Repair and regeneration method for lithium iron phosphate

By roasting and spray granulating technology under carbon dioxide atmosphere, combined with ball milling and calcination steps, the problem of impurity residues in lithium iron phosphate battery recycling is solved, efficient removal of Al and F is achieved, and the stability and electricity consumption of regenerated lithium iron phosphate are improved. performance, achieving high-value recycling.

WO2024212075A1PCT designated stage expired Publication Date: 2024-10-17GUANGDONG BRUNP RECYCLING TECH CO LTD +1

Patent Information

Application Number
PCT/CN2023/087421
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-10
Publication Date
2024-10-17

AI Technical Summary

Technical Problem

In the recycling of existing lithium iron phosphate batteries, there are high levels of impurities (Al and F) and metal residues in the repair and regeneration process of used LiFePO4 cathode materials, resulting in poor stability and electrical performance of the regenerated products, and the need to supplement lithium, iron, Phosphorus source, affecting economic value.

Method used

The waste lithium iron phosphate electrode powder is roasted in a carbon dioxide atmosphere, combined with ball milling, sorting, spray granulation and calcination steps to reduce the content of Al and F impurities, remove Al through CO2 reaction, achieve carbonic acid removal, and avoid the addition of lithium, iron, The phosphorus source is directly calcined to obtain regenerated lithium iron phosphate.

Benefits of technology

It significantly reduces the Al and carbon impurity content in regenerated lithium iron phosphate, improves product stability and electrical performance, avoids impurity residues, achieves high-value recycling, and meets the use requirements of lithium-ion battery cathode materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN2023087421_17102024_PF_FP_ABST
    Figure CN2023087421_17102024_PF_FP_ABST
Patent Text Reader

Abstract

The present application relates to the technical field of lithium ion batteries, and discloses a repair and regeneration method for lithium iron phosphate. The repair and regeneration method for the lithium iron phosphate in the present application comprises crushing, soaking, screening, ball-milling and sorting a waste lithium iron phosphate electrode sheet first to obtain waste lithium iron phosphate electrode sheet powder, then roasting the waste lithium iron phosphate electrode sheet powder at 750-900°C under a carbon dioxide atmosphere, evenly stirring a roasted product with water, introducing carbon dioxide, and carrying out spray granulation on a mixture obtained from reaction to obtain a lithium iron phosphate precursor; finally calcining the obtained lithium iron phosphate precursor to obtain regenerated lithium iron phosphate. The repair and regeneration method for lithium iron phosphate in the present application does not require the addition of carbon, phosphorus, and lithium sources, the content of carbon in the prepared regenerated lithium iron phosphate is less than 0.15%, the content of Al therein is less than 0.015%, and the charge-discharge capacity is high.
Need to check novelty before this filing date? Find Prior Art

Description

A repair and regeneration method for lithium iron phosphate Technical Field

[0001] The present application belongs to the technical field of lithium-ion batteries, and specifically relates to a method for repairing and regenerating lithium iron phosphate. Background Art

[0002] With global energy shortages and environmental damage becoming increasingly severe, reducing resource consumption and protecting the environment are becoming a widely recognized trend. Lithium-ion batteries, due to their high energy density, high voltage, excellent cycle performance, low self-discharge, and environmental friendliness, are widely used in electric vehicles and various electronic devices, providing humanity with a solution to the energy shortage dilemma. Lithium iron phosphate batteries, due to their low cost, safety, excellent thermal stability, and high cycle performance, hold a significant market share among lithium batteries. Lithium iron phosphate batteries have a service life of 5-7 years, and a large number of them have already been retired, with this number expected to increase in the future. Therefore, research on the recycling of spent LiFePO4 batteries is extremely urgent.

[0003] LiFePO4 cathode materials account for approximately 40% of battery costs, making their high-value recycling highly economical. To date, the primary methods for recycling and disposing of spent LiFePO4 cathode materials have been repair, regeneration, and hydrometallurgy. The existing high-temperature sintering and separation of cathode sheets using oxygen or air results in high levels of impurities such as Al and F in the separated lithium iron phosphate waste powder, along with a large amount of residual metal. The sintering process for the LiFePO4 precursor requires the addition of lithium, iron, and phosphorus sources. Furthermore, the pyrolysis of the binder produces fluoride, which reacts with aluminum or lithium iron phosphate, producing lithium fluoride and aluminum fluoride that enter the cathode material. These difficulties hinder the stability of the repaired and regenerated products.

[0004] Summary of the Invention

[0005] The purpose of this application is to overcome the shortcomings of the existing technology and provide a repair and regeneration method for lithium iron phosphate. The method produces regenerated lithium iron phosphate with low carbon content and metal element residue, thereby improving the stability of the regenerated lithium iron phosphate.

[0006] To achieve the above objectives, the technical solution adopted in this application is to provide a method for repairing and regenerating lithium iron phosphate, comprising the following steps:

[0007] S1: ball milling and sorting the waste lithium iron phosphate electrodes to obtain waste lithium iron phosphate electrode powder;

[0008] S2: calcining the lithium iron phosphate waste powder obtained in step S1 at a temperature of 750-900°C under a carbon dioxide atmosphere, stirring the calcined product with water, introducing carbon dioxide, and spray granulating the reaction mixture to obtain a lithium iron phosphate precursor;

[0009] S3: adding the lithium iron phosphate precursor obtained in step S2 into an atmosphere furnace, and calcining it at 550-750° C. under the protection of an inert gas to obtain regenerated lithium iron phosphate.

[0010] In the repair and regeneration method of this application, CO2 is used as the reaction atmosphere to crack PVDF into carbon at high temperature, converting conductive carbon black into CO, achieving the purpose of F and carbon removal. After the lithium iron phosphate waste electrode pieces are crushed, they are soaked in hot water. The soaking can separate the aluminum slag and battery black powder in the waste electrode pieces. After passing through a water screen, the oversize material is aluminum slag, and the undersize material is a mixture of battery black powder and aluminum slag. The resulting undersize material is ball-milled and sorted to separate some of the Al in the lithium iron phosphate waste electrode powder. Calcination can convert the Al in the lithium iron phosphate waste electrode powder into aluminum oxide. After the calcined product is evenly stirred with water, the carbonic acid generated by the introduction of carbon dioxide can further remove the Al in the calcined product. The specific reaction chemical formula is H2O + CO2 → H2CO3, 3H2CO3 + 2Al → Al2(CO3)3 + 3H2. The above steps work together to minimize the Al impurity in the regenerated lithium iron phosphate, while avoiding the introduction of metal impurities that are introduced by other alkaline solution aluminum removal methods, thus ensuring battery safety. In addition, after the calcined product and water are evenly mixed, carbon dioxide is introduced into the reaction, which can cause the calcined product to be weakly dissolved and the aluminum to be filtered out. Combined with the spray drying method, the consumption of residual carbon, in-situ encapsulation of Al, and spherical regeneration of lithium iron phosphate can be achieved; there is no need to add lithium source, iron source, or phosphorus source, and regenerated lithium iron phosphate can be obtained directly through calcination.

[0011] Among them, the roasting temperature is one of the key factors affecting the removal effect of impurities such as Al, carbon and F in the lithium iron phosphate waste powder. If the roasting temperature is too low, impurities such as Al, carbon and F in the lithium iron phosphate waste powder cannot be completely converted into other removable substances, such as Al cannot be completely converted into alumina, and carbon cannot be completely converted into CO; if the roasting temperature is too high, it will cause the lithium iron phosphate to decompose.

[0012] The waste lithium iron phosphate electrodes in this application include the positive electrodes scrapped during the production process of lithium iron phosphate positive electrodes, the positive electrodes decomposed from batteries that have not been injected with electrolyte and scrapped during the battery preparation process, and the lithium iron phosphate positive electrodes disassembled from various scrapped batteries.

[0013] As a further improvement of the present application, in step S2, the heating rate of the calcination temperature is 2-5°C / min.

[0014] If the heating rate of the roasting temperature is too fast, it will easily damage the life of the atmosphere furnace, while if the heating rate of the roasting temperature is too slow, it will affect the experimental efficiency. After optimization, the heating rate within the above range can effectively improve the removal effect of impurities such as Al, carbon and F in lithium iron phosphate waste powder.

[0015] As a further improvement of the present application, in step S2, the calcination time is 2-4 hours. Within the above calcination time range, the decomposition effect of the waste lithium iron phosphate powder is better.

[0016] As a further improvement of the present application, in step S2, the mixture is prepared by uniformly stirring the calcined product and water, heating to 40-80°C, then introducing carbon dioxide, and stirring at a rotation speed of 200-300 rpm for 30-60 minutes.

[0017] As a further improvement of the present application, in step S2, the flow rate of carbon dioxide is 1-100 L / min.

[0018] When the flow rate of carbon dioxide is 1-100 L / min, it can better react with Al in the calcined product, so as to remove Al in the calcined product.

[0019] As a further improvement of the present application, in step S2, the conditions for spray granulation include: carrying out under inert protective gas, the spraying temperature is 170-190°C, the feed rate is 300-650 mL / h, the inlet pressure is 0.1-0.5 MPa, the outlet temperature is 120-150°C, and the inert protective gas is one of nitrogen, argon and helium.

[0020] In the present application, by controlling the spray temperature, feed rate, air intake pressure and other parameters in the spray granulation within the above-mentioned preferred range, the lithium iron phosphate precursor obtained has a better spherical structure and can in situ encapsulate the residual Al in the lithium iron phosphate product after calcination, thereby avoiding the impact of Al impurities on the stability and electrical properties of the product, reducing the Al content in the regenerated lithium iron phosphate, and further improving the electrical performance and stability of the battery.

[0021] As a further improvement of the present application, in step S2, the tail gas obtained by the reaction is absorbed by a saturated HCl-CuCl2 solution.

[0022] As a further improvement of the present application, the step S1 further includes the following steps: crushing, soaking, and screening the waste lithium iron phosphate electrodes;

[0023] As a further improvement of the present application, the specific steps of crushing, soaking and screening the waste lithium iron phosphate electrodes are as follows: cut the waste lithium iron phosphate electrodes into fragments of (1-2cmx1-2cm) size with scissors; soak the obtained fragments in hot water at a soaking temperature of 50-80°C and a soaking time of 5-60min, and pass them through a 2-15 mesh water sieve after soaking.

[0024] As a further improvement of the present application, in step S1, the parameters of ball milling are as follows: ball-to-material ratio is 5-20:1, ball milling speed is 100-400 rpm, and ball milling time is 5-60 min.

[0025] As a further improvement of the present application, in step S1, the sorting is airflow sorting, and the parameters of the airflow sorting are as follows: feeding rate is 3-5 kg / min, pulsation frequency is 30-50 Hz, and airflow speed is 10-12 cm / s.

[0026] This application uses ball milling to further grind and crush the waste lithium iron phosphate electrodes. By optimizing and controlling the parameters of ball milling, the battery black powder and aluminum slag can be effectively separated, and the impurity Al content in the waste lithium iron phosphate electrode powder can be further reduced through the parameters of air flow sorting.

[0027] As a further improvement of the present application, in step S3, the calcination time is 2-8 hours.

[0028] As a further improvement of the present application, in step S3, the lithium iron phosphate precursor needs to be pre-sintered, the pre-sintering temperature is 400-500° C., and the pre-sintering time is 1-4 hours.

[0029] By combining pre-sintering and calcination, bonding, densification, organizational structure changes and rearrangement between lithium iron phosphate precursors can be achieved within different temperature ranges, but there is no dissolution between the tissues, and no new components or new phases appear. The regenerated lithium iron phosphate can be used as a new lithium iron phosphate battery positive electrode material.

[0030] As a further improvement of the present application, in step S4, both the pre-sintering and the calcination are performed under the protection of an inert gas, and the inert gas is one of nitrogen, argon and helium.

[0031] In a second aspect, the present application provides a lithium iron phosphate prepared by the above-mentioned lithium iron phosphate repair and regeneration method.

[0032] In a third aspect, the present application also provides the use of lithium iron phosphate prepared by the above-mentioned lithium iron phosphate repair and regeneration method in the preparation of batteries.

[0033] Compared with the prior art, the present invention has the following advantages:

[0034] (1) In the repair and regeneration method of the present application, CO2 is used as the reaction atmosphere, PVDF is cracked into carbon at high temperature, and the conductive carbon black is converted into CO, thereby achieving the purpose of removing F and carbon; the carbon content in the regenerated lithium iron phosphate of the present application is less than 0.15%.

[0035] (2) The present application combines methods such as crushing, soaking, screening, ball milling, sorting, CO2 high-temperature roasting, and carbonation to remove Al, which can effectively reduce the impurity Al content in the regenerated lithium iron phosphate. The Al content in the regenerated lithium iron phosphate in the present application is less than 0.015%.

[0036] (3) The present application weakly dissolves the calcined product and then spray-dries and granulates it, which can achieve the consumption of residual carbon, in-situ encapsulation of Al, and spherical regeneration of lithium iron phosphate; there is no need to add lithium source, iron source, or phosphorus source, and the regenerated lithium iron phosphate can be directly obtained by calcination. The regenerated lithium iron phosphate can be used as a new positive electrode material for lithium iron phosphate batteries. BRIEF DESCRIPTION OF THE DRAWINGS

[0037] FIG1 is a process flow chart of the repair and regeneration method of lithium iron phosphate of the present application. DETAILED DESCRIPTION

[0038] In order to better illustrate the purpose, technical solutions and advantages of the present application, the present application will be further described below in conjunction with specific embodiments and comparative examples. Its purpose is to understand the content of the present application in detail, rather than to limit the present application. All other embodiments obtained by those of ordinary skill in the art without making creative work are within the scope of protection of the present application. The experimental reagents and instruments involved in the implementation of this application are all commonly used ordinary reagents and instruments unless otherwise specified.

[0039] Example 1

[0040] This embodiment provides a method for repairing and regenerating lithium iron phosphate, comprising the following steps:

[0041] (1) Use scissors to cut the waste lithium iron phosphate electrode into pieces of 2 cm x 2 cm in size; soak the obtained pieces in hot water at a temperature of 50°C for 5 minutes, and then pass them through a 2-mesh water sieve. The upper part of the sieve is aluminum slag, and the lower part of the sieve is a mixture of battery black powder and aluminum slag;

[0042] (2) drying the undersize obtained in step (1), placing it in a ball mill, adding zirconium balls to the ball mill, with a ball-to-material ratio of 5:1, and then placing it on a planetary ball mill and ball milling it at a speed of 400 rpm for 60 min; placing the obtained ball milled product in a pulsating airflow separator, setting the airflow separator feeding rate to 3 kg / min, the pulsating frequency to 30 Hz, and the airflow velocity to 10 cm / s, separating part of the Al in the ball milled product to obtain lithium iron phosphate waste powder;

[0043] (3) The waste lithium iron phosphate electrode powder obtained in step (2) is placed in a crucible, which is then placed in a tube furnace and introduced with CO2. After 60 minutes, the temperature is raised to 750°C at a heating rate of 5°C / min and calcined for 240 minutes to remove the carbon impurities in the electrode powder. At the same time, Al is further converted into Al2O3 and removed. The tail gas is absorbed by a saturated HCl-CuCl2 solution to obtain a calcined product.

[0044] (4) The calcined product obtained in step (3) and water were placed in a beaker, heated to 50° C., and then carbon dioxide was introduced at a flow rate of 100 L / min. The mixture was reacted at a stirring speed of 200 r / min for 60 min, and Al was removed by filtration to obtain a mixture;

[0045] (5) spray granulating the mixture obtained in step (4) to obtain a lithium iron phosphate precursor, wherein the spray granulation parameters are as follows: spray temperature of 170° C., feed rate of 400 mL / h, inlet pressure of 0.2 MPa, outlet temperature of 130° C., and nitrogen gas;

[0046] (6) The lithium iron phosphate precursor obtained in step (5) is placed in a crucible, placed in a tubular furnace and passed through helium. After 60 minutes, the temperature is increased to 400°C at a heating rate of 5°C / min and pre-sintered for 180 minutes. The temperature is then increased to 550°C at a heating rate of 5°C / min and calcined for 300 minutes to obtain regenerated lithium iron phosphate.

[0047] Example 2

[0048] This embodiment provides a method for repairing and regenerating lithium iron phosphate, comprising the following steps:

[0049] (1) Using scissors, cut the waste lithium iron phosphate electrodes into 2 cm x 2 cm pieces; soak the obtained pieces in hot water at 65°C for 30 min, and then pass them through a 10-mesh water sieve. The sieve-surface material is aluminum slag, and the sieve-underside material is a mixture of battery black powder and aluminum slag;

[0050] (2) drying the undersize obtained in step (1), placing it in a ball mill, adding zirconium balls to the ball mill, with a ball-to-material ratio of 10:1, and then placing it on a planetary ball mill and ball milling it at a speed of 400 rpm for 180 min; placing the obtained ball milled product in a pulsating airflow separator, setting the airflow separator feeding rate to 4 kg / min, the pulsating frequency to 40 Hz, and the airflow velocity to 11 cm / s, separating part of the Al in the ball milled product to obtain lithium iron phosphate waste electrode powder;

[0051] (3) The waste lithium iron phosphate electrode powder obtained in step (2) is placed in a crucible, which is then placed in a tube furnace and introduced with CO2. After 30 minutes, the temperature is raised to 800°C at a heating rate of 5°C / min and roasted for 180 minutes to remove the impurity carbon in the electrode powder. At the same time, Al is further converted into Al2O3 and removed. The tail gas is absorbed by a saturated HCl-CuCl2 solution to obtain a roasted product;

[0052] (4) The calcined product obtained in step (3) and water were placed in a beaker, heated to 60° C., and then carbon dioxide was introduced at a flow rate of 50 L / min. The mixture was stirred at a speed of 200 r / min for 50 min to remove Al, thereby obtaining a mixture;

[0053] (5) spray granulating the mixture obtained in step (4) to obtain a lithium iron phosphate precursor, wherein the spray granulation parameters are as follows: spray temperature of 180° C., feed rate of 500 mL / h, inlet pressure of 0.3 MPa, outlet temperature of 140° C., and nitrogen gas;

[0054] (6) The lithium iron phosphate precursor obtained in step (5) was placed in a crucible, placed in a tubular furnace and passed through helium. After 90 minutes, the temperature was increased to 450°C at a heating rate of 5°C / min and pre-sintered for 120 minutes. The temperature was then increased to 600°C at a heating rate of 5°C / min and calcined for 240 minutes to obtain regenerated lithium iron phosphate.

[0055] Example 3

[0056] This embodiment provides a method for repairing and regenerating lithium iron phosphate, comprising the following steps:

[0057] (1) Using scissors, cut the waste lithium iron phosphate electrodes into 2 cm x 2 cm pieces; soak the obtained pieces in hot water at 80°C for 60 min, and then pass them through a 15-mesh water sieve. The sieve-surface material is aluminum slag, and the sieve-underside material is a mixture of battery black powder and aluminum slag;

[0058] (2) drying the undersize obtained in step (1), placing it in a ball mill, adding zirconium balls to the ball mill, with a ball-to-material ratio of 15:1, and then placing it on a planetary ball mill and ball milling it at a speed of 400 rpm for 240 min; placing the obtained ball milled product in a pulsating airflow separator, setting the airflow separator feeding rate to 5 kg / min, the pulsating frequency to 50 Hz, and the airflow velocity to 12 cm / s, separating part of the Al in the ball milled product to obtain lithium iron phosphate waste electrode powder;

[0059] (3) The waste lithium iron phosphate electrode powder obtained in step (2) is placed in a crucible, which is then placed in a tube furnace and introduced with CO2. After 90 minutes, the temperature is raised to 900°C at a heating rate of 5°C / min and roasted for 120 minutes to remove the impurity carbon in the electrode powder. At the same time, Al is further converted into Al2O3 and removed. The tail gas is absorbed by a saturated HCl-CuCl2 solution to obtain a roasted product;

[0060] (4) The calcined product obtained in step (3) and water were placed in a beaker, heated to 70° C., and then carbon dioxide was introduced at a flow rate of 1 L / min. The mixture was stirred at a speed of 200 r / min for 30 min to remove Al, thereby obtaining a mixture;

[0061] (5) spray granulating the mixture obtained in step (4) to obtain a lithium iron phosphate precursor, wherein the spray granulation parameters are as follows: spray temperature of 190° C., feed rate of 600 mL / h, inlet pressure of 0.4 MPa, outlet temperature of 150° C., and nitrogen gas;

[0062] (6) The lithium iron phosphate precursor obtained in step (5) was placed in a crucible, placed in a tubular furnace and passed through helium. After 120 minutes, the temperature was increased to 500°C at a heating rate of 5°C / min and pre-sintered for 90 minutes. The temperature was then increased to 650°C at a heating rate of 5°C / min and calcined for 180 minutes to obtain regenerated lithium iron phosphate.

[0063] Comparative Example 1

[0064] This comparative example provides a method for repairing and regenerating lithium iron phosphate, comprising the following steps:

[0065] (1) Using scissors, cut the waste lithium iron phosphate electrodes into 2 cm x 2 cm pieces; soak the obtained pieces in hot water at 80°C for 60 min, and then pass them through a 15-mesh water sieve. The sieve-surface material is aluminum slag, and the sieve-underside material is a mixture of battery black powder and aluminum slag;

[0066] (2) drying the undersize obtained in step (1), placing it in a ball mill, adding zirconium balls to the ball mill, with a ball-to-material ratio of 15:1, and then placing it on a planetary ball mill and ball milling it at a speed of 400 rpm for 240 min; placing the obtained ball milled product in a pulsating airflow separator, setting the airflow separator feeding rate to 5 kg / min, the pulsating frequency to 50 Hz, and the airflow velocity to 12 cm / s, separating part of the Al in the ball milled product to obtain lithium iron phosphate waste electrode powder;

[0067] (3) The waste lithium iron phosphate powder obtained in step (2) is placed in a crucible, which is then placed in a tubular furnace and air is introduced. After 90 minutes, the temperature is raised to 600°C at a heating rate of 5°C / min and calcined for 120 minutes. After calcination, the structure of the lithium iron phosphate is destroyed, the divalent iron is oxidized to trivalent iron, and the waste lithium iron phosphate powder changes from black to red. If the carbon source, phosphorus source and lithium source are not supplemented and the product is directly calcined under the protection of inert gas, regenerated lithium iron phosphate cannot be obtained.

[0068] Comparative Example 2

[0069] This comparative example provides a method for repairing and regenerating lithium iron phosphate. The only difference between the method for repairing and regenerating lithium iron phosphate in this comparative example and that in Example 1 is that the roasting temperature in step (3) is 700°C. Since the roasting temperature is too low, the carbon and Al in the waste lithium iron phosphate powder cannot be completely removed, resulting in high carbon and Al contents in the regenerated lithium iron phosphate.

[0070] Comparative Example 3

[0071] This comparative example provides a method for repairing and regenerating lithium iron phosphate. The difference between the method for repairing and regenerating lithium iron phosphate in this comparative example and that in Example 1 is that the calcination temperature in step (3) is 950°C.

[0072] Comparative Example 4

[0073] This comparative example provides a method for repairing and regenerating lithium iron phosphate. The difference between the method for repairing and regenerating lithium iron phosphate in this comparative example and that in Example 1 is that CO2 is not introduced in step (4).

[0074] Example 4

[0075] The content of some elements of the regenerated lithium iron phosphate obtained in each embodiment and comparative example was tested, wherein the content of Li, Fe, and Al elements was obtained by testing according to the standard YS / T 1028.5-2015 lithium iron phosphate chemical analysis method; the content of P element was obtained by testing according to the standard YS / T 1028.3-2015 lithium iron phosphate chemical analysis method; the content of C element was obtained according to the test standard YS / T 1028.4-2015 lithium iron phosphate chemical analysis method; the test results are shown in Table 1.

[0076] Table 1

[0077] As can be seen from Table 1, the contents of main elements, Al and C in the regenerated lithium iron phosphate prepared in the embodiment are normal, and meet the industrial production standards of lithium iron phosphate batteries.

[0078] Example 5

[0079] The regenerated lithium iron phosphate obtained in each embodiment and comparative example was made into button batteries for comparative study of electrochemical performance. For button battery production, lithium iron phosphate active material, conductive carbon black and PCDF were mixed in a mass ratio of 8:1:1 to form a slurry, which was coated on aluminum foil and baked at 120°C for 8 hours. It was then rolled and cut into small round electrodes for button battery production. The button batteries were assembled in a glove box. The glove box conditions were that the water and oxygen content was less than or equal to 0.01ppm, and the electrolyte was 1.0M LiPF6in EC:DMC:DEC=1:1:1Vol%. The test conditions for battery performance were: the charge and discharge voltage range was 2.5-4.2V (relative to Li + / Li), the ambient temperature was 25°C, and the battery performance was obtained by charging and discharging with a current density of 0.1C (1C = 150mA / g). See Table 2.

[0080] Table 2

[0081] As can be seen from Table 2, the charging capacity of the lithium-ion battery prepared from the regenerated lithium iron phosphate obtained in the embodiment can reach 158.6 mAh / g, and the initial charge and discharge efficiency can reach 94.5%.

[0082] Finally, it should be noted that the above embodiments are used to illustrate the technical solutions of the present application rather than to limit the scope of protection of the present application. Although the present application has been described in detail with reference to the preferred embodiments, ordinary technicians in this field should understand that the technical solutions of the present application can be modified or replaced by equivalents without departing from the essence and scope of the technical solutions of the present application.

Claims

1. A method for repairing and regenerating lithium iron phosphate, characterized in that: The following steps are involved: Ball milling and sorting the waste lithium iron phosphate pole pieces to obtain waste lithium iron phosphate pole powder; In a carbon dioxide atmosphere, the obtained lithium iron phosphate waste powder is calcined at a temperature of 750-900° C., the obtained calcined product is evenly stirred with water, carbon dioxide is introduced, and the reaction mixture is spray granulated to obtain a lithium iron phosphate precursor; The obtained lithium iron phosphate precursor is added into an atmosphere furnace, and under the protection of an inert gas, the temperature is raised to 550-750° C. for calcination to obtain regenerated lithium iron phosphate.

2. The method for repairing and regenerating lithium iron phosphate according to claim 1, characterized in that: The heating rate of the calcination temperature is 2-5°C / min.

3. The method for repairing and regenerating lithium iron phosphate according to claim 1, characterized in that: The calcination time is 2-4 hours.

4. The method for repairing and regenerating lithium iron phosphate according to claim 1, characterized in that: The preparation method of the mixture is as follows: the roasted product and water are stirred evenly, heated to 40-80° C., then carbon dioxide is introduced, and stirred at a rotation speed of 200-300 rpm for 30-60 minutes to obtain the mixture.

5. The method for repairing and regenerating lithium iron phosphate according to claim 4, characterized in that: The flow rate of the carbon dioxide is 1 to 100 L / min.

6. The method for repairing and regenerating lithium iron phosphate according to claim 1, characterized in that: The spray granulation conditions include: being carried out under inert protective gas, the spray temperature is 170-190° C., the feed rate is 300-650 mL / h, the inlet pressure is 0.1-0.5 MPa, the outlet temperature is 120-150° C., and the inert protective gas is one of nitrogen, argon and helium.

7. The method for repairing and regenerating lithium iron phosphate according to claim 1, characterized in that: The tail gas obtained from the reaction is absorbed by a saturated HCl-CuCl2 solution.

8. The method for repairing and regenerating lithium iron phosphate according to claim 1, characterized in that: The method also includes the following steps before ball milling the waste lithium iron phosphate electrode sheets: crushing, soaking and screening the waste lithium iron phosphate electrode sheets.

9. The method for repairing and regenerating lithium iron phosphate according to claim 8, characterized in that: The specific steps of crushing, soaking and screening the waste lithium iron phosphate electrodes are as follows: cutting the waste lithium iron phosphate electrodes into pieces of (1-2cmx1-2cm) size with scissors; soaking the obtained pieces in hot water at a soaking temperature of 50-80°C and a soaking time of 5-60min, and passing through a 2-15 mesh water sieve after the soaking.

10. The method for repairing and regenerating lithium iron phosphate according to claim 1, characterized in that: The parameters of the ball milling are as follows: the ball-to-material ratio is 5-20:1, the ball milling speed is 100-400 rpm, and the ball milling time is 5-60 min.

11. The method for repairing and regenerating lithium iron phosphate according to claim 1, characterized in that: The sorting is airflow sorting, and the parameters of the airflow sorting are as follows: the feeding speed is 3-5 kg / min, the pulsation frequency is 30-50 Hz, and the airflow speed is 10-12 cm / s.

12. The method for repairing and regenerating lithium iron phosphate according to claim 1, characterized in that: The calcination time is 2-8h.

13. The method for repairing and regenerating lithium iron phosphate according to claim 1, characterized in that: The lithium iron phosphate precursor needs to be pre-sintered before calcination. The pre-sintering temperature is 400-500° C. and the pre-sintering time is 1-4 hours.

14. A lithium iron phosphate, characterized in that: The lithium iron phosphate is prepared by the repair and regeneration method of any one of claims 1 to 13.

15. Use of the lithium iron phosphate as claimed in claim 14 in preparing a battery.

Citation Information

Patent Citations

  • Selective oxidation-reduction regeneration method of waste lithium iron phosphate, regenerated lithium iron phosphate and lithium ion battery

    CN113036253A

  • Method for cyclic regeneration of lithium iron phosphorus components in lithium iron phosphate waste powder

    CN114212765A

  • Modification method for directly repairing and regenerating lithium iron phosphate positive electrode material by pyrogenic process

    CN114566727A

  • Method for recycling waste phosphate positive electrode material

    CN114583313A

  • Repair lithium iron phosphate positive electrode material, preparation method and application

    CN114824544A

Cited By

  • Method for repairing lithium iron phosphate

    CN119349533A

  • Recycling and regenerating method for positive electrode material of waste lithium iron phosphate battery, positive electrode material, positive plate, secondary battery and power utilization device

    CN119528101A

  • Regeneration of lithium iron phosphate anode material from waste lithium iron phosphate battery and preparation and application thereof

    CN119833806B