Zeolite membrane composite and method for producing purified component

The zeolite membrane composite, characterized by specific X-ray diffraction pattern intensity ratios and SiO2/Al2O3 molar ratios, enhances separation performance, enabling efficient purification of components by selectively permeating and concentrating gases or liquids.

WO2024204851A1PCT designated stage expired Publication Date: 2024-10-03MITSUBISHI CHEM CORP
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/013527
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-31
Filing Date
2024-04-01
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Current zeolite membrane composites have limitations in achieving high separation performance and efficient production of purified components, necessitating the development of a composite with enhanced separation capabilities.

Method used

A zeolite membrane composite is formed on an inorganic porous support with a specific X-ray diffraction pattern intensity ratio, where the integrated intensity of peaks near 2θ=9.6° is 6.0 times or more than that near 2θ=20.8°, and the SiO2/Al2O3 molar ratio is between 6 and 500, incorporating a first component with high permeability and a second component with low permeability to achieve effective separation.

Benefits of technology

The resulting zeolite membrane composite demonstrates improved separation performance, allowing for the efficient production of purified components by selectively permeating and concentrating gases or liquids based on their molecular properties.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024013527_03102024_PF_FP_ABST
    Figure JP2024013527_03102024_PF_FP_ABST
Patent Text Reader

Abstract

The purpose of one aspect of the present invention is to provide a zeolite membrane composite having high separation performance. A zeolite membrane composite according to one aspect of the present invention has: an inorganic porous support; and a zeolite membrane formed on the surface of the inorganic porous support. In an X-ray diffraction pattern when the surface of the zeolite membrane is irradiated with X-rays at the minimum incident angle transmitting the zeolite membrane, the integrated intensity of a peak in the vicinity of 2θ=9.6º is at least 6.0 times the integrated intensity of a peak in the vicinity of 2θ=20.8º.
Need to check novelty before this filing date? Find Prior Art

Description

Zeolite membrane composite and method for producing purified component

[0001] The present invention relates to a method for producing a zeolite membrane composite and a purification component.

[0002] In recent years, a technology has been developed for producing a purified component by separating one component from a gas or liquid mixture by passing it through a zeolite membrane composite. Among these zeolite membrane composites, there is known a zeolite membrane composite that is identified by the ratio of the intensities of specific peaks in an X-ray diffraction pattern obtained by irradiating the surface of a zeolite membrane formed on an inorganic porous support with X-rays (see, for example, Patent Document 1).

[0003] International Publication No. 2013 / 125660

[0004] Technologies for producing purified components have been attracting increasing attention, and therefore, there is a demand for zeolite membrane composites with higher separation performance, as well as for more efficient production of purified components using such zeolite membrane composites.

[0005] An object of one aspect of the present invention is to provide a zeolite membrane composite having high separation performance.

[0006] A first aspect of the present invention is a zeolite membrane composite comprising an inorganic porous support and a zeolite membrane formed on the surface thereof, wherein the integrated intensity of a peak near 2θ = 9.6° in an X-ray diffraction pattern obtained when the surface of the zeolite membrane is irradiated with X-rays at the minimum incident angle that allows X-rays to penetrate the zeolite membrane is 6.0 times or more the integrated intensity of a peak near 2θ = 20.8°.

[0007] In a second aspect of the present invention, in the zeolite membrane composite of the first aspect, the integrated intensity of a peak near 2θ = 9.6° in an X-ray diffraction pattern obtained by irradiating a surface of the zeolite membrane with X-rays at the minimum incident angle that transmits through the zeolite membrane is 6.0 times or more the integrated intensity of a peak near 2θ = 16.8°.

[0008] In a third aspect of the present invention, in the zeolite membrane composite of the first or second aspect, an X-ray diffraction pattern obtained by irradiating the surface of the zeolite membrane with X-rays that reach the inorganic porous support has an integrated intensity of a peak near 2θ=17.9° that is less than 0.5 times the integrated intensity of a peak near 2θ=20.8°, and an integrated intensity of a peak near 2θ=9.6° that is 2.0 times or more but less than 6.0 times the integrated intensity of a peak near 2θ=20.8°.

[0009] A fourth aspect of the present invention is directed to the zeolite composite membrane of any one of the first to third aspects, wherein the SiO 2 / Al 2 O 3 The molar ratio is 6 or more and 500 or less.

[0010] A fifth aspect of the present invention is a method for producing a purified component, comprising contacting a mixture containing a first component having higher permeability through the zeolite membrane of a zeolite membrane composite of any one of Aspects 1 to 4 and a second component having lower permeability through the zeolite membrane, with the zeolite membrane composite to obtain either a first purified component which is the first component that has permeated the zeolite membrane, or a second purified component which is the second component that has not permeated the zeolite membrane, or both.

[0011] According to one aspect of the present invention, a zeolite membrane composite having high separation performance can be provided.

[0012] 1 is a diagram schematically showing the structure of a zeolite membrane composite according to one embodiment of the present invention; FIG. 2 is a diagram schematically showing part A of FIG. 1; FIG. 3 is a diagram schematically showing the configuration of an apparatus for carrying out a single-component gas permeation test in an example of the present invention; FIG. 4 is a diagram showing an X-ray diffraction pattern in grazing incidence X-ray diffraction of the membrane composite of Example 1; FIG. 5 is a diagram showing an X-ray diffraction pattern in grazing incidence X-ray diffraction of the membrane composite of Comparative Example 1; and FIG. 6 is a diagram showing an X-ray diffraction pattern in grazing incidence X-ray diffraction of the membrane composite of Comparative Example 2.

[0013] Hereinafter, one embodiment of the present invention will be described in detail. In this specification, a "zeolite membrane composite" is also referred to as a "membrane composite," an "inorganic porous support" is also referred to as a "support," and a "CHA-type aluminosilicate zeolite" is also referred to as a "CHA-type zeolite."

[0014] [Zeolite Membrane Composite] The zeolite membrane composite according to an embodiment of the present invention comprises an inorganic porous support and a zeolite membrane formed on the surface thereof.

[0015] The structure of a zeolite membrane composite according to one embodiment of the present invention is shown schematically in Figure 1. The membrane composite 1 has a support 11 and a zeolite membrane 12 formed on the surface thereof. The position of the zeolite membrane 12 on the support 11 is not limited. For example, when the support 11 has a tubular shape, the zeolite membrane 12 may be on the outer surface of the support 11, on the inner surface, or on both surfaces. From the viewpoints of reducing the permeation resistance and pressure resistance of the zeolite membrane 12, it is preferable that the zeolite membrane 12 be on the outer surface of the support 11.

[0016] The membrane composite 1 is configured by fixing zeolite in the form of a membrane to the surface or the like of the support 11. In some cases, it is preferable that a part of the zeolite is fixed to the inside of the support 11 from the viewpoint of increasing the support strength of the zeolite membrane 12 on the support 11.

[0017] The zeolite membrane 12 may be laminated on the surface of the support 11, or may be formed by crystallizing zeolite so as to fill the pores in the surface layer of the support 11. In this case, from the viewpoint of improving the separation performance of the membrane composite 1, it is preferable that the zeolite membrane 12 does not have continuous cracks or micropores connecting the inside and outside of the zeolite membrane 12, and that it does not contain any lumps of amorphous material other than zeolite crystals, i.e., it is a dense membrane.

[0018] Such a preferable membrane composite 1 can be formed, for example, by crystallizing zeolite into a membrane on the surface of a support by hydrothermal synthesis.

[0019] Fig. 2 is a schematic diagram of part A in Fig. 1. Part A in Fig. 1 is a part including the zeolite membrane 12 in the cross-sectional direction of the membrane composite 1. The zeolite membrane 12 is a part formed from the surface of the support 11 toward the outside of the support 11. Line L0 in Fig. 2 indicates the position of the surface of the zeolite membrane 12. The zeolite membrane 12 is composed of zeolite crystals. The zeolite crystals that make up the zeolite membrane 12 have a specific orientation.

[0020] The support 11 is an inorganic porous body, such as a porous body made of alumina. Line L1 in Fig. 2 indicates the position of the boundary between the zeolite membrane 12 and the support 11. In the first surface layer portion 11A, which is the portion very close to the surface of the support 11, zeolite crystals are embedded in the gaps in the support 11. The zeolite in the first surface layer portion 11A has an orientation that is similar to or slightly lower than that of the zeolite membrane 12.

[0021] Zeolite crystals also penetrate into the gaps in the support 11 in the second surface layer portion 11B, which is a portion near the surface of the support 11 and deeper than the first surface layer portion 11A. The zeolite in the second surface layer portion 11B has an arbitrary orientation different from the orientation of the zeolite membrane 12. The line L2 in Figure 2 indicates the boundary between zeolite showing a specific orientation and zeolite showing an arbitrary orientation.

[0022] Zeolite does not penetrate into the interior 11C of the support 11. Line L3 in Fig. 2 represents the penetration depth of zeolite into the support. As described above, zeolite penetrates into the inside of the support 11 in areas other than the zeolite membrane 12, and its orientation also varies in the thickness direction of the support 11.

[0023] [Orientation] In this embodiment, when the surface of the zeolite membrane is irradiated with X-rays at the minimum incident angle that transmits through the zeolite membrane, the integrated intensity of the peak near 2θ = 9.6° in the X-ray diffraction pattern is 6.0 times or more the integrated intensity of the peak near 2θ = 20.8°.

[0024] In this specification, "X-ray diffraction pattern" refers to a diffraction pattern obtained by irradiating the surface of a zeolite membrane with X-rays from a CuKα radiation source, with the scanning axis set at θ / 2θ. In measuring the X-ray diffraction pattern, if the surface of the zeolite membrane composite (of the zeolite membrane) is curved, an automatic variable slit may be used to fix the irradiation width. An X-ray diffraction pattern obtained using an automatic variable slit refers to a pattern that has undergone variable-to-fixed slit correction.

[0025] In addition, in this specification, "integrated intensity of peak" refers to a value calculated by the method described in the Examples. Furthermore, "peak around 2θ = 9.6°" refers to the largest peak among the peaks that are not derived from the support and exist in the range of 9.6° ± 0.6°. Furthermore, "peak around 2θ = 20.8°" refers to the largest peak among the peaks that are not derived from the support and exist in the range of 20.8° ± 0.6°, and "peak around 2θ = 16.2°" refers to the largest peak among the peaks that are not derived from the support and exist in the range of 16.2° ± 0.6°.

[0026] In this embodiment, the shape of the sample used in measuring the X-ray diffraction pattern may be any shape that allows X-rays to be irradiated onto the surface of the zeolite membrane of the membrane composite. For example, the shape of the sample may be the shape of the membrane composite itself, or may be the shape of the membrane composite cut into an appropriate size limited by the measurement device.

[0027] The "minimum incident angle that transmits through the zeolite membrane" is the X-ray irradiation angle at which a peak specific to the zeolite membrane is detected when the X-ray irradiation angle to the zeolite membrane is changed, and is the X-ray irradiation angle at which one of the following occurs: - When a peak specific to the support is no longer detected - When a peak specific to the support is detected for the first time

[0028] Xr1 in Fig. 1 represents the X-rays irradiated onto the zeolite membrane 12 at this time, and the minimum incident angle is indicated by θ1 in Fig. 1. The X-ray irradiation angle can be defined as 0° when the X-ray irradiation angle onto the zeolite membrane is changed and no peaks derived from the zeolite membrane are detected.

[0029] When X-rays are irradiated at the minimum incident angle and asymmetric reflection measurement is performed at a fixed incident angle, the X-ray diffraction pattern represents the orientation of the zeolite crystals in the zeolite membrane in the portion that exists outside the interface between the support and the zeolite membrane. Therefore, a high proportion of peaks indicating a specific orientation of the zeolite crystals means that a high proportion of the zeolite crystals that make up the zeolite membrane are oriented in that specific direction, i.e., the zeolite membrane 12 portion has a high degree of orientation, which means high separation performance.

[0030] According to COLLECTION OF SIMULATED XRD POWDER PATTERNS FOR ZEOLITE Fourth Revised Edition 2001 ELSEVIER, the peak at about 2θ = 9.6° in the X-ray diffraction pattern is a peak derived from the plane with indices (1,0,0) in the CHA structure when the space group is (No. 166) in the rhombohedral setting. Furthermore, the peak at around 2θ = 20.8° in the X-ray diffraction pattern is a peak derived from the plane with indices (2, 0, -1) in the CHA structure when the space group is (No. 166) in the rhombohedral setting, according to COLLECTION OF SIMULATED XRD POWDER PATTERNS FOR ZEOLITE Fourth Revised Edition 2001 ELSEVIER.

[0031] Furthermore, the peak at about 2θ = 16.2° in the X-ray diffraction pattern is a peak derived from the plane with indices (1, -1, 1) in the CHA structure when the space group is (No. 166) in the rhombohedral setting, according to COLLECTION OF SIMULATED XRD POWDER PATTERNS FOR ZEOLITE Fourth Revised Edition 2001 ELSEVIER.

[0032] In this specification, "a peak around 2θ = 9.6°" means the largest peak among the peaks not attributable to the support that exist in the range of 9.6° ± 0.6°. Similarly, "a peak around 2θ = 20.8°" and "a peak around 2θ = 16.2°" mean the largest peak among the peaks not attributable to the support that exist in the range of 20.8° ± 0.6° and the largest peak among the peaks not attributable to the support that exist in the range of 16.2° ± 0.6°, respectively.

[0033] A high ratio of the integrated intensity of the peak near 2θ = 9.6 ° to the integrated intensity of the peak near 2θ = 20.8 ° in the X-ray diffraction pattern when irradiated with X-rays at the minimum incident angle is thought to mean that the zeolite crystals are growing in a more oriented manner, for example, so that the (1,0,0) plane when the CHA structure is in a rhombohedral setting is oriented closer to parallel to the surface of the membrane composite. Oriented growth of zeolite crystals in the membrane composite is advantageous from the viewpoint of improving the separation performance of the zeolite membrane and obtaining a dense zeolite membrane. From this viewpoint, the higher the ratio, the better, and is usually 6.0 times or more, preferably 6.3 times or more, more preferably 6.5 times or more, even more preferably 6.7 times or more, and particularly preferably 7.0 times or more. The upper limit of the ratio can be determined appropriately from the viewpoint of fully obtaining the effects of the above viewpoint, and may be, for example, 100 times or less.

[0034] A high ratio of the integrated intensity of the peak near 2θ = 9.6 ° to the integrated intensity of the peak near 2θ = 16.2 ° in the X-ray diffraction pattern when irradiated with X-rays at the minimum incident angle is thought to mean that the zeolite crystals are growing in a more oriented manner, for example, so that the (1,0,0) plane when the CHA structure is in a rhombohedral setting is closer to parallel to the surface of the membrane composite. Oriented growth of zeolite crystals in the membrane composite is advantageous from the viewpoint of improving the separation performance of the zeolite membrane and obtaining a dense zeolite membrane. From this viewpoint, the higher the ratio, the better, and is usually 6.0 times or more, preferably 6.5 times or more, more preferably 7.0 times or more, even more preferably 7.5 times or more, particularly preferably 8.0 times or more, and most preferably 10.0 times or more. Within this range, 20.0 times or more is preferred, 25.0 times or more is more preferred, and 30.0 times or more is even more preferred. The upper limit of the ratio can be determined appropriately from the viewpoint of sufficiently obtaining the effects of the above viewpoint, and may be, for example, 100 times or less.

[0035] The integrated intensity of the peaks in the X-ray diffraction pattern obtained by irradiating X-rays at the minimum incident angle can be measured by grazing incidence X-ray diffraction (GIXD). The integrated intensity of the peaks can be adjusted by the conditions for producing the zeolite membrane, for example, by the amount of seed crystals attached when producing the zeolite membrane by hydrothermal synthesis.

[0036] The X-ray diffraction pattern obtained when X-rays are irradiated at the minimum incident angle substantially only shows the measurement results for the zeolite membrane 12 in Figure 2 (between lines L0 and L1 in Figure 2). The X-ray diffraction pattern does not include the measurement results for the first surface layer portion 11A, in which zeolite crystals are embedded in the gaps in the support 11, the second surface layer portion 11B, in which a different orientation of the zeolite is dominant, or the interior portion 11C, which does not contain zeolite. Therefore, the X-ray diffraction pattern can provide information on the orientation of the zeolite membrane 12, which has the greatest impact on the production of purified components (separation or concentration of a mixture), and the separation performance of the membrane composite can be more accurately predicted.

[0037] The integrated intensity of the peak in the X-ray diffraction pattern when irradiated with X-rays at the minimum incident angle is a value measured at at least one location on the film.

[0038] In this embodiment, when the surface of the zeolite membrane is irradiated with X-rays that reach the inorganic porous support, the integrated intensity of the peak near 2θ = 17.9° in the X-ray diffraction pattern is preferably less than 0.5 times the integrated intensity of the peak near 2θ = 20.8°, and the integrated intensity of the peak near 2θ = 9.6° is preferably 2.0 to 6.0 times the integrated intensity of the peak near 2θ = 20.8°. Note that the "X-ray diffraction pattern when the surface of the zeolite membrane is irradiated with X-rays that reach the inorganic porous support" refers to an X-ray diffraction pattern when X-rays are irradiated at an incident angle greater than the minimum incident angle described above. In this embodiment, this refers to the results of symmetric reflection measurement using θ / 2θ measurement. Xr2 in FIG. 1 represents the X-rays irradiating the zeolite membrane 12 at this time, and the incident angle is indicated by θ2 in FIG. 1.

[0039] According to COLLECTION OF SIMULATED XRD POWDER PATTERNS FOR ZEOLITE Fourth Revised Edition 2001 ELSEVIER, the peak at around 2θ = 17.9 ° in the X-ray diffraction pattern is a peak derived from the plane with index (1,1,1) in the CHA structure when the space group is (No. 166) in the rhombohedral setting. In this specification, "peak at around 2θ = 17.9 °" means the largest peak among the peaks present in the range of 17.9 ° ± 0.6 ° that are not derived from the support.

[0040] When the surface of a zeolite membrane is irradiated with X-rays that reach the inorganic porous support, and the integrated intensity of the peak near 2θ = 17.9° in the X-ray diffraction pattern is less than 0.5 times the integrated intensity of the peak near 2θ = 20.8°, and the integrated intensity of the peak near 2θ = 9.6° is 2.0 to 8.0 times the integrated intensity of the peak near 2θ = 20.8°, the above ratio of the integrated intensity of the peak near 2θ = 17.9° to the integrated intensity of the peak near 2θ = 20.8° in the X-ray diffraction pattern when irradiated with X-rays that reach the support indicates that the zeolite crystals in the zeolite membrane have grown in a sufficiently oriented manner, and a dense zeolite membrane with high separation performance has been formed. In order to form a dense zeolite membrane with high separation performance, the ratio of the integrated intensity of the peak near 2θ = 17.9° to the integrated intensity of the peak near 2θ = 20.8° in the X-ray diffraction pattern obtained when irradiated with X-rays that reach the support is more preferably 0.45 or less. The lower limit of this ratio can be determined appropriately so that the effects of the above aspects can be fully obtained, and may be, for example, 0.001 or more.

[0041] Furthermore, in this embodiment, when the surface of the zeolite membrane is irradiated with X-rays that reach the inorganic porous support, and the integrated intensity of the peak near 2θ = 17.9° in the X-ray diffraction pattern is less than 0.5 times the integrated intensity of the peak near 2θ = 20.8°, and the integrated intensity of the peak near 2θ = 9.6° is 2.0 to 8.0 times the integrated intensity of the peak near 2θ = 20.8°, with respect to the ratio of the integrated intensity of the peak near 2θ = 9.6° to the integrated intensity of the peak near 2θ = 20.8° in the X-ray diffraction pattern when the surface of the zeolite membrane is irradiated with X-rays that reach the inorganic porous support, from the viewpoint of forming a dense zeolite membrane with high separation performance, it is preferable that the lower limit of this ratio is higher and the upper limit of this ratio is lower. For example, in an X-ray diffraction pattern obtained by irradiating the support with X-rays, the ratio of the integrated intensity of the peak near 2θ=9.6° to the integrated intensity of the peak near 2θ=20.8° is, from the above-mentioned viewpoints, more preferably 2.1 or more, even more preferably 2.3 or more, and even more preferably 2.5 or more. Also, from the above-mentioned viewpoints, this ratio is more preferably 7.5 or less, even more preferably 7.3 or less, and even more preferably 7.0 or less.

[0042] In this embodiment, when the surface of the zeolite membrane is irradiated with X-rays that reach the inorganic porous support, it is preferable that the peak intensity of the peak near 2θ = 17.9° in the X-ray diffraction pattern is less than 0.5 times the peak intensity of the peak near 2θ = 20.8°, and that the peak intensity of the peak near 2θ = 9.6° is 2.0 times or more but less than 4.0 times the peak intensity of the peak near 2θ = 20.8°.

[0043] When the surface of a zeolite membrane is irradiated with X-rays that reach the inorganic porous support, and the peak intensity of the peak near 2θ = 17.9° in the X-ray diffraction pattern is less than 0.5 times the peak intensity of the peak near 2θ = 20.8°, and the peak intensity of the peak near 2θ = 9.6° is 2.0 to 4.0 times the peak intensity of the peak near 2θ = 20.8°, the above ratio of the integrated intensity of the peak near 2θ = 17.9° to the peak intensity of the peak near 2θ = 20.8° in the X-ray diffraction pattern when irradiated with X-rays that reach the support indicates that the zeolite crystals in the zeolite membrane have grown in a sufficiently oriented manner, and a dense zeolite membrane with high separation performance has been formed. In order to form a dense zeolite membrane with high separation performance, the ratio of the peak intensity of the peak near 2θ = 17.9° to the peak intensity of the peak near 2θ = 20.8° in the X-ray diffraction pattern obtained by irradiating the support with X-rays is more preferably 0.45 or less, even more preferably 0.43 or less, and particularly preferably 0.41 or less. The lower limit of this ratio can be determined appropriately so that the effects of the above aspects can be fully obtained, and may be, for example, 0.001 or more.

[0044] When the surface of a zeolite membrane is irradiated with X-rays that reach the inorganic porous support, and the peak intensity of the peak near 2θ = 17.9° in the X-ray diffraction pattern is less than 0.5 times the peak intensity of the peak near 2θ = 20.8°, and the peak intensity of the peak near 2θ = 9.6° is 2.0 to 4.0 times the peak intensity of the peak near 2θ = 20.8°, with respect to the ratio of the peak intensity of the peak near 2θ = 9.6° to the peak intensity of the peak near 2θ = 20.8° in the X-ray diffraction pattern when the surface of the zeolite membrane is irradiated with X-rays that reach the inorganic porous support, from the viewpoint of forming a dense zeolite membrane with high separation performance, it is preferable that the lower limit of this ratio is higher and the upper limit of this ratio is lower. For example, from the above viewpoints, the ratio of the peak intensity of the peak near 2θ=9.6° to the peak intensity of the peak near 2θ=20.8° in the X-ray diffraction pattern when irradiated with X-rays that reach the support is more preferably 2.1 or more, even more preferably 2.3 or more, and even more preferably 2.5 or more. Also, from the above viewpoints, this ratio is more preferably 3.9 or less, even more preferably 3.8 or less, and even more preferably 3.7 or less.

[0045] In this embodiment, when the surface of the zeolite membrane is irradiated with X-rays that reach the inorganic porous support, the integrated intensity of the peak near 2θ = 17.9° in the X-ray diffraction pattern may be 0.5 times or more the integrated intensity of the peak near 2θ = 20.8°, or the integrated intensity of the peak near 2θ = 9.6° may be 6.0 times or more the integrated intensity of the peak near 2θ = 20.8°.

[0046] When the surface of a zeolite membrane is irradiated with X-rays that reach the inorganic porous support, and the integrated intensity of the peak near 2θ = 17.9° in the X-ray diffraction pattern is 0.5 times or more the integrated intensity of the peak near 2θ = 20.8°, or the integrated intensity of the peak near 2θ = 9.6° is 8.0 times or more the integrated intensity of the peak near 2θ = 20.8°, the above ratio of the integrated intensity of the peak near 2θ = 17.9° to the integrated intensity of the peak near 2θ = 20.8° in the X-ray diffraction pattern when irradiated with X-rays that reach the support indicates that the zeolite crystals in the zeolite membrane have grown with very good orientation, and a dense zeolite membrane with high separation performance has been formed. In this case, the ratio of the integrated intensity of the peak near 2θ = 17.9° to the integrated intensity of the peak near 2θ = 20.8° in the X-ray diffraction pattern when irradiated with X-rays that reach the support to the integrated intensity of the peak near 2θ = 20.8° is preferably 0.5 or more, more preferably 0.8 or more, even more preferably 1.0 or more, particularly preferably 1.2 or more, and most preferably 1.5 or more, from the viewpoint of forming a dense zeolite membrane with high separation performance. The upper limit of this ratio can be determined appropriately from the viewpoint of fully obtaining the effects of the above viewpoint, and may be, for example, 1000 or less. In this case, the ratio of the integrated intensity of the peak near 2θ = 9.6° to the integrated intensity of the peak near 2θ = 20.8° in the X-ray diffraction pattern when irradiated with X-rays that reach the support to the integrated intensity of the peak near 2θ = 9.6° to the integrated intensity of the peak near 2θ = 20.8° is preferably 8.0 times or more, more preferably 8.5 or more, and even more preferably 9.0 or more, from the viewpoint of forming a dense zeolite membrane with high separation performance. The upper limit of this ratio can be determined appropriately from the viewpoint of fully obtaining the effects of the above viewpoint, and may be, for example, 1000 or less.

[0047] In this embodiment, the peak intensity of the peak near 2θ = 17.9 ° in the X-ray diffraction pattern obtained when the surface of the zeolite membrane is irradiated with X-rays that reach the inorganic porous support may be 0.5 times or more the peak intensity of the peak near 2θ = 20.8 °, or the peak intensity of the peak near 2θ = 9.6 ° may be 4.0 times or more the peak intensity of the peak near 2θ = 20.8 °. In this case, it is preferable from the viewpoint of forming a dense zeolite membrane with high separation performance that the peak intensity of the peak near 2θ = 9.6 ° in the X-ray diffraction pattern obtained when the surface of the zeolite membrane is irradiated with X-rays that reach the inorganic porous support is 4.0 times or more the peak intensity of the peak near 2θ = 20.8 °. From the above viewpoints, the ratio of the peak intensity of the peak near 2θ = 9.6 ° to the peak intensity of the peak near 2θ = 20.8 ° in the X-ray diffraction pattern when irradiated with X-rays that reach the support is more preferably 4.1 or more, even more preferably 4.2 or more, and even more preferably 4.5 or more. The upper limit of this ratio can be appropriately determined from the viewpoint of fully obtaining the effects of the above viewpoints, and may be, for example, 1000 or less. In this case, from the viewpoint of forming a dense zeolite membrane with high separation performance, it is preferable that the peak intensity of the peak near 2θ = 17.9 ° in the X-ray diffraction pattern when the surface of the zeolite membrane is irradiated with X-rays that reach the inorganic porous support is 0.5 times or more the integrated intensity of the peak near 2θ = 20.8 °. From the above viewpoints, the ratio of the peak intensity of the peak near 2θ=17.9° to the peak intensity of the peak near 2θ=20.8° in the X-ray diffraction pattern obtained when irradiated with X-rays that reach the support is more preferably 0.5 or more, even more preferably 0.6 or more, and particularly preferably 0.65 or more. The upper limit of this ratio can be determined appropriately from the viewpoint of fully obtaining the effects of the above viewpoints, and may be, for example, 1000 or less.

[0048] The integrated intensities and peak intensity ratios of peaks in an X-ray diffraction pattern obtained by irradiating the support with X-rays reaching the support can be determined using a known X-ray diffractometer capable of measuring X-ray diffraction on a tubular or curved surface. Furthermore, the ratio of the integrated intensities of the peaks can be adjusted by the conditions of the hydrothermal synthesis for producing the zeolite membrane, as will be described later. For example, the ratio can be adjusted by using a specific organic template in the hydrothermal synthesis, or by using a relatively high concentration of SiO. 2 / Al 2 O 3 The use of an aqueous reaction composition with a high molar ratio and the inclusion of K in the reaction mixture + This can be achieved and controlled by the presence of other ions, such as Na / K ratio, Na and K to Al ratio in the aqueous reaction mixture, and the amount of seed crystals pre-deposited on the support.

[0049] [Membrane Thickness] The thickness of the zeolite membrane of this embodiment is not particularly limited, but is usually 0.1 μm or more, preferably 0.6 μm or more, and more preferably 1.0 μm or more. By being equal to or greater than the above lower limit, the strength of the membrane composite can be further improved. Furthermore, the thickness of the zeolite membrane is not particularly limited, but is usually 100 μm or less, preferably 60 μm or less, and more preferably 20 μm or less. When the membrane composite is used for gas separation, a thinner thickness is preferable. Therefore, the thickness of the zeolite membrane is more preferably 10 μm or less, even more preferably 5 μm or less, particularly preferably 4 μm or less, and most preferably 3.5 μm or less. By being equal to or less than the above upper limit, the permeation performance of the membrane composite can be further improved. The thickness of the zeolite membrane can be measured using the method described in the Examples below.

[0050] [Amount of defects] In this embodiment, the CF of the membrane complex 4 Permeance or SF 6Permeance indicates the amount of defects in the zeolite membrane. Defects are gaps between zeolite particles, such as cracks caused by thermal expansion or grain boundaries that remain when zeolite particles do not grow sufficiently. When the type of zeolite constituting the zeolite membrane is CHA-type zeolite, which will be described later, the CF of the membrane composite is 4 Permeance is usually 5.0 x 10 -9 mol / (m 2 s Pa) or less, preferably 3.5 × 10 -9 mol / (m 2 s Pa) or less, more preferably 3.0 × 10 -9 mol / (m 2 s Pa) or less, more preferably 1.5 × 10 -9 mol / (m 2 s Pa) or less, particularly preferably 1.0 × 10 -9 mol / (m 2 s Pa), most preferably 5.0 x 10 -10 mol / (m 2 s Pa) or less. -10 mol / (m 2 s Pa) or less, preferably 5.0 × 10 -11 mol / (m 2 s Pa) or less, more preferably 3.0 × 10 -11 mol / (m 2 When the type of zeolite is a CHA-type zeolite described later, the SF of the membrane composite may be 6 Permeance is usually 5.0 x 10 -9 mol / (m 2 s Pa) or less, preferably 3.5 × 10 -9 mol / (m 2 s Pa) or less, more preferably 3.0 × 10 -9 mol / (m 2 s Pa) or less, more preferably 1.5 × 10 -9 mol / (m 2 s Pa) or less, particularly preferably 1.0 × 10 -9 mol / (m 2 s Pa), most preferably 5.0 x 10 -10 mol / (m 2s Pa) or less. -10 mol / (m 2 s Pa) or less, preferably 5.0 × 10 -11 mol / (m 2 s Pa) or less, more preferably 3.0 × 10 -11 mol / (m 2 .s.Pa) or less. CF of the membrane complex 4 Permeance or SF 6 When the permeance is within the above range, defects present in the membrane composite are reduced, and the membrane composite has better separation performance. Note that the above values ​​may be values ​​for the membrane composite before modification such as ion exchange treatment or silylation treatment of the membrane composite. 4 Permience, or SF 6 The permeance is a value measured by a single gas at a measurement temperature of 50°C and a differential pressure between the inside and outside of the membrane of 0.1 MPa. The permeance of other gases is also a value measured by a single gas at a measurement temperature of 50°C and a differential pressure between the inside and outside of the membrane of 0.1 MPa, unless otherwise specified. In addition, gases that hardly permeate the zeolite pores, for example, CH in the case of a CHA-type zeolite membrane, 4 The gas permeance may be used as an index of the defect amount.

[0051] [Permeability coefficient] CF of membrane complex 4 Permeance or SF 6 Although permeance can be regarded as the amount of defects, it is more preferable to consider the membrane thickness related to the permeation resistance when examining the performance of the membrane composite as a whole. Therefore, in this embodiment, the CF of the membrane composite is used as an index of the amount of defects of the membrane composite. 4 Permeance or SF 6 CF, which is the product of permeance and the thickness of the zeolite membrane 4 The transmission coefficient or SF 6 When the type of zeolite constituting the zeolite membrane is a CHA-type zeolite, which will be described later, the indicator of the defect amount of the membrane composite is the CF of the membrane composite. 4 In the case of a transmission coefficient of 4.5 × 10 -8(mol・μm) / (m 2 s Pa) or less, preferably 3.5 × 10 -8 (mol・μm) / (m 2 s Pa) or less, more preferably 3.0 × 10 -8 (mol・μm) / (m 2 s Pa) or less, and more preferably 2.0 × 10 -8 (mol・μm) / (m 2 s Pa) or less, particularly preferably 1.0 × 10 -8 (mol・μm) / (m 2 s Pa) or less, most preferably 5.0 × 10 -9 (mol・μm) / (m 2 s Pa). Also, the SF of the membrane complex 6 In the case of a transmission coefficient of 4.5 × 10 -8 (mol・μm) / (m 2 s Pa) or less, preferably 3.5 × 10 -8 (mol・μm) / (m 2 s Pa) or less, more preferably 3.0 × 10 -8 (mol・μm) / (m 2 s Pa) or less, and more preferably 2.0 × 10 -8 (mol・μm) / (m 2 s Pa) or less, particularly preferably 1.0 × 10 -8 (mol・μm) / (m 2 s Pa) or less, most preferably 5.0 × 10 -9 (mol・μm) / (m 2 s·Pa). When the permeability coefficient of the membrane composite is within such a range, defects present in the membrane composite are reduced, and the membrane composite has better separation performance. The above-mentioned values ​​may be values ​​for the membrane composite before modification of the membrane composite such as ion exchange treatment or silylation treatment. As mentioned above, for the purpose of obtaining a rough estimate of the defect amount, when the zeolite membrane is a CHA-type zeolite, the index of the defect amount of the membrane composite is the CH 4 In the case of a permeability coefficient of 5.0 × 10 -7 mol μm / (m 2s Pa) or less. Preferably, it is 1.0 × 10 -7 mol μm / (m 2 s Pa) or less, more preferably 5.0 × 10 -8 mol μm / (m 2 s Pa) or less, and more preferably 3.0 × 10 -8 mol μm / (m 2 s Pa) or less. 4 Transmission coefficient, or SF 6 The permeability coefficient is calculated using the value of a single gas measurement when the measurement temperature is 50°C and the differential pressure inside and outside the membrane is 0.1 MPa. For other gases, the permeability coefficient can also be calculated from the product of permeance and membrane thickness, but in that case, unless otherwise specified, the calculation is performed using the value of a single gas measurement when the measurement temperature is 50°C and the differential pressure inside and outside the membrane is 0.1 MPa. For example, the permeability coefficient can be calculated similarly for methane, but in that case, the calculation is performed using the value of a single gas measurement when the measurement temperature is 50°C and the differential pressure inside and outside the membrane is 0.1 MPa.

[0052] [Permeation Performance of Membrane Composite] The permeation performance of the membrane composite is expressed as the permeance [mol·m 2 ・s・Pa) -1 When carbon dioxide is passed through the membrane composite at a temperature of 50°C and a differential pressure of 0.1 MPa, 2 Permeance is usually 3 x 10 -8 or more, preferably 6.0 × 10 -8 , preferably 9.0×10 -8 or more, preferably 2.0 × 10 -7 or more, preferably 3.0 × 10 -7 More preferably, 5.0 × 10 -7 More preferably, 7.0 × 10 -7 More preferably, 1.0 × 10 -6 That's all. 2 The upper limit of permeance is not limited, and is usually 3.0 × 10 -4As the properties of the membrane composite, it is preferable that the carbon dioxide permeance and the defect amount or defect amount index satisfy the above-mentioned ranges. When the defect amount or defect amount index is within the range, the membrane composite can achieve both high separation performance and high throughput.

[0053] [Other Specifications] The water adsorption amount of the membrane composite of this embodiment, determined from its water vapor adsorption isotherm, at a relative pressure of 0.8 is preferably between two and ten times the water adsorption amount at a relative pressure of 0.2. Here, the "adsorption isotherm" is expressed as a graph obtained by measuring the change in pressure and adsorption amount while maintaining the material at a constant temperature. Generally, the horizontal axis represents the relative pressure (P / P0) obtained by dividing the equilibrium pressure by the saturated vapor pressure, and takes values ​​between 0 and 1. The vertical axis represents the water adsorption amount. In this embodiment, the water (water vapor) adsorption amount (g / g) to the membrane composite at a relative pressure of 0.8 and a relative pressure of 0.2 is used as an index.

[0054] The water adsorption ratio generally correlates with water adsorption into mesopores in the zeolite membrane. A higher ratio means a larger hydrophilic mesopore volume, while a lower ratio means a smaller hydrophilic mesopore volume. If the ratio is too high, the zeolite membrane may have many mesopores and be insufficiently dense, resulting in a high permeation rate but low separation performance. On the other hand, if the ratio is too low, the zeolite membrane has almost no mesopores and is highly dense, resulting in a high separation performance but low permeation rate. From the viewpoint of improving the separation performance and permeation rate of the zeolite membrane, the ratio is preferably 2.1 or more, more preferably 2.2 or more, and more preferably 8 or less, even more preferably 5 or less.

[0055] The air permeability of the membrane composite is usually 10 L / (m 2 ·h) or more, preferably 20 L / (m 2 h) or more, more preferably 30 L / (m 2 ·h) or more, more preferably 35 L / (m 2 ·h) or more, and particularly preferably 100 L / (m 2The upper limit of the permeation rate is not limited, but it is preferably 1000 L / (m 2 ·h) or less, more preferably 800 L / (m 2 ·h) or less, more preferably 700 L / (m 2 The "air permeation rate" is the rate of air permeation [L / (m 2 ・h)].

[0056] The air permeation rate correlates with the gas permeation rate of the membrane composite. A membrane composite with a high air permeation rate also has a high gas permeation rate, but if the air permeation rate is too high, separation performance tends to be reduced. In this embodiment, it is preferable that the membrane composite has a moderately high air permeation rate, a high gas permeation rate, and good separation performance. Such a membrane composite has performance particularly suitable for separating gas components.

[0057] [Inorganic Porous Support] The inorganic porous support described in Patent Document 1 can be used as the inorganic porous support (support) in this embodiment.

[0058] The support may be any porous inorganic material with chemical stability that allows zeolite to crystallize into a membrane on its surface. Specific examples of the support include sintered ceramics such as silica, α-alumina, γ-alumina, mullite, zirconia, titania, yttria, silicon nitride, or silicon carbide; sintered metals such as iron, bronze, or stainless steel; and molded bodies of glass or carbon. The sintered ceramics have the effect of enhancing interfacial adhesion by partially converting to zeolites during the synthesis of the zeolite membrane. Furthermore, supports containing at least one of alumina, silica, and mullite are more likely to be partially zeoliticized. This strengthens the bond between the support and zeolite, facilitating the formation of a dense membrane with high separation performance, making them more preferred.

[0059] The shape of the support may be any shape that can effectively separate a gas mixture or a liquid mixture, and specific examples include flat, tubular, cylindrical, and honeycomb or monolith shapes having a large number of cylindrical or prismatic holes.

[0060] The pore size of the pores in the support is preferably controlled. The pore size is usually 0.02 μm or more, preferably 0.05 μm or more, more preferably 0.1 μm or more, and usually 20 μm or less, preferably 10 μm or less, more preferably 5 μm or less. If the pore size is too small, the permeation amount tends to be small, and if it is too large, the strength of the support itself tends to be insufficient, and it tends to be difficult to form a dense zeolite membrane. The pore size may be an average pore size, and the average pore size can be measured by mercury intrusion porosimetry.

[0061] If necessary, the surface of the support may be polished with a file, etc. The surface of the support means the surface portion of the support on which the zeolite membrane is formed.

[0062] The porosity of the support is preferably 20% or more and 60% or less. The porosity affects the permeation flow rate when separating gas or liquid. If the porosity is less than the above lower limit, the diffusion of the permeant tends to be hindered, and if it exceeds the above upper limit, the strength of the support tends to decrease. The porosity of the support can be measured by mercury intrusion porosimetry.

[0063] [Zeolite Membrane] The zeolite membrane described in Patent Document 1 can be applied to the zeolite membrane in this embodiment as long as it has the above-described specific properties.

[0064] In this embodiment, the components constituting the zeolite membrane may include, in addition to zeolite, inorganic binders such as silica and alumina, organic substances such as polymers, or silylating agents for modifying the zeolite surface, as needed.

[0065] The zeolite membrane may contain a portion of amorphous components, but is preferably composed substantially of zeolite alone.

[0066] The proportion of CHA-type aluminosilicate contained in the zeolite membrane is usually 10% by volume or more, preferably 30% by volume or more, more preferably 60% by volume or more, and even more preferably 80% by volume or more. It is most preferable that the zeolite membrane is composed only of CHA-type aluminosilicate, as this provides the best gas permeability and separation properties.

[0067] The thickness of the zeolite membrane is usually 0.1 μm or more, preferably 0.6 μm or more, more preferably 1.0 μm or more. It is usually 100 μm or less, preferably 60 μm or less, more preferably 20 μm or less. If the zeolite membrane is too thick, the amount of permeation through the zeolite membrane tends to decrease, while if the thickness is too small, the selectivity tends to decrease or the membrane strength tends to decrease.

[0068] If the particle size of the zeolite forming the zeolite membrane is too small, the grain boundaries will become large, which tends to reduce the permeation selectivity, etc. Therefore, it is usually 30 nm or more, preferably 50 nm or more, and more preferably 100 nm or more, with the upper limit being equal to or less than the membrane thickness. Furthermore, it is more preferable if the particle size of the zeolite is the same as the membrane thickness. When the particle size of the zeolite is the same as the membrane thickness, the grain boundaries of the zeolite are smallest. Zeolite membranes obtained by hydrothermal synthesis, which will be described later, are preferred because the particle size of the zeolite and the thickness of the membrane may be the same.

[0069] The shape of the zeolite membrane is not limited, and may be any shape such as tubular, hollow fiber, monolith, honeycomb, etc. The size of the zeolite membrane is also not limited, and for example, in the case of a tubular membrane, it is practical and preferable that the length is usually 2 cm to 200 cm, the inner diameter is 0.5 cm to 2 cm, and the thickness is 0.5 mm to 4 mm.

[0070] <Zeolite> In this embodiment, the zeolite membrane preferably contains a CHA-type aluminosilicate zeolite. More preferably, the zeolite constituting the zeolite membrane is a CHA-type aluminosilicate. The aluminosilicate is mainly composed of oxides of Si and Al. The zeolite may contain other elements as long as the effects of the present invention are obtained.

[0071] SiO of zeolite membrane 2 / Al 2 O 3 The SAR molar ratio (hereinafter also referred to as "SAR") can be measured at an area or a surface point on the surface of the zeolite membrane. The respective measurement methods are as described in the Examples. In the present embodiment, in the surface point SEM-EDX analysis of the zeolite membrane, the SAR is preferably 6 or more and 500 or less. If the SAR is too low, the density of the zeolite membrane may decrease and the durability tends to decrease. From the viewpoint of the density and durability of the zeolite membrane, the SAR of the zeolite membrane is preferably 10 or more, more preferably 20 or more, more preferably 30 or more, even more preferably 32 or more, even more preferably 35 or more, and particularly preferably 40 or more. The upper limit is the SAR at which Al is typically present in an amount similar to that of an impurity, and is preferably 100 or less, more preferably 90 or less, even more preferably 80 or less, particularly preferably 70 or less, and most preferably 50 or less. Although SEM-EDX measurement of the surface area of ​​a zeolite membrane may produce values ​​different from those obtained by surface-point SEM-EDX analysis, it is believed that the values ​​will not be exactly the same due to the uniformity and variability of the sample. Furthermore, the preferred range of SAR for the zeolite membrane in surface-point SEM-EDX measurement may be similar to that in the above-mentioned surface-point SEM-EDX analysis.

[0072] The SAR of a zeolite membrane can be determined by scanning electron microscope-energy dispersive X-ray spectroscopy (SEM-EDX). To obtain information on a membrane only a few microns thick, the X-ray acceleration voltage is usually set to 6 kV. The SAR of a zeolite membrane can be adjusted by the reaction conditions of the hydrothermal synthesis, which will be described later.

[0073] <CHA-type zeolite> In this embodiment, "CHA-type zeolite" refers to a zeolite with a CHA structure, which is a code that specifies the structure of zeolites as defined by the International Zeolite Association (IZA). This is a zeolite that has a crystalline structure equivalent to that of naturally occurring chabazite. CHA-type zeolite has a structure with three-dimensional pores composed of eight-membered oxygen rings with a diameter of 0.38 × 0.38 nm, and this structure is characterized by X-ray diffraction data.

[0074] Framework density of CHA-type zeolite (T / nm 3 The framework density (T / nm) is 14.5. 3 ) is the 1 nm diameter of zeolite. 3 (1000 Å 3 The framework density refers to the number of elements (T elements) other than oxygen that constitute the framework per zeolite. The framework density is determined by the structure of the zeolite. The relationship between the framework density and the structure of the zeolite is shown in ATLAS OF ZEOLITE FRAMEWORK TYPES Fifth Revised Edition 2001 ELSEVIER.

[0075] [Method for Producing Zeolite Membrane Composite] The zeolite membrane of this embodiment can be produced by the same method as that described in Patent Document 1, except for the matters described below.

[0076] The method for forming the zeolite membrane in this embodiment is not limited as long as it can form the above-mentioned specific zeolite membrane on a support. Examples of such methods include a method of crystallizing zeolite into a membrane on a support, a method of fixing zeolite to a support with an inorganic binder or an organic binder, a method of fixing a polymer in which zeolite is dispersed, and a method of fixing zeolite to a support by impregnating the support with a zeolite slurry and, in some cases, suctioning it. Among these, the method of crystallizing zeolite into a membrane on a support is particularly preferred.

[0077] The crystallization method is not limited, but a preferred method is to place the support in a reaction mixture for hydrothermal synthesis used in zeolite production (hereinafter also referred to as "aqueous reaction mixture") and perform direct hydrothermal synthesis to crystallize zeolite on the surface of the support, etc. Specifically, for example, an aqueous reaction mixture whose composition has been adjusted and made uniform may be placed in a heat-resistant and pressure-resistant container such as an autoclave with a support loosely fixed inside, sealed, and heated for a certain period of time.

[0078] The aqueous reaction mixture preferably contains a Si element source, an Al element source, an alkali source, and water, and further preferably contains an organic template as needed.

[0079] Examples of the Si element source that can be used include amorphous silica, colloidal silica, silica gel, sodium silicate, amorphous aluminosilicate gel, tetraethoxysilane (TEOS), and trimethylethoxysilane.

[0080] Examples of Al element sources that can be used include sodium aluminate, aluminum hydroxide, aluminum sulfate, aluminum nitrate, aluminum oxide, and amorphous aluminosilicate gel.

[0081] By substituting Al for Si in the zeolite framework, it is possible to increase the polarity, which allows highly polar gas molecules to be actively adsorbed into and permeate the zeolite pores. Furthermore, decreasing the amount of Al substitution results in a zeolite membrane with low polarity, which is advantageous for the permeation of gas molecules with low polarity.

[0082] In addition, polarity can be controlled by adding Ga, Fe, B, Ti, Zr, Sn, or Zn to an element source other than the Al element source. The pore size is slightly affected by the atomic diameter of the metal species introduced into the zeolite framework. When a metal with an atomic diameter smaller than that of silicon, specifically, boron (B), is introduced, the pore size becomes smaller, while when a metal with an atomic diameter larger than that of silicon, specifically, tin (Sn), is introduced, the pore size becomes larger. In addition, the pore size may be affected by acid treatment, which causes the introduced metal to be desorbed from the framework. Separation performance can also be improved by controlling the effective pore size.

[0083] The type of alkali used as the alkali source is not limited, and alkali metal hydroxides or alkaline earth metal hydroxides can be used.

[0084] Examples of the metal species of the alkali metal hydroxide or alkaline earth metal hydroxide include Na, K, Li, Rb, Cs, Ca, Mg, Sr, and Ba, and are preferably Na or K, and more preferably K. Two or more of the metal species may be used in combination, and specifically, it is preferable to use Na and K, or Li and K in combination.

[0085] Examples of alkali sources that can be used include alkali metal hydroxides such as sodium hydroxide, potassium hydroxide, lithium hydroxide, rubidium hydroxide, and cesium hydroxide, and alkaline earth metal hydroxides such as calcium hydroxide, magnesium hydroxide, strontium hydroxide, and barium hydroxide. Alternatively, hydroxide ions, which are counter anions of the organic template described below, can be used as the alkali source.

[0086] An organic template (structure-directing agent) is preferably used in the crystallization of zeolite. By synthesizing a zeolite membrane using an organic template, the SAR of the crystallized zeolite increases, and the crystallinity of the zeolite membrane can be further improved. Any organic template may be used as long as it can form a desired zeolite membrane, and one type of organic template may be used, or two or more types may be used in combination.

[0087] As the organic template, amines or quaternary ammonium salts are usually used. For example, the organic templates described in U.S. Pat. No. 4,544,538 and U.S. Patent Publication No. 2008 / 0075656 are preferred. Specific examples include cations derived from alicyclic amines, such as a cation derived from 1-adamantanamine, a cation derived from 3-quinacridinal, or a cation derived from 3-exo-aminonorbornene. Of these, a cation derived from 1-adamantanamine is more preferred. When a cation derived from 1-adamantanamine is used as the organic template, a CHA-type zeolite capable of forming a dense membrane is crystallized.

[0088] Of the cations derived from 1-adamantanamine, N,N,N-trialkyl-1-adamantanammonium cations are more preferred. The three alkyl groups in the N,N,N-trialkyl-1-adamantanammonium cation are usually each independently an alkyl group, preferably a lower alkyl group, more preferably a methyl group. The most preferred compound among the N,N,N-trialkyl-1-adamantanammonium cations is N,N,N-trimethyl-1-adamantanammonium cation.

[0089] Alternatively, N,N,N-trialkylbenzylammonium cations can also be used as organic templates. In this case, the alkyl groups are each independently selected from alkyl groups, preferably lower alkyl groups, and more preferably methyl groups. Among N,N,N-trialkylbenzylammonium cations, the most preferred compound is N,N,N-trimethylbenzylammonium cation.

[0090] Such cations are accompanied by anions. Examples of such anions include Cl. - ,Br - or I - These include halogen ions, hydroxide ions, acetates, sulfates, and carboxylates such as those listed above. Among these, hydroxide ions are particularly suitable for use in forming CHA-type zeolite. Hydroxide ions function as an alkali source as described above.

[0091] The ratio of the Si and Al element sources in the aqueous reaction mixture is typically determined by the molar ratio of the oxides of each element, i.e., SiO 2 / Al 2 O 3 The SiO of this aqueous reaction mixture is expressed as a molar ratio. 2 / Al 2 O 3The ratio may be any ratio that allows the formation of a zeolite having the above-mentioned SAR, and is usually 5 or more, preferably 20 or more, more preferably 30 or more, even more preferably 40 or more, particularly preferably 50 or more, and most preferably 60 or more. The upper limit is usually 500 or less, preferably 200 or less, more preferably 150 or less, and even more preferably 140 or less. 2 / Al 2 O 3 The ratio within this range is preferable from the viewpoint of crystallizing the CHA-type aluminosilicate zeolite, which can form a dense membrane. 2 / Al 2 O 3 The molar ratio is the SiO 2 / Al 2 O 3 In relation to the molar ratio, it is also preferable that it is within the preferred range described below.

[0092] The ratio of silica source to organic template in the aqueous reaction mixture is SiO 2 The molar ratio of the organic template to the SiO 2 The organic template / SiO ratio is usually 0.005 or more, preferably 0.01 or more, more preferably 0.02 or more, and usually 1 or less, preferably 0.4 or less, more preferably 0.2 or less. 2 A ratio within this range is preferable from the viewpoints of forming a dense zeolite membrane and of the fact that the formed zeolite has high acid resistance and Al is unlikely to be desorbed. 2 The ratio within the above range is particularly preferred from the viewpoint of forming a dense and acid-resistant CHA-type aluminosilicate zeolite.

[0093] The ratio of the Si element source to the metal hydroxide in the aqueous reaction mixture is M (2/n) O / SiO 2 (wherein M represents an alkali metal or alkaline earth metal, and n represents its valence, 1 or 2) The molar ratio is usually 0.02 or more, preferably 0.04 or more, more preferably 0.05 or more, and usually 0.5 or less, preferably 0.4 or less, more preferably 0.3 or less.

[0094] When forming a CHA-type aluminosilicate zeolite membrane, it is preferable to include potassium (K) among the alkali metals in order to produce a denser and more crystalline membrane. The molar ratio of K to the total of alkali metals and alkaline earth metals is usually 0.01 or more, preferably 0.1 or more, more preferably 0.3 or more, and the upper limit is usually 1 or less. The addition of K to the aqueous reaction mixture constituted in the above-mentioned preferred range is suitable from the viewpoint of controlling the integrated intensity of the peak near 2θ = 9.6 ° in the X-ray diffraction pattern when the surface of the above-mentioned zeolite membrane is irradiated with X-rays that reach the inorganic porous support to 2.0 times or more and less than 6.0 times the integrated intensity of the peak near 2θ = 20.8 °.

[0095] The ratio of elemental Si source to water in the aqueous reaction mixture is 2 The molar ratio of water to 2 O / SiO 2 H is usually 10 or more, preferably 30 or more, more preferably 40 or more, and particularly preferably 50 or more, and usually 1000 or less, preferably 500 or less, more preferably 200 or less, and particularly preferably 150 or less, in terms of mole ratio. 2 O / SiO 2 The molar ratio within the above range is preferable from the viewpoint of producing a dense zeolite membrane.

[0096] The amount of water is particularly important in producing a dense zeolite membrane, and a dense membrane tends to be produced under conditions where the amount of water is greater than the amount of silica, compared to the general conditions of the powder synthesis method. Generally, the amount of water used in synthesizing powdered CHA-type aluminosilicate zeolite is H 2 O / SiO 2 The molar ratio is about 15 to 50. 2 O / SiO 2 By setting the molar ratio high (50 to 1000), i.e., by using conditions with a high water content, the formation of zeolite in the synthesis gel can be suppressed, and as a result, the accumulation of crystals on the support is suppressed. In addition, the growth rate of CHA-type aluminosilicate zeolite on the surface of the support, etc., becomes constant, which is preferable from the viewpoint of obtaining a zeolite membrane composite with high separation performance, which is crystallized into a dense membrane.

[0097] Furthermore, adding seed crystals during hydrothermal synthesis is preferable from the viewpoint of promoting crystallization of zeolite on the support. The method of adding seed crystals is not limited, and may be a method of adding seed crystals to an aqueous reaction mixture, as in the synthesis of powdered zeolite, or a method of attaching seed crystals to a support. When producing a membrane composite, it is preferable to attach seed crystals to a support. Attaching seed crystals to a support in advance makes it easier to produce a dense zeolite membrane with good separation performance.

[0098] The seed crystals to be used may be of any type as long as they are zeolite that promotes crystallization, but for efficient crystallization, they preferably have the same crystal type as the zeolite membrane to be formed. When forming a zeolite membrane of CHA-type aluminosilicate, it is preferable to use CHA-type zeolite seed crystals.

[0099] The particle size of the seed crystals is preferably such that the seed crystals are held on the support so as to be prevented from falling off during hydrothermal synthesis, and do not penetrate into the support in large quantities. The particle size of the seed crystals is, as an average particle size measured with a laser diffraction particle size distribution analyzer, usually 0.5 nm or more, preferably 100 nm or more, and more preferably 500 nm or more, and usually 5 μm or less, preferably 3 μm or less, and more preferably 2 μm or less.

[0100] The method for attaching the seed crystals to the support is not limited, and may be, for example, a dipping method in which the seed crystals are dispersed in a solvent such as water and the support is immersed in the slurry to attach the seed crystals to the surface, or a method in which a slurry in which the seed crystals are mixed with a solvent such as water is applied to the support. From the viewpoint of controlling the amount of attached seed crystals and producing a membrane composite with good reproducibility, the dipping method is more preferred.

[0101] The dispersion medium for the seed crystal slurry is not limited, but is particularly preferably water or an alkaline aqueous solution. The type of alkaline aqueous solution is not limited, but is preferably a sodium hydroxide aqueous solution or a potassium hydroxide aqueous solution. These alkaline species may also be mixed. The alkali concentration in the dispersion medium is not limited, but is usually 0.0001 mol% or more, preferably 0.0002 mol% or more, more preferably 0.001 mol% or more, and even more preferably 0.002 mol% or more. The alkali concentration is also usually 1 mol% or less, preferably 0.8 mol% or less, more preferably 0.5 mol% or less, and even more preferably 0.2 mol% or less.

[0102] The amount of seed crystals, which are the dispersoids in the seed crystal slurry, is not limited and is typically 0.01 mass% or more, preferably 0.02 mass% or more, and more preferably 0.05 mass% or more, relative to the total mass of the dispersion. Furthermore, the amount is typically 20 mass% or less, preferably 10 mass% or less, more preferably 5 mass% or less, and even more preferably 2 mass% or less. When the amount of dispersed seed crystals is equal to or greater than the above-mentioned lower limit, the amount of seed crystals attached to the support is not too small, which can prevent the formation of areas on the support surface where zeolite is not produced during hydrothermal synthesis. Therefore, a defective membrane is less likely to be formed. When the amount of seed crystals in the dispersion is equal to or less than the above-mentioned upper limit, the seed crystals not retained on the support will fall during hydrothermal synthesis, promoting the growth of zeolite crystals in the synthesis gel and reducing the possibility of inhibiting the growth of the zeolite membrane.

[0103] It is preferable to attach seed crystals to a support by dipping or by applying a slurry, and then dry the support before forming the zeolite membrane.

[0104] The amount of seed crystals to be attached to the support in advance is not limited. 2The mass per unit area is usually 0.01 g or more, preferably 0.05 g or more, more preferably 0.5 g or more, and usually 100 g or less, preferably 50 g or less, more preferably 10 g or less, and even more preferably 3 g or less. If the amount of seed crystals is less than the lower limit, crystallization becomes difficult, and the zeolite membrane tends to grow insufficiently or unevenly. If the amount of seed crystals exceeds the upper limit, the seed crystals may increase the surface irregularities of the support, or seed crystals that fall from the support surface may facilitate the growth of spontaneous nuclei, inhibiting membrane growth on the support. In either case, it tends to be difficult to produce a dense zeolite membrane.

[0105] In particular, it is effective to maximize the amount of seed crystals attached on the support within a range that allows the seed crystals to be prevented from falling off during synthesis, from the viewpoints of increasing the ratio of the integrated intensity of the peak near 2θ = 9.6° to the integrated intensity of the peak near 2θ = 20.8° in the X-ray diffraction pattern obtained when X-rays are irradiated at the minimum incident angle that transmits through the zeolite membrane, and of reducing the membrane thickness.

[0106] SiO seed crystal 2 / Al 2 O 3 The molar ratio may be any ratio that allows the formation of a zeolite having the above-mentioned SAR, and is usually 15 or more, preferably 18 or more, more preferably 20 or more, even more preferably 21 or more, particularly preferably 23 or more, and most preferably 25 or more. The upper limit is usually 500 or less, preferably 70 or less, more preferably 50 or less, and even more preferably 40 or less. 2 / Al 2 O 3 A ratio within this range is preferable from the viewpoint of crystallizing the CHA-type aluminosilicate zeolite, which can form a dense film.

[0107] The method for fixing the support in the hydrothermal synthesis is not limited, and can be selected from any method such as vertical placement, horizontal placement, etc. In this case, the zeolite membrane may be formed by a static method, or may be formed while stirring the aqueous reaction mixture.

[0108] The temperature for forming the zeolite membrane is not limited, but is usually 100°C or higher, preferably 120°C or higher, and more preferably 150°C or higher, and usually 200°C or lower, preferably 190°C or lower, and more preferably 180°C or lower. If the reaction temperature is too low, the zeolite may be difficult to crystallize. On the other hand, if the reaction temperature is too high, crystals of a type different from the intended crystal type may be easily formed.

[0109] The heating (reaction) time is not limited, but is usually 1 hour or more, preferably 5 hours or more, and more preferably 10 hours or more, and usually 10 days or less, preferably 5 days or less, more preferably 3 days or less, and even more preferably 1 day or less. If the reaction time is too short, the zeolite may be difficult to crystallize. If the reaction time is too long, a large amount of crystals may grow, resulting in high permeation resistance.

[0110] The heating temperature, heating time, temperature rise time, and SiO of the seed crystals when crystallizing the zeolite 2 / Al 2 O 3 The molar ratio combination is 170 to 190°C for 16 to 20 hours, the temperature rise time from room temperature to the heating temperature is 1.5 to 5.0 hours, and the SiO 2 / Al 2 O 3 The molar ratio is preferably 25 or more. In addition, the H 2 O / SiO 2 The molar ratio is preferably less than 100. Furthermore, it is preferable to maximize the amount of seed crystals attached to the support within the range that allows the seed crystals to be prevented from falling off during synthesis.

[0111] The heating temperature, heating time, temperature rise time, seed crystal conditions, and H of the aqueous reaction mixture for crystallization 2 O / SiO 2When the molar ratio combination is within the above range, the zeolite membrane of the present invention can be obtained. By shortening the time required to reach the reaction temperature, the seed crystals do not completely dissolve and can be kept in a highly reactive state, making it difficult for defects to form in the membrane. Furthermore, by forming the membrane at a high temperature in a short time under this condition, the generation of zeolite crystals in the aqueous reaction mixture can be suppressed, and a membrane with stable performance can be obtained. In addition, the SiO 2 / Al 2 O 3 Increasing the ratio makes it possible to obtain a membrane suitable for gas separation. 2 / Al 2 O 3 When the molar ratio is increased, the surface of the seed crystal melts, making it easier for the seed crystal to function.

[0112] The pressure during zeolite membrane formation is not limited, and the autogenous pressure generated when an aqueous reaction mixture placed in a sealed container is heated to this temperature range is sufficient. If necessary, pressure may be increased by adding a gas inert to hydrothermal synthesis, such as nitrogen.

[0113] The support on which the zeolite membrane has been formed by hydrothermal synthesis is washed with water, then heat-treated and dried. Here, "heat-treated" means drying the zeolite membrane composite by applying heat, or, when an organic template is used, calcining and removing the organic template.

[0114] The temperature of the heat treatment, when aimed at drying, is usually 50° C. or higher, preferably 80° C. or higher, more preferably 100° C. or higher, and usually 200° C. or lower, preferably 150° C. or lower. When aimed at calcining the organic template, the temperature is usually 350° C. or higher, preferably 400° C. or higher, more preferably 430° C. or higher, even more preferably 450° C. or higher, and usually 900° C. or lower, preferably 850° C. or lower, even more preferably 800° C. or lower, particularly preferably 750° C. or lower.

[0115] If the calcination temperature is too low, the proportion of the organic template remaining tends to be high, resulting in fewer pores in the zeolite, which may reduce the amount of gas permeation during separation and concentration.If the calcination temperature is too high, the difference in thermal expansion coefficient between the support and the zeolite becomes large, which may lead to the zeolite membrane becoming more susceptible to cracks, causing the zeolite membrane to lose its density and resulting in reduced separation performance.

[0116] The heat treatment time is not limited as long as it is sufficient to sufficiently dry the zeolite membrane or to calcinate the organic template, and is preferably 0.5 hours or more, more preferably 1 hour or more. The upper limit is not limited, and is usually 200 hours or less, preferably 150 hours or less, more preferably 100 hours or less, and particularly preferably 24 hours or less.

[0117] The calcination time varies depending on the rate of temperature increase or decrease, but is not limited as long as it is a time that allows the organic template to be sufficiently removed, and is preferably 1 hour or more, more preferably 5 hours or more. There is no upper limit, and the calcination time is, for example, usually 200 hours or less, preferably 150 hours or less, more preferably 100 hours or less, and particularly preferably 24 hours or less. Calcination may be carried out in an air atmosphere, or in an atmosphere in which oxygen or an inert gas is added to air.

[0118] The rate of temperature rise during firing is preferably as slow as possible to prevent cracks in the zeolite membrane due to the difference in thermal expansion coefficient between the support and the zeolite membrane. The rate of temperature rise is usually 5°C / min or less, preferably 2°C / min or less, more preferably 1°C / min or less, and particularly preferably 0.5°C / min or less. In consideration of workability, the rate of temperature rise is usually 0.1°C / min or more.

[0119] It is also preferable to control the temperature drop rate after firing to avoid cracking in the zeolite membrane. As with the temperature rise rate, the slower the temperature drop rate, the better from the viewpoint of avoiding cracking. The temperature drop rate is usually 5°C / min or less, preferably 2°C / min or less, more preferably 1°C / min or less, and particularly preferably 0.5°C / min or less. In consideration of workability, the temperature drop rate is usually 0.1°C / min or more.

[0120] When the hydrothermal synthesis is carried out in the presence of an organic template, the organic template can be removed from the obtained zeolite membrane composite by extraction in addition to the heat treatment described above. Preferably, the organic template is removed by heat treatment, i.e., calcination.

[0121] The zeolite membrane may be subjected to ion exchange or silylation treatment as required.

[0122] When a zeolite membrane is synthesized using an organic template, ion exchange is usually performed after removing the organic template. The ions to be exchanged include protons, Na + , K. + or Li + alkali metal ions such as Ca 2+ , Mg 2+ , Sr 2+ or Ba 2+ and ions of transition metals such as Fe, Cu, Zn, Ag, Al, Ga, or La. Among these, protons, Na + , Ca 2+ , Mg 2+ and ions of Fe, Al, Ga or La are preferred.

[0123] Ion exchange is carried out by exchanging the zeolite membrane with NH after calcination (when using an organic template, etc.). 4 NO 3 or NaNO 3 or an aqueous solution containing an ammonium salt such as ammonium hydroxide or the ions to be exchanged, or in some cases an acid such as hydrochloric acid, at a temperature of usually from room temperature to 100°C, followed by washing with water. After ion exchange, the material may be further calcined at 200°C to 500°C, if necessary.

[0124] When ion exchange is performed with monovalent ions having a large ionic radius, the effective pore size tends to become smaller. On the other hand, when ion exchange is performed with monovalent ions having a small ionic radius, the effective pore size becomes close to the pore size of the CHA structure. Also, in the case of divalent ions such as calcium, depending on the position of the exchange site, the effective pore size becomes close to the pore size of the CHA structure. In this way, ion exchange can be used to control the molecular adsorption performance or the pore size of the zeolite, thereby controlling the permeation performance.

[0125] The silylation treatment is carried out by immersing the membrane composite in a solution containing, for example, a Si compound. This modifies the surface of the zeolite membrane with the Si compound, imparting or enhancing the specific physicochemical properties described above to the membrane composite. For example, by reliably forming a layer rich in Si—OH on the surface of the zeolite membrane, the polarity of the membrane surface is improved, which is thought to improve the separation performance of polar molecules. Furthermore, modifying the surface of the zeolite membrane with a Si compound can also have the secondary effect of sealing fine defects present on the membrane surface.

[0126] The effective pore size of zeolite can also be reduced by silylation treatment. By silylating the terminal silanols on the outer surface and then laminating a silylated layer, the effective pore size of the pores facing the outer surface of the zeolite is reduced. In this way, the silylation treatment can control the molecular adsorption performance or the pore size of the zeolite, and thus the permeation performance.

[0127] The solvent used for the silylation treatment may be water or an organic solvent. The solution may be acidic or basic, in which case the silylation reaction is catalyzed by the acid or base. The silylating agent used is not limited, but alkoxysilanes are preferred. The treatment temperature is usually from room temperature to 150°C or less, and the treatment time is about 10 minutes to 30 hours, which may be determined appropriately depending on the silylating agent and solvent type.

[0128] The membrane composite of this embodiment can be produced by the above-described production method, and has the excellent properties described above. The membrane composite can be suitably used for producing purified components by membrane separation of a gas mixture or a liquid mixture.

[0129] [Method for Producing Purified Component] The method for producing a purified component using the membrane composite of this embodiment includes a step of contacting a mixture with the membrane composite.

[0130] The mixture contains a first component and a second component. The first component is a component having higher permeability through the zeolite membrane, and the second component is a component having lower permeability through the zeolite membrane than the first component. Both the first component and the second component may be liquid or gas. Furthermore, both the first component and the second component may be a single component or a mixture of two or more compounds.

[0131] The method for producing a purified component of this embodiment produces one or both of a first purified component and a second purified component. The first purified component is the first component that has permeated the zeolite membrane, and the second purified component is the second component that has not permeated the zeolite membrane.

[0132] In this way, the method for producing a purified component of this embodiment achieves one or both of separation of a first component and concentration of a second component. Such separation of a first component and concentration of a second component can be carried out in the same manner as the method for separating or concentrating a gas mixture or the method for separating or concentrating a liquid mixture described in Patent Document 1, except that the membrane composite of this embodiment is used.

[0133] [Method for Separating or Concentrating a Gas Mixture] The method for separating or concentrating a gas mixture is a method for concentrating a gas mixture by contacting a gas mixture consisting of a plurality of gas components with the above-mentioned membrane composite, and separating a gas component with high permeability from the gas mixture by permeating the gas component, or concentrating a gas component with low permeability by permeating the gas component with high permeability. One of the separation functions of the zeolite membrane in this embodiment is separation as a molecular sieve, and this method can suitably separate gas molecules having a size equal to or larger than the effective pore size of the zeolite used from gas molecules having a size smaller than that.

[0134] Therefore, in this embodiment, a highly permeable gas component is a gas component consisting of gas molecules that easily pass through the pores of the zeolite crystalline phase of the CHA-type aluminosilicate, and a gas component consisting of gas molecules with a molecular diameter of approximately 0.38 nm or less is preferred.

[0135] Another separation function of the membrane composite in this embodiment is to control the adsorption of gas molecules to the zeolite membrane by controlling the surface properties of the zeolite. That is, by controlling the polarity of the zeolite, it is possible to make it easier for molecules with a high adsorption tendency to pass through the zeolite.

[0136] Preferred gas mixtures include gases containing at least one component selected from carbon dioxide, hydrogen, oxygen, nitrogen, methane, ethane, ethylene, propane, propylene, normal butane, isobutane, 1-butene, 2-butene, isobutene, sulfur hexafluoride, helium, carbon monoxide, nitric oxide, water, etc. Among the components of the gas mixture containing such gases, gas components with high permeance permeate the membrane composite and are separated, while gas components with low permeance are concentrated in the feed gas side.

[0137] Furthermore, the gas mixture preferably contains at least two of the above-mentioned components. In this case, the two components are preferably a combination of a component with high permeance and a component with low permeance.

[0138] Gas separation conditions vary depending on the type or composition of the target gas or the performance of the zeolite membrane, but the temperature is usually -20 to 300°C, preferably 0 to 200°C, and more preferably 0 to 150°C. Separation at 0 to 25°C is often close to the ambient temperature, and is therefore preferred in that it does not require energy or requires little energy to adjust the temperature of the gas to be separated. Gases that are highly adsorbable to zeolite membranes tend to have increased permeability at low temperatures. Therefore, in order to increase the permeability of such gases, the gas to be separated may be cooled to a range of 25°C or less and -20°C or more.

[0139] The pressure of the supply gas may be the same if the gas to be separated is at a high pressure, or may be adjusted by reducing the pressure as needed to a desired pressure. If the pressure of the gas to be separated is lower than the pressure used for separation, the pressure may be increased using a compressor or the like.

[0140] The pressure of the supply gas is not limited, but is usually atmospheric pressure or higher, preferably 0.1 MPa or higher, more preferably 0.11 MPa or higher, and the upper limit is usually 20 MPa or lower, preferably 10 MPa or lower, more preferably 1 MPa or lower.

[0141] The pressure difference between the gas on the supply side and the gas on the permeation side is not limited, but is usually 20 MPa or less, preferably 10 MPa or less, more preferably 5 MPa or less, and even more preferably 1 MPa or less. It is usually 0.001 MPa or more, preferably 0.01 MPa or more, and more preferably 0.02 MPa or more. Here, "pressure difference" refers to the difference between the partial pressure of the gas on the supply side and the partial pressure on the permeation side. Furthermore, pressure [Pa] is absolute pressure unless otherwise specified.

[0142] The pressure on the permeation side is not limited, but is usually 10 MPa or less, preferably 5 MPa or less, more preferably 1 MPa or less, and even more preferably 0.5 MPa or less. The lower limit is not particularly limited, as long as it is 0 MPa or more. When the pressure is 0 MPa, separation can be performed until the concentration of the highly permeable gas in the less permeable gas is at its lowest. If there is an application in which the permeation side gas is used at a high pressure, the permeation side pressure can be set high.

[0143] The flow rate of the feed gas may be any flow rate capable of compensating for the decrease in the permeating gas. The flow rate of the feed gas may be any flow rate capable of mixing the gases so that the concentration of the gas with low permeability in the immediate vicinity of the membrane matches the concentration in the entire gas. The flow rate of the feed gas depends on the pipe diameter of the separation unit or the separation performance of the membrane, but is usually 0.5 mm / sec or more, preferably 1.0 mm / sec or more. The upper limit is not limited, but is usually 1 m / sec or less, preferably 0.5 m / sec or less.

[0144] The separation or concentration of a gas mixture may involve the use of a sweep gas, in which a gas different from the feed gas is passed through the permeation side of the membrane and the gas that permeates the membrane is recovered.

[0145] The pressure of the sweep gas is usually atmospheric pressure, but is not limited thereto, and is preferably 20 MPa or less, more preferably 10 MPa or less, and further preferably 1 MPa or less, and the lower limit is preferably 0.09 MPa or more, more preferably 0.1 MPa or more. In some cases, the sweep gas may be used at reduced pressure.

[0146] The flow rate of the sweep gas is not limited, but is sufficient as long as it can sufficiently replace the permeating gas, and is usually 0.5 mm / sec or more, preferably 1.0 mm / sec or more, and the upper limit is not limited, but is usually 1 m / sec or less, preferably 0.5 m / sec or less.

[0147] The apparatus used for gas separation is not limited, but is usually used as a module. The membrane module may be, for example, an apparatus as shown in Fig. 3 described later, or may be, for example, a membrane module exemplified in "Gas Separation and Purification Technology" (Toray Research Center, Inc., 2007, p. 22).

[0148] When performing membrane separation of gas, zeolite membranes may be used in multiple stages. That is, the gas to be separated may be supplied to a membrane module, and the non-permeated gas that does not permeate the zeolite membrane may be supplied to another membrane module. Alternatively, the permeated gas may be supplied to another membrane module. The former method can further increase the concentration of less permeable components in the non-permeated side, while the latter method can further increase the concentration of more permeable components in the permeated gas.

[0149] When separation is performed using multiple zeolite membranes, the gas pressure may be adjusted by a pressure booster or the like as necessary when supplying the gas to the subsequent zeolite membrane.

[0150] Furthermore, when using zeolite membranes in multiple stages, zeolite membranes with different performance may be arranged in each stage. Generally, zeolite membranes with high permeability have low separation performance, while membranes with high separation performance tend to have low permeability. Therefore, when treating a gas component to be separated or concentrated until it reaches a predetermined concentration, a membrane with high permeability requires a smaller membrane area, while the low-permeability component to be concentrated on the non-permeate side tends to easily permeate to the permeate side. A membrane with high separation performance tends to require a larger membrane area, but the low-permeability component to be concentrated on the non-permeate side is less likely to permeate to the permeate side. Separation using a single type of zeolite membrane makes it difficult to control the relationship between the required membrane area and the permeation rate of the concentrated target gas. However, using zeolite membranes with different performance makes this control easier. By arranging zeolite membranes so that the optimal relationship between membrane area and permeation rate of the concentrated target gas is achieved based on the membrane cost and the price of the gas to be separated or recovered, the overall benefits can be maximized.

[0151] The membrane composite of the present embodiment has excellent chemical resistance, oxidation resistance, heat stability, and pressure resistance, and exhibits high permeability and separation performance, has excellent durability, and exhibits excellent separation performance, particularly in separating inorganic gases or lower hydrocarbons.

[0152] The term "high permeability" used herein means a sufficient throughput. For example, the permeance [mol (m 2 ・s・Pa)-1 When carbon dioxide is passed through at a temperature of 50°C and a differential pressure of 0.1 MPa, the -8 or more, preferably 3 × 10 -7 or more, more preferably 5 × 10 -7 More preferably, 7 × 10 -7 More preferably, 1×10 -6 The upper limit is not limited, and is usually 3 × 10 -4 The following is the result.

[0153] The temperature dependence of the carbon dioxide permeance is 2 / Al 2 O 3 When the molar ratio is relatively large, the SiO of the zeolite membrane tends to be small. 2 / Al 2 O 3 By setting the molar ratio within the above-mentioned relatively large range, it is possible to suppress excessive adsorption of carbon dioxide onto the zeolite membrane and reduce the temperature dependency of permeance.

[0154] In addition, the permeance [mol (m 2 ・s・Pa) -1 For example, when methane is passed through under similar conditions, the -7 Below 3 × 10, preferably -8 Less than 1×10, more preferably 1×10 -8 Ideally, the permeance is 0, but in practice it is 10 -10 There may be cases where the order is more than enough.

[0155] Here, "permeance" (also called "permeability") is the value obtained by dividing the amount of a substance that permeates by the product of the membrane area, time, and the partial pressure difference between the supply side and permeation side of the substance that permeates, and its unit is [mol (m 2 ・s・Pa) -1 The permeance can be calculated by the method described in the Examples below.

[0156] The selectivity of a zeolite membrane is expressed by an ideal separation factor and a separation factor. The ideal separation factor and the separation factor are indicators of selectivity generally used in membrane separation. The ideal separation factor is a value calculated by the method in the Examples described later, and the separation factor is a value calculated by the method described below.

[0157] In the separation of a mixed gas, the separation factor is calculated by the following formula (1): 1 and Q' 2 are the permeation amounts [mol (m 2 ・s) -1 ], and P' 1 and P' 2 and Q′ respectively represent the partial pressures [Pa] of the gas with high permeability and the gas with low permeability in the feed gas. 1 / Q' 2 ) / (P' 1 / P' 2 ) (1)

[0158] For example, when carbon dioxide and methane are permeated at a temperature of 50°C and a differential pressure of 0.1 MPa, the ideal separation factor is usually 10 or more, preferably 20 or more, more preferably 30 or more, even more preferably 40 or more, and particularly preferably 50 or more. The upper limit of the ideal separation factor is when only carbon dioxide permeates, in which case the factor is infinite, but in practice the separation factor may be about 100,000 or less.

[0159] For example, when a mixed gas of carbon dioxide and methane in a volume ratio of 1:1 is permeated at a temperature of 50°C and a differential pressure of 0.1 MPa, the separation factor is usually 10 or more, preferably 20 or more, more preferably 30 or more, even more preferably 40 or more, and particularly preferably 50 or more. The upper limit of the separation factor is when only carbon dioxide permeates, in which case the separation factor is infinite, but in practice the separation factor may be about 100,000 or less.

[0160] The membrane composite of this embodiment has excellent properties as described above, and can be particularly suitably used in the following gas separation techniques, for example.

[0161] Carbon dioxide separation technologies include the removal of carbon dioxide from natural gas, and the removal of carbon dioxide from landfill gas (containing approximately 60% methane, approximately 40% carbon dioxide, trace amounts of nitrogen, and water vapor) generated by landfilling organic matter such as household waste.

[0162] Hydrogen separation technologies include hydrogen recovery in the petroleum refining industry, hydrogen recovery and purification (mixtures of hydrogen, carbon monoxide, carbon dioxide, hydrocarbons, etc.) in various reaction processes in the chemical industry, and the production of high-purity hydrogen for fuel cells. Hydrogen for fuel cells is produced by the steam reforming reaction of methane, and H 2 , CO, CH 4 and H 2 There is a need for separation of hydrogen from O gas mixtures.

[0163] Other examples of oxygen separation technology include the production of oxygen-enriched gas from air (for medical use, oxygen-enriched air for combustion, etc.), nitrogen separation technology includes the production of nitrogen-enriched gas from air (for explosion prevention, oxidation prevention, etc.), water vapor separation (dehumidification of precision machinery, etc.), dissolved gas separation (degassing from water and organic liquids), and organic gas separation (organic gas separation in the oil refining industry and petrochemical industry, separation of olefins and paraffins), etc.

[0164] [Method for Separating or Concentrating a Liquid Mixture] The method for separating or concentrating a liquid mixture is a method for concentrating a liquid mixture by contacting the above-mentioned membrane composite with a liquid mixture consisting of a plurality of components, and separating a highly permeable component from the liquid mixture by permeating the highly permeable component, or concentrating a less permeable component by permeating and separating the highly permeable component. In this method, the membrane composite of the present embodiment is used as a preferred embodiment.

[0165] In the above method, a liquid mixture containing an organic compound is contacted with either the support side or the zeolite membrane side through a support equipped with a zeolite membrane, and the other side is pressurized at a lower pressure than the other side, thereby selectively allowing components with high permeability through the zeolite membrane (substances in the mixture with relatively high permeability) to permeate from the liquid mixture, i.e., as the main permeating component. This allows the highly permeable components (substances) to be separated from the liquid mixture. As a result, by increasing the concentration of specific organic compounds in the mixture (substances in the mixture with relatively low permeability), the specific organic compounds can be separated, recovered, or concentrated.

[0166] The liquid mixture to be separated or concentrated is not limited as long as it is a liquid mixture consisting of multiple components that can be separated or concentrated by the membrane composite of this embodiment, and may be any mixture.

[0167] When the liquid mixture is, for example, a mixture of an organic compound and water (hereinafter also referred to as "aqueous organic compound"), water usually has a higher permeability to a zeolite membrane, so the water is separated from the liquid mixture and the organic compound is concentrated in the original liquid mixture. A separation or concentration method called a pervaporation method or a vapor permeation method is one of the preferred embodiments of the method for producing a purified component in this embodiment.

[0168] The pervaporation method is a separation or concentration method in which a liquid mixture is introduced directly into a separation membrane, and therefore can simplify processes including separation or concentration.

[0169] The vapor permeation method is a separation and concentration method in which a liquid mixture is vaporized and then introduced into a separation membrane. Therefore, it can be used in combination with a distillation apparatus, or can be used for separation at higher temperatures or pressures. Furthermore, since the vapor permeation method vaporizes the liquid mixture and then introduces it into the separation membrane, it is possible to further reduce the influence of impurities contained in the feed liquid or substances that form associations or oligomers in the liquid state on the zeolite membrane. The membrane composite of this embodiment can be suitably used for either method.

[0170] Furthermore, when separation is performed at high temperatures using the vapor permeation method, the higher the temperature, the lower the separation performance generally becomes. However, the membrane composite of this embodiment can exhibit high separation performance even at high temperatures. In addition, since the vapor permeation method usually involves vaporizing a liquid mixture before separation, separation usually takes place under more severe conditions than pervaporation. Therefore, durability of the membrane composite is also required. The membrane composite of this embodiment has the durability to enable separation even under high-temperature conditions. Therefore, it is suitable for the vapor permeation method.

[0171] The vapor permeation method can be carried out using an apparatus such as that shown in FIG. 3 of Patent Document 1. In this apparatus, the liquid to be separated is sent to a vaporizer at a predetermined flow rate by a liquid feed pump, and the entire amount is vaporized by heating in the vaporizer to form a gas to be separated. The gas to be separated is introduced into a zeolite membrane composite module in a thermostatic chamber and supplied to the outside of the zeolite membrane composite. The zeolite membrane composite module is composed of a zeolite membrane composite housed in a housing. The inside of the zeolite membrane composite is depressurized by a vacuum pump, creating a pressure difference of approximately 1 atmosphere with the gas to be separated. The internal pressure can be measured with a Pirani gauge (not shown). This pressure difference causes water, a permeating substance in the gas to be separated, to permeate through the zeolite membrane composite. The permeated substance is collected in a permeate collection trap. Any substances that are not completely collected in the permeate collection trap are collected in a cold trap. Meanwhile, the non-permeated components in the gas to be separated are liquefied and collected in a liquid recovery trap.

[0172] The membrane composite of this embodiment exhibits high permeability and selectivity even when treating hydrous organic compounds with a water content of 20% by mass or more, and has the performance as a separation membrane with excellent durability.

[0173] The term "high permeability" as used herein means a sufficient throughput. For example, the permeation flux of a substance permeating a zeolite membrane is 1 atmosphere (1.01 × 10) at 70°C when a mixture of 2-propanol or N-methyl-2-pyrrolidone with a water content of 30% by mass and water is 5 If the pressure difference is 1 kg / (m2 ·h) or more, preferably 3 kg / (m 2 h) or more, more preferably 5 kg / (m 2 The upper limit of the permeation flux is not limited, and is usually 20 kg / (m 2 ·h) or less, preferably 15 kg / (m 2 ・h) The following:

[0174] High permeability can also be expressed in terms of permeance (also referred to as "permeability"). "Permeance" refers to the permeation flux per pressure difference (pressure normalized flux), and is the value obtained by dividing the amount of permeating substance by the product of the membrane area, time, and the partial pressure difference of water. When expressed in units of permeance, the water permeance is, for example, the permeance of a mixture of 2-propanol or N-methyl-2-pyrrolidone with a water content of 30% by mass at 70°C under 1 atmosphere (1.01 x 10 5 When the pressure difference is 3 × 10 -7 mol / (m 2 s Pa) or more, preferably 5×10 -7 mol / (m 2 s Pa) or more, more preferably 1×10 -6 mol / (m 2 s Pa) or more, particularly preferably 2×10 -6 mol / (m 2 The upper limit of the permeance is not limited, and is usually 1×10 -4 mol / (m 2 s Pa) or less, preferably 5×10 -5 mol / (m 2 .s.Pa) or less.

[0175] The selectivity of a zeolite membrane is expressed by a separation factor. The separation factor is an index of selectivity generally used in membrane separation, and is calculated by the following formula (2). In formula (2), P α is the mass percent concentration of the main component in the permeate, P β is the mass percent concentration of the minor component in the permeate, F α is the mass percent concentration of the component that is the main component in the permeate in the mixture to be separated, and F βand P represent the mass percent concentration of the component that becomes a minor component in the permeate in the mixture to be separated. α / P β ) / (F α / F β ) (2)

[0176] The separation factor is, for example, a mixture of 2-propanol or N-methyl-2-pyrrolidone with water having a water content of 30% by mass at 70°C under 1 atmosphere (1.01 × 10 5 When permeated with a pressure difference of 100 Pa, the separation factor is usually 1,000 or more, preferably 4,000 or more, more preferably 10,000 or more, and particularly preferably 20,000 or more. The upper limit of the separation factor is when only water permeates, in which case the separation factor is infinite, but it is preferably 10,000,000 or less, more preferably 1,000,000 or less.

[0177] When the object to be separated is a water-containing organic compound, the water content is usually 20% by mass or more, preferably 30% by mass or more, more preferably 45% by mass or more, and usually 95% by mass or less, preferably 80% by mass or less, more preferably 70% by mass or less.

[0178] In the above-mentioned method, the substance that permeates the zeolite membrane is usually water. In this case, if the water content is low, the throughput decreases, which is inefficient. Also, if the water content is too high, the area of ​​the zeolite membrane required for concentration increases (or the number of zeolite membranes increases if the zeolite membranes are tubular), which reduces the economic effect.

[0179] The water content of the hydrous organic compound may be adjusted in advance by a suitable water-adjusting method. In this case, the preferred water content is the same as that described above. Examples of the water-adjusting method include known methods such as distillation, pressure swing adsorption (PSA), temperature swing adsorption (TSA), and a desiccant system.

[0180] Furthermore, water may be further separated from the hydrous organic compounds from which water has been separated by the zeolite composite membrane, thereby achieving a higher degree of water separation and a higher degree of concentration of the hydrous organic compounds.

[0181] Examples of organic compounds include organic acids, alcohols, ketones, aldehydes, ethers, nitrogen-containing organic compounds, and esters. Examples of organic acids include carboxylic acids, sulfonic acids, sulfinic acids, habituric acids, uric acids, phenols, enols, diketone compounds, thiophenols, imides, oximes, aromatic sulfonamides, and primary and secondary nitro compounds. Examples of carboxylic acids include acetic acid, acrylic acid, propionic acid, formic acid, lactic acid, oxalic acid, tartaric acid, and benzoic acid.

[0182] Examples of alcohols include methanol, ethanol, and isopropanol (2-propanol). Examples of ketones include acetone and methyl isobutyl ketone. Examples of aldehydes include acetaldehyde. Examples of ethers include dioxane and tetrahydrofuran. Examples of nitrogen-containing organic compounds (N-containing organic compounds) include dimethylformamide and N-methylpyrrolidone. Examples of esters include acetate esters and acrylate esters.

[0183] Among these, the membrane composite of the present embodiment can exhibit outstanding effects in a method for separating an organic acid from a mixture of an organic acid and water, which can take advantage of both the characteristics of molecular sieving and hydrophilicity. More preferred examples include separation of carboxylic acids from water, and particularly separation of acetic acid from water.

[0184] When separating an organic substance and water from a mixture of an organic substance other than an organic acid and water, the organic substance preferably has two or more carbon atoms, and more preferably has three or more carbon atoms.

[0185] Among these organic substances other than organic acids, organic compounds containing at least one selected from alcohols, ethers, ketones, aldehydes, and amides are particularly preferred. Among these organic compounds, compounds having 2 to 10 carbon atoms are preferred, and compounds having 3 to 8 carbon atoms are more preferred.

[0186] The organic compound may also be a polymer compound capable of forming a mixture (mixed solution) with water. Examples of such a polymer compound include polymer compounds having a polar group in the molecule, such as polyols such as polyethylene glycol and polyvinyl alcohol; polyamines; polysulfonic acids; polycarboxylic acids such as polyacrylic acid; polycarboxylic acid esters such as polyacrylic acid esters; modified polymer compounds obtained by modifying polymers by graft polymerization or the like; and copolymer polymer compounds obtained by copolymerizing a nonpolar monomer such as an olefin with a polar monomer having a polar group such as a carboxyl group.

[0187] The water-containing organic compound may be a mixture that forms an azeotrope, such as a mixture of water and phenol. Separation of a mixture that forms an azeotrope is preferred in that water can be separated selectively and more efficiently than separation by distillation. Specific examples include mixtures of water with alcohols such as ethanol, 1-propanol, 2-propanol, 1-butanol, or 2-butanol; mixtures of water with esters such as ethyl acetate, ethyl acrylate, or methyl methacrylate; mixtures of water with carboxylic acids such as formic acid, isobutyric acid, or valeric acid; mixtures of water with aromatic organic substances such as phenol or aniline; and mixtures of water with nitrogen-containing substances such as acetonitrile or acrylonitrile.

[0188] Furthermore, the water-containing organic compound may be a mixture of water and a polymer emulsion. Here, "polymer emulsion" refers to a mixture of a surfactant and a polymer, which is commonly used in adhesives, paints, etc. Examples of polymers used in polymer emulsions include polyvinyl acetate, polyvinyl alcohol, acrylic resins, olefin-polar monomer copolymers such as polyolefins or ethylene-vinyl alcohol copolymers, thermoplastic resins such as polystyrene, polyvinyl ether, polyamide, polyesters, or cellulose derivatives, thermosetting resins such as urea resins, phenolic resins, epoxy resins, or polyurethanes, and rubbers such as natural rubber, polyisoprene, polychloroprene, or butadiene copolymers such as styrene-butadiene copolymers. Known surfactants may also be used as the surfactant.

[0189] The membrane composite of this embodiment is acid-resistant, and therefore can be effectively used for separating water from a mixture of water and an organic acid such as acetic acid, or for separating water to promote an esterification reaction.

[0190] The method for separating or concentrating a liquid mixture can be carried out by using the membrane composite of this embodiment in an appropriate separation or concentration device, such as the device shown in Figure 3 of Patent Document 1, and introducing a liquid mixture consisting of multiple components into the device. Such a device used for separation or concentration can be composed of known components.

[0191] [Summary] The membrane composite of the present invention has superior separation performance compared to conventional membrane composites. Therefore, the present invention is expected to contribute to the development and expansion of various separation technologies, and to the achievement of, for example, Goal 9 of the Sustainable Development Goals (SDGs) proposed by the United Nations, "Build resilient infrastructure, promote inclusive and sustainable industrialization, and foster innovation."

[0192] The present invention is not limited to the above-described embodiments, and various modifications are possible within the scope of the claims. Embodiments obtained by appropriately combining the technical means disclosed in different embodiments are also included in the technical scope of the present invention.

[0193] An example of the present invention will be described below. First, the methods for measuring the physical properties and separation performance of the zeolite membranes in the following examples and comparative examples will be described.

[0194] (1) X-ray Diffraction (XRD) XRD measurements were carried out under the following conditions. (Measurement device) Device name: RINT-Ultima III manufactured by Rigaku Corporation Optical system specifications Parallel beam optical system Vertical goniometer D990825A03 Incident side: Sealed X-ray tube (CuKα) Soller Slit (flexible optical system, 5°) Divergence Slit (variable slit) Receiving side: Monochromator Long slit Ni slit (Measurement conditions) X-ray output (CuKα): 40 kV, 30 mA Scanning axis: θ / 2θ Scanning range (2θ): 3.0 to 50.0° Measurement mode: Continuous Reading width: 0.01° Scanning speed: 1° / min Divergence slit: 1.0 mm Divergence vertical limiting slit: 5 mm Scattering slit: Open Receiving slit: Open Offset angle: 0° h: 0 k: 0 l: 0 (Analysis conditions) Software name: PDXL 2 version 2.4.2.0 manufactured by Rigaku Corporation Baseline setting method: Set using the Sonneveld-Visser method. Nodes were set so that the distance between nodes was 2 to 6 degrees and at locations where no peaks existed. Each peak was detected using PDXL2. Detected peaks were visually confirmed, and adjustments were made so that the detection reference point matched the measured peak. The integrated intensity value was calculated by the software. The peak intensity value was calculated by the software.

[0195] During the measurement, the sample was set so that the X-rays were irradiated in a direction parallel to the axial direction of the cylindrical membrane composite, and the top of the sample was set at the same height as the measurement surface of the apparatus.

[0196] (2) Grazing Incidence X-ray Diffraction (GIXD) GIXD measurements were performed in the same manner as XRD, except for controlling the angle of incidence of the X-rays. In GIXD measurements, the angle of incidence of the X-rays was fixed during each measurement, and the angle of incidence was changed for each measurement to perform multiple measurements, thereby controlling the angle of incidence of the X-rays. The angle of incidence was gradually reduced, and the angle of incidence of the X-rays at which all peaks derived from the zeolite membrane were no longer detected was defined as 0°. In addition, the angle of incidence was gradually increased from 0°, and the angle of incidence of the X-rays at which peaks from the support (alumina) began to be detected was defined as the minimum angle of incidence that transmits through the zeolite membrane, and was used as the angle for measuring the zeolite membrane.

[0197] The obtained diffraction pattern was smoothed using analysis software, the Kα2 radiation was removed, and peak detection was performed using the second-order differential method. The obtained peaks were visually confirmed to ensure accurate detection, and the error in the integrated intensity between the actual peak and the detection peak was within 5%. When the irradiation angle was changed, the height of the film surface was fixed so that the X-rays were irradiated at the same position on the film. The integrated intensity value used was the value calculated by the software for the detection peak. The peak intensity value used was the value calculated by the software for the detection peak.

[0198] (3) SEM-EDX measurement (3-1) SEM-EDX measurement on the surface area of ​​the zeolite membrane SiO of the zeolite membrane 2 / Al 2 O 3 To determine the molar ratio, scanning electron microscope-energy dispersive X-ray spectroscopy (SEM-EDX) measurements were performed under the following conditions: The surface of the zeolite membrane was scanned over the entire field of view (25 μm × 18 μm) at a magnification of 5000 times to measure the SiO of the entire field of view. 2 / Al 2 O 3 The average molar ratio was calculated. Apparatus name (SEM): JSM-7900F (manufactured by JEOL Ltd.) Acceleration voltage: 6 kV Detector: secondary electron detector Apparatus name (EDS): Ultim Max 170 (manufactured by Oxford Co.) Acceleration voltage: 6 kV Magnification: 5000x

[0199] (3-2) SEM-EDX measurement at the surface of the zeolite membrane SiO of the zeolite membrane2 / Al 2 O 3 To determine the molar ratio, scanning electron microscope-energy dispersive X-ray spectroscopy (SEM-EDX) measurements were performed under the following conditions: Three surface images of the zeolite membrane at a magnification of 5000 times were used to measure the SiO content at nine or more points in an area of ​​(2±0.5 μm) × (2±0.5) μm. 2 / Al 2 O 3 The molar ratio was measured, and the average value was taken as the surface SAR. Apparatus name (SEM): JSM-7900F (manufactured by JEOL Ltd.) Acceleration voltage: 6 kV Detector: Secondary electron detector Apparatus name (EDS): Ultim Max 170 (manufactured by Oxford Co., Ltd.) Acceleration voltage: 6 kV Magnification: 5000 times (3-3) SEM-EDX measurement of seed crystals SiO of zeolite membrane 2 / Al 2 O 3 To determine the molar ratio, scanning electron microscope-energy dispersive X-ray spectroscopy (SEM-EDX) measurement was performed under the following conditions, and SiO 2 / Al 2 O 3 The average molar ratio was calculated. Apparatus name (SEM): JSM-7900F (manufactured by JEOL Ltd.) Acceleration voltage: 6 kV Detector: secondary electron detector Apparatus name (EDS): Ultim Max 170 (manufactured by Oxford Co.) Acceleration voltage: 6 kV Magnification: 5000x

[0200] (4) Measurement of Membrane Thickness Measurement of the zeolite membrane thickness of the zeolite membrane composite was carried out under the following conditions and by the following procedure.

[0201] A cross section of an arbitrary portion of the zeolite membrane composite was cut out, and the smooth surface prepared using a cross-section polisher was observed under SEM at 2000x magnification. Images of two to six fields of view were then used to measure the arithmetic mean distance from the surface of the zeolite membrane to the surface of the porous support. At low magnification, the tilt of the acquired image was set so that the interface between the porous support and the zeolite membrane was visually horizontal. The arithmetic mean of the lengths of perpendicular lines drawn from the zeolite membrane surface toward the porous support at 1-μm intervals was calculated to determine the membrane thickness. The end of the perpendicular line was designated as the point where the particles of the porous support first appeared on the perpendicular line extending from the surface of the porous support toward the interior of the support. To clarify the interface between the porous support and the zeolite membrane, secondary electron images and EDX images were superimposed and displayed, and then used to calculate the membrane thickness.

[0202] The measurement conditions were as follows: Apparatus: SEM: JSM-7900F (manufactured by JEOL Ltd.) EDX: ULTim MAX (manufactured by Oxford Co.) Acceleration voltage: 6 kV Image generation analysis software: AZtec Live (manufactured by Oxford Co.) Image processing software: ImageJ

[0203] (5) Air permeability Under atmospheric pressure, one end of the membrane composite was sealed, and the other end was connected to a vacuum line of 5 kPa while maintaining airtightness. Then, the flow rate of air permeating the membrane composite was measured using a mass flow meter installed between the vacuum line and the zeolite membrane composite, and the air permeability [L / (m 2 ・h)] was obtained.

[0204] The mass flow meter is KOFLOC 8300, N 2 A gas-use, maximum flow rate of 500 ml / min (20°C, 1 atmospheric pressure equivalent) was used. When the mass flow meter reading of the KOFLOC 8300 was 10 ml / min (20°C, 1 atmospheric pressure equivalent) or less, the air permeation rate was measured using a Lintec MM-2100M for air gas, maximum flow rate of 20 ml / min (0°C, 1 atmospheric pressure equivalent).

[0205] (6) Water Vapor Adsorption Isotherm The water vapor adsorption isotherm at 35° C. was measured using an adsorption isotherm measuring device (Bellsorp 18, manufactured by Nippon Bell Co., Ltd.).

[0206] The zeolite membrane composite was cut into a suitable size to fit into the measurement cell, and then heated and dried at 120°C for 5 hours while evacuating to a vacuum before use. The measurement was performed under the following conditions: air thermostat temperature 50°C, adsorption temperature 35°C, initial introduction pressure 3 torr (4.00 x 10 2 Pa), saturated vapor pressure 42.181 torr (56.237×10 2 The test was carried out under the conditions of 500 Pa and equilibration time of 500 seconds.

[0207] From the measurement results obtained, the amount of water adsorbed (g) per 1 g of the membrane composite at relative pressures of 0.8 and 0.2 was determined.

[0208] (7) Single-component gas permeation test Single-component gas permeation tests were carried out as follows using the apparatus shown schematically in Fig. 3. The sample gases used were carbon dioxide (purity 99.9%, manufactured by Koatsu Gas Kogyo Co., Ltd.), methane (purity 99.999%, manufactured by Japan Fine Products Co., Ltd.), hydrogen (purity 99.99% or higher, manufactured by Keiyo Hydrogen Co., Ltd.), nitrogen (purity 99.99%, manufactured by Toho Oxygen Industry Co., Ltd.), and helium (purity 99.99%, manufactured by Japan Helium Center Co., Ltd.).

[0209] In Fig. 3, a cylindrical zeolite membrane composite (membrane composite) 31 is placed in a thermostatic chamber (not shown) while being housed in a stainless steel pressure vessel 32. The thermostatic chamber is equipped with a temperature control device so that the temperature of the sample gas can be adjusted.

[0210] The membrane composite 31 is the membrane composite in this embodiment described above. One end of the membrane composite 31 is sealed with a cylindrical end pin 33. The other end is connected by a connection part 34, and the other end of the connection part 34 is connected to the pressure-resistant vessel 32. The inside of the membrane composite 31 is connected to a pipe (permeation gas discharge pipe) 38 for discharging a permeation gas 37 via the connection part 34, and the pipe 38 extends to the outside of the pressure-resistant vessel 32. A pressure gauge 35 for measuring the pressure on the supply side of the sample gas is connected to any point leading to the pressure-resistant vessel 32. Each connection part is airtight.

[0211] In the apparatus of FIG. 3 , when a single-component gas permeation test is performed, a sample gas (supply gas 36) is supplied at a constant pressure between the pressure vessel 32 and the membrane composite 31, and a permeated gas 37 that has permeated the membrane composite 31 is measured by a flow meter (not shown) connected to a pipe 38.

[0212] More specifically, in order to remove components such as moisture or air, the sample is dried at a temperature equal to or higher than the measurement temperature, and then purged with exhaust or the supply gas to be used. After the sample temperature and the differential pressure between the supply gas 36 side and the permeated gas 37 side of the zeolite membrane composite 1 are kept constant, the flow rate of the sample gas (permeated gas 37) that has permeated the membrane composite 31 is measured, and the gas permeance [mol (m 2 ・s・Pa) -1 The pressure used to calculate the permeance is the pressure difference (differential pressure) between the supply side and the permeation side of the feed gas.

[0213] Based on the above measurement results, the ideal separation factor α is calculated by the following formula (3): In formula (3), Q1 and Q2 are the permeation amounts [mol (m 2 ・s) -1 ], and P1 and P2 represent the pressure difference [Pa] between the supply side and the permeation side of the high-permeability gas and the low-permeability gas, respectively. α = (Q1 / Q2) / (P1 / P2) (3)

[0214] The ideal separation factor α indicates the ratio of the permeance of a gas with high permeability to that of a gas with low permeability, and can therefore be determined from the ratio of the permeances of the gases calculated.

[0215] (8) Index of Defect Amount The product of the permeation amount (permeance) of methane gas and the thickness of the zeolite membrane was used as an index of the defect amount.

[0216] The evaluation results in the following examples are summarized in Tables 1 and 2. [Example 1] [Preparation of reaction mixture] A solution of 189.5 g of a 1 mol / L NaOH aqueous solution, 170.1 g of a 25 wt % KOH aqueous solution, and 14,709 g of water was mixed, and aluminum hydroxide (Al 2 O 325.6 g of 53.9% by mass of PEG-400 (manufactured by Kyowa Chemical Industry Co., Ltd.) was added and dissolved with stirring to prepare a clear solution.

[0217] To the obtained transparent solution, 401.7 g of an aqueous solution of N,N,N-trimethyl-1-adamantanammonium hydroxide (hereinafter referred to as "TMADAOH") (containing 20% ​​by mass of TMADAOH, manufactured by Seichem Co., Ltd.) was added as an organic template, and 1421.1 g of colloidal silica (manufactured by Nissan Chemical Industries, Ltd., Snowtex-40) was further added and stirred for 2 hours. In this way, an aqueous reaction mixture was obtained. The composition (molar ratio) of this reaction mixture was: SiO 2 / Al 2 O 3 / NaOH / KOH / H 2 O / TMADAOH=1 / 0.014 / 0.02 / 0.08 / 95 / 0.04, and SiO 2 / Al 2 O 3 =70.

[0218] [Preparation of Inorganic Porous Support] A porous alumina tube (outer diameter 12 mm, inner diameter 9 mm, length 1002 mm) was washed by passing water through it and then dried to obtain an inorganic porous support.

[0219] [Preparation of seed crystals] SiO 2 / Al 2 O 3 / NaOH / KOH / H 2 Hydrothermal synthesis was carried out at 160°C for 2 days using a gel composition (molar ratio) of 0.017 / 0.12 / 0.055 / 20 / 0.07. The resulting precipitate was filtered, washed with water, and dried. CHA-type zeolite particles were thus obtained and used as seed crystals. The particle size of the seed crystals was approximately 1 μm.

[0220] [Production of Zeolite Membrane] The seed crystals were dispersed in water. The support was immersed in the resulting dispersion for a predetermined time, and then dried at 120°C for 2 hours or more to adhere the seed crystals. The increase in mass after drying relative to the mass of the support was determined, and the amount of adhered seed crystals was calculated from the surface area of ​​the support in contact with the dispersion. The amount of adhered seed crystals was 1 g / m 2 It was.

[0221] The support with the seed crystals attached was placed in a PFA inner cylinder (1200 mm long) inside the autoclave, and the reaction mixture was placed in the inner cylinder to immerse the support. The autoclave was then sealed and heated at 180°C for 18 hours in a static state under autogenous pressure. After a predetermined time had passed, the support was allowed to cool, removed from the reaction mixture, washed, and dried at 120°C for at least 2 hours. The support was then fired in air in an electric furnace at 500°C for 5 hours. The heating and cooling rates were both 0.5°C / min. In this way, a membrane composite 1 was obtained in which a zeolite membrane of CHA-type zeolite was formed on the outer surface of the support.

[0222] The mass of the CHA-type zeolite crystallized on the support was calculated from the difference between the mass of the membrane composite 1 and the mass of the support. The mass of the CHA-type zeolite in the membrane composite 1 was 32 g / m 2 It was.

[0223] [Measurement Results] From the XRD measurement of the membrane composite 1, it was confirmed that CHA-type zeolite was produced. In the XRD, the ratio p2 / p1 of the integrated intensity p2 of the peak near 2θ=17.9° to the integrated intensity p1 of the peak near 2θ=20.8° was 0.4. In addition, the ratio p3 / p1 of the integrated intensity p3 of the peak near 2θ=9.6° to the integrated intensity p1 of the peak near 2θ=20.8° was 5.4.

[0224] The X-ray diffraction pattern of membrane composite 1 in GIXD is shown in Figure 4. The incident angle of the X-rays relative to the surface incident angle was 0.5°. The ratio p3 / p1 of the integrated intensity p3 of the peak near 2θ = 9.6° to the integrated intensity p1 of the peak near 2θ = 20.8° in GIXD was 7.8. Furthermore, the ratio p3 / p4 of the integrated intensity p3 of the peak near 2θ = 9.6° to the integrated intensity p4 of the peak near 2θ = 16.2° in GIXD was 14.1.

[0225] In the single-component gas permeation test, as a pretreatment, carbon dioxide was introduced between the pressure vessel 2 and the membrane composite 1 at 140°C to maintain the pressure (external pressure of the membrane composite 1) at approximately 0.16 MPa, and the inside of the cylinder of the membrane composite 1 (internal pressure of the membrane composite 1) was set to 0.10 MPa (atmospheric pressure), and the membrane composite was dried for approximately 70 minutes. Next, the external pressure of the membrane composite 1 was set to 0.2 MPa. At this time, the pressure difference between the external and internal pressures of the membrane composite 1 was 0.1 MPa. Next, the temperature was set to 50°C, and after the temperature stabilized, the supply gas 7 was changed to the gas to be measured, and the gas permeation amount was measured. During the measurement, the pressure difference between the external and internal pressures of the membrane composite 1 was 0.1 MPa.

[0226] The SAR of the surface area of ​​the zeolite membrane of membrane composite 1 was 46. The average thickness of the zeolite membrane of membrane composite 1 was 2.8 μm.

[0227] The gas permeation amount of the membrane composite 1 in the single component gas permeation test was 1.58 × 10 for carbon dioxide at 50 °C. -6 [mol (m 2 ・s・Pa) -1 ] and 9.97 × 10 for methane. -9 [mol (m 2 ・s・Pa) -1 ] and 5.39 × 10 for hydrogen. -7 [mol (m 2 ・s・Pa) -1 ] and 9.66 × 10 for nitrogen. -8 [mol (m 2 ・s・Pa) -1 ] and 1.92 × 10 for helium. -7 [mol (m 2 ・s・Pa) -1 The gas permeation amount of the membrane composite 1 at 140°C was 5.68 × 10 for carbon dioxide. -7 [mol (m 2 ・s・Pa) -1 Furthermore, the ideal separation factor α between carbon dioxide and methane at 50°C was 159. The defect index was 2.8 × 10 -8 It was.

[0228] [Example 2] [Preparation of reaction mixture] A solution of 681.5 g of 1 mol / L NaOH aqueous solution, 294.7 g of 25 wt % KOH aqueous solution, and 13,000 g of water was mixed, and aluminum hydroxide (Al 2 O 3 To the mixture was added 104.96 g of a 53.9% by mass content cellulose acetate, manufactured by Kyowa Chemical Industry Co., Ltd., and the mixture was stirred and dissolved to prepare a transparent solution.

[0229] To the obtained transparent solution, 406.2 g of an aqueous solution of N,N,N-trimethyl-1-adamantanammonium hydroxide (hereinafter referred to as "TMADAOH") (containing 20% ​​by mass of TMADAOH, manufactured by Seichem Co., Ltd.) was added as an organic template, and 1745.8 g of colloidal silica (manufactured by Nissan Chemical Industries, Ltd., Snowtex-S) was further added and stirred for 2 hours. In this way, an aqueous reaction mixture was obtained. The composition (molar ratio) of this reaction mixture was SiO 2 / Al 2 O 3 / NaOH / KOH / H 2 O / TMADAOH=1 / 0.064 / 0.02 / 0.08 / 95 / 0.04, and SiO 2 / Al 2 O 3 = 15.7.

[0230] [Preparation of seed crystals] SiO 2 / Al 2 O 3 / NaOH / KOH / H 2 Hydrothermal synthesis was carried out at 160°C for 2 days using a gel composition (molar ratio) of 0.017 / 0.12 / 0.055 / 20 / 0.07. The resulting precipitate was filtered, washed with water, and dried. CHA-type zeolite particles were thus obtained and used as seed crystals. The particle size of the seed crystals was approximately 1 μm.

[0231] [Production of Zeolite Membrane] The seed crystals were dispersed in water. The support was immersed in the resulting dispersion for a predetermined time, and then dried at 120°C for 2 hours or more to adhere the seed crystals. The increase in mass after drying relative to the mass of the support was determined, and the amount of adhered seed crystals was calculated from the surface area of ​​the support in contact with the dispersion. The amount of adhered seed crystals was 0.67 g / m 2 It was.

[0232] The support with the seed crystals attached was placed in a PFA inner cylinder (1200 mm long) inside the autoclave, and the reaction mixture was placed in the inner cylinder to immerse the support. The autoclave was then sealed and heated at 180°C for 18 hours in a static state under autogenous pressure. After a predetermined time had passed, the support was allowed to cool, removed from the reaction mixture, washed, and dried at 120°C for at least 2 hours. The support was then calcined in air in an electric furnace at 500°C for 10 hours. The temperature increase and decrease rates were both 0.5°C / min. In this way, a membrane composite 1 was obtained in which a zeolite membrane of CHA-type zeolite was formed on the outer surface of the support.

[0233] The mass of the CHA-type zeolite crystallized on the support was calculated from the difference between the mass of the membrane composite 2 and the mass of the support. The mass of the CHA-type zeolite in the membrane composite 2 was 82 g / m 2 It was.

[0234] [Measurement Results] From the XRD measurement of the membrane composite 2, it was confirmed that CHA-type zeolite was produced. In the XRD, the ratio p2 / p1 of the integrated intensity p2 of the peak near 2θ = 17.9 ° to the integrated intensity p1 of the peak near 2θ = 20.8 ° was 0.50. In addition, the ratio p3 / p1 of the integrated intensity p3 of the peak near 2θ = 9.6 ° to the integrated intensity p1 of the peak near 2θ = 20.8 ° in the XRD was 2.84. In the XRD, the ratio p2 / p1 of the peak intensity p2 of the peak near 2θ = 17.9 ° to the peak intensity p1 of the peak near 2θ = 20.8 ° was 0.65. In addition, the ratio p3 / p1 of the peak intensity p3 of the peak near 2θ = 9.6 ° to the peak intensity p1 of the peak near 2θ = 20.8 ° in the XRD was 1.52.

[0235] The incidence angle of the X-rays relative to the surface incidence angle was 0.5°. The ratio p3 / p1 of the integrated intensity p3 of the peak near 2θ = 9.6° to the integrated intensity p1 of the peak near 2θ = 20.8° in GIXD was 32.7. The ratio p3 / p4 of the integrated intensity p3 of the peak near 2θ = 9.6° to the integrated intensity p4 of the peak near 2θ = 16.2° in GIXD was 51.0. The ratio p3 / p1 of the peak intensity p3 of the peak near 2θ = 9.6° to the peak intensity p1 of the peak near 2θ = 20.8° in GIXD was 32.7. The ratio p3 / p4 of the peak intensity p3 of the peak near 2θ = 9.6° to the peak intensity p4 of the peak near 2θ = 16.2° in GIXD was 51.0.

[0236] In the single-component gas permeation test, as a pretreatment, carbon dioxide was introduced between the pressure vessel 2 and the membrane composite 2 at 140°C to maintain the pressure (external pressure of the membrane composite 1) at approximately 0.16 MPa, and the inside of the cylinder of the membrane composite 2 (internal pressure of the membrane composite 1) was set to 0.10 MPa (atmospheric pressure), followed by drying for approximately 70 minutes. Next, the external pressure of the membrane composite 2 was set to 0.2 MPa. At this time, the pressure difference between the external and internal pressures of the membrane composite 2 was 0.1 MPa. Next, the temperature was set to 50°C, and after the temperature stabilized, the supply gas 7 was changed to the gas to be measured, and the gas permeation amount was measured. When measuring CF4 and SF6, the external pressure of the membrane composite 2 was set to 0.4 MPa. During the measurement, the pressure difference between the external and internal pressures of the membrane composite 1 was 0.1 MPa.

[0237] The SAR at the surface point of the zeolite membrane of membrane composite 2 was 29. The average thickness of the zeolite membrane of membrane composite 2 was 9.4 μm.

[0238] The gas permeation amount of the membrane composite 2 in the single component gas permeation test was 4.49 × 10 for carbon dioxide at 50 °C. -7 [mol (m 2 ・s・Pa) -1 ] and 2.16 × 10 for methane. -9 [mol (m 2 ・s・Pa) -1 ] and 1.34 × 10 for hydrogen. -7 [mol (m 2 ・s・Pa) -1] and 2.38 × 10 for nitrogen. -8 [mol (m 2 ・s・Pa) -1 ] and 4.81 × 10 for helium. -8 [mol (m 2 ・s・Pa) -1 The gas permeation amount of the membrane composite 2 at 110°C was 2.00 x 10 for carbon dioxide. -7 [mol (m 2 ・s・Pa) -1 Furthermore, the ideal separation factor α between carbon dioxide and methane at 50°C was 208. The defect index was 2.03 × 10 -8 [mol μm (m 2 ・s・Pa) -1 In addition, when the pressure difference between the external pressure and the internal pressure of the membrane composite 2 was set to 0.3 MPa, the gas permeation amount was SF 6 So 1.50 x 10 -11 [mol (m 2 ・s・Pa) -1 ] and CF 4 So 1.50 x 10 -11 [mol (m 2 ・s・Pa) -1 ] was.

[0239] [Example 3] Membrane composite 3 was synthesized using SiO 2 / Al 2 O 3 The procedure was the same as in Example 1, except that the solubility of the seed crystals was 130. The weight of the seed crystals attached to the support was 1.2 g.

[0240] [Measurement Results] From the XRD measurement of the membrane composite 3, it was confirmed that CHA-type zeolite was produced. In the XRD, the ratio p2 / p1 of the integrated intensity p2 of the peak near 2θ = 17.9 ° to the integrated intensity p1 of the peak near 2θ = 20.8 ° was 0.41. In addition, the ratio p3 / p1 of the integrated intensity p3 of the peak near 2θ = 9.6 ° to the integrated intensity p1 of the peak near 2θ = 20.8 ° in the XRD was 6.08. In the XRD, the ratio p2 / p1 of the peak intensity p2 of the peak near 2θ = 17.9 ° to the peak intensity p1 of the peak near 2θ = 20.8 ° in the XRD was 0.47. In addition, the ratio p3 / p1 of the peak intensity p3 of the peak near 2θ = 9.6 ° to the peak intensity p1 of the peak near 2θ = 20.8 ° in the XRD was 3.56.

[0241] The incidence angle of the X-rays relative to the surface incidence angle was 0.3°. The ratio p3 / p1 of the integrated intensity p3 of the peak near 2θ=9.6° to the integrated intensity p1 of the peak near 2θ=20.8° in GIXD was 11.5. Furthermore, the ratio p3 / p4 of the integrated intensity p3 of the peak near 2θ=9.6° to the integrated intensity p4 of the peak near 2θ=16.2° in GIXD was 15.0.

[0242] In the single-component gas permeation test, as a pretreatment, carbon dioxide was introduced between the pressure vessel 2 and the membrane composite 3 at 140°C to maintain the pressure (external pressure of the membrane composite 1) at approximately 0.16 MPa, and the inside of the cylinder of the membrane composite 3 (internal pressure of the membrane composite 1) was set to 0.101 MPa (atmospheric pressure), and the membrane composite was dried for approximately 70 minutes. Next, the external pressure of the membrane composite 2 was set to 0.2 MPa. At this time, the pressure difference between the external and internal pressures of the membrane composite 2 was 0.1 MPa. Next, the temperature was set to 50°C, and after the temperature stabilized, the supply gas 7 was changed to the gas to be measured, and the gas permeation amount was measured. During the measurement, the pressure difference between the external and internal pressures of the membrane composite 1 was 0.1 MPa.

[0243] The SAR at the surface point of the zeolite membrane of membrane composite 3 was 52. The average thickness of the zeolite membrane of membrane composite 3 was 3.0 μm.

[0244] The gas permeation amount of the membrane composite 3 in the single component gas permeation test was 2.22 × 10 for carbon dioxide at 50 °C.-6 [mol (m 2 ・s・Pa) -1 ] and 2.37 × 10 for methane. -8 [mol (m 2 ・s・Pa) -1 ] and 8.25 × 10 for hydrogen. -7 [mol (m 2 ・s・Pa) -1 ] and 1.30 × 10 for nitrogen. -7 [mol (m 2 ・s・Pa) -1 ] and 2.95 × 10 for helium. -7 [mol (m 2 ・s・Pa) -1 ] and SF 6 So 8.15 x 10 -9 [mol (m 2 ・s・Pa) -1 ] and CF 4 So 9.23 x 10 -9 [mol (m 2 ・s・Pa) -1 Furthermore, the ideal separation factor α between carbon dioxide and methane at 50°C was 94. The defect index was 7.12 × 10 -8 [mol μm (m 2 ・s・Pa) -1 ] was.

[0245] Example 4 Membrane composite 4 was obtained in the same manner as in Example 1, except that a pressure treatment was performed after obtaining a membrane composite in the same manner as in Example 1. The pressure treatment involved using demineralized water as the solvent, applying a water pressure of 10 MPaG to the outside of the membrane for several seconds, and then releasing the water. This operation was repeated 30 times. Specifically, the membrane was placed in a water-sealed module, and water was supplied using a hydraulic pump (T-100K, manufactured by Kyowa Corporation) to apply pressure. One end of the zeolite membrane composite was sealed with a plug, and the other end was sealed with a top insert with a hole. The interior of the zeolite membrane composite was designed to communicate with the outside of the autoclave through the hole in the top insert (leak), and the inside of the support was maintained at atmospheric pressure during pressurization.

[0246] The mass of the CHA-type zeolite crystallized on the support was calculated from the difference between the mass of the membrane composite 4 and the mass of the support. The mass of the CHA-type zeolite in the membrane composite 4 was 32.2 g / m 2 It was.

[0247] [Measurement Results] From the XRD measurement of the membrane composite 4, it was confirmed that CHA-type zeolite was produced. In the XRD, the ratio p2 / p1 of the integrated intensity p2 of the peak near 2θ=17.9° to the integrated intensity p1 of the peak near 2θ=20.8° was 0.50. In addition, the ratio p3 / p1 of the integrated intensity p3 of the peak near 2θ=9.6° to the integrated intensity p1 of the peak near 2θ=20.8° was 6.35.

[0248] The X-ray diffraction pattern of membrane composite 4 measured by GIXD is shown in Figure 4. The incident angle of the X-rays relative to the surface incident angle was 0.5°. The ratio p3 / p1 of the integrated intensity p3 of the peak near 2θ = 9.6° to the integrated intensity p1 of the peak near 2θ = 20.8° in GIXD was 45.94. Furthermore, the ratio p3 / p4 of the integrated intensity p3 of the peak near 2θ = 9.6° to the integrated intensity p4 of the peak near 2θ = 16.2° in GIXD was 1.15.

[0249] In the single-component gas permeation test, as a pretreatment, carbon dioxide was introduced between the pressure vessel 2 and the membrane composite 1 at 140°C to maintain the pressure (external pressure of the membrane composite 1) at approximately 0.16 MPa, and the inside of the cylinder of the membrane composite 1 (internal pressure of the membrane composite 1) was set to 0.10 MPa (atmospheric pressure), followed by drying for approximately 70 minutes. Next, the external pressure of the membrane composite 1 was set to 0.2 MPa. At this time, the pressure difference between the external and internal pressures of the membrane composite 4 was 0.1 MPa. Next, the temperature was set to 50°C, and after the temperature stabilized, the supply gas 7 was changed to the gas to be measured, and the gas permeation amount was measured. During the measurement, the pressure difference between the external and internal pressures of the membrane composite 1 was 0.1 MPa.

[0250] The SAR at the surface point of the zeolite membrane of membrane composite 4 was 54. The average thickness of the zeolite membrane of membrane composite 4 was 2.5 μm.

[0251] The gas permeation amount of the membrane composite 4 in the single component gas permeation test was 1.44 × 10 for carbon dioxide at 50°C.-6 [mol (m 2 ・s・Pa) -1 ] and 6.87 × 10 for methane. -9 [mol (m 2 ・s・Pa) -1 ] and 5.05 × 10 for hydrogen. -7 [mol (m 2 ・s・Pa) -1 ] and 8.18 × 10 for nitrogen. -8 [mol (m 2 ・s・Pa) -1 ] and 1.76 × 10 for helium. -7 [mol (m 2 ・s・Pa) -1 ] and SF 6 So 1.59 x 10 -9 [mol (m 2 ・s・Pa) -1 ] and CF 4 So 2.28 x 10 -9 [mol (m 2 ・s・Pa) -1 The ideal separation factor α between carbon dioxide and methane at 50°C was 210. The defect index was 1.72 × 10 -8 It was.

[0252] Comparative Example 1 In preparing the reaction mixture, a 1 mol / L aqueous KOH solution was used as the aqueous KOH solution, and aluminum hydroxide (Al 2 O 3 The amount of SiO2 (containing 53.5% by mass of SiO2, manufactured by Aldrich) added was 0.152 g, and the composition (molar ratio) of the reaction mixture was SiO2 2 / Al 2 O 3 / NaOH / KOH / H 2 O / TMADAOH = 1 / 0.01 / 0.15 / 0.1 / 100 / 0.04, and SiO 2 / Al 2 O 3 A membrane composite C1 was produced in the same manner as in Example 1, except that the seed crystal adhesion amount in the production of the membrane composite C1 was 9.9 g / m 2 The mass of the CHA-type zeolite in the membrane composite C1 was 122 g / m 2 It was.

[0253] [Measurement Results] From the XRD measurement of the membrane composite C1, it was confirmed that CHA-type zeolite was produced. The peak integrated intensity ratio p2 / p1 in the XRD was 0.3. The peak integrated intensity ratio p3 / p1 in the XRD was 3.1.

[0254] The X-ray diffraction pattern of membrane complex C1 by GIXD is shown in Figure 5. The incident angle of X-rays was 0.4°. The ratio of integrated peak intensities p3 / p1 by GIXD was 2.9. The ratio of integrated peak intensities p3 / p4 by GIXD was 5.7.

[0255] The SAR of the zeolite membrane of the membrane composite C1 was 40.2. The average thickness of the zeolite membrane of the membrane composite C1 was about 8 μm. The air permeability of the membrane composite C1 was 570 L / (m 2 Furthermore, the amount of water adsorption at a relative pressure of 0.8 measured by the water vapor adsorption isotherm of membrane composite C1 was 2.2 times the amount of water adsorption at a relative pressure of 0.2.

[0256] The gas permeation amount of the membrane composite C1 at 50°C is 2.36 x 10 for carbon dioxide. -6 [mol (m 2 ・s・Pa) -1 ] and 3.91 × 10 for methane. -8 [mol (m 2 ・s・Pa) -1 ] and 1.01 × 10 for hydrogen. -6 [mol (m 2 ・s・Pa) -1 ] and 1.81 × 10 for nitrogen. -7 [mol (m 2 ・s・Pa) -1 ] and 4.28 × 10 for helium. -7 [mol (m 2 ・s・Pa) -1 The gas permeation amount of the membrane composite 1 at 140°C was 8.20 × 10 for carbon dioxide. -7 [mol (m 2 ・s・Pa) -1 ] and 7.07 × 10 for methane. -8 [mol (m2 ・s・Pa) -1 ] and 8.93 × 10 for hydrogen. -7 [mol (m 2 ・s・Pa) -1 ] and 1.34 × 10 for nitrogen. -7 [mol (m 2 ・s・Pa) -1 ] and 4.79 × 10 for helium. -7 [mol (m 2 ・s・Pa) -1 Furthermore, the ideal separation factor α between carbon dioxide and methane at 50°C was 60. The defect index was 3.13 × 10 -7 [mol μm (m 2 ・s・Pa) -1 ] was.

[0257] Comparative Example 2 Preparation of reaction mixture 1.24 g of 1 mol / L-NaOH aqueous solution, 4.98 g of 1 mol / L-KOH aqueous solution, aluminum hydroxide (Al 2 O 3 To a mixture of 0.104 g of 53.5% by mass of PEG-400 (manufactured by Aldrich), 114 g of water was added and the mixture was stirred to dissolve, thereby preparing a transparent solution.

[0258] To the obtained transparent solution, 2.44 g of an aqueous TMADAOH solution (containing 25% by mass of TMADAOH, manufactured by Seichem Co., Ltd.) was added as an organic template, and 10.8 g of colloidal silica (Snowtec-40 manufactured by Nissan Chemical Industries, Ltd.) was further added and stirred for 2 hours. In this way, an aqueous reaction mixture was obtained. The composition (molar ratio) of this reaction mixture was: SiO 2 / Al 2 O 3 / NaOH / KOH / H 2 O / TMADAOH=1 / 0.0077 / 0.017 / 0.069 / 100 / 0.04, and SiO 2 / Al 2 O 3 =130.

[0259] [Preparation of Inorganic Porous Support] A porous alumina tube (outer diameter 12 mm, inner diameter 9 mm) was cut to a length of 400 mm, and powder generated during cutting was removed by a compressed air jet to obtain an inorganic porous support.

[0260] [Preparation of seed crystals] SiO 2 / Al 2 O 3 / NaOH / KOH / H 2 CHA-type zeolite particles with a particle size of about 0.5 μm were obtained by hydrothermal synthesis at 160° C. for 2 days using a gel composition of O / TMADAOH=1 / 0.033 / 0.1 / 0.06 / 40 / 0.07. These were used as seed crystals.

[0261] [Zeolite membrane production] The seed crystals were dispersed in demineralized water at a concentration of about 1% by mass, and the support was immersed in the dispersion for a predetermined period of time. The support was then dried at 100°C for 4 hours or more to allow the seed crystals to adhere. The amount of attached seed crystals was 1.4 g / m 2 It was.

[0262] In the same manner as in Example 1, the support to which the seed crystals were attached was immersed in the reaction mixture in the autoclave, heated at 160°C for 48 hours under autogenous pressure, washed, dried, and calcined to obtain membrane composite C2. The mass of the CHA-type zeolite in membrane composite C2 was 46 g / m 2 It was.

[0263] [Measurement Results] From the XRD measurement of the membrane composite C2, it was confirmed that CHA-type zeolite was produced. The peak integrated intensity ratio p2 / p1 in the XRD was 0.3. The peak integrated intensity ratio p3 / p1 in the XRD was 3.3.

[0264] The X-ray diffraction pattern of membrane complex C2 by GIXD is shown in Figure 6. The incident angle of X-rays was 0.1°. The ratio of the integrated peak intensities p3 / p1 by GIXD was 5.7. The ratio of the integrated peak intensities p3 / p4 by GIXD was 5.8.

[0265] The air permeability of the membrane composite C2 was 315 L / (m 2 Furthermore, the amount of water adsorption at a relative pressure of 0.8 measured by the water vapor adsorption isotherm of membrane composite C2 was 2.3 times the amount of water adsorption at a relative pressure of 0.2.

[0266] The gas permeation amount of the membrane composite C2 at 50°C was 2.01 x 10 for carbon dioxide.-6 [mol (m 2 ・s・Pa) -1 ] and 1.60 × 10 for methane. -8 [mol (m 2 ・s・Pa) -1 ] and 6.65 × 10 for hydrogen. -7 [mol (m 2 ・s・Pa) -1 ] and 1.13 × 10 for nitrogen. -7 [mol (m 2 ・s・Pa) -1 ] and 2.46 × 10 for helium. -7 [mol (m 2 ・s・Pa) -1 The gas permeation amount of the membrane composite C2 at 140°C was 6.17 × 10 for carbon dioxide. -7 [mol (m 2 ・s・Pa) -1 ] and 1.52 × 10 for methane. -8 [mol (m 2 ・s・Pa) -1 ] and 4.97 × 10 for hydrogen. -7 [mol (m 2 ・s・Pa) -1 ] and 6.18 × 10 for nitrogen. -8 [mol (m 2 ・s・Pa) -1 ] and 2.34 × 10 for helium. -7 [mol (m 2 ・s・Pa) -1 Furthermore, the ideal separation factor α between carbon dioxide and methane at 50°C was 126. The defect index was 4.80 × 10 -7 [mol μm (m 2 ・s・Pa) -1 ] was.

[0267] [Comparative Example 3] [Supporting Step] A porous alumina tube (outer diameter 12 mm, inner diameter 9 mm, average pore size 1.45 μm) was used as the porous support. SiO 2 / Al 2 O 3 / NaOH / KOH / H 2A gel composition of O / N,N,N-trimethyl-1-adamantanammonium hydroxide (TMADAOH) = 1.00 / 0.033 / 0.120 / 0.0550 / 22.317 / 0.07 was prepared using CHA-type zeolite as a seed crystal and SiO 2 CHA-type zeolite seed crystals were used, which were obtained by adding 2% by weight of the zeolite seed crystals to the zeolite solution and crystallizing them by hydrothermal synthesis at 160° C. for 2 days. The average particle size of the zeolite seed crystals was 1.02 μm.

[0268] The porous support was immersed for 3 minutes in a dispersion of 0.5% by mass of zeolite seed crystals dispersed in water, and then dried at 120°C for 2 hours or more to support the zeolite seed crystals on the porous support. The mass of the porous support was measured before and after the support, and the amount of the zeolite seed crystals supported was 1.70 g / m 2 It was.

[0269] [Hydrothermal synthesis step] A 25% aqueous solution of KOH and a 1N aqueous solution of NaOH were added to demineralized water to obtain aluminum hydroxide (Al 2 O 3 53.5% by mass of N,N,N-trimethyl-1-adamantanammonium hydroxide (hereinafter referred to as "TMADAOH") was added and dissolved to obtain a transparent solution. Furthermore, an aqueous solution (containing 20% ​​by mass of TMADAOH, manufactured by Seichem Co., Ltd.) of N,N,N-trimethyl-1-adamantanammonium hydroxide (hereinafter referred to as "TMADAOH") was added as an organic template, and then colloidal silica (Snowtex ST-S, manufactured by Nissan Chemical Industries, Ltd.) was added and stirred for 120 minutes or more to obtain an aqueous reaction mixture. The composition (molar ratio) of this aqueous reaction mixture was: SiO 2 / Al 2 O 3 / NaOH / KOH / H 2 O / TMADAOH=1.0 / 0.064 / 0.075 / 0.15 / 100 / 0.044, SiO 2 / Al 2 O 3 = 15.7.

[0270] The support with the attached seed crystals was immersed vertically in a reactor containing the aqueous reaction mixture, the reactor was sealed, and the mixture was heated to 180°C over 5 hours, and then heated at 180°C for 24 hours under autogenous pressure in a stationary state. The ratio of the aqueous reaction mixture to the support was about 2050 g per m of support, and the entire support was in contact with the aqueous reaction mixture. After a predetermined time had passed and the zeolite composite membrane was allowed to cool, it was removed from the aqueous reaction mixture, washed, and dried at 120°C for 2 hours or more. The air permeation flux of the unsintered membrane composite during the production process of membrane composite C3 was 0 mL / (m 2 ・minutes).

[0271] [Removal step] After the hydrothermal synthesis and subsequent cooling, the membrane composite was removed from the inner cylinder, washed, and then dried at 120°C for 5 hours or more. After drying, the membrane composite was fired in an electric furnace at 500°C for 10 hours to remove the organic template remaining in the porous support, thereby obtaining a porous support-zeolite membrane composite C3 of Comparative Example 3. The temperature increase and decrease rates during firing were both 0.5°C / min.

[0272] [Measurement Results] From the XRD measurement of the membrane composite C3, it was confirmed that CHA-type zeolite was produced. The peak integrated intensity ratio p2 / p1 in the XRD was 1.04. The peak integrated intensity ratio p3 / p1 in the XRD was 3.29.

[0273] The incidence angle of X-rays in the GIXD X-ray diffraction of membrane complex C3 was 0.6°. The ratio of the integrated peak intensities p3 / p1 in GIXD was 4.62. The ratio of the integrated peak intensities p3 / p4 in GIXD was 6.57.

[0274] The SAR at the surface point of the zeolite membrane of membrane composite C3 was 21. The average thickness of the zeolite membrane of membrane composite 4 was 17.1 μm.

[0275] The gas permeation amount of the membrane composite C3 at 50°C is 3.62 x 10 for carbon dioxide. -7 [mol (m 2 ・s・Pa) -1 ] and 5.51 × 10 for methane. -9[mol (m 2 ・s・Pa) -1 ] and 7.14 × 10 for hydrogen. -8 [mol (m 2 ・s・Pa) -1 ] and 1.61 × 10 for nitrogen. -7 [mol (m 2 ・s・Pa) -1 ] and 2.70 × 10 for helium. -8 [mol (m 2 ・s・Pa) -1 ] and SF 6 So 8.40 x 10 -10 [mol (m 2 ・s・Pa) -1 ] and CF 4 So 1.10 x 10 -9 [mol (m 2 ・s・Pa) -1 The ideal separation factor α between carbon dioxide and methane at 50°C was 66. The defect index was 9.42 × 10 -8 It was.

[0276] [Discussion] The results of Examples 1 to 4 are shown in Table 1 and Figure 4. The results of Comparative Examples 1 to 3 are shown in Table 2 and Figures 5 and 6.

[0277]

[0278]

[0279] As is clear from Tables 1 and 2, while the ratios p2 / p1 and p3 / p1 in XRD of membrane composites 1 to 4 are comparable to those of membrane composites C1 to C3, the ratios p3 / p1 in GIXD of membrane composites 1 to 4 are clearly higher than those of membrane composites C1 to C3. Furthermore, membrane composites 1 to 4 generally have higher separation performance than membrane composites C1 to C3. Therefore, membrane composites 1 to 4 have more highly oriented zeolite membranes than membrane composites C1 to C3, and as a result, they exhibit higher separation performance. Furthermore, in the relationship between the GIXD integrated intensity ratio p3 / p1 and the defect index, as p3 / p1 increases, the defect index decreases, indicating improved membrane performance.

[0280] The present invention can be utilized in the production of purified components from mixtures of liquids or gases.

[0281] REFERENCE SIGNS LIST 1, 31 Membrane composite 11 Support 11A First surface layer portion 11B Second surface layer portion 11C Interior 12 Zeolite membrane 32 Pressure-resistant vessel 33 End pin 34 Connection portion 35 Pressure gauge 36 Supply gas 37 Permeate gas 38 Piping

Claims

1. A zeolite membrane composite comprising an inorganic porous support and a zeolite membrane formed on the surface thereof, wherein an integrated intensity of a peak near 2θ = 9.6° in an X-ray diffraction pattern obtained when the surface of the zeolite membrane is irradiated with X-rays at the minimum incident angle that transmits through the zeolite membrane is 6.0 times or more greater than the integrated intensity of a peak near 2θ = 20.8°.

2. The zeolite membrane composite according to claim 1, wherein an integrated intensity of a peak near 2θ = 9.6° in an X-ray diffraction pattern obtained by irradiating a surface of the zeolite membrane with X-rays at a minimum incident angle that transmits through the zeolite membrane is 6.0 times or more greater than an integrated intensity of a peak near 2θ = 16.8°.

3. The zeolite membrane composite according to claim 1, wherein an integrated intensity of a peak near 2θ = 17.9° in an X-ray diffraction pattern obtained when a surface of the zeolite membrane is irradiated with X-rays that reach the inorganic porous support is less than 0.5 times the integrated intensity of a peak near 2θ = 20.8°, and an integrated intensity of a peak near 2θ = 9.6° is 2.0 times or more and less than 6.0 times the integrated intensity of a peak near 2θ = 20.8°.

4. SiO of the zeolite membrane 2 / Al 2 O 3 The zeolite composite membrane according to claim 1 , wherein the molar ratio is 6 or more and 500 or less.

5. A method for producing a purified component, comprising contacting a mixture containing a first component having higher permeability through the zeolite membrane of the zeolite membrane composite according to any one of claims 1 to 4 and a second component having lower permeability through the zeolite membrane composite, to obtain either or both of a first purified component which is the first component that has permeated the zeolite membrane and a second purified component which is the second component that has not permeated the zeolite membrane.

Citation Information

Patent Citations

  • Preparation of Molecular Sieves Using a Structure Directing Agent and An N, N, N-Triakyl Benzyl Quaternary Ammonium Cation

    US20080075656A1

  • Zeolite SSZ-13 and its method of preparation

    US4544538A

  • Separation or concentration method of mixture gas containing carbon dioxide

    JP2020196008A

  • Separation member and separation method

    JP2022074397A

  • Zeolite membrane complex

    WO2013125660A1