Electrode recovery method and electrode for power storage device

The electrode recovery method addresses the issue of increased resistance in secondary batteries by evaluating and compressing electrodes, applying conductive agents, and using ultrasonic waves to restore adhesion, thereby improving energy efficiency.

WO2024204686A1PCT designated stage expired Publication Date: 2024-10-03HONDA MOTOR CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/012993
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-31
Filing Date
2024-03-29
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Existing methods for reusing secondary batteries fail to recover from increased resistance due to decreased particle adhesion, which affects energy efficiency.

Method used

An electrode recovery method involving evaluation, compression, and potential application of a conductive agent to restore particle contact and reduce resistance, including steps for measuring resistance and thickness, and applying ultrasonic waves for improved conductivity.

Benefits of technology

The method effectively recovers from increased resistance by restoring particle adhesion, enhancing energy efficiency in power storage devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024012993_03102024_PF_FP_ABST
    Figure JP2024012993_03102024_PF_FP_ABST
Patent Text Reader

Abstract

This electrode recovery method is a method for recovering an electrode from a used power storage device, the recovery method comprising: a first step (S1) for evaluating the state of the electrode; and a second step (S2) for compressing the electrode in the thickness direction of the electrode.
Need to check novelty before this filing date? Find Prior Art

Description

Electrode recovery method and electrode for power storage device

[0001] The present invention relates to a method for restoring an electrode and an electrode for a power storage device. This application claims priority to Japanese Patent Application No. 2023-057930, filed on March 31, 2023, the contents of which are incorporated herein by reference.

[0002] In recent years, research and development has been conducted on the reuse of secondary batteries, which contribute to energy efficiency, in order to ensure that more people have access to affordable, reliable, sustainable, and advanced energy (see, for example, Patent Document 1).

[0003] Japanese Patent Application Publication No. 2012-022969

[0004] However, in the technology relating to the reuse of secondary batteries such as that disclosed in Patent Document 1, although it is possible to remove deteriorated materials on the surface of the active material, there is a problem in that it is not possible to recover the increased resistance due to the decrease in the adhesion of particles.

[0005] The present invention aims to solve the above-mentioned problems by recovering the increase in resistance caused by the decrease in particle adhesion, which will ultimately contribute to improving energy efficiency.

[0006] In order to solve the above problems, the present invention proposes the following measures. <1> A method for recovering an electrode according to Aspect 1 of the present invention may be a method for recovering an electrode of a used energy storage device, comprising: a first step of evaluating the state of the electrode; and a second step of compressing the electrode in a thickness direction of the electrode. <2> Aspect 2 of the present invention is the method for recovering an electrode according to Aspect 1, wherein the first step further comprises a step of measuring a resistance component of the electrode. <3> Aspect 3 of the present invention is the method for recovering an electrode according to Aspect 1 or Aspect 2, wherein the resistance component may be a composite layer resistance or an interface resistance of the electrode. <4> Aspect 4 of the present invention is the method for recovering an electrode according to any one of Aspects 1 to 3, wherein the second step may involve compressing the electrode while heating. <5> Aspect 5 of the present invention is the method for recovering an electrode according to any one of Aspects 1 to 4, wherein the second step further comprises a calculation step of measuring a thickness of the electrode and calculating a difference between the thickness and an estimated pre-use thickness, and wherein the second step may involve compressing the electrode in the thickness direction so as to reduce the thickness of the electrode by the difference obtained in the calculation step. <6> Aspect 6 of the present invention is the electrode recovery method of any one of Aspects 1 to 5, wherein the second step may further include a coating step of coating a conductive agent on the surface of the electrode. <7> Aspect 7 of the present invention is the electrode recovery method of any one of Aspects 1 to 6, wherein the conductive agent may be carbon fiber. <8> Aspect 8 of the present invention is the electrode recovery method of any one of Aspects 1 to 7, wherein the coating step may be a step of applying a dispersion liquid in which the conductive agent is dispersed and drying the dispersion liquid. <9> Aspect 9 of the present invention is the electrode recovery method of any one of Aspects 1 to 8, wherein ultrasonic waves may be applied to the electrode in the coating step. <10> A power storage device electrode of Aspect 10 of the present invention is obtained by the electrode recovery method of any one of Aspects 1 to 9.

[0007] According to the above-described aspects of the present invention, it is possible to recover from the increase in resistance caused by the decrease in particle adhesion, which in turn contributes to the improvement of energy efficiency.

[0008] Fig. 1 is a flowchart of an electrode recovery method according to a first embodiment of the present invention. Fig. 2 is a schematic diagram showing the configuration of an electrode. Fig. 3 is a diagram for explaining an example of a dV / dQ curve for a single electrode, each of a positive electrode and a negative electrode, in an initial state. Fig. 4 is a diagram for explaining an example of a curve obtained by fitting an actually measured dV / dQ curve of an electricity storage device. Fig. 5 is a diagram for explaining a comparison between a dV / dQ curve in an initial state and a diagnostic dV / dQ curve. Fig. 6 is a flowchart of an electrode recovery method according to a second embodiment of the present invention.

[0009] A method for restoring an electrode according to one embodiment of the present invention will be described below with reference to the drawings. Fig. 1 is a flowchart of the method for restoring an electrode according to one embodiment of the present invention. The electrode restoring method of the present disclosure is a method for restoring an electrode of a used energy storage device, and includes a first step S1 of evaluating the state of the electrode, and a second step S2 of compressing the electrode in the thickness direction of the electrode. Each step will be described below.

[0010] (First Step S1) In the first step S1, the state of the electrodes of the used energy storage device is evaluated. In the first step S1, the state of the electrodes of the used energy storage device may be evaluated based on physical quantity data obtained when the used energy storage device is charged or discharged. The physical quantity data may be, for example, a voltage value and a current value during charging.

[0011] (Used Electricity Storage Device) A used electricity storage device has electrodes containing an active material, a binder, and a current collector. The electricity storage device is not particularly limited as long as it can store electricity and has electrodes containing an active material, a binder, and a current collector. The electricity storage device is, for example, a lithium ion secondary battery. FIG. 2 is a schematic diagram showing the configuration of the electrodes. The electrodes targeted by the active material separation method of the present disclosure are a positive electrode 10 and a negative electrode 20. The configuration of the electrodes will be described below.

[0012] "Positive Electrode" The positive electrode 10, which is an electrode, includes a positive electrode active material 11, a positive electrode conductive additive 12, a positive electrode binder 13, and a positive electrode current collector 14. A layer consisting of the positive electrode active material 11, the positive electrode conductive additive 12, and the positive electrode binder 13 is referred to as a positive electrode mixture layer. The positive electrode mixture layer may be formed on one or both sides of the positive electrode current collector 14. Note that, as long as the positive electrode active material 11 is conductive, the positive electrode mixture layer does not need to include the positive electrode conductive additive 12.

[0013] The positive electrode active material 11 used in the positive electrode is not particularly limited as long as it can absorb and release Li ions. The positive electrode active material 11 can be, for example, lithium nickel oxide (e.g., LiNiO 2 ), lithium cobalt oxide (e.g., LiCoO 2 ), lithium nickel cobalt oxide, lithium nickel cobalt manganese oxide, LiFePO 4 , LiMn 1-x Fe x P.O. 4 , LiMnPO 4 , LiCoPO 4 , LiNiPO 4 The positive electrode active material 11 preferably contains one or more elements selected from the group consisting of manganese, nickel, and cobalt.

[0014] The positive electrode conductive additive 12, which is a conductive additive used in the positive electrode 10, assists in forming a conductive path between the positive electrode active material 11 and the positive electrode current collector 14. The positive electrode conductive additive 12 is not particularly limited as long as it has conductivity, and examples thereof include carbon black such as acetylene black, carbon nanotubes, and graphite such as artificial graphite.

[0015] The positive electrode binder 13, which is a binder for the positive electrode active material 11, binds the positive electrode active material 11, the positive electrode conductive additive 12, and the positive electrode current collector 14 together. Examples of the positive electrode binder 13 include polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), polyamide (PA), polyimide (PI), polyacrylic acid and its copolymers, polyamideimide (PAI), polybenzimidazole, polyethersulfone (PES), maleic anhydride-modified polypropylene, and mixtures thereof. The positive electrode binder 13 preferably contains a crystalline polymer having a melting point. The positive electrode binder 13 is preferably a polymer containing fluorine. Examples of fluorine-containing polymers include PVDF and PTFE.

[0016] Examples of the positive electrode current collector 14 include metal foils such as aluminum foil, stainless steel foil, and nickel foil. A carbon coating layer may be formed on the positive electrode current collector 14. The positive electrode current collector 14 may also be processed into a mesh shape.

[0017] The negative electrode 20, which is an electrode, includes a negative electrode active material 21, a negative electrode conductive additive 22, a negative electrode binder 23, and a negative electrode current collector 24. A layer consisting of the negative electrode active material 21, the negative electrode conductive additive 22, and the negative electrode binder 23 is referred to as a negative electrode mixture layer. The negative electrode mixture layer may be formed on one or both sides of the negative electrode current collector 24. Note that, as long as the negative electrode active material 21 is conductive, the negative electrode mixture layer does not need to include the negative electrode conductive additive 22.

[0018] The negative electrode active material 21, which is the active material of the negative electrode 20, is not particularly limited as long as it is capable of absorbing and releasing Li ions. Examples of the negative electrode active material 21 include graphite (artificial graphite, natural graphite), amorphous carbon (hard carbon), mesocarbon microbeads, carbon fiber, and Si materials (silicon, Si alloy, Si oxide).

[0019] The negative electrode conductive additive 22, which is a conductive additive for the negative electrode 20, assists in forming a conductive path between the negative electrode active material 21 and the negative electrode current collector 24. The negative electrode conductive additive 22 is not particularly limited as long as it has conductivity, and examples thereof include carbon black such as acetylene black, carbon nanotubes, and graphite such as artificial graphite.

[0020] The negative electrode binder 23, which is a binder for the negative electrode 20, binds the negative electrode active material 21, the negative electrode conductive additive 22, and the negative electrode current collector 24 together. Examples of the negative electrode binder 23 include carboxymethyl cellulose, polyvinylidene fluoride, polytetrafluoroethylene, polyacrylic acid, fluororubber, and diene rubber such as styrene butadiene rubber. The negative electrode binder 23 preferably contains a crystalline polymer having a melting point. The negative electrode binder 23 is preferably a polymer containing fluorine. Examples of the polymer containing fluorine include PVDF, PTFE, and fluororubber.

[0021] The negative electrode current collector 24, which is a current collector for the negative electrode 20, may be, for example, a metal foil such as copper foil, stainless steel foil, or nickel foil. A carbon coating layer may be formed on the negative electrode current collector 24. The negative electrode current collector 24 may also be processed into a mesh shape.

[0022] (Preliminary Preparation) More specifically, as a preliminary preparation for the first step S1, for example, a storage device with the same specifications as the target storage device is first disassembled, and single-electrode data for each coin cell, i.e., dV / dQ curves for the positive and negative electrodes in the initial state, as shown in FIG. 3, are obtained. Furthermore, these single-electrode dV / dQ curves are added together and fitted to the actual measured curve of the storage device (the curve drawn by the dashed line in FIG. 4) as shown in FIG. 4. In FIG. 4, the fitted curve is shown by the solid line. This allows each extreme value of the actual measured curve to be assigned to the positive and negative electrodes. In this way, a dV / dQ curve for the initial state of a used storage device is obtained in advance. Then, the positions of each peak in the dV / dQ curve based on the positive and negative electrodes are determined, and the peak widths for the initial state of each positive and negative electrode are determined.

[0023] 3 and 4, the horizontal axis represents the cell capacity (Ah), and the vertical axis represents the amount of change in voltage relative to a change in reference capacity (dV / dQ).

[0024] Here, if a peak position can be detected between 5% and 95% of the charge rate or state of charge (SOC: State of Charge), assuming a fully charged state as 100%, differential capacity analysis becomes possible. Specifically, in the dV / dQ curve in the initial state, two peaks based on the positive electrode are identified, and the width between these peaks is determined. In Figures 3 and 4, the two peaks based on the positive electrode are located at the intersections with the dashed lines. Furthermore, in the dV / dQ curve in the initial state, two peaks based on the negative electrode are identified, and the width between these peaks is determined. In Figures 3 and 4, the two peaks based on the negative electrode are located at the intersections with the dashed lines.

[0025] For example, as a guideline, the two peaks between 0 and 30% on the low SOC side may be determined as the positive electrode peaks, the two peaks between 30 and 60% as the negative electrode (graphite in this embodiment) peaks (intersections with the dashed line Gr), and the two peaks between 60 and 100% on the high SOC side as the silicon oxide (SiO) peaks in the negative electrode (intersections with the dashed line SiO). It can also be determined that the positive electrode peaks are convex on the negative side of dV / dQ, and the negative electrode peaks are convex on the positive side of dV / dQ. Note that although peaks derived from the materials constituting the electrodes will appear, for example, if the negative electrode does not contain SiO, no peaks derived from SiO will appear.

[0026] (After Battery Use Begins) After the battery begins to be used, the voltage and current are continuously measured by charging at a low current. It is important that the current be relatively low. The capacity is obtained by integrating the current value over time, and a curve of the voltage value versus the capacity can be obtained from this. Furthermore, a differential capacity curve (dV / dQ curve) versus the capacity can be obtained by differentiating the voltage value with respect to the capacity.

[0027] Analysis is possible even with a typical charging rate of 0.2 to 0.5 C. However, a lower rate of, for example, 0.02 to 0.07 C allows for more accurate analysis. Note that once charging has progressed to a certain extent and the voltage has stabilized, charging can be continued by gradually reducing the current.

[0028] As described above, the dV / dQ curve is obtained by calculating the derivative of the voltage in the charge / discharge curve of the power storage device with respect to the reference capacity. This method makes it possible to accurately recognize the fluctuation characteristics of the voltage with respect to the reference capacity of the power storage device whose degradation is to be determined. Therefore, by comparing the generated dV / dQ curve for degradation determination with the dV / dQ curve obtained when the power storage device is in its initial state, it becomes possible to evaluate and determine the degree to which the battery has deteriorated from its initial state at that time.

[0029] The dV / dQ curve obtained for the used electricity storage device is referred to as a diagnostic dV / dQ curve that indicates the amount of change in voltage relative to the change in the reference capacity of the used electricity storage device.

[0030] Next, based on the obtained diagnostic dV / dQ curve and the dV / dQ curve in the initial state, the first capacity loss rate due to deterioration of the positive electrode, the second capacity loss rate due to deterioration of the negative electrode, and the amount of capacity loss due to other factors are each evaluated.

[0031] Specifically, for a cell of a used energy storage device, two peaks originating from each electrode are identified, and the change in the width between these two peaks (peak width) between the initial state and the state after the battery has started to be used is evaluated. That is, the peak widths of the positive and negative electrodes after the battery has started to be used are determined, and the change in the peak widths due to use of the energy storage device is evaluated by comparing them with the peak widths in the initial state.

[0032] (First Capacity Decline Rate and Second Capacity Decline Rate) The dV / dQ curve in the initial state is compared with the diagnostic dV / dQ curve to calculate the rate of change in the width between two peaks based on the positive electrode and the negative electrode. The rate of change in the width between two peaks based on the positive electrode of the diagnostic dV / dQ curve relative to the dV / dQ curve in the initial state is defined as the first capacity decline rate, and the rate of change in the width between two peaks based on the negative electrode of the diagnostic dV / dQ curve relative to the dV / dQ curve in the initial state is defined as the second capacity decline rate.

[0033] FIG. 5 shows a comparison between the dV / dQ curve in the initial state and the diagnostic dV / dQ curve. In FIG. 5, the solid line represents the dV / dQ curve in the initial state, and the dashed line represents the diagnostic dV / dQ curve. The diagnostic dV / dQ curves are shifted along the vertical axis to avoid overlap. As shown in FIG. 5, comparing the dV / dQ curve in the initial state with the diagnostic dV / dQ curve, it can be seen that the width between the two peaks based on the positive and negative poles has changed.

[0034] (Capacity Loss Due to Other Factors) The amount of shift of the diagnostic dV / dQ curve relative to the dV / dQ curve in the initial state is defined as the amount of capacity loss due to factors (other factors) other than the deterioration of the positive or negative electrode. The amount of shift of the diagnostic dV / dQ curve relative to the dV / dQ curve in the initial state is determined to be primarily due to a decrease in the amount of Li involved in charge and discharge due to the deposition of a Li-containing negative electrode coating caused by swelling and shrinkage of the active material. For example, the amount of shift in the midpoint of the two peaks based on the negative electrode is defined as the amount of capacity loss due to other factors.

[0035] The control unit 10 determines whether the first and second capacity decline rates are both below a predetermined threshold (e.g., 5%) and whether the capacity decline amount exceeds a predetermined threshold. The threshold can be set for each power storage device.

[0036] When it is confirmed that the first capacity loss rate and the second capacity loss rate are equal to or less than the threshold, it is preferable to analyze the state of the electrode in more detail. Specifically, the resistance component of the electrode is measured. That is, in the electrode recovery method, the first step S1 preferably further includes a step of measuring the resistance component of the electrode. The resistance component of the electrode can be measured using an AC impedance method or a multi-point probe method. Note that, for example, when replenishing the energy storage device with Li, the electrode may be removed and the second step S2 described below may be performed without performing the measurement using the AC impedance method or the multi-point probe method.

[0037] When measuring resistance components using the AC impedance method, for example, the following method can be used. AC impedance is measured, for example, in the state of a power storage device (cell) using a commercially available AC impedance measuring device. For example, an AC voltage with an amplitude of 10 mV superimposed on the OCV (open circuit voltage) is applied from 1 MHz to 1 mHz, and the internal resistance can be determined from the response current. The obtained results are plotted as a cole-cole plot. Examples of the resistance components of the electrode to be measured include composite layer resistance and interface resistance. Each resistance component can be separated based on the time constant. Measurement conditions are appropriately set depending on the power storage device. Separation of each resistance component based on the time constant can be achieved by, for example, determining the measurement results from 1 MHz to 1 kHz as the high-frequency side resistance and judging them as metal resistance and resistance due to deterioration of the coating at the battery interface and electrolyte components, determining the results from 1 kHz to 1 Hz as ionic conduction resistance between active materials, and determining the results below 1 Hz as solid ion diffusion within particles.

[0038] When determining the state of the electrodes using the AC impedance method, for example, a reference curve obtained from the AC impedance of a power storage device immediately after manufacture is compared with the curve of a used power storage device. For example, if, in a cole-cole plot of the used power storage device, the region where the impedance component increases substantially linearly with increasing frequency (the region rising to the right) becomes larger than that of the initial power storage device, it is determined that the conductive resistance has increased, and the second step S2 is performed.

[0039] In the case of the multi-point probe measurement method, the electrodes removed from the electricity storage layer are evaluated. The method for removing the positive electrode 10 and negative electrode 20, which are electrodes, from the electricity storage device is not particularly limited, and any known method can be used. The electrode to be evaluated is preferably the positive electrode 10. Since it is dangerous to dismantle an electricity storage device while it is charged, it is preferable to fully discharge the electricity storage device. After discharging, the exterior material of the electricity storage device is cut, and the positive electrode 10 and negative electrode 20 are removed from the electricity storage device.

[0040] In the multi-point probe measurement method, a fine probe is applied to the electrode surface, a constant current is passed, and the potential at multiple points is measured. A virtual electrode is also assumed, and modeling is performed to calculate the potential generated on the surface. Then, using the composite layer resistance and interfacial resistance as variables, measurements are repeatedly performed until the actual potential and the measured potential match. If the composite layer resistance and interfacial resistance obtained in this way are determined to be higher than a predetermined threshold, the second step S2 is performed. For example, if the resistance of the composite layer of the electrode increases by 10% or more compared to before use, it is determined that the resistance of the composite layer has increased, and the second step S2 is performed. An example of a multi-point probe measurement system that can be used is the Hioki RM2610 electrode resistance measurement system.

[0041] (Second Step S2) In the second step S2, the electrode is compressed in the thickness direction of the electrode. Compression can be performed by a known means such as a roll press. The electrode may be either the positive electrode 10 or the negative electrode 20, but the positive electrode 10 is preferred. In the second step S2, compression while heating is preferably performed. Pressing while heating softens the binders 13, 23, making it easier to restore adhesion. The heating temperature is, for example, from the melting point of the binder to 200°C.

[0042] The second step S2 preferably further includes a calculation step of measuring the thickness of the electrodes 10, 20 and calculating the difference from the estimated pre-use thickness. In the second step S2, the electrodes 10, 20 are preferably compressed in the thickness direction so that the thickness of the electrodes 10, 20 is reduced by the difference obtained in the calculation step. By compressing them in this manner, it is possible to restore inter-particle contact that has been reduced due to the expansion and contraction of the active material associated with charging and discharging. If information on the thickness of the electrodes at the time of manufacture of the energy storage device is available, that information is used for the estimated pre-use thickness. If information on the thickness at the time of initial manufacture is unavailable, the estimated pre-use thickness may be, for example, the thickness of the used electrode excluding voids in the electrode portion.

[0043] The electrode recovery method according to the first embodiment has been described above. The electrode recovery method according to this embodiment can recover the increased resistance caused by the decrease in particle adhesion. A recovered energy storage device electrode can be obtained by the electrode recovery method according to this embodiment.

[0044] Next, a method for restoring an electrode according to a second embodiment of the present invention will be described. FIG. 6 is a flowchart of the method for restoring an electrode according to the second embodiment of the present invention. The electrode restoring method according to the present disclosure is a method for restoring an electrode of a used energy storage device, and includes a first step S1 of evaluating the state of the electrode, and a second step S2A of compressing the electrode in the thickness direction of the electrode. In the following description, the same components as those in the first embodiment will be given the same reference numerals, and a description thereof may be omitted. Each step will be described below.

[0045] (Second Step S2) The second step S2A preferably further includes a coating step of coating the surfaces of the electrodes 10, 20 with a conductive agent. The electrode may be either the positive electrode 10 or the negative electrode 20, but the positive electrode 10 is preferred. The conductive agent is not particularly limited, but examples include carbonaceous materials such as acetylene black and carbon nanotubes. Carbon fiber is preferred as the conductive agent. By applying the conductive agent, the addition of the conductive agent can compensate for conductivity and reduce the composite layer resistance and interface resistance.

[0046] In the coating process, the method for coating the conductive agent is not particularly limited. For example, in the coating process, a dispersion liquid in which the conductive agent is dispersed may be coated and then dried. That is, the coating process may be a process in which a dispersion liquid in which the conductive agent is dispersed is coated and then dried. It is also preferable to apply ultrasonic waves in the coating process. By applying ultrasonic waves, the conductive agent can penetrate into the voids in the electrodes 10 and 20, thereby further reducing the resistance. This can further improve and restore the condition of the electrodes.

[0047] In the second step S2A, the electrodes 10, 20 after the coating step are compressed in the thickness direction of the electrodes 10, 20. Compression can be performed by a known means such as a roll press. In the second step S2A, the electrodes 10, 20 are preferably compressed while being heated. Pressing while being heated softens the binders 13, 23, making it easier to restore adhesion. The heating temperature is, for example, from the melting point of the binder to 200°C.

[0048] Preferably, the second step S2A further includes a calculation step of measuring the thickness of the electrodes 10, 20 and calculating the difference from the estimated thickness before use. In the second step S2A, the electrodes 10, 20 are preferably compressed in the thickness direction so that the thickness of the electrodes 10, 20 is reduced by the difference obtained in the calculation step. By compressing the electrodes in this manner, it is possible to restore interparticle contact and the like that has been reduced due to the expansion and contraction of the active material during charging and discharging.

[0049] As described above, the active material separation method according to the second embodiment makes it possible to recover from the increase in resistance caused by the decrease in adhesion between particles.

[0050] The technical scope of the present invention is not limited to the above-described embodiments, and various modifications can be made without departing from the spirit of the present invention. In addition, the components in the above-described embodiments can be replaced with well-known components as appropriate without departing from the spirit of the present invention.

[0051] The recovery method of the present disclosure makes it possible to recover from the increase in resistance caused by a decrease in particle adhesion, and therefore has high industrial applicability.

[0052] REFERENCE SIGNS LIST 10 Positive electrode, 11 Positive electrode active material, 12 Positive electrode conductive additive, 13 Positive electrode binder, 14 Positive electrode current collector, 20 Negative electrode, 21 Negative electrode active material, 22 Negative electrode conductive additive, 23 Negative electrode binder, 24 Negative electrode current collector, S1 First step, S2 Second step

Claims

1. A method for restoring an electrode of a used electricity storage device, comprising: a first step of evaluating a condition of the electrode; and a second step of compressing the electrode in a thickness direction of the electrode.

2. The method for recovering an electrode according to claim 1, wherein said first step further comprises a step of measuring a resistance component of said electrode.

3. The method for recovering an electrode according to claim 2, wherein the resistance component is a composite layer resistance or an interface resistance of the electrode.

4. The method for recovering an electrode according to claim 1, wherein in the second step, compression is performed while heating.

5. A method for restoring an electrode as described in claim 1, wherein the second step further includes a calculation step of measuring a thickness of the electrode and calculating a difference from an estimated thickness before use, and in the second step, the electrode is compressed in the thickness direction so that the thickness of the electrode is reduced by the difference obtained in the calculation step.

6. The method for recovering an electrode according to claim 1, wherein the second step further comprises a coating step of coating a conductive agent on the surface of the electrode.

7. The method for restoring an electrode according to claim 6, wherein the conductive agent is carbon fiber.

8. The method for recovering an electrode according to claim 6, wherein the coating step is a step of coating a dispersion liquid in which the conductive agent is dispersed, and drying the coating liquid.

9. The method for recovering an electrode according to claim 8, wherein ultrasonic waves are applied to the electrode in the coating step.

10. An electrode for a power storage device, obtained by the electrode recovery method according to any one of claims 1 to 9.

Citation Information

Patent Citations

  • Reuse method of anode active material for nonaqueous electrolyte secondary battery

    JP2006228510A

  • Regeneration processing method for lithium ion secondary battery

    JP2019212482A