Laminated spring
The laminated spring design addresses durability issues by applying compressive residual stress through shot peening on the second spring member, enhancing its resistance to stress concentrations and improving operational performance.
Patent Information
- Application Number
- PCT/JP2024/012142
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-31
- Filing Date
- 2024-03-27
- Publication Date
- 2024-10-03
AI Technical Summary
Conventional laminated springs face challenges in durability due to warpage and stress concentration issues during manufacturing, which affect their yield and operational performance, particularly under tensile stress.
A laminated spring design where the second spring member undergoes surface modification by shot peening to apply compressive residual stress around the hole, extending in the width direction and potentially through the central axis, improving durability by alleviating stress concentrations.
The surface modification enhances the durability of the laminated spring by distributing compressive stress effectively, reducing the risk of delayed fracture and improving the overall performance under operational loads.
Smart Images

Figure JP2024012142_03102024_PF_FP_ABST
Abstract
Description
Laminated springs
[0001] The present invention relates to a laminated spring.
[0002] Conventionally, suspension systems have been known that are provided on vehicles and have a buffering function to prevent vibrations caused by road surface irregularities from being transmitted to the vehicle body via the wheels, thereby improving the vehicle's ride comfort, steering stability, etc. Among such suspension systems, leaf spring type suspension systems are configured using leaf springs (see, for example, Patent Document 1).
[0003] Patent Document 1 describes a laminated spring formed by stacking multiple spring members. Each spring member is fastened with fastening members (bolts and nuts) through holes formed in the center of the spring member's longitudinal direction. Generally, the surface of the spring member that receives tensile stress is subjected to surface modification by shot peening.
[0004] Japanese Patent Application Laid-Open No. 2015-121262
[0005] However, spring members may have a curvature that curves away from other spring members that they abut against during stacking. In this case, the spring members are fastened together to suppress the curvature. When the leaf spring operates, tensile stress is generated around the hole on the surface that is subjected to compressive stress. Conventionally, strict tolerance control was required during manufacturing to prevent this tensile stress from exceeding a certain level, and improving the durability of spring members to improve yields was a challenge.
[0006] The present invention has been made in view of the above, and an object of the present invention is to provide a laminated spring formed by stacking a plurality of spring members, which can improve durability.
[0007] In order to solve the above-mentioned problems and achieve the object, the laminated spring of the present invention is a laminated spring formed by stacking a plurality of spring members, and comprises a first spring member that serves as a base, one or more second spring members that are stacked on the first spring member, and a fastening member that fastens the first and second spring members, wherein the first and second spring members are formed with holes through which the fastening members are inserted, and the second spring member is formed with a surface-modified portion that is a part of the surface that receives compressive stress during operation and that includes a part of the opening edge of the hole, and wherein the surface-modified portion is imparted with a compressive residual stress of 300 MPa or more.
[0008] Furthermore, in the laminated spring according to the present invention, the surface modified portion extends in the width direction of the second spring member.
[0009] Furthermore, in the laminated spring according to the present invention, the surface modified portion extends to both widthwise ends of the second spring member.
[0010] In addition, the laminated spring of the present invention is characterized in that, in the above invention, the formation range of the surface modified portion in the longitudinal direction of the second spring member is larger than the diameter of the hole formed in the second spring member.
[0011] In addition, the laminated spring of the present invention is characterized in that, in the above invention, the formation range of the surface modified portion in the longitudinal direction of the second spring member is equal to the diameter of the hole formed in the second spring member.
[0012] In addition, the laminated spring of the present invention is characterized in that, in the above invention, the formation range of the surface modified portion in the longitudinal direction of the second spring member is smaller than the diameter of the hole formed in the second spring member.
[0013] Furthermore, the laminated spring of the present invention is characterized in that, in the above invention, the surface modified portion passes through the longitudinal center of the second spring member, and the central axis extending in the width direction passes through the center of the hole formed in the second spring member.
[0014] Furthermore, the laminated spring according to the present invention is characterized in that, in the above invention, the opening edge of the second spring member on the side receiving the compressive stress among the opening edge of the hole has an R-shape forming a curved surface.
[0015] According to the present invention, it is possible to achieve an effect of improving the durability of a laminated spring formed by laminating a plurality of spring members.
[0016] FIG. 1 is a diagram showing the configuration of a laminated spring according to one embodiment of the present invention. FIG. 2 is a partial cross-sectional view showing the configuration of a main part of the laminated spring shown in FIG. 1. FIG. 3 is a diagram showing an example of the shape of a spring member before fastening. FIG. 4 is a diagram showing the configuration of a portion of a spring member included in a laminated spring according to one embodiment of the present invention. FIG. 5 is a diagram showing the configuration of a portion of a spring member included in a laminated spring according to a first modified example of the present invention. FIG. 6 is a diagram showing the configuration of a portion of a spring member included in a laminated spring according to a second modified example of the present invention. FIG. 7 is a diagram showing the configuration of a portion of a spring member included in a laminated spring according to a third modified example of the present invention. FIG. 8 is a diagram showing the configuration of a portion of a spring member included in a laminated spring according to a fourth modified example of the present invention.
[0017] Hereinafter, embodiments for carrying out the present invention (hereinafter referred to as "embodiments") will be described with reference to the accompanying drawings. Note that the drawings are schematic, and the relationship between the thickness and width of each part, the thickness ratio of each part, etc. may differ from the actual ones, and the drawings may also include parts with different dimensional relationships and ratios.
[0018] (Embodiment) Fig. 1 is a diagram showing the configuration of a laminated spring according to one embodiment of the present invention. The laminated spring shown in Fig. 1 is provided, for example, on the body of a vehicle and used as a leaf spring type suspension device that supports the axles that support the wheels. This leaf spring type suspension device has a buffer function that prevents vibrations caused by road surface irregularities from being transmitted to the vehicle body via the wheels, thereby improving the ride comfort and steering stability of the vehicle. The laminated spring 2 is formed, for example, using a metal material (e.g., spring steel), a resin material, or fiber reinforced plastics (FRP).
[0019] The laminated spring 2 is formed by stacking a plurality of spring members. In this embodiment, an example in which the laminated spring is formed by stacking two spring members will be described. The laminated spring 2 includes a first spring member 11 serving as a base, a second spring member 12 stacked on the first spring member 11, washers 13 and 14, and a fastening member 15.
[0020] The first spring member 11 is formed by bending both ends of a strip-shaped member, and is curved in an arc shape from one end to the other end in the longitudinal direction.
[0021] The second spring member 12 is formed by bending a strip-shaped member into an arc from one end to the other in the longitudinal direction. Hereinafter, the direction perpendicular to the longitudinal direction and thickness direction of the spring member will be referred to as the width direction.
[0022] Fig. 2 is a partial cross-sectional view showing the configuration of a main part of the laminated spring shown in Fig. 1. Fig. 2 shows a cross-section taken along a plane parallel to the longitudinal direction and the plate thickness direction at the center of the longitudinal direction of the laminated spring 2. The fastening member 15 includes a bolt 151 consisting of a head and a shaft, and a nut 152 that screws onto the shaft of the bolt 151.
[0023] Here, the first spring member 11 and the second spring member 12 are formed with holes 11a and 12a, respectively, through which the shank of the bolt 151 is inserted.
[0024] The laminated spring 1 is fabricated by laminating a first spring member 11 and a second spring member 12, disposing a washer 13 on the side of the hole 11a opposite to the second spring member 12 side, and disposing a washer 14 on the side of the hole 12a opposite to the first spring member 11 side. Thereafter, a bolt 151 is inserted through the holes 11a, 12a and the washers 13, 14, and a nut 152 is screwed onto the shaft of the bolt 151, thereby fabricating the laminated spring 1.
[0025] FIG. 3 is a diagram showing an example of the shape of the spring members before fastening. During operation, the laminated spring 2 has a side that receives compressive stress and a side that receives tensile stress due to deformation caused by the operation. Specifically, in the laminated spring 2 shown in FIG. 1 , the lower side is the side that receives compressive stress during operation, and the upper side is the side that receives tensile stress during operation. Hereinafter, the surface that receives compressive stress is referred to as the CS surface, and the surface that receives tensile stress is referred to as the TS surface. Although individual differences exist, the first spring member 11 and the second spring member 12 may have warpage that separates holes when stacked in a natural state where no load other than gravity is applied. In this embodiment, the second spring member 12 is described as having warpage, so that the holes separate from each other when stacked, as shown in FIG. 3 .
[0026] FIG. 4 is a diagram showing the configuration of a portion of a spring member included in a laminated spring according to one embodiment of the present invention. The second spring member 12 has a surface-modified portion 12b formed by surface modification by shot peening on a portion of the CS surface. The surface-modified portion 12b is formed in a region that includes the hole 12a and extends from one end to the other end in the width direction. The surface-modified portion 12b is imparted with compressive residual stress. For example, the surface-modified portion 12b is imparted with compressive residual stress of 300 MPa or more. In this case, the surface-modified portion 12b extends in the width direction, and the central axis N passing through the center of the second spring member 12 in the longitudinal direction passes through the center 121 of the hole 12a. In other words, the surface-modified portion 12b is formed in a region that extends the same length in the longitudinal direction, with the center of the hole 12a as the boundary. The TS surfaces of the first spring member 11 and the second spring member 12 are entirely subjected to a surface modification process by shot peening.
[0027] The second spring member 12 is stacked with the TS surface facing the CS surface of the first spring member 11, and is fastened by the fastening member 15. At this time, the surface modified portion 12b on the CS surface of the second spring member 12 is in pressure contact with the TS surface of the first spring member 11.
[0028] In the embodiment of the present invention described above, in the second spring member 12 laminated on the first spring member 11, a surface modified portion 12b extending in the width direction is provided on a portion of the CS surface including the hole 12a through which the fastening member 15 is inserted. By modifying the surface around the hole 12a on the CS surface, compressive residual stress is imparted around the hole 12a, thereby improving durability against delayed fracture. According to this embodiment, the durability of a laminated spring formed by laminating multiple spring members can be improved.
[0029] Furthermore, according to this embodiment, the surface modified portion 12b may be formed along the width direction of the second spring member 12 from one end to the other end, and can be performed by a simple shot peening process.
[0030] (Variation 1) Next, Variation 1 of the embodiment of the present invention will be described with reference to Fig. 5. Fig. 5 is a diagram showing the configuration of a portion of a spring member included in a laminated spring according to Variation 1 of the present invention. The laminated spring according to Variation 1 differs from the embodiment in the manner in which the surface modified portion of the second spring member 12 is formed. The other components have the same configuration as the embodiment, and therefore description thereof will be omitted.
[0031] The second spring member 12 has a surface-modified portion 12c formed by surface modification using shot peening on a portion of the CS surface. The surface-modified portion 12c is formed in a region that includes the hole 12a and extends from one end to the other end in the width direction. Compressive residual stress is imparted to the surface-modified portion 12c. At this time, the length of the surface-modified portion 12c in the longitudinal direction of the second spring member 12 is equal to the diameter of the hole 12a. In other words, the surface-modified portion 12c extends in the width direction of the second spring member 12 while maintaining a length equal to the diameter of the hole 12a.
[0032] As in the embodiment, the second spring member 12 is stacked with the CS surface facing the TS surface of the first spring member 11, and fastened by the fastening member 15. At this time, the surface modified portion 12c on the CS surface of the second spring member 12 is in pressure contact with the TS surface of the first spring member 11.
[0033] In the above-described modified example 1, as in the embodiment, in the second spring member 12 stacked on the first spring member 11, a surface modified portion 12c extending in the width direction is provided on a part of the CS surface including the hole 12a through which the fastening member 15 is inserted, thereby improving the durability of the laminated spring formed by stacking multiple spring members.
[0034] (Variation 2) Next, Variation 2 of the embodiment of the present invention will be described with reference to Fig. 6. Fig. 6 is a diagram showing the configuration of a portion of a spring member included in a laminated spring according to Variation 2 of the present invention. The laminated spring according to Variation 2 differs from the embodiment in the formation mode of the surface modified portion of the second spring member 12. The other components have the same configuration as the embodiment, and therefore description thereof will be omitted.
[0035] The second spring member 12 has a surface-modified portion 12d formed by surface modification using shot peening on a portion of the CS surface. The surface-modified portion 12d is formed in a region that passes through the hole 12a in the width direction and extends from one end to the other end in the width direction. Compressive residual stress is imparted to the surface-modified portion 12d. In this case, the surface-modified portion 12d extends in the width direction, and the central axis passing through the center of the second spring member 12 in the longitudinal direction passes through the center of the hole 12a. Furthermore, the longitudinal length of the surface-modified portion 12d of the second spring member 12 is smaller than the diameter of the hole 12a.
[0036] As in the embodiment, the second spring member 12 is stacked with the TS surface facing the CS surface of the first spring member 11, and fastened by the fastening member 15. At this time, the surface modified portion 12d on the CS surface of the second spring member 12 is in pressure contact with the TS surface of the first spring member 11.
[0037] In the second modification described above, similar to the embodiment, the second spring member 12 stacked on the first spring member 11 has a surface modified portion 12d extending in the width direction on a portion of the CS surface including the hole 12a through which the fastening member 15 is inserted, thereby improving the durability of the laminated spring formed by stacking multiple spring members.
[0038] (Variation 3) Next, Variation 3 of the embodiment of the present invention will be described with reference to Fig. 7. Fig. 7 is a diagram showing the configuration of a portion of a spring member included in a laminated spring according to Variation 3 of the present invention. The laminated spring according to Variation 3 differs from the embodiment in the formation mode of the surface modified portion of the second spring member 12. The other components have the same configuration as the embodiment, and therefore description thereof will be omitted.
[0039] The second spring member 12 has a surface-modified portion 12e formed by surface modification by shot peening on a portion of the CS surface. The surface-modified portion 12e is formed in a region that passes through the hole 12a in the width direction and extends in the width direction. The region in which the surface-modified portion 12e is formed is shorter than the width (width) of the second spring member 12 and does not reach both ends in the width direction. The width of the surface-modified portion 12e, specifically, the extension range in the width direction from the hole 12a, is set, for example, based on the analysis results of stress concentration around the opening edge of the hole 12a. In this case, the surface-modified portion 12e extends in the width direction, and its central axis passing through the longitudinal center of the second spring member 12 passes through the center of the hole 12a. Furthermore, the longitudinal length of the surface-modified portion 12e of the second spring member 12 is smaller than the diameter of the hole 12a. The surface modified portion 12e is given compressive residual stress.
[0040] As in the embodiment, the second spring member 12 is stacked with the TS surface facing the CS surface of the first spring member 11, and fastened by the fastening member 15. At this time, the surface modified portion 12e on the CS surface of the second spring member 12 is in pressure contact with the TS surface of the first spring member 11.
[0041] In the third modified example described above, as in the embodiment, in the second spring member 12 stacked on the first spring member 11, a surface modified portion 12e extending in the width direction is provided on a part of the CS surface including the hole 12a through which the fastening member 15 is inserted, thereby improving the durability of the laminated spring formed by stacking multiple spring members.
[0042] (Variation 4) Next, Variation 4 of the embodiment of the present invention will be described with reference to Fig. 8. Fig. 8 is a diagram showing the configuration of a portion of a spring member included in a laminated spring according to Variation 4 of the present invention. The laminated spring according to Variation 4 differs from the embodiment in the shape of the opening edge of the hole on the surface modified portion side of the second spring member 12. The other components have the same configuration as the embodiment, and therefore description thereof will be omitted.
[0043] In the fourth modification, at least a portion of the opening edge of the hole 12a formed in the second spring member 12 on the CS surface side is rounded to form a curved surface. This opening edge may be formed by plastic deformation by shot peening, or the rounded shape may be formed in advance before shot peening. Furthermore, this rounded shape may be formed partially around the opening edge, or may be formed over the entire circumference.
[0044] In the fourth modified example described above, as in the embodiment, in the second spring member 12 stacked on the first spring member 11, a surface modified portion 12b extending in the width direction is provided on a part of the CS surface including the hole 12a through which the fastening member 15 is inserted, thereby improving the durability of the laminated spring formed by stacking multiple spring members.
[0045] Furthermore, according to this variant example 4, at least a portion of the opening edge on the CS surface side is formed into a curved R-shape, which alleviates stress concentration on the opening edge of hole 12a, thereby further improving durability.
[0046] Up to this point, the embodiments for carrying out the present invention have been described, but the present invention should not be limited to only the above-described embodiments. The surface modified portion formed on the second spring member 12 is not limited to the region shown in the above-described embodiments and modifications. For example, the length of the surface modified portion in the longitudinal direction of the second spring member 12 is set to 50% or more and 200% or less of the diameter of the hole 12a. Furthermore, in the CS surface, the surface area where a compressive residual stress of 300 MPa or more occurs is set to 100 mm 2 More than 2000mm 2Furthermore, the area ratio of TS surface / CS surface that results in a compressive residual stress of 300 MPa or more is set to be 20 or more and 2200 or less. In addition, various methods of shot peening, such as air type and ultrasonic type, can be adopted depending on the required performance of the spring member, and conditions such as the material, shape, size, spray velocity, and temperature of the particles are also set appropriately.
[0047] In addition, although the above-described embodiment and modified examples have been described with respect to a configuration having one second spring member, a configuration having multiple second members may also be used. In the case of a configuration having multiple second spring members, each second member is formed with a surface modified portion as described above. Furthermore, the laminated spring may be configured without a washer.
[0048] As such, the present invention may include various embodiments not described here, and various design changes may be made within the scope of the technical idea specified by the claims.
[0049] Hereinafter, examples of the laminated spring according to the present invention will be described, but the present invention is not limited to these examples.
[0050] Example 1 In Example 1, a delayed fracture test was conducted using a test specimen with a hole formed in the center of a plate-shaped member. <Test Specimen> A plate-shaped member was used, formed using spring steel (SUP10) with a width of 70 mm, length of 180 mm, and thickness of 22 mm and a hardness of 500 HV. A φ12.9 mm hole was formed in the center of this plate-shaped member by hot punching. Furthermore, shot peening was performed on the entire TS surface of the plate-shaped member and around the hole on the CS surface to prepare a test specimen. Shot peening was performed using an air method. In Example 1, shot peening was performed on the CS surface in the region shown in Figure 4 to impart compressive residual stress. A compressive residual stress of approximately 900 MPa was imparted to the shot peened region of the CS surface. <Delayed Fracture Test> A given bending stress was applied to a test piece by three-point bending, and the test piece was immersed in 10 L of a 1% aqueous solution of ammonium thiocyanate at room temperature for 100 hours, and the presence or absence of breakage in the test piece after immersion was confirmed.
[0051] Example 2 In Example 2, a delayed fracture test was carried out in the same manner as in Example 1, except that shot peening was performed on the CS surface in the region shown in FIG. 6 to impart compressive residual stress.
[0052] In the delayed fracture test, both Examples 1 and 2 showed good delayed fracture resistance.
[0053] As described above, the laminated spring according to the present invention is suitable for improving the durability of a laminated spring formed by stacking a plurality of spring members.
[0054] REFERENCE SIGNS LIST 1 laminated spring 11 first spring member 11a, 12a hole 12 second spring member 12b surface modified portion 13, 14 washer 15 fastening member 151 bolt 152 nut
Claims
1. A laminated spring comprising a plurality of spring members stacked together, the laminated spring comprising: a first spring member serving as a base; one or more second spring members stacked on the first spring member; and a fastening member fastening the first and second spring members together, the first and second spring members having holes through which the fastening members are inserted, the second spring member having a surface-modified portion formed by surface-modifying a part of the surface that receives compressive stress during operation, the part including a part of the opening edge of the hole, and a compressive residual stress of 300 MPa or more being imparted to the surface-modified portion.
2. The laminated spring according to claim 1, characterized in that the surface modified portion extends in the width direction of the second spring member.
3. The laminated spring according to claim 2, characterized in that the surface modified portion extends to both ends of the second spring member in the width direction.
4. The laminated spring according to claim 1, characterized in that the surface modified portion has a formation area in the longitudinal direction of the second spring member that is larger than the diameter of the hole formed in the second spring member.
5. The laminated spring according to claim 1, characterized in that the area in the longitudinal direction of the second spring member where the surface modified portion is formed is equal to the diameter of the hole formed in the second spring member.
6. The laminated spring according to claim 1, characterized in that the area in the longitudinal direction of the second spring member where the surface modified portion is formed is smaller than the diameter of the hole formed in the second spring member.
7. A laminated spring as described in any one of claims 1 to 6, characterized in that the surface modified portion passes through the longitudinal center of the second spring member, and the central axis extending in the width direction passes through the center of a hole formed in the second spring member.
8. The laminated spring as described in claim 1, characterized in that at least a portion of the opening edge of the hole on the side receiving the compressive stress is curved in an R-shape.
Citation Information
Patent Citations
Spring leaf and method for producing a spring leaf
US20210054895A1
Cited By
Laminated spring
WO2025205298A1