Method for leaching scheelite
Through the low-temperature leaching of scheelite with sulfuric acid-hydrochloric acid/nitric acid and the regeneration and recycling technology of incomplete calcium precipitation in acid leaching solution, the problems of hazardous waste and equipment corrosion in the tungsten smelting process have been solved, and efficient tungsten metal recycling and low-cost production have been achieved.
Patent Information
- Application Number
- PCT/CN2023/127776
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-14
- Filing Date
- 2023-10-30
- Publication Date
- 2024-10-17
AI Technical Summary
In the existing tungsten smelting process, alkali decomposed tungsten smelting slag is classified as a hazardous waste and requires high reaction temperatures, resulting in equipment corrosion and difficulty in wastewater treatment, making it difficult to achieve low-cost, low-pollution, and low-wastewater scheelite treatment.
Using sulfuric acid-hydrochloric acid/nitric acid low-temperature leaching of scheelite and incomplete calcium precipitation regeneration and recycling technology of acid leaching liquid, the acid leaching liquid is processed through incomplete calcium precipitation to achieve closed-circuit recycling of acid leaching liquid and complete leaching under low temperature conditions For scheelite, steel-lined PTFE material is used to improve the corrosion resistance of the equipment.
It improves the recovery rate of tungsten metal, reduces the process requirements for equipment, realizes closed-circuit recycling of acid leaching liquid, reduces waste liquid discharge and production costs, and enhances the corrosion resistance of the equipment.
Smart Images

Figure CN2023127776_17102024_PF_FP_ABST
Abstract
Description
A leaching method for scheelite Technical Field
[0001] The invention belongs to the technical field of tungsten smelting, and in particular relates to a leaching method for scheelite. Background Art
[0002] Tungsten is a strategic mineral resource, playing a vital role in both the national economy and the defense industry. Decades of continuous mining have significantly shifted the distribution structure of tungsten ore, shifting from being primarily wolframite to being primarily scheelite. According to statistics, by 2020, scheelite accounted for over 75% of my country's tungsten ore resources, and this proportion continues to increase. In tungsten smelting, the alkaline decomposition process of tungsten concentrate is widely used in the tungsten industry due to its stability, adaptability to various complex ores, and high tungsten recovery rates. However, since 2016, alkaline decomposition tungsten smelting slag has been classified as hazardous waste, inevitably increasing pressure on tungsten smelting companies with limited profits. Furthermore, national environmental protection regulations are currently tightening controls on non-ferrous metal smelting wastewater discharge, encouraging companies to adopt advanced technologies and equipment to reduce or even achieve zero wastewater discharge. Therefore, the low-cost, low-pollution, and low-wastewater treatment of scheelite is a key focus of the tungsten industry and holds significant practical significance.
[0003] To address this issue, industry researchers have proposed using hydrochloric acid to decompose tungsten concentrate to produce solid tungstic acid and waste acid solution. The tungstic acid is then dissolved in ammonia to produce an ammonium tungstate solution. Impurities such as phosphorus, arsenic, and silicon are then removed with magnesium salts. The resulting pure ammonium tungstate solution is then evaporated and crystallized to produce ammonium paratungstate. This process offers advantages such as a short process flow, minimal wastewater generation, non-hazardous tungsten slag, and low production costs. However, this process requires high reaction temperatures (above 95°C), placing significant demands on the reactor's sealing and corrosion resistance. Otherwise, acid mist can pollute the surrounding environment and cause significant corrosion damage to equipment, especially when treating fluorine-containing tungsten ores, where hydrogen fluoride is produced, which can be even more corrosive. Furthermore, the acid leachate produced by this process is difficult to recycle. Directly neutralizing it with lime not only wastes a significant amount of acid resources and incurs significant lime neutralization costs, but also generates a large amount of wastewater treatment sludge that is difficult to dispose of. If the acid leachate is directly returned to decompose the scheelite, problems such as incomplete decomposition can occur. Summary of the Invention
[0004] In order to solve the problems existing in the prior art, the main purpose of the present invention is to propose a leaching method for scheelite, which can achieve complete leaching of scheelite under low temperature conditions and increase the tungsten recovery rate to more than 99.5%.
[0005] To solve the above technical problems, according to one aspect of the present invention, the present invention provides the following technical solutions:
[0006] A scheelite leaching method comprises the following steps:
[0007] S1. Scheelite Leaching
[0008] A certain amount of scheelite is placed in a reactor, and hydrochloric acid is added according to the liquid-solid ratio of hydrochloric acid to scheelite of 2-4:1 mL / g. Then, sulfuric acid or nitric acid with a volume of 0.3-1.0% of the hydrochloric acid is added for stirring and leaching. The mixture is cooled and filtered to obtain tungstic acid and acid leaching solution.
[0009] S2. Closed-circuit recycling of acid leaching solution
[0010] Sulfuric acid is added to the acid leaching solution for incomplete calcium precipitation. The volume of sulfuric acid added is 0.1-2.5% of the volume of the acid leaching solution. After the reaction, the solution is cooled to room temperature and filtered and washed to obtain calcium sulfate and regenerated acid solution. The regenerated acid solution is returned to leaching scheelite. The insufficient amount is supplemented with hydrochloric acid. Other parameters are carried out according to the process of step S1.
[0011] As a preferred embodiment of the scheelite leaching method of the present invention, the method further comprises:
[0012] S3. Tungstate ammonia solution removal
[0013] Ammonia dissolution is performed according to the liquid-solid ratio of ammonia water and tungstic acid of 3~5:1mL / g, and the ammonia slag and ammonium tungstate solution are obtained by filtration. Ammonium sulfide, magnesium sulfate and copper sulfate are added to the ammonium tungstate solution in sequence, and the mixture is fully reacted to remove impurities. After filtration, pure ammonium tungstate solution can be obtained, and then the ammonium paratungstate product can be obtained by evaporation and crystallization.
[0014] As a preferred embodiment of the scheelite leaching method of the present invention, in step S1, the concentration of hydrochloric acid is 17-31 wt%.
[0015] As a preferred embodiment of the scheelite leaching method of the present invention, in step S1, the concentration of sulfuric acid is 98 wt %, and the concentration of nitric acid is 96-98 wt %.
[0016] As a preferred embodiment of the scheelite leaching method of the present invention, in step S1, the inner wall of the reactor is made of steel-lined PTFE material, and is provided with a heating tube and a temperature measuring device made of steel-lined PTFE material.
[0017] As a preferred embodiment of the scheelite leaching method of the present invention, in step S1, the leaching temperature is 60-95° C., and the leaching time is 1.5-6.0 h.
[0018] As a preferred embodiment of the scheelite leaching method of the present invention, in step S2, the concentration of sulfuric acid is 98 wt%.
[0019] As a preferred embodiment of the scheelite leaching method of the present invention, in step S2, the reaction time is 25 to 35 minutes.
[0020] As a preferred embodiment of the scheelite leaching method of the present invention, in step S3, the concentration of the ammonia water is 3-6 wt%.
[0021] As a preferred embodiment of the scheelite leaching method of the present invention, in step S3, the ammonia dissolution temperature is room temperature, and the ammonia dissolution time is 1 to 2 hours.
[0022] The beneficial effects of the present invention are as follows:
[0023] This invention proposes a scheelite leaching method that utilizes a low-temperature sulfuric acid-hydrochloric acid / nitric acid-hydrochloric acid leaching method and a novel technology for the regeneration and recycling of the acid leaching solution through incomplete calcium precipitation. This technology not only achieves complete low-temperature leaching of the scheelite, improves tungsten metal recovery, and reduces process equipment requirements, but also utilizes a steel-lined PTFE material for the reactor, heating tube, and temperature measurement device. This material is not only resistant to hydrochloric acid corrosion but also can process high-fluorine scheelite and withstand hydrogen fluoride corrosion, further improving the equipment's corrosion resistance. Furthermore, this invention successfully achieves closed-loop recycling of the acid leaching solution, significantly reducing production costs. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the following briefly introduces the drawings required for use in the embodiments or the description of the prior art. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on the structures shown in these drawings without paying any creative work.
[0025] FIG1 is a schematic flow diagram of a scheelite leaching method according to the present invention.
[0026] The purpose, features and advantages of the present invention will be further described with reference to the accompanying drawings and in conjunction with the embodiments. Implementation Method
[0027] The following will be a clear and complete description of the technical solutions in the embodiments. Obviously, the embodiments described are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making any creative efforts are within the scope of protection of the present invention.
[0028] A method for leaching scheelite addresses the current short-cycle process for preparing ammonium paratungstate from tungsten concentrate, which involves "acid decomposition + ammonia dissolution + purification and impurity removal + evaporation and crystallization." This process requires high reaction temperatures (above 95°C), places significant strain on the reactor's sealing and corrosion resistance, and easily generates significant acid mist pollution, causing significant corrosion damage to equipment. This is especially difficult when processing fluorine-containing scheelite, especially when hydrogen fluoride-resistant materials are difficult to find. Furthermore, the acid leachate produced by this process is difficult to handle. Direct lime neutralization not only wastes significant acid resources and incurs significant lime neutralization costs, but also produces a large amount of wastewater and sludge that is difficult to dispose of. If the acid leachate is directly returned to the scheelite, the resulting tungstic acid residue, after alkaline dissolution, contains over 20% WO3, indicating incomplete decomposition. This new technology utilizes low-temperature leaching of scheelite using sulfuric acid, hydrochloric acid, or nitric acid, and recycling of the acid leachate using incomplete calcium precipitation. Specifically, during the scheelite leaching process, the dense membrane structure of the reaction product, tungstic acid, is destroyed, increasing the contact area between scheelite and hydrochloric acid and boosting the reaction rate. Furthermore, due to the high concentration of sulfuric acid / nitric acid, the acid concentration in the reaction system remains high as the reaction proceeds, ensuring thorough leaching of the scheelite. Furthermore, based on the important discovery that calcium sulfate has a certain solubility in a mixed solution of hydrochloric acid and calcium chloride, a novel incomplete calcium precipitation technique was invented to treat the acid leaching solution to produce regenerated acid. By strictly controlling the sulfate ion concentration in the regenerated acid, the regenerated acid can be recycled for efficient leaching of scheelite. This technology significantly reduces the acid leaching process temperature, achieving low-temperature, thorough leaching of scheelite, improving scheelite metal recovery, and lowering process equipment requirements. It also successfully enables closed-loop recycling of the acid leaching solution, transforming waste into valuable resources, reducing wastewater emissions, and significantly lowering production costs. The generated calcium sulfate can also be returned to the main workshop for sodium tungstate dephosphorization, further reducing production costs.
[0029] According to one aspect of the present invention, the present invention provides the following technical solutions:
[0030] A scheelite leaching method comprises the following steps:
[0031] S1. Scheelite Leaching
[0032] A certain amount of scheelite is placed in a reactor. Hydrochloric acid is added at a liquid-to-solid ratio of 2-4:1 mL / g. Sulfuric acid or nitric acid at a concentration of 0.3-1.0% of the volume of the hydrochloric acid is then added for stirring and leaching. The mixture is cooled and filtered to obtain tungstic acid and an acid leaching solution. The concentration of hydrochloric acid is 17-31wt%, the concentration of sulfuric acid is 98wt%, and the concentration of nitric acid is 96-98wt%. The scheelite leaching process destroys the dense membrane structure of the tungstic acid product, increasing the contact area between the scheelite and the hydrochloric acid and boosting the reaction rate. Furthermore, due to the high concentration of sulfuric acid or nitric acid, the acid concentration in the reaction system remains high as the reaction proceeds, ensuring thorough leaching of the scheelite. Alkali dissolution of a small amount of tungstic acid produces an alkaline slag containing 0.2-1.0wt% WO3. Specifically, the liquid-to-solid ratio of hydrochloric acid to scheelite can be, for example but not limited to, any one of 2:1 mL / g, 2.2:1 mL / g, 2.5:1 mL / g, 2.7:1 mL / g, 3:1 mL / g, 3.3:1 mL / g, 3.5:1 mL / g, 3.8:1 mL / g, 4:1 mL / g, or a range between any two of them; the sulfuric acid or nitric acid can be, for example but not limited to, any one of 0.3%, 0.4%, 0.5%, 0.6%, 0.7%, 0.8%, 0.9%, 1.0% by volume of the hydrochloric acid, or any two of them. the concentration of hydrochloric acid may be, for example, but not limited to, any one of 17wt%, 18wt%, 19wt%, 20wt%, 21wt%, 22wt%, 23wt%, 24wt%, 25wt%, 26wt%, 27wt%, 28wt%, 29wt%, 30wt%, 31wt% or a range between any two thereof; the concentration of nitric acid may be, for example, but not limited to, any one of 96wt%, 96.5wt%, 97wt%, 97.5wt%, 98wt% or a range between any two thereof;
[0033] S2. Closed-circuit recycling of incomplete calcium precipitation in acid leaching solution
[0034] Sulfuric acid is added to the acid leaching solution for incomplete calcium precipitation, with the volume of sulfuric acid added being 0.1-2.5% of the volume of the acid leaching solution. After the reaction, the solution is cooled to room temperature, filtered and washed to obtain calcium sulfate and regenerated acid. The regenerated acid is returned to leach scheelite, and the remaining amount is supplemented with hydrochloric acid. Other parameters are the same as those in step S1. The resulting secondary tungstic acid is dissolved in alkali to produce an alkaline slag containing 0.2-1.5wt% WO3. Based on the important discovery that calcium sulfate has a certain solubility in a mixed solution of hydrochloric acid and calcium chloride, an incomplete calcium precipitation technology was creatively invented to treat the acid leaching solution to prepare the regenerated acid. By strictly controlling the sulfate ion concentration in the regenerated acid, the regenerated acid can be recycled to efficiently leach scheelite. If the amount of sulfuric acid added is too small, there will be insufficient sulfate particles available for reaction; if the amount of sulfuric acid added is too large, the excess sulfate will react with calcium ions to form calcium sulfate, which will react with tungstate ions during alkali dissolution to cause tungsten loss. Therefore, the volume of sulfuric acid added can be, for example but not limited to, any one of 0.1%, 0.3%, 0.5%, 0.7%, 1.0%, 1.2%, 1.5%, 1.8%, 2.0%, 2.2%, 2.5% of the volume of the acid leaching solution, or a range between any two of these.
[0035] Preferably, the method further comprises: S3. removing impurities by dissolving tungstate with ammonia
[0036] Ammonia dissolution is performed at a liquid-to-solid ratio of 3-5:1 mL / g of ammonia water to tungstic acid, with an ammonia water concentration of 3-6 wt%, room temperature, and a dissolution time of 1-2 hours. Filtering yields an ammonia slag and ammonium tungstate solution. Ammonium sulfide, magnesium sulfate, and copper sulfate are added to the ammonium tungstate solution in sequence for full reaction and impurity removal. After filtration, pure ammonium tungstate solution is obtained, which is then evaporated and crystallized to yield the ammonium paratungstate product. The ammonia slag can be discarded or recycled after treatment. Specifically, the liquid-to-solid ratio of ammonia water and tungstic acid can be, for example, but not limited to, any one of 3:1 mL / g, 3.3:1 mL / g, 3.5:1 mL / g, 3.7:1 mL / g, 4:1 mL / g, 4.2:1 mL / g, 4.5:1 mL / g, 4.8:1 mL / g, 5:1 mL / g, or a range between any two thereof; the concentration of ammonia water can be, for example, but not limited to, any one of 3 wt%, 3.5 wt%, 4 wt%, 4.5 wt%, 5 wt%, 5.5 wt%, or 6 wt%, or a range between any two thereof; the ammonia dissolution time can be, for example, but not limited to, any one of 1 h, 1 h 10 min, 1 h 20 min, 1 h 30 min, 1 h 40 min, 1 h 50 min, or 2 h, or a range between any two thereof;
[0037] Preferably, in step S1, the inner wall of the reactor is made of steel-lined PTFE material, and is provided with a heating tube and a temperature measuring device made of steel-lined PTFE material. The use of steel-lined PTFE material to prepare the reactor, heating and temperature measuring devices can not only prevent high-temperature corrosion from hydrochloric acid, but also prevent corrosion from hydrogen fluoride;
[0038] Preferably, in step S1, the leaching temperature is 60-95°C, and the leaching time is 1.5-6.0h. The present invention achieves low-temperature and thorough leaching of scheelite, improves the recovery rate of tungsten metal, and reduces the requirements of the process on equipment; specifically, the leaching temperature can be, for example, but not limited to, any one of 60°C, 65°C, 70°C, 75°C, 80°C, 85°C, 90°C, and 95°C, or a range between any two thereof; the leaching time can be, for example, but not limited to, any one of 1.5h, 2.0h, 2.5h, 3.0h, 3.5h, 4.0h, 4.5h, 5.0h, 5.5h, and 6.0h, or a range between any two thereof;
[0039] Preferably, in step S2, the concentration of concentrated sulfuric acid is 98wt%; the incomplete calcium precipitation time is 25-35min. Specifically, the incomplete calcium precipitation time can be, for example but not limited to, any one of 25min, 26min, 27min, 28min, 29min, 30min, 31min, 32min, 33min, 34min, and 35min, or a range between any two thereof.
[0040] The technical solution of the present invention is further described below with reference to specific embodiments.
[0041] The equipment in each embodiment and comparative example is a steel-lined polytetrafluoroethylene reactor, a heating and temperature measuring device, all of which are used to process a domestic scheelite concentrate, the main components of which are as follows:
[0042] Name WO3FeSiO2K2OCa Other Content / wt% 551.7100.6417.515.16 Example
[0043] A scheelite leaching method comprises the following steps:
[0044] S1. Scheelite Leaching
[0045] 200g of scheelite was placed in a reactor. 400mL of 31wt% hydrochloric acid was added according to the liquid-solid ratio of hydrochloric acid to scheelite of 2:1mL / g. 3.2mL of 98wt% sulfuric acid was then added for stirring and leaching. The leaching temperature was 95°C and the leaching time was 3.0h. After cooling and filtration, 130g of dry tungstic acid and 360mL of acid leaching solution were obtained. A small amount of tungstic acid was dissolved in alkali to obtain an alkaline slag containing 0.22wt% WO3.
[0046] S2. Closed-circuit recycling of acid leaching solution
[0047] 9 mL of 98 wt% sulfuric acid was added to 360 mL of acid leaching solution for incomplete calcium precipitation for 30 min. The solution was cooled to room temperature, filtered and washed to obtain 31 g of calcium sulfate dihydrate and 305 mL of regenerated acid solution. 200 g of scheelite, 305 mL of regenerated acid solution, 95 mL of 31 wt% hydrochloric acid and 3.2 mL of 98 wt% sulfuric acid were added to the reactor in sequence for stirring and leaching at 95 ° C for 3.0 h. The solution was cooled and filtered to obtain 131 g of dry tungstic acid and 355 mL of acid leaching solution. A small amount of tungstic acid was dissolved in alkali to obtain an alkaline slag containing 0.26 wt% WO3.
[0048] S3. Tungstate ammonia solution removal
[0049] Ammonia dissolution is performed according to a liquid-solid ratio of ammonia water to tungstic acid of 4:1 mL / g, an ammonia water concentration of 5wt%, a dissolution temperature of room temperature, and a dissolution time of 1.5 h. Ammonia slag and ammonium tungstate solution are obtained by filtration. Ammonium sulfide, magnesium sulfate, and copper sulfate are added to the ammonium tungstate solution in sequence for sufficient reaction and impurity removal. After filtration, pure ammonium tungstate solution can be obtained, which is then evaporated and crystallized to obtain the ammonium paratungstate product. Example
[0050] A scheelite leaching method comprises the following steps:
[0051] S1. Scheelite Leaching
[0052] 200g of scheelite was placed in a reactor. 400mL of 31wt% hydrochloric acid was added according to the liquid-solid ratio of hydrochloric acid to scheelite of 2:1mL / g. 2.5mL of 98wt% sulfuric acid was then added for stirring and leaching. The leaching temperature was 95°C and the leaching time was 3.0h. After cooling and filtration, 130g of dry tungstic acid and 358mL of acid leaching solution were obtained. A small amount of tungstic acid was dissolved in alkali to obtain an alkaline slag containing 0.51wt% WO3.
[0053] S2. Closed-circuit recycling of acid leaching solution
[0054] 5.4 mL of 98 wt% sulfuric acid was added to 358 mL of acid leaching solution for incomplete calcium precipitation for 30 min. The solution was cooled to room temperature, filtered and washed to obtain 18 g of calcium sulfate dihydrate and 311 mL of regenerated acid solution. 200 g of scheelite, 311 mL of regenerated acid solution, 89 mL of 31 wt% hydrochloric acid and 2.5 mL of 98 wt% sulfuric acid were added to the reactor in sequence for stirring and leaching at 95 ° C for 3.0 h. The solution was cooled and filtered to obtain 131 g of dry tungstic acid and 358 mL of acid leaching solution. A small amount of tungstic acid was alkali-dissolved to obtain an alkaline slag containing 1.21 wt% WO3.
[0055] S3. Tungstate ammonia solution removal
[0056] Ammonia dissolution is performed according to a liquid-solid ratio of ammonia water to tungstic acid of 3:1 mL / g, an ammonia water concentration of 6wt%, a room temperature, and a time of 1 h. Ammonia slag and ammonium tungstate solution are obtained by filtration. Ammonium sulfide, magnesium sulfate, and copper sulfate are added to the ammonium tungstate solution in sequence for sufficient reaction and impurity removal. After filtration, pure ammonium tungstate solution can be obtained, which is then evaporated and crystallized to obtain the ammonium paratungstate product.
[0057] A scheelite leaching method comprises the following steps:
[0058] S1. Scheelite Leaching
[0059] 200g of scheelite was placed in a reactor. 400mL of 31wt% hydrochloric acid was added according to the liquid-solid ratio of hydrochloric acid to scheelite of 2:1mL / g. 6.4mL of 98wt% sulfuric acid was then added for stirring and leaching. The leaching temperature was 95°C and the leaching time was 3.0h. After cooling and filtration, 133g of dry tungstic acid and 362mL of acid leaching solution were obtained. A small amount of tungstic acid was dissolved in alkali to obtain an alkaline slag containing 2.69wt% WO3.
[0060] S2. Closed-circuit recycling of acid leaching solution
[0061] 11 mL of 98 wt% sulfuric acid was added to 362 mL of acid leaching solution for incomplete calcium precipitation for 30 min. The solution was cooled to room temperature, filtered and washed to obtain 38 g of calcium sulfate dihydrate and 299 mL of regenerated acid solution. 200 g of scheelite, 299 mL of regenerated acid solution, 101 mL of 31 wt% hydrochloric acid, and 3.2 mL of 98 wt% sulfuric acid were added to the reactor in sequence for stirring and leaching at 95 ° C for 3.0 h. The solution was cooled and filtered to obtain 132 g of dry tungstic acid and 356 mL of acid leaching solution. A small amount of tungstic acid was alkali-dissolved to obtain an alkaline slag containing 0.25 wt% WO3.
[0062] S3. Tungstate ammonia solution removal
[0063] Ammonia dissolution is performed according to a liquid-solid ratio of ammonia water to tungstic acid of 4:1 mL / g, an ammonia water concentration of 3wt%, a dissolution temperature of room temperature, and a dissolution time of 2 h. Ammonia slag and ammonium tungstate solution are obtained by filtration. Ammonium sulfide, magnesium sulfate, and copper sulfate are added to the ammonium tungstate solution in sequence for sufficient reaction and impurity removal. After filtration, pure ammonium tungstate solution can be obtained, which is then evaporated and crystallized to obtain the ammonium paratungstate product.
[0064] A scheelite leaching method comprises the following steps:
[0065] S1. Scheelite Leaching
[0066] 200g of scheelite was placed in a reactor. 400mL of 31wt% hydrochloric acid was added according to the liquid-solid ratio of hydrochloric acid to scheelite of 2:1mL / g. 3.2mL of 98wt% sulfuric acid was then added for stirring and leaching. The leaching temperature was 75°C and the leaching time was 3.0h. After cooling and filtration, 130g of dry tungstic acid and 360mL of acid leaching solution were obtained. A small amount of tungstic acid was dissolved in alkali to obtain an alkaline slag containing 0.24wt% WO3.
[0067] S2. Closed-circuit recycling of acid leaching solution
[0068] 28 mL of 98 wt% sulfuric acid was added to 360 mL of acid leaching solution for incomplete calcium precipitation for 30 min. The solution was cooled to room temperature, filtered and washed to obtain 43 g of calcium sulfate dihydrate and 285 mL of regenerated acid solution. 200 g of scheelite, 285 mL of regenerated acid solution and 115 mL of 31 wt% hydrochloric acid were added to the reactor in sequence for stirring and leaching at 75 ° C for 3.0 h. The solution was cooled and filtered to obtain 150 g of dry tungstic acid and 350 mL of acid leaching solution. A small amount of tungstic acid was dissolved in alkali to obtain an alkaline slag containing 26.8 wt% of WO3.
[0069] S3. Tungstate ammonia solution removal
[0070] Ammonia dissolution is performed according to a liquid-solid ratio of ammonia water to tungstic acid of 4:1 mL / g, an ammonia water concentration of 5wt%, a dissolution temperature of room temperature, and a dissolution time of 1.5 h. Ammonia slag and ammonium tungstate solution are obtained by filtration. Ammonium sulfide, magnesium sulfate, and copper sulfate are added to the ammonium tungstate solution in sequence for sufficient reaction and impurity removal. After filtration, pure ammonium tungstate solution can be obtained, which is then evaporated and crystallized to obtain the ammonium paratungstate product.
[0071] A scheelite leaching method comprises the following steps:
[0072] S1. Scheelite Leaching
[0073] 200g of scheelite was placed in a reactor, and 400mL of 31wt% hydrochloric acid was added at a liquid-solid ratio of 2:1mL / g to scheelite for stirring and leaching. The leaching temperature was 95°C and the leaching time was 3.0h. After cooling and filtration, 133g of dry tungstic acid and 360mL of acid leaching solution were obtained. A small amount of tungstic acid was dissolved in alkali to obtain an alkaline slag containing 1.53wt% WO3.
[0074] S2. Closed-circuit recycling of acid leaching solution
[0075] 9 mL of 98 wt% sulfuric acid was added to 360 mL of acid leaching solution for incomplete calcium precipitation. The incomplete calcium precipitation time was 30 min. The mixture was cooled to room temperature, filtered and washed to obtain 30.5 g of calcium sulfate dihydrate and 311 mL of regenerated acid solution. 200 g of scheelite, 311 mL of regenerated acid solution, 89 mL of 31 wt% hydrochloric acid, and 2.5 mL of 98 wt% sulfuric acid were added to the reactor in sequence for stirring and leaching. The leaching temperature was 95 ° C. The leaching time was 3.0 h. The mixture was cooled and filtered to obtain 129 g of dry tungstic acid and 360 mL of acid leaching solution. A small amount of tungstic acid was alkali-dissolved to obtain an alkaline slag containing 0.68 wt% WO3.
[0076] S3. Tungstate ammonia solution removal
[0077] Ammonia dissolution is performed according to a liquid-solid ratio of ammonia water to tungstic acid of 4:1 mL / g, an ammonia water concentration of 5wt%, a dissolution temperature of room temperature, and a dissolution time of 1.5 h. Ammonia slag and ammonium tungstate solution are obtained by filtration. Ammonium sulfide, magnesium sulfate, and copper sulfate are added to the ammonium tungstate solution in sequence for sufficient reaction and impurity removal. After filtration, pure ammonium tungstate solution can be obtained, which is then evaporated and crystallized to obtain the ammonium paratungstate product.
[0078] A scheelite leaching method comprises the following steps:
[0079] S1. Scheelite Leaching
[0080] 200g of scheelite was placed in a reactor. 400mL of 31wt% hydrochloric acid was added at a liquid-solid ratio of 2:1mL / g to scheelite for stirring and leaching. The leaching temperature was 75°C and the leaching time was 3.0h. After cooling and filtration, 128g of dry tungstic acid and 353mL of acid leaching solution were obtained. A small amount of tungstic acid was dissolved in alkali to obtain an alkaline slag containing 2.47wt% WO3.
[0081] S2. Closed-circuit recycling of acid leaching solution
[0082] 18 mL of 98 wt% sulfuric acid was added to 353 mL of acid leaching solution for incomplete calcium precipitation for 30 min. The solution was cooled to room temperature, filtered and washed to obtain 59 g of calcium sulfate dihydrate and 291 mL of regenerated acid solution. 200 g of scheelite, 291 mL of regenerated acid solution and 109 mL of 31 wt% hydrochloric acid were added to the reactor in sequence for stirring and leaching at 75 ° C for 3.0 h. The solution was cooled and filtered to obtain 140 g of dry tungstic acid and 355 mL of acid leaching solution. A small amount of tungstic acid was dissolved in alkali to obtain an alkaline slag containing 5.89 wt% WO3.
[0083] S3. Tungstate ammonia solution removal
[0084] Ammonia dissolution is performed according to a liquid-solid ratio of ammonia water to tungstic acid of 4:1 mL / g, an ammonia water concentration of 5wt%, a dissolution temperature of room temperature, and a dissolution time of 1.5 h. Ammonia slag and ammonium tungstate solution are obtained by filtration. Ammonium sulfide, magnesium sulfate, and copper sulfate are added to the ammonium tungstate solution in sequence for sufficient reaction and impurity removal. After filtration, pure ammonium tungstate solution can be obtained, which is then evaporated and crystallized to obtain the ammonium paratungstate product.
[0085] A scheelite leaching method comprises the following steps:
[0086] S1. Scheelite Leaching
[0087] 200g of scheelite was placed in a reactor, and 400mL of 31wt% hydrochloric acid was added at a liquid-solid ratio of 2:1mL / g to scheelite for stirring and leaching. The leaching temperature was 75°C and the leaching time was 3.0h. After cooling and filtration, 128g of dry tungstic acid and 353mL of acid leaching solution were obtained. A small amount of tungstic acid was dissolved in alkali to obtain an alkaline slag containing 2.48wt% WO3.
[0088] S2. 200g of scheelite, 353mL of acid leaching solution, and 47mL of 31wt% hydrochloric acid were added to the reactor in sequence for stirring and leaching at 75°C for 3.0h. The mixture was cooled and filtered to obtain 152g of dry tungstic acid and 341mL of acid leaching solution. A small amount of tungstic acid was dissolved in alkali to obtain an alkaline slag containing 21.4wt% WO3.
[0089] S3. Tungstate ammonia solution removal
[0090] Ammonia dissolution is performed according to a liquid-solid ratio of ammonia water to tungstic acid of 4:1 mL / g, an ammonia water concentration of 5wt%, a dissolution temperature of room temperature, and a dissolution time of 1.5 h. Ammonia slag and ammonium tungstate solution are obtained by filtration. Ammonium sulfide, magnesium sulfate, and copper sulfate are added to the ammonium tungstate solution in sequence for sufficient reaction and impurity removal. After filtration, pure ammonium tungstate solution can be obtained, which is then evaporated and crystallized to obtain the ammonium paratungstate product.
[0091] This invention utilizes a novel low-temperature leaching method using sulfuric acid, hydrochloric acid, or nitric acid, and a new technology for the regeneration and recycling of the acid leaching solution through incomplete calcium precipitation. This technology not only achieves low-temperature, thorough leaching of scheelite, improves tungsten metal recovery, and reduces process equipment requirements, but also proposes the use of steel-lined PTFE materials for the reactor, heating tubes, and temperature measuring devices. This material is not only resistant to hydrochloric acid corrosion but also capable of processing high-fluorine scheelite and withstanding hydrogen fluoride corrosion, further improving the equipment's corrosion resistance. Furthermore, this invention successfully achieves closed-loop recycling of the acid leaching solution, significantly reducing production costs. Comparative Examples 1-5 (which do not employ the method described in this invention, without the addition of sulfuric acid) would not achieve the desired low-temperature, thorough leaching of scheelite and improved tungsten metal recovery described in this invention.
[0092] The above description is only a preferred embodiment of the present invention and does not limit the patent scope of the present invention. All equivalent structural transformations made by using the contents of the present invention specification under the inventive concept of the present invention, or direct / indirect application in other related technical fields are included in the patent protection scope of the present invention.
Claims
1. A leaching method for scheelite, characterized in that: The steps include: S1. Scheelite Leaching Take a certain amount of scheelite and place it in a reactor, add hydrochloric acid according to the liquid-solid ratio of hydrochloric acid to scheelite of 2~4:1mL / g, then add sulfuric acid or nitric acid with a volume of 0.3~1.0% of the hydrochloric acid to stir and leach, cool and filter to obtain tungstic acid and acid leaching solution; S2. Closed-circuit recycling of acid leaching solution Sulfuric acid is added to the acid leaching solution for incomplete calcium precipitation. The volume of sulfuric acid added is 0.1-2.5% of the volume of the acid leaching solution. After the reaction, it is cooled to room temperature and filtered and washed to obtain calcium sulfate and regenerated acid solution. The regenerated acid solution is returned to leaching scheelite. The insufficient part is supplemented with hydrochloric acid. Other parameters are carried out according to the process of step S1.
2. The leaching method of scheelite according to claim 1, characterized in that: The method further comprises: S3. removing impurities by dissolving in tungstate ammonia Ammonia solution is carried out according to the liquid-solid ratio of ammonia water and tungstic acid of 3~5:1mL / g, and ammonia slag and ammonium tungstate solution are obtained by filtration. Ammonium sulfide, magnesium sulfate and copper sulfate are added to the ammonium tungstate solution in sequence for sufficient reaction and impurity removal, and then filtered to obtain pure ammonium tungstate solution, and then the ammonium paratungstate product is obtained by evaporation and crystallization.
3. The leaching method of scheelite according to claim 1, characterized in that: In step S1, the concentration of hydrochloric acid is 17-31 wt %.
4. The leaching method of scheelite according to claim 1, characterized in that: In step S1, the concentration of sulfuric acid is 98 wt %, and the concentration of nitric acid is 96-98 wt %.
5. The leaching method of scheelite according to claim 1, characterized in that: In the step S1, the inner wall of the reactor is made of steel-lined polytetrafluoroethylene material, and is provided with a heating tube and a temperature measuring device made of steel-lined polytetrafluoroethylene material.
6. The leaching method of scheelite according to claim 1, characterized in that: In step S1, the leaching temperature is 60-95° C., and the leaching time is 1.5-6.0 h.
7. The leaching method of scheelite according to claim 1, characterized in that: In step S2, the concentration of sulfuric acid is 98 wt %.
8. The leaching method of scheelite according to claim 1, characterized in that: In step S2, the reaction time is 25 to 35 minutes.
9. The leaching method of scheelite according to claim 2, characterized in that: In step S3, the concentration of aqueous ammonia is 3-6 wt %.
10. The leaching method of scheelite according to claim 2, characterized in that: In step S3, the ammonia dissolution temperature is room temperature, and the ammonia dissolution time is 1 to 2 hours.
Citation Information
Patent Citations
Method for decomposing scheelite
CN111187904A
Low-grade scheelite treatment method
CN112899503A
Method for preparing ammonium paratungstate
CN113428902A
Method for leaching scheelite
CN116121566A
Extracting tungsten from ores and concentrates
US4168296A