Method for producing polypeptide molecule by means of energy radiation

Through the light radiation activation of the plasmon catalyst on the nano-substrate structure, the one-step preparation of peptide molecules is realized, which solves the complexity and environmental protection issues of the artificial peptide synthesis process, improves the yield and the efficiency of industrial flue gas utilization, and provides A low-cost path to mass production of peptides.

WO2024213116A1PCT designated stage expired Publication Date: 2024-10-17BEIJING GUANGHE ORIGINAL TECH CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
PCT/CN2024/087496
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-13
Filing Date
2024-04-12
Publication Date
2024-10-17

AI Technical Summary

Technical Problem

The existing synthetic peptide process is complex, costly, not environmentally friendly, and difficult to mass-produce. Moreover, the solid-phase synthesis method has many steps, many by-products, and difficult to guarantee the yield, making it difficult to effectively utilize the resources in industrial flue gas.

Method used

Plasmon catalysts are used to combine nano-substrate structures with atomic sites through light radiation, activating nitrogen-containing sources, hydrogen-containing sources and carbon-containing sources to achieve one-step preparation of peptide molecules, reducing the difficulty of processing and purification, and controlling Light intensity and wavelength increase yield.

Benefits of technology

It simplifies the synthesis steps, reduces costs, increases the yield of peptide molecules, provides the possibility of low-cost, mass production of peptides, and uses industrial flue gas resources to simplify the separation and purification process.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure PCTCN2024087496-FTAPPB-I100001
    Figure PCTCN2024087496-FTAPPB-I100001
  • Figure 00000018_0000
    Figure 00000018_0000
  • Figure 00000018_0001
    Figure 00000018_0001
Patent Text Reader

Abstract

A method for producing a polypeptide molecule by means of energy radiation. The method comprises: bringing a composite catalyst into contact with at least one hydrogen-containing source, at least one carbon-containing source, and at least one nitrogen-containing source; and energy-radiating the composite catalyst, the hydrogen-containing source, the carbon-containing source, and the nitrogen-containing source so as to produce a polypeptide molecule. Wherein the composite catalyst comprises at least one nano-substrate structure and at least one atomic site, the atomic site comprising one or more of the chemical elements Mn, Co, Fe, Ru, Rh, Al, Ag, Au, Pt, Pd, Cu, Ni, Zn, Ti, Os, Ir and La.
Need to check novelty before this filing date? Find Prior Art

Description

Method for producing polypeptide molecules by energy radiation Technical Field

[0001] The present invention relates to a method for catalytically producing polypeptide molecules through energy radiation. Background Art

[0002] Peptides (or "polypeptides") are naturally occurring small biological molecules composed of two or more amino acids, preferably α-amino acid residues. Typically, amino acid molecules are arranged linearly, with the carboxyl group of one amino acid residue and the amino group of the next or adjacent amino acid forming a peptide bond through a condensation reaction, ultimately linking them together. The substances referred to by peptides and proteins overlap to a certain extent. Peptides are substances between amino acids and proteins, formed by the condensation of amino acids, but do not have the three-dimensional structure of proteins.

[0003] Peptides play an important role in various life activities in organisms and are primarily obtained through protein hydrolysis reactions in organisms. With the advancement of science and technology, research on synthetic peptides has been carried out for over 40 years.

[0004] Currently, artificial peptide synthesis is primarily achieved through organic synthesis. Solid-phase synthesis is a commonly used method for the organic synthesis of peptides and proteins. The process involves steps such as coupling and deprotection, and reactions can only proceed stepwise. The yield of each step affects the overall yield of the final product. Therefore, this synthesis process is subject to the common constraints of multi-step organic reactions: numerous steps, resulting in numerous byproducts and difficult-to-guarantee yields. The solvents and intermediates used in the reaction also complicate the isolation and purification of the final product. Furthermore, the process is subject to high costs, environmental concerns, and difficulties in mass production.

[0005] Research on plasmon effects has been ongoing for nearly a century. Plasmon catalysts can significantly enhance local energy on nanostructured surfaces, activating relatively stable molecules (such as carbon dioxide, nitrogen, and water) under relatively mild conditions. This cleaves covalent bonds within the molecules and causes the resulting elements to rearrange as free radicals, generating new substances. Substances proven to produce plasmon effects are primarily metals (including transition metals, noble metals, and rare earth metals) and their corresponding oxides.

[0006] Since its recent introduction, the concept of single-atom catalysis has garnered widespread attention and research. With the development of advanced characterization techniques, single-atom catalysts have made it possible to elucidate the structure-activity relationship of catalysts at the atomic and molecular levels, and to bridge heterogeneous and homogeneous catalysis. Due to their unique structure, single-atom catalysts exhibit activity, selectivity, and stability that differ from conventional nanocatalysts.

[0007] The present invention unexpectedly discovered that by using a single-atom catalyst that can produce a plasmon effect, under the condition of controlling the reaction temperature, a nitrogen-containing source, a hydrogen-containing source and a carbon-containing source, preferably an inorganic carbon-containing source, can be activated and recombined in one step to generate polypeptide molecules (or "peptide molecules") through steps that are much simpler than existing technical methods such as solid-phase synthesis methods. This makes it possible to prepare polypeptides by non-organic synthesis means, greatly reducing the difficulty of processing and purification.

[0008] The present invention also found that when the light radiation intensity and wavelength are preferably controlled, peptide molecules can be obtained with higher efficiency and / or yield, providing a possible path for future low-cost and mass production of polypeptides.

[0009] Summary of the Invention

[0010] Based on the technical problems existing in the background technology, the present invention clarifies a new plasmon catalysis technology, which includes atomic sites, such as single atomic sites and / or atomic clusters containing 2-25 atoms, and provides a unique method for preparing polypeptide molecules by light radiation using N2 and CO or CO2 from industrial flue gas or atmosphere in the presence of a cost-effective catalyst.

[0011] One aspect of the present invention is a method for producing polypeptide molecules by energy radiation, comprising:

[0012] The composite catalyst is contacted with at least one hydrogen-containing source, at least one carbon-containing source and at least one nitrogen-containing source, and energy is irradiated to the composite catalyst, the hydrogen-containing source, the carbon-containing source and the nitrogen-containing source to produce polypeptide molecules, wherein the composite catalyst comprises at least one nano-based structure and at least one atomic site, and the atomic site comprises one or more chemical elements selected from the group consisting of Mn, Co, Fe, Ru, Rh, Al, Ag, Au, Pt, Pd, Cu, Ni, Zn, Ti, Os, Ir and La.

[0013] In a preferred embodiment of the present invention, the energy radiation is light radiation.

[0014] In a preferred embodiment of the present invention, the energy radiation is such that the reaction is carried out at a temperature between about 0°C and about 80°C, preferably about 0°C to about 60°C, about 0°C to about 40°C, about 2°C to about 40°C, about 5°C to about 40°C, about 10°C to about 40°C, about 10°C to about 35°C.

[0015] In a preferred embodiment of the present invention, the optical radiation power of the optical radiation is 10-1500 mW / m 2 , preferably 10-500mW / m 2 , most preferably 100-200mW / m2 .

[0016] In a preferred embodiment of the present invention, the wavelength of the optical radiation is from about 250 nm to about 1000 μm, preferably from 400 nm to about 1000 μm, most preferably from 750 nm to about 500 μm, and preferably from about 900 nm to about 15 μm.

[0017] In a preferred embodiment of the present invention, the polypeptide molecule is a molecule comprising two or more amino acids, and the amino acids are natural amino acids or non-natural amino acids.

[0018] In a preferred embodiment of the present invention, the distance between the nano-base structure and the atomic site is less than or equal to 5 nm, preferably less than or equal to 1 nm, more preferably less than 0.1 nm, and most preferably the two are in close contact.

[0019] In a preferred embodiment of the present invention, the atomic sites are bound to the nano-based structure, for example, physically or chemically.

[0020] In a preferred embodiment of the present invention, the mass percentage of the atomic sites to the nano-based structure is less than or equal to 50%, preferably 0.01% to 30%, preferably 0.01% to 5%, more preferably 0.1% to 2%, and most preferably 0.1% to 1%.

[0021] In a preferred embodiment of the present invention, the atomic sites are loaded on the surface of the nano-based structure, the internal pores, or distributed in the internal lattice of the nano-based structure. Preferably, the atomic sites are evenly distributed, and the interval between the atomic sites is 0.2-500nm, preferably 1-50nm, and more preferably 1-10nm.

[0022] In a preferred embodiment of the present invention, the nano-based structure is selected from the group consisting of Mn, Co, Ce, Fe, Al, Ca, Ce, Cu, Ni, Ti, Zn, Si, Mo, Bi, V, C, N and their oxides, nitrides, sulfides, carbides, hydroxides, chlorides and metal-organic frameworks (MOFs), preferably metal-organic frameworks, TiO2 or Al2O3.

[0023] In a preferred embodiment of the present invention, the composite catalyst is a catalyst loaded with Co and Mn or bound to a metal organic framework, a catalyst loaded with Fe or bound to Al2O3, a catalyst loaded with Co or bound to Al2O3, a catalyst loaded with Ru or bound to Al2O3, a catalyst loaded with Ru and Fe or bound to Al2O3, or a catalyst loaded with Ru and Co or bound to Al2O3.

[0024] In a preferred embodiment of the present invention, at least one dimension of the length, width, and height of the nano-base structure is about 1 nm to about 1000 nm, preferably about 70 nm to about 1000 nm, about 100 nm to about 800 nm, or about 200 nm to about 500 nm.

[0025] In a preferred embodiment of the present invention, the nano-based structures are each independently about 1 nm to about 3000 nm in length, width and height, preferably, the length is about 100 nm to about 3000 nm, about 500 nm to about 2500 nm, or about 1000 nm to about 2000 nm, and / or the width or height is about 1 nm to about 1000 nm, about 70 nm to about 1000 nm, about 100 nm to about 800 nm, or about 200 nm to about 500 nm, or the nano-based structures each independently have an aspect ratio of about 1 to about 20, preferably about 1 to about 10, or about 2 to about 8.

[0026] In a preferred embodiment of the present invention, the shape of the nano-based structure is sphere, spike, flake, needle, blade, column, polyhedron, three-dimensional cone, cube, sheet, hemisphere, irregular three-dimensional shape, porous structure or any combination thereof.

[0027] In a preferred embodiment of the present invention, the plurality of atomic sites are arranged in a pattern on the nano-base structure, preferably in a multi-layer arrangement, or the plurality of atomic sites are randomly dispersed in and / or on the surface of the nano-base structure.

[0028] In a preferred embodiment of the present invention, the carbon source is C 1-4 A hydrocarbon or non-organic carbon source, wherein the non-organic carbon source is selected from the group consisting of CO2, CO, synthesis gas, bicarbonate and any combination thereof, or air, industrial flue gas, tail gas or emission containing one or more of these carbon sources, and the carbon source is preferably CO2 and CO.

[0029] In a preferred embodiment of the present invention, the hydrogen source is selected from water, H2, C 1-4 The group consisting of hydrocarbons and any combination thereof, or air, industrial flue gas, tail gas or emission containing more than one of these hydrogen-containing sources, preferably water.

[0030] In a preferred embodiment of the present invention, the nitrogen source includes nitrogen, nitrates, nitrogen oxides and any combination thereof, or air, industrial flue gas, tail gas or emissions containing more than one of these nitrogen sources, preferably nitrogen. BRIEF DESCRIPTION OF THE DRAWINGS

[0031] FIG1 shows a transmission electron microscope (TEM) image of the Co-Al2O3 composite catalyst.

[0032] FIG2 shows a transmission electron microscope (TEM) image of the Fe-Al2O3 composite catalyst.

[0033] FIG3 shows the HPLC-MS spectrum of the product in Example 2.

[0034] FIG4 shows the HPLC-MS spectrum of the product in Example 3.

[0035] FIG5 shows the HPLC-MS spectrum of the product in Example 4. DETAILED DESCRIPTION

[0036] The present invention demonstrates that, unexpectedly, N2, water and CO2 or CO can be converted into polypeptide molecules in the presence of a composite catalyst with plasmonic action using light radiation as energy input.

[0037] Before further describing the present invention, the following sections collect certain terms used in the specification, examples, and appended claims. The definitions listed herein should be read and understood by those skilled in the art in light of the remainder of the present invention. Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by those of ordinary skill in the art to which this invention belongs.

[0038] definition

[0039] As used herein, the term "catalyst" refers to a substance that increases the rate of a chemical reaction by reducing the activation energy of the reaction. This rate-increasing effect is known as "catalysis." Catalysts are not consumed in catalyzing reactions, so they can continue to catalyze further reactions of the reactants in small quantities.

[0040] As used herein, the term "plasmon donor" refers to a conductor whose real part of the dielectric constant is negative. When excited by electromagnetic radiation, a plasmon donor can provide surface plasmons.

[0041] As used herein, the term "chemical element" refers to a chemical substance composed of atoms with the same number of protons in their nuclei. Specifically, a chemical element is one listed in the periodic table of chemical elements. Chemical elements include both naturally occurring and synthetic elements. Chemical elements also include yet-to-be-discovered elements with more than 118 protons in their nuclei.

[0042] The terms "binding" or "loading" used in this article refer to physical or chemical binding or loading on the surface, internal pores or internal lattice, where physical methods include van der Waals forces, metallic bonds and other conventional physical binding methods, and chemical methods include ionic bonds, covalent bonds, coordination bonds and other conventional chemical binding methods.

[0043] As used herein, the term "alloy" refers to a mixture of metals or a mixture of metals and other elements. An alloy is defined by the properties of the metallic bonding. An alloy can be a solid solution of a metallic element (a single phase) or a mixture of two or more metallic phases (a solution of two or more).

[0044] As used herein, the term "metal-organic framework (MOF)" refers to an organic-inorganic hybrid material with intramolecular pores or a metal-organic framework structure with a periodic network structure formed by self-assembly of organic ligands and metal ions or clusters. MOFs may contain transition metals, rare earth metals, main group metals such as alkali metals and alkaline earth metals, and the like as metallic elements, for example, Cu, Zn, Cd, Fe, Ti, Mn, Al, and Co, preferably Ti, and may also contain non-metallic elements such as O, N, S, P, and halogens (e.g., F, Cl, Br, I). MOFs can be prepared by methods known in the art, such as solvent evaporation, diffusion, hydrothermal or solvothermal methods, ultrasound, and microwave methods.

[0045] The term "specific catalyst activity" as used herein refers to the number of moles of product produced per unit mass of active catalyst per unit time under certain reaction conditions. Specifically, specific catalyst activity = number of moles of reaction product / mass of active catalyst / reaction time.

[0046] The term "close contact" used herein means that there is substantially no gap between the two, for example, the distance between the two is less than or equal to 1 nm, less than or equal to 0.1 nm, or substantially 0 nm, preferably forming a metallic bond or a coordination bond.

[0047] The term "C 1-4 “Hydrocarbons” include C1, C2, C3 and C4 hydrocarbons, such as methane, ethane, n-propane, isopropane, n-butane and isobutane.

[0048] As used herein, the term "peptide" or "polypeptide" refers to a molecule composed of two or more amino acid residues, preferably α-amino acid residues, linked together. As used herein, the term "peptide" or "polypeptide" preferably refers to a molecule having the following structure: amino acid molecules, preferably α-amino acid molecules, are arranged linearly, and the carboxyl group of one amino acid residue and the amino group of the next or adjacent amino acid are linked together by a condensation reaction to form a peptide bond.

[0049] As used herein, the term "amino acid" refers to conventional amino acids (also known as natural amino acids) or non-natural amino acids (any type of non-oligomeric compound containing an amino group and a carboxyl group that is not a conventional amino acid). The non-natural amino acid may be a molecule formed by substituting a natural amino acid.

[0050] In the case of an amino acid containing more than one amino and / or carboxyl group, all orientations of the amino acid are possible in principle, but in the case of α-amino acids, it is preferred to utilize α-amino and α-carboxyl groups, other preferred orientations being explicitly indicated. Unless otherwise indicated, amino acid sequences are presented herein in an N-terminal to C-terminal direction.

[0051] Amino acids may exist in either the L or D configuration.

[0052] As used herein, when "about" is followed by a value or ratio, it means ±10%, preferably ±5%, and more preferably ±1% of such value or ratio.

[0053] Plasmonic composite catalysts

[0054] One aspect of the present invention is a plasmon composite catalyst that generates polypeptide molecules through light radiation.

[0055] Without wishing to be bound by theory, the plasmonic composite catalyst of the present invention interacts with the raw materials in the reaction to lower the activation energy of the reaction, thereby enabling the reaction to be initiated by light irradiation and increasing the reaction rate.

[0056] The plasmonic composite catalyst of the present invention comprises two structures: atomic sites and a nano-based structure, wherein the atomic sites and the nano-based structure are in contact with each other. In a preferred embodiment, the mass percentage of the atomic sites and the nano-based structure in the plasmonic composite catalyst is less than or equal to 50%, preferably 0.01% to 30%, preferably 0.01% to 5%, more preferably 0.1% to 2%, and most preferably 0.1% to 1%.

[0057] Atomic sites

[0058] The term "atomic site" as used in the present invention refers to mutually independent metal single atoms and / or mutually independent atomic clusters comprising 2-25, preferably 2-20 metal atoms, wherein the metal single atoms and / or the atomic clusters are stably bound or loaded on the surface of the nano-substrate structure and / or in the internal pores and / or internal lattice, preferably uniformly distributed on the nano-substrate structure, more preferably uniformly distributed on the surface of the nano-substrate structure. The atoms in the metal single atoms or the atomic clusters exist in a valence state between 0 valence and the highest valence state normally present in the metal, and the average valence state of the metal atoms is, for example, 0 to +4 valence, or 0 to +3 valence, or 0 to +2 valence, or 0 to +1 valence, preferably 0 valence. The interatomic distance in the atomic clusters is less than 1 nm, preferably 0.1-0.5 nm.

[0059] The atoms in the atomic sites are combined with the atoms in the nano-based structure by physical or chemical means, such as van der Waals forces, metallic bonds and other conventional physical bonding methods, or ionic bonds, covalent bonds, coordination bonds and other conventional chemical bonding methods, such as forming alloys through metallic bonds, or forming complexes through coordination bonds.

[0060] When the atomic sites are independent single metal atoms, the interactions between the metal atoms and the atoms in the nanostructured substrate can prevent the metal atoms from agglomerating, making them more stable. In some embodiments, within the catalytic metal single atom sites, all catalytic metals exist as isolated atoms, i.e., the dispersion of the catalytic metal atoms is 100%, which maximizes the utilization of the catalytic metal atoms. Preferably, all catalytic metal atoms are directly fixed to the surface of the nanostructured substrate, forming 100% of the interface atoms, which maximizes the utilization of the metal-substrate interface interactions to optimize catalytic performance.

[0061] When the atomic sites are independent metal atom clusters, the metal atom clusters are physically or chemically combined with the atoms in the nano-based structure, and the metal atom clusters are stably dispersed on and / or in the nano-based structure.

[0062] When the atomic site is a single atom of a single metal element, in some embodiments, the single metal element acts as both a plasmon donor and a catalytic property donor, and the nano-based structure provides physical support; in other embodiments, the single metal element acts as a plasmon donor, and the nano-based structure provides physical support and serves as a catalytic property donor.

[0063] When the atomic sites are metal atomic clusters, in some embodiments, some atomic clusters containing specific elements act as plasmon donors, other atomic clusters containing specific elements act as catalytic property donors, and the nano-based structure provides physical support; in other embodiments, the atomic clusters act as plasmon donors, and the nano-based structure provides physical support and acts as a catalytic property donor.

[0064] In other embodiments, the atomic sites and the nano-based structure act together as both plasmon donors and catalytic property donors, and the nano-based structure provides physical support.

[0065] Nanostructured substrate

[0066] As used herein, the term "nanosubstrate structure" refers to a structure having a size range of the nanometer scale, i.e., at least one of the length, width, and height dimensions is from about 1 nm to about 1000 nm, preferably from about 70 nm to about 1000 nm, from about 100 nm to about 800 nm, or from about 200 nm to about 500 nm. A nanosubstrate structure can have a dimension exceeding 1000 nm, for example, having a length in the micrometer scale range, such as 1 μm to 5 μm. In some cases, tubular objects and fibers having only two dimensions in the nanometer range are also considered nanosubstrate structures. Materials having nanosubstrate structures can exhibit size-related properties that are significantly different from those observed in bulk materials.

[0067] The nanobase structures of the present invention each independently have a length, width, and height of about 1 nm to about 3000 nm. Preferably, the length is about 100 nm to about 3000 nm, more preferably about 500 nm to about 2500 nm, and even more preferably about 1000 nm to about 2000 nm. Preferably, the width or height is about 1 nm to about 1000 nm, preferably about 70 nm to about 1000 nm, more preferably about 100 nm to about 800 nm, and even more preferably about 200 nm to about 500 nm.

[0068] The nano-based structures of the present invention each independently have an aspect ratio (i.e., the ratio of length to width / height) of about 1 to about 20, preferably an aspect ratio of about 1 to about 10, or about 2 to about 8. The nano-based structures of the present invention can also have a relatively low aspect ratio, for example, about 1 to about 2.

[0069] The nano-based structures of the present invention each independently have the following shapes: sphere, spike, flake, needle, blade, column, polyhedron, three-dimensional cone, cube, sheet, hemisphere, irregular three-dimensional shape, porous structure or any combination thereof.

[0070] The nano-based structure is selected from the group consisting of Mn, Co, Ce, Fe, Al, Ca, Ce, Cu, Ni, Ti, Zn, Si, Mo, Bi, V, C, N and their oxides, nitrides, sulfides, carbides, hydrocarbon molecular oxides, chlorides and metal organic frameworks.

[0071] The term "nano-based structure" as used herein comprises more than 25, preferably more than 30 atoms.

[0072] The present invention can be a plurality of nano-base structures arranged in a patterned manner on a substrate, preferably in a multi-layer arrangement, or a plurality of nano-base structures can be randomly dispersed in a medium. For example, the nano-base structures can be attached to a substrate. In this case, the nano-base structures generally do not aggregate with each other, but are arranged or stacked in a regular pattern. Alternatively, a plurality of nano-base structures can be dispersed in a liquid medium, wherein each nano-base structure can move freely relative to the other nano-base structures.

[0073] For example, the nano-based structure can have a spike-like or blade-like geometry. Optionally, the nano-based structure is a flake-like geometry with a relatively thin thickness. Preferably, the nano-based structure has a nano-jungle, nano-grass, and / or nano-snowflake structure. The nano-based structure can have a relatively large aspect ratio, such that the nano-based structure can adopt the structure of nano-spikes, nano-snowflakes, or nano-needles. The aspect ratio can be from about 1 to about 20, from about 1 to about 10, or from about 2 to about 8. Preferably, the length of the nano-based structure can be from about 100 nm to about 3000 nm, from about 500 nm to about 2500 nm, or from about 1000 nm to about 2000 nm; the width or height can be from about 1 nm to about 1000 nm, from about 70 nm to about 1000 nm, from about 100 nm to about 800 nm, or from about 200 nm to about 500 nm.

[0074] The nanostructures can be bound to a matrix. Thus, the nanostructures are generally not aggregated together, but arranged in an ordered manner. The matrix can be formed of a metal or a polymer material (e.g., polyimide, PTFE, polyester, polyethylene, polypropylene, polystyrene, polyacrylonitrile, etc.).

[0075] In other examples, the nano-based structures have a spherical, cylindrical, polyhedral, three-dimensional pyramidal, cubic, plate-like, hemispherical, irregular three-dimensional shape, porous structure or any combination thereof. Such nano-based structures are each independently about 1 nm to about 1000 nm in length, width, and height, about 70 nm to about 1000 nm, about 100 nm to about 800 nm, or about 200 nm to about 500 nm.

[0076] In addition, the plasmon atom catalyst of the present invention can function in various states, such as dispersed, aggregated, or attached / grown on the surface of other materials. In a preferred embodiment, the plasmon atom catalyst is dispersed in a medium, which is preferably a reactant of the reaction, such as water.

[0077] Methods for producing polypeptide molecules

[0078] Another aspect of the present invention is a method for producing polypeptide molecules by light radiation, comprising the following steps:

[0079] A plasmon composite catalyst is contacted with at least one hydrogen source, at least one carbon source, and at least one nitrogen source; and the plasmon composite catalyst, the hydrogen source, the carbon source, and the nitrogen source are irradiated with light to produce polypeptide molecules.

[0080] Under the catalytic action of the plasmonic composite catalyst, energy radiation, i.e., light radiation, triggers the reaction for synthesizing polypeptide molecules. Without wishing to be bound by theory, the plasmonic composite catalyst is capable of converting and transferring the energy of the light radiation, thereby enabling the reaction of the present invention to proceed continuously. Within a specific temperature range, maintaining a lower temperature can result in a higher energy conversion rate for producing polypeptide molecules.

[0081] The light irradiation step is carried out at a temperature between about 0°C and about 80°C, preferably between about 0°C and about 60°C, about 0°C and about 40°C, about 2°C and about 40°C, about 5°C and about 40°C, about 10°C and about 40°C, about 10°C and about 35°C, etc. At the above temperature, the unit catalyst activity of producing polypeptide molecules is greater than 0.04 μg·g -1 ·h -1 , greater than 0.34 μg·g in the preferred temperature range -1 ·h -1 .

[0082] In the reaction of the present invention, light radiation simulates the wavelength composition and intensity of sunlight, so it can increase the temperature of the irradiated catalyst and reaction mixture to achieve the effect of activating the reactants. During the reaction, a heat preservation device is used to maintain the temperature of the reaction system within a certain range (not higher than 80°C, preferably not higher than 60°C, and most preferably not higher than 40°C). When the radiation intensity reaches a certain level, the plasmon composite catalyst, hydrogen source, carbon source and nitrogen source are activated by light radiation. Preferably, light radiation is the only source of activation of the initial reactants.

[0083] In the reaction of the present invention, after the reaction is started, the reaction continues under light radiation. The term "light" as used herein refers to electromagnetic waves with a wavelength between about 250nm and about 1000μm. In other words, light refers to radiation of visible light or infrared light. Preferably, in the reaction of the present invention, the light radiation power is much lower than the solar radiation power (i.e., the solar constant). For example, the light radiation power is 10-1500mW / m 2 , preferably 10-500mW / m 2 , most preferably 100-200mW / m 2The light radiation can be sunlight (optionally filtered through a filter to obtain an infrared light portion), or an infrared light portion obtained by filtering other light sources through a filter, or light emitted by an artificial light source. The wavelength of the light radiation is between about 250 nm and about 1000 μm, preferably in the infrared radiation wavelength range, that is, a wavelength of about 750 nm to about 500 μm, preferably about 900 nm to about 15 μm. In other words, the present invention uses light with a longer wavelength, that is, lower energy, to enable the reaction to proceed smoothly and generate a polypeptide comprising at least two amino acids.

[0084] The reaction time varies depending on the size of the reaction, radiation intensity, temperature, and other factors. The reaction is carried out continuously using a complete apparatus and with the continuous addition of a hydrogen-containing source and a carbon-containing source. The reaction time can be 0.1 hours or more, preferably 0.1 hours to 1000 hours, preferably 0.1 hours to 800 hours, preferably 0.5 hours to 600 hours, preferably 1 hour to 500 hours, preferably 2 hours to 300 hours, and most preferably 4 hours to 250 hours.

[0085] The reaction can be carried out under low pressure, normal pressure or high pressure, and the appropriate reaction pressure can be selected according to the size of the reaction, radiation intensity, temperature and other factors. For example, the reaction pressure can be at least 1 bar, such as 1 bar to 30 bar, preferably 1 bar to 20 bar, and more preferably 1.5 bar to 5 bar.

[0086] Reaction raw materials

[0087] The carbon source is C 1-4 A hydrocarbon or non-organic carbon source, wherein the non-organic carbon source is selected from the group consisting of CO2, CO, synthesis gas, bicarbonate and any combination thereof, or air, industrial flue gas, tail gas or emission containing one or more of these carbon sources, and the carbon source is preferably CO2 and CO.

[0088] The hydrogen source is selected from water, H2, C 1-4 The group consisting of hydrocarbons and any combination thereof, or air, industrial flue gas, tail gas or emission containing more than one of these hydrogen-containing sources, preferably water.

[0089] The nitrogen source is selected from the group consisting of N2, nitrogen oxides, hydrogen nitrates and any combination thereof, or air, industrial flue gas, tail gas or emissions containing more than one of these nitrogen sources, preferably N2.

[0090] As can be seen from the above-mentioned reaction raw materials, the carbon-containing source, hydrogen-containing source and nitrogen-containing source that can be used in the present invention are widely present in industrial waste gas, wastewater, flue gas, combustion emissions and automobile exhaust, etc., so they can be used as the reaction raw materials of the present invention, thereby facilitating the recycling of industrial waste.

[0091] In addition, the present invention makes it possible to efficiently prepare polypeptide molecules from non-organic carbon-containing sources.

[0092] Furthermore, the present invention prepares polypeptide molecules in a one-step reaction, eliminating the multi-step reaction and complicated treatment and purification steps in the prior art, and provides a cost-effective method for preparing polypeptide molecules.

[0093] Reaction products

[0094] The reaction of the present invention can produce polypeptide molecules. In a preferred embodiment, the polypeptide molecule is a molecule comprising two or more amino acids, for example, a molecule comprising two, three, four, five or more amino acids; the amino acids are natural amino acids or non-natural amino acids, including but not limited to glycine (Gly, G), alanine (Ala, A), valine (Val, V), leucine (Leu, L), isoleucine (Ile, I), methionine (Met, M), proline (Pro, P), tryptophan (Trp, W), serine (Ser, S), tyrosine (Tyr, Y), cysteine ​​(Cys, C), phenylalanine (Phe, F), asparagine (Asn, N), glutamine (Gln, Q), threonine (Thr, T), aspartic acid (Asp, D), glutamic acid (Glu, E), lysine (Lys, K), arginine (Arg, R) and histidine (His, H), preferably one or more selected from alanine, proline, glutamine, aspartic acid, and glutamic acid. In one exemplary embodiment, the polypeptide molecule is a dipeptide comprising an aspartic acid residue and a proline residue. In another exemplary embodiment, the polypeptide molecule is a tripeptide comprising a glutamic acid residue, an aspartic acid residue, and a proline residue. Without wishing to be bound by theory, the reaction mechanism of the present invention may involve the decomposition and recombination of various reaction raw material molecules at the atomic sites of the plasmonic composite catalyst and the nanostructured substrate.

[0095] Example

[0096] Example 1 Preparation of Plasmon Composite Catalyst

[0097] Preparation method of Co-Al2O3 (Co loaded or combined with Al2O3) composite catalyst:

[0098] 3g of nano-activated alumina (Al2O3, γ-phase, 10-20nm), 2.7g of lithium chloride (LiCl), 3.3g of potassium chloride (KCl), and 60mg of cobalt chloride hexahydrate (CoCl2·6H2O) were weighed and ground in an agate mortar for 30 minutes. The ground powder was spread on the bottom of a quartz boat and placed in a tube furnace. Nitrogen (N2) was first passed through the boat at a flow rate of 80mL / min for 30 minutes. The nitrogen flow rate was maintained constant and the tube furnace was heated to 500°C at a heating rate of 8°C / min. After calcination for 4 hours, the sample was cooled to room temperature. The calcined sample was placed in a 500mL beaker, filled with 500mL of deionized water, and soaked for approximately 4 hours. The supernatant was discarded, and the solution was washed with deionized water six times and separated by centrifugation at 8000rpm. It was then dried in an 80°C oven for 12 hours to obtain the 0.5% Co-Al2O3 composite catalyst used in the experiment.

[0099] By adjusting the amount of cobalt chloride hexahydrate added, Co-Al2O3 composite catalysts with loadings of 0.25% and 1% can be obtained respectively.

[0100] Preparation method of Fe-Al2O3 (Fe loaded on or combined with Al2O3), Ru-Al2O3 (Ru loaded on or combined with Al2O3), RuFe-Al2O3 (Ru and Fe loaded on or combined with Al2O3), RuCo-Al2O3 (Ru and Co loaded on or combined with Al2O3) composite catalysts:

[0101] (1) 0.125 g of ferric acetylacetonate and 50 g of aluminum acetylacetonate were evenly placed in a 100 mL zirconia ball mill.

[0102] (2) 50 zirconia balls with a diameter of 6 mm and 20 zirconia balls with a diameter of 10 mm were added to the above jar and ball milled for 10 h using a planetary ball mill at a speed of 400 rpm / min.

[0103] (3) The powder was placed in a porcelain boat and calcined in a muffle furnace in an air atmosphere for 5 hours at a temperature of 400°C.

[0104] (4) The calcined product is taken out to obtain a Fe-Al2O3 composite catalyst with a loading of about 0.25%.

[0105] (5) Replacing 0.125 g of ferric acetylacetonate with 0.125 g of ruthenium acetylacetonate in the above preparation process can obtain a Ru-Al2O3 composite catalyst with a loading of about 0.25%; replacing 0.125 g of ferric acetylacetonate with 0.0625 g of ruthenium acetylacetonate and 0.0625 g of ferric acetylacetonate, or replacing it with 0.0625 g of ruthenium acetylacetonate and 0.0625 g of cobalt acetylacetonate can obtain a RuFe-Al2O3 composite catalyst with a Ru and Fe loading of about 0.125% and a RuCo-Al2O3 composite catalyst with a Ru and Co loading of about 0.125% each.

[0106] The CoMn-MOF (Co and Mn supported or combined with MOF) composite catalyst was prepared by the following method:

[0107] 1. Synthesis of Metal-Organic Framework (MOF) Substrates

[0108] 4.2 mL of isopropyl titanate and 7.06 g of terephthalic acid were added to a mixed solution containing 108 mL of N,N-dimethylformamide and 12 mL of methanol. The mixture was stirred magnetically at 25°C for 30 minutes until a transparent, homogeneous solution was obtained. This solution was transferred to a 200 mL stainless steel autoclave, which was placed in an oven and heated to 150°C for 16 hours. After cooling to room temperature, the mixture was washed with methanol three times, centrifuged, and dried in an oven at 80°C for 16 hours to obtain the MOF substrate, which was then used. Scanning electron microscopy (SEM) revealed the MOF substrate to be columnar nanoparticles with a diameter of 700 nm and a height of 200 nm.

[0109] 2. Preparation of CoMn-MOF catalyst

[0110] To a 250mL beaker, add 2g of MOF substrate and 100mL of methanol and stir magnetically until uniform. In another 100mL beaker, weigh 18mg of manganese nitrate tetrahydrate (Mn(NO3)2·4H2O) and 12mg of cobalt nitrate hexahydrate (Co(NO3)2·6H2O), add 20mL of methanol, and stir to dissolve. Pour the mixture into the MOF dispersion. After stirring for 1 hour, wash with methanol, separate the mixture using a Buchner funnel, and dry in an oven at 80°C for 16 hours to obtain a CoMn-MOF catalyst with approximately 0.5% Co and Mn loadings.

[0111] Figures 1 and 2 show transmission electron micrographs of Co-Al2O3 and Fe-Al2O3 plasmonic composite catalysts, respectively. The yellow circles in the figures mark the atomic sites prepared on the nanosubstrate (only partially marked). It can be seen that the atomic sites are relatively evenly distributed on the substrate, with an atomic site spacing of approximately 1-10 nm.

[0112] Example 2 Photocatalytic reaction to produce polypeptide molecules

[0113] The catalyst is a CoMn-MOF composite catalyst prepared according to Example 1. The MOF (metal organic framework) is a nano-substrate structure, and the main component of MOF is TiO2. SEM characterization shows that the morphology of the MOF substrate is columnar nanoparticles with a diameter of 700 nm and a height of 200 nm; the atomic sites include Co and Mn, which are atomic clusters formed by 2-4 metals, distributed on the MOF surface, and the atomic clusters are spaced 5-10 nm apart.

[0114] In a 35 mL sealable pressure-bearing glass tube, add 1.9 g of CoMn-MOF composite catalyst and 5 mL of ultrapure water. Expel the air with CO2 and fill with 2 bar of CO2 and 2 bar of N2. Place the glass tube flat on glass wool to evenly distribute the catalyst and water. Irradiate vertically from above using a voltage-controlled halogen lamp. The incident light intensity is approximately 100-150 mW / m 2 A thermocouple was connected to the lower half of the glass tube to monitor the temperature. The tube temperature was maintained at 35°C ± 5°C, and the photocatalytic reaction was carried out under continuous illumination for 168 hours. After the reaction, the reaction system was centrifuged, and the liquid phase was collected for product analysis.

[0115] Add 0.04mL, 0.12mL, 0.2mL, 0.28mL, and 0.36mL of the standard solution (Thermo Scientific Bovine Serum Albumin 2mL / mL Pierce #23209) to a 10mL volumetric flask, dilute to volume, and shake well. The corresponding concentrations are 0.008, 0.024, 0.04, 0.056, and 0.072mol / L, respectively. Add 3mL of the Protein Quantification Assay Kit (Coomassie Plus REF 23236) to a 10mL glass vial. Add 0.1mL of purified water and the above standard solution to the glass vial, shake well, and test to generate a standard curve. Test the synthesized samples using the same procedure as above and compare to the standard curve to determine the total concentration of the reaction product polypeptide molecules.

[0116] After measurement and analysis, the concentration of peptide products in the product after stable reaction is about 23 μg / mL. It can be calculated that the unit catalyst activity is about 0.51 μg·g, which corresponds to the loading amount of catalyst active single atoms. -1 ·h -1 .

[0117] The product was analyzed by HPLC-MS (as shown in Figure 3). Its structure was a dipeptide formed by the condensation of an aspartic acid molecule and a proline molecule. It was a DP fragment containing a peptide bond in a tripeptide with the sequence EDP (glutamic acid-aspartic acid-proline) (molecular weight of approximately 231.1 g / mol).

[0118] Example 3. Effect of temperature on the photocatalytic reaction of producing polypeptide molecules

[0119] The photocatalytic reaction was carried out using the catalyst, reaction conditions, and process described in Example 2, with the glass tube temperatures controlled at 0°C ± 2°C, 5°C ± 2°C, 10°C ± 5°C, and 35°C ± 5°C, respectively, and continuous illumination for 168 hours. After completion of the reaction, the reaction system was centrifuged, and the liquid phase was analyzed for product using the method described in Example 2.

[0120] The total concentration of polypeptide products in the products after the reaction is stable within the above temperature range is listed in Table 1.

[0121] Table 1 Concentration of polypeptide molecules generated by reactions at different temperatures

[0122] The product was subjected to HPLC-MS analysis (as shown in FIG4 ). When the reaction temperature was within the aforementioned range (0-40° C.), the main product structure was a dipeptide formed by the condensation of an aspartic acid molecule and a proline molecule, which was a DP fragment containing a peptide bond in a tripeptide having the sequence EDP (molecular weight of 231.1 g / mol).

[0123] Example 4. Effect of energy radiation wavelength on the photocatalytic reaction of producing polypeptide molecules

[0124] The catalyst, reaction conditions and process in Example 2 were used, and the halogen lamp in Example 2 was replaced with a silicon nitride infrared light source (THORLABS-SLS303), and the radiation intensity was the same as that in Example 2. The temperature of the glass tube was controlled to be 10°C ± 5°C, and the light was continuously irradiated for 120 hours to carry out the photocatalytic reaction. After the reaction was completed, the reaction system was centrifuged and the liquid phase was taken for product analysis using the method in Example 2. After measurement and analysis, the concentration of polypeptide products in the product after the stable reaction was about 19 μg / mL. It was calculated that the unit catalyst activity was about 0.42 μg·g, corresponding to the loading amount of the catalyst active single atom. -1 ·h -1 .

[0125] HPLC-MS analysis (as shown in FIG5 ) showed that the main product was a tripeptide with the sequence EDP, which was formed by the condensation of one glutamic acid molecule, one aspartic acid molecule, and one proline molecule (molecular weight 360.14 g / mol).

[0126] In this specification and the appended claims, the singular forms "a," "an," and "the" include plural referents unless the context clearly dictates otherwise. Unless defined otherwise, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art. The methods described herein can be performed in any order that is logically possible, except for the specific order disclosed.

[0127] The representative examples are intended to help illustrate the present invention and are not intended to, and should not be construed as, limiting the scope of the present invention. Indeed, various modifications of the present invention and many other embodiments thereof, in addition to those shown and described herein, will become apparent to those skilled in the art, including the examples and the scientific and patent literature references cited herein. The examples contain important additional information, illustrations, and guidance that can be employed in the practice of the present invention in its various embodiments and equivalents.

Claims

1. A method for producing polypeptide molecules by energy radiation, comprising: contacting the composite catalyst with at least one hydrogen-containing source, at least one carbon-containing source, and at least one nitrogen-containing source, and energy irradiation of the composite catalyst, the hydrogen-containing source, the carbon-containing source and the nitrogen-containing source to produce polypeptide molecules, wherein The composite catalyst comprises at least one nano-based structure and at least one atomic site, wherein the atomic site comprises one or more chemical elements selected from the group consisting of Mn, Co, Fe, Ru, Rh, Al, Ag, Au, Pt, Pd, Cu, Ni, Zn, Ti, Os, Ir, and La.

2. The method of claim 1, wherein The energy radiation is light radiation.

3. The method according to claim 1 or 2, wherein The energy radiation allows the reaction to be carried out at a temperature between about 0°C and about 80°C, preferably about 0°C to about 60°C, about 0°C to about 40°C, about 2°C to about 40°C, about 5°C to about 40°C, about 10°C to about 40°C, about 10°C to about 35°C.

4. The method according to claim 2 or 3, wherein The optical radiation power of the optical radiation is 10-1500 mW / m 2 , preferably 10-500mW / m 2 , most preferably 100-200mW / m 2 .

5. The method according to any one of claims 2 to 4, wherein The wavelength of the optical radiation is from about 250 nm to about 1000 μm, preferably from 400 nm to about 1000 μm, preferably from 750 nm to about 500 μm, and most preferably from about 900 nm to about 15 μm.

6. The method according to any one of claims 1 to 5, wherein The polypeptide molecule is a molecule comprising two or more amino acids, wherein the amino acids are natural amino acids or non-natural amino acids.

7. The method according to any one of claims 1 to 6, wherein the distance between the nano-base structure and the atomic site is less than or equal to 5 nm, preferably less than or equal to 1 nm, more preferably less than 0.1 nm, and most preferably the two are in close contact.

8. The method according to any one of claims 1 to 7, wherein The atomic sites are bound to the nano-based structure, for example, physically or chemically.

9. The method according to any one of claims 1 to 8, wherein The mass percentage of the atomic sites to the nano-based structure is less than or equal to 50%, preferably 0.01% to 30%, preferably 0.01% to 5%, more preferably 0.1% to 2%, and most preferably 0.1% to 1%.

10. The method according to any one of claims 1 to 9, wherein The atomic sites are supported on the surface of the nano-based structure, in the internal pores, or distributed in the internal lattice of the nano-based structure, preferably the atomic sites are evenly distributed, and The interval between each atomic site is 0.2-500 nm, preferably 1-50 nm, more preferably 1-10 nm.

11. The method according to any one of claims 1 to 10, wherein The nano-based structure is selected from the group consisting of Mn, Co, Ce, Fe, Al, Ca, Ce, Cu, Ni, Ti, Zn, Si, Mo, Bi, V, C, N and their oxides, nitrides, sulfides, carbides, hydroxides, chlorides and metal-organic frameworks (MOFs), preferably metal-organic frameworks, TiO2 or Al2O3.

12. The method according to any one of claims 1 to 11, wherein The composite catalyst is a catalyst loaded with Co and Mn or combined with a metal organic framework, a catalyst loaded with Fe or combined with Al2O3, a catalyst loaded with Co or combined with Al2O3, a catalyst loaded with Ru or combined with Al2O3, a catalyst loaded with Ru and Fe or combined with Al2O3, or a catalyst loaded with Ru and Co or combined with Al2O3.

13. The method according to any one of claims 1 to 12, wherein At least one dimension of the length, width and height of the nano-base structure is about 1 nm to about 1000 nm, preferably about 70 nm to about 1000 nm, about 100 nm to about 800 nm, about 200 nm to about 500 nm.

14. The method according to any one of claims 1 to 13, wherein The nano-based structures are each independently about 1 nm to about 3000 nm in length, width, and height, preferably about 100 nm to about 3000 nm in length, about 500 nm to about 2500 nm in length, or about 1000 nm to about 2000 nm in length, and / or about 1 nm to about 1000 nm in width or height, about 70 nm to about 1000 nm in width, about 100 nm to about 800 nm in width, or about 200 nm to about 500 nm in height, or The nano-based structures each independently have an aspect ratio of about 1 to about 20, preferably about 1 to about 10, or about 2 to about 8.

15. The method according to any one of claims 1 to 14, wherein The nano-based structure has a shape of sphere, spike, flake, needle, blade, column, polyhedron, three-dimensional cone, cube, sheet, hemisphere, irregular three-dimensional shape, porous structure or any combination thereof.

16. The method according to any one of claims 1 to 15, wherein A plurality of said atomic sites are arranged in a pattern on said nanostructured substrate, preferably in a multi-layer arrangement, or A plurality of the atomic sites are randomly dispersed in the nano-based structure and / or on the surface.

17. The method according to any one of claims 1 to 16, wherein The carbon source is C 1-4 A hydrocarbon or non-organic carbon source, wherein the non-organic carbon source is selected from the group consisting of CO2, CO, synthesis gas, bicarbonate and any combination thereof, or air, industrial flue gas, tail gas or emissions containing more than one of these carbon sources, and the carbon source is preferably CO2 and CO.

18. The method according to any one of claims 1 to 17, wherein The hydrogen source is selected from water, H2, C 1-4 The group consisting of hydrocarbons and any combination thereof, or air, industrial flue gas, tail gas or emissions containing more than one of these hydrogen-containing sources, preferably water.

19. The method according to any one of claims 1 to 18, wherein The nitrogen source includes the group consisting of nitrogen, nitrates, nitrogen oxides and any combination thereof, or air, industrial flue gas, tail gas or emissions containing more than one of these nitrogen sources, preferably nitrogen.

Citation Information

Patent Citations

  • Method for producing polypeptide-based molecules by energy radiation

    CN116589523A

  • Methods for Producing Long-chain Hydrocarbon Molecules Using Heat Source

    US20210379570A1

  • Amino acid composition and method for catalytic synthesis of amino acid by means of energy radiation

    WO2021227077A1

  • Method for catalytic synthesis of ammonia by means of radiation

    WO2021227078A1

  • Method for producing hydrocarbon molecule by means of energy radiation

    WO2022120824A1