Surface contact non-lay length adhesive-coated steel cord and manufacturing method therefor
By using a cluster drawing die and steel glue in the three-layer structure of the steel cord, a surface contact structure is formed, which solves the problem of insufficient friction of the steel cord in the existing technology and significantly improves the stiffness and stability of the steel cord. .
Patent Information
- Application Number
- PCT/CN2023/089970
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-12
- Filing Date
- 2023-04-23
- Publication Date
- 2024-10-17
AI Technical Summary
Existing steel cords suffer from insufficient friction due to point contact after twisting, resulting in layer torsion and reduced stiffness.
It adopts a three-layer structure design of surface contact untwisted glue-coated steel cords. Steel glue is added into the water tank through a cluster drawing die to form surface contact between the core strands, middle strands and outer strands, and is coated in the gaps. Steel glue increases friction.
It effectively alleviates the layer torsion problem of steel cords, improves the stiffness of steel cords, and enhances the friction between steel wires through surface contact.
Smart Images

Figure CN2023089970_17102024_PF_FP_ABST
Abstract
Description
Surface contact twist-free rubberized steel cord and manufacturing method thereof Technical Field
[0001] The invention relates to a surface contact twist-free rubberized steel cord and a manufacturing method thereof, belonging to the technical field of steel cords. Background Art
[0002] Steel cord is a special purpose fine gauge steel wire strand or rope made of high quality high carbon steel with brass coating on the surface.
[0003] Currently, after the existing steel cord is twisted through the conventional process, the steel wires are formed by twisting and there is point contact between the steel wires. The contact area is insufficient, resulting in insufficient friction between the steel wires, which causes the steel cord to twist and reduce its stiffness.
[0004] Summary of the Invention
[0005] The purpose of the present invention is to overcome the deficiencies in the prior art and provide a surface contact twist-free rubberized steel cord and a method for manufacturing the same, so as to solve the problems of insufficient friction between steel wires, layer torsion of the steel cord and decreased stiffness.
[0006] In order to achieve the above object, the technical solution adopted by the present invention is:
[0007] In a first aspect, the present invention provides a surface contact twistless rubberized steel cord, wherein the steel cord has at least a three-layer structure including a core strand, an intermediate strand, and an outer strand, wherein the core strand, the intermediate strand, and the outer strand are integrally formed by bundle drawing;
[0008] The gap between the core strand and the middle strand is larger than the gap between the middle strand and the outer strand. The gap between the core strand and the middle strand, and the gap between the middle strand and the outer strand are both coated with steel glue.
[0009] In combination with the first aspect, further, the core strand includes at least three steel wires.
[0010] Furthermore, the middle strand is provided with six steel wires and the outer strand is provided with nine steel wires; or the middle strand is provided with nine steel wires and the outer strand is provided with fifteen steel wires.
[0011] In a second aspect, a method for manufacturing a surface-contact, twist-free, rubberized steel cord according to any of the above-mentioned steps comprises the following steps:
[0012] Place the cluster drawing die into the water tank;
[0013] Add twisting liquid into the water tank until it covers the cluster drawing die;
[0014] Several semi-finished steel wires are put into a cluster drawing die for drawing to obtain surface contact twist-free rubber-coated steel cords.
[0015] In combination with the second aspect, further, the surface contact twist-free rubberized steel cord is wound through a reel using an I-shaped wheel.
[0016] Furthermore, surface contact is formed between the steel wires in the drawn surface contact twist-free rubberized steel cord.
[0017] Furthermore, the several semi-finished steel wires that have been processed are arranged according to the three-layer structure and then placed in a cluster drawing die for drawing.
[0018] Furthermore, the twisting liquid is steel rubber, or a mixture of steel rubber and twisting oil, and the weight ratio of twisting oil to steel rubber in the mixture is 2:8.
[0019] Compared with the prior art, the present invention has the following beneficial effects:
[0020] The present invention places the drawing die into a water tank filled with steel glue, so that the steel cord is coated with steel glue between the strands during the drawing process, thereby increasing the friction between the steel wires.
[0021] The present invention changes the contact between the outer strands and the middle strands, and between the middle strands and the core strands from point contact to surface contact through cluster drawing, further increasing the friction between the steel wires, alleviating the torsion problem of the steel cord layer, and improving the stiffness of the steel cord. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] FIG1 is a schematic diagram of a drawing process of a surface contact twist-free rubberized steel cord provided by an embodiment of the present invention;
[0023] FIG2 is a schematic cross-sectional view of a surface-contact, twist-free, rubberized steel cord provided by an embodiment of the present invention;
[0024] In the figure: 1: semi-finished steel wire, 2: water tank, 3: cluster drawing die, 4: roller, 5: I-shaped pulley, 6: steel glue, 7: outer strand, 8: middle strand, 9: core strand, 10: gap between core strand and middle strand, 11: gap between middle strand and outer strand. DETAILED DESCRIPTION
[0025] The present invention will be further described below in conjunction with the accompanying drawings. The following embodiments are only used to more clearly illustrate the technical solutions of the present invention and are not intended to limit the scope of protection of the present invention.
[0026] Example 1:
[0027] As shown in Figure 2, it is a cross-sectional schematic diagram of a surface-contact, twist-free, rubber-coated steel cord provided in an embodiment of the present invention. The steel cord has a three-layer structure, including a core strand 9, an intermediate strand 8, and an outer strand 7, wherein the core strand 9, the intermediate strand 8, and the outer strand 7 are integrally formed by cluster drawing.
[0028] Due to the clustered drawing, the outer strands 7 deform and come into surface contact with the intermediate strands 8. However, the intermediate strands 8 do not deform significantly and come into surface contact with the core strands 9. A gap 10 exists between the intermediate strands 8 and the core strands 9. In this embodiment, the steel glue 6 is added to the drawing environment so that the gap 10 between the core strands and the intermediate strands is coated with the steel glue 6, thereby increasing the friction between the steel wires.
[0029] Similarly, the gap 11 between the middle strand 8 and the outer strand 7 is also coated with the steel glue 6.
[0030] It is feasible that the core strand 9 of this embodiment includes at least three steel wires, and this embodiment uses three steel wires; the middle strand 8 is provided with six steel wires, and the outer strand 7 is provided with nine steel wires; or the middle strand 8 is provided with nine steel wires, and the outer strand 7 is provided with fifteen steel wires.
[0031] Example 2:
[0032] This embodiment provides a method for manufacturing a surface-contact, twist-free, rubber-coated steel cord, comprising:
[0033] Add steel glue 6 or a mixture of steel glue and twisting oil into the drawing water tank 2;
[0034] Place the cluster drawing die 3 into the water tank 2, wherein the steel glue 6 can cover the cluster drawing die 3;
[0035] This product is produced by placing several semi-finished steel wires that have been processed into a cluster-type drawing die for drawing.
[0036] The weight ratio of twisting oil to steel rubber in the mixture of this embodiment is 2:8.
[0037] The raw material wire rod is processed through the front-end process. Specifically, the raw material wire rod is processed through rough drawing, heat treatment, intermediate drawing, electroplating, and water tank drawing to form a semi-finished steel wire 1.
[0038] As shown in Figure 1, it is a schematic diagram of the drawing process of a surface contact twist-free rubber-coated steel cord provided by an embodiment of the present invention. The semi-finished steel wire 1 after the previous process passes through a guide wheel and enters the bundled drawing die 3 in the water tank 2 for bundled drawing. After drawing, it passes through a roller 4 and is wound using an I-shaped wheel 5 to obtain a surface contact twist-free rubber-coated steel cord.
[0039] It is feasible that the three-layer structure of core strands, middle strands and outer strands are arranged in a three-layer structure according to the required quantity before entering the cluster drawing die, and then can be produced by a single cluster drawing.
[0040] The cluster drawing process is provided with only one pass, which is the cluster drawing pass. In the water tank 2 in the present embodiment, a mixture of twisting oil and steel glue is added to carry out drawing so that the gaps between the steel wires in the steel cord are filled with steel glue.
[0041] Example 3:
[0042] The present invention can also be provided with a surface contact untwisted pitch coated steel cord having a four-layer structure, including a core strand 9, an intermediate strand 8, an outer strand 7 and a ring outer strand. Based on the method of Example 2, the four-layer structure is integrally formed by cluster drawing, so that surface contact is formed between the steel wires in the steel cord.
[0043] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the technical principles of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A surface contact twistless rubber coated steel cord, characterized in that: The steel cord is at least a three-layer structure including a core strand, a middle strand and an outer strand, and the core strand, the middle strand and the outer strand are integrally formed by bundling and drawing; The gap between the core strand and the middle strand is larger than the gap between the middle strand and the outer strand. The gap between the core strand and the middle strand, and the gap between the middle strand and the outer strand are both coated with steel glue.
2. The surface contact twist-free rubber-coated steel cord according to claim 1, characterized in that: The core strand comprises at least three steel wires.
3. The surface contact twist-free rubber-coated steel cord according to claim 1, characterized in that: The middle strand is provided with six steel wires, and the outer strand is provided with nine steel wires; or the middle strand is provided with nine steel wires, and the outer strand is provided with fifteen steel wires.
4. The method for manufacturing the surface contact twist-free rubber-coated steel cord according to any one of claims 1 to 3, characterized in that: The steps include: Place the cluster drawing die into the water tank; Add twisting liquid into the water tank until it covers the cluster drawing die; A plurality of semi-finished steel wires are put into a cluster-type drawing die for drawing to obtain surface-contact non-twist-pitch rubber-coated steel cords.
5. The method according to claim 4, characterized in that: The surface contact untwisted pitch rubber coated steel cord is taken up by an I-shaped wheel through a reel.
6. The method according to claim 4, characterized in that: Surface contact is formed between the steel wires in the drawn surface contact twist-free rubber-coated steel cord.
7. The method according to claim 4, characterized in that: The several semi-finished steel wires that have been processed are arranged according to the three-layer structure and then placed in a cluster-type drawing die for drawing.
8. The manufacturing method according to claim 4, characterized in that: The twisting liquid is steel rubber, or a mixture of steel rubber and twisting oil, and the weight ratio of the twisting oil to the steel rubber in the mixture is 2:8.
Citation Information
Patent Citations
Rubber-steel cord composite and tire using the same
CN101370979A
Method and device for producing a three-layer cord
CN102365404A
Die-drawing pre-stress steel strand production line
CN103669056A
17-strand radial tire steel cord
CN110735340A
Steel cord with compact structure and preparation method thereof
CN112064385A