Protective sheet, and method for manufacturing electronic component
The protective sheet, with its tailored polyvinyl alcohol composition, balances retention during blade dicing and easy removal, addressing the challenge of existing sheets by maintaining the protective layer on electronic components during processing and facilitating efficient post-processing removal.
Patent Information
- Application Number
- PCT/JP2024/011310
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-30
- Filing Date
- 2024-03-22
- Publication Date
- 2024-10-03
AI Technical Summary
Existing protective sheets for electronic components during blade dicing fail to adequately retain the protective layer during the dicing process while also being easily removable post-dicing, lacking a balance between retention and peel-off properties.
A protective sheet with a protective layer that exhibits a specific mass reduction rate of 0-30% in water and 40-100% in a 55% alcohol solution, formed from polyvinyl alcohol with a degree of saponification of 45 or less and an average polymerization degree of 100-3000, ensuring retention during dicing and easy removal afterward.
The protective sheet effectively retains the protective layer during blade dicing, preventing peeling from cooling water, and easily peels off with an organic solvent, ensuring efficient processing of electronic components like semiconductor chips and wafer level packages.
Smart Images

Figure JP2024011310_03102024_PF_FP_ABST
Abstract
Description
Protective sheet and method for manufacturing electronic components CROSS-REFERENCE TO RELATED APPLICATIONS
[0001] This application claims priority from Japanese Patent Application No. 2023-055134, which is incorporated herein by reference.
[0002] The present invention relates to a protective sheet and a method for manufacturing an electronic component. For example, the present invention relates to a protective sheet that is attached to a surface to be protected, such as an electronic component assembly in which a plurality of electronic components are connected, and a method for manufacturing an electronic component using the protective sheet.
[0003] Conventionally, examples of electronic component connections include semiconductor wafers, wafer-level packages, and image sensor packages. Electronic components are obtained by dividing these electronic component connections. Semiconductor chips serving as electronic components are obtained, for example, by dicing a semiconductor wafer serving as an electronic component connection to separate (divide) it into individual semiconductor chips (see, for example, Patent Document 1). The semiconductor wafer described in Patent Document 1 includes a semiconductor wafer body and electrode portions arranged to sandwich the semiconductor wafer body in the thickness direction. In such a semiconductor wafer, circuit-forming surfaces are formed on both sides of the semiconductor wafer body. The circuit-forming surfaces typically include multiple circuits, including elements such as transistors or wiring. The semiconductor wafer includes one or more pairs of electrodes as described above for each circuit on the circuit-forming surface. Dicing such a semiconductor wafer yields multiple semiconductor chips, each including a semiconductor chip body, at least one circuit, and at least two electrode portions.
[0004] The semiconductor chip described in Patent Document 1 obtained as described above is used, for example, by attaching the electrode portion arranged on one surface to the electrode portion of a circuit board and further attaching the electrode portion arranged on the other surface to the electrode portion of another semiconductor chip.
[0005] The wafer-level package as the electronic component assembly includes a circuit board and a plurality of semiconductor packages mounted on one side of the circuit board. The wafer-level package is usually divided into individual semiconductor packages as electronic components by dicing or the like.
[0006] Furthermore, the image sensor package laminate as the electronic component assembly includes, for example, a sensor wafer main body having a plurality of circuits formed on one surface side, and a glass plate having substantially the same dimensions as the sensor wafer main body in a plan view, and arranged so as to cover one surface side of the sensor wafer main body (the surface on which the plurality of circuits are formed) and fixed by an adhesive layer made of adhesive, glass frit, etc. The image sensor package laminate is then singulated (divided) by dicing or the like into individual image sensor packages each including at least one circuit.
[0007] Japanese Patent Application Publication No. 2015-170754
[0008] When an electronic component assembly (e.g., a semiconductor wafer) is diced by blade dicing using a dicing blade (cutting grindstone), heat is generated due to wear of the dicing blade while the dicing blade is cutting the diced object, and cutting debris is generated as the diced object is cut. Therefore, in blade dicing, cooling water is usually sprayed onto the surface of the diced object on the side where the dicing blade enters (hereinafter also referred to as the cutting start surface) to suppress the heat and remove the cutting debris.
[0009] When spraying cooling water, blade dicing may be performed with the start-of-cut surface covered with a protective layer to prevent chips generated during cutting of the dicing object from adhering to the start-of-cut surface of the dicing object. When performing blade dicing in this manner, it is desirable that the protective layer covering the start-of-cut surface not be peeled off by the cooling water, i.e., that the protective layer be sufficiently retained on the start-of-cut surface. On the other hand, after the blade dicing of the dicing object is completed, a liquid other than water, for example, a solution containing an organic solvent such as alcohol, is sprayed onto the protective layer covering the start-of-cut surface to remove the protective layer from the start-of-cut surface. Therefore, after the blade dicing of the dicing object is performed, it is desirable that the protective layer be easily peeled off from the start-of-cut surface.
[0010] However, it cannot be said that sufficient research has yet been conducted into protective sheets having a protective layer that can exhibit sufficient holding power to the dicing object during blade dicing and can also be easily peeled off from the dicing object after the blade dicing.
[0011] Therefore, an object of the present invention is to provide a protective sheet having a protective layer that exhibits sufficient holding power to the dicing object during blade dicing and that can be easily peeled off from the dicing object after the blade dicing. Another object of the present invention is to provide a method for manufacturing electronic components, more specifically, a method for manufacturing electronic components using the above-mentioned protective layer.
[0012] That is, the protective sheet according to the present invention is a protective sheet having a protective layer attached to a surface to be protected of an electronic component having a surface to be protected, or to a surface to be protected of an electronic component assembly in which a plurality of electronic components are connected, and has a mass reduction rate W of the protective layer after immersion in water at 25° C. for 180 seconds. W is 0% by mass or more and 30% by mass or less, and the mass reduction rate W of the protective layer after immersion in an aqueous alcohol solution having an alcohol concentration of 55% by mass at 25°C for 180 seconds is S is 40% by mass or more and 100% by mass or less.
[0013] A method for manufacturing an electronic component according to the present invention is a method for manufacturing an electronic component from an electronic component connected body having a protective layer attached thereto, using a protective sheet having a protective layer attached to at least a part of a surface of the electronic component connected body, the method comprising: attaching the protective layer to an electronic component connected body in which a plurality of electronic components having surfaces to be protected are connected with the surfaces to be protected facing the same direction, so as to protect the surfaces to be protected of the plurality of electronic components; dividing the electronic component connected body with the protective layer attached thereto while washing with water, to obtain the plurality of divided electronic components each having the protective layer attached thereto; and removing the divided protective sheet from each of the surfaces to be protected of the plurality of electronic components, wherein a mass reduction rate W of the protective layer after immersion in water at 25° C. for 180 seconds is W is 0% by mass or more and 30% by mass or less, and the mass reduction rate W of the protective layer after immersion in an aqueous alcohol solution having an alcohol concentration of 55% by mass at 25°C for 180 seconds is S is 40% by mass or more and 100% by mass or less, and in removing the divided protective sheets, a solution containing an organic solvent at a concentration of 55% by mass or more is brought into contact with the divided protective layers to dissolve at least a portion of the protective layers, and the divided protective sheets are removed from the plurality of electronic components.
[0014] 1 is a schematic cross-sectional view showing the configuration of a wafer-level package; FIG. 2 is a schematic cross-sectional view showing the configuration of an image sensor package; FIG. 3 is a schematic cross-sectional view showing the configuration of a laminate for an image sensor package; FIG. 4 is a schematic view showing an example of a semiconductor wafer having electrode portions on both sides; FIG. 5 is a schematic cross-sectional view showing the configuration of a protective sheet according to one embodiment of the present invention; FIG. 6 is a cross-sectional view showing an example of a state in which a protective layer of a protective sheet is bonded in a method for manufacturing a TSV type semiconductor chip; FIG. 7 is a cross-sectional view showing an example of a state in which a semiconductor wafer is divided in a method for manufacturing a TSV type semiconductor chip; FIG. 8 is a cross-sectional view showing an example of a state in which a protective layer of a protective sheet is removed in a method for manufacturing a TSV type semiconductor chip; FIG. 9 is a schematic cross-sectional view showing an example of a state in which a semiconductor wafer is ground; FIG. 10 is a schematic cross-sectional view showing an example of a semiconductor wafer after grinding; FIG. 11 is a schematic cross-sectional view showing the configuration of a protective sheet according to another embodiment of the present invention.
[0015] An embodiment of the present invention will be described below.
[0016] [Protective Sheet] The protective sheet according to this embodiment includes a protective layer that is attached to a surface to be protected of an electronic component having a surface to be protected, or to a surface to be protected of an electronic component assembly in which a plurality of electronic components are connected. In the protective sheet according to this embodiment, the mass loss rate W of the protective layer after immersion in water at 25°C for 180 seconds relative to the mass of the protective layer before immersion in water at 25°C is W In the protective sheet according to this embodiment, the mass reduction rate W of the protective layer after immersion in an aqueous alcohol solution at 25°C for 180 seconds relative to the mass of the protective layer before immersion in the aqueous alcohol solution at 25°C having an alcohol concentration of 55% by mass is S The alcohol concentration is 40% by mass or more and 100% by mass or less. In the following description, an alcohol aqueous solution having an alcohol concentration of 55% by mass may also be simply referred to as a 55% alcohol aqueous solution.
[0017] The inventors of the present invention have conducted extensive research and have found that in a protective sheet having a protective layer to be attached to the surface of an electronic component to be protected or the surface of an electronic component assembly to be protected, the mass loss rate W after immersing the protective layer in water at 25° C. for 180 seconds is Wis in a specific range, and the mass loss rate W after immersing the protective layer in the alcohol aqueous solution at 25°C for 180 seconds is S The present inventors have found that the above-mentioned problems can be solved by setting the value of the total weight of the polymer in a specific range, and have arrived at the present invention.
[0018] The mass reduction rate W of the protective layer W is a value determined by immersing the protective layer in water at 25°C stirred at a stirring speed of 1000 rpm for a predetermined period of time. S is a value determined by immersing the protective layer for a predetermined period of time in a 55% aqueous alcohol solution at 25° C. and stirred at a stirring speed of 1000 rpm.
[0019] Specifically, the mass reduction rate W of the protective layer after immersion in water at 25°C for 180 seconds relative to the mass of the protective layer before immersion in water at 25°C is W can be determined by the following procedure: (1) A protective layer is formed on a film (e.g., a release liner) to a thickness of 160 μm. The 160 μm protective layer is formed, for example, by stacking four 40 μm protective layers in the thickness direction. (2) The 160 μm thick protective layer is punched out to a diameter of 9 mm to prepare a cylindrical test piece (hereinafter referred to as a cylindrical test piece) with a diameter of 9 mm and a thickness (height) of 160 μm. Then, the cylindrical test piece is peeled off from the film. (3) The mass W of the cylindrical test piece is determined by the following procedure: (1) A protective layer is formed on a film (e.g., a release liner) to a thickness of 160 μm. The ... formed on a film (e.g., a release liner) to a thickness of 160 μm. The protective layer is formed on a film (e.g., a release liner) to a thickness of 160 μm. The protective layer is formed on a film (e.g., a 0 (4) A wire mesh (100 mesh) is prepared by bending a flat wire mesh at a right angle. This wire mesh has a horizontal portion that extends horizontally and a vertical portion that extends upward from one end of the horizontal portion. The cylindrical test specimen is placed on the top surface of the horizontal portion. With the cylindrical test specimen placed on the wire mesh, it is immersed in 25°C water in a beaker for 180 seconds. The wire mesh is formed so that the upper end of the vertical portion is hooked onto the upper end of the side wall of the beaker. The 25°C water is stirred at a stirring speed of 1000 rpm using a stirrer. (5) The cylindrical test specimen is removed from the 25°C water in the beaker, lightly dried using a dryer (pre-drying), and then subjected to main drying at 110°C for 2 minutes. The mass W of the cylindrical test specimen after main drying is then measured. 1(6) [(W 0 -W 1 ) / W 0 (7) The above (1) to (6) are carried out for three cylindrical specimens, and the calculated values obtained for each cylindrical specimen are arithmetically averaged to obtain the mass reduction rate W W Find the value of .
[0020] The mass loss rate W of the protective layer after immersion in an aqueous alcohol solution having an alcohol concentration of 55% by mass at 25°C for 180 seconds S is the mass reduction rate W except that the liquid in the beaker is replaced from 25°C water to the alcohol aqueous solution (alcohol concentration 55% by mass) at 25°C. W It should be noted that the mass loss rate W of the protective layer after immersion in an aqueous alcohol solution having an alcohol concentration of 20% by mass at 25° C. for 180 seconds, which is described in the Examples section, can be calculated in the same manner as above. S’ is the mass reduction rate W except that the liquid placed in the beaker is the alcohol aqueous solution (alcohol concentration 20 mass%) at 25°C. W can be found in the same way.
[0021] Here, the mass reduction rate W W The closer to 0 mass %, the less soluble the protective layer is in water at 25°C. W The closer to 100% by mass the protective layer is to water at 25°C. S is closer to 100% by mass, the more easily the protective layer dissolves in an aqueous alcohol solution at 25°C having an alcohol concentration of 55% by mass. W is in the range of 0% by mass or more and 30% by mass or less, the protective layer of the protective sheet can be said to be relatively insoluble in water. S is in the range of 40% by mass or more and 100% by mass or less, the protective layer of the protective sheet can be said to be relatively soluble in an organic solvent such as alcohol. W is within the above numerical range, and the mass reduction rate W Sis within the above-mentioned numerical range. Therefore, when a blade dicing process is performed with the protective layer attached to the surface of an electronic component assembly such as a semiconductor wafer, which is the object to be diced, the protective layer is unlikely to peel off even when cooling water is sprayed onto the protective layer. Furthermore, after multiple electronic components (such as semiconductor chips) are obtained by blade dicing, the protective layer is likely to peel off when an organic solvent is sprayed onto it. In other words, the protective layer of the protective sheet according to this embodiment can exhibit sufficient retention to the object to be diced during blade dicing, and is easily peeled off from the object to be diced after the blade dicing. The temperature of the cooling water used during blade dicing is usually 25°C or lower.
[0022] Examples of the electronic component include a semiconductor chip or a circuit board, etc. Examples of the electronic component assembly include a semiconductor wafer for obtaining the semiconductor chip, or a linked circuit board formed by linking a plurality of the circuit boards.
[0023] The electronic component assembly may also be a pseudo wafer including a support substrate and a package formed by collectively sealing a plurality of semiconductor chips with resin while the plurality of semiconductor chips are arranged on the support substrate. Such a pseudo wafer may be the package removed from the support substrate. A rewiring layer may be formed on at least one surface of the pseudo wafer. In such a case, the protective layer of the protective sheet may be used to protect the rewiring layer. Note that divided pseudo wafers obtained by dividing the pseudo wafer into units each including at least one semiconductor chip are classified as electronic components.
[0024] An example of the electronic component assembly is a wafer-level package (WLP) as shown in FIG. 1 . As shown in FIG. 1 , the wafer-level package 100 includes a circuit board 110 and a plurality of semiconductor packages 120 mounted on the circuit board 110. In the wafer-level package 100, a plurality of semiconductor chips are each resin-encapsulated on the circuit board 110. In the wafer-level package 100, the surfaces of the plurality of semiconductor packages 120 (the surfaces opposite to the surfaces mounted on the circuit board 110) may be configured with one surface of a glass piece 120a. That is, in the wafer-level package 100, each of the plurality of semiconductor packages 120 may include a glass piece 120a on its surface side (the surface opposite to the surface mounted on the circuit board 110). When the wafer-level package 100 is configured in this manner, the protective layer of the protective sheet is used to protect one surface of each of the glass pieces 120a of the plurality of semiconductor packages 120. The wafer-level package 100 is divided (cut) into individual semiconductor packages by dicing or the like along a cutting line L as shown in Fig. 1. The individual semiconductor packages cut from the wafer-level package 100 are classified as electronic components.
[0025] An example of the electronic component is an image sensor package 200 as shown in FIG. 2A . The image sensor package 200 includes a sensor chip body 210 having a circuit formed on one surface thereof, and a glass piece 230 (cover glass) laminated on one surface (the surface on which the circuit is formed) of the sensor chip body 210 via an adhesive layer 220 made of an adhesive, glass frit, or the like. The image sensor package 200 is used, for example, as an imaging element for a camera or the like. In the image sensor package 200 configured as described above, the protective layer of the protective sheet is used to protect the surface (the surface opposite to the side closer to the sensor chip body 210) of the glass piece 230 laminated on the sensor chip body 210. Note that the image sensor package 200 is typically obtained by dividing an image sensor package laminate 200′ as shown in FIG. 2B into a plurality of image sensor packages 200. Specifically, the image sensor package laminate 200′ includes a sensor wafer main body 210′ having a plurality of circuits formed on one surface side thereof, and a glass plate 230′ having substantially the same dimensions as the sensor wafer main body 210′ in a plan view and laminated on one surface (the surface on which the plurality of circuits are formed) of the sensor wafer main body 210′ via an adhesive layer 220′ made of an adhesive, glass frit, or the like. The image sensor package laminate 200′ is divided by a dicing process or the like to separate into image sensor packages 200 each including at least one circuit. Specifically, the image sensor package laminate 200′ is divided along a cleavage line L′ as shown in FIG. 2B to separate into individual image sensor packages 200. As described above, the image sensor package laminate 200′ is classified as an electronic component assembly because it is composed of a plurality of image sensor packages 200 connected together.
[0026] The semiconductor chip typically has a semiconductor chip body and electrode portions arranged on at least one side of the semiconductor chip body. These electrode portions are electrically connected to, for example, electrode portions of another component. In a semiconductor chip, a circuit is formed on at least one side of the semiconductor chip body, and the surface on which the circuit is formed is the circuit formation surface. Examples of the other component include a circuit board or another semiconductor chip configured similarly to the semiconductor chip. Examples of the semiconductor chip include a TSV (Through Silicon Via) type semiconductor chip. Such a TSV type semiconductor chip includes electrode portions arranged on both sides of the semiconductor chip body so as to sandwich the semiconductor chip body in the thickness direction, and electrically connected to other components, and a conductive portion penetrating the semiconductor chip body in the thickness direction to electrically connect the electrode portions facing each other in the thickness direction. In a TSV type semiconductor chip, the circuit formation surface may be formed on only one side, or on both sides.
[0027] The semiconductor chip may also be a sensor chip in which the circuit includes a sensor element (for example, a light receiving element or a vibration element) as an element. Examples of the sensor chip include a CMOS (Complementary Metal-Oxide Semiconductor) chip and a MEMS (Micro Electro Mechanical Systems) chip.
[0028] The above-described TSV type semiconductor chip can be obtained, for example, by dividing a semiconductor wafer that is an electronic component assembly shown in Fig. 3 by dicing or the like. The semiconductor wafer 20 shown in Fig. 3 includes a semiconductor wafer main body 20a, electrode portions 20b and 20c that are arranged on both sides of the semiconductor wafer main body 20a so as to sandwich the semiconductor wafer main body 20a in the thickness direction and are electrically connected to other members, and a conductive portion 20d that penetrates the semiconductor wafer main body 20a in the thickness direction and connects the two electrode portions 20b and 20c to each other.
[0029] In the example semiconductor wafer 20 shown in FIG. 3 , the conductive portion 20d is composed of a solid conductor. On the other hand, the conductive portion 20d may be composed of, for example, a hollow conductor. That is, the conductive portion 20d is only required to be configured to electrically connect the two electrode portions 20b and 20c to each other. Furthermore, in the semiconductor wafer 20 shown in FIG. 3 , insulating layers 20e are formed on both sides of the semiconductor wafer body 20a to prevent electrical conduction between adjacent electrode portions in the surface direction (specifically, between adjacent electrode portions 20b or between adjacent electrode portions 20c). In the semiconductor wafer 20 shown in FIG. 3 , on one side, the outermost surface of the insulating layer 20e is flush with the outermost surface of each electrode portion 20b. Similarly, on the other side, the outermost surface of the insulating layer 20e is flush with the outermost surface of each electrode portion 20c. 3, each electrode portion 20b is arranged so that only the outermost surface is exposed. Alternatively, each electrode portion 20b may be arranged so that the entire surface is covered by the insulating layer 20e on each side of the semiconductor wafer 20. That is, each electrode portion 20b may be embedded in the insulating layer 20e.
[0030] The two electrode portions 20b, 20c and the conductive portion 20d may be integrated with each other or may be separate. For example, the electrode portions 20b, 20c, and the conductive portion 20d are inserted, in an integrated state, into conductive portion through-holes formed to penetrate the semiconductor wafer main body 20a. Examples of materials constituting the electrode portions 20b, 20c, and the conductive portion 20d include copper and aluminum. The electrode portions 20b, 20c may have a thickness of 5 nm to 10 μm from the outermost surface of the semiconductor wafer main body 20a. The length of the conductive portion 20d may be approximately the same as the length of the conductive portion through-hole (i.e., the thickness of the semiconductor wafer main body 20a). The dimensions and shape of the conductive portion 20d are selected appropriately depending on the shape of the conductive portion through-hole. For example, when the shape of the conductive portion through hole is cylindrical, the dimensions and shape of the conductive portion 20d are selected to be a cylinder having an outer diameter slightly smaller than that of the conductive portion through hole.
[0031] The insulating layer 20e is made of, for example, silicon dioxide (SiO 2 The insulating layer 20e is made of a material such as silicon nitride (SiN). The insulating layer 20e can be formed on both sides of the semiconductor wafer main body 20a by a CVD method or the like. The thickness of the insulating layer 20e is selected appropriately depending on the thickness of the electrodes 20b and 20c.
[0032] As shown in Figure 4, the protective sheet 10 according to this embodiment includes a protective layer 10a and may further include a first release liner 10b overlying one surface of the protective layer 10a. The protective sheet 10 may further include a second release liner 10c overlying the other surface of the protective layer 10a (the surface opposite the one surface). That is, the protective sheet 10 according to this embodiment may be configured such that the protective layer 10a is sandwiched between two release liners (the first release liner 10b and the second release liner 10c) on both sides. The protective sheet 10 according to this embodiment is used by bonding the protective layer 10a to the surface to be protected of an electronic component having a surface to be protected, or to the surface to be protected of an electronic component assembly in which a plurality of such electronic components are connected.
[0033] The protective sheet 10 can be produced, for example, as follows. Specifically, a solvent-containing protective layer-forming composition is applied to the first release liner 10b using an applicator to a predetermined thickness (e.g., 40 μm). The solvent is evaporated by drying at a predetermined temperature for a predetermined time (e.g., 115°C for 90 seconds), forming a protective layer 10a on the first release liner 10b. Thereafter, a second release liner 10c is superimposed on the surface of the protective layer 10a opposite the surface that overlaps with the first release liner 10b. Examples of the protective layer-forming composition include compositions containing polyvinyl alcohol (PVA). The polyvinyl alcohol-containing composition may be prepared by suspending and dissolving polyvinyl alcohol in water.
[0034] 4, protective sheet 10 is configured by sandwiching protective layer 10a between two release liners (first release liner 10b and second release liner 10c) from both sides of protective layer 10a, but the configuration of protective sheet 10 is not limited to this. For example, protective sheet 10 may be configured with only protective layer 10a, or a release liner may be superimposed on only one side of protective layer 10a. In other words, protective sheet 10 is required to include at least protective layer 10a.
[0035] The protective layer 10a of the protective sheet 10 is preferably composed of a protective layer-forming composition containing polyvinyl alcohol. As described above, the protective layer-forming composition contains a solvent. The solvent is preferably water. When the protective layer-forming composition contains water as the solvent, it preferably contains 5 to 80 parts by weight of polyvinyl alcohol per 100 parts by weight of water, more preferably 10 to 70 parts by weight, and even more preferably 15 to 60 parts by weight. In the protective layer-forming composition, the polyvinyl alcohol is preferably dissolved in a solvent (e.g., water). For example, the protective layer-forming composition can be prepared by heat treatment at a temperature of 20°C to 90°C, dissolving the polyvinyl alcohol dispersed in the solvent in the solvent (e.g., water). The heat treatment temperature is appropriately selected depending on the saponification degree of the polyvinyl alcohol. Specifically, polyvinyl alcohol with a low saponification degree (e.g., a saponification degree of 45 or less) is difficult to dissolve in water at room temperature (25±2°C). In such cases, a higher treatment temperature is preferable. On the other hand, polyvinyl alcohol with a high degree of saponification (for example, a degree of saponification of 60 or more) is easily soluble in water at room temperature (25±2°C). In such cases, the treatment temperature does not need to be high.
[0036] The viscosity of the protective layer-forming composition at 25°C is preferably 0.03 Pa·s or more, more preferably 0.05 Pa·s or more, and even more preferably 0.1 MPa·s or more. When the viscosity at 25°C is equal to or greater than the above-mentioned lower limit, when the protective layer-forming composition is applied to a release liner to form the protective layer 10a, variation in the thickness of the protective layer 10a can be suppressed. The viscosity of the protective layer-forming composition at 25°C is preferably 15 Pa·s or less, more preferably 10 Pa·s or less, and even more preferably 5 Pa·s or less. When the viscosity at 25°C is equal to or less than the above-mentioned upper limit, the coatability of the protective layer-forming composition when applied to a release liner can be improved. The viscosity of the protective layer-forming composition at 25°C can be measured using a digital viscometer (product name "DV-I Prime") manufactured by Eiko Seiki Co., Ltd. as the measuring device, using an LV-3 spindle at a rotation speed of 50 rpm.
[0037] The saponification degree of the polyvinyl alcohol is preferably 45 or less, more preferably 35 or less, even more preferably 15 or less, even more preferably 12 or less, and particularly preferably 11 or less. The saponification degree of the polyvinyl alcohol is preferably 1 or more, more preferably 2 or more, even more preferably 4 or more, even more preferably 6 or more, and particularly preferably 8 or more. Having a saponification degree within the above range makes the polyvinyl alcohol less soluble in water at room temperature (25±2°C). As described above, the temperature of the cooling water sprayed onto the dicing target, such as an electronic component assembly, during blade dicing is typically 25°C or less. Therefore, by forming the protective layer 10a using polyvinyl alcohol having a saponification degree within the above range, the protective layer 10a can be more sufficiently retained on the surface of the dicing target during blade dicing. Furthermore, as the water solubility of the polyvinyl alcohol decreases, the lipophilicity of the polyvinyl alcohol can be enhanced. Therefore, polyvinyl alcohol having a saponification degree within the above range can have relatively high liposolubility. Therefore, by forming the protective layer 10a using polyvinyl alcohol having a degree of saponification within the above range, the protective layer 10a can be more easily peeled off from the surface of the object to be diced after blade dicing. The degree of saponification of the polyvinyl alcohol can be measured by proton nuclear magnetic resonance spectroscopy ( 1The saponification degree of polyvinyl alcohol can be measured by H-NMR (H-NMR measurement method). If the measurement sample contains additives and the peaks derived from the additives overlap with the peaks used to calculate the saponification degree, the measurement sample is subjected to a methanol extraction treatment or the like to separate and remove the additives, and then the saponification degree of polyvinyl alcohol is measured. The saponification degree of polyvinyl alcohol can be measured under the following conditions. <Measurement Conditions> Analytical Instrument: FT-NMR: Bruker Biospin, AVANCE III-400 Observation Frequency: 400 MHz (1H) Measurement Solvent: Deuterated Water or Deuterated Dimethyl Sulfoxide (Deuterated DMSO) Measurement Temperature: 80°C Chemical Shift Standard: External Standard TSP-d4 (0.00 ppm) (for heavy water measurement) Measurement Solvent: (2.50 ppm) (for deuterated DMSO measurement) The saponification degree of the polyvinyl alcohol is calculated based on the following formula using the peaks derived from the methylene groups of the vinyl alcohol unit (VOH) (heavy water: 2.0 to 1.0 ppm, deuterated DMSO: 1.9 to 1.0 ppm) and the peaks derived from the acetyl groups of the vinyl acetate unit (VAc) (heavy water: around 2.1 ppm, deuterated DMSO: around 2.0 ppm): In the following formula, [VOH(-CH2)-] represents the peak intensity derived from -CH2- in the vinyl alcohol unit. [VAc(CH3CO-)] indicates the peak intensity derived from CH3CO- in the vinyl acetate unit.
[0038]
[0039] The average degree of polymerization of the polyvinyl alcohol is preferably 100 or more, more preferably 150 or more, even more preferably 200 or more, and even more preferably 250 or more. The average degree of polymerization of the polyvinyl alcohol is preferably 3000 or less, more preferably 2000 or less, even more preferably 1000 or less, even more preferably 700 or less, particularly preferably 400 or less, and most preferably 300 or less. As the average degree of polymerization increases, the polyvinyl alcohol becomes less soluble in water at room temperature (25±2°C). As described above, such polyvinyl alcohol has reduced hydrophilicity and therefore improved lipophilicity. Therefore, by forming the protective layer 10a using polyvinyl alcohol with a higher average degree of polymerization, the protective layer 10a can be more sufficiently retained on the surface of the dicing target during blade dicing. Furthermore, by forming the protective layer 10a using polyvinyl alcohol with a lower average degree of polymerization, the protective layer 10a can be more easily peeled from the surface of the dicing target after blade dicing. The average degree of polymerization of polyvinyl alcohol can be measured by aqueous GPC under the following conditions. <Measurement Conditions> - Analytical Instrument: Agilent 1260Infinity - Columns: TSKgel G6000PWXL (Tosoh Corporation) and TSKgel G3000PWXL (Tosoh Corporation) The two columns are connected in series. - Column Temperature: 40°C - Eluent: 0.2 M aqueous sodium nitrate solution - Injection Volume: 100 μL - Detector: Differential Refractometer (RI) - Standard Samples: PEG Standard Sample and PVA Standard Sample Specific measurements are performed as follows: (1) The mass-average molecular weight Mw of the sample (PVA) and the PVA standard sample are calculated by GPC measurement using the PEG standard sample. The average degree of polymerization of the PVA standard sample is known. (2) A calibration curve is created using the average degree of polymerization of the PVA standard sample and the calculated mass-average molecular weight Mw of the PVA standard sample. (3) Using the created calibration curve, the average degree of polymerization of the sample (PVA) is determined from the mass average molecular weight Mw of the sample (PVA).
[0040] As the polyvinyl alcohol, a combination of polyvinyl alcohols having different degrees of saponification may be used, or a combination of polyvinyl alcohols having different average degrees of polymerization may be used.
[0041] The polyvinyl alcohol preferably does not have an oxyalkylene group represented by the following formula (1) on a side chain in the molecule or on the end of the main chain in the molecule. When the protective layer 10a is formed from a protective layer-forming composition containing polyvinyl alcohol, if the polyvinyl alcohol has the oxyalkylene group, the water resistance of the protective layer 10a may be reduced due to the influence of steric hindrance caused by the oxyalkylene group. Therefore, since the polyvinyl alcohol does not have an oxyalkylene group in the molecule, the influence of steric hindrance caused by the oxyalkylene group is eliminated, and the protective layer 10a can have more sufficient water resistance.
[0042]
[0043] The protective layer 10a of the protective sheet 10 may contain an organic compound other than polyvinyl alcohol. Examples of organic compounds other than polyvinyl alcohol include polyvinyl butyral (PVB) and acrylic polymers. Various known acrylic polymers can be used as the acrylic polymer. Such acrylic polymers preferably have a carboxyl group. Examples of acrylic polymers having a carboxyl group include "Alphon UC-3150" manufactured by Toagosei Co., Ltd. When polyvinyl butyral is used as the organic compound other than polyvinyl alcohol, it is preferable to use an organic solvent as a solvent for suspending and dissolving the polyvinyl butyral. Examples of such organic solvents include alcohols such as ethanol, isopropyl alcohol (IPA), and butanol. Furthermore, when the acrylic polymer is used as the organic compound other than polyvinyl alcohol, it is preferable to use an organic solvent as a solvent for suspending and dissolving the acrylic polymer. Examples of such organic solvents include ethanol, isopropyl alcohol (IPA), methyl ethyl ketone (MEK), and acetone.
[0044] In addition, organic compounds other than polyvinyl alcohol include polymers having betaine units in the molecule (betaine polymers). Betaine polymers are polymers having both cationic and anionic groups in their side chains. The mass-average molecular weight Mw of the betaine polymer is preferably 50,000 or more, more preferably 80,0000 or more. The betaine polymer can also be suspended or dissolved in alcohols such as ethanol, isopropyl alcohol (IPA), or butanol. The mass-average molecular weight Mw of the betaine polymer can be determined in the same manner as the mass-average molecular weight Mw of polyvinyl alcohol described above. Examples of the betaine polymer include (ethyl methacrylate betaine / acrylates) copolymer. Commercially available products of (ethyl methacrylate betaine / acrylates) copolymer include the RAM Resin series manufactured by Osaka Organic Chemical Industry Co., Ltd. The RAM Resin series is prepared by dissolving the betaine polymer in ethanol to a solids concentration of 30% by mass.
[0045] The mass reduction rate W of the protective layer 10a after immersion in water at 25°C for 180 seconds relative to the mass of the protective layer 10a before immersion in water at 25°C W The mass reduction rate W may be 1% by mass or more, 3% by mass or more, 5% by mass or more, or 10% by mass or more. W may be 25% by mass or less, 20% by mass or less, or 15% by mass or less.
[0046] The mass reduction rate W of the protective layer 10a after immersion in an aqueous alcohol solution at 25°C for 180 seconds relative to the mass of the protective layer 10a before immersion in the aqueous alcohol solution at 25°C having an alcohol concentration of 55% by mass is S may be 45% by mass or more, 60% by mass or more, or 80% by mass or more.
[0047] Naturally, the mass reduction rate W W The closer to 0 mass %, the less soluble the protective layer 10a is in water. SThe closer to 100% by mass the protective layer 10a becomes, the more easily it dissolves in an organic solvent such as alcohol. W is preferably close to 0 mass%, while the mass reduction rate W S is preferably close to 100% by mass.
[0048] The thickness of the protective layer 10a is preferably 2 μm to 70 μm, more preferably 3 μm to 50 μm, and even more preferably 5 μm to 40 μm. The thickness of the protective layer 10a can be determined by measuring the thickness at five randomly selected points using, for example, a dial gauge (manufactured by PEACOCK, Model R-205) and calculating the arithmetic average of these thicknesses.
[0049] The first release liner 10b may be, for example, a base sheet made of a resin such as polyethylene terephthalate (PET) that has been subjected to a release treatment. Examples of release treatments include silicone release treatment. An example of such a release liner is MRA50, a product manufactured by Mitsubishi Chemical Corporation. The second release liner 10c may also be the same as the first release liner 10b.
[0050] The thicknesses of the first release liner 10b and the second release liner 10c are each independently preferably 15 μm or more and 75 μm or less, and more preferably 20 μm or more and 60 μm or less. The thicknesses of the first release liner 10b and the second release liner 10c may be the same or different. The thicknesses of the first release liner 10b and the second release liner 10c can be determined in the same manner as the thickness of the protective layer 10a.
[0051] [Method for Manufacturing Electronic Components] Next, a method for manufacturing electronic components using the protective sheet 10 according to this embodiment will be described.
[0052] The method for manufacturing an electronic component according to the present embodiment is a method for manufacturing an electronic component from an electronic component connected body with a protective layer attached thereto, using a protective sheet having a protective layer attached to at least a portion of the surface of the electronic component connected body. The method includes: attaching the protective layer to an electronic component connected body in which a plurality of electronic components, each having a surface to be protected, are connected with the surfaces to be protected facing the same direction, so as to protect the surfaces to be protected of the plurality of electronic components; dividing the electronic component connected body with the protective layer attached thereto while washing with water, to obtain a plurality of divided electronic components each with the protective layer attached thereto; and removing the divided protective sheet from each of the surfaces to be protected of the plurality of electronic components. In the method for manufacturing an electronic component according to the present embodiment, a mass reduction rate W of the protective layer after immersion in water at 25° C. for 180 seconds is W The mass loss rate W of the protective layer after immersion in an aqueous alcohol solution having an alcohol concentration of 55% by mass at 25° C. for 180 seconds is S In the method for producing an electronic component according to this embodiment, removing the divided protective sheets involves bringing the divided protective layers into contact with a solution containing an organic solvent at a concentration of 55% by mass or more to dissolve at least a portion of the protective layers, and removing the divided protective sheets from the plurality of electronic components.
[0053] In the electronic component manufacturing method according to this embodiment, the electronic component assembly may be a semiconductor wafer in which multiple semiconductor chips are connected with their surfaces to be protected facing the same direction. The multiple semiconductor chips may be connected in a manner that they are arranged on the same plane with their surfaces to be protected facing the same direction, thereby constituting a semiconductor wafer. Furthermore, when the electronic component assembly is a semiconductor wafer, the electronic component manufacturing method according to this embodiment may include grinding the semiconductor wafer from the side on which the protective sheet is not attached while cooling it with water to reduce the thickness of the semiconductor wafer. Furthermore, when the electronic component assembly is a semiconductor wafer, the electronic component manufacturing method according to this embodiment may include grinding the semiconductor wafer before obtaining the multiple semiconductor chips to which the divided protective sheets are attached. Grinding a semiconductor wafer from the side on which the protective sheet is not attached, as described above, is typically referred to as backgrinding.
[0054] As an example of a method for manufacturing an electronic component, a method for manufacturing a TSV type semiconductor chip using a TSV type semiconductor wafer as shown in Figure 3 and a protective sheet 10 according to this embodiment as shown in Figure 4 will be described below. Note that the TSV type semiconductor wafer corresponds to an electronic component assembly, and the TSV type semiconductor chip corresponds to an electronic component. Furthermore, in the method for manufacturing an electronic component, the term "cut into individual pieces" is a concept that is included in the term "divided."
[0055] A method for manufacturing TSV-type semiconductor chips includes: laminating a protective sheet 10 to at least one circuit-forming surface of a TSV-type semiconductor wafer (S1, laminating the protective sheet); dividing the semiconductor wafer (more specifically, the semiconductor wafer body) with the protective sheet 10 while washing it with water to obtain a plurality of TSV-type semiconductor chips with the separated protective sheets 10 attached (S2, dividing the semiconductor wafer); and removing the separated protective sheets 10 from the plurality of TSV-type semiconductor chips (S3, removing the protective sheet). A method for manufacturing TSV-type semiconductor chips using a blade dicing apparatus 300 including a stage ST, a liquid ejection unit SP, and a dicing blade DB as shown in FIG. 5A will be described in more detail below.
[0056] <Laminating the Protective Sheet S1> In a method for manufacturing TSV-type semiconductor chips, as shown in FIG. 5A , a TSV-type semiconductor wafer 20 is placed on a stage ST of a blade dicing device 300 so that the circuit-formation surface is exposed. Next, the protective layer 10a of the protective sheet 10 is laminated onto the semiconductor wafer 20 so as to cover the circuit-formation surface. Specifically, the first release liner 10b is peeled off from the protective sheet 10 to expose one surface of the protective layer 10a. This exposed surface is then laminated to the surface of the semiconductor wafer 20 (the surface on which the electrode portions 20b are exposed), and the second release liner 10c is then peeled off. In this manner, the protective sheet 10 is laminated to the semiconductor wafer 20 with one surface of the protective layer 10a exposed.
[0057] As described above, after the protective layer 10a of the protective sheet is attached to the semiconductor wafer, grinding S1' of the semiconductor wafer may be performed from the side where the protective sheet 10 is not attached.
[0058] In the semiconductor wafer grinding step S1', as shown in FIG. 6A, a grinding process (back grinding) is performed using a polishing pad P until the semiconductor wafer 20 reaches a predetermined thickness. The grinding process reduces the thickness of the semiconductor wafer 20 to a predetermined thickness (see FIG. 6B). The grinding process is performed while cooling the semiconductor wafer 20 with water (e.g., by spraying cooling water onto the semiconductor wafer 20, which is the object to be ground) to reduce the frictional heat generated during grinding with the polishing pad P. The electronic component manufacturing method according to this embodiment is performed using the protective layer 10a having the above-described characteristics. Therefore, even if the semiconductor wafer 20 is ground while spraying cooling water onto the semiconductor wafer 20, peeling of the protective layer 10a from the semiconductor wafer 20 can be suppressed. In other words, the protective sheet 10 according to this embodiment can also be used as a back grinding tape. Note that, in the case of a TSV-type semiconductor wafer, multiple electrode portions 20b and 20c are arranged on both sides, and therefore, the semiconductor wafer grinding step S1' is not usually performed. Grinding S1' of the semiconductor wafer is performed on, for example, the surface of the semiconductor wafer on which no circuit is formed.
[0059] <Semiconductor Wafer Dividing S2> Next, as shown in FIG. 5B , in the blade dicing device 300, cooling water is sprayed from the liquid spraying unit SP to wash the semiconductor wafer 20 and protective layer 10a laminated body with water, while the dicing blade DB is used to divide the semiconductor wafer 20 and protective layer 10a laminated body so as to have at least a pair of electrode portions 20b and 20c facing each other in the thickness direction. Specifically, the dicing blade DB cleaves the semiconductor wafer 20 along the cleaving line L″ shown in FIG. 5A to create individual pieces. Note that in the example shown in FIG. 5B , the semiconductor wafer 20 is divided so as not to be cleaved at the electrode portions 20b and 20c. This results in multiple laminated bodies each consisting of a semiconductor chip 20′ and a divided protective layer 10a. In other words, the dicing blade DB divides not only the semiconductor wafer 20 but also the protective layer 10a into pieces of chip size.
[0060] As described above, in the protective sheet 10 according to this embodiment, the mass loss rate W of the protective layer 10a after immersion in water at 25°C for 180 seconds is W is 0 mass % or more and 30 mass % or less. Therefore, protective layer 10a has a property of being relatively insoluble in water. Therefore, even if cooling water is sprayed onto protective layer 10a during blade dicing while it is attached to the surface of semiconductor wafer 20 as described above, protective layer 10a is sufficiently held on the surface of semiconductor wafer 20, which is the object to be diced.
[0061] 5C, in the blade dicing device 300, a solution containing an organic solvent at a concentration of 55% by mass or more is sprayed from the liquid spraying part SP to dissolve at least a portion of the protective layer 10a. This removes the protective layer 10a divided into pieces of chip size from the surfaces of the multiple semiconductor chips 20′. The temperature of the organic solvent solution is, for example, 25°C or less.
[0062] As the organic solvent, various known organic solvents such as methanol, ethanol, n-propanol, iso-propanol, acetone, methyl ethyl ketone, diethyl ether, ethyl acetate, toluene, or n-hexane can be used. Among these, ethanol is preferred from the viewpoints of ease of availability and low toxicity. The solution containing the organic solvent may contain the organic solvent at a concentration of 50% by mass or more, 60% by mass or more, 70% by mass or more, 80% by mass or more, or 90% by mass or more. The solution containing the organic solvent may contain the organic solvent at a concentration of 100% by mass. In other words, the solution containing the organic solvent may be the organic solvent itself. Note that, from the viewpoint of reducing the environmental load, it is not necessarily preferable to use a solution containing the organic solvent at a concentration of 100% by mass, i.e., the organic solvent itself. From the viewpoint of reducing the environmental load, the solution containing the organic solvent preferably contains the organic solvent at a concentration of 50% by mass or more and 80% by mass or less.
[0063] As described above, in the protective sheet 10 according to this embodiment, the mass loss rate W of the protective layer 10a after immersion in an aqueous alcohol solution having an alcohol concentration of 55% by mass at 25°C for 180 seconds was S is 40% by mass or more and 100% by mass or less. Therefore, the protective layer 10a has a certain degree of lipophilicity and is easily soluble in an organic solvent. Therefore, when a solution containing an organic solvent is sprayed onto the protective layer 10a that has been separated and bonded to the surfaces of the plurality of semiconductor chips 20′ after blade dicing as described above, the separated protective layer 10a can be easily peeled off from the plurality of semiconductor chips 20′.
[0064] The matters disclosed by this specification include the following.
[0065] (1) A protective sheet having a protective layer attached to a surface to be protected of an electronic component having a surface to be protected, or to a surface to be protected of an electronic component assembly in which a plurality of electronic components are connected, wherein the protective layer has a mass loss rate W after immersion in water at 25°C for 180 seconds. W is 0% by mass or more and 30% by mass or less, and the mass reduction rate W of the protective layer after immersion in an aqueous alcohol solution having an alcohol concentration of 55% by mass at 25°C for 180 seconds is S A protective sheet having such a configuration can provide a protective sheet that can exhibit sufficient holding ability to the dicing object during blade dicing and can be easily peeled from the dicing object after the blade dicing.
[0066] (2) The protective sheet according to (1), wherein the protective layer is formed from a protective layer-forming composition containing polyvinyl alcohol, and the polyvinyl alcohol has a degree of saponification of 45 or less and an average degree of polymerization of 100 or more and 3,000 or less.
[0067] (3) A method for manufacturing electronic components from an electronic component connected body with a protective layer attached thereto, using a protective sheet having a protective layer attached to at least a part of a surface of the electronic component connected body, the method comprising: attaching the protective layer to an electronic component connected body in which a plurality of electronic components having surfaces to be protected are connected with the surfaces to be protected facing the same direction, so as to protect the surfaces to be protected of the plurality of electronic components; dividing the electronic component connected body with the protective layer attached thereto while washing with water, to obtain the plurality of divided electronic components with the plurality of protective layers attached thereto; and removing the divided protective sheet from each of the surfaces to be protected of the plurality of electronic components, wherein the mass reduction rate W of the protective layer after immersion in water at 25° C. for 180 seconds is W is 0% by mass or more and 30% by mass or less, and the mass reduction rate W of the protective layer after immersion in an aqueous alcohol solution having an alcohol concentration of 55% by mass at 25°C for 180 seconds is S is 40% by mass or more and 100% by mass or less, and removing the divided protective sheets includes bringing the divided protective layers into contact with a solution containing an organic solvent at a concentration of 55% by mass or more to dissolve at least a portion of the protective layers, and removing the divided protective sheets from the plurality of electronic components.
[0068] (4) The method for manufacturing an electronic component according to (3) above, wherein the electronic component assembly is a semiconductor wafer in which a plurality of semiconductor chips are connected with the surfaces to be protected facing the same direction, and the method further comprises grinding the semiconductor wafer from the side on which the protective sheet is not attached while cooling with water in order to reduce the thickness of the semiconductor wafer, and grinding the semiconductor wafer is carried out before obtaining the plurality of semiconductor chips with the divided plurality of protective layers attached as the plurality of electronic components.
[0069] (5) The method for producing an electronic component according to (3) or (4), wherein the protective layer is formed of a water-soluble resin composition containing polyvinyl alcohol, and the polyvinyl alcohol has a degree of saponification of 45 or less and an average degree of polymerization of 100 or more and 3,000 or less.
[0070] It should be noted that the protective sheet and the method for manufacturing electronic components according to the present invention are not limited to the above-described embodiment. Furthermore, the protective sheet and the method for manufacturing electronic components according to the present invention are not limited by the above-described effects. The protective sheet and the method for manufacturing electronic components according to the present invention can be modified in various ways without departing from the gist of the present invention.
[0071] In the above embodiment, a protective sheet 10 including a protective layer 10a, a first release liner 10b overlapping one surface of the protective layer 10a, and a second release liner 10c on the other surface (the surface opposite the one surface) of the protective layer 10a has been described in detail (see FIG. 4 ). However, the configuration of the protective sheet according to the present invention is not limited to this. For example, the protective sheet 10 may be configured as shown in FIG. 7 . Specifically, the protective sheet 10 may include a backgrind tape BG, which is a laminate of a pressure-sensitive adhesive layer 10d and a substrate 10e, instead of the second release liner 10c. That is, the protective sheet 10 may be configured by laminating the first release liner 10b, the protective layer 10a, the pressure-sensitive adhesive layer 10d, and the substrate 10e in this order. By configuring the protective sheet 10 in this manner, an electronic component assembly, such as a semiconductor wafer, can be bonded to the exposed surface of the protective layer 10a after peeling off the first release liner 10b, and then a back-grinding process can be performed to thin the electronic component assembly. From the perspective of preventing the electronic component assembly from peeling off from the protective layer 10a during the background grinding process, it is preferable that the protective layer 10a have sufficient adhesion to the electronic component assembly. For example, a high storage modulus (e.g., 0.1 MPa or more) of the protective layer 10a at room temperature (23±2°C) can ensure sufficient adhesion to the electronic component assembly. Furthermore, a relatively low viscosity of the protective layer 10a at the temperature (e.g., 40°C) at which the protective layer 10a is bonded to the electronic component assembly can improve the conformability of the protective layer 10a to the electronic component assembly. This ensures sufficient adhesion to the electronic component assembly. Furthermore, the difference in surface energy between the surface of protective layer 10a that is bonded to the connected electronic component body and the surface of protective layer 10a that is bonded to the connected electronic component body is 25 mJ / m 2 85mJ / m or more 2 Also by satisfying the condition below, protective layer 10a can exhibit sufficient adhesion to the electronic component assembly.
[0072] In the above embodiment, an example has been described in which the outermost surface of the insulating layer 20e and the outermost surface of each electrode portion are flush with each other on both sides of the semiconductor wafer 20. However, the arrangement of the electrodes 20b, 20c on the semiconductor wafer 20 is not limited to this. For example, on the semiconductor wafer 20, the surface portion of each electrode portion may protrude from the outermost surface of the insulating layer 20e. Furthermore, the electrodes 20b, 20c may be formed of solder balls.
[0073] In the above embodiment, an example of a method for manufacturing an electronic component has been described in which a TSV-type semiconductor wafer is used as an electronic component assembly to obtain a plurality of semiconductor chips as electronic components. However, the method for manufacturing an electronic component of the present invention is not limited to this. For example, the method for manufacturing an electronic component of the present invention may be applied to a case in which a wafer-level package 100 such as that shown in FIG. 1 is used as an electronic component assembly to obtain a plurality of semiconductor packages 120 as electronic components. Furthermore, the method for manufacturing an electronic component of the present invention may be applied to a case in which an image sensor package stack 200' such as that shown in FIG. 2B is used as an electronic component assembly to obtain a plurality of image sensor packages 200 as electronic components.
[0074] The present invention will now be described in more detail with reference to examples. The following examples are intended to explain the present invention in more detail, but are not intended to limit the scope of the present invention.
[0075] Example 1 An aqueous dispersion solution was prepared in a container by dispersing polyvinyl alcohol (PVA, saponification degree 35, average polymerization degree 380) in water. The container containing the aqueous dispersion solution was then placed in a water bath at 90°C, and the aqueous dispersion solution was stirred to dissolve the polyvinyl alcohol in water, thereby obtaining a protective layer-forming composition according to Example 1. Subsequently, the protective layer-forming composition was applied to a thickness of 40 μm using an applicator onto the release-treated surface of a first PET release liner (manufactured by Mitsubishi Chemical Corporation, product name MRA50, thickness 50 μm) having a silicone release-treated surface. Furthermore, the first PET release liner to which the protective layer-forming composition had been applied was dried at 115°C for 90 seconds, thereby forming a protective layer on the first PET release liner. This resulted in a protective sheet according to Example 1.
[0076] The saponification degree and average polymerization degree of polyvinyl alcohol were measured according to the methods described in the above embodiment section. Furthermore, the mass loss rate W of the protective layer after immersion in water at 25°C for 180 seconds relative to the mass of the protective layer before immersion in water at 25°C was measured according to the procedure described in the above embodiment section. W Furthermore, according to the procedure described in the embodiment section above, the mass reduction rate W of the protective layer after immersion in an aqueous alcohol solution at 25°C for 180 seconds relative to the mass of the protective layer before immersion in the aqueous alcohol solution at 25°C having an alcohol concentration of 55% by mass was determined. S Furthermore, following the procedure described in the embodiment section above, the mass reduction rate W of the protective layer after immersion in an aqueous alcohol solution at 25°C for 180 seconds relative to the mass of the protective layer before immersion in the aqueous alcohol solution at 25°C having an alcohol concentration of 20% by mass was determined. S Ethanol (EtOH) was used as the alcohol. The measurement results of the saponification degree and average polymerization degree, as well as the mass loss rate W W , mass reduction rate W S , and mass reduction rate W S’ The results are shown in Table 1.
[0077] [Example 2] A protective sheet according to Example 2 was obtained in the same manner as in Example 1, except that polyvinyl alcohol with a saponification degree of 10 and an average polymerization degree of 250 was used. The saponification degree of the polyvinyl alcohol and the average polymerization degree of the polyvinyl alcohol were determined in the same manner as in Example 1. The mass reduction rate W W , mass reduction rate W S , and mass reduction rate W S’ The measurement results of the saponification degree and average polymerization degree, and the mass reduction rate W W , mass reduction rate W S , and mass reduction rate W S’ The results are shown in Table 1.
[0078] [Example 3] A protective sheet according to Example 3 was obtained in the same manner as in Example 1, except that polyvinyl alcohol with a saponification degree of 5 and an average polymerization degree of 200 was used. The saponification degree of the polyvinyl alcohol and the average polymerization degree of the polyvinyl alcohol were determined in the same manner as in Example 1. The mass reduction rate W W , mass reduction rate W S , and mass reduction rate W S’ The measurement results of the saponification degree and average polymerization degree, and the mass reduction rate W W , mass reduction rate W S , and mass reduction rate W S’ The results are shown in Table 1.
[0079] [Example 4] A protective sheet according to Example 4 was obtained in the same manner as in Example 1, except that polyvinyl alcohol with a saponification degree of 22 and an average polymerization degree of 2000 was used. The saponification degree of the polyvinyl alcohol and the average polymerization degree of the polyvinyl alcohol were determined in the same manner as in Example 1. The mass reduction rate W W , mass reduction rate W S , and mass reduction rate W S’ The measurement results of the saponification degree and average polymerization degree, and the mass reduction rate W W , mass reduction rate W S , and mass reduction rate W S’The results are shown in Table 1.
[0080] [Example 5] A protective sheet according to Example 5 was obtained in the same manner as in Example 1, except that a betaine polymer dissolved in ethanol (hereinafter referred to as a betaine polymer-containing composition) was used as the protective layer-forming composition instead of a polyvinyl alcohol dissolved in water. W , mass reduction rate W S , and mass reduction rate W S’ The mass reduction rate W W , mass reduction rate W S , and mass reduction rate W S’ The results are shown in Table 1. The betaine polymer-containing composition used was a product name "RAM Resin-1000" manufactured by Osaka Organic Chemical Industry Ltd. (solid content concentration: 30% by mass, mass average molecular weight Mw: approximately 80,000, glass transition temperature Tg: 60°C).
[0081] [Comparative Example 1] A protective sheet according to Comparative Example 1 was obtained in the same manner as in Example 1, except that polyvinyl alcohol with a saponification degree of 65 and an average polymerization degree of 240 was used. The saponification degree of the polyvinyl alcohol and the average polymerization degree of the polyvinyl alcohol were determined in the same manner as in Example 1. The mass reduction rate W W and mass reduction rate W S The measurement results of the saponification degree and average polymerization degree, and the mass reduction rate W W and mass reduction rate W S The results are shown in Table 1.
[0082] <Water Resistance> A protective layer of a protective sheet according to each example having the same planar dimensions as the bare wafer was bonded to one surface of a bare wafer (outer diameter 12 inches (300 mm), thickness 200 μm). The first PET release liner was then peeled off from the protective layer to produce a laminate of the bare wafer and the protective layer as the dicing target. Dicing was then performed under the following conditions using a blade dicing device (dicing saw manufactured by DISCO Corporation, model "DFD6361") equipped with a stage, a liquid ejection unit, and a dicing blade. Specifically, while the laminate was being diced into a plurality of small pieces (bare chips) having planar dimensions of 10 mm × 10 mm, the degree of peeling of the protective layer of the protective sheet according to each example was evaluated for 10 random bare chips present in the center of the bare wafer. Dicing conditions: Single cut; Blade: ZH05 SD-3000-N1-70 CC; Blade rotation speed: 45,000 rpm; Blade running speed: 50 mm sec; Water volume: 0.5 mL / min; Water temperature: 23 °C. In this way, the degree of peeling of the divided protective layer from the bare chip was evaluated for a laminate of a bare chip and a protective layer of a divided protective sheet. The laminate of the bare wafer and the protective layer of the protective sheet was placed on the stage of a blade dicing device so that the protective sheet side was the cutting start surface. That is, during dicing with the blade dicing device, water was sprayed onto the protective layer of the protective sheet. The laminate of the bare wafer and the protective layer of the protective sheet was placed on the stage with the bare wafer attached to the dicing tape. Specifically, the laminate was attached to the adhesive layer of a dicing tape comprising a substrate and an adhesive layer laminated on the substrate, and the exposed surface of the dicing tape was then placed on the stage. The degree of peeling of the protective layer of the protective sheet according to each example was evaluated by observation at 30x magnification using a digital microscope (Keyence Corporation, model "VHX-6000"). The degree of peeling of the divided protective layer from the bare chip was then evaluated according to the following evaluation criteria. Evaluation criteria: Excellent: For the portions where the divided protective layer had peeled, the average distance from the edge of the bare chip to the unpeeled portion (average of 10 portions) was 500 μm or less.Good: For the portions where the divided protective layer had peeled, the average distance from the edge of the bare chip to the unpeeled portion (average of 10 portions) was more than 500 μm and 1 mm or less. Poor: For the portions where the divided protective layer had peeled, the average distance from the edge of the bare chip to the unpeeled portion (average of 10 portions) was more than 1 mm. The results of evaluating the water resistance of the protective layer for the protective sheets of each example are shown in Table 1.
[0083] <Removability> As described above, a laminate of a bare wafer (as an object to be diced) and the protective layer of the protective sheet according to each example was diced into multiple small pieces (bare chips and the divided protective layer laminated together) each having a planar dimension of 10 mm x 10 mm. The dicing tape with the multiple small pieces attached was then removed from the stage. The dicing tape with the multiple small pieces attached was then immersed in a running water bath containing an aqueous alcohol solution (ethanol solution) with an alcohol concentration (ethanol concentration) of 55%. This removed the protective layer of the divided protective sheet from the surface of each bare chip. Ten randomly selected bare chips were then evaluated for the degree of removability of the protective layer of the protective sheet. The degree of removability of the protective layer was evaluated according to the following criteria. Evaluation Criteria: Excellent: After immersion for 60 seconds, no remaining protective layer was visually observed on the surface of any of the ten bare chips. Good: After immersion for 60 seconds, residual protective layer was visually observed on the surface of one of the 10 bare chips at a level that would be problematic for practical use, but after immersion for 300 seconds, residual protective layer was not visually observed on the surface of any of the 10 bare chips. Poor: Even after immersion for 300 seconds, residual protective layer was visually observed on the surface of one of the 10 bare chips at a level that would be problematic for practical use. The removability (55%) of the protective layer of the protective sheet according to each example was evaluated, and the results are shown in Table 1. The removability (20%) of the protective layer of the protective sheet according to each example was also evaluated in the same manner using an aqueous alcohol solution (aqueous ethanol solution) having an alcohol concentration (ethanol concentration) of 20%. The results are also shown in Table 1.
[0084]
[0085] As can be seen from Table 1, for the protective sheets according to each Example, the water resistance of the protective layer was evaluated as excellent or good, and the removability of the protective layer was also evaluated as excellent or good. In contrast, for the protective sheet according to Comparative Example 1, the water resistance of the protective layer could not be evaluated. Since the water resistance of the protective layer could not be evaluated, the removability of the protective layer could not be evaluated. As can be seen from the above results, the mass loss rate W W is 0 mass% or more and 30 mass% or less and the mass reduction rate W S A protective layer having an alcohol content of 40% by mass or more and 100% by mass or less can exhibit sufficient retention (adhesion) to the dicing object during blade dicing and can be easily peeled off from the dicing object after blade dicing. Note that the results in Table 1 also show that an alcohol aqueous solution at 25°C having an alcohol concentration of 20% by mass does not sufficiently remove the protective layer.
[0086] The protective sheet of the present invention is preferably used, for example, as an auxiliary tool when manufacturing electronic components such as semiconductor chips. The method for manufacturing an electronic component of the present invention is preferably used, for example, when manufacturing electronic components such as semiconductor chips.
[0087] 10 Protective sheet, 10a Protective layer, 10b First release liner, 10c Second release liner, 10d Adhesive layer, 10e Substrate, 20 Semiconductor wafer, 20a Semiconductor wafer body, 20b Electrode portion, 20c Electrode portion, 20d Conductive portion, 20e Insulating layer, 20' Semiconductor chip, 100 Wafer-level package, 110 Circuit board, 120 Semiconductor package, 120a Glass piece, 200 Image sensor package, 210 Sensor chip body, 220 Adhesive layer, 230 Glass piece, 200' Laminate for image sensor package, 210' Sensor wafer body, 220' Adhesive layer, 230' Glass plate, 300 Blade dicing device, BG Backgrinding tape, DB Dicing blade, SP Liquid jetting portion, ST Stage.
Claims
1. A protective sheet having a protective layer attached to a surface to be protected of an electronic component having a surface to be protected, or to a surface to be protected of an electronic component assembly in which a plurality of electronic components are connected, the protective layer having a mass reduction rate W after being immersed in water at 25° C. for 180 seconds. W is 0% by mass or more and 30% by mass or less, and the mass reduction rate W of the protective layer after immersion in an aqueous alcohol solution having an alcohol concentration of 55% by mass at 25° C. for 180 seconds is S A protective sheet, wherein the content of the polymer is 40% by mass or more and 100% by mass or less.
2. The protective sheet according to claim 1, wherein the protective layer is formed from a composition for forming a protective layer containing polyvinyl alcohol, and the polyvinyl alcohol has a degree of saponification of 45 or less and an average degree of polymerization of 100 or more and 3,000 or less.
3. A method for manufacturing electronic components using a protective sheet having a protective layer bonded to at least a portion of a surface of an electronic component connected body, the method comprising: bonding the protective layer to an electronic component connected body in which a plurality of electronic components having surfaces to be protected are connected with the surfaces to be protected facing the same direction, so as to protect the surfaces to be protected of the plurality of electronic components; dividing the electronic component connected body with the protective layer bonded thereto while washing with water, to obtain a plurality of divided electronic components each having a plurality of the protective layers bonded thereto; and removing the divided protective sheet from each of the surfaces to be protected of the plurality of electronic components, W is 0% by mass or more and 30% by mass or less, and the mass reduction rate W of the protective layer after immersion in an aqueous alcohol solution having an alcohol concentration of 55% by mass at 25° C. for 180 seconds is S is 40% by mass or more and 100% by mass or less, and in removing the divided protective sheets, a solution containing an organic solvent at a concentration of 55% by mass or more is brought into contact with the divided protective layers to dissolve at least a portion of the protective layers, and the divided protective sheets are removed from the plurality of electronic components.
4. The method for manufacturing an electronic component as described in claim 3, wherein the electronic component assembly is a semiconductor wafer in which a plurality of semiconductor chips are connected with the surfaces to be protected facing the same direction, and the method further comprises grinding the semiconductor wafer from the side on which the protective sheet is not attached while cooling with water in order to reduce the thickness of the semiconductor wafer, and grinding the semiconductor wafer is carried out before obtaining the plurality of semiconductor chips with the plurality of separated protective layers attached as the plurality of electronic components.
5. The method for manufacturing an electronic component according to claim 3 or 4, wherein the protective layer is formed from a water-soluble resin composition containing polyvinyl alcohol, and the polyvinyl alcohol has a degree of saponification of 45 or less and an average degree of polymerization of 100 or more and 3,000 or less.
Citation Information
Patent Citations
Substrate surface protecting tape and substrate backside grinding method
JP1996148452A
Method of dividing semiconductor wafer
JP2011198875A
Tentatively fixing film, tentatively fixing film sheet and manufacturing method of semiconductor device
JP2014029999A
Protective film substrate for dicing, protective film composition for dicing, protective sheet for dicing, and method for producing wafer to be processed
JP2018129365A
Tentatively fixing sheet, processing method, coated film formation method, and method for manufacturing electronic component
JP2021161735A