Ultraviolet curable hygroscopic agent

The UV-curable moisture absorbent composition with hygroscopic particles and a two-component reactive silicone binder addresses the issue of oil bleeding in electronic devices, offering effective long-term suppression and stable curing for improved device performance.

WO2024203973A1PCT designated stage expired Publication Date: 2024-10-03DYNIC CORPORATION
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/011530
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-29
Filing Date
2024-03-24
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Conventional liquid moisture absorbers experience oil bleeding issues, which lead to poor appearance and quality problems in electronic devices, and this phenomenon persists over time despite initial suppression efforts.

Method used

A UV-curable moisture absorbent composition containing hygroscopic particles and a two-component reactive silicone binder, with specific viscosity and particle size characteristics, is developed to effectively suppress oil bleeding over a long period after curing.

Benefits of technology

The UV-curable moisture absorbent provides stable and efficient suppression of oil bleeding, allowing for long-term prevention and simultaneous curing with the adhesive, suitable for various applications including organic EL elements and other electronic devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JPOXMLDOC01-APPB-T000001
    Figure JPOXMLDOC01-APPB-T000001
  • Figure JPOXMLDOC01-APPB-T000002
    Figure JPOXMLDOC01-APPB-T000002
  • Figure JPOXMLDOC01-APPB-T000003
    Figure JPOXMLDOC01-APPB-T000003
Patent Text Reader

Abstract

[Problem] To provide a hygroscopic agent that can effectively prevent or suppress bleeding of oil over a relatively long period. [Solution] The present invention relates to an ultraviolet curable hygroscopic agent, which is a curable composition comprising hygroscopic particles and a binder, the hygroscopic agent being characterized in that: (1) the binder comprises an ultraviolet curable two-component reactive silicone; and (2) the viscosity (20 °C) of the curable composition is 10-200 Pa·s after the two liquid agents of the ultraviolet curable two-component reactive silicone are mixed and reacted and before ultraviolet irradiation.
Need to check novelty before this filing date? Find Prior Art

Description

UV-curable moisture absorbent

[0001] The present invention relates to a novel ultraviolet-curable moisture absorbent.

[0002] In various electronic devices, the interior of the housing is sealed to prevent moisture, dust, and the like from entering from the outside. In such cases, a moisture absorbent may be placed inside the housing to remove even a small amount of moisture that may enter or be generated inside the housing. For example, in display devices such as organic electroluminescence (EL) displays, moisture is known to cause the generation of non-luminous areas known as dark spots or shrinkage. For this reason, moisture-sensitive electronic devices and the like often have a moisture absorbent placed inside the housing to remove moisture.

[0003] Moisture absorbents are available in various forms, such as powder, sheet, and liquid, when used. In particular, liquid moisture absorbents can be disposed by applying them to a predetermined location within an electronic device. In this respect, liquid moisture absorbents are considered to be advantageous over other forms because they can be used relatively freely regardless of the location (shape, size, surface properties, etc. of the object to be coated).

[0004] Various liquid moisture absorbents have been developed so far, and in particular, liquid moisture absorbents in which moisture-absorbing particles are dispersed in a binder resin have been proposed.

[0005] For example, the binder resin may contain a silicone resin and oxide particles dispersed in the binder resin, at least some of the oxide particles forming secondary particles containing a plurality of primary particles, the oxide particles having an average particle size of 4 μm or less, and the oxide particles having a specific surface area of ​​5 to 60 m. 2 A desiccant having a solubility of 1 / g is known (Patent Document 1).

[0006] Also provided, for example, is a desiccant composition comprising particles of at least one first hygroscopic inorganic oxide and a polymeric binder, the particles having an exterior surface, the particles of the at least one first hygroscopic inorganic oxide having a general formula C, where n is an integer greater than 11: n H 2n+1 COO -A desiccant composition characterized in that the outer surface thereof is functionalized with an anion of the formula (Patent Document 2) has been proposed.

[0007] Furthermore, a getter composition containing a silicon copolymer having at least one functional group selected from the group consisting of a carboxylic acid group and a polyalkylene oxide group and a moisture absorbent is known (Patent Document 3).

[0008] In addition, for example, a transparent moisture-absorbing composition has been proposed, which contains a moisture-absorbing agent (B) having an average particle size of 0.3 μm or less in a transparent polymer (A), and the transparent polymer (A) is one or more of a diene polymer, an olefin polymer, an acrylic polymer, a urethane polymer, a polyamide polymer, a polyester polymer, a vinyl chloride polymer, a fluorine-containing polymer, and a silicone polymer (Patent Document 4).

[0009] Furthermore, as a technology relating to organic EL panels, an organic EL panel has been proposed which includes an element formation substrate on which organic EL elements are formed, a sealing substrate, and a sealing layer tightly interposed between the element formation substrate and the sealing substrate, wherein the sealing layer comprises an internal moisture absorbent which covers the organic EL elements, a peripheral moisture absorbent which is provided along the outer periphery of the internal moisture absorbent, and a peripheral adhesive which is provided along the outer periphery of the peripheral moisture absorbent, wherein the internal moisture absorbent is made of an ultraviolet-curable or heat-curable gel-like resin and a desiccant added to the resin at a weight ratio of 0.3% to less than 10%, and the peripheral moisture absorbent is made of the resin and a desiccant added to the resin at a weight ratio of 10% to 80% (Patent Document 6).

[0010] JP 2017-124383, International Publication WO2013 / 182917, Japanese Patent Application Laid-Open No. 2015-509041, JP 2006-272190, International Publication W2019 / 235630, JP 2017-183191

[0011] Although conventional liquid moisture absorbents can achieve a predetermined moisture absorption effect, when they are applied to an object to be coated, a phenomenon may occur in which liquid components (especially oily components) derived mainly from the binder in the liquid moisture absorbent seep into the object to be coated (oil bleeding). This phenomenon not only causes poor appearance, but also may cause quality problems in electronic devices such as organic EL elements.

[0012] To solve these problems, the present inventors have previously developed and filed a patent application for a liquid moisture absorbent, which is a liquid composition containing moisture-absorbing particles and a binder, characterized in that (1) the binder contains a two-component silicone mixture, and (2) the viscosity of the liquid composition (at 20°C) is 10 to 300 Pa s (Patent Document 5). This is a type of moisture absorbent that exhibits moisture absorption properties while remaining in liquid form, and thereby can obtain the desired moisture absorption properties while suppressing oil bleeding.

[0013] However, even with moisture absorbents such as those described in Patent Document 5, further improvement is required in terms of suppressing oil-bleeding. More specifically, there is a growing demand for a long-term oil-bleed suppression effect. Even with moisture absorbents that can suppress oil-bleeding in the early stages, oil-bleeding may gradually increase over time, and over a long period of time, the amount of oil-bleeding may reach a non-negligible level.

[0014] Therefore, a main object of the present invention is to provide a moisture absorbent that can effectively suppress or prevent oil-bleeding for a relatively long period of time. In particular, an object of the present invention is to provide an ultraviolet-curable moisture absorbent that is liquid and has good coatability, and that can effectively suppress or prevent oil-bleeding for a relatively long period of time after curing.

[0015] The present inventors have conducted extensive research in light of the problems of the prior art and have found that a specific curable composition can achieve the above object, thereby completing the present invention.

[0016] That is, the present invention relates to the following ultraviolet-curable moisture absorbent. 1. A curable composition comprising moisture-absorbing particles and a binder, wherein (1) the binder comprises an ultraviolet-curable two-component reactive silicone, and (2) the viscosity (20°C) of the curable composition after the two components of the ultraviolet-curable two-component reactive silicone have been mixed and reacted and before ultraviolet irradiation is 10 to 200 Pa s. 2. The ultraviolet-curable moisture absorbent according to item 1, wherein the moisture-absorbing particles comprise at least one of calcium oxide particles and strontium oxide. 3. The calcium oxide particles have a specific surface area of ​​5 to 80 m 2 / g, and the specific surface area of ​​the strontium oxide particles is 1 to 6 m 2 3. The ultraviolet-curable moisture absorbent according to Item 2, wherein the average particle size of the moisture-absorbing particles is 0.1 to 50 μm. 4. The ultraviolet-curable moisture absorbent according to Item 1, wherein the content of the binder is 20 to 70 wt %. 5. The ultraviolet-curable moisture absorbent according to Item 1, wherein the complex viscosity η of the curable composition before ultraviolet irradiation is measured using a rheometer equipped with parallel plates having a diameter of 20 mm under conditions of a temperature of 20° C., a frequency of 5.0 Hz, and a strain of 0.1%. 1 7. The ultraviolet-curable moisture absorbent according to item 1, wherein the viscosity of the ultraviolet-curable moisture absorbent is 10 to 700 Pa·s. 2 The complex viscosity η of the cured product obtained by irradiating the cured product for 150 seconds was measured using a rheometer equipped with parallel plates having a diameter of 20 mm under the conditions of a temperature of 20°C, a frequency of 5.0 Hz, and a strain of 0.1%. 2 8. (a) The ultraviolet-curable moisture absorbent according to Item 1, wherein the complex viscosity η of the curable composition before ultraviolet irradiation is measured using a rheometer equipped with parallel plates having a diameter of 20 mm under conditions of a temperature of 20°C, a frequency of 5.0 Hz, and a strain of 0.1%. 1 and (b) irradiating the curable composition with ultraviolet light having a wavelength of 365 nm at an illuminance of 100 mW / cm before ultraviolet irradiation. 2The complex viscosity η of the cured product obtained by irradiating the cured product for 150 seconds was measured using a rheometer equipped with parallel plates having a diameter of 20 mm under the conditions of a temperature of 20°C, a frequency of 5.0 Hz, and a strain of 0.1%. 2 The difference between 2 -η 1 ) / 150] is 0.2 or more. 9. A cured film obtained by curing the ultraviolet-curable moisture absorbent according to item 1. 10. The ultraviolet-curable moisture absorbent according to item 1, which is used in a step of forming a coating film of the ultraviolet-curable moisture absorbent in a space of an electronic device in the atmosphere or an inert gas atmosphere, and then curing the coating film by irradiating the coating film with ultraviolet rays. 11. A method for manufacturing an electronic device having a built-in moisture absorbent, comprising: (1) a step of forming a coating film of the ultraviolet-curable moisture absorbent according to item 1 in a space of the electronic device in the atmosphere or an inert gas atmosphere, (2) a step of sealing the space in an inert gas-containing atmosphere or in the atmosphere, and (3) a step of curing the coating film by irradiating the coating film with ultraviolet rays.

[0017] According to the present invention, it is possible to provide a moisture absorbent that can effectively suppress or prevent oil bleeding for a relatively long period of time.

[0018] In particular, the ultraviolet-curable moisture absorbent of the present invention contains an ultraviolet-curable two-component reactive silicone as a binder, and is in a liquid form adjusted to a specific viscosity as a moisture absorbent. Therefore, when in use, the moisture absorbent can be imparted by applying it to an item, and after curing, it can exert the effect of suppressing or preventing oil bleeding for a relatively long period of time.

[0019] Furthermore, since the ultraviolet-curable moisture absorbent of the present invention can be cured by irradiation with ultraviolet light, the moisture absorbent can be applied to articles that are sensitive to heat.

[0020] Furthermore, unlike conventional liquid moisture absorbents that do not harden, the moisture absorbent of the present invention is composed of a curable composition, and therefore can be more stably and efficiently fixed (fixed) to articles such as electronic devices by utilizing ultraviolet irradiation when sealing the device. Therefore, the UV-curable adhesive for sealing the device and the moisture absorbent of the present invention can be cured simultaneously by ultraviolet irradiation.

[0021] The liquid moisture absorbent of the present invention having such characteristics is expected to be applied to a variety of uses, such as electronic materials (organic EL elements, etc.), mechanical materials, automobiles, communication devices, building materials, medical materials, precision instruments, etc.

[0022] Fig. 1 is a diagram showing an outline of a sample preparation procedure in the evaluation of "(5) Presence or absence of oil bleeding" in Test Example 1. Fig. 2 is a schematic diagram of a cross-sectional configuration of an organic EL element. Fig. 3 is a schematic diagram of a rheometer equipped with parallel plates.

[0023] 1. Ultraviolet-Curable Moisture Absorbent The ultraviolet-curable moisture absorbent of the present invention (moisture absorbent of the present invention) is a curable composition containing moisture-absorbing particles and a binder, characterized in that: (1) the binder contains an ultraviolet-curable two-component reactive silicone; and (2) the viscosity (20°C) of the curable composition after the two components of the two-component reactive silicone have been mixed and reacted and before ultraviolet irradiation is 10 to 200 Pa s.

[0024] Hygroscopic particles The hygroscopic particles may be either inorganic or organic particles as long as they are made of a material that can substantially irreversibly absorb moisture (for example, a material that can substantially irreversibly absorb moisture in the atmosphere in which the moisture absorbent of the present invention is used), but inorganic particles are particularly preferably used.

[0025] The inorganic particles include alkaline earth metal oxides such as barium oxide (BaO), calcium oxide (CaO), magnesium oxide (MgO), and strontium oxide (SrO), lithium sulfate (Li 2 SO 4 ), sodium sulfate (Na 2 SO 4 ), calcium sulfate (CaSO 4 ), magnesium sulfate (MgSO 4), cobalt sulfate (CoSO 4 ), gallium sulfate (Ga 2 (SO 4 ) 3 ), titanium sulfate (Ti(SO 4 ) 2 ), nickel sulfate (NiSO 4 ) and other sulfates. Among these, it is preferable to use at least one alkaline earth metal oxide, and it is particularly preferable to use at least one of calcium oxide (CaO) and strontium oxide (SrO), because they are highly safe, do not generate toxic gases after processing, have a fast moisture absorption rate, and are less likely to lose moisture absorption performance even when mixed with silicone. Therefore, the present invention includes, for example, a) a case in which calcium oxide is contained but not strontium oxide, and b) a case in which both calcium oxide and strontium oxide are contained. In the present invention, it is preferable that the moisture-absorbing particles contain calcium oxide and strontium oxide.

[0026] The average particle size of the hygroscopic particles (powder) can be varied as appropriate depending on the type of hygroscopic particles used, but is typically about 0.1 to 50 μm, preferably 1 to 30 μm, and more preferably 2 to 15 μm. Therefore, for example, the average particle size can be about 0.1 to 5 μm, and even 0.5 to 2 μm. It can also be, for example, 1 μm or more but less than 4 μm. In particular, in the case of calcium oxide, a particle size of 4 to 9 μm is preferable. Furthermore, in the case of strontium oxide, a particle size of 2 to 8 μm is preferable.

[0027] When the composition of the present invention is applied as a moisture absorbent for organic EL devices, etc., it is generally applied to a thickness of 50 to 500 μm. Therefore, the maximum particle size of the moisture-absorbing particles is generally 50 μm or less, preferably 20 μm or less, and more preferably 15 μm or less.

[0028] The specific surface area of ​​the hygroscopic particles can be appropriately changed depending on the type of hygroscopic particles used, but is usually 1 to 100 m 2 / g, preferably 2 to 90 m 2 / g, more preferably 2 to 85 m 2In particular, in the case of calcium oxide, the range is 5 to 80 m 2 In the case of strontium oxide, it is preferable that the content is 1 to 6 m / g. 2 It is preferable to set the value to / g.

[0029] The content of the hygroscopic particles in the hygroscopic agent (solid content) of the present invention is not limited, but from the viewpoint of ensuring better hygroscopicity and good curing properties, it is usually about 30 to 80% by weight, more preferably about 40 to 80% by weight, preferably 55 to 75% by weight, and even more preferably 55 to 70% by weight. Note that when two or more types of hygroscopic particles are used, the above content indicates the total content of those.

[0030] Furthermore, when calcium oxide and strontium oxide are used as the hygroscopic particles, the ratio of the two is preferably within the range of calcium oxide:strontium oxide=5% by weight:95% by weight to 50% by weight:50% by weight, where the total of the two is 100% by weight. By setting the ratio within this range, better hygroscopicity, hardening properties, etc. can be obtained.

[0031] Binder The moisture absorbent of the present invention contains an ultraviolet-curable two-component reactive silicone (the binder of the present invention) as a binder.

[0032] The ultraviolet-curable two-component reactive silicone may be any silicone that undergoes a three-dimensional crosslinking reaction through photoinitiated polymerization upon irradiation with ultraviolet light. For example, it may be of either a photoradical reaction type or a cationic reaction type. In other words, a silicone of the type that is formed by mixing two components to form a liquid having a predetermined viscosity and then cured by irradiating the liquid with ultraviolet light can be preferably used.

[0033] The binder of the present invention preferably contains a siloxane component (e.g., a polysiloxane compound which may have a functional group), and may also contain various other components such as a photopolymerization initiator, a curing catalyst, and a solvent.

[0034] UV-curable silicones are generally available in one-component and two-component types, but the present invention uses the two-component type, as described above, which allows for smooth mixing with the hygroscopic particles and, after mixing, produces a liquid composition with the desired curing properties.

[0035] Two-component types are generally divided into two components, a base component and a curing agent, and the liquid obtained by mixing these components in a predetermined ratio can be used as a binder. Note that a small amount of one-component silicone may be included as long as it does not impair the effects of the present invention.

[0036] Such ultraviolet-curable two-component reactive silicone may be a known or commercially available product, such as "Bestcure UV Reactive Silicone (Components A and B)" (manufactured by T&K TOKA) or "Shin-Etsu Silicone X-62-7028A, B" (manufactured by Shin-Etsu Chemical Co., Ltd.).

[0037] The content of the binder of the present invention in the moisture absorbent of the present invention (solid content) can be appropriately changed depending on the type of binder used, etc., but from the viewpoint of moisture absorption and curing property in particular, it is usually about 20 to 70% by weight, particularly 20 to 45% by weight, and even more preferably 20 to 40% by weight. The content of the binder of the present invention is the total amount of the two liquids.

[0038] The binder may contain binders other than the binder of the present invention as long as the effects of the present invention are not impaired, but the content of the binder of the present invention in the total amount of binders is usually 90 to 100% by weight, more preferably 95 to 100% by weight, and most preferably 98 to 100% by weight. Therefore, for example, the content of the binder of the present invention can be set to 100% by weight.

[0039] Examples of binders other than the binder of the present invention include polyolefin-based, polyacrylic-based, polyacrylonitrile-based, polyamide-based, polyester-based, epoxy-based, polycarbonate-based, etc. Known or commercially available binders can be used.

[0040] Other Components Other components can be added to the moisture absorbent of the present invention as needed, as long as they do not impair the effects of the present invention. Examples include surfactants, antistatic agents, pigments, indicators, fragrances, lubricant fillers, antioxidants, etc. These are also preferably in powder form. The amount of these components added can be about 5% by weight or less in total in the moisture absorbent of the present invention, but is not limited to this.

[0041] Form and Properties of the Moisture Absorbent of the Present Invention The moisture absorbent of the present invention is liquid, and in particular, has a viscosity (20°C) of 10 to 200 Pa·s (preferably 20 to 100 Pa·s). This viscosity is the viscosity of the curable composition obtained after mixing two liquid components of a UV-curable two-component reactive silicone, mixing the resulting mixture with the moisture absorbent, and before irradiating with ultraviolet (UV) rays. By controlling the viscosity within this range, even if a predetermined amount of hygroscopic particles (powder) is contained, the composition can exhibit good coatability before UV curing, while exhibiting high moisture absorption and oil-bleed suppression effects after UV curing. If the viscosity exceeds 200 Pa·s, the desired curability cannot be obtained. If the viscosity is less than 10 Pa·s, it becomes difficult to maintain the coating shape (coating film shape).

[0042] Although there is no particular limitation on the method for setting the viscosity within the above range, a method of adjusting the mixing ratio of the two liquid components of the two-component reactive ultraviolet curing silicone is particularly preferred. In the case of two liquid components consisting of a base component and a curing agent, this can be achieved by adjusting the ratio of the curing agent to the base component. More specifically, the amount of curing agent (liquid B) added (W) sufficient to completely cure the liquid component is added to 100 parts by weight of the base component (liquid A). B When the amount of curing agent actually added is W, the present invention is usually in the range of 0 < W B ≦W≦1W B (preferably 0.1W B ≦W≦0.5W B ) by adjusting the amount W added, the viscosity range described above can be more reliably obtained. Therefore, for example, when an ultraviolet-curable two-component reactive silicone is commercially available, the amount added recommended by the commercial manufacturer is usually adjusted to the above W BTherefore, the amount of hardener added W in this case is the amount of hardener added W recommended by the manufacturer. B The same amount or less (for example, the amount of hardener recommended by the manufacturer (W B (parts by weight), 0<W≦1W B , and 0.01W B ≦W≦1W B , and 0.02W B ≦W≦1W B , and another 0.1W B ≦W≦0.5W B By adding a curing agent to the base resin so that the viscosity becomes approximately the same as the viscosity of the base resin, the desired viscosity can be obtained more reliably.

[0043] In the present invention, viscosity is measured by a method conforming to Japanese Industrial Standard JIS K5600-2-3, with a shear rate of 1 to 100 s. -1 Within the range of 1S -1 , 2.15S -1 , 4.64S -1 , 10S -1 , 21.5S -1 , 100S -1 The viscosity at 20°C was measured at a shear rate of 10 s. -1 This shows the viscosity when

[0044] The viscoelasticity of the curable composition of the moisture absorbent of the present invention before ultraviolet irradiation was measured using a rheometer equipped with parallel plates having a diameter of 20 mm under the conditions of a temperature of 20°C, a frequency of 5.0 Hz, and a strain of 0.1%. 1 From the viewpoint of ease of application of the curable composition, it is desirable that the viscosity is 10 to 700 Pa·s (particularly preferably 10 to 150 Pa·s).

[0045] In addition, the viscoelasticity of the moisture absorbent of the present invention after ultraviolet irradiation was measured by irradiating ultraviolet light with a wavelength of 365 nm at an illuminance of 100 mW / cm. 2 The complex viscosity η of the cured product of the moisture absorbent of the present invention obtained by irradiating the cured product with 150 seconds of irradiation was measured using a rheometer equipped with parallel plates having a diameter of 20 mm under the conditions of a temperature of 20°C, a frequency of 5.0 Hz, and a strain of 0.1%. 2It is particularly desirable for the ultraviolet curing reaction to proceed appropriately and for oil bleeding to be effectively suppressed, that is, for the viscosity to be 10 to 10,000 Pa·s (particularly 50 to 500 Pa·s).

[0046] Furthermore, the moisture absorbent of the present invention has a complex viscosity η of 20° C., measured under the conditions of a temperature of 20° C., a frequency of 5.0 Hz, and a strain of 0.1% using a rheometer equipped with parallel plates having a diameter of 20 mm in the curable composition before ultraviolet irradiation. 1 and (b) irradiating the curable composition with ultraviolet light having a wavelength of 365 nm at an illuminance of 100 mW / cm before ultraviolet irradiation. 2 The complex viscosity η of the cured product obtained by irradiating the cured product for 150 seconds was measured using a rheometer equipped with parallel plates having a diameter of 20 mm under the conditions of a temperature of 20°C, a frequency of 5.0 Hz, and a strain of 0.1%. 2 The difference between these values ​​is divided by the irradiation time, and the value X=[(η 2 -η 1 ) / 150] (increase in complex viscosity per unit time of ultraviolet irradiation) is preferably 0.2 or more. The above X is an index showing the degree of progress of the ultraviolet curing reaction, and the larger the value, the more the curing reaction has progressed. In this respect, if the above X is 0.2 or more, it can be said that it indicates that the ultraviolet curing reaction has substantially progressed. Therefore, for example, it can be set to 0.25 or more.

[0047] From the above viewpoint, in the present invention, a value of X of 4.4 or more is classified as "fully cured," a value of 1.4 or more but less than 4.4 is classified as "cured," a value of 0.2 or more but less than 1.4 is classified as "semi-cured," and a value of less than 0.2 is classified as "uncured." In particular, in the present invention, "cured" and "semi-cured" are preferred, with "semi-cured" being more preferred. These points are also described in Test Example 1 "(4) UV curability" below.

[0048] 2. Method for Producing the Moisture Absorbent of the Present Invention The moisture absorbent of the present invention can be prepared, for example, by mixing raw materials including the moisture-absorbing particles and a binder.

[0049] The types and blending ratios of the hygroscopic particles, binder, etc. used here may be the same as those described above. The order of mixing these components is not limited, and each component may be mixed simultaneously or sequentially. Mixing can be carried out using a known or commercially available mixer, kneader, etc.

[0050] In the present invention, two liquid components (main component, curing agent) of a UV-curable two-component reactive silicone are used as the binder. The order of addition of the hygroscopic particles and the two liquid components is not limited, but it is usually preferable to prepare a reaction product liquid by mixing the two liquid components and reacting them in advance before mixing with the hygroscopic particles. Then, this reaction product liquid is mixed with the hygroscopic particles and, if necessary, other additives. In this way, the hygroscopic agent of the present invention can be produced in a state where the two liquid components have been sufficiently reacted.

[0051] 3. Use of Liquid Moisture Absorbent The method for using the moisture absorbent of the present invention is not particularly limited, and for example, a method including: (1) a step of forming a coating film of the moisture absorbent of the present invention on the surface of an object to be coated (coating film forming step); and (2) a step of irradiating the coating film with ultraviolet light to harden the coating film, thereby forming a hardened film (hardening step) can be suitably employed.

[0052] In the coating film forming step, a coating film of the moisture absorbent of the present invention is formed on the surface of the object to be coated. The method for forming the coating film is not limited, but a method of applying the moisture absorbent of the present invention to the surface of the object to be coated can be preferably used.

[0053] In this case, the method for applying the moisture absorbent of the present invention is not particularly limited, and may be, for example, a method of applying it manually using a brush, spatula, trowel, nozzle, needle, etc., or a method of applying it using a coating device such as a bar coater, doctor blade, spray, slit coater, high-precision dispenser, etc. These methods can be appropriately selected depending on the size, shape, etc. of the object to be applied.

[0054] The coating thickness of the moisture absorbent of the present invention is not limited and can be appropriately set depending on the application site, etc., but it is usually sufficient to adjust the thickness after ultraviolet curing (final target thickness) to about 50 to 500 μm, and further to about 80 to 150 μm.

[0055] In the present invention, the coating film may be subjected to aging at about room temperature or under heating, as necessary. The atmosphere for aging is not particularly limited, and conditions such as air or inert gas may be appropriately selected depending on the material of the object to be coated, etc.

[0056] The object to be coated is not limited as long as it is a component constituting a space (enclosed space) that needs to absorb moisture from the atmosphere, and can be used, for example, in electronic devices installed in various electronic products (communications equipment, medical equipment, office equipment, home appliances, etc.). In particular, it can be suitably used in display devices (e.g., organic electroluminescent devices, liquid crystal displays, inorganic light-emitting diodes, field emission displays, micro LEDs, etc.) that require high moisture removal. By applying the moisture absorbent of the present invention to the housing of these devices, moisture present or generated within the housing can be absorbed and removed.

[0057] For example, in the case of an organic electroluminescent element (organic EL element), a coating film made of the moisture absorbent of the present invention can be formed on the inner surface of a sealing glass used to seal the organic EL element. Organic EL elements include bottom emission type, top emission type, etc., and the moisture absorbent of the present invention can be applied to either type.

[0058] Next, in the curing step, the coating film is irradiated with ultraviolet light to cure the coating film, thereby forming a cured film.

[0059] The method of ultraviolet irradiation is not particularly limited, and can be carried out using a known or commercially available ultraviolet irradiation device.

[0060] In this case, any of the following can be used as the ultraviolet light source: a UV-LED lamp, a mercury lamp, a metal halide lamp, a halogen lamp, a black light lamp, a sodium lamp, a xenon lamp, a fluorescent lamp, sunlight, etc. The wavelength of the ultraviolet light may be, for example, about 200 to 500 nm (particularly, 250 to 400 nm). The irradiation intensity may be, for example, 30 to 10,000 mW / cm. 2 The irradiation dose can be set appropriately within a range of about 100 to 20,000 mJ / cm. 2 The temperature during ultraviolet irradiation can be set appropriately within the range of about 10 to 60°C.

[0061] By irradiating ultraviolet rays, a predetermined cured film can be obtained. The cured film thus obtained may be completely cured, but may also be in a semi-cured state that is not completely cured, as long as the effects of the present invention are not impaired. In particular, the cured film has a complex viscosity η 2 It is desirable that the viscosity is in the range of 10 to 10,000 Pa·s (particularly 50 to 1,800 Pa·s). This makes it possible to more reliably obtain excellent moisture absorption properties and a high oil-bleed suppression effect.

[0062] The present invention also encompasses cured products formed by such ultraviolet irradiation. As described above, this cured product includes not only fully cured products (solids) in which curing is completely completed, but also semi-cured products in which curing is not yet complete. Semi-cured products include, for example, viscous products in which the entire cured product remains liquid, and core-shell products in which the surface of the cured product is solidified and the interior is liquid. In particular, the core-shell products are preferred in that they provide better moisture absorption, oil-bleed suppression, storage properties, etc.

[0063] 4. Manufacturing Method of Electronic Device The present invention encompasses a manufacturing method of an electronic device having a built-in moisture absorbent, comprising: (1) a step of forming a coating film of the ultraviolet-curable moisture absorbent according to claim 1 in a space of the electronic device in the atmosphere or an inert gas atmosphere (coating film forming step); (2) a step of sealing the space in an inert gas-containing atmosphere or in the atmosphere (sealing step); and (3) a step of curing the coating film by irradiating the coating film with ultraviolet light (curing step).

[0064] Coating Film Forming Step In the coating film forming step, a coating film of the moisture absorbent of the present invention is formed in the space (inside the housing) of the electronic device in the air or in an inert gas atmosphere.

[0065] The application method, application amount, etc. of the moisture absorbent of the present invention may be in accordance with the above-described contents. In addition, any of the above-described examples can be suitably adopted as the electronic device.

[0066] When coating is performed in an atmosphere containing an inert gas, examples of the inert gas include nitrogen gas, helium gas, argon gas, etc. The proportion of the inert gas can be appropriately set within the range of usually about 80 to 100% by volume.

[0067] In the sealing step, the space is sealed in an inert gas-containing atmosphere or in the air, that is, the space is isolated from the outside air to form a sealed space.

[0068] The sealing step is basically carried out in an atmosphere containing an inert gas such as nitrogen gas, in which the oxygen concentration and moisture concentration are extremely low, but depending on the processing step, it may be carried out in the air (at normal temperature and humidity).

[0069] When the container is sealed in an atmosphere containing an inert gas, examples of the inert gas include nitrogen gas, helium gas, argon gas, etc. The proportion of the inert gas can be appropriately set within the range of usually 80 to 100% by volume.

[0070] The sealing method itself can be carried out according to a known method, for example, by using an adhesive such as an epoxy resin or an ultraviolet-curable resin, and optionally by heat sealing, ultraviolet irradiation, welding, or the like.

[0071] In the curing step, the coating film is cured by irradiating it with ultraviolet light. The ultraviolet light irradiation conditions can be the same as those described above.

[0072] In the manufacturing method of the present invention, since a curing step is performed after the sealing step, it is preferable that the member used for sealing has transparency. That is, after sealing an electronic device with a sealing glass having a coating film of the moisture absorbent of the present invention formed on the inner surface, ultraviolet light can be irradiated from the outside of the electronic device, whereby ultraviolet light can be irradiated from the back side of the coating film, and as a result, the coating film inside the sealed device can be cured.

[0073] 2, in an organic EL element 20, a sealing glass 22 is used to seal a circuit board 21, and a coating film 23 of the moisture absorbent of the present invention is formed on the inner surface of the sealing glass 22. Then, ultraviolet light is irradiated from above the outside of the sealing glass 22, and the coating film 23 can be cured together with a UV-curable adhesive 24 by the ultraviolet light that has passed through the sealing glass 22.

[0074] Therefore, the manufacturing method of the present invention is particularly suitable for manufacturing electronic devices (for example, organic EL elements) that use a transparent sealing member.

[0075] The features of the present invention will be described in more detail below with reference to examples and comparative examples, but the scope of the present invention is not limited to these examples.

[0076] Example 1 A curable composition was prepared by uniformly mixing calcium oxide powder, strontium oxide powder, and ultraviolet-curable two-component reactive silicone to obtain the composition shown in Table 1. The two components of the ultraviolet-curable two-component reactive silicone were mixed and reacted at room temperature in advance, and then predetermined amounts of calcium oxide powder and strontium oxide powder were added to the resulting reaction product liquid at room temperature and mixed uniformly to prepare a paste-like curable composition. Note that "parts" in Table 1 means "parts by weight."

[0077] Examples 2 to 26 Pasty curable compositions were prepared in the same manner as in Example 1, except that the compositions were changed to those shown in Tables 1 to 4.

[0078] Comparative Examples 1 to 4 Paste-like curable compositions were prepared in the same manner as in Example 1, except that the compositions were changed to those shown in Table 5. In Comparative Examples 2 and 3, the two components were mixed according to the formulation recommended by the product manufacturer.

[0079]

[0080]

[0081]

[0082]

[0083]

[0084] The components in each table were the following products or products obtained by the following manufacturing methods: (1) Strontium oxide (SrO) powder: Strontium hydroxide was calcined at 700°C under reduced pressure for 12 hours to obtain a powder with an average particle size of 5µm and a specific surface area of ​​5m 2 (2) Calcium oxide (CaO) powder: Calcium hydroxide was calcined at 500°C under reduced pressure for 15 hours to obtain strontium oxide with an average particle size of 5µm and a specific surface area of ​​60m. 2 / g of calcium oxide was obtained. (3) Silicones (3-1) UV-1: UV-curable two-component reactive silicone: Product name Bestcure UV-reactive silicone (component A, component B) (manufactured by T&K TOKA) (component A: base component, component B: curing agent, recommended blending ratio: 100 parts by weight of component A / 10 parts by weight of component B) (3-2) UV-2: UV-curable two-component reactive silicone: Product name Shin-Etsu Silicone X-62-7028A, B (manufactured by Shin-Etsu Chemical Co., Ltd.) (component A: base component, component B: curing agent, recommended blending ratio: 100 parts by weight of component A / 90 parts by weight of component B) (4) KE-1013: Two-component addition reaction silicone: Product name KE-1013 (manufactured by Shin-Etsu Chemical Co., Ltd.) (two-component addition reaction type consisting of components A and B) (5) KE-200: Two-component condensation silicone: Product name "KE-200" manufactured by Shin-Etsu Chemical Co., Ltd. (two-component addition reaction type consisting of component A and component B) (6) ECC-3050S: One-component condensation silicone: Product name "ECC-3050S" manufactured by Momentive Performance Materials Japan, LLC

[0085] Test Example 1 The curable compositions obtained in each of the Examples and Comparative Examples were examined for moisture absorption, viscosity, complex viscosity, curability, and oil-bleeding properties. The results are shown in Tables 1 to 5. Each physical property was measured as follows.

[0086] (1) Moisture absorption A curable composition was applied as a thin film to a thickness of 80 to 200 μm to a glass plate etched to have a recess of approximately 0.3 mm. The coated material was then exposed to ultraviolet light in a glove box under the conditions of ultraviolet light having a wavelength of 385 nm and an illuminance of 100 mW / cm. 2 The test piece (32 mm x 42 mm, thickness 0.3 mm) was prepared in a glove box filled with nitrogen gas with a dew point of -40°C or less, and the weight of the test piece was measured with a precision balance in an atmosphere of a temperature of 10 to 30°C and a humidity of 30 to 70% (this measured value was recorded as W 0Next, the test piece was left to stand in a constant temperature and humidity chamber at a temperature of 20°C and a humidity of 65% RH for a set period of time (1 hour, 3 hours, or 24 hours), and the weight of the test piece was measured using a precision balance in an atmosphere at a temperature of 10 to 30°C and a humidity of 30 to 70% (this measured value was designated as Wt). The weight of the test piece was designated as Ws, and the hygroscopicity (C) was calculated using the following formula: C (wt%) = [(Wt - Wo) / Ws] x 100

[0087] (2) Viscosity (Viscosity) Using a viscometer ("HAAKE Viscotester iQ Air" manufactured by Thermo Fisher Scientific Co., Ltd.), a cone plate with a diameter of 20 mm and a cone angle of 2 degrees was used, and the viscosity was measured at a shear rate of 1 to 100 S in accordance with the method of Japanese Industrial Standard JIS K5600-2-3. -1 1S within the range -1 , 2.15S -1 , 4.64S -1 , 10S -1 , 21.5S -1 , 100S -1 The viscosity at 20°C was measured. -1 The values ​​at this time are shown in Tables 1 to 5.

[0088] (3) Viscoelasticity (Complex Viscosity) Measurements were performed using a dynamic viscoelastic meter ("MCR302ST" manufactured by Anton Paar Japan Co., Ltd.). As shown in FIG. 3 , the sample S was sandwiched between two parallel plates 32a and 32b attached to a rotatable drive shaft 31, and the complex viscosity was measured while the drive shaft 31 was rotated forward and backward at a constant cycle. This device was housed in a housing capable of adjusting temperature, etc., but the housing is not shown in FIG. 3 . Measurements were performed using a rheometer equipped with parallel plates 20 mm in diameter (parallel plates 32a in FIG. 3 ). The thickness (gap) of the sample S in FIG. 3 was 0.150 mm, and measurements were performed at a temperature of 20°C, a frequency of 5.0 Hz, and a strain of 0.1%. The complex viscosity of the cured product was measured by irradiating the sample (hygroscopic agent) with ultraviolet light while it was still placed on the parallel plates. The ultraviolet irradiation conditions were ultraviolet light with a wavelength of 365 nm and an illuminance of 100 mW / cm. 2The irradiation time was 150 seconds.

[0089] (4) UV curability The curable composition was applied as a thin film to a thickness of 80 to 200 μm to a glass plate etched to have a recess of approximately 0.3 mm. The coated material was exposed to UV light in a glove box under the conditions of UV light with a wavelength of 385 nm and an illuminance of 100 mW / cm. 2 and irradiation time was 300 seconds to obtain a cured film. If the cured film could be completely peeled off from the glass, it was rated as completely cured (△), if it peeled off from the glass but the peeled cured film broke, it was rated as cured (◯), if it peeled off from the glass but some of the cured film remained on the glass, it was rated as semi-cured (◎), and if it could not be peeled off at all, it was rated as x.

[0090] (5) Presence or absence of oil bleeding In a glove box filled with nitrogen gas and with a dew point of -40°C or less, a curable composition 11 was applied to a glass substrate 10 that had been etched as shown in Figure 1A (width 3 mm x flow 15 mm, thickness 0.080 to 0.100 mm). The etched glass portion was frosted. Next, as shown in Figure 1Ba, a commercially available ultraviolet-curable adhesive (ThreeBond -3124P) was applied to the outer edge 12 of the glass substrate, and then the glass was covered with a flat glass 13 as shown in Figure 1Bb. Thereafter, as shown in Figure 1C, an ultraviolet irradiation device 14 was used to apply an integrated light dose of 6.0 J / cm from directly above the flat glass. 2 The adhesive and curable composition were cured by irradiating them with ultraviolet light so that the curable composition became viscous. The sample prepared as shown in FIG. 1D was sealed in an aluminum packaging material 15. The sample prepared as shown in FIG. 1E was then placed vertically in a dedicated container 16, and the container was left in a thermostatic chamber. Because the aluminum packaging material used had a thick aluminum layer of 15 μm, moisture essentially did not penetrate into the aluminum packaging material. The thermostatic chamber conditions were a temperature of 20°C and 30 days. The sample was then removed from the aluminum packaging material, and the presence or absence of oil seepage was visually observed at the bottom of the cured film formed on the sample. Results were evaluated as "○" when no oil seepage was observed, and "×" when oil seepage was observed.

Claims

1. A curable composition comprising hygroscopic particles and a binder, characterized in that: (1) the binder comprises an ultraviolet-curable two-component reactive silicone; and (2) the viscosity of the curable composition (20°C) after the two liquid components of the ultraviolet-curable two-component reactive silicone are mixed and reacted and before ultraviolet light is applied is 10 to 200 Pa·s.

2. The ultraviolet-curable moisture absorbent according to claim 1, wherein the moisture-absorbing particles include at least one of calcium oxide particles and strontium oxide particles.

3. The specific surface area of ​​calcium oxide particles is 5 to 80 m 2 / g, and the specific surface area of ​​the strontium oxide particles is 1 to 6 m 2 The ultraviolet-curable moisture absorbent according to claim 2 , wherein the molecular weight of the ultraviolet-curable moisture absorbent is 100%.

4. The ultraviolet-curable moisture absorbent according to claim 1, wherein the average particle size of the moisture-absorbing particles is 0.1 to 50 μm.

5. The ultraviolet-curable moisture absorbent according to claim 1, wherein the binder content is 20 to 70% by weight.

6. The complex viscosity η of the curable composition before UV irradiation was measured using a rheometer equipped with parallel plates having a diameter of 20 mm under the conditions of a temperature of 20° C., a frequency of 5.0 Hz, and a strain of 0.1%. 1 The ultraviolet-curable moisture absorbent according to claim 1, wherein the viscosity is 10 to 700 Pa·s.

7. The curable composition is exposed to ultraviolet light having a wavelength of 365 nm at an illumination intensity of 100 mW / cm 2 The complex viscosity η of the cured product obtained by irradiating the cured product for 150 seconds was measured using a rheometer equipped with a parallel plate having a diameter of 20 mm under the conditions of a temperature of 20° C., a frequency of 5.0 Hz, and a strain of 0.1%. 2 The ultraviolet-curable moisture absorbent according to claim 1, wherein the viscosity is 10 to 10,000 Pa·s.

8. (a) The complex viscosity η of the curable composition before ultraviolet irradiation was measured using a rheometer equipped with a parallel plate having a diameter of 20 mm under the conditions of a temperature of 20°C, a frequency of 5.0 Hz, and a strain of 0.1%. 1 (b) irradiating the curable composition with ultraviolet light having a wavelength of 365 nm at an illuminance of 100 mW / cm before ultraviolet light irradiation. 2 The complex viscosity η of the cured product obtained by irradiating the cured product for 150 seconds was measured using a rheometer equipped with a parallel plate having a diameter of 20 mm under the conditions of a temperature of 20° C., a frequency of 5.0 Hz, and a strain of 0.1%. 2 The difference between the 2 -η 1 2. The ultraviolet-curable moisture absorbent according to claim 1 , wherein the ratio of [(x,y) / 150] is 0.2 or more.

9. A cured film obtained by curing the ultraviolet-curable moisture absorbent according to claim 1.

10. The ultraviolet-curable moisture absorbent according to claim 1, which is used in a process in which a coating film of the ultraviolet-curable moisture absorbent is formed in the space of an electronic device in the air or in an inert gas atmosphere, and then the coating film is cured by irradiating the coating film with ultraviolet rays.

11. A method for manufacturing an electronic device having a built-in moisture absorbent, comprising: (1) a step of forming a coating film of the ultraviolet-curable moisture absorbent described in claim 1 in a space of the electronic device in the atmosphere or in an inert gas atmosphere; (2) a step of sealing the space in an inert gas-containing atmosphere or in the atmosphere; and (3) a step of curing the coating film by irradiating the coating film with ultraviolet light.

Citation Information

Patent Citations

  • Marking sheet

    JP1994344655A

  • Ultraviolet-curable resin composition, method of manufacturing organic el light-emitting device, and organic el light-emitting device

    JP2019001995A

  • Curable composition and sealant for organic electroluminescent display element

    JP2020024938A

  • Coated magnesium oxide powder exhibiting high flowability, and resin composition comprising the powder

    WO2005033214A1

  • Film for transfer of gas barrier multilayer film and organic el device

    WO2018016346A1