Ceramic sintered compact and telescope

The ceramic sintered body with cordierite and spinel crystals addresses the challenges of temperature control and mechanical properties in cordierite ceramics, enabling their broader application by controlling the zero cross temperature and enhancing mechanical and electrical properties, thus reducing costs and complexity in space and other fields.

WO2024204422A1PCT designated stage expired Publication Date: 2024-10-03KYOCERA CORP

Patent Information

Application Number
PCT/JP2024/012404
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-30
Filing Date
2024-03-27
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Conventional cordierite ceramics used in applications requiring low thermal expansion face challenges such as increased manufacturing costs, weight, and power consumption due to strict temperature control requirements, especially in space applications, where temperature adjustments are necessary to maintain the zero cross temperature (ZCT) near room temperature.

Method used

A ceramic sintered body composed of cordierite crystals and spinel crystals with a total content of 95% by mass or more, where the spinel crystal content is between 0.1% and 17% by mass, allowing for controlled ZCT within the range of -120°C to 45°C, reducing the need for strict temperature adjustments and enhancing mechanical properties like specific stiffness and dielectric constants.

Benefits of technology

This configuration enables the application of cordierite ceramics in various fields, including space, by minimizing dimensional changes, reducing launch costs, and improving mechanical strength and reliability, while maintaining a low dielectric constant and reducing signal delay in high-frequency circuits.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JPOXMLDOC01-APPB-T000001
    Figure JPOXMLDOC01-APPB-T000001
  • Figure JPOXMLDOC01-APPB-T000002
    Figure JPOXMLDOC01-APPB-T000002
  • Figure JPOXMLDOC01-APPB-T000003
    Figure JPOXMLDOC01-APPB-T000003
Patent Text Reader

Abstract

This ceramic sintered compact comprises cordierite crystals and spinel crystals. Moreover, the total content of the cordierite crystals and the spinel crystals is 95 mass% or greater. Furthermore, the spinel crystal content is 0.1-17 mass%.
Need to check novelty before this filing date? Find Prior Art

Description

Sintered ceramic body and telescope

[0001] The disclosed embodiments relate to a ceramic sintered body and a telescope.

[0002] In recent years, ceramic members having low thermal expansion have been applied to devices in various fields, and cordierite ceramics have been attracting attention as such low thermal expansion ceramics (see, for example, Patent Document 1).

[0003] Japanese Patent Application Laid-Open No. 2016-204198

[0004] A ceramic sintered body according to one aspect of the present invention contains cordierite crystals and spinel crystals, the total content of the cordierite crystals and the spinel crystals being 95 mass% or more, and the content of the spinel crystals being 0.1 mass% or more and 17 mass% or less.

[0005] Hereinafter, embodiments of the ceramic sintered body and the telescope disclosed in the present application will be described. Note that the present disclosure is not limited to the embodiments described below.

[0006] In recent years, ceramic members having low thermal expansion have been applied to devices in various fields, and cordierite ceramics have been attracting attention as such low thermal expansion ceramics.

[0007] However, the above-mentioned conventional techniques leave room for further improvement in terms of applying cordierite ceramics to various fields, and therefore, it is desired to realize a ceramic sintered body that can solve the above-mentioned problems and be applicable to various fields.

[0008] It is known that the temperature dependence of the thermal expansion coefficient of cordierite ceramics exhibits a linear relationship from −100° C. or lower to near room temperature. In conventional cordierite ceramics, the zero cross temperature of the thermal expansion coefficient is near room temperature, for example, near 22° C. In the present disclosure, the zero cross temperature of the thermal expansion coefficient is also referred to as "ZCT."

[0009] Cordierite ceramics have traditionally been used in components that must be protected from dimensional changes due to temperature changes, such as components for semiconductor exposure devices and optical components such as telescope mirrors. For such components that must be protected from dimensional changes due to temperature changes, low-thermal expansion glass, for example, has been used.

[0010] However, the low expansion glass has a small Young's modulus of 100 GPa or less, and a specific rigidity, which is the value obtained by dividing the Young's modulus by the specific gravity, of 30 GPa / g / cm 3 Because the glass is low, there was concern that if it were to be used for a satellite mirror, for example, it could be broken by the impact during launch if it were made thin. Furthermore, if the low-expansion glass was made thicker to ensure strength, there was also the issue of the weight increasing during launch.

[0011] To address this issue, cordierite ceramics have a large Young's modulus of approximately 140 GPa and a specific rigidity of 55 GPa / g / cm 3 Since the expansion coefficient is about the same as that of low-expansion glass, it is possible to make thinner components compared to low-expansion glass, which allows for lighter devices. This has attracted attention in recent years because it has the great advantage of reducing launch costs for devices launched into space.

[0012] On the other hand, cordierite ceramics have a greater temperature dependency of the thermal expansion coefficient than low-expansion glass, so when utilizing the zero expansion property, it is necessary to use them at temperatures near the ZCT.

[0013] For this reason, when cordierite ceramics are applied to components mounted on artificial satellites, for example, it is necessary to adjust the temperature inside the device in order to maintain the temperature of the components at around 22°C, which is the ZCT, and particularly strict temperature control is required around the applied components.

[0014] Therefore, if cordierite ceramics are used in multiple components, temperature control for each component is required, making equipment design complicated. This leads to issues such as increased manufacturing costs, increased weight due to the addition of additional equipment, and increased power consumption in spacecraft with limited power sources.

[0015] One possible solution to this problem is to control the ZCT of the cordierite ceramics in accordance with the temperature at which the device is used.

[0016] The ceramic sintered body according to the embodiment may contain cordierite crystals and spinel crystals. The total content of the cordierite crystals and the spinel crystals may be 95 mass% or more. The content of the spinel crystals may be 0.1 mass% or more and 17 mass% or less.

[0017] With this configuration, it is possible to control the ZCT of the cordierite-based ceramic within the range of -120°C to 45°C. Therefore, according to the embodiment, the cordierite-based ceramic can be applied to various fields, including the space field. Furthermore, it is possible to provide cordierite-based ceramics having the required ZCT as desired.

[0018] Furthermore, the ceramic sintered body according to the embodiment may have a spinel crystal content of 5 mass % or less. When the amount of spinel crystal, which has a higher dielectric constant than cordierite crystal, is 5 mass % or less, a cordierite ceramic having a relatively low dielectric constant can be provided.

[0019] Furthermore, the ceramic sintered body according to the embodiment may have a cordierite crystal content of 90 mass % or more. When the amount of cordierite crystals, which have a lower dielectric constant than spinel crystals, is 90 mass % or more, a cordierite ceramic having a relatively low dielectric constant can be provided.

[0020] Furthermore, in the ceramic sintered body according to the embodiment, when crystals other than cordierite crystals and spinel crystals are detected in Rietveld analysis of an X-ray diffraction pattern, the total amount of such crystals may be 3 mass% or less.

[0021] When the precipitation amount of crystalline phases other than cordierite and spinel is 3 mass% or less, the firing temperature dependence of ZCT is relatively small, and a sintered body with the desired ZCT can be easily produced. In particular, in the case of a large-sized sintered body, a temperature difference occurs during firing between the outer periphery and the center of the sintered body, so it is desirable to set the precipitation amount of crystalline phases other than cordierite and spinel to 3 mass% or less.

[0022] Furthermore, when the ZCT is taken as the reference temperature, the ceramic sintered body according to the embodiment may have a thermal expansion coefficient within 0±1 ppb / K in a temperature range from the reference temperature −1 K to the reference temperature +1 K. This reduces dimensional changes of the ceramic sintered body near the ZCT.

[0023] Furthermore, the ceramic sintered body according to the embodiment may have a ZCT of not less than −100° C. and not more than 35° C. This makes the ceramic sintered body applicable to various fields, including the space field.

[0024] Furthermore, the ceramic sintered body according to the embodiment may have a relative dielectric constant at a measurement frequency of 10 GHz of not less than 4 and not more than 5. With such a configuration, for example, when the ceramic sintered body according to the present disclosure is used as a substrate for a high-frequency circuit, signal delay can be reduced.

[0025] Furthermore, the ceramic sintered body according to the embodiment has a specific gravity of 2.8 g / cm 3 This makes it possible to reduce launch costs when cordierite ceramics are applied to the space field.

[0026] Furthermore, the ceramic sintered body according to the embodiment has a specific rigidity of 50 GPa / g / cm 3 This makes it possible to reduce launch costs when cordierite ceramics are applied to the space field.

[0027] Furthermore, the ceramic sintered body according to the embodiment may be substantially free of mullite crystals, which can reduce the surface roughness after processing, making it suitable for use as an optical component such as a reflecting mirror component.

[0028] The ceramic sintered body according to the embodiment may be dense. With such a structure, the ceramic sintered body has excellent strength. Furthermore, in the embodiment, the ceramic sintered body may have a water absorption rate of 0.05% or less. With such a structure, the surface can be mirror-finished with minimal irregularities.

[0029] Furthermore, it is important that the ceramic sintered body according to the embodiment maintains homogeneity within the sintered body, which means that the CTE (coefficient of thermal expansion) and ZCT variations at various locations within the sintered body are small. For example, the CTE variation within a reflective mirror member used in the astronomy and space fields may be homogeneous such that the ZCT variation is within ±1°C.

[0030] Furthermore, the telescope according to the embodiment may have the ceramic sintered body described above as a mirror component. Furthermore, the telescope according to the embodiment may have the ceramic sintered body described above as a support member that directly or indirectly supports the mirror component. Furthermore, the telescope according to the embodiment may have the ceramic sintered body described above as a mirror component and a support member that directly or indirectly supports the mirror component.

[0031] As a result, in a space astronomical telescope, even if the speed of optical axis adjustment is increased, vibrations caused by inertia can be reduced. Therefore, according to the embodiment, it is possible to increase the speed of optical axis adjustment. In addition, vibration damping is improved throughout the device. Furthermore, due to its high mechanical strength, it has excellent long-term reliability. Furthermore, due to its light weight and high rigidity, launch costs are reduced.

[0032] Next, the cordierite ceramics of this embodiment were specifically produced and their properties were evaluated. First, magnesium hydroxide (Mg(OH) 2 ), alumina and silicon dioxide powders were prepared.

[0033] In addition, as the raw material powder, Mg 2 Al 4 Si 5 O18 A powder of synthetic cordierite raw material represented by the formula (I) was prepared, and a powder of calcium carbonate was also prepared. The purity of the prepared magnesium hydroxide powder was 99.3%, the purity of the prepared alumina powder was 99.9%, the purity of the prepared silicon dioxide powder was 99.5%, and the purity of the prepared calcium carbonate powder was 99.5%.

[0034] Next, magnesium hydroxide powder, alumina powder, and silicon dioxide powder were mixed together to form a mixture of MgO:Al 2 O 3 : SiO 2 were mixed at a molar ratio of 2:2.4:5 to 3:2.4:5 to prepare a plurality of types of raw material mixed powders.

[0035] Next, the synthetic cordierite raw material powder and the raw material mixture powder were mixed in a mass ratio of 70:30. Furthermore, calcium carbonate was added externally in an amount of 0.892 mass%, and a binder, such as paraffin wax, was added to the mixture to prepare several types of granulated powders.

[0036] Next, the prepared multiple types of granulated powder were press-molded to produce multiple types of cylindrical molded bodies with a diameter of 150 mm and a height of 100 mm, and these molded bodies were fired in the air to produce cordierite ceramic samples No. 1 to 39. The firing temperature for each sample was 1375°C, and the holding time at this firing temperature was 7 hours.

[0037] The composition of each of the prepared samples was determined by ICP emission spectrometry, and it was found that the composition of each sample was identical to the compounded composition.

[0038] Next, the following evaluations were carried out on the prepared samples Nos. 1 to 39. The identification of the crystalline phase and the measurement of the proportion of the crystalline phase were carried out by powder X-ray diffraction and the Rietveld method. This measurement was carried out on one sample for each.

[0039] The thermal expansion characteristics were measured using an optical heterodyne interferometer in the temperature range of -100°C to 50°C, with the dimensions at 22°C as the reference. The temperature dependence of the thermal expansion coefficient was then determined from the measured data, and the temperature at which the thermal expansion coefficient showed zero was defined as the ZCT.

[0040] Furthermore, the ZCT of each sample obtained by the above method was used as the reference temperature, and the thermal expansion coefficient of each sample was measured in the temperature range from the reference temperature −1 K to the reference temperature +1 K, and the obtained thermal expansion coefficient was defined as the thermal expansion coefficient of each sample near the ZCT (CTE at ZCT).

[0041] The bulk density and water absorption were measured by the Archimedes method. The water absorption was 0.0% for all samples. The Young's modulus was measured by the ultrasonic resonance method. The size of the samples used for the measurement was 10 mm in diameter and 5 mm in height. The specific rigidity was calculated by dividing the Young's modulus by the bulk density.

[0042] Thermal conductivity was measured by the laser flash method. Flexural strength was measured by machining test pieces from each sample according to JIS R 1601 and measuring the four-point bending strength. Fracture toughness was measured according to the indenter method of JIS R 1607-1995.

[0043] The void fraction was measured using the following procedure. First, the cross section of each sample was mirror-polished. Next, the percentage of the area occupied by void openings in the measurement region of this cross section (area %) was calculated. This percentage was then regarded as the void fraction (volume %), and the void fraction of each sample was calculated.

[0044] The relative dielectric constant was measured at a measurement frequency of 10 GHz by the dielectric cylindrical resonator method (International Standard IEC61338-1-3 (1999)).

[0045] Here, for Samples No. 1 to 39, the measurement results of the total cordierite crystal content and spinel crystal content, the cordierite crystal content, the spinel crystal content, the ZCT, the thermal expansion coefficient near the ZCT, the bulk density, Young's modulus, the specific rigidity, the thermal conductivity, the flexural strength, the fracture toughness, the void fraction, and the relative dielectric constant are shown in Tables 1 and 2. Note that the mass % of "other crystals" in Tables 1 and 2 refers to the mass % of only crystals other than cordierite crystals and spinel crystals, and does not include the mass of glassy materials. Examples of other crystals include enstatite and forsterite.

[0046]

[0047]

[0048] As shown in Tables 1 and 2, when the total content of cordierite crystals and the content of spinel crystals is 95 mass% or more and the content of spinel crystals is 0.1 mass% or more and 17 mass% or less, the ZCT can be controlled within a range of −120° C. to 45° C. Therefore, in the embodiment, it is possible to solve the above-mentioned problems.

[0049] Furthermore, as shown in Tables 1 and 2, when the total content of cordierite crystals and the content of spinel crystals is 95 mass% or more and the content of spinel crystals is 0.1 mass% or more and 9 mass% or less, the ZCT can be controlled within a range of -30°C to 45°C. Therefore, in the embodiment, it is possible to solve the above-mentioned problems.

[0050] As shown in Tables 1 and 2, the specific rigidity of all the samples was 55 GPa / g / cm 3 The above-mentioned sample allows the components to be thinner than low-expansion glass, and the device can be made lighter.

[0051] The ZCT was measured for each sample shown in Tables 1 and 2. The values ​​are shown in the ZCT (1) column in Table 3 below. The ZCT of a sample fired at a temperature 50°C higher than the firing temperature was also measured. This temperature is shown as ZCT (2) in Table 3. The difference between ZCT (1) and ZCT (2) is also shown in Table 3. The smaller this difference, the smaller the change in ZCT due to firing temperature.

[0052]

[0053] Although the embodiments of the present disclosure have been described above, the present disclosure is not limited to the above-described embodiments, and various modifications are possible without departing from the spirit of the present disclosure.

[0054] The embodiments disclosed herein should be considered to be illustrative in all respects and not restrictive. Indeed, the above-described embodiments may be embodied in various forms. Furthermore, the above-described embodiments may be omitted, substituted, or modified in various ways without departing from the scope and spirit of the appended claims.

[0055] The present technology can also be configured as follows: (1) A ceramic sintered body containing cordierite crystals and spinel crystals, wherein the total content of the cordierite crystals and the spinel crystals is 95 mass% or more, and the content of the spinel crystals is 0.1 mass% or more and 17 mass% or less. (2) The ceramic sintered body according to (1), wherein the content of the spinel crystals is 5 mass% or less. (3) The ceramic sintered body according to (1) or (2), wherein the content of the cordierite crystals is 90 mass% or more. (4) The ceramic sintered body according to any one of (1) to (3), wherein, when crystals other than the cordierite crystals and the spinel crystals are detected in a Rietveld analysis of an X-ray diffraction pattern, the total amount of the other crystals is 3 mass% or less. (5) The ceramic sintered body according to any one of (1) to (4), wherein, when the zero cross temperature of the thermal expansion coefficient is taken as a reference temperature, the thermal expansion coefficient in the temperature range of the reference temperature -1K to the reference temperature +1K is within 0±1 ppb / K. (6) The ceramic sintered body according to any one of (1) to (5), wherein the zero cross temperature of the thermal expansion coefficient is -100°C or more and 35°C or less. (7) The ceramic sintered body according to any one of (1) to (6), wherein the relative dielectric constant at a measurement frequency of 10 GHz is 4 or more and 5 or less. (8) The specific gravity is 2.8 g / cm 3 (9) The ceramic sintered body according to any one of (1) to (7), wherein the specific rigidity is 50 GPa / g / cm or less. 3The ceramic sintered body according to any one of (1) to (8) above. (10) A telescope having the ceramic sintered body according to any one of (1) to (9) above as a mirror component. (11) A telescope having the ceramic sintered body according to any one of (1) to (9) above as a support member that directly or indirectly supports a mirror component. (12) A telescope having the ceramic sintered body according to any one of (1) to (9) above as a mirror component and a support member that directly or indirectly supports the mirror component.

Claims

1. A ceramic sintered body containing cordierite crystals and spinel crystals, wherein the sum of the content of the cordierite crystals and the content of the spinel crystals is 95 mass% or more, and the content of the spinel crystals is 0.1 mass% or more and 17 mass% or less.

2. The ceramic sintered body according to claim 1, wherein the content of the spinel crystal is 5 mass% or less.

3. The ceramic sintered body according to claim 1 or 2, wherein the content of the cordierite crystals is 90 mass% or more.

4. The ceramic sintered body according to any one of claims 1 to 3, wherein when crystals other than the cordierite crystals and the spinel crystals are detected in a Rietveld analysis of an X-ray diffraction pattern, the total amount of the other crystals is 3 mass% or less.

5. A ceramic sintered body according to any one of claims 1 to 4, wherein, when the zero cross temperature of the thermal expansion coefficient is taken as a reference temperature, the thermal expansion coefficient in the temperature range from said reference temperature -1K to said reference temperature +1K is within 0±1 ppb / K.

6. The ceramic sintered body according to any one of claims 1 to 5, wherein the zero cross temperature of the thermal expansion coefficient is -100°C or higher and 35°C or lower.

7. The ceramic sintered body according to any one of claims 1 to 6, wherein the relative dielectric constant at a measurement frequency of 10 GHz is 4 or more and 5 or less.

8. Specific gravity is 2.8 g / cm 3 The ceramic sintered body according to any one of claims 1 to 7, wherein:

9. Specific rigidity is 50 GPa / g / cm 3 The ceramic sintered body according to any one of claims 1 to 8.

10. A telescope having a mirror part made of the ceramic sintered body according to any one of claims 1 to 9.

11. A telescope having the ceramic sintered body according to any one of claims 1 to 9 as a support member for directly or indirectly supporting a mirror component.

12. A telescope comprising the ceramic sintered body according to any one of claims 1 to 9 as a mirror component and a supporting member for directly or indirectly supporting the mirror component.

Citation Information

Patent Citations

  • Cordierite sintered body

    JP2016204198A

  • Cordierite-based sintered body

    WO2010087099A1

  • Cordierite ceramic, and member for semiconductor manufacture devices which comprises same

    WO2012057215A1

  • Cordierite sintered body

    WO2016170953A1