Transfer film, electromagnetic wave shield film provided with transfer film, and shield printed wiring board
The transfer film with a 1.2 μm or less protruding peak height on its surface addresses the adhesion and hiding power trade-off, ensuring effective peeling and reduced glossiness in electromagnetic shielding films, enhancing both releasability and hiding performance.
Patent Information
- Application Number
- PCT/JP2024/012564
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-30
- Filing Date
- 2024-03-28
- Publication Date
- 2024-10-03
AI Technical Summary
Conventional transfer films with uneven surfaces for reducing glossiness in protective layers of electromagnetic shielding films face challenges in peeling off without leaving part of the protective layer attached, leading to a trade-off between reducing adhesion and achieving sufficient hiding power.
A transfer film with a first main surface featuring an uneven shape where the protruding peak height Spk is 1.2 μm or less, improving releasability and reducing glossiness by scattering light, thereby preventing anchor effects and ensuring easy peeling without protective layer attachment.
The solution effectively lowers the glossiness of the protective layer while enhancing the peelability of the transfer film, allowing for successful peeling without protective layer remnants and achieving high hiding power.
Smart Images

Figure JP2024012564_03102024_PF_FP_ABST
Abstract
Description
Transfer film, electromagnetic wave shielding film with transfer film, and shielded printed wiring board
[0001] The present invention relates to a transfer film, an electromagnetic wave shielding film with a transfer film, and a shielded printed wiring board.
[0002] Flexible printed circuit boards are widely used to incorporate circuits into complex mechanisms in electronic devices such as mobile phones, video cameras, and laptops, which are rapidly becoming smaller and more functional. Furthermore, taking advantage of their excellent flexibility, they are also used to connect moving parts such as printer heads to control units.
[0003] Shielded printed wiring boards use electromagnetic wave shielding films. For example, an electromagnetic wave shielding film disposed on a printed wiring board includes a protective layer and a shielding layer made of a metal layer, a conductive adhesive layer, or the like laminated on the protective layer.
[0004] In recent years, in shielded printed wiring boards, the protective layer serving as the outermost layer of an electromagnetic wave shielding film laminated on the printed wiring board may be required to have low gloss in order to conceal the printed circuit formed on the printed wiring board. One method for reducing the gloss of the protective layer is to form an uneven shape on the outer main surface of the protective layer. One method for producing such a protective layer is to apply a resin composition for forming the protective layer to the uneven surface of a transfer film, followed by solidification to form the protective layer. This allows the uneven shape of the uneven surface of the transfer film to be transferred to the protective layer, thereby reducing the gloss of the protective layer. Conventionally, it has been believed that the glossiness of the uneven surface of the transfer film correlates with the glossiness of the protective layer to which the uneven shape is transferred, and an uneven shape has been formed to reduce the glossiness of the uneven surface of the transfer film.
[0005] As such a transfer film, Patent Document 1 discloses a biaxially oriented polyester film that is a laminated polyester film having a base layer and a particle-containing matte layer on at least one surface, wherein the matte layer surface has a center line average roughness (Ra) of 400 to 1000 nm, a 10-point average roughness (Rz) of 4000 to 8000 nm, a glossiness (G60) of 6 to 20, a void breaking rate of protrusions on the surface of 20% or less, and a hue L value of the base layer of 60 to 80.
[0006] JP 2017-71107 A
[0007] As disclosed in Patent Document 1, conventional transfer films having an uneven surface intended to impart hiding properties to a protective layer have a problem in that the anchor effect resulting from the uneven surface when laminated with the protective layer makes it difficult to peel the transfer film from the protective layer. Even when the transfer film can be peeled off, a portion of the protective layer remains attached to the transfer film. One possible method for preventing a portion of the protective layer from adhering to the transfer film is to shallow the unevenness formed on the transfer surface (reducing the glossiness of the transfer surface). However, if the unevenness formed on the transfer surface is shallow, the unevenness transferred to the protective layer also becomes shallow, resulting in an insufficient reduction in the glossiness of the protective layer and an insufficient increase in hiding properties. In other words, there is a trade-off between preventing a portion of the protective layer from adhering to the transfer film and improving the hiding properties of the protective layer.
[0008] The present invention has been made in consideration of the above-mentioned problems, and an object of the present invention is to provide a transfer film having a main surface on which a textured shape is formed, which can sufficiently reduce the glossiness of an object to be transferred having a textured shape, and which has sufficiently high releasability.
[0009] That is, the transfer film of the present invention is characterized by having a first main surface on which an uneven shape is formed, and the height Spk of the protruding peaks of the first main surface being 1.2 μm or less.
[0010] In the transfer film of the present invention, a transfer target having a textured surface is placed on the first main surface, and the textured surface is transferred. The transfer target having the textured surface tends to scatter light. Therefore, the glossiness of the transfer target having the textured surface of the first main surface can be reduced.
[0011] The peak height Spk is a parameter defined in ISO 25178, and means the average height of predetermined protrusions among the convex portions of the uneven shape.
[0012] When the height Spk of the protruding peaks of the first main surface is 1.2 μm or less, the anchor effect is less likely to occur, and the peelability of the transfer film is improved.
[0013] In other words, when the height Spk of the protruding peaks of the first main surface is 1.2 μm or less, it is possible to achieve both the effect of reducing the glossiness of the transferred object to which the uneven shape of the first main surface is transferred, and the effect of improving the releasability of the transfer film.
[0014] In the transfer film of the present invention, the minimum autocorrelation length Sal of the first principal surface is preferably 6 μm or less. The minimum autocorrelation length Sal is a parameter defined in ISO 25178 and represents the shortest distance in the direction in which the autocorrelation function decays to a specific value. When Sal is small, a steeply inclined uneven shape predominates, while when Sal is large, a gently inclined uneven shape predominates. When the minimum autocorrelation length Sal of the first principal surface is 6 μm or less, the releasability of the transfer film tends to be improved. Furthermore, light is easily scattered in a transfer target to which the uneven shape of the first principal surface has been transferred. Therefore, the glossiness of the transfer target to which the uneven shape of the first principal surface has been transferred can be reduced.
[0015] In the transfer film of the present invention, the transfer film may include a resin and a filler, and the uneven shape may be formed by the filler protruding from the first main surface. Such a transfer film can be easily produced by kneading the filler into the resin that is the material of the transfer film during production.
[0016] The electromagnetic wave shielding film with transfer film of the present invention is an electromagnetic wave shielding film with transfer film comprising: an electromagnetic wave shielding film including a protective layer and a shielding layer laminated on the protective layer; and a transfer film having a first main surface on which an uneven shape is formed and arranged so that the first main surface is in contact with the protective layer, and is characterized in that the height Spk of the protruding peaks of the first main surface is 1.2 μm or less.
[0017] In the electromagnetic wave shielding film with a transfer film of the present invention, the transfer film is peeled off during use. In the electromagnetic wave shielding film with a transfer film of the present invention, the protective layer of the electromagnetic wave shielding film and the first main surface of the transfer film are in contact with each other, so the uneven shape of the first main surface of the transfer film is transferred to the protective layer of the electromagnetic wave shielding film. The protective layer to which the uneven shape has been transferred tends to scatter light. This makes it possible to reduce the glossiness of the protective layer of the electromagnetic wave shielding film.
[0018] In the electromagnetic wave shielding film with transfer film of the present invention, the protruding peak height Spk of the first main surface of the transfer film is 1.2 μm or less. Therefore, an anchor effect is unlikely to occur between the transfer film and the protective layer of the electromagnetic wave shielding film. As a result, the releasability of the transfer film is improved, and when the transfer film is peeled from the electromagnetic wave shielding film, it is possible to prevent a part of the protective layer from peeling off while remaining attached to the transfer film.
[0019] In the electromagnetic wave shielding film with a transfer film of the present invention, the shielding layer may be a metal layer, and an adhesive layer may be further laminated on the surface of the shielding layer opposite to the surface on the protective layer side. Furthermore, in the electromagnetic wave shielding film with a transfer film of the present invention, the shielding layer may be an isotropically conductive adhesive layer. Whether the shielding layer is a metal layer or a conductive adhesive layer, it can provide suitable shielding of electromagnetic waves.
[0020] The shielded printed wiring board of the present invention is a shielded printed wiring board comprising: a base film, a printed circuit including a ground circuit arranged on the base film, a cover lay covering the printed circuit, an electromagnetic wave shielding film including a protective layer and a shielding layer laminated on the protective layer, the electromagnetic wave shielding film being arranged so that the shielding layer is located on the printed wiring board side, and a transfer film having a first main surface on which an uneven shape is formed and being arranged so that the first main surface is in contact with the protective layer, and is characterized in that the protruding peak height Spk of the first main surface is 1.2 μm or less.
[0021] In the shielded printed wiring board of the present invention, the transfer film is peeled off during use. In the shielded printed wiring board of the present invention, the protective layer of the electromagnetic wave shielding film and the first main surface of the transfer film are in contact with each other, so the uneven shape of the first main surface of the transfer film is transferred to the protective layer of the electromagnetic wave shielding film. This allows the glossiness of the protective layer of the electromagnetic wave shielding film to be reduced. As a result, the printed circuit of the printed wiring board can be suitably concealed.
[0022] In the shielded printed wiring board of the present invention, the height Spk of the protruding peaks on the first main surface of the transfer film is 1.2 μm or less. This makes it difficult for an anchor effect to occur between the transfer film and the protective layer of the electromagnetic wave shielding film. As a result, the releasability of the transfer film is improved, and when the transfer film is peeled from the electromagnetic wave shielding film, it is possible to prevent a portion of the protective layer from peeling off while remaining attached to the transfer film.
[0023] According to the present invention, it is possible to provide a transfer film having a main surface on which an uneven shape is formed, which can sufficiently reduce the gloss of an object to be transferred having an uneven shape, and which has sufficiently high releasability.
[0024] FIG. 1 is a cross-sectional view schematically showing an example of an electromagnetic wave shielding film with a transfer film according to a first embodiment of the present invention. FIG. 2 is a cross-sectional view schematically showing an example of a transfer film according to the first embodiment of the present invention. FIG. 3 is a schematic view showing an example of a transfer film preparation step in the method for manufacturing an electromagnetic wave shielding film with a transfer film according to the first embodiment of the present invention. FIG. 4 is a schematic view showing an example of a protective layer formation step in the method for manufacturing an electromagnetic wave shielding film with a transfer film according to the first embodiment of the present invention. FIG. 5 is a schematic view showing an example of a shielding layer formation step in the method for manufacturing an electromagnetic wave shielding film with a transfer film according to the first embodiment of the present invention. FIG. 6 is a schematic view showing an example of an adhesive layer formation step in the method for manufacturing an electromagnetic wave shielding film with a transfer film according to the first embodiment of the present invention. FIG. 7 is a cross-sectional view schematically showing an example of a shielded printed wiring board according to the first embodiment of the present invention. FIG. 8 is a cross-sectional view schematically showing an example of a state in which the transfer film is peeled off in the shielded printed wiring board according to the first embodiment of the present invention. FIG. 9 is a cross-sectional view schematically showing another example of an electromagnetic wave shielding film with a transfer film according to a second embodiment of the present invention.
[0025] The transfer film, the electromagnetic wave shielding film with the transfer film, and the printed wiring board of the present invention are specifically described below. However, the present invention is not limited to the following embodiments, and can be appropriately modified and applied within the scope of the present invention.
[0026] First Embodiment FIG. 1 is a cross-sectional view schematically showing an example of an electromagnetic wave shielding film with a transfer film according to a first embodiment of the present invention.
[0027] The electromagnetic wave shielding film 10 with transfer film shown in Figure 1 comprises an electromagnetic wave shielding film 20 in which a protective layer 21, a shielding layer 22, and an adhesive layer 23 are laminated in that order, and a transfer film 30 having a first main surface 30a on which an uneven shape 31 is formed and arranged so that the first main surface 30a is in contact with the protective layer 21.
[0028] When the electromagnetic wave shielding film 10 with a transfer film is used, the transfer film 30 is peeled off. In the electromagnetic wave shielding film 10 with a transfer film, the protective layer 21 of the electromagnetic wave shielding film 20 and the first main surface 30a of the transfer film 30 are in contact with each other, so the uneven shape 31 of the first main surface 30a of the transfer film 30 is transferred to the protective layer 21 of the electromagnetic wave shielding film 20. The protective layer 21 to which the uneven shape 31 has been transferred tends to scatter light. This makes it possible to reduce the glossiness of the protective layer 21 of the electromagnetic wave shielding film 20.
[0029] In the transfer film 30, the protruding peak height Spk of the first main surface 30a is 1.2 μm or less. The protruding peak height Spk of the first main surface 30a is preferably 0.35 to 1.2 μm, and more preferably 0.6 to 1.1 μm. When the protruding peak height Spk of the first main surface 30a is 1.2 μm or less, an anchor effect is less likely to occur between the transfer film 30 and the protective layer 21 of the electromagnetic wave shielding film 20. As a result, the releasability of the transfer film 30 is improved, and when the transfer film 30 is peeled from the electromagnetic wave shielding film 20, it is possible to prevent a portion of the protective layer 21 from remaining attached to the transfer film 30 while peeling. When the protruding peak height Spk is 0.35 μm or more, the transfer film 30 does not easily peel off during handling before processing of the electromagnetic wave shielding film 10 with the transfer film, and the transfer film 30 can be peeled from the electromagnetic wave shielding film 20 after processing of the electromagnetic wave shielding film 10 with the transfer film.
[0030] In this specification, surface condition parameters such as the protruding peak height Spk (such as "Smr2" and "Sal" described later) conform to ISO 25178 and can be measured using a confocal microscope (trade name "OPTELICS HYBRID", manufactured by Lasertec, 50x objective lens).
[0031] In the transfer film 30, the minimum autocorrelation length Sal of the first main surface 30a is preferably 6 μm or less. When the minimum autocorrelation length Sal of the first main surface 30a is 6 μm or less, the releasability of the transfer film 30 tends to be improved. Furthermore, in the protective layer 21 to which the concave-convex shape is transferred, light is easily scattered. Therefore, the glossiness of the protective layer 21 of the electromagnetic wave shielding film 20 can be reduced.
[0032] In the transfer film 30, the protruding peak height Spk of the first main surface 30a is preferably 1.2 μm or less, and the area load ratio Smr2 separating the valleys and cores of the first main surface 30a is preferably 89% or more. When the protruding peak height Spk of the first main surface 30a is 1.2 μm or less and the area load ratio Smr2 separating the valleys and cores of the first main surface 30a is 89% or more, it is predicted that few deep recesses will be formed on the first main surface 30a, thereby improving the releasability of the transfer film 30. Furthermore, the protective layer 21 to which the concave-convex shape 31 is transferred is prone to light scattering. This allows the glossiness of the protective layer 21 of the electromagnetic wave shielding film 20 to be reduced.
[0033] In the transfer film 30, the root-mean-square height Sq of the first main surface 30a is preferably 0.7 μm or less. In the transfer film 30, the aspect ratio Str of the surface texture of the first main surface 30a is preferably 0.8 or less. In the transfer film 30, the root-mean-square slope Sdq of the first main surface 30a is preferably greater than 0.92 and less than 2.0. In the transfer film 30, the developed area ratio Sdr of the interface of the first main surface 30a is preferably 28 to 150%. When the root-mean-square height Sq, aspect ratio Str of the surface texture, root-mean-square slope Sdq, and developed area ratio Sdr of the interface of the first main surface 30a are within the above ranges, the gloss of the protective layer 21 is low and the hiding power is improved.
[0034] In the transfer film-attached electromagnetic wave shielding film 10, when the transfer film 30 is peeled off, the 60° gloss of the release surface of the protective layer 21 of the electromagnetic wave shielding film 20 is preferably 5.0 or less, more preferably 0.1 to 5.0, and even more preferably 0.1 to 3.0. When the 60° gloss of the release surface of the protective layer 21 of the electromagnetic wave shielding film 20 is within the above range, it can be said that the concealing property is sufficiently high. Therefore, when the electromagnetic wave shielding film 20 is placed on a printed wiring board, it can suitably conceal the printed circuits formed on the printed wiring board.
[0035] In this specification, the "60° gloss" conforms to JIS Z8741 and can be measured using a Gardner Micro-Gloss (portable gloss meter, manufactured by BYK).
[0036] Hereinafter, each component of the electromagnetic wave shielding film with a transfer film of the present invention will be described.
[0037] (Transfer Film) Figure 2 is a cross-sectional view schematically showing an example of a transfer film according to the first embodiment of the present invention. The transfer film constituting the above-mentioned electromagnetic wave shielding film with transfer film is also the transfer film of the present invention. The transfer film 30 shown in Figure 2 has a first main surface 30a on which an uneven shape 31 is formed, and the protruding peak height Spk of the first main surface 30a is 1.2 µm or less. The preferred surface condition of the first main surface 30a of the transfer film 30 has already been described, so a description thereof will be omitted here.
[0038] The configuration of the transfer film 30 is not particularly limited, but may be composed of only a resin layer, or may be composed of a resin layer laminated on a substrate layer. When the transfer film 30 is composed of a resin layer laminated on a substrate layer, the surface opposite to the surface of the resin layer on the substrate side becomes the first main surface.
[0039] Examples of the substrate layer include plastic substrates (particularly plastic films), porous materials such as paper, cloth, and nonwoven fabric, nets, foam sheets, and metal foils. The substrate layer may be a single layer or a laminate of the same or different substrates. The surface of the substrate layer may be subjected to a surface treatment such as a physical treatment such as corona discharge treatment or plasma treatment, or a chemical treatment such as a primer treatment.
[0040] Examples of resins constituting the plastic substrate include polyolefin resins such as low-density polyethylene, linear low-density polyethylene, medium-density polyethylene, high-density polyethylene, very low-density polyethylene, random copolymer polypropylene, block copolymer polypropylene, homopolypropylene, polybutene, polymethylpentene, ethylene-vinyl acetate copolymer (EVA), ionomer, ethylene-(meth)acrylic acid copolymer, ethylene-(meth)acrylic acid ester (random, alternating) copolymer, ethylene-butene copolymer, and ethylene-hexene copolymer; polyurethane; polyesters such as polyethylene terephthalate (PET), polyethylene naphthalate, and polybutylene terephthalate (PBT); polycarbonate; polyimide; polyether ether ketone; polyetherimide; polyamides such as aramid and wholly aromatic polyamide; polyphenyl sulfide; fluororesin; polyvinyl chloride; polyvinylidene chloride; cellulose resin; and silicone resin. The resins may be used alone or in combination of two or more.
[0041] The resin forming the resin layer is not particularly limited, and examples thereof include thermoplastic resins, thermosetting resins, active energy ray curable resins, and other curable resins. In this specification, the term "curable resin" refers to a resin that can be cured to form a resin (curable resin) and a resin formed by curing a curable resin. The resin is preferably a curable resin from the viewpoint of excellent releasability after curing. These resins may be used alone or in combination of two or more.
[0042] Examples of thermoplastic resins include polystyrene resins, vinyl acetate resins, polyester resins, polyolefin resins (such as polyethylene resins and polypropylene resin compositions), polyimide resins, and acrylic resins.
[0043] Examples of thermosetting resins include phenolic resins, epoxy resins, urethane resins, melamine resins, alkyd resins, and silicone resins.
[0044] Examples of epoxy resins include bisphenol-type epoxy resins, spirocyclic-type epoxy resins, naphthalene-type epoxy resins, biphenyl-type epoxy resins, terpene-type epoxy resins, glycidyl ether-type epoxy resins, glycidyl amine-type epoxy resins, and novolac-type epoxy resins.
[0045] Examples of bisphenol-type epoxy resins include bisphenol A-type epoxy resins, bisphenol F-type epoxy resins, bisphenol S-type epoxy resins, and tetrabromobisphenol A-type epoxy resins. Examples of the glycidyl ether-type epoxy resins include tris(glycidyloxyphenyl)methane and tetrakis(glycidyloxyphenyl)ethane. Examples of the glycidylamine-type epoxy resins include tetraglycidyldiaminodiphenylmethane. Examples of the novolac-type epoxy resins include cresol novolac-type epoxy resins, phenol novolac-type epoxy resins, α-naphthol novolac-type epoxy resins, and brominated phenol novolac-type epoxy resins.
[0046] Examples of active energy ray-curable resins include polymerizable resins having at least two radical reactive groups (e.g., (meth)acryloyl groups) in the molecule. Examples of the active energy ray include electron beams, ultraviolet rays, α rays, β rays, γ rays, and X-rays.
[0047] The resin layer may also contain a low-adhesion resin containing a fluorine-based polymer or a low-adhesion resin containing a non-polar polymer. Examples of fluorine-based polymers include polytetrafluoroethylene, polychlorotrifluoroethylene, polyvinyl fluoride, polyvinylidene fluoride, tetrafluoroethylene-hexafluoropropylene copolymer, and chlorofluoroethylene-vinylidene fluoride copolymer. Examples of non-polar polymers include olefin-based resins (e.g., polyethylene, polypropylene, etc.). When the resin layer contains these resins, the releasability of the transfer film 30 can be improved even if a release treatment layer (described later) is not formed.
[0048] The unevenness 31 may be formed on the first main surface 30a of the transfer film 30 by, for example, incorporating a filler into a resin layer and causing the filler to protrude from the first main surface 30a. That is, the transfer film 30 may contain a resin and a filler, and the unevenness 31 may be formed by the filler protruding from the first main surface 30a. Such a transfer film 30 can be easily manufactured by kneading the filler into the resin that is the material for the transfer film 30 during manufacturing.
[0049] In addition, the uneven shape 31 may be formed by pressing a mold having an uneven shape onto the first main surface 30a, by sand matting the first main surface 30a, or by spraying dry ice or the like onto the first main surface 30a.
[0050] When the unevenness 31 is formed by adding a filler, examples of the filler include organic particles and inorganic particles. Examples of organic particles include acrylic resins such as polymethyl methacrylate, polyacrylonitrile resins, polyurethane resins, polyamides, and polyimides. Examples of inorganic particles include calcium carbonate, calcium silicate, clay, kaolin, talc, silica, glass, diatomaceous earth, mica powder, alumina, magnesium oxide, zinc oxide, barium sulfate, aluminum sulfate, calcium sulfate, and magnesium carbonate. One type of these particles may be used alone, or two or more types may be used.
[0051] The median diameter (D50) of the filler is not particularly limited, but is preferably 0.5 to 20 μm, and more preferably 1 to 10 μm. When the median diameter (D50) is within the above range, a concave-convex shape can be easily formed. In this specification, the median diameter (D50) means the particle size at 50% of the cumulative value in the particle size distribution determined by a laser diffraction / scattering method.
[0052] The content of the filler in the resin layer is not particularly limited, but is preferably 5 to 70 parts by weight, more preferably 10 to 40 parts by weight, relative to 100 parts by weight of the resin forming the resin layer. When the content of the filler in the resin layer is within the above range, the uneven shape can be easily formed.
[0053] The surface condition of the first main surface 30a can be adjusted by adjusting the median diameter (D50) and content of the filler.
[0054] The thickness of the transfer film 30 is not particularly limited, but is preferably 10 to 200 μm, and more preferably 15 to 200 μm. If the thickness of the transfer film 30 is less than 10 μm, the strength will be low and it will be difficult to protect the electromagnetic wave shielding film until the transfer film 30 is peeled off. If the thickness of the transfer film 30 exceeds 200 μm, it will be difficult to handle and its peelability will be reduced.
[0055] The transfer film 30 may be provided with a release treatment layer in a portion that comes into contact with the protective layer 21 of the electromagnetic wave shielding film 20. Examples of the release treatment layer include layers formed by surface treatment with a release treatment agent such as a silicone-based, long-chain alkyl-based, fluorine-based, or molybdenum sulfide-based agent. When a release treatment layer is formed, the first main surface 30a refers to the surface of the release treatment layer that comes into contact with the protective layer 21 of the electromagnetic wave shielding film 20.
[0056] (Protective Layer of Electromagnetic Wave Shielding Film) The protective layer 21 constituting the electromagnetic wave shielding film 20 is not particularly limited as long as it has sufficient insulating properties and can protect the shielding layer 22 and the adhesive layer 23, but is preferably composed of, for example, a thermoplastic resin composition, a thermosetting resin composition, an active energy ray-curable composition, etc. Examples of the thermoplastic resin composition include, but are not particularly limited to, a styrene-based resin composition, a vinyl acetate-based resin composition, a polyester-based resin composition, a polyethylene-based resin composition, a polypropylene-based resin composition, an imide-based resin composition, an acrylic-based resin composition, etc.
[0057] The thermosetting resin composition is not particularly limited, but examples thereof include phenolic resin compositions, epoxy resin compositions, urethane resin compositions, melamine resin compositions, and alkyd resin compositions.
[0058] The active energy ray-curable composition is not particularly limited, but examples thereof include polymerizable compounds having at least two (meth)acryloyloxy groups in the molecule.
[0059] The material of the protective layer 21 may be one type alone or a combination of two or more types.
[0060] The protective layer 21 may contain, as needed, a curing accelerator, a tackifier, an antioxidant, a pigment, a dye, a plasticizer, an ultraviolet absorber, an antifoaming agent, a leveling agent, a filler, a flame retardant, a viscosity adjuster, an antiblocking agent, and the like.
[0061] The pigment is not particularly limited, but examples thereof include black pigments such as carbon black.
[0062] The thickness of the protective layer 21 is not particularly limited and can be set appropriately as needed, but is preferably 1 to 15 μm, and more preferably 3 to 10 μm. If the thickness of the protective layer 21 is less than 1 μm, it is too thin and therefore does not adequately protect the shielding layer 22 and the adhesive layer 23. If the thickness of the protective layer 21 exceeds 15 μm, it is too thick, making it difficult for the electromagnetic wave shielding film 20 to bend, and the toughness of the protective layer 21 decreases. This makes it difficult to apply the protective layer 21 to components that require bending resistance.
[0063] (Metal Layer of Electromagnetic Wave Shielding Film) The shielding layer 22 of the electromagnetic wave shielding film 20 may be made of any material as long as it can shield electromagnetic waves, but is preferably made of a metal layer or a conductive adhesive layer. Whether the shielding layer 22 is a metal layer or a conductive adhesive layer, it can provide suitable shielding of electromagnetic waves.
[0064] When the shielding layer 22 is a metal layer, the metal layer preferably contains at least one metal selected from the group consisting of copper, silver, gold, aluminum, nickel, tin, palladium, chromium, titanium, and zinc. The metal layer may also be made of an alloy of at least two metals selected from this group. A shielding layer 22 made of these metals can effectively shield electromagnetic waves.
[0065] The metal layer may be a rolled metal foil, a metal plated layer, or a metal vapor deposition layer.
[0066] The thickness of the metal layer is preferably 0.05 to 10 μm, and more preferably 0.1 to 5 μm. If the thickness of the metal layer is less than 0.05 μm, the metal layer will be too thin and will have low strength. This will result in reduced bending resistance. In addition, it will be difficult to sufficiently reflect and absorb electromagnetic waves, which will tend to reduce the electromagnetic wave shielding properties. If the thickness of the metal layer exceeds 10 μm, the entire electromagnetic wave shielding film will become thick and difficult to handle.
[0067] (Adhesive Layer of Electromagnetic Wave Shielding Film) The adhesive layer 23 of the electromagnetic wave shielding film 20 may be made of any material as long as it has adhesive properties, and examples of materials that can be used include thermoplastic resin compositions such as styrene-based resin compositions, vinyl acetate-based resin compositions, polyester-based resin compositions, polyethylene-based resin compositions, polypropylene-based resin compositions, imide-based resin compositions, amide-based resin compositions, and acrylic-based resin compositions, and thermosetting resin compositions such as phenol-based resin compositions, epoxy-based resin compositions, urethane-based resin compositions, melamine-based resin compositions, and alkyd-based resin compositions. The material for the adhesive layer 23 may be one of these alone or a combination of two or more of them.
[0068] The adhesive layer 23 may contain conductive particles. The adhesive layer 23 containing conductive particles becomes a conductive adhesive layer. When the adhesive layer 23 is a conductive adhesive layer, when the electromagnetic wave shielding film 20 is disposed on a printed wiring board, the adhesive layer 23 can be connected to a ground circuit formed on the printed wiring board, thereby electrically connecting the ground circuit to the shielding layer 22 of the electromagnetic wave shielding film 20. This improves the electromagnetic wave shielding properties.
[0069] When the adhesive layer 23 is a conductive adhesive layer, it may have either isotropic conductivity or anisotropic conductivity, but preferably has anisotropic conductivity. When the adhesive layer 23 has anisotropic conductivity, the transmission characteristics of high-frequency signals transmitted through the signal circuit of the printed wiring board are improved compared to when the adhesive layer 23 has isotropic conductivity.
[0070] The conductive particles are not particularly limited, but may be metal fine particles, carbon nanotubes, carbon fibers, metal fibers, or the like.
[0071] When the conductive particles are metal fine particles, the metal fine particles are not particularly limited, but may be silver powder, copper powder, nickel powder, solder powder, aluminum powder, silver-coated copper powder obtained by silver-plating copper powder, fine particles obtained by coating polymer fine particles, glass beads, etc. with a metal, etc. Among these, copper powder or silver-coated copper powder, which are inexpensively available, is preferred from the viewpoint of economy.
[0072] The shape of the conductive particles is not particularly limited, but can be appropriately selected from spherical, flat, scale-like, dendritic, rod-like, fibrous, and other shapes.
[0073] The median diameter (D50) of the conductive particles is preferably 3.0 to 15 μm, more preferably 5.0 to 11 μm, and even more preferably 5.0 to 8.0 μm.
[0074] The content of conductive particles in the adhesive layer 23 is preferably 3% to 50% by weight, more preferably 3% to 39% by weight, and even more preferably 3% to 30% by weight or less. If the proportion of conductive particles is less than 3% by weight, conductivity is difficult to exhibit. If the proportion of conductive particles exceeds 50% by weight, the proportion of resin in the adhesive layer becomes relatively small, and the adhesive strength of the adhesive layer is likely to decrease. Furthermore, since conductive particles are more likely to come into contact with each other (current is more likely to flow in the surface direction), electrical characteristics such as transmission characteristics are likely to decrease. Note that if the proportion of conductive particles is 3% to 39% by weight or less, anisotropic conductivity can be imparted to the adhesive layer 23.
[0075] The adhesive layer 23 may contain, as necessary, a curing accelerator, a tackifier, an antioxidant, a pigment, a dye, a plasticizer, an ultraviolet absorber, an antifoaming agent, a leveling agent, a filler, a flame retardant, a viscosity adjuster, etc.
[0076] In the electromagnetic wave shielding film 20, the thickness of the adhesive layer 23 is preferably 5 to 50 μm, and more preferably 5 to 30 μm. If the thickness of the adhesive layer is less than 5 μm, the adhesive layer is too thin and the adhesiveness is reduced. If the thickness of the adhesive layer is more than 50 μm, the adhesive layer becomes too thick, making it difficult to miniaturize the electromagnetic wave shielding film.
[0077] Next, a method for producing an electromagnetic wave shielding film with a transfer film of the present invention will be described. The method for producing an electromagnetic wave shielding film with a transfer film of the present invention includes a transfer film preparation step, a protective layer formation step, a shielding layer formation step, and an adhesive layer formation step.
[0078] (Transfer film preparation step) Figure 3 is a schematic diagram showing an example of the transfer film preparation step in the manufacturing method of the transfer film-attached electromagnetic wave shielding film according to the first embodiment of the present invention. As shown in Figure 3, a transfer film 30 is prepared having a concave-convex shape 31 formed on its first main surface 30a. Note that in Figure 3, for convenience, the transfer film 30 is prepared so that the first main surface 30a faces upward, but the orientation of the first main surface 30a is not particularly limited. The method for forming the concave-convex shape 31 on the first main surface 30a of the transfer film 30 has already been explained, so explanation will be omitted here.
[0079] (Protective Layer Forming Step) Figure 4 is a schematic diagram showing an example of the protective layer forming step in the manufacturing method of the electromagnetic wave shielding film with transfer film according to the first embodiment of the present invention. Next, as shown in Figure 4, a protective layer 21 is applied to the first main surface 30a of the transfer film 30. The method for applying the protective layer 21 is not particularly limited, and examples thereof include conventionally known coating methods such as gravure coating, kiss coating, die coating, lip coating, comma coating, blade coating, roll coating, knife coating, spray coating, bar coating, spin coating, and dip coating. By performing this step, the uneven shape 31 of the first main surface 30a of the transfer film 30 can be transferred to the protective layer 21.
[0080] 5 is a schematic diagram showing an example of the shielding layer forming step in the method for producing an electromagnetic wave shielding film with a transfer film according to the first embodiment of the present invention. Next, as shown in FIG. 5, a shielding layer 22 is disposed on the surface of the protective layer 21.
[0081] When the shielding layer 22 is a metal layer, the method for arranging the metal layer is not particularly limited, and a method of bonding a metal foil formed to a predetermined thickness to the protective layer 21, or a method of forming a metal layer on the surface of the protective layer 21 by vapor deposition or plating, etc., can be used.
[0082] When the shield layer 22 is a conductive adhesive layer, the shield layer 22 can be formed by applying a conductive adhesive by a conventionally known coating method.
[0083] (Adhesive layer forming step) Fig. 6 is a schematic view showing an example of the adhesive layer forming step in the method for producing an electromagnetic wave shielding film with a transfer film according to the first embodiment of the present invention. Next, as shown in Fig. 6, an adhesive layer 23 is applied to the surface of the shielding layer 22. A conventionally known coating method can be used as a method for applying the adhesive layer 23.
[0084] The above steps can be used to manufacture the electromagnetic wave shielding film 10 with a transfer film. When the electromagnetic wave shielding film 10 with a transfer film shown in Fig. 6 is rotated 180°, its orientation becomes the same as that of the electromagnetic wave shielding film 10 with a transfer film shown in Fig. 1.
[0085] Next, a shielded printed wiring board using the electromagnetic wave shielding film with transfer film according to the first embodiment of the present invention will be described. Note that in the following shielded printed wiring board, the adhesive layer of the electromagnetic wave shielding film with transfer film is a conductive adhesive layer.
[0086] 7 is a cross-sectional view schematically illustrating an example of a shielded printed wiring board according to the first embodiment of the present invention. The shielded printed wiring board 50 shown in FIG. 7 includes a printed wiring board 40 and an electromagnetic wave shielding film 10 with a transfer film disposed on the printed wiring board 40. The electromagnetic wave shielding film 10 with a transfer film is disposed so that the shielding layer 22 is closer to the printed wiring board 40 than the protective layer 21. That is, in the shielded printed wiring board 50, the electromagnetic wave shielding film 10 with a transfer film is disposed so that the adhesive layer 23 is in contact with the printed wiring board 40.
[0087] The printed wiring board 40 includes a base film 41, a printed circuit 42 including a ground circuit 42a arranged on the base film 41, and a coverlay 43 covering the printed circuit 42. An opening 43a is formed in the coverlay 43 to expose the ground circuit 42a.
[0088] The adhesive layer 23 fills the opening 43a and is in contact with the ground circuit 42a. When the adhesive layer 23 is a conductive adhesive layer as described above, the ground circuit 42a and the shielding layer 22 are electrically connected to each other. This improves the electromagnetic wave shielding characteristics.
[0089] In the printed wiring board 40, the base film 41 and the coverlay 43 are preferably both made of engineering plastics, such as polypropylene, cross-linked polyethylene, polyester, polybenzimidazole, polyimide, polyimideamide, polyetherimide, and polyphenylene sulfide (PPS).
[0090] In the printed wiring board 40, the printed circuit 42 can be made of a common circuit material such as copper.
[0091] The base film 41 and the printed circuit 42 may be bonded with an adhesive, or may be bonded without adhesive, similar to a so-called adhesiveless copper-clad laminate. The coverlay 43 may be formed by bonding multiple flexible insulating films with an adhesive, or may be formed by a series of methods such as coating a photosensitive insulating resin, drying, exposing, developing, and heat treating.
[0092] A conventionally known method can be used to attach the electromagnetic wave shielding film 10 with a transfer film to the printed wiring board 40. For example, it is preferable to place the electromagnetic wave shielding film 10 with a transfer film on the printed wiring board 40 so that the adhesive layer 23 of the electromagnetic wave shielding film 10 with a transfer film contacts the coverlay 43 of the printed wiring board 40, and then perform thermocompression bonding under conditions of 150 to 200°C, 2 to 5 MPa, and 1 to 60 minutes.
[0093] 8 is a cross-sectional view schematically illustrating an example of a state in which the transfer film is peeled off from the shielded printed wiring board according to the first embodiment of the present invention. As shown in FIG. 8 , the transfer film 30 is peeled off from the shielded printed wiring board 50 during use. In the shielded printed wiring board 50, the protective layer 21 of the electromagnetic wave shielding film 20 and the first main surface 30 a of the transfer film 30 are in contact with each other, so that the concave-convex shape 31 of the first main surface 30 a of the transfer film 30 is transferred to the protective layer 21 of the electromagnetic wave shielding film 20. This allows the glossiness of the protective layer 21 of the electromagnetic wave shielding film 20 to be reduced. As a result, the printed circuit 42 of the printed wiring board 40 can be suitably concealed.
[0094] Furthermore, in the shielded printed wiring board 50, the protruding peak height Spk of the first main surface 30a of the transfer film 30 is 1.2 μm or less. This makes it difficult for an anchor effect to occur between the transfer film 30 and the protective layer 21 of the electromagnetic wave shielding film 20. As a result, the releasability of the transfer film 30 is improved, and when the transfer film 30 is peeled off from the electromagnetic wave shielding film 20, it is possible to prevent part of the protective layer 21 from being peeled off while remaining attached to the transfer film 30.
[0095] Second Embodiment Next, an electromagnetic wave shielding film with a transfer film according to a second embodiment of the present invention will be described. Fig. 9 is a cross-sectional view schematically showing another example of the electromagnetic wave shielding film with a transfer film according to the second embodiment of the present invention. The electromagnetic wave shielding film 110 with a transfer film shown in Fig. 9 comprises an electromagnetic wave shielding film 120 in which a protective layer 121 and a shielding layer 122 are laminated in this order, and a transfer film 130 having a first main surface 130a on which an uneven shape 131 is formed and arranged so that the first main surface 130a is in contact with the protective layer 121.
[0096] In the transfer film-attached electromagnetic wave shielding film 110, the shielding layer 122 is an isotropically conductive adhesive layer, and the shielding layer and the adhesive layer are integrated.
[0097] In the electromagnetic wave shielding film 110 with a transfer film, the shielding layer 122 provides electromagnetic wave shielding properties and also exerts the effect of adhering the electromagnetic wave shielding film 110 with a transfer film to a printed wiring board.
[0098] The preferred configurations of the protective layer 121 and transfer film 130 of the electromagnetic wave shielding film with a transfer film 110 are the same as the preferred configurations of the protective layer 21 and transfer film 30 of the electromagnetic wave shielding film with a transfer film 10 described above.
[0099] Examples will be given below to explain the present invention more specifically, but the present invention is not limited to these examples.
[0100] (Example 1) (Transfer Film Preparation Step) A matte coating material was prepared by blending 83.3 wt% of epoxy resin as a resin and 16.7 wt% of silica particles as a filler.
[0101] Next, the prepared matte coating material was coated onto a 50 μm PET film by gravure coating to produce a 4.5 μm thick transfer film according to Example 1. When the first main surface (exposed surface) of the transfer film according to Example 1 was observed, the filler protruded and formed an uneven shape.
[0102] The surface condition of the first main surface of the transfer film according to Example 1 was measured using a confocal microscope (product name "OPTELICS HYBRID", manufactured by Lasertec, 50x objective lens). The results are shown in Table 1. Note that each parameter of the surface condition shown in Table 1 refers to a parameter defined in ISO 25178. In addition, the 60° gloss of the first main surface of the transfer film according to Example 1 was measured using a Gardner Micro-Gloss (portable gloss meter, manufactured by BYK). The results are shown in Table 1.
[0103]
[0104] (Protective Layer Forming Step) Next, a protective layer made of epoxy resin and having a thickness of 5.0 μm was formed on the first main surface of the transfer film according to Example 1. As a result, the concave-convex shape formed on the first main surface was transferred to the surface of the protective layer.
[0105] (Shielding Layer Forming Step) Next, silver was vapor-deposited on the protective layer to form a silver layer having a thickness of 0.1 μm, which functions as a shielding layer.
[0106] (Adhesive layer forming process) Next, a conductive adhesive was prepared by blending 85% by weight of epoxy resin as the resin and 15% by weight of silver-coated copper powder as the conductive particles. Next, the conductive adhesive was applied to the copper layer to a thickness of 20 μm, thereby producing an electromagnetic wave shielding film with a transfer film according to Example 1.
[0107] Examples 2 to 4 Electromagnetic wave shielding films with transfer film according to Examples 2 to 4 were produced in the same manner as in Example 1, except that the materials used were changed as shown in Table 1.
[0108] (Comparative Example 1) An electromagnetic wave shielding film with a transfer film according to Comparative Example 1 was produced in the same manner as in Example 1, except that in the transfer film preparation process, one main surface of a 50 μm thick PET film was subjected to a sand matting process to form an uneven shape.
[0109] Comparative Examples 2 and 3 Electromagnetic wave shielding films with transfer film according to Comparative Examples 2 and 3 were produced in the same manner as in Example 1, except that the materials used were changed as shown in Table 1.
[0110] (Preparation of Evaluation Substrates) Each electromagnetic wave shielding film with transfer film was laminated onto a printed wiring board, and then vacuumed using a press at a temperature of 170°C and a pressure of 2 MPa for 60 seconds, followed by heating and pressing for an additional 180 seconds to bond the boards together to prepare evaluation substrates. The printed wiring boards used were those in which a printed circuit was formed on a base film made of polyimide film. The printed circuit was formed of copper foil with a line width of 0.1 mm and a height of 12 μm. A coverlay made of a 12.5 μm thick polyimide film was provided on the base film to cover the printed circuit.
[0111] (Evaluation of Peelability) Using a strength tester (product name "PFT50S", manufactured by Palmec Co., Ltd.), the peel strength was measured when the transfer film was peeled from each evaluation substrate under the conditions of a sample width of 10 mm, a peel angle of 170°, and a peel speed of 1000 mm / min. The results are shown in Table 1. In addition, after peeling, it was observed whether or not a part of the protective layer was attached to the transfer film.
[0112] (Evaluation of 60° Gloss of Protective Layer) After peeling off the transfer film from each evaluation substrate, the 60° gloss of the protective layer was measured using a Gardner Micro-Gloss (portable gloss meter, manufactured by BYK). The results are shown in Table 1.
[0113] (Measurement of Surface State of Protective Layer) After peeling off the transfer film from each evaluation substrate, the surface state of the protective layer was measured using a confocal microscope (trade name "OPTELICS HYBRID", manufactured by Lasertec, objective lens 50x). The results are shown in Table 1. Note that each parameter of the surface state shown in Table 1 means a parameter specified in ISO 25178.
[0114] (Evaluation of Concealment Ability) Each evaluation substrate was placed on a flat table surface, and the transfer film was peeled off. After that, it was evaluated whether the printed circuit was visible from the electromagnetic wave shielding film side at a height of 30 cm from the evaluation substrate and at an angle of 45° in an environment with a surface illuminance of 500 lux. The evaluation criteria were as follows. The results are shown in Table 1. ◯: The printed circuit was not visible. ×: The printed circuit was visible.
[0115] As shown in Table 1, in the electromagnetic wave shielding films with transfer films according to each Example, the peel strength of the transfer film was not too high, and part of the protective layer was not adhered. In addition, the 60° gloss of the protective layer after peeling of the transfer film was low, and the hiding power was high.
[0116] As shown in Table 1, there is no correlation between the 60° gloss of the first main surface of the transfer film and the 60° gloss of the protective layer after the transfer film is peeled off, and it was found that the 60° gloss of the first main surface of the transfer film does not contribute much to the hiding property of the protective layer.
[0117] 10, 110 Electromagnetic wave shielding film with transfer film 20, 120 Electromagnetic wave shielding film 21, 121 Protective layer 22, 122 Shielding layer 23 Adhesive layer 30, 130 Transfer film 30a, 130a First main surface of transfer film 31, 131 Concave and recessed shape 40 Printed wiring board 41 Base film 42 Printed circuit 42a Ground circuit 43 Coverlay 43a Opening 50 Shielded printed wiring board
Claims
1. A transfer film having a first main surface on which an uneven shape is formed, the height Spk of the protruding peaks of the first main surface being 1.2 μm or less.
2. The transfer film according to claim 1, wherein the minimum autocorrelation length Sal of the first main surface is 6 μm or less.
3. A transfer film as described in claim 1 or 2, wherein the transfer film contains a resin and a filler, and the uneven shape is formed by the filler protruding from the first main surface.
4. An electromagnetic wave shielding film with a transfer film, comprising: an electromagnetic wave shielding film including a protective layer and a shielding layer laminated on the protective layer; and a transfer film having a first main surface with an uneven shape formed thereon and arranged so that the first main surface is in contact with the protective layer, wherein the height Spk of the protruding peaks of the first main surface is 1.2 μm or less.
5. An electromagnetic wave shielding film with a transfer film as described in claim 4, wherein the shielding layer is a metal layer, and an adhesive layer is further laminated on the surface of the shielding layer opposite to the surface on the protective layer side.
6. The electromagnetic wave shielding film with transfer film according to claim 4, wherein the shielding layer is an isotropically conductive adhesive layer.
7. A shielded printed wiring board comprising: a base film, a printed circuit including a ground circuit arranged on the base film, and a coverlay covering the printed circuit; an electromagnetic wave shielding film including a protective layer and a shielding layer laminated on the protective layer, the shielding layer being arranged so as to be positioned on the printed wiring board side; and a transfer film having a first main surface with an uneven shape formed thereon, the first main surface being arranged so as to be in contact with the protective layer, wherein the shielded printed wiring board comprises: a protruding peak height Spk of the first main surface is 1.2 μm or less.
Citation Information
Patent Citations
Electromagnetic wave shield film and manufacturing method of flexible printed wiring board with electromagnetic wave shield film
JP2016054259A
Peelable film
JP2017132251A
Method of manufacturing electromagnetic wave shield film and method of manufacturing printed wiring board with electromagnetic wave shield film
JP2021044342A
Biaxially stretched polypropylene film
WO2016051897A1