Heat dissipation grease

By controlling the aspect ratio of boron nitride particles and incorporating a spherical filler, the thermal grease achieves reduced interfacial thermal resistance and enhanced thermal conductivity, addressing the challenges of viscosity and wettability in boron nitride-based thermal greases.

WO2024204366A1PCT designated stage expired Publication Date: 2024-10-03DENKA CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/012275
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-28
Filing Date
2024-03-27
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Thermal greases using boron nitride particles as heat dissipation fillers face challenges in reducing viscosity, leading to poor wettability and ability to follow microscopic irregularities on surfaces, resulting in increased interfacial thermal resistance.

Method used

Controlling the aspect ratio of boron nitride primary particles within 0.3 to 9 and incorporating a spherical filler, such as alumina, to enhance thermal conductivity while maintaining low viscosity and good wettability.

Benefits of technology

The solution effectively reduces interfacial thermal resistance and increases thermal conductivity, allowing for efficient heat dissipation in electronic devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JPOXMLDOC01-APPB-C000001
    Figure JPOXMLDOC01-APPB-C000001
  • Figure JPOXMLDOC01-APPB-T000002
    Figure JPOXMLDOC01-APPB-T000002
  • Figure JPOXMLDOC01-APPB-T000003
    Figure JPOXMLDOC01-APPB-T000003
Patent Text Reader

Abstract

This heat dissipation grease contains boron nitride primary particles, and the aspect ratio of the boron nitride primary particles is 0.3-9. The present invention makes it possible to provide a heat dissipation grease that can reduce interfacial thermal resistance.
Need to check novelty before this filing date? Find Prior Art

Description

thermal grease

[0001] The present invention relates to a thermal grease.

[0002] In recent years, as electronic devices become more powerful and smaller, the heat density inside them is increasing year by year, posing a challenge for how to efficiently dissipate the heat generated during use. While the details of the cooling mechanism of an electronic device vary depending on the heat-generating part of the electronic device, a basic method of heat removal is to bring the heat-generating part into contact with a cooling member inside the electronic device. In this case, if there is a gap between the heat-generating part and the cooling member, the heat removal efficiency decreases, so heat removal is generally achieved by indirectly contacting the heat-generating part and the cooling member via a heat dissipation member.

[0003] An example of such a heat dissipating material is thermal grease. Thermal grease is made by kneading a heat dissipating filler and a liquid polymer into a paste. Thermal grease has good wettability to the surface of the mounting member and good conformability to the microscopic irregularities on the surface of the mounting member, thereby reducing the interfacial thermal resistance. Furthermore, because thermal grease is fluid, when it is crushed under pressure, the grease layer can be made thinner, thereby reducing the internal thermal resistance of the grease layer. Therefore, thermal grease has high thermal conductivity among heat dissipating materials.

[0004] Thermally conductive greases using boron nitride particles as a thermally conductive filler are known in the prior art (see, for example, Patent Document 1). Because boron nitride particles have high thermal conductivity, using boron nitride particles as a thermally conductive filler can further improve the thermal conductivity of the thermal grease.

[0005] Japanese Patent Application Laid-Open No. 2002-194379

[0006] However, using boron nitride particles as a thermal filler makes it difficult to reduce the viscosity of the thermal grease, resulting in poor wettability of the thermal grease to the surface of the mounting component, which in turn impairs the thermal grease's ability to conform to the microscopic irregularities on the surface of the mounting component, resulting in high interfacial thermal resistance.

[0007] SUMMARY OF THE INVENTION It is therefore an object of the present invention to provide a thermal grease that can reduce the interfacial thermal resistance.

[0008] The present inventors conducted extensive research to solve the above problems. As a result, they discovered that the above problems could be solved by controlling the aspect ratio of the boron nitride primary particles in a thermally conductive grease, and thus completed the present invention. Specifically, the present invention is as follows: [1] A thermally conductive grease containing boron nitride primary particles, wherein the aspect ratio of the boron nitride primary particles is 0.3 to 9. [2] The thermally conductive grease according to [1] above, wherein the boron nitride primary particles have a major axis length of 0.5 to 20 μm. [3] The thermally conductive grease according to [1] or [2] above, further containing a thermally conductive filler different from the boron nitride primary particles, wherein the thermally conductive filler includes a spherical filler.

[0009] According to the present invention, it is possible to provide a thermal grease that can reduce interfacial thermal resistance.

[0010] Fig. 1 is a diagram showing an X-ray diffraction pattern of amorphous boron nitride, and Fig. 2 is a scanning electron microscope (SEM) photograph of boron nitride primary particles 1 used in the examples.

[0011] [Thermal Dissipative Grease] The thermal dissipative grease of the present invention contains boron nitride primary particles, and the boron nitride primary particles have an aspect ratio of 0.3 to 9.

[0012] (Boron Nitride Primary Particles) <Aspect Ratio> The aspect ratio (hereinafter simply referred to as the aspect ratio) of the boron nitride primary particles used in the thermal grease of the present invention, defined as the maximum width of the crystal ab plane divided by the maximum thickness in the crystal c-axis direction, is preferably 0.3 to 9. If the aspect ratio of the boron nitride primary particles is less than 0.3 or greater than 9, the viscosity of the thermal grease increases. This reduces the wettability of the thermal grease to the surface of the mounting component, impairing the thermal grease's ability to conform to microscopic irregularities on the surface of the mounting component, resulting in increased interfacial thermal resistance. From these perspectives, the aspect ratio of the boron nitride primary particles used in the thermal grease of the present invention is preferably 0.3 to 9, more preferably 0.6 to 8, and even more preferably 0.9 to 7. The aspect ratio of the boron nitride primary particles can be measured by the method described in the Examples below.

[0013] <Major axis length> The major axis length of the boron nitride primary particles used in the thermal grease of the present invention is preferably 0.5 μm or more. When the major axis length of the boron nitride primary particles is 0.5 μm or more, the interfacial thermal resistance of the thermal grease can be further reduced, and the thermal conductivity of the thermal grease can be increased even if the content of boron nitride primary particles in the thermal grease is low. From this perspective, the major axis length of the boron nitride primary particles used in the thermal grease of the present invention is more preferably 3.5 to 15 μm. The major axis length of the boron nitride primary particles can be measured by the method described in the Examples below.

[0014] <Method for producing boron nitride primary particles> The boron nitride primary particles used in the thermally conductive grease of the present invention can be produced, for example, by a production method using the flux method described below. The method for producing the boron nitride primary particles used in the thermally conductive grease of the present invention includes, for example, a step (A) of melting a mixture containing amorphous boron nitride obtained by firing boric acid and melamine and lithium borate to produce a melt, a step (B) of cooling the melt, and a step (C) of dissolving the lithium borate with acid and extracting boron nitride particles from the lithium borate. Each step of an example of the method for producing the boron nitride primary particles used in the thermally conductive grease of the present invention will be described in detail below.

[0015] (1) Step (A) In step (A), a mixture containing amorphous boron nitride obtained by calcining boric acid and melamine and lithium borate is melted to produce a melt. <Amorphous Boron Nitride> The amorphous boron nitride used in step (A) is obtained by calcining boric acid and melamine. The molar ratio of boron atoms to nitrogen atoms in the total boric acid and melamine does not necessarily have to be fixed at 5:5, and can be changed appropriately within a range of 2:8 to 8:2, preferably within a range of 3:7 to 7:3, depending on reactivity and yield.

[0016] The firing is preferably carried out in a non-oxidizing atmosphere, the firing temperature is preferably 400 to 1200°C, and the firing time is preferably 1 to 5 hours. By setting the firing temperature to 400°C or higher, it is possible to prevent oxygen and carbon from remaining in the amorphous boron nitride. Furthermore, by setting the firing temperature to 1200°C or lower, it is possible to prevent the progress of crystallization of boron nitride. The firing temperature may be maintained constant or may be changed continuously or discontinuously, and there are no particular restrictions on the firing time or the rate of heating and cooling. Furthermore, there are no particular restrictions on the firing equipment, but the container for storing the raw materials may be made of, for example, hexagonal boron nitride, and the heating device may be a firing furnace using, for example, an electric heater.

[0017] The amorphous boron nitride does not need to be completely amorphous and may be partially crystallized. In addition, the mixed powder of boric acid and melamine may be subjected to briquetting or tableting in order to increase the reaction efficiency by increasing the adhesion between the boric acid particles and the melamine particles.

[0018] By using amorphous boron nitride as a raw material for the boron nitride primary particles, boron nitride can be more completely dissolved in lithium borate, and boron nitride can be more uniformly dissolved in lithium borate. This promotes crystal growth in the thickness direction (c-axis direction) of the boron nitride primary particles, and reduces the aspect ratio (F / T) of the maximum length in the plane direction (long axis length) (F) to the length in the thickness direction (T) of the boron nitride particles. On the other hand, when crystalline boron nitride is used as a raw material for the boron nitride primary particles, it is thought that crystalline boron nitride is less soluble in lithium borate, and the formation of boron nitride primary particles with a low aspect ratio does not proceed. Furthermore, undissolved boron nitride remains in the lithium borate and acts as a nucleus to promote crystal growth in the plane direction (a-axis direction or b-axis direction) of the boron nitride primary particles. This is thought to increase the aspect ratio (F / T) of the maximum plane length (major axis length) (F) to the thickness direction length (T) of the boron nitride primary particles.

[0019] (1-1) Lithium borate By using lithium borate as a flux in step (A), crystal growth in the thickness direction (c-axis direction) of the boron nitride primary particles is promoted, and the aspect ratio (F / T) of the maximum length (long axis length) in the plane direction to the length (T) in the thickness direction of the boron nitride primary particles can be reduced. The lithium borate used in step (A) can be, for example, lithium tetraborate (Li 2 B 4 O 7 ), trilithium borate (Li 3 BO 3 ), lithium metaborate (LiBO 2 These lithium borates can be used alone or in combination of two or more. Among these lithium borates, trilithium borate (Li 3 BO 3 ) is preferred.

[0020] (1-2) Mixture containing amorphous boron nitride and lithium borate The number of moles of amorphous boron nitride in the mixture containing amorphous boron nitride and lithium borate is preferably 10 to 0.5 moles per mole of lithium borate. When the number of moles of amorphous boron nitride is 8 to 0.7 moles, the boron nitride primary particles used in the thermal grease of the present invention can be easily produced. From this perspective, the number of moles of amorphous boron nitride is more preferably 8 to 0.7 moles, and even more preferably 5 to 1 mole, per mole of lithium borate.

[0021] (1-3) Preparation of Melt In step (A), the mixture is melted to prepare a melt. The crucible used when melting the mixture is preferably a carbon crucible or a boron nitride crucible. The melting temperature at which the mixture is melted is not particularly limited as long as it is a temperature at which the mixture can be completely dissolved and volatilization of lithium borate can be suppressed. The melting temperature when melting the mixture is, for example, 1000 to 1700°C, and preferably 1100 to 1500°C. The melting time when melting the mixture is not particularly limited as long as it is a time at which the mixture can be completely dissolved. The melting time when melting the mixture is, for example, 1 to 30 hours, and preferably 5 to 20 hours. The atmosphere when melting the mixture is preferably a nitrogen atmosphere.

[0022] (2) Step (B) In step (B), the melt is cooled. The cooling method of the melt is not particularly limited, and the melt may be cooled slowly or allowed to cool naturally. The cooling rate when the melt is cooled slowly is, for example, 0.5 to 10°C / min.

[0023] (3) Step (C) In step (C), lithium borate is dissolved in acid to extract boron nitride primary particles from the lithium borate. The crucible containing the lithium borate and boron nitride particles may be introduced into the acid, or the contents removed from the crucible may be introduced into the acid. From the viewpoint of dissolving lithium borate and not dissolving the boron nitride primary particles very much, the acid used to dissolve the lithium borate is preferably dilute nitric acid.

[0024] <Content of Boron Nitride Primary Particles in Thermal Grease> The content of boron nitride primary particles in the thermal grease of the present invention is 1 to 20% by volume. When the content of boron nitride primary particles in the thermal grease is 1% by volume or more, the thermal conductivity of the thermal grease is increased, resulting in a lower interfacial thermal resistance. On the other hand, when the content of boron nitride primary particles in the thermal grease is 20% by volume or less, the viscosity of the thermal grease can be prevented from increasing, resulting in improved wettability of the thermal grease to the surface of the mounting component. Furthermore, the thermal grease's ability to conform to microscopic irregularities on the surface of the mounting component is improved, further reducing the interfacial thermal resistance. From these perspectives, the content of boron nitride primary particles in the thermal grease is preferably 2.5 to 15% by volume, and more preferably 5 to 10% by volume.

[0025] (Thermal Conductive Filler Other Than Boron Nitride Primary Particles) The thermal conductive grease of the present invention preferably contains, in addition to the boron nitride primary particles, a thermal conductive filler other than the boron nitride primary particles (hereinafter simply referred to as the thermal conductive filler). Examples of the thermal conductive filler include amorphous granular fillers, spherical fillers, needle-like fillers, fibrous fillers, and plate-like fillers. These thermal conductive fillers can be used alone or in combination of two or more. Of these thermal conductive fillers, spherical fillers are preferred from the viewpoint of being able to increase the content of the thermal conductive filler while suppressing an increase in the viscosity of the thermal conductive grease. Examples of spherical fillers include alumina, silica, calcium carbonate, and zinc oxide. These spherical fillers can be used alone or in combination of two or more. Of these spherical fillers, alumina is preferred from the viewpoint of being able to further increase the thermal conductivity of the thermal conductive grease.

[0026] <Content of Spherical Filler in Heat-Dissipating Filler> When the heat-dissipating filler contains spherical fillers, the content of the spherical fillers in the heat-dissipating filler is preferably 80 to 100% by volume, more preferably 90 to 100% by volume, and even more preferably 95 to 100% by volume.

[0027] <Total Content of Thermally Conductive Filler and Content of Boron Nitride Primary Particles> The total content of the thermally conductive filler and content of the boron nitride primary particles is preferably 45 to 90 volume %. When the total content of the thermally conductive filler and content of the boron nitride primary particles is 45 to 90 volume %, the thermal conductivity of the thermally conductive grease can be further increased while suppressing an increase in the viscosity of the thermally conductive grease. From this perspective, the total content of the thermally conductive filler and content of the boron nitride primary particles is more preferably 55 to 88 volume %, and even more preferably 75 to 85 volume %.

[0028] <Average Particle Diameter of the Thermally Conductive Filler> The volume-based average particle diameter of the thermally conductive filler is preferably 0.1 to 150 μm, more preferably 0.1 to 120 μm. Having an average particle diameter of the thermally conductive filler within the above range tends to further improve fluidity and dispersibility of the thermally conductive filler, and to further suppress the occurrence of voids and cracks. When multiple types of thermally conductive fillers are used, it is preferable that the average particle diameter of each of the thermally conductive fillers be within the above range. When multiple types of thermally conductive fillers are used, taking into account the average particle diameter of each filler, by blending large to small particle diameters in an appropriate ratio to ensure dense packing, it is possible to improve fluidity and dispersibility of the thermally conductive filler even when the packing amount is high.

[0029] <Sphericity of the Thermally Conductive Filler> The sphericity of the thermally conductive filler is usually less than 1, and preferably 0.8 or greater. When the sphericity of the thermally conductive filler is 0.8 or greater, the content of the thermally conductive filler can be increased while suppressing an increase in the viscosity of the thermally conductive grease, thereby further increasing the thermal conductivity of the thermally conductive grease. From this perspective, the sphericity of the thermally conductive filler is more preferably 0.85 or greater, and even more preferably 0.9 or greater. The sphericity of the thermally conductive filler can be measured by the method described in the Examples below.

[0030] (Liquid Polymer) The thermal grease of the present invention preferably contains a liquid polymer in addition to the boron nitride primary particles. The liquid polymer used in the thermal grease of the present invention is not particularly limited as long as it is a liquid polymer commonly used in greases. Examples of liquid polymers used in the thermal grease of the present invention include hydrocarbon oils such as polyolefins, alkyl aromatics, and alicyclic compounds, polyethers such as polyglycols and phenyl ethers, esters such as diesters and polyol esters, phosphorus compounds such as aromatic phosphate esters, silicon compounds such as silicone oils, halogen compounds such as fluorinated polyethers, mineral oils, fluorosilicones, acrylic resins, and urethane resins. Among these liquid polymers, silicone oils are preferred from the viewpoints of heat resistance, weather resistance, electrical insulation, and chemical stability.

[0031] <Content> From the viewpoint of the viscosity and thermal conductivity of the thermal grease, the content of the liquid polymer is preferably 5 to 55 vol%, more preferably 7 to 45 vol%, and even more preferably 10 to 25 vol%, when the total of the boron nitride, thermally conductive filler, liquid polymer, and dispersant is taken as 100 vol%.

[0032] <Viscosity> The viscosity of the liquid polymer used in the thermal grease of the present invention at a temperature of 25°C and 1 s -1 The viscosity measured at a temperature of 25°C and a shear rate of 1 s is preferably 100 Pa s or less. -1 The application properties of the thermal grease are further improved if the viscosity measured at a temperature of 25° C. and a shear rate of 1 s is 10 Pa·s or less. -1 In order to suppress the pumping-out phenomenon of the thermal grease, the viscosity of the liquid polymer used in the thermal grease of the present invention when measured at a temperature of 25° C. and a shear rate of 1 Pa·s is more preferably 1 Pa·s or less. -1 The viscosity measured at a shear rate of 1000 kJ / min is preferably 0.01 Pa·s or more, more preferably 0.1 Pa·s or more. The viscosity of the liquid polymer can be measured by the method described in the examples below.

[0033] (Dispersant) The thermally conductive grease of the present invention may contain a dispersant in addition to the boron nitride primary particles and the liquid polymer. The inclusion of a dispersant in the thermally conductive grease can further reduce the viscosity of the thermally conductive grease. The dispersant is used for the purpose of uniformly dispersing the boron nitride primary particles in the liquid polymer. The dispersant is not particularly limited as long as it can reduce the viscosity of the thermally conductive grease containing the boron nitride primary particles. However, a dispersant having an anionic group and a cationic group is preferred, and a dispersant containing a copolymer described below is more preferred. The dispersant may further contain a solvent or other optional additives, as necessary.

[0034] The dispersant can prevent aggregation and sedimentation of the boron nitride primary particles and the thermally conductive filler in the thermal grease, improving its stability, and can also enable the boron nitride primary particles and the thermally conductive filler to be highly loaded into the liquid polymer and reduce the viscosity of the thermal grease. Furthermore, the dispersant can also improve various other effects associated with the improved dispersibility of the boron nitride primary particles and the thermally conductive filler.

[0035] The dispersant disperses the boron nitride primary particles and the heat-dissipating filler by electrostatic repulsion and prevents the heat-dissipating filler from re-aggregating. Preferably, the dispersant also has the effect of improving dispersibility by steric repulsion.

[0036] <Copolymer> The copolymer used in the dispersant has (meth)acrylic monomer units A having an anionic group, (meth)acrylic monomer units B having a cationic group, and (meth)acrylic monomer units C other than the (meth)acrylic monomer units A and the (meth)acrylic monomer units B, and it is preferable that the weight average molecular weight of the (meth)acrylic monomer units C is 2,000 to 9,000. By having the above structure, the copolymer can significantly reduce the viscosity of the thermally conductive grease.

[0037] In this specification, the term "monomer" refers to a monomer having a polymerizable unsaturated bond before polymerization, and the term "monomer unit" refers to a repeating unit that constitutes a part of a copolymer after polymerization and is derived from a specific monomer. Hereinafter, "(meth)acrylic monomer unit A" will also be referred to simply as "unit A," "(meth)acrylic monomer unit B" will also be referred to simply as "unit B," and "(meth)acrylic monomer unit C" will also be referred to simply as "unit C."

[0038] <(Meth)acrylic Monomer Unit A Having Anionic Group> The (meth)acrylic monomer unit A is a repeating unit having an anionic group. The anionic group is not particularly limited, but examples thereof include a carboxy group, a phosphate group, a phenolic hydroxy group, and a sulfonic acid group. Among these, one or more groups selected from the group consisting of a carboxy group, a phosphate group, and a phenolic hydroxy group are preferred, and a carboxy group is more preferred. The presence of such a group tends to further improve the dispersibility of the boron nitride primary particles and the thermally conductive filler. As a result, the viscosity of the thermally conductive grease of the present invention can be sufficiently reduced.

[0039] Furthermore, it is preferable that the unit A further has an electron-withdrawing group bonded to the anionic group. Such an electron-withdrawing group is not particularly limited as long as it has the effect of stabilizing the anion of the anionic group. For example, an acrylic monomer containing an electron-withdrawing substituent such as a halogen element on the carbon atom at the α-position of the carboxyl group may be used. The presence of such a group tends to further improve the dispersibility of the nitrided particles and the thermally conductive filler. As a result, the viscosity of the thermally conductive grease of the present invention can be sufficiently reduced.

[0040] Preferably, the unit A does not have an electron-donating group bonded to the anionic group or has a group with low electron-donating properties. Such electron-donating groups are not particularly limited as long as they have the effect of destabilizing the anion of the anionic group. For example, acrylic monomers that do not contain an electron-donating group substituent, such as a methyl group, on the carbon atom at the α-position of the carboxyl group may be used. This structure tends to further improve the dispersibility of the thermally conductive filler. As a result, the copolymer can sufficiently reduce the viscosity of the thermally conductive grease of the present invention.

[0041] Such (meth)acrylic monomers are not particularly limited, but examples include acrylic acid, methacrylic acid, acid phosphooxypropyl methacrylate, acid phosphooxypolyoxyethylene glycol monomethacrylate, acid phosphooxypolyoxypropylene glycol monomethacrylate, phosphoric acid-modified epoxy acrylate, 2-acryloyloxyethyl acid phosphate, 2-methacryloyloxyethyl acid phosphate, 4-hydroxyphenyl acrylate, 4-hydroxyphenyl methacrylate, 2-methacryloyloxyethyl succinic acid, 2-acrylamido-2-methylpropanesulfonic acid, etc. Among these, acrylic acid, 2-methacryloyloxyethyl phosphate, 4-hydroxyphenyl methacrylate, and 2-acrylamido-2-methylpropanesulfonic acid are preferred, and acrylic acid is more preferred. The inclusion of units derived from such monomers tends to improve the affinity of the copolymer for the boron nitride primary particles and the thermally conductive filler, and to improve the dispersibility of the boron nitride primary particles and the thermally conductive filler. As a result, the copolymer can sufficiently reduce the viscosity of the thermally conductive grease of the present invention. The units A may be used alone or in combination of two or more.

[0042] ((Meth)acrylic Monomer Unit B Having a Cationic Group) The (meth)acrylic monomer unit B is a repeating unit having a cationic group. The cationic group is not particularly limited, but for example, the cationic group is preferably one or more selected from the group consisting of a primary amino group, a secondary amino group, a tertiary amino group, and a quaternary ammonium salt. Of these, a tertiary amino group is more preferred. The presence of such a group tends to further improve the dispersibility of the heat-dissipating filler. As a result, the copolymer can sufficiently reduce the viscosity of the heat-dissipating grease of the present invention.

[0043] Furthermore, it is preferable that the unit B further has an electron-donating group bonded to the cationic group. Such an electron-donating group is not particularly limited as long as it has the effect of stabilizing the cation of the cationic group. For example, an acrylic monomer containing an electron-donating substituent, such as a methyl group, on the carbon atom at the α-position of the amino group may be used. The presence of such a group tends to further improve the dispersibility of the boron nitride primary particles and the thermally conductive filler. As a result, the copolymer can sufficiently reduce the viscosity of the thermally conductive grease of the present invention.

[0044] Preferably, the unit B does not have an electron-withdrawing group bonded to the cationic group or has a group with low electron-withdrawing properties. Such electron-withdrawing groups are not particularly limited as long as they have the effect of destabilizing the cation of the cationic group. For example, an acrylic monomer that does not contain a substituent of an electron-withdrawing group such as a carboxyl group on the carbon atom at the α-position of the amino group may be used. This structure tends to further improve the dispersibility of the boron nitride primary particles and the thermally conductive filler. As a result, the copolymer can sufficiently reduce the viscosity of the thermally conductive grease of the present invention.

[0045] Such (meth)acrylic monomers are not particularly limited, but examples thereof include 1-aminoethyl acrylate, 1-aminopropyl acrylate, 1-aminoethyl methacrylate, 1-aminopropyl methacrylate, dimethylaminoethyl methacrylate, diethylaminoethyl methacrylate, t-butylaminoethyl (meth)acrylate, dimethylaminoethyl methacrylate quaternary salt, 1,2,2,6,6-pentamethyl-4-piperidyl methacrylate, 2,2,6,6-tetramethyl-4-piperidyl methacrylate, dimethylaminoethyl acrylate benzyl chloride quaternary salt, etc. Among these, 1,2,2,6,6-pentamethyl-4-piperidyl methacrylate and 2,2,6,6-tetramethyl-4-piperidyl methacrylate are preferred, and 1,2,2,6,6-pentamethyl-4-piperidyl methacrylate is more preferred. The inclusion of units derived from such monomers tends to improve the affinity of the copolymer for the boron nitride primary particles and the thermally conductive filler, and to improve the dispersibility of the boron nitride primary particles and the thermally conductive filler. As a result, the copolymer can sufficiently reduce the viscosity of the thermally conductive grease of the present invention. The unit B may be used alone or in combination of two or more types.

[0046] ((Meth)acrylic Monomer Unit C) The (meth)acrylic monomer unit C is a (meth)acrylic monomer unit other than the unit A and the unit B, and is a (meth)acrylic monomer that does not contain a cationic group or an anionic group in the molecule.

[0047] When the copolymer is to be mixed into a thermal grease, the (meth)acrylic monomer C preferably has a skeleton that has high affinity or compatibility with the liquid polymer used in the thermal grease. Examples of such skeletons include, but are not limited to, amphiphilic skeletons such as oxyalkylene skeletons, siloxane skeletons such as dimethylsiloxane, hydrophobic skeletons such as hydrocarbon skeletons of alkyl or aryl groups, and hydrophilic skeletons such as phosphate diester skeletons. Among these, oxyalkylene skeletons, siloxane skeletons, and hydrocarbon skeletons are preferred, with siloxane skeletons and hydrocarbon skeletons being more preferred, and siloxane skeletons being even more preferred. Having such a skeleton further improves the compatibility between the copolymer and the liquid polymer, which tends to further improve the dispersibility of the boron nitride primary particles and the thermally conductive filler in the thermal grease. As a result, the copolymer can sufficiently reduce the viscosity of the thermal grease of the present invention.

[0048] Such (meth)acrylic monomers are not particularly limited, and examples thereof include (meth)acrylic monomers having an oxyalkylene skeleton, such as ethoxycarbonylmethyl (meth)acrylate, phenol ethylene oxide modified (meth)acrylate, phenol (ethylene oxide 2 mol modified) (meth)acrylate, phenol (ethylene oxide 4 mol modified) (meth)acrylate, paracumylphenol ethylene oxide modified (meth)acrylate, nonylphenol ethylene oxide modified (meth)acrylate, nonylphenol (ethylene oxide 4 mol modified) (meth)acrylate, nonylphenol (ethylene oxide 8 mol modified) (meth)acrylate, nonylphenol (propylene oxide 2.5 mol modified) acrylate, 2-ethylhexylcarbitol (meth)acrylate, ethylene oxide modified phthalic acid (meth)acrylate, ethylene oxide modified succinic acid (meth)acrylate, and tetrahydrofurfuryl (meth)acrylate; (meth)acrylate, propyl (meth)acrylate, butyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, isooctyl (meth)acrylate, isodecyl (meth)acrylate, lauryl (meth)acrylate, stearyl (meth)acrylate, phenyl (meth)acrylate, cyclohexyl (meth)acrylate, dicyclopentanyl (meth)acrylate, dicyclopentenyl (meth)acrylate, dicyclopentenyloxyethyl (meth)acrylate, isobornyl ( (Meth)acrylic monomers in which the ester moiety has a hydrocarbon skeleton, such as 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, 2-hydroxy-3-phenoxypropyl (meth)acrylate, and 3-chloro-2-hydroxypropyl (meth)acrylate; (meth)acrylic monomers having a hydroxyl group, such as 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, 2-hydroxy-3-phenoxypropyl (meth)acrylate, and 3-chloro-2-hydroxypropyl (meth)acrylate;(Meth)acrylic monomers having an amide bond such as N,N-dimethyl(meth)acrylamide, N,N-diethyl(meth)acrylamide, N-isopropyl(meth)acrylamide, diacetone(meth)acrylamide, or acryloylmorpholine; (meth)acrylic monomers having a siloxane skeleton such as α-butyl-ω-(3-methacryloxypropyl)polydimethylsiloxane; (meth)acrylic monomers having a phosphoric acid diester skeleton such as (meth)acryloyloxyethyl dialkylphosphate; 1,3-butylene glycol di(meth)acrylate, 1,4-butanediol di(meth)acrylate, 1,6-hexamethylpropional; Examples of suitable (meth)acrylic monomers include diol di(meth)acrylate, 1,9-nonanediol di(meth)acrylate, neopentyl glycol di(meth)acrylate, dicyclopentanyl di(meth)acrylate, 2-ethyl-2-butyl-propanediol (meth)acrylate, neopentyl glycol-modified trimethylolpropane di(meth)acrylate, stearic acid-modified pentaerythritol di(meth)acrylate, 2-(1,2-cyclohexacarboximide)ethyl (meth)acrylate, hexanediol di(meth)acrylate, and polyfunctional (meth)acrylic monomers having a bisphenol structure. The unit C may be used alone or in combination of two or more. Among these, (meth)acrylic monomers having a siloxane skeleton, such as α-butyl-ω-(3-methacryloxypropyl)polydimethylsiloxane, are preferred.

[0049] The weight-average molecular weight of the (meth)acrylic monomer C is preferably 2,000 to 9,000. When the weight-average molecular weight of the (meth)acrylic monomer C is 2,000 or more, the affinity of the copolymer to the liquid polymer is improved, further improving the dispersibility of the boron nitride primary particles and the thermally conductive filler. As a result, the viscosity of the thermally conductive grease of the present invention can be sufficiently reduced. Furthermore, when the weight-average molecular weight of the (meth)acrylic monomer C is 9,000 or less, the copolymer can be easily dissolved in the liquid polymer. From this perspective, the weight-average molecular weight of the (meth)acrylic monomer C is more preferably 2,500 to 7,000, even more preferably 3,000 to 6,000, and even more preferably 3,500 to 5,500. The weight-average molecular weight of the (meth)acrylic monomer C is the weight-average molecular weight of the (meth)acrylic monomer unit C.

[0050] The content of unit A is preferably 30 to 80 mol%, and more preferably 40 to 65 mol%, relative to 100 mol% of the total of unit A, unit B, and unit C. A content of unit A of 30 mol% or more tends to further improve the affinity of the copolymer with the liquid polymer and further improve the dispersibility of the boron nitride primary particles and the thermally conductive filler. As a result, the copolymer can sufficiently reduce the viscosity of the thermally conductive grease of the present invention. Furthermore, a content of unit A of 80 mol% or less allows the copolymer to contain sufficient amounts of unit B and unit C.

[0051] The content of unit B is preferably 0.1 to 5 mol%, more preferably 0.5 to 3 mol%, relative to 100 mol% of the total of unit A, unit B, and unit C. By setting the content of unit B to 0.1 mol% or more, the copolymer has good affinity with the heat-dissipating filler. Furthermore, by setting the content to 5 mol% or less, the copolymer can contain a sufficient amount of unit A and unit C.

[0052] The total content of units A and units B is preferably 30.1 to 85 mol%, and more preferably 35 to 75 mol%, relative to 100 mol% of the total of units A, units B, and units C. When the total content of units A and units B is 30.1 mol% or more, the affinity of the copolymer for the liquid polymer is further improved, and the dispersibility of boron nitride primary particles and heat-dissipating filler tends to be further improved. Furthermore, when the total content of units A and units B is 85 mol% or less, a sufficient amount of units C can be contained in the copolymer.

[0053] The molar ratio of units A to units B is preferably 6 to 800, and more preferably 20 to 400. When the molar ratio of units A to units B is within the above range, the affinity of the copolymer for the liquid polymer is improved, and the dispersibility of the boron nitride primary particles and the heat-dissipating filler tends to be improved.

[0054] The content of unit C is preferably 20 to 70 mol%, more preferably 30 to 55 mol%, relative to 100 mol% of the total of unit A, unit B, and unit C. By making the content of unit C 20 mol% or more, the handleability due to the viscosity of the copolymer is improved. Furthermore, by making the content 70 mol% or less, the copolymer can contain a sufficient amount of unit A and unit B.

[0055] The weight-average molecular weight of the copolymer is preferably 40,000 to 80,000, and more preferably 50,000 to 70,000. When the weight-average molecular weight of the copolymer is 40,000 or more, the steric repulsion of the copolymer makes the boron nitride primary particles and the thermally conductive filler less likely to aggregate, further improving the dispersibility of the boron nitride primary particles and the thermally conductive filler in the thermally conductive grease. Furthermore, when the weight-average molecular weight of the copolymer is 80,000 or less, the copolymer can be more easily dissolved in a liquid polymer. The weight-average molecular weight can be determined by gel permeation chromatography (GPC).

[0056] The copolymer is preferably a copolymer represented by the following general formula (1). The copolymer represented by general formula (1) may be a random copolymer or a block copolymer. In the copolymer represented by the following general formula (1), unit A is derived from acrylic acid, and the anionic group is a carboxy group. In addition, unit B in the copolymer represented by the following general formula (1) is derived from 1,2,2,6,6-pentamethyl-4-piperidyl methacrylate, and the cationic group is a tertiary amino group. Furthermore, unit C in the copolymer represented by the following general formula (1) is derived from α-butyl-ω-(3-methacryloxypropyl)polydimethylsiloxane and has a siloxane skeleton.

[0057] In the formula, s is an integer such that, when the weight-average molecular weight of the copolymer is 40,000 to 80,000, the content of unit A is 30 to 80 mol % relative to 100 mol % of the total of unit A, unit B, and unit C; t is an integer such that, when the weight-average molecular weight of the copolymer is 40,000 to 80,000, the content of unit C is 20 to 70 mol % relative to 100 mol % of the total of unit A, unit B, and unit C; u is an integer such that, when the weight-average molecular weight of the copolymer is 40,000 to 80,000, the content of unit B is 0.1 to 5.0 mol % relative to 100 mol % of the total of unit A, unit B, and unit C. Furthermore, v is an integer such that the weight-average molecular weight of unit C is 2,000 to 9,000.

[0058] <Method for Producing Copolymer> The method for producing the copolymer is not particularly limited, and any known polymerization method for (meth)acrylic monomers can be used. Examples of the polymerization method include radical polymerization and anionic polymerization. Among these, radical polymerization is preferred.

[0059] The thermal polymerization initiator used in the radical polymerization is not particularly limited, but examples thereof include azo compounds such as azobisisobutyronitrile; and organic peroxides such as benzoyl peroxide, tert-butyl hydroperoxide, and di-tert-butyl peroxide. Furthermore, the photopolymerization initiator used in the radical polymerization is not particularly limited, but examples thereof include benzoin derivatives. Furthermore, known polymerization initiators used in living radical polymerization such as ATRP and RAFT can also be used.

[0060] The polymerization conditions are not particularly limited and can be appropriately adjusted depending on the initiator and boiling point of the solvent used, as well as the types of other monomers.

[0061] The order of addition of the monomers is not particularly limited. For example, from the viewpoint of synthesizing a random copolymer, the monomers may be mixed to initiate polymerization, or from the viewpoint of synthesizing a block copolymer, the monomers may be added sequentially to the polymerization system.

[0062] <Content> From the viewpoint of the viscosity of the thermally conductive grease, the content of the dispersant in the thermally conductive grease is preferably 0.1 to 5% by volume, more preferably 0.1 to 4.5% by volume, and even more preferably 0.1 to 4% by volume.

[0063] (Other Components) The thermally conductive grease of the present invention may contain components other than the boron nitride primary particles, the thermally conductive filler other than the boron nitride primary particles, the liquid polymer, and the dispersant (hereinafter referred to as "other components"), as long as the effects of the present invention are not impaired. Examples of other components include colorants, coupling agents, and leveling agents. In addition to the other components, the thermally conductive grease of the present invention may further contain additives such as reaction retarders, as needed. When the thermally conductive grease contains a colorant, the content of the colorant is preferably 0.001 to 0.2 parts by mass per 100 parts by mass of the thermally conductive grease.

[0064] (Viscosity) The thermal grease of the present invention has a viscosity of 1 s at 25°C. -1 The viscosity when measured at a temperature of 25°C and a shear rate of 1 s is preferably 4000 Pa s or less. -1If the viscosity measured at a temperature of 25° C. and a shear rate of 1 s is 4000 Pa·s or less, the spreadability of the thermal grease will be even better. -1 The viscosity of the thermal grease of the present invention measured at a temperature of 25° C. and a shear rate of 1 s is more preferably 2500 Pa·s or less, and even more preferably 2000 Pa·s or less. -1 The viscosity when measured at a shear rate of 100 Pa·s or more is preferably 100 Pa·s or more, and more preferably 200 Pa·s or more. The viscosity of the thermal grease can be measured by the method described in the examples below.

[0065] (Thermal Conductivity) The thermal conductivity of the thermally conductive grease of the present invention is preferably 1.0 W / m·K or more. When the thermal conductivity of the thermally conductive grease is 1.0 W / m·K or more, the thermal conductivity between the heat-generating part and the cooling member can be further improved. From this perspective, the thermal conductivity of the thermally conductive grease of the present invention is more preferably 3.0 W / m·K or more, and even more preferably 5.0 W / m·K or more. The upper limit of the range of the thermal conductivity of the thermally conductive grease of the present invention is not particularly limited, but is usually 10 W / m·K or less. The thermal conductivity of the thermally conductive grease can be measured by the method described in the Examples below.

[0066] (Interfacial Thermal Resistance) The interfacial thermal resistance of the thermally conductive grease of the present invention is preferably 0.154 K / W or less. When the interfacial thermal resistance of the thermally conductive grease is 0.154 K / W or less, the thermal conductivity between the heat-generating portion and the cooling member can be further improved. From this perspective, the interfacial thermal resistance of the thermally conductive grease of the present invention is more preferably 0.154 K / W or less, and even more preferably 0.130 K / W or less. The lower limit of the range of the interfacial thermal resistance of the thermally conductive grease of the present invention is not particularly limited, but is usually 0.05 K / W or more. The interfacial thermal resistance of the thermally conductive grease can be measured by the method described in the Examples below.

[0067] (Method for Producing Thermally Dissipating Grease) The thermally dissipating grease of the present invention can be produced by kneading raw materials such as boron nitride primary particles with a planetary mixer, a universal mixer, a kneader, a hybrid mixer or the like.

[0068] The present invention will be described in more detail below using examples and comparative examples, but the present invention is not limited to the following examples.

[0069] [Raw materials for preparing thermally conductive grease] The following raw materials were prepared for preparing the thermally conductive grease. The boron nitride primary particles and dispersant were prepared by the following methods. (Liquid polymer) Silicone oil: Shin-Etsu Silicone Co., Ltd.'s "KF-96-100CS", dimethyl silicone oil, viscosity 0.1 Pa·s (Thermal conductive filler) Alumina A: DAW45S (trade name, manufactured by Denka Co., Ltd.), spherical alumina, average particle size: 45 μm, circularity 0.98 Alumina B: DAW05 (trade name, manufactured by Denka Co., Ltd.), spherical alumina, average particle size: 5 μm, circularity 0.98 Alumina C: ASFP40 (trade name, manufactured by Denka Co., Ltd.), ultrafine alumina, average particle size: 0.4 μm, circularity 0.99

[0070] The viscosity of the liquid polymer was measured by the same method as that for measuring the viscosity of the thermal grease described below.

[0071] The average particle size of the thermally conductive filler was measured using a laser diffraction particle size distribution analyzer, SALD-20, manufactured by Shimadzu Corporation. The evaluation sample was prepared by adding 50 ml of pure water and 5 g of the thermally conductive filler to be measured to a glass beaker, stirring with a spatula, and then dispersing in an ultrasonic cleaner for 10 minutes. The dispersed dispersion of the thermally conductive filler was added drop by drop to the sampler section of the analyzer using a dropper, and measurement was performed once the absorbance had stabilized. The average particle size was measured as D50 (median diameter).

[0072] The sphericity of the thermally conductive filler was measured using a wet flow particle size and shape analyzer (product name "FPIA-3000", manufactured by Malvern Panalytical). After dispersing the sample in pure water, the liquid was flowed into a planar extensional flow cell, and images of 100 or more thermally conductive fillers moving within the cell were recorded using an objective lens. The average circularity was calculated from this recorded image and the following formula (1). In formula (1), HD represents the circular equivalent diameter, which was determined from the ratio of the projected area of ​​the target particle to the area of ​​a perfect circle. PM represents the projected perimeter of the target particle. The average value of 200 thermally conductive fillers calculated in this way was taken as the average circularity. Formula (1): Average circularity = π HD / PM From this average circularity, the formula: Average sphericity = (average circularity) 2 The average sphericity was calculated by the following.

[0073] [Preparation of Boron Nitride Primary Particles] (Preparation of Boron Nitride Primary Particles 1) A mixed powder was prepared by mixing 100 g of boric acid (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) and 100 g of melamine (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.). The prepared mixed powder was placed in a thermo-hygrostat and humidified at 80°C and 95% relative humidity for 1 hour, followed by drying for 1 hour to obtain melamine borate. The melamine borate salt was calcined in a nitrogen atmosphere at a calcination temperature of 1000°C for 2 hours to prepare amorphous boron nitride. The X-ray diffraction pattern of the prepared amorphous boron nitride is shown in Figure 1. For comparison, the X-ray diffraction pattern of hexagonal boron nitride powder (manufactured by Denka Co., Ltd., product name "SP-3") is also shown in Figure 1. The X-ray diffraction pattern confirmed that the obtained amorphous boron nitride was amorphous.

[0074] Boron nitride (BN) and trilithium borate (Li 3 BO 3The resulting amorphous boron nitride and trilithium borate (manufactured by Toshima Manufacturing Co., Ltd.) were introduced into a low-frequency resonant acoustic mixer (manufactured by Resodyn Acoustic Mixers, Inc., trade name "LabRAM II") and mixed to produce a mixture, so that the molar ratio of amorphous boron nitride to trilithium borate was 2:1 (calculated as molten boron nitride). The resulting mixture was filled into a boron nitride container, and the boron nitride container filled with the mixture was placed in a tubular furnace. The mixture was then melted for 20 hours at a melting temperature of 1300°C in a nitrogen atmosphere (nitrogen gas flow rate 1 L / min) to produce a molten mixture. The melt was then cooled to a temperature of 650°C at a cooling rate of 5°C / min, and allowed to cool naturally above 650°C, resulting in the precipitation and growth of boron nitride particles. The boron nitride container was then cooled to room temperature, and the contents of the boron nitride container were removed. 5 g of the contents of the boron nitride container, 22 mL of distilled water, and 10 mL of 60% nitric acid were placed in a beaker, and the contents of the beaker were stirred using a stirrer for 1 hour to dissolve the trilithium borate in the contents of the boron nitride container with dilute nitric acid. Then, boron nitride primary particles were extracted from the contents of the beaker by suction filtration. The extracted boron nitride primary particles were dried at a drying temperature of 100°C for 2 hours to obtain boron nitride primary particles 1. A scanning electron microscope photograph of the obtained boron nitride primary particles 1 is shown in Figure 2.

[0075] (Preparation of Boron Nitride Primary Particles 2) A mixture was prepared so that the molar ratio of amorphous boron nitride and trilithium borate (LiBO) was 2:1, calculated as boron nitride (BN) and trilithium borate, and boron nitride primary particles 2 were prepared in the same manner as the preparation of boron nitride primary particles 1, except that the melting temperature was 1500°C.

[0076] (Preparation of Boron Nitride Primary Particles 3) Boron nitride primary particles 3 were prepared in the same manner as the preparation of boron nitride primary particles 1, except that a mixture was prepared so that the molar ratio of amorphous boron nitride and trilithium borate (LiBO) was 1:1, calculated as boron nitride (BN) and trilithium borate, and the mixture was melted for 1 hour.

[0077] (Preparation of Boron Nitride Primary Particles 4) Boron nitride primary particles 4 were prepared in the same manner as the preparation of boron nitride primary particles 1, except that a mixture was prepared so that the molar ratio of amorphous boron nitride and trilithium borate (LiBO) was 10:1, calculated as boron nitride (BN) and trilithium borate, and the mixture was melted at 1500°C.

[0078] (Preparation of Boron Nitride Primary Particles 5) Boron nitride primary particles 5 were prepared in the same manner as the preparation of boron nitride primary particles 1, except that a mixture of amorphous boron nitride and trilithium borate (LiBO) was prepared so that the molar ratio of boron nitride (BN) to trilithium borate was 1:1, and the mixture was melted at 1100°C for 20 hours.

[0079] (Preparation of Boron Nitride Primary Particles 6) Scaly boron nitride primary particles (manufactured by Denka Co., Ltd., trade name "SP3-7") were used as the boron nitride primary particles.

[0080] (Major axis length and aspect ratio of boron nitride primary particles) The major axis length and aspect ratio of the obtained boron nitride primary particles were measured as follows. Using a scanning electron microscope (manufactured by JEOL Ltd., product name "JSM-7001F"), the length in the thickness direction and the maximum length in the plane direction (major axis length) of 100 arbitrarily selected boron nitride primary particles were measured. These average values ​​were then taken as the length in the thickness direction (T) and the maximum length in the plane direction (major axis length) (F). The aspect ratio (F / T) was calculated from the results.

[0081] [Preparation of Dispersant] The following raw materials were used to prepare the dispersant. ((Meth)acrylic monomer A having an anionic group) (A-1) acrylic acid, manufactured by Toagosei Co., Ltd. ((Meth)acrylic monomer B having a cationic group) (B-1) 1,2,2,6,6-pentamethyl-4-piperidyl methacrylate, "ADEKA STAB LA-82" manufactured by ADEKA Corporation ((Meth)acrylic monomer C) (C-1) α-butyl-ω-(3-methacryloxypropyl)polydimethylsiloxane, "Silaplane FM-0721" manufactured by JNC Corporation, weight average molecular weight 5,000

[0082] The dispersant was prepared by the following method. First, 100 parts by mass of a (meth)acrylic monomer consisting of 48.4 mol% acrylic acid, 1.6 mol% 1,2,2,6,6-pentamethyl-4-piperidyl methacrylate, and 50.0 mol% α-butyl-ω-(3-methacryloxypropyl)polydimethylsiloxane (weight average molecular weight 5,000) was added to an autoclave equipped with a stirrer. Next, 0.05 parts by mass of azobisisobutyronitrile (manufactured by Tokyo Chemical Industry Co., Ltd.) was added as an initiator relative to 100 parts by mass of the total (meth)acrylic monomer, and 1,000 parts by mass of a mixed solution of toluene (special reagent grade) and 2-propanol (special reagent grade) in a volume ratio of 7:3 was added as a solvent, and the atmosphere inside the autoclave was replaced with nitrogen. Thereafter, the autoclave was heated in an oil bath at 65°C for 20 hours, and radical polymerization was carried out. After the polymerization was completed, the mixture was degassed under reduced pressure at 120°C for 1 hour to obtain a dispersant. Note that since the weight average molecular weight of α-butyl-ω-(3-methacryloxypropyl)polydimethylsiloxane was 5,000, the weight average molecular weight of unit C was 5,000.

[0083] The polymerization rate relative to 100% of the dispersant charge was analyzed by gas chromatography and found to be 98% or more. From this, it was estimated that the ratio of each monomer unit contained in the dispersant was approximately the same as the charge ratio of the dispersant.

[0084] The weight-average molecular weight of the resulting dispersant was determined as a weight-average molecular weight converted into standard polystyrene using GPC (gel permeation chromatography). The measurement conditions were as follows: High-speed GPC apparatus: "HLC-8020" manufactured by Tosoh Corporation Column: One "TSK guard column MP (xL)" manufactured by Tosoh Corporation, 6.0 mm ID x 4.0 cm, and two "TSK-GELMULTIPORE HXL-M" manufactured by Tosoh Corporation, 7.8 mm ID x 30.0 cm (theoretical plate number: 16,000), for a total of three (total theoretical plate number: 32,000) Developing solvent: tetrahydrofuran Detector: RI (differential refractometer)

[0085] The dispersant compositions shown in Table 1 are expressed as molar ratios (%) calculated from the amounts and molecular weights of the individual monomers. The molar ratio of α-butyl-ω-(3-methacryloxypropyl)polydimethylsiloxane was calculated based on the weight-average molecular weight.

[0086] The compositions and weight average molecular weights of the dispersants synthesized as above are shown in Table 1 below.

[0087] <Preparation of Thermally Conductive Grease> (Example 1) Boron nitride primary particles 1, thermally conductive filler, liquid polymer, and dispersant were weighed and added to a universal mixer so that the proportion of boron nitride primary particles 1 was 10 volume %, the proportion of thermally conductive filler was 72 volume %, the proportion of liquid polymer was 14 volume %, and the proportion of dispersant was 4 volume %. The mixture was then vacuum mixed in the universal mixer to prepare the thermally conductive grease of Example 1. The evaluation results of the obtained thermally conductive grease are shown in Table 2.

[0088] (Examples 2 to 7 and Comparative Examples 1 to 3) Thermal greases of Examples 2 to 7 and Comparative Examples 1 to 3 were prepared in the same manner as the thermal grease of Example 1, except that the type and content of the boron nitride primary particles, the content of the thermally conductive filler, etc. were changed to those shown in Table 2. The evaluation results of the obtained thermally conductive greases are shown in Table 2.

[0089] The thermal grease was evaluated by the following method. (Viscosity) Using a rotational rheometer MARS III manufactured by Thermo Scientific, a 35 mm diameter parallel plate was used as the upper jig, and the thermal grease was placed on a 35 mm diameter lower plate whose temperature could be controlled by a Peltier element. The grease was compressed to a thickness of 0.5 mm by the upper jig, and any excess was scraped off. Measurement was performed at 25°C. Shear rates were 0.1 to 100 s -1 The viscosity was measured at a shear rate of 1 s -1 The viscosity of the liquid polymer was also measured in the same manner.

[0090] (Interfacial Thermal Resistance and Internal Thermal Resistance) The thermal resistance of the thermal grease was measured using a resin material thermal resistance measuring device (manufactured by Hitachi Technology and Services Co., Ltd.) while varying the thickness of the thermal grease. The obtained data on the thickness (x) (mm) and thermal resistance (y) (K / W) of the thermal grease were then approximated to a linear equation of y = ax + b using the least squares method. The value of b was then defined as the interfacial thermal resistance (K / W), and the value of ax (K / W) when the value of x was 1 mm was defined as the internal thermal resistance.

[0091] (Thermal Conductivity) The reciprocal of the internal resistance was taken as the thermal conductivity.

[0092]

[0093]

[0094] In the thermal greases of Examples 1 to 7, the aspect ratio of the boron nitride primary particles was within the range of 0.3 to 9, so the interfacial thermal resistance of the thermal grease was low. In the thermal grease of Comparative Example 1, the aspect ratio of the boron nitride primary particles was smaller than 0.3, so the viscosity of the thermal sheet was high and it did not become a paste. As a result, it was impossible to measure the thermal conductivity, interfacial thermal resistance, and internal thermal resistance. The thermal grease of Comparative Example 2 did not contain boron nitride primary particles, so the thermal conductivity was low and, as a result, the interfacial thermal resistance was high.

Claims

1. A thermal grease comprising primary particles of boron nitride, the primary particles of boron nitride having an aspect ratio of 0.3 to 9.

2. The thermal grease according to claim 1, wherein the major axis length of the primary particles of boron nitride is 0.5 to 20 μm.

3. The thermal grease according to claim 1 or 2, further comprising a thermally conductive filler different from the boron nitride primary particles, the thermally conductive filler comprising a spherical filler.

Citation Information

Patent Citations

  • Phase change heat-conducting thermal silicone grease composition for central processing unit (CPU) radiating and preparation method thereof

    CN103214848A

  • Insulating and heat-conducting silicone grease and preparation method thereof

    CN103709757A

  • High thermal conductive grease composition and cooling apparatus using the same

    JP2002201483A

  • Thermal conductive grease

    JP2006188638A

  • Heat-conductive grease composition

    JP2007106809A