Sintering paste composition for controlling drying shrinkage

The silver paste composition with carboxylic acid additive addresses drying shrinkage issues in conductive pastes, ensuring stable and reliable sintering by inducing a bottlenecking phenomenon, resulting in improved printability and sintering performance.

WO2024205096A1PCT designated stage expired Publication Date: 2024-10-03EVERTECH ENTERPRISE CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
PCT/KR2024/003377
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-29
Filing Date
2024-03-18
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Conductive pastes with sphere-type metal powder face significant drying shrinkage issues during the drying process, leading to potential product defects such as cracking and poor bonding strength, especially when using binder-free types, which can result in low reliability and uneven printability.

Method used

A silver paste composition incorporating sphere-type silver powder and an organic solvent with carboxylic acid as an acid additive, which induces a bottlenecking phenomenon between particles, reducing drying shrinkage and achieving high sintering shrinkage rates during pressure sintering.

Benefits of technology

The silver paste composition ensures excellent printability and stability during drying, with reduced drying shrinkage and high sintering shrinkage rates, enhancing the reliability and physical properties of the sintered products.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure KR2024003377_03102024_PF_FP_ABST
    Figure KR2024003377_03102024_PF_FP_ABST
Patent Text Reader

Abstract

The present invention relates to a sintering paste composition for controlling drying shrinkage and, more specifically, to a silver paste composition for sinter bonding, comprising: a silver powder; and an organic solvent containing a carboxylic acid as an acid additive. If the silver paste composition for sinter bonding, of the present invention, is used, excellent printability is exhibited, necking between some silver powder particles is induced during drying so as to reduce drying shrinkage, and a high sintering shrinkage is exhibited even during follow-up pressure sintering, and thus the reliability of a product to which same is applied can be improved.
Need to check novelty before this filing date? Find Prior Art

Description

Sintering paste composition for drying shrinkage control

[0001] The present invention relates to a sintering paste composition for controlling drying shrinkage, and more particularly, to a silver paste composition for sintering, comprising silver powder and an organic solvent including a carboxylic acid as an acid additive.

[0002] Recent advancements in the electronic component industry have led to weight reduction, higher capacity, and higher reliability in components. In particular, conductive materials used in semiconductor packaging are undergoing refinement in patterns and line widths. Consequently, the particle size of the filler material in the screen printing process for conductive materials is limited. Large particles used in the printing process, or particle agglomeration, can cause scratches on the surface of the printed material, potentially leading to product defects. Typically, binder-free conductive pastes containing nanomaterials experience partial cracking during the drying process due to cohesion between nanoparticles, and significant volumetric shrinkage (drying shrinkage) occurs during the drying process. Specifically, when only spherical metal powders are used, printability is excellent, but the particle shape results in a large surface area in contact with the solvent, resulting in significant drying shrinkage during the solvent evaporation process. If drying shrinkage is significant, the pressure may not be properly distributed to the dried body during pressure sintering after drying, which may prevent smooth sintering and may result in destruction of the printed body.

[0003] An alternative to reducing cracking and drying shrinkage in binder-free conductive pastes is to use micro-sized or flake-type metal powders in a high-filling ratio of at least 85 wt% of the total weight of the conductive paste. However, the use of micro-sized metal powders has limitations in printing fine patterns. Furthermore, the use of flake-type metal powders can lead to uneven particle distribution on the printing surface, which reduces printability. In addition, the low thixotropy of the paste can cause the paste to stretch due to its elongational rheological properties when the squeegee is raised after printing, which can cause it to smear on non-target areas or the printed pattern. If the paste has poor printability, the printed surface may not be flat and may exhibit tilt, pores, or crafting. These can lead to problems such as low bonding strength and low reliability of the applied product after the sintering process.

[0004] Therefore, there is a need to develop a conductive paste that can secure printability while reducing drying shrinkage by using spherical type metal powder as a metal filler.

[0005] [Prior Art Literature]

[0006] [Patent Document]

[0007] (Patent Document 1) Republic of Korea Patent No. 10-1165426 (registered on July 6, 2012)

[0008] The present inventors have conducted extensive research efforts to develop a conductive paste that can secure printability while reducing drying shrinkage using spherical metal powder as a metal filler. As a result, the present invention was completed by elucidating that when a specific acid additive is added to a conductive paste composition using spherical silver powder as a silver filler, a necking phenomenon is induced between some particles during the drying process, which reduces volume shrinkage, thereby reducing the drying shrinkage rate and enabling a high sintering shrinkage rate to be exhibited during the subsequent pressure sintering process.

[0009] Accordingly, an object of the present invention is to provide a silver paste composition for sintering bonding comprising silver powder and an organic solvent including a carboxylic acid as an acid additive.

[0010] Another object of the present invention is to provide a sintering bonding method using the silver paste composition for sintering bonding described above.

[0011] According to one aspect of the present invention, the present invention provides a silver paste composition for sintering bonding, which comprises silver powder and an organic solvent, wherein the organic solvent comprises a carboxylic acid as an acid additive.

[0012] The present inventors have conducted extensive research efforts to develop a conductive paste that can secure printability while reducing drying shrinkage using spherical metal powder as a metal filler. As a result, it was discovered that when a specific acid additive is added to a conductive paste composition using spherical silver powder as a silver filler, a necking phenomenon is induced between some silver powder particles during the drying process, which reduces volume shrinkage, thereby reducing drying shrinkage and enabling a high sintering shrinkage rate to be exhibited during the subsequent pressure sintering process.

[0013] In this specification, the term 'sintering' refers to a phenomenon in which powders that have been pressurized into an appropriate shape are heated to firmly adhere to each other and solidify, and 'sintering bonding' refers to bonding using sintering. The most representative method for replacing the existing solder alloy as a chip bonding material for power semiconductor modules is the sintering technology using silver (Ag) and copper (Cu) paste. Silver sintering technology is a bonding method using nano- or micro-sized particles, and has excellent high-temperature stability, thermal / electrical conductivity, and long-term reliability. Sintering methods include normal sintering, pressure sintering, reaction sintering, and isostatic sintering, and in a specific embodiment of the present invention, the silver paste composition for sintering bonding of the present invention is used for pressure sintering, but is not limited thereto.

[0014] In this specification, the term 'silver paste' means a conductive paste in which silver powder is used as a filler.

[0015] In one embodiment of the present invention, the silver powder may include spherical silver powder. Unlike flake-type silver powder, which has low printability but low porosity, thus high reliability, and excellent thermal properties and bonding strength, spherical silver powder is known to have excellent printability but may cause cracks during the drying process and have high porosity after sintering, which may reduce reliability. The inventors of the present invention have found that when a specific acid additive is added to a conductive paste composition using spherical silver powder as a silver filler, a necking phenomenon is induced between some particles during the drying process, thereby reducing drying shrinkage, and exhibiting high sintering shrinkage and low porosity during the subsequent pressure sintering process. Therefore, the silver paste composition for sintering bonding of the present invention not only has excellent printability, but is also stable during the drying process and has excellent physical properties after sintering, so that it can be used in a wide range of applications.

[0016] The silver powder used in the present invention is a sintered powder containing fine particles of 1 μm or less, and may be a sintered powder containing a metal in which some of the particles forming the fine particles are partially coated with a capping agent. The 'capping agent' can reduce the agglomeration of the metal particles and prevent an increase in the sintering temperature of the sintered powder.

[0017] In one embodiment of the present invention, the average particle size (D) of the silver powder described above 50) may be 10 nm to 1000 nm, and more specifically, 10 nm to 1000 nm, 10 nm to 800 nm, 10 nm to 600 nm, 10 nm to 400 nm, 10 nm to 300 nm, 10 nm to 280 nm, 50 nm to 1000 nm, 50 nm to 800 nm, 50 nm to 600 nm, 50 nm to 400 nm, 50 nm to 300 nm, 50 nm to 280 nm, 100 nm to 1000 nm, 100 nm to 800 nm, 100 nm to 600 nm, 100 nm to 400 nm, 100 nm to 300 nm, 100 nm to 280 nm, 150 nm to 1000 nm, 150 nm to 800 nm, 150 nm to 600 nm, 150 nm to 400 nm, 150 nm to 300 nm, 150 nm to 280 nm, 200 nm to 1000 nm, 200 nm to 800 nm, 200 nm to 600 nm, 200 nm to 400 nm, 200 nm to 300 nm, 200 nm to 280 nm, 250 nm to 1000 nm, 250 nm to 800 nm, 250 nm to 600 nm, 250 nm to 400 nm, 250 nm to 300 nm, 250 nm to 280 nm, 260 nm to 1000 nm, 260 nm to 800 nm, 260 nm to 600 nm, It may be, but is not limited to, 260 nm to 400 nm, 260 nm to 300 nm, or 260 nm to 280 nm, more specifically 260 nm to 280 nm.

[0018] In this specification, the term "organic solvent" refers to an organic solvent added to control the fluidity of the silver paste composition of the present invention, and generally refers to all organic solvents that can be used industrially. The viscosity of the paste can be significantly affected depending on the content of the organic solvent.

[0019] In one embodiment of the present invention, the above-mentioned carboxylic acid is a carboxylic acid having an aliphatic chain of 1 to 26 carbon atoms, such as oxalic acid, malonic acid, succinic acid, glutaric acid, adipic acid, 2,2-bis(hydroxymethyl)propionic acid, itaconic acid, diglycolic acid, boric acid, ethylenediaminetetraacetic acid, oleic acid, stearic acid, sebacic acid, salicylic acid, citric acid, dodecanedioic acid, maleic acid, palmitic acid. The acid additive may be, but is not limited to, suberic acid, or a combination thereof. Depending on the amount or type of the acid additive present, the viscosity of the paste composition or the thickness of the dried coating film may vary, and two or three or more carboxylic acids may be combined and added as the acid additive, if necessary.

[0020] In a specific embodiment of the present invention, the carboxylic acid may be, but is not limited to, oxalic acid, malonic acid, succinic acid, glutaric acid, adipic acid, 2,2-bis(hydroxymethyl)propionic acid, itaconic acid, diglycolic acid, boric acid, ethylenediaminetetraacetic acid, or a combination thereof, more specifically, malonic acid; oxalic acid; succinic acid; or a combination of malonic acid and succinic acid.

[0021] In a specific embodiment of the present invention, when the above-described carboxylic acid is a combination of malonic acid and succinic acid, the weight ratio of malonic acid and succinic acid may be 1:0.5 to 1:10, and more specifically, 1:0.5 to 1:10, 1:0.5 to 1:7, 1:0.5 to 1:5, 1:0.5 to 1:3, 1:1 to 1:10, 1:1 to 1:7, 1:1 to 1:5, 1:1 to 1:3, 1:1.5 to 1:10, 1:1.5 to 1:7, 1:1.5 to 1:5, 1:1.5 to 1:3, 1:2 to 1:10, 1:2 to 1:7, 1:2 to 1:5, 1:2 to 1:3, 1:2.5 to It may be, but is not limited to, 1:10, 1:2.5 to 1:7, 1:2.5 to 1:5, or 1:2.5 to 1:3.

[0022] In one embodiment of the present invention, the content of the above-described acid additive may be 0.01 wt% to 10 wt% relative to the entire composition. More specifically, 0.01 wt% to 10 wt%, 0.01 wt% to 7 wt%, 0.01 wt% to 5 wt%, 0.01 wt% to 3 wt%, 0.05 wt% to 10 wt%, 0.05 wt% to 7 wt%, 0.05 wt% to 5 wt%, 0.05 wt% to 3 wt%, 0.1 wt% to 10 wt%, 0.1 wt% to 7 wt%, 0.1 wt% to 5 wt%, 0.1 wt% to 3 wt%, 0.5 wt% to 10 wt%, 0.5 wt% to 7 wt%, 0.5 wt% to 5 wt%, 0.5 wt% to 3 wt%, 1 wt% to 10 wt%, 1 wt% to 7 wt%, 1 wt% to 5 wt%, 1 wt% to It may be, but is not limited to, 3 wt%, 1.5 wt% to 10 wt%, 1.5 wt% to 7 wt%, 1.5 wt% to 5 wt%, or 1.5 wt% to 3 wt%.

[0023] In one embodiment of the present invention, the organic solvent described above may be water, hydrocarbons, alcohols, ethers, esters, acetates, ketones or glycol solvents, such as toluene, benzene, octanol, decanol, terpineol (α-terpineol, β-terpineol, γ-terpineol), terpineol acetate, dihydroterpineol, dihydroterpineol acetate, carbitol, butyl carbitol, cellosolve, butyl cellosolve, butyl carbitol acetate, cellosolve acetate, ethylene glycol diacetate, propylene glycol diacetate, or a mixed solvent thereof, but is not limited thereto.

[0024] In one embodiment of the present invention, the organic solvent described above may be water, alcohol, acetate, or a mixed solvent thereof.

[0025] In one embodiment of the present invention, the organic solvent described above may include an additive. More specifically, the organic solvent described above may additionally include one or more additives selected from the group consisting of a coupling agent, an antioxidant, a curing accelerator, a leveling agent, an antifoaming agent, a filler, a fluidity regulator, and a dispersing agent.

[0026] In this specification, the term 'additive' refers to a substance that can improve the insufficient properties of the paste, and plays a role in improving the workability of the paste and the properties such as conductivity, dispersibility, storage stability, and printability after the drying process. Even a small amount of 1 to 2 wt% of the total composition can have a great effect, but it can also be a factor in reducing conductivity, so the optimal content should be added at a minimum, and the reaction principle of the additive must be known to be able to add an appropriate additive. The types of additives are diverse and subdivided, such as surfactants to improve the printability of the silver paste composition, coupling agents (adhesion accelerators) to improve the adhesion of the silver paste composition to the substrate, antioxidants, curing accelerators, leveling agents, acid additives, defoaming agents, fillers, and dispersants.

[0027] In one embodiment of the present invention, the content of the above-described additive may be 0.05 wt% to 2 wt% based on the total composition, and more specifically, may include 0.05 wt% to 2 wt%, 0.05 wt% to 1 wt%, 0.05 wt% to 0.5 wt%, 0.1 wt% to 2 wt%, 0.1 wt% to 1 wt%, 0.1 wt% to 0.75 wt%, or 0.1 wt% to 0.5 wt%, but is not limited thereto.

[0028] In one embodiment of the present invention, the organic solvent described above may include a dispersant as an additive. The dispersant stabilizes the filler by ensuring that the solid particles in the paste composition are evenly distributed within the liquid medium, thereby improving long-term stability. The dispersant prevents particle agglomeration through various mechanisms, such as electrostatic and steric effects.

[0029] In one embodiment of the present invention, the organic solvent described above may contain a dispersant as an additive in an amount of 0.05 wt% to 2 wt% based on the total silver paste composition. More specifically, the organic solvent described above may contain a dispersant as an additive in an amount of 0.05 wt% to 2 wt%, 0.05 wt% to 1 wt%, 0.05 wt% to 0.5 wt%, 0.05 wt% to 0.3 wt%, 0.1 wt% to 2 wt%, 0.1 wt% to 1 wt%, 0.1 wt% to 0.5 wt%, or 0.1 wt% to 0.3 wt% based on the total silver paste composition, but is not limited thereto. In a specific embodiment of the present invention, the organic solvent described above may contain a dispersant in an amount of 0.2 wt% based on the total silver paste composition, but is not limited thereto.

[0030] In one embodiment of the present invention, the organic solvent described above may include a fluidity regulator as an additive. The fluidity regulator is a substance added to control the viscosity of the paste, and depending on the amount or type of the fluidity regulator present, the viscosity of the paste, the thickness of the coating film after printing and drying using the paste, and the presence or absence of sedimentation may vary. The fluidity regulator may be a modified urea-based, amine-amide-based, amine-based, urea / acrylate-based, or modified ester-based agent, and examples thereof include, but are not limited to, RHEOBYK-425, RHEOBYK-T 1000VF, RHEOBYK-L 1400 VF, RHEOBYK-H 3300 VF from BYK, H1335, HY124 from Spectrum, or a combination thereof.

[0031] In one embodiment of the present invention, the organic solvent described above may contain a dispersant as an additive in an amount of 0.05 wt% to 2 wt% based on the total silver paste composition. More specifically, the organic solvent described above may contain a dispersant as an additive in an amount of 0.05 wt% to 2 wt%, 0.05 wt% to 1 wt%, 0.05 wt% to 0.5 wt%, 0.1 wt% to 2 wt%, 0.1 wt% to 1 wt%, or 0.1 wt% to 0.5 wt% based on the total silver paste composition, but is not limited thereto. In a specific embodiment of the present invention, the organic solvent described above may contain a dispersant in an amount of 0.4 wt% based on the total silver paste composition, but is not limited thereto.

[0032] In one embodiment of the present invention, the weight ratio of the above-described silver powder and organic solvent may be 1:1 to 9:1. When the weight ratio of the organic solvent is less than 10 wt%, the silver powder may not be filled smoothly, making it difficult to manufacture the silver paste composition. On the other hand, when the weight ratio of the organic solvent exceeds 50 wt%, the viscosity may be low, causing the silver paste composition to spread when the metal mask is separated, and the drying time may be long, drying shrinkage may be large, and the thickness may become thin or cracks may occur after drying.

[0033] More specifically, the weight ratio of the silver powder and the organic solvent is 1:1 to 9:1, 1:1 to 85:15, 1:1 to 82.5:17.5, 1:1 to 81:19, 65:35 to 9:1, 65:35 to 85:15, 65:35 to 82.5:17.5, 65:35 to 81:19, 75:15 to 9:1, 75:15 to 85:15, 75:15 to 82.5:17.5, 75:15 to 81:19, 77.5:22.5 to 9:1, 77.5:22.5 to 85:15, 77.5:22.5 to 82.5:17.5, or It can be, but is not limited to, 77.5:22.5 to 81:19.

[0034] In one embodiment of the present invention, the silver paste composition for sintering bonding of the present invention may be binder-free.

[0035] In this specification, the term 'binder-free' means that the silver paste composition does not contain a binder.

[0036] In this specification, the term 'binder' refers to a substance in which a polymer resin is dissolved in a solvent at a certain ratio to improve the fluidity of the paste composition or to allow the paste composition to adhere to a substrate and to control physical properties such as strength and durability. In the case of a typical silver paste composition, one or more types of thermosetting resins or thermoplastic resins such as epoxy resin, phenol resin, saturated polyester resin, unsaturated polyester resin, polyimide resin, polyamide resin, and acrylic resin have been mixed and used as a binder. However, if the binder is well mixed with the metal powder, it may interfere with the contact between the metal particles, thereby reducing the conductivity, and the porosity may increase during sintering, reducing the adhesive strength and thus lowering the reliability of the applied product. In addition, the binder may be decomposed by heat during the sintering process, generating fumes that may contaminate the substrate.

[0037] In the case of silver powder containing silver microparticles or silver nanoparticles, the surface energy is high, so there is a strong tendency to aggregate with each other for stabilization. At this time, the binder plays a role in preventing aggregation between silver powders and ensuring stable dispersion of silver powders. Therefore, in the absence of a binder, aggregation between silver powders may increase. The present inventors have determined the average particle size (D) of spherical silver powders. 50 ), shape (plate or spherical), presence or absence of acid additive in organic solvent, and type of acid additive were tested, and a silver paste composition was developed that has excellent stability during the drying process and physical properties after sintering without agglomeration of silver powder without a binder, and has high usability due to good printability.

[0038] In one embodiment of the present invention, the silver paste composition for sintering bonding of the present invention has reduced drying shrinkage. More specifically, the silver paste composition for sintering bonding has reduced drying shrinkage compared to a case in which an acid additive including a carboxylic acid is not added.

[0039] In this specification, the term "drying shrinkage" refers to a phenomenon that commonly occurs when solvents are removed from solid materials such as metal particles, concrete, and ceramics. Drying shrinkage can be influenced by factors such as particle shape, size, and surface area. The present inventors have discovered that drying shrinkage can be reduced by adjusting the composition of the acid additive in the organic solvent included in a silver paste composition for sintering.

[0040] As demonstrated in the examples described below, the silver paste composition for sintering bonding of the present invention has the effect of reducing drying shrinkage by including a carboxylic acid as an acid additive. This effect is due to the fact that during the drying process of the conductive paste, the decomposition of the acid additive induces a weak necking phenomenon between the metal particles, thereby reducing the contact area between the metal particles.

[0041] In one embodiment of the present invention, the drying shrinkage rate of the silver paste composition for sintering bonding of the present invention after drying may be 0.5% to 30%, and more specifically, 0.5% to 30%, 0.5% to 27%, 0.5% to 25%, 0.5% to 20%, 0.5% to 18%, 1% to 30%, 1% to 27%, 1% to 25%, 1% to 20%, 1% to 18%, 5% to 30%, 5% to 27%, 5% to 25%, 5% to 20%, 5% to 18%, 10% to 30%, 10% to 27%, 10% to 25%, 10% to 20%, 10% to 18%, 15% to It may be, but is not limited to, 30%, 15% to 27%, 15% to 25%, 15% to 20%, 15% to 18%, 17% to 30%, 17% to 27%, 17% to 25%, 17% to 20%, or 17% to 18%.

[0042] In this specification, the term 'drying shrinkage' means the shrinkage when the printed paste dries, and is calculated as follows.

[0043] ceremony

[0044] Drying shrinkage rate (%) = [1-(thickness of silver paste composition after drying (㎛) / thickness of printing mask (㎛))] x 100

[0045] Therefore, the smaller the drying shrinkage rate, the less drying shrinkage occurs, and accordingly, the sintering shrinkage rate in the subsequent sintering bonding can increase, thereby increasing the reliability of the applied product.

[0046] In one embodiment of the present invention, the silver paste composition for sintering bonding of the present invention may have a sintering shrinkage rate of 55% to 75% after pressure sintering, and more specifically, 55% to 75%, 55% to 72%, 55% to 69%, 55% to 67%, 55% to 66%, 55% to 65%, 55% to 64%, 58% to 75%, 58% to 72%, 58% to 69%, 58% to 67%, 58% to 66%, 58% to 65%, 58% to 64%, 61% to 75%, 61% to 72%, 61% to 69%, 61% to 67%, 61% to 66%, 61% to It may be, but is not limited to, 65%, 61% to 64%, 63% to 75%, 63% to 72%, 63% to 69%, 63% to 67%, 63% to 66%, 63% to 65%, or 63% to 64%.

[0047] In this specification, the term 'sintering shrinkage' means the shrinkage when the dried paste is sintered, and is calculated as follows.

[0048] ceremony

[0049] Sintering shrinkage (%) = [1-(thickness after sintering of silver paste composition (㎛) / dry thickness of silver paste composition (㎛)] x 100

[0050] If the sintering shrinkage of the conductive paste is low, the chip may be destroyed or dense bonding may not be achieved, which may result in a decrease in the conductivity or reliability of the applied product.

[0051] In one embodiment of the present invention, the above-described pressure sintering can be performed at a temperature of 150°C to 350°C. More specifically, the above-described pressure sintering may be performed at a temperature of 150°C to 350°C, 150°C to 300°C, 150°C to 280°C, 150°C to 260°C, 200°C to 350°C, 200°C to 300°C, 200°C to 280°C, 200°C to 260°C, 220°C to 350°C, 220°C to 300°C, 220°C to 280°C, 220°C to 260°C, 240°C to 350°C, 240°C to 300°C, 240°C to 280°C, or 240°C to 260°C, and most specifically, may be 250°C, but is not limited thereto.

[0052] In one embodiment of the present invention, the above-described pressure sintering may be performed at a pressure of 0.1 MPa to 20 MPa. More specifically, the above-described pressure sintering may be 0.1 MPa to 20 MPa, 0.1 MPa to 15 MPa, 0.1 MPa to 12 MPa, 0.1 MPa to 10 MPa, 0.2 MPa to 20 MPa, 0.2 MPa to 15 MPa, 0.2 MPa to 12 MPa, 0.2 MPa to 10 MPa, 0.3 MPa to 20 MPa, 0.3 MPa to 15 MPa, 0.3 MPa to 12 MPa, or 0.3 MPa to 10 MPa, and more specifically, may be 0.4 MPa, but is not limited thereto.

[0053] In one embodiment of the present invention, the silver paste composition for sintering bonding of the present invention had a good printing state and no cracks on the surface after printing, as shown in the examples below.

[0054] In one embodiment of the present invention, the silver paste composition for sintering bonding of the present invention, as shown in the examples below, when dried at 130°C for 30 minutes after printing, had a large dry thickness, so that stability was maintained when pressure was applied during the bonding process, and a decrease in reliability due to an increase in internal porosity was prevented.

[0055] In one embodiment of the present invention, the silver paste composition for sintering bonding of the present invention, as shown in the examples below, when dried at 130°C for 30 minutes after printing and then subjected to pressure sintering at 250°C for 180 seconds without a heating section at a pressure of 0.4 MPa, had a sintering shrinkage ratio of 60% or more, which prevented chip breakage and improved reliability.

[0056] Therefore, the silver paste composition for sintering bonding of the present invention can be usefully used for bonding in the production of electronic products such as automobile electrical components, IT devices, and home appliances, and specifically, can be applied in the production of electronic control devices (power modules, thermoelectric modules), chip components, piezoelectric components of electronic ceramics, membranes of flexible circuits, RFID tags, touch screens, and the like.

[0057] According to another aspect of the present invention, the present invention provides a sintering bonding method using the silver paste composition for sintering bonding described above, comprising the steps of (a) forming a silver paste layer by printing or dispensing the silver paste composition for sintering bonding on a first bonding member; and (b) placing a second bonding member on the silver paste layer and performing sintering bonding.

[0058] In one embodiment of the present invention, the first bonded body may be a direct bonded copper (DBC) substrate (such as a silver-coated (Ag coated) DBC substrate), a silver-coated lead frame, a substrate or interposer made of other materials such as silicon, and the second bonded body may be, but is not limited to, a high-heat element such as an IGBT, a silicon carbide chip, or a silicon chip (Si chip).

[0059] In one embodiment of the present invention, the method of forming a silver paste layer by printing or dispensing the silver paste composition for sintering bonding of step (a) onto the first bonded body may be selected from various known coating methods or printing methods. More specifically, inkjet, stencil, tape caster, gravure and offset printing, and screen printing may be selected as the printing method, and more specifically, screen printing may be used, but is not limited thereto.

[0060] In one embodiment of the present invention, the method of forming a silver paste layer by printing or dispensing the silver paste composition for sintering bonding of step (a) onto the first bonded body is a screen printing method, and the printing speed may be 5 mm / s to 500 mm / s, and the pressure of the squeegee may be 0.01 MPa to 5 MPa.

[0061] In a specific embodiment of the present invention, the printing speed is 5 mm / s to 500 mm / s, 5 mm / s to 400 mm / s, 5 mm / s to 300 mm / s, 5 mm / s to 200 mm / s, 5 mm / s to 150 mm / s, 5 mm / s to 100 mm / s, 5 mm / s to 80 mm / s, 5 mm / s to 60 mm / s, 5 mm / s to 50 mm / s, 10 mm / s to 500 mm / s, 10 mm / s to 400 mm / s, 10 mm / s to 300 mm / s, 10 mm / s to 200 mm / s, 10 mm / s to 150 mm / s, 10 mm / s to 100 mm / s, 10 mm / s to 80 mm / s, 10 mm / s to 60 mm / s, 10 mm / s to 50 mm / s, 20 mm / s to 500 mm / s, 20 mm / s to 400 mm / s, 20 mm / s to 300 mm / s, 20 mm / s to 200 mm / s, 20 mm / s to 150 mm / s, 20 mm / s to 100 mm / s, 20 mm / s to 80 mm / s, 20 mm / s to 60 mm / s, 20 mm / s to 50 mm / s, 30 mm / s to 500 mm / s, 30 mm / s to 400 mm / s, 30 mm / s to 300 mm / s, 30 mm / s to 200 mm / s, 30 mm / s to 150 mm / s, 30 mm / s to 100 mm / s, 30 mm / s to 80 mm / s, 30 mm / s to 60 mm / s, 30 mm / s to 50 mm / s, 40 mm / s to 500 mm / s, 40 mm / s to 400 mm / s, 40 mm / s to 300 mm / s, 40 mm / s to 200 mm / s, 40 mm / s to 150 mm / s, 40 mm / s to 100 mm / s, 40 mm / s to 80 mm / s, 40 mm / s to 60 mm / s, or 40 mm / s to 50 mm / s, most specifically, but not limited to, 50 mm / s.

[0062] In a specific embodiment of the present invention, the pressure of the squeegee is 0.01 MPa to 5 MPa, 0.01 MPa to 5 MPa, 0.01 MPa to 4 MPa, 0.01 MPa to 3 MPa, 0.01 MPa to 2.5 MPa, 0.01 MPa to 2.25 MPa, 0.1 MPa to 5 MPa, 0.1 MPa to 4 MPa, 0.1 MPa to 3 MPa, 0.1 MPa to 2.5 MPa, 0.1 MPa to 2.25 MPa, 0.5 MPa to 5 MPa, 0.5 MPa to 4 MPa, 0.5 MPa to 3 MPa, 0.5 MPa to 2.5 MPa, 0.5 MPa to 2.25 MPa, 1 MPa to 5 MPa, 1 MPa to It may be, but is not limited to, 4 MPa, 1 MPa to 3 MPa, 1 MPa to 2.5 MPa, 1 MPa to 2.25 MPa, 1.5 MPa to 5 MPa, 1.5 MPa to 4 MPa, 1.5 MPa to 3 MPa, 1.5 MPa to 2.5 MPa, 1.5 MPa to 2.25 MPa, 1.75 MPa to 5 MPa, 1.75 MPa to 4 MPa, 1.75 MPa to 3 MPa, 1.75 MPa to 2.5 MPa, or 1.75 MPa to 2.25 MPa.

[0063] In one embodiment of the present invention, the step (a) may additionally include a process of drying the silver paste layer.

[0064] In one embodiment of the present invention, the process of drying the silver paste may be performed at 80°C to 200°C. More specifically, the process of drying the silver paste may be performed at 80°C to 200°C, 80°C to 170°C, 80°C to 140°C, 100°C to 200°C, 100°C to 170°C, 100°C to 140°C, 120°C to 200°C, 120°C to 170°C, or 120°C to 140°C, and most specifically, at 130°C, but is not limited thereto.

[0065] In one embodiment of the present invention, the sintering bonding in step (b) can be achieved by heating.

[0066] In one embodiment of the present invention, the sintering bonding heating temperature in step (b) may be 150°C to 350°C. More specifically, the sintering bonding heating temperature of step (b) may be 150°C to 350°C, 150°C to 300°C, 150°C to 280°C, 150°C to 260°C, 200°C to 350°C, 200°C to 300°C, 200°C to 280°C, 200°C to 260°C, 220°C to 350°C, 220°C to 300°C, 220°C to 280°C, 220°C to 260°C, 240°C to 350°C, 240°C to 300°C, 240°C to 280°C, or 240°C to 260°C, and most specifically, may be 250°C, but is not limited thereto.

[0067] In one embodiment of the present invention, the sintering in step (b) can be performed by applying pressure.

[0068] In one embodiment of the present invention, the sintering bonding pressure in step (b) may be 0.1 MPa to 20 MPa. More specifically, the sintering bonding pressure of the step (b) is 0.1 MPa to 20 MPa, 0.1 MPa to 10 MPa, 0.1 MPa to 5 MPa, 0.1 MPa to 3 MPa, 0.1 MPa to 2 MPa, 0.1 MPa to 1 MPa, 0.1 MPa to 0.5 MPa, 0.2 MPa to 20 MPa, 0.2 MPa to 10 MPa, 0.2 MPa to 5 MPa, 0.2 MPa to 3 MPa, 0.2 MPa to 2 MPa, 0.2 MPa to 1 MPa, 0.2 MPa to 0.5 MPa, 0.3 MPa to 20 MPa, 0.3 MPa to 10 MPa, 0.3 MPa to 5 MPa, 0.3 MPa to 3 MPa, It may be 0.3 MPa to 2 MPa, 0.3 MPa to 1 MPa or 0.3 MPa to 0.5 MPa, most specifically, but not limited to, 0.4 MPa.

[0069] In one embodiment of the present invention, the sintering in step (b) can be performed by heating and pressurizing. More specifically, the sintering bonding heating temperature of step (b) may be 150°C to 350°C, 150°C to 300°C, 150°C to 280°C, 150°C to 260°C, 200°C to 350°C, 200°C to 300°C, 200°C to 280°C, 200°C to 260°C, 220°C to 350°C, 220°C to 300°C, 220°C to 280°C, 220°C to 260°C, 240°C to 350°C, 240°C to 300°C, 240°C to 280°C, or 240°C to 260°C, and most specifically, may be 250°C, but is not limited thereto.

[0070] Since the sintering bonding method of the present invention is a method performed using the silver paste composition for sintering bonding of the present invention described above, description of common contents between the two is omitted to avoid excessive complexity of the present specification.

[0071] The features and advantages of the present invention are summarized as follows:

[0072] (a) The present invention provides a silver paste composition for sintering bonding, which comprises silver powder and an organic solvent, wherein the organic solvent comprises a carboxylic acid as an acid additive.

[0073] (b) The present invention provides a sintering bonding method using the silver paste composition for sintering bonding described above.

[0074] When the silver paste composition for sintering bonding of the present invention is used, not only is the printability excellent, but a necking phenomenon is induced between some silver powder particles during the drying process, thereby reducing drying shrinkage, and a high sintering shrinkage rate is exhibited during the subsequent pressure sintering process, thereby improving the reliability of the applied product.

[0075] Figure 1 shows the surface condition of a dried silver paste composition after printing observed using a digital microscope.

[0076] Figure 2 shows a cross-section of a dried silver paste composition polished, and the thickness and microstructure of the cross-section observed using a digital microscope.

[0077] Figure 3 shows a cross-section of a sintered paste composition that was polished, and the thickness and microstructure of the cross-section were observed using a digital microscope.

[0078] Hereinafter, the present invention will be described in more detail through examples. These examples are intended solely to illustrate the present invention more specifically, and it will be apparent to those skilled in the art that the scope of the present invention is not limited by these examples, in accordance with the gist of the present invention.

[0079] Example

[0080] Throughout this specification, "%" used to indicate the concentration of a particular substance is (weight / weight) % for solid / solid, (weight / volume) % for solid / liquid, and (volume / volume) % for liquid / liquid, unless otherwise stated.

[0081] <Example 1> Preparation of silver paste composition for sintering bonding

[0082] A silver paste composition was prepared by mixing silver filler, organic solvent, and acid additive. The silver filler had an average particle size (D) of 270 nm. 50 ) was used, and was used at a weight ratio of 80 wt% based on the total silver paste composition. The composition of the organic solvent used is shown in Table 1 below. As shown in Table 1, 0.05 wt% of malonic acid and 0.15 wt% of succinic acid were used as acid additives based on the total silver paste composition. The acid additives of Example 1 and the following Examples 2, 3, and Comparative Examples 1 to 11 were all purchased from TCI (Tokyo Chemical Industry) and used.

[0083] [Table 1]

[0084]

[0085] The mixture was stirred at 1,000 rpm for 1 minute using a paste mixer, and three-roll milling was repeated three times to improve dispersibility. Thereafter, the mixture was stirred again at 1,000 rpm for 1 minute using a paste mixer to prepare a conductive silver paste composition.

[0086]

[0087] <Example 2> Preparation of silver paste composition for sintering bonding

[0088] A silver paste composition for sintering was prepared in the same manner as in Example 1, except that 0.2 wt% malonic acid was added instead of the acid additive of Example 1 (0.05 wt% malonic acid and 0.15 wt% succinic acid) as the acid additive.

[0089]

[0090] <Example 3> Preparation of silver paste composition for sintering bonding

[0091] A silver paste composition for sintering was prepared in the same manner as in Example 1, except that 0.2 wt% oxalic acid was added instead of the acid additive (0.05 wt% malonic acid and 0.15 wt% succinic acid) of Example 1 as the acid additive.

[0092]

[0093] <Comparative Example 1> Preparation of silver paste composition for sintering bonding

[0094] A silver paste composition for sintering bonding was prepared in the same manner as in Example 1, except that 0.2 wt% succinic acid was added instead of the acid additive of Example 1 (0.05 wt% malonic acid and 0.15 wt% succinic acid).

[0095]

[0096] <Comparative Example 2> Preparation of silver paste composition for sintering bonding

[0097] A silver paste composition for sintering was prepared in the same manner as in Example 1, except that 0.2 wt% glutaric acid was added instead of the acid additive (0.05 wt% malonic acid and 0.15 wt% succinic acid) of Example 1 as the acid additive.

[0098]

[0099] <Comparative Example 3> Preparation of silver paste composition for sintering bonding

[0100] A silver paste composition for sintering was prepared in the same manner as in Example 1, except that 0.2 wt% of adipic acid was added instead of the acid additive (0.05 wt% of malonic acid and 0.15 wt% of succinic acid) of Example 1 as the acid additive.

[0101]

[0102] <Comparative Example 4> Preparation of silver paste composition for sintering bonding

[0103] A silver paste composition for sintering was prepared in the same manner as in Example 1, except that 0.2 wt% of 2,2-bis(hydroxymethyl)propionic acid (purity 97% or higher) was added instead of the acid additive of Example 1 (0.05 wt% of malonic acid and 0.15 wt% of succinic acid) as the acid additive.

[0104]

[0105] <Comparative Example 5> Preparation of silver paste composition for sintering bonding

[0106] A silver paste composition for sintering was prepared in the same manner as in Example 1, except that 0.2 wt% itaconic acid (purity 99% or higher) was added instead of the acid additive of Example 1 (0.05 wt% malonic acid and 0.15 wt% succinic acid) as the acid additive.

[0107]

[0108] <Comparative Example 6> Preparation of silver paste composition for sintering bonding

[0109] A silver paste composition for sintering was prepared in the same manner as in Example 1, except that 0.2 wt% of diglycolic acid was added instead of the acid additive (0.05 wt% of malonic acid and 0.15 wt% of succinic acid) of Example 1 as the acid additive.

[0110]

[0111] <Comparative Example 7> Preparation of silver paste composition for sintering bonding

[0112] A silver paste composition for sintering was prepared in the same manner as in Example 1, except that 0.2 wt% of boric acid was added instead of the acid additive (0.05 wt% of malonic acid and 0.15 wt% of succinic acid) of Example 1 as the acid additive.

[0113]

[0114] <Comparative Example 8> Preparation of silver paste composition for sintering bonding

[0115] A silver paste composition for sintering was prepared in the same manner as in Example 1, except that 0.2 wt% of ethylenediaminetetraacetic acid was added instead of the acid additive of Example 1 (0.05 wt% of malonic acid and 0.15 wt% of succinic acid) as the acid additive.

[0116]

[0117] <Comparative Example 9> Preparation of silver paste composition for sintering bonding

[0118] A silver paste composition was prepared by mixing a silver filler and an organic solvent. At this time, no acid additive was added. As for the silver filler, an average particle size (D) of 270 nm was used as in Example 1. 50) was used as a spherical type silver powder (Metalor Technologies, product name: P620-7), and was used at a weight ratio of 80 wt% based on the entire silver paste composition. The composition of the organic solvent used is shown in Table 2 below. The ratio between the organic solvent components in Table 2 below is the same as the ratio between the remaining components except for the acid additive and the fluidity regulator in the organic solvents in Examples 1 to 3 and Comparative Examples 1 to 8 shown in Table 1 above, and the change in weight% based on the entire silver paste composition is due to not adding the acid additive and the fluidity regulator.

[0119] [Table 2]

[0120]

[0121]

[0122] <Comparative Example 10> Preparation of silver paste composition for sintering bonding

[0123] The average particle size (D) of silver filler is 270 nm. 50 ) with an average particle size (D) of 80 nm at a weight ratio of 70 wt% based on the total silver paste composition. 50 ) was used in a weight ratio of 10 wt% based on the total silver paste composition, a silver paste composition for sintering was prepared in the same manner as in Comparative Example 9.

[0124]

[0125] <Comparative Example 11> Preparation of silver paste composition for sintering bonding

[0126] The average particle size (D) of silver filler is 2.2 ㎛ 50) with a spherical type silver powder (Metalor Technologies, product name: EA-0030) at a weight ratio of 60 wt% relative to the total silver paste composition, and an average particle size (D) of 80 nm. 50 ) was used in a weight ratio of 20 wt% based on the total silver paste composition, a silver paste composition for sintering was prepared in the same manner as in Comparative Example 9.

[0127]

[0128] <Experimental Example> Evaluation of physical properties of silver paste compositions for sintering bonding in examples and comparative examples

[0129] Experimental Example 1. Measurement of viscosity and thixotropic index of silver paste composition for sintering bonding

[0130] Using a Brookfield Viscometer DV-ii+ pro model and a CPA-51Z spindle, the viscosity and thixotropic index of 0.5 ml of silver paste composition were measured at 25℃ and 0.5 rpm, and the results are shown in Table 3 below. If the thixotropic index is 6 or higher, the paste can be considered to have little stretching. If the paste stretching is large, when the squeegee is separated after printing, the paste may stretch and adhere to the printed pattern or non-target areas, which may deteriorate printability.

[0131] [Table 3]

[0132]

[0133] As shown in Table 3, the silver paste compositions of Examples 1, 2, and 3 had viscosity that was not excessively high and had a thixotropic index greater than 6, so it was found that they would have excellent printability.

[0134]

[0135] Experimental Example 2. Observation of the printing status of a silver paste composition for sintering bonding.

[0136] 10 x 10 mm (width x height) 2 A 250 ㎛ thick metal mask with an opening area was placed on a silver-coated lead frame, which is a printed object. At this time, the gap between the lead frame and the metal mask was maintained at a minimum through close contact. An appropriate amount of silver paste composition was placed on the metal mask, and printing was performed at a speed of 50 mm / s by applying a pressure of 2 MPa with a metal squeegee. After that, the printed shape was confirmed by separating the plate. The confirmed printing status is shown in Table 4 below.

[0137] [Table 4]

[0138]

[0139] As shown in Table 4, unlike some comparative examples in which bubbles were generated and cracks or spreading occurred, it was confirmed that the printing conditions of Examples 1, 2, and 3 were excellent. Therefore, it was confirmed that the excellent printability of the spherical silver powder was maintained even when an acid additive having the same composition as Examples 1, 2, and 3 was added.

[0140]

[0141] Experimental Example 3. Observation of the surface condition after drying of a silver paste composition for sintering bonding.

[0142] The silver paste composition printed in the above-described Experimental Example 2 was dried in a convection oven at 130°C for 30 minutes without a heating period. The surface condition of the dried silver paste composition was observed with the naked eye or using a digital microscope at a magnification of 35 times, and the results are shown in Table 5 and Fig. 1.

[0143] [Table 5]

[0144]

[0145] As shown in Table 5, unlike some comparative examples in which fine pinholes or cracks occurred, the compositions of Examples 1, 2, and 3 maintained a crack-free surface state even after drying. Therefore, it was confirmed that drying shrinkage was reduced when an acid additive having the same composition as Examples 1, 2, and 3 was added. It is believed that this effect is due to the fact that, during the drying process of the conductive paste, the decomposition of the acid additive induces a weak necking phenomenon between the metal particles, thereby reducing the contact area between the metal particles.

[0146]

[0147] Experimental Example 4. Observation of the cross-sectional state of the silver paste composition for sintering bonding after drying, measurement of the film thickness after drying, and measurement of the drying shrinkage rate.

[0148] 4-1. Observation of cross-sectional condition after drying of silver paste composition for sintering bonding

[0149] To observe the cross-section of the dried body, the printed and dried silver paste composition from Experimental Example 3 described above was molded using an acrylic-curable molding agent. The cross-section of the cured molded body was processed using only a polishing machine, and cross-section observation was performed at 500x magnification using a digital microscope. The results of the observation are shown in Fig. 2.

[0150] As a result, as shown in Fig. 2, it was found that no cracks or pinholes occurred in the cross-sections after drying in Examples 1, 2, and 3. Accordingly, it was confirmed that when an acid additive having the same composition as in Examples 1, 2, and 3 was added, drying shrinkage was reduced.

[0151] 4-2. Measurement of film thickness and drying shrinkage rate after drying of silver paste composition for sintering bonding

[0152] The thickness from the contact point between the silver paste composition and the substrate to the surface of the silver paste composition was measured using a micrometer capable of measuring up to 0.001 mm through distance measurement. The average value of five measurements was derived, and the results are shown in Table 6 below.

[0153] [Table 6]

[0154]

[0155] In addition, the shrinkage rate (drying shrinkage rate) when the printed paste dries was calculated using the following equation and is shown in Table 7 below.

[0156] ceremony

[0157] Drying shrinkage rate (%) = [1-(thickness of silver paste composition after drying (㎛) / thickness of printing mask (㎛))] x 100

[0158] [Table 7]

[0159]

[0160] As a result, as shown in Tables 6 and 7, the drying shrinkage rates of Examples 1, 2, and 3 were all less than 30%, and it was confirmed that the drying shrinkage was reduced when an acid additive having the same composition as Examples 1, 2, and 3 was added. It is believed that this effect is due to the fact that the contact area between the metal particles is reduced as a weak necking phenomenon is induced between the metal particles due to the decomposition of the acid additive during the drying process of the conductive paste.

[0161]

[0162] Experimental Example 5. Observation of the cross-sectional state after sintering of silver paste for sintering bonding, measurement of film thickness after sintering, and measurement of sintering shrinkage rate

[0163] 5-1. Observation of the cross-sectional state after sintering of the silver paste composition for sintering bonding

[0164] In the above-described Experimental Example 3, the printed and dried silver paste composition was subjected to pressure sintering by applying pressure of 0.4 MPa for 180 seconds using a hot press preheated to 250°C to induce metal bonding with the lead frame. The sintered paste was molded together with the bonded substrate using an acrylic curing molding agent. The cross-section of the molded body after curing was processed using only a polishing machine, and cross-sectional observation was performed at 500x magnification using a digital microscope. The results of the observation are shown in Fig. 3.

[0165] As a result, as shown in Fig. 3, it was found that no cracks or pinholes occurred in the cross-sections after sintering in Examples 1, 2, and 3, and that sintering bonding occurred densely. Accordingly, it was confirmed that sintering bonding occurred smoothly when an acid additive having the same composition as in Examples 1, 2, and 3 was added.

[0166] 5-2. Measurement of film thickness and sintering shrinkage after sintering of silver paste composition for sintering bonding

[0167] The thickness from the contact point between the silver paste composition and the substrate to the surface of the silver paste composition was measured using a micrometer capable of measuring up to 0.001 mm through distance measurement. The average value of five measurements was derived, and the results are shown in Table 8 below.

[0168] [Table 8]

[0169]

[0170] In addition, the shrinkage rate (sintering shrinkage rate) when the dried paste is sintered was calculated using the following equation, and the sintering shrinkage rate was obtained, and is shown in Table 9.

[0171] ceremony

[0172] Sintering shrinkage (%) = [1-(thickness after sintering of silver paste composition (㎛) / dry thickness of silver paste composition (㎛)] x 100

[0173] [Table 9]

[0174]

[0175] As shown in Tables 8 and 9 above, Examples 1, 2, and 3 exhibited high sintering shrinkage rates, which prevented chip breakage and thereby increased production yields. Furthermore, they achieved dense bonding, thereby enhancing the reliability and stability of the applied products. Furthermore, it was confirmed that the bottleneck phenomenon, which was the cause of the reduced drying shrinkage rate, did not affect the sintering bonding process.

[0176]

[0177] Experimental Example 6. Measurement of density, specific heat, thermal diffusivity, and thermal conductivity of a silver paste composition for sintering bonding after sintering.

[0178] Width x Length x Height 10 x 10 x 2 mm 3 The silver paste composition was filled into the hole, air bubbles were removed, and dried at 130°C for 30 minutes. The dried silver paste composition was pressure-sintered at 250°C for 180 seconds without a heating section to produce a specimen. At this time, the pressure was 10 x 10 mm in width x length. 2 The test was conducted at a pressure of 0.4 MPa as the standard.

[0179] The density of the manufactured specimen was measured using an Archimedes density balance and is shown in Table 10 below.

[0180] A specimen with a weight similar to 37 mg of sapphire to be used as a reference to measure the specific heat was prepared, and the size was 3 x 3 mm. 2The following sizes were prepared. The specific heat was measured under the conditions of -10℃ to 50℃, heating rate 10℃ / min, and nitrogen inflow rate 20 ml / min using Netzsch's DSC214 equipped with Intracooler 85. An isothermal section of 10 minutes was set at -10℃ to allow the specimen time to stabilize, and then the measurement was conducted through a program of heating up to 50℃ at 10℃ / min and an isothermal section of 10 minutes at 50℃, and the results are shown in Table 10 below.

[0181] Thermal diffusivity and thermal conductivity were measured through five shots at 25°C using LFA467 from Netzsch, and the results are shown in Table 10 below.

[0182] [Table 10]

[0183]

[0184] As shown in Table 10 above, when the silver paste compositions of Examples 1, 2, and 3 were used, the density of the sintered body tended to be higher, confirming that dense sintering was possible. In addition, when the silver paste compositions of Examples 1, 2, and 3 were used, the specific heat was similar to that of the comparative examples, confirming that there were no problems with stability and reliability. Furthermore, when the silver paste compositions of Examples 1, 2, and 3 were used, the thermal conductivity tended to be higher than that of the comparative examples, and the thermal diffusivity was similar to that of the comparative examples, confirming that there were no problems with stability and reliability.

[0185]

[0186] Experimental Example 7. Measurement of electrical conductivity after sintering of silver paste composition for sintering bonding

[0187] To confirm the electrical conductivity of the specimens manufactured using the same method as Experimental Example 6, the volume resistivity was measured. The resistance of the manufactured specimens was measured using a HIOKI RM3545 resistance meter equipped with a 4-probe probe. The volume resistivity was automatically calculated using HIOKI's resistance measurement software, RM9010App for Cuboid DUT, by inputting the specimen size value, and is shown in Table 11 below.

[0188] [Table 11]

[0189]

[0190] As shown in Table 11 above, the volume resistivity of the specimens using the silver paste compositions of Examples 1, 2, and 3 tended to be low, confirming that the electrical conductivity would be excellent.

Claims

1. A silver paste composition for sintering bonding comprising silver powder and an organic solvent, A silver paste composition for sintering, wherein the organic solvent comprises a carboxylic acid as an acid additive.

2. In paragraph 1, A silver paste composition for sintering bonding, wherein the silver powder comprises spherical silver powder.

3. In paragraph 1, The average particle size of the above silver powder (D 50 ) is 10 nm to 1000 nm, a silver paste composition for sintering bonding.

4. In paragraph 1, A silver paste composition for sintering, wherein the carboxylic acid is oxalic acid, malonic acid, succinic acid, glutaric acid, adipic acid, 2,2-bis(hydroxymethyl)propionic acid, itaconic acid, diglycolic acid, boric acid, ethylenediaminetetraacetic acid, or a combination thereof.

5. In paragraph 1, A silver paste composition for sintering, wherein the content of the above acid additive is 0.01 wt% to 10 wt% based on the total composition.

6. In paragraph 1, A silver paste composition for sintering, wherein the organic solvent is water, alcohol, ester, acetate or a mixed solvent thereof.

7. In paragraph 1, A silver paste composition for sintering, wherein the organic solvent further comprises at least one additive selected from the group consisting of a coupling agent, an antioxidant, a curing accelerator, a leveling agent, an antifoaming agent, a filler, a fluidity regulator, and a dispersing agent.

8. In paragraph 1, A silver paste composition for sintering, wherein the weight ratio of the silver powder and the organic solvent is 1:1 to 9:

1.

9. In paragraph 1, A silver paste composition for sintering, wherein the silver paste composition for sintering is binder-free.

10. In paragraph 1, The above silver paste composition for sintering bonding is a silver paste composition for sintering bonding having reduced drying shrinkage.

11. In paragraph 1, The silver paste composition for sintering bonding has a drying shrinkage rate of 0.5% to 30% after drying.

12. In paragraph 1, The silver paste composition for sintering bonding has a sintering shrinkage rate of 55% to 75% after pressure sintering.

13. A sintering bonding method using a silver paste composition for sintering bonding of any one of claims 1 to 12, (a) a step of forming a silver paste layer by printing or dispensing the silver paste composition for sintering bonding onto a first bonded body; and (b) A sintering bonding method comprising a step of placing a second bonding member on the silver paste layer and performing sintering bonding.

14. In paragraph 13, A sintering bonding method, wherein the step (a) further includes a process of drying the silver paste layer.

15. In paragraph 14, A sintering method wherein the process of drying the silver paste is performed at 80°C to 200°C.

16. In paragraph 13, A sintering method in which the sintering in step (b) is performed by heating.

17. In paragraph 16, A sintering method, wherein the sintering bonding heating temperature of the above step (b) is 150°C to 350°C.

18. In paragraph 13, A sintering method in which the sintering in step (b) is performed by applying pressure.

19. In paragraph 18, A sintering method, wherein the sintering bonding pressure of the above step (b) is 0.1 MPa to 20 MPa.

Citation Information

Patent Citations

  • Metal nanoparticle paste and conductive base material

    JP2010177084A

  • Metal paste composition

    KR1020140038391A

  • Apparatus for plasma treatment and method for plasma treatment

    KR1020220065698A

  • Non-face-to-face medical treatment system and non-face-to-face treatment method executed by it

    KR1020230172960A

  • Binder Free Cupper Paste and Sinter Bonding Method using the Same

    KR102279083B1