Method and apparatus for monitoring warping of wafer in real time
By real-time monitoring of the heating power change rate and wafer warpage on the heating tray, and adjusting process conditions, the problem of wafer warp control in semiconductor chip production is solved, the uniformity of film deposition and heating efficiency are improved, and arc risks are avoided.
Patent Information
- Application Number
- PCT/CN2024/080077
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-10
- Filing Date
- 2024-03-05
- Publication Date
- 2024-10-17
AI Technical Summary
In the production process of semiconductor chips, the existing technology cannot monitor the warpage of the wafer in real time during the film formation process, making it difficult to control the film stress, which may lead to reduced heating efficiency, poor film uniformity and arc generation.
By real-time monitoring of the heating power change rate of each heating area on the heating tray and the wafer warpage change, it is determined whether the wafer is separated from the heating tray, and the process conditions are adjusted according to the mapping relationship to control the warpage within the target range.
It achieves real-time monitoring during the film deposition process, avoids the need for additional measuring machines, improves the uniformity and heating efficiency of film deposition, and reduces the risk of arcing caused by warpage.
Smart Images

Figure CN2024080077_17102024_PF_FP_ABST
Abstract
Description
Method and device for real-time monitoring of wafer warpage Technical Field
[0001] The present invention relates to the technical field of semiconductor chip manufacturing, and in particular to a method and device for real-time monitoring of wafer warping. Background Art
[0002] In the semiconductor chip production process, plasma-enhanced chemical vapor deposition (PECVD) is often used to deposit various dielectric and metal layers. A robotic arm places the wafer on a heated tray within a chamber. Reactive gases enter the chamber through a showerhead located directly above the tray. Radio frequency (RF) induces a plasma formation, which then reacts with the reacting ions on the wafer surface, forming thin films such as silicide.
[0003] During the thin film deposition process, due to the different thermal expansion coefficients of the newly formed film and the wafer substrate, stress is generated between the two, causing the wafer to warp.
[0004] When the film stress is large, especially when the film thickness is thick, the wafer will bend to a large extent and partially detach from the heating tray, the heating efficiency will be reduced, the film uniformity will deteriorate, and in severe cases, arcing may occur.
[0005] Currently, the industry mainly uses measurement equipment before and after film formation to monitor film stress and control it within a certain range, but it cannot monitor the deformation of the wafer during the film formation process in real time.
[0006] Summary of the Invention
[0007] In view of the above-mentioned problems, the object of the present invention is to provide a method and apparatus for real-time monitoring of wafer warpage, so as to monitor the wafer warpage in real time during the film forming process.
[0008] To achieve the above object, the present invention provides the following technical solutions:
[0009] A method for real-time monitoring of wafer warpage comprises: during a process of depositing a thin film on the wafer, real-time monitoring of a heating power change rate ΔP / P0 of each heating area on a heating tray, wherein ΔP is the heating power change of the heating area, and P0 is the heating power of the heating area in an initial state, the heating tray comprising at least two heating areas, each heating area being in a set constant temperature control state, the wafer being arranged on the at least two heating areas, the wafer having a wafer area corresponding to each of the heating areas; and judging, based on the heating power change rate ΔP / P0, whether the corresponding wafer area is detached from the heating tray.
[0010] The present invention also provides a method for real-time monitoring of wafer warpage, comprising: during a process of depositing a thin film on the wafer, real-time monitoring of a change in wafer warpage ΔBOW;
[0011] If the wafer warpage change ΔBOW exceeds a preset threshold, the process conditions that need to be changed are determined based on the mapping relationship between the wafer warpage change ΔBOW and the process conditions, and the wafer is processed using the changed process conditions, so that the wafer warpage is controlled within the target warpage range.
[0012] The present invention also provides a device for real-time monitoring of wafer warpage, comprising: a memory configured to store at least one mapping relationship, wherein the mapping relationship is a mapping relationship between a wafer warpage change ΔBOW and a process condition; a monitor configured to monitor the wafer warpage change ΔBOW in real time; a controller configured to receive the wafer warpage change ΔBOW, and if the wafer warpage change ΔBOW exceeds a preset threshold, determine the process condition that needs to be changed based on the mapping relationship between the wafer warpage change ΔBOW and the process condition; and an operator configured to receive the changed process condition and use the changed process condition to process the wafer.
[0013] Compared with the prior art, the present invention has the following beneficial effects:
[0014] By using this invention, the warpage of the wafer can be monitored in real time during the thin film deposition process, that is, the warpage change ΔBOW of the wafer can be monitored in real time without the need for an additional measurement machine.
[0015] Summary of the Figures
[0016] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the following briefly introduces the drawings required for use in the embodiments or the description of the prior art. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative work.
[0017] FIG1 is a flow chart of a method for real-time monitoring of wafer warpage provided in a first embodiment of the present invention.
[0018] FIG2 is a first schematic diagram of a state where a heating tray provides heating wafers according to the first embodiment of the present invention.
[0019] FIG3 is a second schematic diagram of the state of the heating tray heating the wafer provided in the first embodiment of the present invention.
[0020] FIG4 is a third schematic diagram of the state of the heating tray heating the wafer provided in the first embodiment of the present invention.
[0021] FIG5 is a fitting curve diagram showing the relationship between the change in heating power of the inner heating coil and the outer heating coil and the warpage according to the first embodiment of the present invention.
[0022] FIG6 is a flow chart of a method for real-time monitoring of wafer warpage provided by a second embodiment of the present invention.
[0023] FIG7 is a schematic diagram of a thin film deposition device provided in the second embodiment of the present invention.
[0024] 8 to 13 are diagrams showing the relationship between film stress and process conditions according to the second embodiment of the present invention.
[0025] Preferred embodiments of the present invention
[0026] To more clearly illustrate the technical solutions of the embodiments of this application, the following is a brief introduction to the drawings required for describing the embodiments. Obviously, the drawings described below are merely examples or embodiments of this application. Those skilled in the art can apply this application to other similar scenarios based on these drawings without inventive effort. Unless otherwise apparent from the context or otherwise noted, the same reference numerals in the figures represent the same structure or operation.
[0027] As used in this application and the claims, unless the context clearly indicates otherwise, the words "a," "an," "an," and / or "the" are not intended to refer to the singular but may include the plural. Generally speaking, the terms "comprises" and "include" only indicate the inclusion of the steps and elements specifically identified, and these steps and elements do not constitute an exclusive list. A method or apparatus may also include other steps or elements.
[0028] Unless otherwise specifically stated, the relative arrangement of the parts and steps, numerical expressions and numerical values set forth in these embodiments do not limit the scope of the present application. At the same time, it should be understood that, for ease of description, the sizes of the various parts shown in the drawings are not drawn according to actual proportional relationships. The techniques, methods and equipment known to those of ordinary skill in the relevant art may not be discussed in detail, but where appropriate, the techniques, methods and equipment should be considered as part of the authorization specification. In all examples shown and discussed here, any specific values should be interpreted as being merely exemplary and not as limitations. Therefore, other examples of the exemplary embodiments may have different values. It should be noted that similar numbers and letters represent similar items in the following figures, and therefore, once an item is defined in one figure, it does not need to be further discussed in subsequent figures.
[0029] In the description of this application, it should be understood that the directions or positional relationships indicated by directional words such as "front, back, up, down, left, right", "horizontal, vertical, vertical, horizontal" and "top, bottom" are usually based on the directions or positional relationships shown in the accompanying drawings. They are only for the convenience of describing this application and simplifying the description. Unless otherwise specified, these directional words do not indicate or imply that the device or element referred to must have a specific direction or be constructed and operated in a specific direction. Therefore, they cannot be understood as limiting the scope of protection of this application; the directional words "inside and outside" refer to the inside and outside relative to the outline of each component itself.
[0030] For ease of description, spatially relative terms such as "above", "above", "on the upper surface of", "above", etc. may be used herein to describe the spatial positional relationship of a device or feature to other devices or features as shown in the figures. It should be understood that spatially relative terms are intended to include different orientations of the device in use or operation in addition to the orientation described in the figures. For example, if the device in the drawings is inverted, the device described as "above other devices or structures" or "above other devices or structures" will be positioned as "below other devices or structures" or "below other devices or structures". Thus, the exemplary term "above" can include both "above" and "below". The device can also be positioned in other different ways (rotated 90 degrees or in other orientations), and the spatially relative descriptions used here are interpreted accordingly.
[0031] Furthermore, it should be noted that the use of terms such as "first" and "second" to define components is solely for the purpose of distinguishing the corresponding components. Unless otherwise stated, these terms have no special meaning and therefore should not be construed as limiting the scope of protection of this application. Furthermore, while the terms used in this application are selected from commonly known and commonly used terms, some terms mentioned in this specification may have been selected by the applicant at his or her discretion, and their detailed meanings are explained in the relevant sections of this description. Furthermore, this application should be understood not only by the actual terms used, but also by the meaning implied by each term.
[0032] The technical solution of the present invention will be further described below with reference to the accompanying drawings and through specific implementation methods.
[0033] Example 1
[0034] Referring to FIG. 1 , this embodiment provides a method for real-time monitoring of wafer warpage. The method of this embodiment includes the following steps:
[0035] Step S110: During the thin film deposition process on the wafer, monitoring in real time the heating power change rate ΔP / P0 of each heating zone on the heating tray, wherein ΔP is the heating power change of the heating zone, and P0 is the heating power of the heating zone in the initial state, the heating tray includes at least two heating zones, each heating zone is in a set constant temperature control state, the wafer is placed on the at least two heating zones, and the wafer has a wafer area corresponding to each heating zone; and
[0036] Step S120 : determining whether the corresponding wafer area is out of the heating tray according to the heating power change rate ΔP / P0.
[0037] The above-mentioned step S110 and step S120 are explained below in conjunction with Figures 2 to 5. Continuing to refer to Figure 2, during the thin film deposition process, the wafer 2 is located on the heating tray 1, and the heating tray 1 heats the wafer 2. The heating tray 1 includes a central heating area 11 and an edge heating area 12, and the edge heating area 12 is arranged on the periphery of the central heating area 11. The heating tray 1 heats the wafer 2 in a dual-zone manner. The edge heating area 12 includes an external heating coil for heating the portion of the wafer located on the edge heating area 12, and the central heating area 11 includes an internal heating coil for heating the portion of the wafer located on the central heating area 11. The edge heating area 12 and the central heating area 11 are combined to heat the entire wafer 2. The internal heating coil and the external heating coil dynamically adjust the heating power so that each heating area of the heating tray 1 is in a set constant temperature control state.
[0038] For example, if the temperature of the heating area is lower or higher than the set temperature, the heating power is increased or decreased through the relay.
[0039] During the thin film deposition process, when the wafer 2 does not warp, as shown in FIG2 , the wafer 2 is flat as a whole, the center of the wafer 2 contacts the center heating area 11 , and the edge of the wafer 2 contacts the edge heating area 12 .
[0040] However, when the wafer 2 warps, some parts of the wafer will detach from the heating tray 1, that is, they will not be in contact with the heating tray 1. The method for real-time monitoring of wafer warpage in this embodiment determines the warpage state of the wafer based on the heating power change rate ΔP(C) / P0(C) of the central heating area 11 and the heating power change rate ΔP(E) / P0(E) of the edge heating area 12. Among them, ΔP(C) represents the heating power change corresponding to the central heating area, ΔP(E) represents the heating power change corresponding to the edge heating area, P0(C) is the heating power corresponding to the central heating area in the initial state, and P0(E) is the heating power corresponding to the edge heating area in the initial state.
[0041] Referring to FIG3 , if the edge of the wafer 2 has less contact with the edge heating area 12 of the heating tray 1 , the load of the external heating coil decreases to maintain the set temperature, and the heating power of the edge heating area 12 decreases. The heating power of the central heating area 11 remains unchanged, and |ΔP(C) / P0(C)|<|ΔP(E) / P0(E)|, resulting in an upward bowl-shaped warp of the wafer 2.
[0042] Referring to Figure 4 , if the center of wafer 2 decreases contact with central heating zone 11 of heating tray 1, the load on the internal heating coils decreases, and the heating power in central heating zone 11 decreases, with |ΔP(C) / P0(C)| > |ΔP(E) / P0(E)|, causing wafer 2 to warp downward, forming an inverted bowl shape. It should be noted that the magnitude of the change in heating coil heating power varies depending on the degree of wafer 2 warpage.
[0043] In this application, the BOW value is used to represent the warpage of the wafer 2. The warpage state of the wafer 2 can be distinguished by the positive or negative value of the wafer warpage BOW. Referring to Figures 3 and 4, assuming that the upper surface of the wafer 2 is the front side and the lower surface is the back side, the warpage state of the wafer 2 includes: the edge of the wafer 2 is bent toward its back side and the middle is convex, that is, the wafer 2 is warped downward, and the wafer warpage BOW value is defined as negative, as shown in Figure 4; or the edge of the wafer 2 is bent toward its front side and the middle is concave, that is, the wafer 2 is warped upward, and the wafer warpage BOW value is defined as positive, as shown in Figure 3.
[0044] Exemplarily, the heating tray 1 is not limited to including two heating zones, and the heating tray 1 may include multiple heating zones, each heating zone being used to heat the wafer 2 .
[0045] According to steps S110 and S120, the method disclosed in this application monitors the heating power change rate ΔP / P0 of each heating zone in real time, and determines whether the portion of wafer 2 corresponding to the heating zone has detached from heating tray 1 based on the heating power change rate ΔP / P0. For example, based on the magnitude of the heating power change rate ΔP / P0, when the heating power change rate ΔP / P0 is less than a certain value, it indicates that the portion of wafer 2 has detached from heating tray 1.
[0046] In some embodiments, if ΔP / P0 of a certain heating area is less than 0, it indicates that the heating power of the heating area has changed, which means that the wafer portion corresponding to the heating area has separated from the heating tray 1 .
[0047] In the embodiments disclosed herein, the warpage of the wafer 2 is not limited to the two states described above. For example, the overall warpage of the wafer 2 is determined based on the heating power change rate ΔP / P0 across all heating zones. The warpage of the wafer 2 may be saddle-shaped or other irregular shapes.
[0048] Further research found that there is a corresponding relationship between the heating power change rate ΔP / P0 in the heating area and the wafer warpage change ΔBOW. The wafer warpage change ΔBOW is calculated by the corresponding relationship ΔP(C) / P0(C)=f1′(ΔBOW), ΔP(E) / P0(E)=f2′(ΔBOW), where f1′ represents the relationship between ΔP(C) / P0(C) and ΔBOW, and f2′ represents the relationship between ΔP(E) / P0(E) and ΔBOW. f1′ and f2′ can be a function, such as a linear function, a quadratic function, etc., and this application does not impose any restrictions on this. If ΔBOW exceeds a preset threshold, a reminder signal is triggered to the controller. After receiving the reminder signal, the controller can adjust the wafer warpage.
[0049] Exemplarily, the wafer warpage variation ΔBOW is the difference between the current wafer warpage and the initial warpage of wafer 2. The heating power variation ΔP is the difference between the heating power of the current heating area and the heating power of the initial heating area.
[0050] The above correspondence is established based on experimental results. The experiment may include the following steps:
[0051] Taking the heating tray 1 including the central heating area 11 and the edge heating area 12 as an example, the heating tray 1 and the wafer 2 are arranged in the chamber, and the wafer 2 without thin film deposition is placed on the heating tray 1. After the temperature of the wafer 2 stabilizes to the target process temperature and the chamber stabilizes to the target process temperature, target pressure, target airflow and other conditions, the average heating power of the inner heating coil and the outer heating coil of the heating tray 1 within a certain period of time is collected: P0′(C) and P0′(E). At this time, the wafer 2 is in a flat state, and its wafer warpage BOW0 value is 0, where P0′(C) can be the heating power corresponding to the central heating area in the initial state, and P0′(E) can be the heating power corresponding to the edge heating area in the initial state;
[0052] A silicon nitride film of known thickness is deposited on wafer 2. Wafer 2 is then bent upward (or downward). The wafer warpage BOW1 is known. After wafer 2 stabilizes to target process temperature, target pressure, target airflow, and other conditions, the average heating power of the inner and outer heating coils of heating tray 1 over a certain period of time is measured: P1(C) and P1(E).
[0053] A second layer of the same silicon nitride film is deposited on wafer 2. At this point, the wafer warpage BOW2 is known. The average heating power of the inner and outer heating coils of heating tray 1 over a certain period of time is collected: P2(C) and P2(E).
[0054] By analogy, we can obtain the BOW of wafer 2 after depositing n layers of known film. nIt is known that the average heating power P of the inner heating coil and the outer heating coil of the heating tray 1 within a certain period of time is collected. n (C) and P n (E).
[0055] Referring to Figure 5, a fitting procedure reveals the relationship between the heating power of the internal and external heating coils of the heating tray 1 and the change in the wafer bow (BOW): P(C) = f1(BOW) and P(E) = f2(BOW). Here, f1 represents the relationship between P(C) and BOW, and f2 represents the relationship between P(E) and BOW. Both f1 and f2 can be functions, such as linear or quadratic functions, and this application does not impose any restrictions on this. It should be noted that f1′ is different from f1, and f2′ is different from f2.
[0056] During the thin film deposition process, the heating power of heating tray 1 is not only affected by the change in heat transfer caused by the warpage of wafer 2, but also by the thermal effects of the plasma field, chemical reaction, flow field, and thermal field acting on wafer 2 during the PECVD process deposition process, which will cause changes in the heating power of heating tray 1. After the thermal effects are in a stable state, the thermal effects brought by the plasma field, chemical reaction, flow field, and thermal field tend to be constant. At this time, the change in the heating power of heating tray 1 is mainly affected by the change in the wafer warpage BOW value. When taking the thermal effects into account, the relationship between the heating power of the internal and external heating coils of heating tray 1 and the change in the wafer warpage BOW value is expressed as:
[0057] P(C)=f1(BOW)+C1 and P(E)=f2(BOW)+C2, where C1 and C2 are the heating power constants of the influence of plasma field, chemical reaction, flow field and thermal field on the central heating area 11 and the edge heating area 12 respectively.
[0058] It should be noted that the wafer thin film deposition process of the present method includes a PECVD process deposition process. During this process, each time a thin film is deposited, the plasma field, chemical reaction, flow field, and thermal field act on the wafer 2, which will cause a thermal impact. The heat release during the thin film deposition process is divided into three stages: the first deposition fluctuation stage, the deposition film stability stage, and finally the second deposition fluctuation stage. The thermal impact in a stable state here refers to the deposition film stability stage. According to these embodiments, only when it is determined that the thin film deposition reaction is in the deposition film stability stage is step S110 of real-time monitoring the heating power change rate ΔP / P0 of each heating area on the heating tray 1 performed.
[0059] In some embodiments, the wafer thin film deposition process of the present method includes a CVD process deposition process, in which a thin film is deposited once, and the chemical reaction, flow field, and thermal field acting on the wafer 2 will bring about thermal effects. After the thin film deposition reaction stabilizes, the thermal effects brought about by the chemical reaction, flow field, and thermal field tend to be constant. At this time, the change in the heating power of the heating tray 1 is mainly affected by the change in the wafer warpage BOW value. According to these embodiments, when it is determined that the thin film deposition reaction is in the stable stage of depositing the thin film, the step of real-time monitoring the heating power change rate ΔP / P0 of each heating area on the heating tray 1 is performed. P(C)=f1(BOW)+C3 and P(E)=f2(BOW)+C4, where C3 and C4 are the heating power constants of the effects of chemical reaction, flow field, and thermal field on the central heating area 11 and the edge heating area 12, respectively.
[0060] During the CVD deposition process, heat release during thin film deposition occurs in three stages: the first deposition fluctuation stage, the deposited film stability stage, and finally the second deposition fluctuation stage. The term "thermal influence in a stable state" refers to the deposited film stability stage.
[0061] To obtain the change in heating power, the current heating power P is subtracted from the initial heating power P0, so that the constant terms C1 to C4 in the above formula are eliminated, thereby eliminating the thermal effects of plasma field, chemical reaction, flow field, thermal field, etc.
[0062] Exemplarily, ΔP(C)=(f1(BOW)+C1)−(f1(BOW0)+C1)=f1(BOW)−f1(BOW0), where BOW0 is the initial warpage of the wafer 2 .
[0063] Since ΔP(C) / P0(C)=f1′(ΔBOW),
[0064] f1′(ΔBOW)=(f1(BOW)−f1(BOW0)) / P0(C) is an example of the relationship between f1 and f1′.
[0065] During the film deposition process, starting from the stable stage of film deposition, the heating power P(E) of the central heating area and the heating power P(C) of the edge heating area are read every x seconds. This allows real-time monitoring of ΔP(C) / P0(C) and ΔP(E) / P0(E). The corresponding relationship ΔP(C) / P0(C) = f1′(ΔBOW) and ΔP(E) / P0(E) = f2′(ΔBOW) is obtained. The wafer bow change ΔBOW is calculated from ΔP(C) and ΔP(E). If ΔBOW exceeds a preset threshold, an alert signal is triggered to the controller. Here, f1′ represents the relationship between ΔP(C) / P0(C) and ΔBOW, and f2′ represents the relationship between ΔP(E) / P0(E) and ΔBOW.
[0066] In summary, the method for monitoring wafer warpage does not require an additional measurement machine, and directly utilizes the changes in the heating power of the inner heating coil and the outer heating coil of the heating tray 1 to calculate the wafer warpage change ΔBOW in real time.
[0067] In some embodiments, when the wafer warpage change ΔBOW exceeds a preset threshold, a reminder signal is triggered to the controller. The method of the present application also determines the process conditions that need to be changed based on the mapping relationship between the wafer warpage change ΔBOW and the process conditions, and processes the wafer according to the changed process conditions, so that the wafer warpage is controlled within the target warpage range.
[0068] Example 2
[0069] This embodiment provides a method for real-time monitoring of the warpage of a wafer 2, as shown in FIG6 , the method comprising the following steps:
[0070] Step S210: During the process of depositing a thin film on the wafer, real-time monitoring of a change in wafer warpage ΔBOW;
[0071] Step S220: If the wafer warpage change ΔBOW exceeds a preset threshold, the process conditions that need to be changed are determined based on the mapping relationship between the wafer warpage change ΔBOW and the process conditions, and the wafer is processed using the changed process conditions, so that the wafer warpage is controlled within the target warpage range.
[0072] When the warpage of the wafer 2 is within the target warpage range, the overall stress distribution of the wafer 2 is relatively uniform, and the wafer 2 is relatively flat, which can ensure the smooth progress of subsequent semiconductor manufacturing processes. The warpage of the wafer 2 is represented by the BOW value.
[0073] The following uses a thin film deposition device as an example to schematically illustrate the method for adjusting the warpage of the wafer 2 provided in the present application.
[0074] Referring to FIG. 7 , the thin film deposition apparatus includes: a chamber for performing thin film deposition; a gas supply assembly 3 for supplying process gas into the chamber; a heating tray 1 disposed below the gas supply assembly 3 for supporting and heating a wafer 2; and an RF source for providing RF power to excite the process gas within the chamber to dissociate into plasma and form a plasma field 4, which deposits the thin film on the wafer 2. The present application does not limit the location of the gas supply assembly 3; in some embodiments, the gas supply assembly 3 may be disposed on the ceiling of the chamber.
[0075] In step S220 , the mapping relationship between the wafer warpage variation ΔBOW and the process conditions includes a first corresponding relationship and a second corresponding relationship, wherein the first corresponding relationship is the relationship between the wafer warpage variation ΔBOW and the film stress.
[0076] For example, the wafer bow variation ΔBOW is positively correlated with the absolute value of the film stress, that is, ΔBOW increases as the film stress increases.
[0077] The second corresponding relationship is the relationship between film stress (Stress) and process conditions.
[0078] For example, when a thin film is deposited on wafer 2, the film stress can be divided into tensile stress and compressive stress. If the wafer 2 warps upward, the corresponding film stress is tensile stress; if the wafer 2 warps downward, the corresponding film stress is compressive stress.
[0079] For example, if the wafer 2 is warped downward, the wafer warpage BOW is defined as a negative value; if the wafer 2 is warped upward, the wafer warpage BOW is defined as a positive value.
[0080] The process conditions in step S220 include but are not limited to any one or more combinations of gas flow rate, RF power, chamber pressure, gas composition ratio, film deposition time, terminal matching parameters, and the spacing between the gas supply assembly 3 and the wafer 2.
[0081] Exemplary terminal matching parameters include, but are not limited to, adjustable capacitance (C), a frequency matcher, etc. By changing the potential of the heating tray 1 through the adjustable capacitance (C), the potential difference between the gas supply assembly 3 and the heating tray 1 is adjusted, thereby adjusting the distribution and energy of the plasma field 4 in the chamber, thereby changing the impact force of the plasma on the wafer 2. When the plasma deposits thin films on the wafer 2, the film stress changes.
[0082] The frequency matcher is mounted on the rear end of the RF source, and is adjusted to match the frequency of the RF source's transmitting power source with the frequency of the chamber.
[0083] For example, the film stress is positively correlated with the film deposition time. That is, the longer the film deposition time is and the thicker the film layer is, the greater the corresponding film stress is.
[0084] Different film qualities (silicon nitride / silicon oxide / a-Si / carbon, etc.), different processes, and different component ratios (recipes) have different response directions and sensitivities to process conditions.
[0085] For example, in the second correspondence, the film stress may vary with changes in process conditions. The relationship between the film stress and the process conditions may be a linear relationship. Of course, the relationship between the film stress and the process conditions may also be a nonlinear relationship, depending on the influence of the process conditions on the film stress.
[0086] Taking silicon nitride films as an example, a silicon nitride film is formed by filling a chamber with silane (SiH4), ammonia (NH3), and nitrogen (N2) at a specific ratio and flow rate. The chamber then maintains a set pressure and temperature, and radio frequency (RF) is used to form a plasma, which then forms a film. Experiments are conducted by adjusting process conditions, and the stress and refractive index (RI) of the film are monitored in real time. Stress and refractive index (RI) are both film properties. When depositing a specific film, the purpose of adjusting process conditions is to change the stress, but the refractive index (RI) of the film remains unchanged. See Figures 8-13 for details. Stress is measured in MPa.
[0087] As shown in Figure 8, film stress (Stress) is positively correlated with SiH4 flow rate, increasing with increasing SiH4 flow rate. The refractive index (RI) is also positively correlated with SiH4 flow rate, increasing with increasing SiH4 flow rate. The unit of flow rate is sccm, and the units for the following different gases are the same.
[0088] As shown in Figure 9, there is a positive correlation between film stress and NH3 flow rate, that is, film stress increases with increasing NH3 flow rate. There is a negative correlation between refractive index (RI) and NH3 flow rate.
[0089] As shown in Figure 10, there is a negative correlation between film stress and N2 flow rate, that is, film stress decreases as N2 flow rate increases. There is a positive correlation between refractive index (RI) and N2 flow rate.
[0090] As shown in Figure 11, film stress is negatively correlated with RF power, meaning that film stress decreases as RF power increases. Refractive index (RI) is positively correlated with RF power. RF power is measured in watts (W).
[0091] As shown in Figure 12, film stress (Stress) and chamber pressure (Pressure) are positively correlated, meaning that film stress (Stress) increases with increasing chamber pressure. Refractive index (RI) and chamber pressure are negatively correlated. Chamber pressure is measured in Torr.
[0092] As shown in Figure 13, film stress is positively correlated with the distance (Spacing) between the gas supply assembly 3 and wafer 2. That is, film stress increases with increasing Spacing. Refractive index (RI) is negatively correlated with Spacing. The unit of distance is mil.
[0093] By leveraging the relationship between film stress and process conditions, the film stress is adjusted, thereby adjusting the wafer bow variation ΔBOW. For example, if the wafer bow variation ΔBOW exceeds a preset threshold, the film stress can be reduced by reducing the SiH4 flow rate and the spacing. This can shift the film stress from tensile to compressive, thereby reducing the wafer bow variation ΔBOW or even achieving ΔBOW = 0 while maintaining the RI constant.
[0094] In addition to film stress and refractive index (RI), other film properties include etch rate (ER), extinction coefficient (EC), and dielectric constant (k). By experimentally studying the relationship between these properties and process conditions, when it is necessary to adjust film stress without changing other properties, the required process conditions can be calculated based on these relationships.
[0095] In some embodiments, before the step S210 of real-time monitoring of the wafer warpage variation ΔBOW, the method further includes: acquiring a wafer warpage BOW value in real time, and obtaining the wafer warpage variation ΔBOW according to the wafer warpage BOW value.
[0096] During the process of depositing thin films on wafers, a first film layer and a second film layer are alternately deposited to form a stacked structure. The first film layer has tensile stress and the second film layer has compressive stress. The wafer warpage BOW value is obtained in real time, and the warpage of the stacked structure is adjusted by adjusting the film deposition time to change the thickness of one of the film layers.
[0097] Exemplarily, the first film layer is a SiN film layer, and the second film layer is a SiO2 film layer. When the wafer warpage BOW value is positive, the average thickness of the subsequent SiO2 film layer is increased or the average thickness of the subsequent SiN film layer is decreased; when the wafer warpage BOW value is negative, the average thickness of the subsequent SiN film layer is increased or the average thickness of the subsequent SiO2 film layer is decreased, so that the wafer warpage is controlled within the target warpage range.
[0098] It should be noted that the first film layer is a film layer having tensile stress, and the second film layer is a film layer having compressive stress. The first film layer and the second film layer may include multiple film layers or a single film layer, and the number of film layers is not limited here.
[0099] In an optional embodiment, the heating tray 1 includes at least two heating zones. In step S210 , the wafer warpage variation ΔBOW is monitored according to the heating power variation rate ΔP / P0 of the heating zones.
[0100] Exemplarily, the heating tray 1 includes a central heating area 11 and an edge heating area 12, and the edge heating area 12 is arranged on the periphery of the central heating area 11. Step S210 is specifically implemented as follows: real-time monitoring of the heating power change rate ΔP(C) / P0(C) of the central heating area 11 and the heating power change rate ΔP(E) / P0(E) of the edge heating area 12, and judging the warping state of the wafer 2 according to ΔP(C) / P0(C) and ΔP(E) / P0(E); if |ΔP(C) / P0(C)|>|ΔP(E) / P0(E)|, it is judged that the edge of the wafer 2 is bent toward its back side and convex in the middle, that is, bent downward; if |ΔP(C) / P0(C)|<|ΔP(E) / P0(E)|, it is judged that the edge of the wafer 2 is bent toward its front side and concave in the middle, that is, bent upward.
[0101] The wafer warpage change ΔBOW is calculated from the corresponding relationship ΔP(C) / P0(C)=f1′(ΔBOW), ΔP(E) / P0(E)=f2′(ΔBOW). If ΔBOW exceeds a preset threshold, a reminder signal is triggered to the controller.
[0102] In some embodiments, after receiving the reminder signal, the controller activates a film forming process condition adjustment program. When the film forming process condition adjustment program is executed, it is used to obtain the mapping relationship between the wafer warpage change ΔBOW and the process conditions, and determine the process conditions that need to be changed based on the mapping relationship. The wafer 2 is processed using the changed process conditions, so that the warpage of the wafer 2 is controlled within the target warpage range.
[0103] In an optional embodiment, the heating tray 1 includes an electrostatic chuck, the process conditions in step S220 include the voltage of the electrostatic chuck, and the method further includes: changing the voltage of the electrostatic chuck according to the wafer warpage change ΔBOW, thereby improving the wafer warpage.
[0104] Exemplarily, the adsorption force of the heating tray 1 on the wafer 2 is increased by increasing the voltage of the electrostatic chuck, so as to improve the warping state of the wafer 2 on the heating tray 1 .
[0105] In summary, during the deposition of the thin film, the warpage state of the wafer 2 in the chamber is monitored in real time. If the change in the wafer warpage ΔBOW exceeds the preset threshold, the film forming process condition adjustment program is automatically activated to change the warpage state of the wafer 2, thereby avoiding the deterioration of the film quality and arcing caused by the warpage of the wafer 2. Since the thicker the film layer, the more likely it is to warp, the method of real-time monitoring of the warpage of the wafer 2 is of greater significance for films with high film stress and high thickness. Compared with Example 1, the technical solution of Example 2 not only obtains the wafer warpage and its change, but also adjusts the process conditions according to these results to improve the wafer warpage.
[0106] Example 3
[0107] Corresponding to the method for real-time monitoring of the warpage of the wafer 2 provided in the second embodiment, this embodiment provides a device for real-time monitoring of the warpage of the wafer 2. The device for monitoring the warpage of the wafer 2 includes a memory, a monitor, a controller, and an operator.
[0108] The memory is configured to store at least one mapping relationship, where the mapping relationship is a mapping relationship between a wafer warpage variation ΔBOW and a process condition.
[0109] Exemplarily, a device for real-time monitoring of the warpage of the wafer 2 is used in a thin film deposition process, and the process conditions include any one or more combinations of gas flow, RF power, chamber pressure, gas composition ratio, terminal matching parameters, and the distance between the gas supply assembly 3 and the wafer 2.
[0110] The thin film deposition process is achieved with the aid of a thin film deposition apparatus. The thin film deposition apparatus includes: a chamber for thin film deposition; a gas supply assembly 3 for supplying process gas into the chamber; a heating tray 1 disposed below the gas supply assembly 3 for supporting and heating the wafer 2; and an RF source for providing RF power to excite the process gas in the chamber to dissociate into plasma gas, which then deposits the thin film on the wafer 2.
[0111] Exemplarily, the mapping relationship includes a first corresponding relationship and a second corresponding relationship, and the memory is further configured to store the first corresponding relationship and the second corresponding relationship.
[0112] The first corresponding relationship is the relationship between the wafer warpage variation ΔBOW and the film stress, and the second corresponding relationship is the relationship between the film stress and the process conditions.
[0113] The monitor is configured to monitor a wafer bow variation ΔBOW.
[0114] Exemplarily, the monitor is configured to monitor the heating power change rate ΔP / P0 of each heating area on the heating tray, and determine the corresponding wafer warpage change ΔBOW based on the heating power change rate ΔP / P0 of each area, wherein ΔP is the heating power change of the heating area, and P0 is the heating power of the heating area in the initial state. The heating tray includes at least two heating areas, each heating area is in a set constant temperature control state, and the wafer is set on at least two heating areas, and the wafer has a wafer area corresponding to each heating area.
[0115] The controller is configured to receive information from the monitor, the information including the wafer warpage variation ΔBOW, and then activate the film forming process condition adjustment program and determine the changed process conditions according to the corresponding mapping relationship.
[0116] Exemplarily, the monitor is connected to the controller via an electrical signal. The mapping relationships include a plurality of mapping relationships, and the controller determines a mapping relationship to be used from the plurality of mapping relationships, thereby determining the process conditions to be changed according to the mapping relationship.
[0117] The operator is configured to receive the changed process conditions from the controller and process the wafer 2 using the changed process conditions.
[0118] Exemplarily, the operator is electrically connected to the controller. After receiving the changed process conditions, the operator inputs the corresponding process conditions into the thin film deposition apparatus. Adjusting the process conditions changes the film stress, thereby changing the warpage of the wafer 2.
[0119] In summary, during the thin film deposition process, the warping of wafer 2 is monitored in real time. If the change in wafer warping ΔBOW exceeds a preset threshold, the pre-set film forming process condition adjustment program is activated, the corresponding mapping relationship is called, and the film forming process conditions are calculated and changed, thereby changing the subsequent film stress, so that the warping of wafer 2 can be controlled, and the warped wafer 2 can even be restored to a flat state by using the opposite film stress.
[0120] The basic concepts have been described above. It will be apparent to those skilled in the art that the above disclosures are merely illustrative and do not constitute limitations on this application. Although not explicitly stated herein, those skilled in the art may make various modifications, improvements, and amendments to this application. Such modifications, improvements, and amendments are suggested in this application and remain within the spirit and scope of the exemplary embodiments of this application.
[0121] At the same time, this application uses specific terms to describe the embodiments of this application. For example, "one embodiment," "an embodiment," and / or "some embodiments" refer to a certain feature, structure, or characteristic related to at least one embodiment of this application. Therefore, it should be emphasized and noted that "one embodiment," "an embodiment," "an alternative embodiment," or "exemplary" mentioned twice or multiple times in different locations in this specification do not necessarily refer to the same embodiment. In addition, certain features, structures, or characteristics in one or more embodiments of this application may be appropriately combined.
[0122] Similarly, it should be noted that, in order to simplify the presentation of this application and thus facilitate understanding of one or more embodiments of the invention, the foregoing descriptions of the embodiments of this application sometimes combine multiple features into a single embodiment, figure, or description thereof. However, this disclosure method does not mean that the subject matter of this application requires more features than those recited in the claims. In fact, an embodiment may have fewer features than all of the features of a single embodiment disclosed above.
Claims
1. A method for real-time monitoring of wafer warpage, characterized in that: include: During the process of depositing a thin film on a wafer, a heating power change rate ΔP / P0 of each heating area on the heating tray is monitored in real time, wherein ΔP is the heating power change amount of the heating area, and P0 is the heating power of the heating area in the initial state, the heating tray comprises at least two heating areas, each heating area is in a set constant temperature control state, the wafer is arranged on the at least two heating areas, and the wafer has a wafer area corresponding to each of the heating areas; as well as It is determined according to the heating power change rate ΔP / P0 whether the corresponding wafer area is out of the heating tray.
2. The method for real-time monitoring of wafer warpage according to claim 1, characterized in that: The step of judging whether the corresponding wafer area is separated from the heating tray according to the heating power change rate ΔP / P0 includes: when the heating power change rate ΔP / P0 is less than 0, the wafer area corresponding to the corresponding heating area is separated from the heating tray.
3. The method for real-time monitoring of wafer warpage according to claim 1, characterized in that: The at least two heating regions include a central heating region and an edge heating region, wherein the edge heating region is arranged at the periphery of the central heating region; The step of judging whether the corresponding wafer area is out of the heating tray according to the heating power change rate ΔP / P0 comprises: If |ΔP(C) / P0(C)|>|ΔP(E) / P0(E)|, it is judged that the edge of the wafer is bent toward its back side and convex in the middle; if |ΔP(C) / P0(C)|<|ΔP(E) / P0(E)|, it is judged that the edge of the wafer is bent toward its front side and concave in the middle, wherein ΔP(C) represents the change in heating power corresponding to the central heating area, ΔP(E) represents the change in heating power corresponding to the edge heating area, P0(C) is the heating power corresponding to the central heating area in the initial state, and P0(E) is the heating power corresponding to the edge heating area in the initial state.
4. The method for real-time monitoring of wafer warpage according to claim 3, characterized in that: Also includes: Obtain the correspondence between the heating power change rate ΔP / P0 and the wafer warpage change ΔBOW, and obtain the wafer warpage change ΔBOW corresponding to the current heating power change rate ΔP / P0 according to the correspondence. If the wafer warpage change ΔBOW exceeds a preset threshold, trigger a reminder signal to the controller.
5. The method for real-time monitoring of wafer warpage according to claim 4, characterized in that: The corresponding relationship includes: ΔP(C) / P0(C)=f1′(ΔBOW) and ΔP(E) / P0(E)=f2′(ΔBOW), wherein f1′ represents the relationship between ΔP(C) / P0(C) and ΔBOW, and f2′ represents the relationship between ΔP(E) / P0(E) and ΔBOW.
6. The method for real-time monitoring of wafer warpage according to claim 1, characterized in that: The process of depositing a thin film on a wafer includes a PECVD process deposition process. Before the step of real-time monitoring the heating power change rate ΔP / P0 of each heating area on the heating tray, it also includes: determining that the thermal effects of the plasma field, chemical reaction, flow field, and thermal field on the heating tray are in a stable state.
7. The method for real-time monitoring of wafer warpage according to claim 1, characterized in that: The process of depositing a thin film on a wafer includes a CVD process deposition process. Before the step of real-time monitoring the heating power change rate ΔP / P0 of each heating area on the heating tray, it also includes: determining that the thermal effects of chemical reactions, flow fields, and thermal fields on the heating tray are in a stable state.
8. The method for real-time monitoring of wafer warpage according to claim 4, characterized in that: After receiving the reminder signal, the controller determines the process conditions that need to be changed based on the mapping relationship between the wafer warpage change ΔBOW and the process conditions, and processes the wafer according to the changed process conditions, so that the wafer warpage is controlled within the target warpage range.
9. A method for real-time monitoring of wafer warpage, characterized in that: include: During the process of depositing thin films on wafers, the change in wafer warpage ΔBOW is monitored in real time; If the wafer warpage change ΔBOW exceeds a preset threshold, the process conditions that need to be changed are determined based on the mapping relationship between the wafer warpage change ΔBOW and the process conditions, and the wafer is processed using the changed process conditions, so that the wafer warpage is controlled within the target warpage range.
10. The method for real-time monitoring of wafer warpage according to claim 9, characterized in that: The mapping relationship includes a first corresponding relationship and a second corresponding relationship, wherein: The first corresponding relationship includes the relationship between the wafer warpage variation ΔBOW and film stress, and the second corresponding relationship includes the relationship between the film stress and the process conditions.
11. The method for real-time monitoring of wafer warpage according to claim 9, characterized in that: The step of real-time monitoring the wafer warpage change ΔBOW includes: real-time monitoring the heating power change rate ΔP / P0 of each heating area on the heating tray, and real-time monitoring the wafer warpage change ΔBOW according to the heating power change rate ΔP / P0, wherein the heating tray includes at least two heating areas, each heating area is in a set constant temperature control state, the wafer is arranged on the at least two heating areas, the wafer has a wafer area corresponding to each of the heating areas, ΔP is the heating power change of the heating area, and P0 is the heating power of the heating area in the initial state.
12. The method for real-time monitoring of wafer warpage according to claim 11, characterized in that: The at least two heating regions include a central heating region and an edge heating region, wherein the edge heating region is arranged at the periphery of the central heating region; The steps of real-time monitoring of the wafer warpage variation ΔBOW also include: If |ΔP(C) / P0(C)|>|ΔP(E) / P0(E)|, it is judged that the edge of the wafer is bent toward its back side and convex in the middle; if |ΔP(C) / P0(C)|<|ΔP(E) / P0(E)|, it is judged that the edge of the wafer is bent toward its front side and concave in the middle, wherein ΔP(C) / P0(C) represents the heating power change rate corresponding to the central heating area, ΔP(E) / P0(E) represents the heating power change rate corresponding to the edge heating area, P0(C) is the heating power corresponding to the central heating area in the initial state, and P0(E) is the heating power corresponding to the edge heating area in the initial state.
13. The method for real-time monitoring of wafer warpage according to claim 12, characterized in that: Also includes: Obtain the correspondence between the heating power change rate ΔP / P0 and the wafer warpage change ΔBOW, and obtain the wafer warpage change ΔBOW corresponding to the current heating power change rate ΔP / P0 according to the correspondence. If the wafer warpage change ΔBOW exceeds a preset threshold, trigger a reminder signal to the controller.
14. The method for real-time monitoring of wafer warpage according to claim 13, characterized in that: The corresponding relationship includes: ΔP(C) / P0(C)=f1′(ΔBOW) and ΔP(E) / P0(E)=f2′(ΔBOW), wherein f1′ represents the relationship between ΔP(C) / P0(C) and ΔBOW, and f2′ represents the relationship between ΔP(E) / P0(E) and ΔBOW.
15. The method for real-time monitoring of wafer warpage according to claim 9, characterized in that: The process conditions include one or any combination of gas flow rate, radio frequency power, chamber pressure, gas composition ratio, terminal matching parameters, and film deposition time.
16. The method for real-time monitoring of wafer warpage according to claim 11, characterized in that: The heating tray is arranged below a gas supply assembly, and the gas supply assembly is used to supply process gas deposited on the surface of the wafer; the process conditions include the distance between the gas supply assembly and the wafer.
17. The method for real-time monitoring of wafer warpage according to claim 9, characterized in that: Before the step of real-time monitoring the wafer warpage variation ΔBOW, the method further includes: acquiring a wafer warpage BOW value in real time, and obtaining the wafer warpage variation ΔBOW according to the wafer warpage BOW value.
18. The method for real-time monitoring of wafer warpage according to claim 17, characterized in that: During the process of depositing a thin film on a wafer, a first film layer and a second film layer are alternately deposited to form a stacked structure, the first film layer has tensile stress, and the second film layer has compressive stress. The method also includes: when the wafer warpage BOW value is positive, increasing the average thickness of the subsequent second film layer or reducing the average thickness of the subsequent first film layer; when the wafer warpage BOW value is negative, increasing the average thickness of the subsequent first film layer or reducing the average thickness of the subsequent second film layer, so that the wafer warpage is controlled within the target warpage range.
19. The method for real-time monitoring of wafer warpage according to claim 18, characterized in that: The first film layer is a SiN film layer, and the second film layer is a SiO2 film layer.
20. The method for real-time monitoring of wafer warpage according to claim 10, characterized in that: The wafer warpage variation ΔBOW is positively correlated with the absolute value of the film stress.
21. The method for real-time monitoring of wafer warpage according to claim 10, characterized in that: The process conditions include film deposition time, and the film stress is positively correlated with the film deposition time.
22. The method for real-time monitoring of wafer warpage according to claim 11, characterized in that: The heating tray includes an electrostatic chuck, the process conditions include a voltage of the electrostatic chuck, and the method further includes: adjusting the voltage of the electrostatic chuck according to the wafer warpage variation ΔBOW.
23. A device for real-time monitoring of wafer warpage, characterized in that: include: A memory configured to store at least one mapping relationship, wherein the mapping relationship is a mapping relationship between a wafer warpage variation ΔBOW and a process condition; A monitor configured to monitor the wafer warpage variation ΔBOW in real time; A controller configured to receive the wafer warpage variation ΔBOW, and if the wafer warpage variation ΔBOW exceeds a preset threshold, determine the process conditions that need to be changed according to a mapping relationship between the wafer warpage variation ΔBOW and the process conditions; The operator is configured to receive the changed process conditions and process the wafer using the changed process conditions.
24. The device for real-time monitoring of wafer warpage according to claim 23, characterized in that: The mapping relationship includes a first corresponding relationship and a second corresponding relationship; The first corresponding relationship includes the relationship between the wafer warpage change ΔBOW and the film stress, The second corresponding relationship includes the relationship between the film stress and the process condition.
25. The device for real-time monitoring of wafer warpage according to claim 23, characterized in that: The monitor is configured to monitor the heating power change rate ΔP / P0 of each heating area on the heating tray, and determine the corresponding wafer warpage change ΔBOW according to the heating power change rate ΔP / P0 of each area, wherein ΔP is the heating power change of the heating area, and P0 is the heating power of the heating area in the initial state. The heating tray includes at least two heating areas, each heating area is in a set constant temperature control state, and the wafer is arranged on the at least two heating areas, and the wafer has a wafer area corresponding to each of the heating areas.
Citation Information
Patent Citations
Method for detecting abnormal placement state of substrate, substrate processing method, computer-readable storage medium and substrate processing apparatus
CN101990707A
Wafer processing apparatus and wafer processing method using the same
CN112309894A
Heat treatment system
JP1999329940A
Cited By
Wafer adsorption system and wafer adsorption method
CN119170553A
Stress monitoring method and monitoring device for wafer thinning sheet, and semiconductor process equipment
CN119901399A
Film coating equipment compatible with whole area and subarea
CN120776280A
Wafer warping correction device
CN121548253A