Ceramic electronic component and method for manufacturing same

The ceramic electronic component design addresses crack issues in multilayer capacitors by alternately stacking nickel-based internal electrode layers and using copper external electrodes to manage copper diffusion, enhancing mechanical strength and capacitance in high-density components.

WO2024204743A1PCT designated stage expired Publication Date: 2024-10-03TAIYO YUDEN KK
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/013108
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-30
Filing Date
2024-03-29
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Ceramic electronic components, particularly multilayer ceramic capacitors, face challenges in suppressing cracks due to the diffusion of copper from external electrodes into internal electrode layers during baking, especially when low melting point metals are used, leading to stress and cracking issues as the component height and layer count increase.

Method used

A ceramic electronic component design featuring alternately stacked first and second internal electrode layers primarily composed of nickel, with a dielectric layer in between, and external electrodes made of copper, where the first internal electrode layer has a higher concentration of low melting point metals like tin, and the second layer has a narrower width to reduce copper diffusion and stress, thereby minimizing crack occurrence.

Benefits of technology

The design effectively suppresses crack formation and maintains mechanical strength by controlling copper diffusion and stress distribution, ensuring reliable operation and capacitance in high-density, high-capacity ceramic electronic components.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024013108_03102024_PF_FP_ABST
    Figure JP2024013108_03102024_PF_FP_ABST
Patent Text Reader

Abstract

Provided is a ceramic electronic component of which the dimension in a first direction is equal to or greater than 1.3 times the dimension in a second direction. First and second internal electrode layers mainly composed of Ni are alternately laminated with a dielectric layer interposed therebetween. The ceramic electronic component comprises a first external electrode and a second external electrode that are formed so as to draw out the first and second internal electrode layers alternately to first and second end surfaces opposing each other in a third direction orthogonal to the first direction and the second direction, the first external electrode having a contact layer which is in contact with the first end surface and is mainly composed of Cu, and the second external electrode having a contact layer which is in contact with the second end surface and is mainly composed of Cu. The concentration of a low melting point metal is higher in the first internal electrode layer than in the second internal electrode layer. The width in a direction orthogonal to the lamination direction is narrower in a part of the first internal electrode layer that is connected to the first external electrode than in a part thereof opposing the second internal electrode layer. The width in the direction orthogonal to the lamination direction is greater in a part of the second internal electrode layer that is connected to the second external electrode than in the part of the first internal electrode layer that is connected to the first external electrode. 
Need to check novelty before this filing date? Find Prior Art

Description

Ceramic electronic component and manufacturing method thereof

[0001] The present invention relates to a ceramic electronic component and a method for manufacturing the same.

[0002] In recent years, electronic devices such as mobile information terminals have become smaller and more functional, limiting the mounting area of ​​electronic components on circuit boards. At the same time, ceramic electronic components such as multilayer ceramic capacitors are required to have even more layers.

[0003] Japanese Patent Application Laid-Open No. 2020-031152 Republished No. 2015 / 016309 Republished No. 2015 / 087688 Japanese Patent Application Laid-Open No. 2018-198292 Republished No. 2014 / 175034

[0004] In order to mount more electronic components on a circuit board in a smaller area, component structures with increased height dimensions have been proposed to achieve higher density mounting and larger capacity (see, for example, Patent Document 1). On the other hand, to achieve even higher capacity, structures have been proposed that include low-melting-point metals such as Sn (see, for example, Patent Document 2) and In, Ga, Bi, and Pb (see, for example, Patent Document 3) in the internal electrode layers, which achieve thinner dielectric layers and longer high-temperature load life. Among these, a structure has been proposed in which Sn is included in one of the internal electrode layers (see, for example, Patent Document 4).

[0005] However, when the internal electrode layer and the external electrode react with each other during baking, copper (Cu), a metal component of the external electrode, diffuses into the nickel (Ni) internal electrode layer, causing the internal electrode layer to expand, resulting in outward stress in the cover and side margins, which cannot withstand the stress and cause cracks (see, for example, Patent Document 5). When the height dimension is increased and the number of layers is increased, the expansion of the internal electrode layer becomes even greater, making it very difficult to prevent cracks from occurring. In particular, when an internal electrode layer containing a low-melting-point metal such as tin (Sn) is used, the diffusion of Cu from the external electrode to the internal electrode layer is promoted during baking of the external electrode, making the occurrence of the above-mentioned cracks a greater problem.

[0006] The present invention has been made in view of the above-mentioned problems, and has an object to provide a ceramic electronic component that can suppress the occurrence of cracks, and a method for manufacturing the same.

[0007] A ceramic electronic component according to the present invention includes a laminated chip having a substantially rectangular parallelepiped shape in which first internal electrode layers mainly composed of Ni and second internal electrode layers mainly composed of Ni are alternately stacked with dielectric layers sandwiched therebetween, the laminated chip being formed so that the first internal electrode layers and the second internal electrode layers are alternately drawn out to first end faces and second end faces opposing each other of the substantially rectangular parallelepiped shape, and when a first direction, a second direction, and a third direction in which the first end faces and the second end faces are opposed are orthogonal to each other, the dimension in the second direction is 1.3 times or more the dimension in the third direction; a first external electrode provided on the first end face, the contact layer in contact with the first end face being mainly composed of Cu; and a second external electrode provided on the second end face, the and a second external electrode having a contact layer in contact with the two end faces, the main component of which is Cu, wherein at least the first internal electrode layer of the first and second internal electrode layers contains a low-melting-point metal having a melting point lower than the melting point of Pb, the concentration of the low-melting-point metal being higher in the first internal electrode layer than in the second internal electrode layer, the width of the portion of the first internal electrode layer that connects to the first external electrode in a direction perpendicular to the stacking direction is narrower than the width of the portion facing the second internal electrode layer, and the width of the portion of the second internal electrode layer that connects to the second external electrode in a direction perpendicular to the stacking direction is wider than the width of the portion of the first internal electrode layer that connects to the first external electrode.

[0008] In the ceramic electronic component, the low-melting-point metal may be Sn.

[0009] In the ceramic electronic component, the second internal electrode layers may contain a metal element other than the low-melting-point metal that forms a stable compound with hydrogen.

[0010] In the ceramic electronic component, the metal element that forms a stable compound with hydrogen may be at least one of Ag, Au, Ga, and Ge.

[0011] In the ceramic electronic component, a width in a direction perpendicular to the stacking direction of a portion of the second internal electrode layer that is connected to the second external electrode may be the same as a width of a portion of the second internal electrode layer that faces the first internal electrode layer.

[0012] In the ceramic electronic component, a width of a portion of the first internal electrode layer that is connected to the first external electrode may be 60% or more and 90% or less of a width of a portion that faces the second internal electrode layer in a direction perpendicular to the stacking direction.

[0013] In the ceramic electronic component, a third internal electrode layer connected to the first external electrode may be provided in a central portion in the stacking direction, and a width of a portion of the third internal electrode layer connected to the first external electrode in a direction perpendicular to the stacking direction may be the same as a width of a portion facing the second internal electrode layer.

[0014] In the ceramic electronic component, the number of the third internal electrode layers may be 5% or more and 40% or less of the internal electrode layers connected to the first external electrode.

[0015] In the ceramic electronic component, in the direction in which the first end face and the second end face face each other, a length of a portion of the first internal electrode layer that is connected to the first external electrode and is narrower than a width of a portion that faces the second internal electrode layer may be greater than or equal to 1 / 4 and less than or equal to 1 / 1 of the length of the first external electrode.

[0016] In the ceramic electronic component, the first internal electrode layers and the second internal electrode layers may be stacked in the second direction.

[0017] In the ceramic electronic component, the first internal electrode layers and the second internal electrode layers may be stacked in the third direction.

[0018] A method for manufacturing a ceramic electronic component according to the present invention includes: a ceramic electronic component in which first internal electrode layers mainly composed of Ni and second internal electrode layers mainly composed of Ni are alternately laminated with dielectric layers sandwiched therebetween, the ceramic electronic component has a substantially rectangular parallelepiped shape; the first internal electrode layers and the second internal electrode layers are alternately drawn out to first end faces and second end faces opposing the substantially rectangular parallelepiped shape; when a first direction, a second direction, and a third direction in which the first end faces and the second end faces oppose each other are orthogonal to each other, the dimension in the second direction is 1.3 times or more the dimension in the third direction; and at least the first internal electrode layers of the first internal electrode layers and the second internal electrode layers contain a metal oxide layer containing Pb. The method includes the steps of preparing a laminated chip containing a low-melting point metal having a melting point lower than the melting point of the first internal electrode layer, the concentration of the low-melting point metal being higher in the first internal electrode layer than in the second internal electrode layer, the width of the portion of the first internal electrode layer extended to the first end face in a direction perpendicular to the stacking direction being narrower than the width of the portion facing the second internal electrode layer, and the width of the portion of the second internal electrode layer extended to the second end face in a direction perpendicular to the stacking direction being wider than the width of the portion of the first internal electrode layer extended to the first end face, and firing external electrodes mainly composed of Cu to each of the first end face and the second end face.

[0019] According to the present invention, it is possible to provide a ceramic electronic component that can suppress the occurrence of cracks, and a method for manufacturing the same.

[0020] 1 is an external view of the multilayer ceramic capacitor in accordance with the first embodiment; FIG. 2 is a partial cross-sectional perspective view of the multilayer ceramic capacitor in accordance with the first embodiment; FIG. 3 is a cross-sectional view taken along line A-A in FIG. 2; FIG. 4 is a cross-sectional view taken along line B-B in FIG. 2; (a) is an enlarged cross-sectional view of the vicinity of the first external electrode, and (b) is an enlarged cross-sectional view of the vicinity of the second external electrode; FIG. 5 is a diagram illustrating a crack; (a) is a plan view of the first internal electrode layer, and (b) is a plan view of the second internal electrode layer 12b; FIG. 6 is a diagram illustrating the wraparound length of the external electrodes; FIG. 7 is a diagram illustrating a flow of a manufacturing method of a multilayer ceramic capacitor; FIG. 8 is a diagram illustrating a lamination step; (a) is a plan view of the first internal electrode layer, and (b) is a plan view of the second internal electrode layer; FIG. 9 is a diagram illustrating a first end face of a laminated chip; FIG. 10 is a diagram illustrating a lamination step; (a) and (b) are partial cross-sectional perspective views of the multilayer ceramic capacitor in accordance with a third embodiment; FIG. 11 is a diagram illustrating the first internal electrode layer; FIG. 12 is a diagram illustrating a lamination step; (a) and (b) are partial cross-sectional perspective views of the multilayer ceramic capacitor in accordance with a fourth embodiment; 1 is a diagram illustrating an example of the shapes of a first internal electrode layer, a second internal electrode layer, and a third internal electrode layer; FIG. 2 is a diagram illustrating a lamination process; FIG. 3 is a side view of a circuit board including a multilayer ceramic capacitor; FIG. 4 is a diagram illustrating an example of a packaging body; FIG. 5 is a diagram illustrating an example of a packaging body;

[0021] Hereinafter, embodiments will be described with reference to the drawings.

[0022] First Embodiment FIG. 1 is an external view of a multilayer ceramic capacitor 100 according to a first embodiment. As illustrated in FIG. 1 , the multilayer ceramic capacitor 100 includes a laminated chip 10 having a substantially rectangular parallelepiped shape, and a first external electrode 20a and a second external electrode 20b provided on two opposing end surfaces of the laminated chip 10. Of the four surfaces of the laminated chip 10 other than the two end surfaces, the two surfaces at both ends in the stacking direction are referred to as the top surface and bottom surface. The other two surfaces other than the two end surfaces, top surface, and bottom surface are referred to as side surfaces. The external electrodes 20a and 20b extend on the top surface, bottom surface, and two side surfaces of the laminated chip 10 in the stacking direction. However, the first external electrode 20a and the second external electrode 20b are spaced apart from each other.

[0023] The T direction (first direction) is the stacking direction of each layer in the laminated chip 10, the height direction of the laminated ceramic capacitor 100, and the direction in which the upper and lower surfaces of the laminated chip 10 face each other. The W direction (second direction) is the direction in which the two side surfaces of the laminated chip 10 face each other. The L direction (third direction) is the direction in which the two end surfaces of the laminated chip 10 face each other, and the direction in which the first external electrode 20a and the second external electrode 20b face each other. The L direction, W direction, and T direction are perpendicular to each other. As illustrated in FIG. 1 , the height of the laminated ceramic capacitor 100 in the T direction is referred to as the height T 0 The width in the W direction is W 0 The length in the L direction is length L 0 In addition, the height T 0 , width W 0 , and length L 0 , are the maximum dimensions in the T, W, and L directions, respectively.

[0024] FIG. 2 is a partial cross-sectional perspective view of the multilayer ceramic capacitor 100. FIG. 3 is a cross-sectional view taken along line A-A in FIG. 2. FIG. 4 is a cross-sectional view taken along line B-B in FIG. 2. As illustrated in FIGS. 2 to 4, the multilayer chip 10 has a configuration in which dielectric layers 11 containing a ceramic material that functions as a dielectric and internal electrode layers are alternately stacked. The internal electrode layers include a plurality of first internal electrode layers 12a and a plurality of second internal electrode layers 12b. The first internal electrode layers 12a and the second internal electrode layers 12b are alternately stacked. The edges of the first internal electrode layers 12a extend to the first end surface of the multilayer chip 10 on which the first external electrode 20a is provided. The edges of the second internal electrode layers 12b extend to the second end surface of the multilayer chip 10 on which the second external electrode 20b is provided. As a result, the first internal electrode layers 12a and the second internal electrode layers 12b are alternately electrically connected to the first external electrode 20a and the second external electrode 20b. As a result, the multilayer ceramic capacitor 100 has a configuration in which capacitor units are stacked. In addition, in a laminate of the dielectric layers 11 and the internal electrode layers, the internal electrode layers are arranged as the outermost layers in the stacking direction, and the upper and lower surfaces of the laminate are covered with cover layers 13. The cover layers 13 are mainly composed of a ceramic material. For example, the composition of the cover layers 13 may be the same as or different from that of the dielectric layers 11.

[0025] The multilayer ceramic capacitor 100 according to this embodiment has a shape in which the size in the T direction is larger than the size in the W direction. Specifically, as illustrated in FIG. 0 ≧W 0 × 1.3. By adopting such a configuration, the capacitance can be increased. 0 , width W 0 , and length L 0 is not particularly limited, but for example, the height T 0 can be set to 0.15 mm or more and 1.0 mm or less, and the width W 0 can be set to 0.1 mm or more and 0.7 mm, and the length L 0 In order to realize a high capacity, T 0 Is W 0 It is preferably 1.5 times or more, and more preferably 2.0 times or more.

[0026] The dielectric layer 11 is, for example, a compound represented by the general formula ABO 3 The main phase is a ceramic material having a perovskite structure represented by the formula: 3-α For example, the ceramic material includes BaTiO 3 (barium titanate), CaZrO 3 (Calcium zirconate), CaTiO 3 (Calcium titanate), SrTiO 3 (strontium titanate), MgTiO 3 (magnesium titanate), Ba that forms a perovskite structure 1-x-y Ca x Sr y Ti 1-z Zr z O 3 (0≦x≦1, 0≦y≦1, 0≦z≦1) and the like. 1-x-y Ca x Sr y Ti 1-z Zr z O3 are barium strontium titanate, barium calcium titanate, barium zirconate, barium titanate zirconate, calcium titanate zirconate, barium calcium titanate zirconate, etc. The thickness of the dielectric layer 11 is, for example, 0.3 μm or more and 3 μm or less.

[0027] The cover layer 13 may be, for example, a polymer having the general formula ABO 3 The main phase is a ceramic material having a perovskite structure represented by the formula: 3-α For example, the ceramic material includes BaTiO 3 (barium titanate), CaZrO 3 (Calcium zirconate), CaTiO 3 (Calcium titanate), SrTiO 3 (strontium titanate), MgTiO 3 (magnesium titanate), Ba that forms a perovskite structure 1-x-y Ca x Sr y Ti 1-z Zr z O 3 (0≦x≦1, 0≦y≦1, 0≦z≦1) and the like. 1-x-y Ca x Sr y Ti 1-z Zr z O 3 Examples of the dielectric layer 11 include barium strontium titanate, barium calcium titanate, barium zirconate, barium titanate zirconate, calcium titanate zirconate, and barium calcium titanate zirconate. The main component of the cover layer 13 may be the same as or different from that of the dielectric layer 11.

[0028] Additives may be added to the dielectric layer 11 and the cover layer 13. Examples of additives to the dielectric layer 11 and the cover layer 13 include oxides of magnesium (Mg), manganese (Mn), molybdenum (Mo), vanadium (V), chromium (Cr), rare earth elements (yttrium (Y), samarium (Sm), europium (Eu), gadolinium (Gd), terbium (Tb), dysprosium (Dy), holmium (Ho), erbium (Er), thulium (Tm), and ytterbium (Yb)), oxides containing cobalt (Co), nickel (Ni), lithium (Li), boron (B), sodium (Na), potassium (K), or silicon (Si), or glasses containing Co, Ni, Li, B, Na, K, or Si.

[0029] The first internal electrode layer 12a and the second internal electrode layer 12b are mainly composed of Ni. For example, the first internal electrode layer 12a and the second internal electrode layer 12b contain 85 at% or more of Ni. The first internal electrode layer 12a and the second internal electrode layer 12b may contain ceramic particles or the like as a co-material. The thickness of the first internal electrode layer 12a and the second internal electrode layer 12b is, for example, 0.1 μm or more and 2 μm or less.

[0030] 3, the region where the first internal electrode layer 12a connected to the first external electrode 20a and the second internal electrode layer 12b connected to the second external electrode 20b face each other is a region where capacitance is generated in the multilayer ceramic capacitor 100. Therefore, this region where capacitance is generated is referred to as a capacitance portion 14. In other words, the capacitance portion 14 is a region where adjacent internal electrode layers connected to different external electrodes face each other.

[0031] The region where the first internal electrode layers 12a connected to the first external electrode 20a face each other in the stacking direction without the second internal electrode layer 12b connected to the second external electrode 20b intervening therebetween is referred to as the first end margin 15a. The region where the second internal electrode layers 12b connected to the second external electrode 20b face each other in the stacking direction without the first internal electrode layer 12a connected to the first external electrode 20a intervening therebetween is referred to as the second end margin 15b. Each end margin is a region where internal electrode layers connected to the same external electrode face each other in the stacking direction without the internal electrode layer connected to a different external electrode intervening therebetween. The first end margin 15a and the second end margin 15b are regions that do not generate electrical capacitance.

[0032] As illustrated in Figure 4, in the laminated chip 10, the side margin 16 is a region provided to cover the ends (ends in the W direction) of two side surfaces of the dielectric layer 11, the first internal electrode layer 12a, and the second internal electrode layer 12b. That is, in Figure 4, the side margin 16 is a region provided outside the capacitance section 14 in the W direction. In other words, the side margin 16 is an outer region adjacent to the capacitance section 14 when viewed from the stacking direction, and is an outer region adjacent to the capacitance section 14 on the side where the internal electrode layers are not drawn out. The side margin 16 is also a region that does not generate electrical capacitance.

[0033] Fig. 5(a) is an enlarged cross-sectional view of the vicinity of the first external electrode 20a. Hatching is omitted in Fig. 5(a). As illustrated in Fig. 5(a), the first external electrode 20a has a structure in which a plating layer 22a is provided on an underlayer 21a. The underlayer 21a functions as a contact layer that contacts the first end surface of the laminated chip 10. The underlayer 21a is mainly composed of Cu. The underlayer 21a may also contain a glass component. The underlayer 21a contains 80 at% or more of Cu.

[0034] The plating layer 22a is primarily composed of a metal such as Ni, Cu, Al (aluminum), Zn (zinc), or Sn, or an alloy of two or more of these metals. The plating layer 22a may be a plating layer of a single metal component, or may be a plurality of plating layers of different metal components. For example, in FIG. 5( a), the plating layer 22a has a structure in which a first plating layer 23a and a second plating layer 24a are formed in this order from the base layer 21a side. The first plating layer 23a is, for example, a Ni plating layer. The second plating layer 24a is, for example, a Sn plating layer.

[0035] Fig. 5(b) is an enlarged cross-sectional view of the vicinity of the second external electrode 20b. Hatching is omitted in Fig. 5(b). As illustrated in Fig. 5(b), the second external electrode 20b has a structure in which a plating layer 22b is provided on an underlayer 21b. The underlayer 21b functions as a contact layer that contacts the second end surface of the laminated chip 10. The underlayer 21b is mainly composed of Cu. The underlayer 21b may also contain a glass component. The underlayer 21a contains 80 at% or more of Cu.

[0036] The plating layer 22b is primarily composed of a metal such as Ni, Cu, Al, Zn, or Sn, or an alloy of two or more of these metals. The plating layer 22b may be a plating layer of a single metal component, or may be a plurality of plating layers of different metal components. For example, the plating layer 22b may have a structure in which a first plating layer 23b and a second plating layer 24b are formed in this order from the base layer 21b side. The first plating layer 23b is, for example, a Ni plating layer. The second plating layer 24b is, for example, a Sn plating layer.

[0037] The base layer 21a and the base layer 21b may have the same composition or different compositions. The plating layer 22a and the plating layer 22b may have the same layered structure or different layered structures. For example, the number of layers of the plating layers may be different. The first plating layer 23a and the first plating layer 23b may have the same composition or different compositions. The second plating layer 24a and the second plating layer 24b may have the same composition or different compositions.

[0038] The first internal electrode layer 12a contains a low-melting-point metal in addition to the main component Ni. The low-melting-point metal is a metal having a melting point lower than that of lead (Pb (melting point: 327.5°C)). For example, it includes bismuth (Bi (melting point: 271.4°C)), Sn (melting point: 231.97°C), indium (In (melting point: 156.61°C)), etc. The second internal electrode layer 12b does not contain a low-melting-point metal. The second internal electrode layer 12b may contain a low-melting-point metal, but the concentration of the low-melting-point metal is lower in the second internal electrode layer 12b than in the first internal electrode layer 12a.

[0039] This configuration can change the stress distribution inside the multilayer ceramic capacitor 100, thereby improving mechanical strength such as flexural strength. For example, in the first internal electrode layer 12a, when the main component Ni is 100 at%, the low-melting-point metal is contained at 0.5 at% to 3 at% inclusive, 0.7 at% to 2 at% inclusive, or 1 at% to 1.5 at% inclusive. In the second internal electrode layer 12b, when the main component Ni is 100 at% inclusive, the low-melting-point metal is contained at 0.5 at% or less, 0.3 at% or less, or 0.1 at% or less.

[0040] When multiple types of low melting point metals are contained, the concentration of the low melting point metals means the atomic percentage of the total amount of all the low melting point metals when Ni is taken as 100 atomic percentage.

[0041] In the multilayer ceramic capacitor 100, when the first external electrode 20a and the second external electrode 20b are baked, a crack 40 as shown in Figure 6 may occur in the area where the cover layer and the side margin, which are covered by the external electrodes, overlap (the corner near the external electrodes).

[0042] This occurs based on the following mechanism: When the internal electrode layers react with the base layers 21a, 21b during baking of the base layers 21a, 21b, Cu, a metal component of the base layers 21a, 21b, diffuses toward the Ni side of the internal electrode layers, causing the internal electrode layers to expand. This expansion of the internal electrode layers generates outward stress in the cover layer 13 and the side margins 16, resulting in cracks. In particular, if the internal electrode layers contain a low-melting-point metal, the diffusion of the external electrode components toward the internal electrode side is promoted during baking of the external electrodes, making the occurrence of cracks 40 a greater problem.

[0043] The multilayer ceramic capacitor 100 according to this embodiment has a configuration that can suppress the occurrence of the cracks 40. Details will be described below.

[0044] FIG. 7A is a plan view of the first internal electrode layer 12a. As illustrated in FIG. 7A, the first internal electrode layer 12a has a first region 121 (lead portion) connected to the first external electrode 20a in a region corresponding to the first end margin 15a and having a width W1, and a second region 122 in a region corresponding to the capacitance portion 14 and having a width W2. The second region 122 faces the second internal electrode layer 12b. The width W1 is smaller than the width W2. The widths W1 and W2 refer to the widths in the W direction, i.e., the widths in the direction perpendicular to the stacking direction. This configuration narrows the diffusion path of Cu when the first external electrode 20a is baked. This suppresses Cu diffusion even if the first internal electrode layer 12a contains a low-melting-point metal. This suppresses the occurrence of cracks 40.

[0045] The first region 121 may have a shape such that its width narrows as it approaches the first external electrode 20 a. In this case, the width W1 refers to the width of the portion where the first region 121 is connected to the first external electrode 20 a.

[0046] 7B is a plan view of the second internal electrode layer 12b. As illustrated in FIG. 7B, the width in the W direction of the portion of the second internal electrode layer 12b that connects to the second external electrode 20b is wider than the width in the W direction of the first region 121. For example, the width in the W direction of the second internal electrode layer 12b is substantially constant at any point in the L direction. For example, the width in the W direction of the portion of the second internal electrode layer 12b that connects to the second external electrode 20b is substantially equal to W2. This configuration ensures good contact between the second internal electrode layer 12b and the second external electrode 20b, ensuring the capacitance of the multilayer ceramic capacitor 100.

[0047] For example, if W1 / W2 is small, there is a risk of a decrease in capacity due to poor contact between the first external electrode 20a and the first internal electrode layer 12a. Therefore, it is preferable to set a lower limit for W1 / W2. In this embodiment, when W2 is 100%, W1 is preferably 60% or more, and more preferably 70% or more. On the other hand, from the viewpoint of suppressing cracks 40 due to expansion of the first internal electrode layer 12a, W1 is preferably 90% or less, and more preferably 80% or less.

[0048] Furthermore, from the viewpoint of suppressing cracks 40 due to expansion of the first internal electrode layer 12a, the length in the L direction of the first region 121 is preferably ¼ or more, and more preferably ½ or more, of the wraparound length in the L direction of the first external electrode 20a (dimension e in FIG. 8 ). On the other hand, from the viewpoint of ensuring the intersection area between the first internal electrode layer 12a and the second internal electrode layer 12b, the length in the L direction of the first region 121 is preferably ½ or less, and more preferably ¾ or less of dimension e.

[0049] Next, a description will be given of a method for manufacturing the multilayer ceramic capacitor 100 according to the first embodiment.

[0050] (Step of Preparing Raw Material Powder) First, a dielectric material is prepared for forming the dielectric layer 11. The A-site elements and B-site elements contained in the dielectric layer 11 are usually ABO 3 The dielectric layer 11 contains a sintered body of BaTiO particles.3 is a tetragonal compound with a perovskite structure and exhibits a high dielectric constant. 3 Generally, it can be obtained by synthesizing barium titanate by reacting a titanium raw material such as titanium dioxide with a barium raw material such as barium carbonate. Various methods have been known for synthesizing the ceramic that is the main component of the dielectric layer 11, such as a solid-phase method, a sol-gel method, and a hydrothermal method. Any of these methods can be used in this embodiment.

[0051] To the obtained ceramic powder, a predetermined additive compound is added depending on the purpose. Examples of the additive compound include oxides of Mg, Mn, Mo, V, Cr, rare earth elements (Y, Sm, Eu, Gd, Tb, Dy, Ho, Er, Tm, and Yb), oxides containing Co, Ni, Li, B, Na, K, or Si, and glasses containing Co, Ni, Li, B, Na, K, or Si. Of these, SiO is mainly used. 2 functions as a sintering aid.

[0052] For example, a ceramic material is prepared by wet-mixing a ceramic raw material powder with a compound containing an additive compound, followed by drying and pulverization. For example, the ceramic material obtained as described above may be pulverized as necessary to adjust the particle size, or may be combined with a classification process to adjust the particle size. A dielectric material is obtained by the above process.

[0053] (Lamination Process) Next, a binder such as polyvinyl butyral (PVB) resin, an organic solvent such as ethanol or toluene, and a plasticizer are added to the obtained raw material powder and wet mixed. Using the obtained slurry, a dielectric green sheet is coated on a substrate by, for example, a die coater method or a doctor blade method, and then dried. The substrate is, for example, a polyethylene terephthalate (PET) film.

[0054] Next, the internal electrode pattern 52a is formed on the dielectric green sheet 51, which constitutes a first lamination unit. The internal electrode pattern 52a corresponds to the shape of the first internal electrode layer 12a. The width of the internal electrode pattern 52a is set to approximately match the width of the dielectric green sheet 51. A metal paste containing the metal component of the first internal electrode layer 12a is used for the internal electrode pattern 52a. The film formation method may be printing, sputtering, vapor deposition, etc. Furthermore, the internal electrode pattern 52 is formed on the dielectric green sheet 51, which constitutes a second lamination unit. The internal electrode pattern 52 corresponds to the shape of the second internal electrode layer 12b. The width of the internal electrode pattern 52 is set to approximately match the width of the dielectric green sheet 51. A metal paste containing the metal component of the second internal electrode layer 12b is used for the internal electrode pattern 52. The film formation method may be printing, sputtering, vapor deposition, etc.

[0055] Next, while peeling the dielectric green sheet 51 from the substrate, the first and second stacking units are alternately stacked as shown in FIG. 10 . Next, a predetermined number of cover sheets 53 (e.g., 2 to 10 layers) are stacked on top and bottom of the laminate obtained by stacking the first and second stacking units, and are thermocompression bonded. The cover sheets 53 can be formed by the same method as the dielectric green sheet 51. Next, a plurality of side margin sheets 54 are attached to each of both side surfaces of the laminate. The side margin sheets 54 can be formed by the same method as the dielectric green sheet 51.

[0056] (Firing step) After that, the oxygen partial pressure is 10 -5 ~10 -8 The mixture is fired in a reducing atmosphere at 1100 to 1300° C. for 10 minutes to 2 hours.

[0057] (Reoxidation treatment step) Then, N 2 A reoxidation treatment may be carried out in a gas atmosphere at 600° C. to 1000° C.

[0058] (Coating Step) Next, a metal paste that will become the underlayers 21a and 21b is coated on the first side surface of the laminate by a dipping method, etc. This metal paste contains a glass component such as glass frit.

[0059] (Baking Step) Next, the metal paste is baked at a temperature of about 700° C. to 900° C. to form the underlayers 21a and 21b.

[0060] (Plating Process) Thereafter, the base layers 21 a, 21 b may be coated with a metal such as Cu, Ni, or Sn by plating. For example, a first plating layer and a second plating layer are formed in this order on the base layers 21 a, 21 b. This completes the multilayer ceramic capacitor 100.

[0061] According to the manufacturing method of this embodiment, the diffusion path of Cu is narrowed when the first external electrode 20a is baked. As a result, even if the first internal electrode layer 12a contains a low-melting-point metal, Cu diffusion is suppressed. As a result, the occurrence of cracks 40 is suppressed. Meanwhile, the width in the W direction of the portion of the second internal electrode layer 12b that connects to the second external electrode 20b is wider than the width in the W direction of the first region 121. As a result, good contact is achieved between the second internal electrode layer 12b and the second external electrode 20b, and the capacitance of the multilayer ceramic capacitor 100 is ensured.

[0062] Second Embodiment In the first embodiment, all of the internal electrode layers connected to the first external electrode 20a include the first region 121, but some of the internal electrode layers may include the first region 121. The multilayer ceramic capacitor 100a according to the second embodiment has a configuration in which some of all of the internal electrode layers connected to the first external electrode 20a include the first region 121.

[0063] Of all the internal electrode layers connected to the first external electrode 20a, some are third internal electrode layers 12c. FIG. 11( a) is a plan view of the first internal electrode layer 12a. FIG. 11( b) is a plan view of the third internal electrode layer 12c. As illustrated in FIG. 11( b), the width in the W direction of the portion of the third internal electrode layer 12c connected to the first external electrode 20a is wider than the width in the W direction of the first region 121. For example, the width in the W direction of the third internal electrode layer 12c is approximately constant at any point in the L direction. For example, the width in the W direction of the portion of the third internal electrode layer 12c connected to the first external electrode 20a is approximately equal to W2. This configuration ensures good contact between the third internal electrode layer 12c and the first external electrode 20a, ensuring the capacitance of the multilayer ceramic capacitor 100.

[0064] FIG. 12 is a diagram illustrating a first end surface of the laminated chip 10. That is, FIG. 12 is a view of the end surface of the laminated chip 10 viewed through the first external electrode 20a in the multilayer ceramic capacitor 100a. As illustrated in FIG. 12, one or more third internal electrode layers 12c are provided in the center of the stacking direction without the first internal electrode layers 12a interposed therebetween. The first internal electrode layers 12a are provided further outward in the T direction than a group of these third internal electrode layers 12c. This configuration narrows the width of the internal electrode layers in the W direction in the region close to the cover layer 13. This suppresses diffusion in corners where cracks 40 are likely to occur, thereby suppressing cracks 40. Meanwhile, good contact between the internal electrode layers and the first external electrode 20a is achieved near the center of the stacking direction. As a result, it is possible to both suppress cracks 40 and ensure capacitance.

[0065] For example, if the number of third internal electrode layers 12c is small, there is a risk that sufficient capacitance cannot be ensured. Therefore, it is preferable to set a lower limit on the number of third internal electrode layers 12c. On the other hand, if the number of third internal electrode layers 12c is large, there is a risk that the occurrence of cracks 40 cannot be sufficiently suppressed. Therefore, it is preferable to set a lower limit and an upper limit on the number of third internal electrode layers 12c. In this embodiment, when all internal electrode layers connected to the first external electrode 20a are taken as 100%, it is preferable that the number of third internal electrode layers 12c is 5% or more and 40% or less.

[0066] In the multilayer ceramic capacitor 100a according to this embodiment, for example, as illustrated in FIG. 13, when stacking the multilayer units, a third stack unit in which an internal electrode pattern 52b having the same width as the dielectric green sheet 51 is formed on the dielectric green sheet 51 is used in the central portion instead of a first stack unit in which an internal electrode pattern 52a is formed on the dielectric green sheet 51.

[0067] Third Embodiment Figures 14(a) and 14(b) are partial cross-sectional perspective views of a multilayer ceramic capacitor 100b according to a third embodiment. The multilayer ceramic capacitor 100b differs from the multilayer ceramic capacitor 100 according to the first embodiment in the stacking direction of the first internal electrode layers 12a and the second internal electrode layers 12b. In this embodiment, the W direction (second direction) corresponds to the stacking direction of the first internal electrode layers 12a and the second internal electrode layers 12b, and is the direction in which the upper and lower surfaces of the laminated chip 10 face each other. The T direction (first direction) is the direction in which two side surfaces of the laminated chip 10 face each other. The L direction (third direction) is the direction in which two end surfaces of the laminated chip 10 face each other.

[0068] In this embodiment, the dimension of the first internal electrode layer 12a in the T direction is varied. As illustrated in FIG. 15 , the first region 121 is connected to the first external electrode 20a in a region corresponding to the first end margin 15a and has a dimension T1 in the T direction. The second region 122 has a dimension T2 in the T direction in a region corresponding to the capacitance section 14. Dimension T1 is smaller than dimension T2. ​​This configuration narrows the diffusion path of Cu when the first external electrode 20a is baked. This suppresses Cu diffusion even if the first internal electrode layer 12a contains a low-melting-point metal. This suppresses the occurrence of cracks 40.

[0069] The first region 121 may have a shape that narrows toward the first external electrode 20 a. In this case, the dimension T1 is the width of the portion where the first region 121 is connected to the first external electrode 20 a.

[0070] The dimension in the T direction of the portion of the second internal electrode layer 12b that is connected to the second external electrode 20b is larger than the dimension in the T direction of the first region 121. For example, the dimension in the T direction of the second internal electrode layer 12b is approximately constant at any point in the L direction. For example, the dimension in the T direction of the portion of the second internal electrode layer 12b that is connected to the second external electrode 20b is approximately equal to T2. This configuration ensures good contact between the second internal electrode layer 12b and the second external electrode 20b, ensuring the capacitance of the multilayer ceramic capacitor 100b.

[0071] For example, if T1 / T2 is small, there is a risk of a decrease in capacity due to poor contact between the first external electrode 20a and the first internal electrode layer 12a. Therefore, it is preferable to set a lower limit for T1 / T2. In this embodiment, when T2 is 100%, T1 is preferably 60% or more, and more preferably 70% or more. On the other hand, from the viewpoint of suppressing cracks 40 due to expansion of the first internal electrode layer 12a, T1 is preferably 90% or less, and more preferably 80% or less.

[0072] Furthermore, from the viewpoint of suppressing cracks 40 due to expansion of the first internal electrode layer 12a, the length in the L direction of the first region 121 is preferably ¼ or more, and more preferably ½ or more, of the wraparound length in the L direction (dimension e) of the first external electrode 20a. On the other hand, from the viewpoint of ensuring the intersection area between the first internal electrode layer 12a and the second internal electrode layer 12b, the length in the L direction of the first region 121 is preferably ½ or less, and more preferably ¾ or less of dimension e.

[0073] In the lamination process of FIG. 9 , the multilayer ceramic capacitor 100b is produced by alternately laminating first lamination units, each having an internal electrode pattern 52a formed on a dielectric green sheet 51, and second lamination units, each having an internal electrode pattern 52 formed on a dielectric green sheet 51, in the W direction, as illustrated in FIG. 16 . The internal electrode pattern 52a corresponds to the shape of the first internal electrode layer 12a. The internal electrode pattern 52 corresponds to the shape of the second internal electrode layer 12b. Next, in the laminate obtained by laminating the first lamination units and the second lamination units, a predetermined number of cover sheets 53 (e.g., 2 to 10 layers) are laminated and thermocompression bonded to both ends in the W direction. The cover sheets 53 can be formed using the same method as the dielectric green sheets 51. Next, a plurality of side margin sheets 54 are attached to both ends in the T direction of the laminate. The side margin sheets 54 can be formed using the same method as the dielectric green sheets 51.

[0074] 17(a) and 17(b) are partial cross-sectional perspective views of a multilayer ceramic capacitor 100c according to a fourth embodiment. The multilayer ceramic capacitor 100c differs from the multilayer ceramic capacitor 100a according to the second embodiment in the stacking direction of the first internal electrode layers 12a, the second internal electrode layers 12b, and the third internal electrode layers 12c. In this embodiment, the W direction (second direction) corresponds to the stacking direction of the first internal electrode layers 12a, the second internal electrode layers 12b, and the third internal electrode layers 12c, and is the direction in which the upper and lower surfaces of the laminated chip 10 face each other. The T direction (first direction) is the direction in which two side surfaces of the laminated chip 10 face each other. The L direction (third direction) is the direction in which two end surfaces of the laminated chip 10 face each other.

[0075] 18 is a diagram illustrating the shapes of the first internal electrode layer 12a, the second internal electrode layer 12b, and the third internal electrode layer 12c. As illustrated in FIG. 18, the width in the T direction of the portion of the third internal electrode layer 12c that connects to the first external electrode 20a is wider than the width in the T direction of the first region 121. For example, the width in the T direction of the third internal electrode layer 12c is approximately constant at any point in the L direction. This configuration ensures good contact between the third internal electrode layer 12c and the first external electrode 20a, ensuring the capacitance of the multilayer ceramic capacitor 100.

[0076] As illustrated in FIG. 17( b), one or more third internal electrode layers 12c are provided in the center of the stacking direction without first internal electrode layers 12a in between. The first internal electrode layers 12a are provided further outward in the W direction than a group of these third internal electrode layers 12c. This configuration narrows the width of the internal electrode layers in the T direction in regions close to the cover layer 13. This suppresses diffusion in corners where cracks 40 are likely to occur, thereby suppressing cracks 40. Meanwhile, good contact between the internal electrode layers and the first external electrode 20a is achieved near the center of the stacking direction. As a result, it is possible to both suppress cracks 40 and ensure capacitance.

[0077] For example, if the number of third internal electrode layers 12c is small, there is a risk that sufficient capacitance cannot be ensured. Therefore, it is preferable to set a lower limit on the number of third internal electrode layers 12c. On the other hand, if the number of third internal electrode layers 12c is large, there is a risk that the occurrence of cracks 40 cannot be sufficiently suppressed. Therefore, it is preferable to set a lower limit and an upper limit on the number of third internal electrode layers 12c. In this embodiment, when all internal electrode layers connected to the first external electrode 20a are taken as 100%, it is preferable that the number of third internal electrode layers 12c is 5% or more and 40% or less.

[0078] In the multilayer ceramic capacitor 100c according to this embodiment, for example, as illustrated in FIG. 19 , when stacking the laminate units, a third laminate unit in which an internal electrode pattern 52b having the same width as the dielectric green sheet 51 is formed on the dielectric green sheet 51 is used in the central portion in the stacking direction instead of a first laminate unit in which an internal electrode pattern 52a is formed on the dielectric green sheet 51.

[0079] Now, the mounting of the multilayer ceramic capacitors 100b and 100c will be described. Fig. 20 is a side view of a circuit board 200 including the multilayer ceramic capacitors 100b and 100c. The circuit board 200 has a mounting substrate 210 on which the multilayer ceramic capacitors 100b and 100c are mounted. The mounting substrate 210 has a base material 211 that extends along a plane in the L direction and the W direction and has a mounting surface G that is perpendicular to the T direction, and a pair of connection electrodes 212 provided on the mounting surface G.

[0080] In the circuit board 200, the first external electrodes 20a and the second external electrodes 20b of the multilayer ceramic capacitors 100b, 100c are respectively connected to a pair of connection electrodes 212 of the mounting substrate 210 via solder H. As a result, in the circuit board 200, the multilayer ceramic capacitors 100b, 100c are fixed to and electrically connected to the mounting substrate 210.

[0081] Here, in the multilayer ceramic capacitors 100b and 100c, it is known that when a voltage is applied to the first external electrode 20a and the second external electrode 20b via the connection electrode 212 of the mounting substrate 210 during operation of the circuit board 200, electrostriction occurs in the laminated chip 10 due to the piezoelectric effect. The electrostriction occurring in the laminated chip 10 causes a relatively large deformation in the stacking direction of the internal electrode layers.

[0082] In the circuit board 200, repeated electrostriction occurs in the multilayer ceramic capacitors 100b, 100c when an AC voltage is applied, which may cause vibration in the thickness direction of the substrate 211 of the mounting substrate 210. In the circuit board 200, when the vibration generated in the substrate 211 becomes large, noise may be generated from the substrate 211, which may cause a phenomenon known as "ringing noise."

[0083] However, in the multilayer ceramic capacitors 100b and 100c according to this embodiment, the lamination direction of the internal electrode layers is the in-plane direction of the substrate 211, and therefore vibrations in the thickness direction of the substrate 211 are unlikely to occur due to electrostriction of the laminated chip 10. Furthermore, in the multilayer ceramic capacitors 100b and 100c, the number of laminated internal electrode layers is small, and the amount of deformation due to electrostriction is kept small, so even if vibrations occur in the substrate 211, they are unlikely to be large enough to generate noise.

[0084] The multilayer ceramic capacitors 100b and 100c are prepared in a packaged state as a package 300 when mounted on a mounting substrate 210. Figures 21 and 22 are diagrams illustrating the package 300. Figure 21 is a partial plan view of the package 300. Figure 22 is a cross-sectional view of the package 300 taken along line DD in Figure 21.

[0085] The package 300 includes the multilayer ceramic capacitors 100b and 100c, a carrier tape 310, and a top tape 320. The carrier tape 310 is configured as a long tape extending in the W direction. The carrier tape 310 has a plurality of recesses 311 arranged at intervals in the W direction, each recess 311 accommodating one of the multilayer ceramic capacitors 100b and 100c.

[0086] The carrier tape 310 has a sealing surface P, which is an upward surface perpendicular to the T direction, and the plurality of recesses 311 are recessed downward in the T direction from the sealing surface P. In other words, the carrier tape 310 is configured so that the multilayer ceramic capacitors 100b, 100c in the plurality of recesses 311 can be removed from the sealing surface P side.

[0087] The carrier tape 310 is provided with a plurality of feed holes 312 that penetrate in the T direction and are arranged at intervals in the W direction at positions offset in the L direction from the row of the plurality of recesses 311. The feed holes 312 are configured as engagement holes that are used by the tape transport mechanism to transport the carrier tape 310 in the W direction.

[0088] In the package 300, the top tape 320 is attached to the seal surface P of the carrier tape 310 along the row of the recesses 311, and the recesses 311 accommodating the multilayer ceramic capacitors 100b, 100c are collectively covered by the top tape 320. This allows the multilayer ceramic capacitors 100b, 100c to be held in the recesses 311.

[0089] 22 , in the multilayer ceramic capacitors 100b and 100c in the recess 311 of the carrier tape 310, the first main surface M1 of the laminated chip 10 facing upward in the T direction faces the top tape 320. In addition, the second main surface M2 of the laminated chip 10 facing downward in the T direction faces the bottom surface of the recess 311.

[0090] When mounting the multilayer ceramic capacitors 100b, 100c packaged as the package 300, the top tape 320 is peeled off along the W direction from the seal surface P of the carrier tape 310. This allows the package 300 to sequentially open the multiple recesses 311 accommodating the multiple multilayer ceramic capacitors 100b, 100c upward in the T direction.

[0091] The multilayer ceramic capacitors 100b, 100c accommodated in the opened recess 110 are removed with the first main surface M1 of the laminated chip 10 facing upward in the T direction being sucked onto the tip of the suction nozzle of the mounting device. The mounting device moves the suction nozzle to move the multilayer ceramic capacitors 100b, 100c onto the mounting surface G of the mounting board 210.

[0092] Next, the mounting device positions the second main surface M2 of the laminated chip 10 opposite the mounting surface G, aligns the first external electrode 20a and the second external electrode 20b over the pair of connection electrodes 212 to which the solder paste has been applied, and then releases the suction nozzle from suction onto the first main surface M1 of the laminated chip 10. This places the laminated ceramic capacitors 100b and 100c on the mounting surface G.

[0093] Then, the solder paste is melted and then hardened using a reflow oven or the like on the mounting substrate 210 on which the multilayer ceramic capacitors 100b, 100c are placed on the mounting surface G. As a result, the first external electrode 20a and the second external electrode 20b are connected to the pair of connection electrodes 212 of the mounting substrate 210 via the solder H, thereby obtaining the circuit board 200 shown in FIG.

[0094] In each of the above embodiments, an element that forms a stable compound with hydrogen reduces the effect of hydrogen generated during the plating process and suppresses insulation deterioration. Therefore, it is preferable that the second internal electrode layer 12b contains an element that forms a stable compound with hydrogen other than a low-melting-point metal. Specifically, it is preferable that the second internal electrode layer 12b contains Ni as the main component, Ag (silver), Au (gold), Ga (gallium), Ge (germanium), etc.

[0095] Although the above embodiments have been described with reference to a multilayer ceramic capacitor as an example of a ceramic electronic component, the present invention is not limited to this. For example, the configurations of the above embodiments can be applied to other multilayer ceramic electronic components such as varistors and thermistors.

[0096] The multilayer ceramic capacitors according to the respective embodiments were fabricated and their characteristics were examined.

[0097] Example 1 In Example 1, the multilayer ceramic capacitor described in the first embodiment was fabricated. 3 A slurry containing the above as a main component was blended and coated to obtain a dielectric green sheet. An internal electrode pattern was printed on each dielectric green sheet to obtain a laminate unit. Nickel powder was used for the internal electrode pattern. In the first laminate unit, the width of the end of the internal electrode pattern was made smaller than the width of the dielectric green sheet. In addition, in the first laminate unit, 1.0 at% Sn was added when Ni was 100 at% in the internal electrode pattern. 350 layers of the obtained laminate unit were stacked to obtain a laminate. In the second laminate unit, Sn was not added to the internal electrode pattern.

[0098] Multiple cover sheets were laminated and pressed onto the top and bottom of the laminate in the stacking direction, followed by a binder removal process. The laminate was then fired and re-oxidized. A Cu-based metal paste was applied to the two end faces of the resulting laminated chip and baked at approximately 800°C. Through these processes, a multilayer ceramic capacitor with a length L of 600 μm, a width W of 300 μm, and a height T of 400 μm and 350 internal electrode layers was fabricated.

[0099] In the fired multilayer ceramic capacitor, the first internal electrode layer 12a and the second internal electrode layer 12b had a thickness of 0.5 μm, and each dielectric layer 11 had a thickness of 0.5 μm. The thickness of each cover layer in the T direction was 25 μm. The thickness of each side margin in the W direction was 25 μm. The width W2 of each internal electrode layer in the W direction was 250 μm. The width W1 of the first region 121 of the first internal electrode layer 12a was 200 μm. The length of the first region 121 of the first internal electrode layer 12a in the L direction was 50 μm. The dimension e of the first external electrode 20a was 150 μm. The number of stacked layers of the first internal electrode layer 12a was 175, and the number of stacked layers of the second internal electrode layer 12b was 175.

[0100] Example 2 In Example 2, the multilayer ceramic capacitor described in the second embodiment was fabricated. In Example 2, of the internal electrode layers connected to the first external electrode 20a, the central 95 layers in the lamination direction were designated as third internal electrode layers 12c, and the top and bottom 40 layers were designated as first internal electrode layers 12a. The thickness of the third internal electrode layers 12c was 0.5 μm. The width W2 of the third internal electrode layers 12c in the W direction was 250 μm. The other conditions were the same as in Example 1.

[0101] In Comparative Example 1, instead of the 175 first internal electrode layers 12a, internal electrode layers whose width in the W direction was constant at any point in the L direction were used. Other conditions were the same as in Example 1.

[0102] Example 3 In Example 3, the multilayer ceramic capacitor described in the first embodiment was fabricated. In Example 3, a multilayer ceramic capacitor was fabricated having a length L of 600 μm, a width W of 300 μm, and a height T of 500 μm, and having 450 laminated internal electrode layers.

[0103] In the fired multilayer ceramic capacitor, the first internal electrode layer 12a and the second internal electrode layer 12b had a thickness of 0.5 μm, and each dielectric layer 11 had a thickness of 0.5 μm. The thickness of each cover layer in the T direction was 25 μm. The thickness of each side margin in the W direction was 25 μm. The width W2 of each internal electrode layer in the W direction was 250 μm. The width W1 of the first region 121 of the first internal electrode layer 12a was 200 μm. The length of the first region 121 of the first internal electrode layer 12a in the L direction was 50 μm. The dimension e of the first external electrode 20a was 150 μm. The number of stacked layers of the first internal electrode layer 12a was 225, and the number of stacked layers of the second internal electrode layer 12b was 225. Other conditions were the same as in Example 1.

[0104] Example 4 In Example 4, the multilayer ceramic capacitor described in the second embodiment was fabricated. In Example 4, of the internal electrode layers connected to the first external electrode 20a, the central 125 layers in the lamination direction were designated as third internal electrode layers 12c, and the top and bottom 50 layers were designated as first internal electrode layers 12a. The thickness of the third internal electrode layers 12c was 0.5 μm. The width W2 of the third internal electrode layers 12c in the W direction was 250 μm. The other conditions were the same as in Example 3.

[0105] In Comparative Example 2, instead of the 225 first internal electrode layers 12a, internal electrode layers whose width in the W direction was constant at any point in the L direction were used. The other conditions were the same as in Example 3.

[0106] Example 5 In Example 5, the multilayer ceramic capacitor described in the third embodiment was fabricated. In Example 5, a multilayer ceramic capacitor was fabricated having a length L of 600 μm, a width W of 300 μm, and a height T of 500 μm, and having 250 laminated internal electrode layers.

[0107] In the fired multilayer ceramic capacitor, the thickness of the first internal electrode layer 12a and the second internal electrode layer 12b was 0.5 μm, and the thickness of each dielectric layer 11 was 0.5 μm. The thickness of each cover layer in the W direction was 25 μm. The thickness of each side margin in the T direction was 25 μm. The width T2 of each internal electrode layer in the T direction was 450 μm. The width T1 of the first region 121 of the first internal electrode layer 12a was 350 μm. The length of the first region 121 of the first internal electrode layer 12a in the L direction was 50 μm. The dimension e of the first external electrode 20a was 150 μm. The number of stacked layers of the first internal electrode layer 12a was 125, and the number of stacked layers of the second internal electrode layer 12b was 125. The other conditions were the same as in Example 1.

[0108] Example 6 In Example 6, the multilayer ceramic capacitor described in the fourth embodiment was fabricated. In Example 6, of the internal electrode layers connected to the first external electrode 20a, the central 65 layers in the stacking direction were designated as third internal electrode layers 12c, and 30 layers on either side of a group of third internal electrode layers 12c were designated as first internal electrode layers 12a. The thickness of the third internal electrode layers 12c was 0.5 μm. The width T2 of the third internal electrode layers 12c in the T direction was 450 μm. The other conditions were the same as in Example 5.

[0109] In Comparative Example 3, instead of the 125 first internal electrode layers 12a, internal electrode layers whose width in the T direction was constant at any point in the L direction were used. The other conditions were the same as in Example 5.

[0110] The results of the conditions for Examples 1 to 5 and Comparative Examples 1 to 3 are shown in Tables 1 and 2.

[0111] (Crack Generation) For each of Examples 1 to 6 and Comparative Examples 1 to 3, 100 samples were prepared, and the WT cross sections at the locations where the first external electrodes 20a were provided were observed. No cracks were observed in any of Examples 1 to 6. This is thought to be because the width of the end of the first internal electrode layer 12a on the first external electrode 20a side was narrowed, thereby suppressing expansion of the first internal electrode layer 12a due to diffusion of Cu from the first external electrode 20a. In contrast, in Comparative Examples 1 to 3, cracks were observed in at least one of the four corners. This is thought to be because the width of the internal electrode layer connected to the first external electrode 20a was not narrow.

[0112] (Capacitance) Next, the capacitance of 100 samples for each of Examples 1 to 6 was measured under conditions of 1 kHz and 0.5 Vrms. The average capacitance was calculated. In Example 1, the capacitance was 2.45 μF, in Example 2, the capacitance was 2.63 μF, in Example 3, the capacitance was 2.84 μF, in Example 4, the capacitance was 2.97 μF, in Example 5, the capacitance was 2.92 μF, and in Example 6, the capacitance was 3.01 μF. Thus, sufficient capacitance was obtained in all of Examples 1 to 6. This is thought to be because the width of the second internal electrode layer 12b connected to the second external electrode 20b was wide.

[0113] Furthermore, the average capacitance of the samples of Examples 2 and 4 was 5% or more higher than that of the samples of Examples 1 and 3. This is thought to be because the width of the lead-out portion of the internal electrode at the center in the height direction was not narrowed in the samples of Examples 2 and 4, so that the connection with the external electrode was sufficiently secured and a decrease in capacitance due to poor contact (so-called capacitance loss) was suppressed. Note that in Comparative Examples 1 to 3, the capacitance could not be measured due to poor insulation caused by cracks.

[0114] (Volume) For Examples 3 to 6, 100 samples for each were mounted on a substrate and the volume was measured. Specifically, an AC voltage of 5 V was applied to each sample while increasing the frequency from 0 to 1 MHz, and the intensity (unit: dB) of the audible sound generated at this time was measured individually in a soundproof, anechoic chamber (manufactured by Yokohama Sound Environment Systems) using a TYPe-3560-B130 manufactured by Brüel & Kjær Japan.

[0115] In Examples 3 and 4, it was confirmed that all samples exceeded 25 dB, which is the allowable value for acoustic noise. On the other hand, in Examples 5 and 6, it was confirmed that all samples had a volume below 25 dB. This is thought to be because, compared to the structures of Examples 3 and 4, Examples 5 and 6 have a smaller number of laminations, resulting in smaller electrostrictive vibrations, and because the layers are laminated in a direction that makes it difficult for electrostrictive vibrations to be transmitted to the substrate. Note that in Comparative Examples 1 to 3, cracks occurred and the volume could not be measured due to poor insulation.

[0116] The results of crack generation, capacitance, and sound volume are shown in Table 3.

[0117] Although the embodiments of the present invention have been described in detail above, the present invention is not limited to such specific embodiments, and various modifications and changes are possible within the scope of the gist of the present invention as described in the claims.

[0118] REFERENCE SIGNS LIST 10 laminated chip 11 dielectric layer 12a first internal electrode layer 12b second internal electrode layer 12c third internal electrode layer 13 cover layer 14 capacitance portion 15a first end margin 15b second end margin 16 side margin 20a first external electrode 20b second external electrode 21a, 21b underlayer 22a, 22b plating layer 23a, 23b first plating layer 24a, 24b second plating layer 51 dielectric green sheet 52 internal electrode pattern 53 cover sheet 54 side margin sheet 100 laminated ceramic capacitor 121 first region 122 second region

Claims

1. A capacitor having a dimension in a first direction that is 1.3 times or more the dimension in a second direction perpendicular to the first direction, wherein first internal electrode layers mainly composed of Ni and second internal electrode layers mainly composed of Ni are alternately laminated with dielectric layers sandwiched therebetween, and having a substantially rectangular parallelepiped shape, wherein the first internal electrode layers and the second internal electrode layers are alternately drawn out to first and second end faces that face each other in a third direction perpendicular to the first and second directions in the substantially rectangular parallelepiped shape, comprising: a first external electrode provided on the first end face, the main component of a contact layer in contact with the first end face being Cu; and a second external electrode provided on the second end face, the main component of a contact layer in contact with the second end face being Cu; at least the first internal electrode layer of the first and second internal electrode layers contains a low-melting point metal having a melting point equal to or lower than the melting point of Pb, and the concentration of the low-melting point metal is higher in the first internal electrode layer than in the second internal electrode layer, a width in a direction perpendicular to the stacking direction of a portion of the first internal electrode layer that connects to the first external electrode is narrower than a width of a portion of the first internal electrode layer that faces the second internal electrode layer, and a width in a direction perpendicular to the stacking direction of a portion of the second internal electrode layer that connects to the second external electrode is wider than a width of a portion of the first internal electrode layer that connects to the first external electrode.

2. The ceramic electronic component according to claim 1, wherein the low melting point metal is Sn.

3. The ceramic electronic component according to claim 1, wherein the second internal electrode layer contains a metal element other than the low-melting point metal that forms a stable compound with hydrogen.

4. The ceramic electronic component according to claim 3, wherein the metal element that forms a stable compound with hydrogen is at least one of Ag, Au, Ga, and Ge.

5. A ceramic electronic component as described in claim 1, wherein the width of the portion of the second internal electrode layer that connects to the second external electrode in a direction perpendicular to the stacking direction is the same as the width of the portion of the second internal electrode layer that faces the first internal electrode layer.

6. A ceramic electronic component as described in claim 1, wherein the width of the portion of the first internal electrode layer that connects to the first external electrode in a direction perpendicular to the stacking direction is 60% or more and 90% or less of the width of the portion that faces the second internal electrode layer.

7. A ceramic electronic component as set forth in claim 1, wherein a third internal electrode layer connected to said first external electrode is provided in a central portion in the stacking direction, and the width of the portion of said third internal electrode layer connected to said first external electrode in a direction perpendicular to the stacking direction is the same as the width of the portion facing said second internal electrode layer.

8. The ceramic electronic component according to claim 7, wherein the number of said third internal electrode layers is 5% to 40% of the number of said internal electrode layers connected to said first external electrodes.

9. A ceramic electronic component as described in claim 1, wherein, in the direction in which the first end face and the second end face oppose each other, a length of a portion of the first internal electrode layer that connects to the first external electrode and is narrower than a width of a portion that opposes the second internal electrode layer is between 1 / 4 and 1 / 1 of the length of the first external electrode.

10. The ceramic electronic component according to claim 1, wherein the first internal electrode layers and the second internal electrode layers are stacked in the first direction.

11. The ceramic electronic component according to claim 1, wherein the first internal electrode layers and the second internal electrode layers are laminated in the second direction.

12. A semiconductor device comprising a first internal electrode layer mainly composed of Ni and a second internal electrode layer mainly composed of Ni, which are alternately laminated with a dielectric layer sandwiched therebetween, and having a substantially rectangular parallelepiped shape, the first internal electrode layer and the second internal electrode layer are alternately drawn out to a first end face and a second end face opposing the substantially rectangular parallelepiped shape, and when a first direction, a second direction, and a third direction in which the first end face and the second end face are opposed to each other are orthogonal to each other, the dimension in the second direction is 1.3 times or more the dimension in the third direction, and at least one of the first internal electrode layer and the second internal electrode layer a first internal electrode layer containing a low-melting point metal having a melting point lower than the melting point of Pb, the first internal electrode layer having a higher concentration of the low-melting point metal than the second internal electrode layer, a portion of the first internal electrode layer extended to the first end face having a width in a direction perpendicular to the stacking direction that is narrower than a width of a portion facing the second internal electrode layer, and a portion of the second internal electrode layer extended to the second end face having a width in a direction perpendicular to the stacking direction that is wider than the width of the portion of the first internal electrode layer extended to the first end face; and a step of firing external electrodes mainly composed of Cu to each of the first end face and the second end face.

Citation Information

Patent Citations

  • Laminated ceramic capacitor

    JP2009027148A

  • Multilayer ceramic electronic component and manufacturing method for the same

    JP2013098525A

  • Multilayer ceramic capacitor

    JP2018198292A

  • Multilayered ceramic capacitor

    WO2022210627A1