 as shown in FIG. 4A, heating the substrate 36 in this state to melt the solder balls 34, and then cooling the solder balls 34 to solidify them. The joint 14 electrically connects the joining surface of the substrate 36 with the mating surface to be joined to the joining surface. The joint 14 shown in FIG. 4B has a basic joint portion 59 and an extension portion 60.

[0036] 5 is a schematic diagram showing an example of a linear joint according to the embodiment. The extensions may be formed at regular intervals in an area other than the corners, for example, in a linear portion as shown in FIG.

[0037] After the ball bumps 34 are mounted on the bonding surface as described above, the surface to be bonded to is aligned and placed opposite the bonding surface, and the solder balls are heated in this state to melt, and then cooled and solidified to form a bond, electrically connecting the bonding surface and the surface to be bonded to the other surface. The solder ball mounting method and bonding method can be the same as those described in Patent Document 3, except for the above.

[0038] (5) Actions and Effects If an Au-rich phase is precipitated in a solder ball made of an Au-Sn alloy, even if there are no shrinkage cavities, the ball will have a polyhedral shape like a mirror ball, and the sphericity will be low, which will result in poor mounting on a ball mounter or clogging in a solder jet device.

[0039] In the solder ball 34 of this embodiment, one of Mg, Al, Si, Ti, V, Cr, Mn, and Ce is dispersed in the AuSn at 0.01 weight ppm or more and less than 0.1 weight ppm, so that there are many nucleation sites during solidification, and the generation of a non-uniform Au-rich phase during cooling is suppressed, and the Au-rich phase is mainly Au. 5 A uniform lamellar structure is formed by a first phase (also called an Au-rich phase) made of Sn and a second phase mainly made of AuSn. Therefore, the solder ball 34 of this embodiment is a solder ball with a smooth, mirror-finished surface that is free of surface irregularities and shrinkage cavities and has improved sphericity. This can prevent mounting defects in a ball mounter or clogging in a solder jet device.

[0040] Any metal element that is more easily oxidized than Sn can be used as an additive element to the Au—Sn alloy. The same effect can be achieved by adding 0.01 ppm by weight or more but less than 0.1 ppm by weight of any one of Mg, Al, Si, Ti, V, Cr, Mn, and Ce.

[0041] (6) Semiconductor Light-Emitting Device Manufactured Using the Solder Ball of the Present Embodiment The LED (Light Emitting Diode) package 10 shown in FIG. 6 includes a semiconductor light-emitting device 11 as a bonded structure. The semiconductor light-emitting device 11 includes an LED chip 12 as a first structure and a substrate 16 as a second structure bonded to the LED chip 12 via a joint 14 formed of a solder alloy. The LED chip 12 is a light-emitting element having a substrate 20 and a crystal layer 18 including a light-emitting layer formed on the substrate 20. An electrode 22 and an electrode 24 are formed on the surface of the substrate 20 opposite the surface on which the crystal layer 18 is formed. The electrode 22 and the electrode 24 are made of a conductive material such as Au, Ag, Cu, or Al. The LED chip 12 is a flip-chip light-emitting element in which the electrodes 22 and 24 face downward. One of the electrodes 22 and 24 is an n-side electrode, and the other is a p-side electrode. The bonding portion 14 is formed of an Au-Sn alloy containing 19% by mass or more and 25% by mass or less of Sn and having Au as the main component, and contains one additive element selected from Mg, Al, Si, Ti, V, Cr, Mn, and Ce at a concentration of 0.01 ppm by weight or more and less than 0.1 ppm by weight. Except for the above, the bonding portion 14 can have the same configuration as the semiconductor light-emitting device described in Patent Document 3.

[0042] The LED package 10 can be applied to light sources such as automobile headlights that require high brightness.

[0043] The solder ball 34 of this embodiment can be used as a bonding material for the LED package 10, as well as a bonding material for a sealing package that hermetically seals electronic devices such as a semiconductor light-emitting device in which a semiconductor light-emitting element is mounted on a circuit board, a SAW filter, an FBAR filter, and a quartz oscillator, or as a bonding material for other semiconductor devices.

[0044] 2. Examples The present invention will be described in detail below based on the following examples, but these examples are merely examples of the present invention and the present invention is not limited to these examples in any way.

[0045] (Sample) The solder balls shown in Table 1 were produced using the procedure explained in "(2) Manufacturing Method of Solder Balls" above. First, Au, Sn, and additive elements were weighed, and an ingot was produced by high-frequency melting. Since the additive elements are consumed as oxides during granulation, an amount 5 to 10 times the desired component concentration was added. The ingot was placed in a solder reservoir, and N 2 -5% by volume H 2 The solder reservoir was heated to 385°C in an atmosphere, and the frequency of the piezoelectric element was adjusted to 10 to 50 kHz to obtain solder balls of the desired diameter. More than 10,000 solder balls were produced.

[0046] (Evaluation Method) The Sn concentration of the produced solder balls was evaluated using the ICP-OES method, and the concentration of each added element was evaluated using the ICP-MS method, using 1g of each solder ball. The spherical diameter and sphericity (%) were measured using an image processing device based on the coordinate data of the outline of a two-dimensional image of the solder ball taken from directly above. The spherical diameter was determined as the diameter (D1) of a reference circle using the least squares method. The sphericity (%) was calculated by determining the diameter of the circumscribed circle (D2) and the diameter of the inscribed circle (D3), as (D2 - D3) / D1 x 100, and was taken as a simple average of 50 solder balls. The results are shown in Table 1.

[0047]

[0048] (Evaluation Results) Comparative Examples 1 and 5 and Examples 2 to 4 had an Sn concentration of 18 wt% to 26 wt% and an Mg concentration of 0.05 wtppm in the solder balls. When the Sn concentration was 19 wt% to 25 wt%, the sphericity was 0.58 to 0.65%, which was high.

[0049] In Examples 6 to 12, Al, Si, Ti, V, Cr, Mn, and Ce were investigated as additive elements for the solder balls. The concentration of the additive elements in the solder balls measured by ICP-MS was 0.05 ppm by weight, and the spherical diameter was 125 μm. The sphericity was 0.49 to 0.58%, demonstrating high sphericity.

[0050] Comparative Examples 13 and 16 and Examples 14 and 15 were evaluated with a solder ball diameter of 50 μm and an Si concentration of 0 to 0.1 ppm by weight. When the concentration of the Si additive element was 0.01 ppm by weight or more and less than 0.1 ppm by weight, the sphericity was 0.63% and 0.64%, respectively, which were high degrees of sphericity.

[0051] In Examples 17 to 20, the solder balls had an Sn concentration of 25 wt %, a V concentration of 0.08 wt ppm, and a spherical diameter of 10 μm to 500 μm. The sphericity was high, ranging from 0.58 to 0.65%.

[0052] In Examples 21 to 25, the solder balls had an Sn concentration of 19 wt %, a Cr concentration of 0.01 wt ppm to 0.09 wt ppm, and a spherical diameter of 100 μm. The sphericity was high, ranging from 0.52 to 0.64%.

[0053] In Example No. 26, the Sn concentration in the solder ball was 20 wt %, and the Al concentration was 0.04 wt ppm. In Example No. 27, the Sn concentration in the solder ball was 19 wt %, and the Ti concentration was 0.06 wt ppm. In Example No. 28, the Sn concentration in the solder ball was 21 wt %, and the Mn concentration was 0.07 wt ppm, and each sphere diameter was 150 μm. The sphericity was 0.52 to 0.55%, which was high.

[0054] REFERENCE SIGNS LIST 10 LED package 11 Semiconductor light emitting device 12 LED chip 14 Joint portion 16 Substrate 22, 24 Electrodes 26, 28 Electrodes 34 Solder ball 36 Substrate 44 Flange portion 46 Conductive layer 59 Basic joint portion 60 Extension portion 61 Basic joint portion 62 Extension portion

Claims

1. A solder ball containing 19% by mass or more and 25% by mass or less of Sn, with the remainder being primarily Au, and containing one additional element selected from the group consisting of Mg, Al, Si, Ti, V, Cr, Mn, and Ce, and the concentration of the additional element relative to the entire solder ball being 0.01 ppm by weight or more and less than 0.1 ppm by weight.

2. The solder ball according to claim 1, having a spherical diameter of 500 μm or less.

3. The solder ball according to claim 1 or 2, having a sphericity of 0.7% or less.

Citation Information

Patent Citations

  • Manufacture of metallic ultra fine ball

    JP1992262895A

  • Semiconductor device spherical bump

    JP1995283228A

  • Solder ball

    JP2001267730A

  • Au-Sn-BASED SOLDER ALLOY WHERE SURFACE CONDITION IS CONTROLLED AND SEALED OR BONDED ELECTRONIC COMPONENT USING THE SAME

    JP2016112588A

  • Metal nanoparticle dispersion solution for solder paste and manufacturing method therefor, and solder paste and manufacturing method therefor